Polyfunctional vinylbenzyl compound, resin composition, prepreg, resin film, metal-clad laminated sheet, printed wiring board, and semiconductor package
The polyfunctional vinylbenzyl compound, formed by reacting aromatic condensed rings, biphenylene groups, and vinylbenzyl groups, addresses the challenge of achieving high flame retardancy and excellent dielectric properties in resin compositions for electronic devices, ensuring effective performance in metal-clad laminates and semiconductor packages.
Patent Information
- Application Number
- PCT/JP2024/015876
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-23
- Publication Date
- 2024-10-31
AI Technical Summary
Current resin compositions used in electronic devices face challenges in achieving high flame retardancy and excellent dielectric properties simultaneously, particularly with the increasing demand for halogen-free phosphorus-based flame retardants, which can compromise dielectric properties when used in large quantities.
A polyfunctional vinylbenzyl compound is developed by reacting a compound with an aromatic condensed ring, a biphenylene group, and a vinylbenzyl group, resulting in a resin composition that maintains excellent dielectric properties while providing high flame retardancy, suitable for use in metal-clad laminates, printed wiring boards, and semiconductor packages.
The polyfunctional vinylbenzyl compound enhances the flame retardancy and dielectric properties of the cured resin, achieving low dielectric loss tangent and constant, particularly in high frequency bands, while maintaining the resin's structural integrity and performance in electronic devices.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Polyfunctional vinylbenzyl compounds, resin compositions, prepregs, resin films, metal-clad laminates, printed wiring boards, and semiconductor packages
[0001] The present disclosure relates to a polyfunctional vinylbenzyl compound, a resin composition, a prepreg, a resin film, a metal-clad laminate, a printed wiring board, and a semiconductor package.
[0002] Metal-clad laminates, such as copper-clad laminates, prepregs that can be used with metal-clad laminates, and semiconductor packages that use metal-clad laminates are used in a variety of electronic devices, such as smartphones and other portable communication devices, personal computers, industrial computers, servers, large servers, routers, and mobile base stations. They are also used in electronic devices installed in home appliances, automobiles, etc. In particular, with the spread of 5G, there is an increasing demand for electronic communication devices to process massive amounts of data at high speeds.
[0003] When electronic devices process huge amounts of data at high speeds, circuit board materials with low transmission loss in the high-frequency range are required. Resins with excellent dielectric properties are used as circuit board materials, and circuit boards with low transmission loss are provided, but recent advances in communication technology have created a demand for the development of resins with even better dielectric properties.
[0004] In recent years, growing awareness of environmental issues has made it essential to consider the environment when it comes to electronic devices and components. Therefore, there is a growing demand for halogen-free phosphorus-based flame retardants as additives to circuit board materials, replacing conventional halogen-containing flame retardants. However, when a large amount of phosphorus-based flame retardants is added to circuit board materials to enhance flame retardancy, there is a concern that the dielectric properties of the circuit board materials may be reduced.
[0005] Patent Document 1 proposes a resin composition that maintains the excellent dielectric properties of polyphenylene ether and provides a cured product with excellent heat resistance and flame retardancy. The resin composition contains a modified polyphenylene ether compound, a cross-linking curing agent, and a flame retardant, and the flame retardant contains a compatible phosphorus compound that is soluble in the mixture of the modified polyphenylene ether compound and the cross-linking curing agent, and an incompatible phosphorus compound that is not soluble in this mixture.
[0006] JP 2015-86330 A
[0007] The technology disclosed in Patent Document 1 attempts to suppress inhibition of the curing reaction between a modified polyphenylene ether compound and a crosslinking curing agent by using a compatible phosphorus compound and an incompatible phosphorus compound as a flame retardant, thereby improving the flame retardancy of the cured product. Meanwhile, in the resin composition disclosed in Patent Document 1, the modified polyphenylene ether contains a polyphenylene ether chain, and a substituent having a carbon-carbon unsaturated double bond is bonded to the oxygen atom of the phenol group instead of the hydrogen atom of the phenol group. Because such modified polyphenylene ether contains a large number of ether bonds, it may not be able to withstand the increasingly stringent dielectric property requirements of recent years. Furthermore, the technology disclosed in Patent Document 1 does not consider the flame retardancy of the thermosetting resin itself.
[0008] An object of the present disclosure is to provide a polyfunctional vinylbenzyl compound for providing products that exhibit high flame retardancy and excellent dielectric properties, a resin composition containing the polyfunctional vinylbenzyl compound, and a prepreg, a resin film, a metal-clad laminate, a printed wiring board, and a semiconductor package that are each made of the resin composition.
[0009] The present disclosure includes the following embodiments. The present disclosure is not limited to the following embodiments. One embodiment relates to a polyfunctional vinylbenzyl compound obtained by reacting a compound having an aromatic fused ring, a compound having a biphenylene group, and a compound having a vinylbenzyl group.
[0010] Another embodiment relates to a polyfunctional vinylbenzyl compound comprising a unit having an aromatic fused ring and a unit having a biphenylene group, wherein the aromatic fused ring is bonded to two carbon atoms on the ring of the biphenylene group, respectively, directly or via a linking group, and the linking group has a structure that is a divalent hydrocarbon group, and wherein the compound has a vinylbenzyl group that is bonded directly to a carbon atom on the ring of the aromatic fused ring.
[0011] Another embodiment relates to a polyfunctional vinylbenzyl compound represented by the following formula (1):
[0012] (In formula (1), R1 are each independently a monovalent group having 1 to 30 carbon atoms or a hydrogen atom, 2 are each independently a monovalent group having 1 to 30 carbon atoms, a hydrogen atom, or a bonding position to another structure; each X is independently an alkylene group having 1 to 4 carbon atoms or a single bond; and n is an integer of 1 or greater.
[0013] The present disclosure can provide a polyfunctional vinylbenzyl compound for providing products that exhibit high flame retardancy and excellent dielectric properties, a resin composition containing the polyfunctional vinylbenzyl compound, and a prepreg, resin film, metal-clad laminate, printed wiring board, and semiconductor package that are each made of the resin composition.
[0014] The present invention will be described in detail below using several embodiments, but the present invention is not limited to the following embodiments.
[0015] In the present disclosure, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper or lower limit of a certain numerical range may be replaced with the upper or lower limit of another numerical range. Furthermore, the upper or lower limit of a numerical range described in the present disclosure may be replaced with a value shown in the examples. In the present disclosure, unless otherwise specified, each component may contain one or more corresponding substances. In the present disclosure, when a resin composition contains multiple substances corresponding to each component, the content of each component in the resin composition means the total amount of the multiple substances present in the resin composition, unless otherwise specified.
[0016] In the present disclosure, the weight average molecular weight (Mw) and number average molecular weight (Mn) of a polymer are measured according to the following measurement method, unless otherwise specified.
[0017] The weight average molecular weight (Mw) and number average molecular weight (Mn) are calculated by gel permeation chromatography (GPC) from a calibration curve using standard polystyrene. The calibration curve is approximated by a cubic equation using standard polystyrene: TSKstandard POLYSTYRENE (Types: A-500, A-2500, A-5000, F-2, F-2, F-4, F-40, F-128, F-288) [manufactured by Tosoh Corporation, trade name]. The GPC conditions are shown below.
[0018] Apparatus: High-speed GPC apparatus "HLC-8320GPC" (Tosoh Corporation, trade name) Detector: Ultraviolet absorption detector "UV-8320" (Tosoh Corporation, trade name) Columns: Guard column; TSKgel guard column Super (HZ)-M+, column; TSKgel SuperMultipore HZ-M (2 columns), reference column; TSKgel Super H-RC (2 columns) (all Tosoh Corporation, trade names) Column size: 4.6 x 20 mm (guard column), 4.6 x 150 mm (column), 6.0 x 150 mm (reference column)
[0019] Eluent: tetrahydrofuran Sample concentration: 10 mg / 1 mL Injection volume: 2 μL Flow rate: 0.35 mL / min Measurement temperature: 40° C.
[0020] "Polyfunctional vinylbenzyl compound" According to one embodiment, there is provided a polyfunctional vinylbenzyl compound obtained by reacting a compound having an aromatic fused ring, a compound having a biphenylene group, and a compound having a vinylbenzyl group.
[0021] The polyfunctional vinylbenzyl compound may contain a biphenyl skeleton derived from a compound having a biphenylene group. The biphenyl skeleton is a thermally and chemically stable skeleton that is resistant to decomposition even at high temperatures, thereby enhancing the flame retardancy of cured resin materials obtained using the polyfunctional vinylbenzyl compound. Furthermore, the biphenyl skeleton, together with the aromatic fused ring derived from a compound having an aromatic fused ring and the vinylbenzyl group derived from a compound having a vinylbenzyl group, has a low polarity structure, contributing to a low dielectric constant and low dielectric dissipation factor of cured resin materials obtained using the polyfunctional vinylbenzyl compound, and achieving a low dielectric dissipation factor, particularly in the high frequency range. The polyfunctional vinylbenzyl compound contains an aromatic fused ring, which has a rigid and low polarity structure, contributing to a low dielectric dissipation factor, particularly in the high frequency range, of cured resin materials obtained using the polyfunctional vinylbenzyl compound.
[0022] (Compound Having Aromatic Fused Ring) In a compound having an aromatic fused ring, the number of rings in the aromatic fused ring is not particularly limited, but 2 to 5 rings are preferred. The aromatic fused ring may be a fused ring of two or more aromatic rings. Furthermore, the aromatic fused ring may have at least one aromatic ring, and may be a fused ring of at least one aromatic ring with one or two or more alicyclic hydrocarbon rings. The aromatic fused ring may be substituted or unsubstituted. The substituent may be an alkyl group or the like. The alkyl group for the substituent may have 1 to 30, 1 to 12, or 1 to 4 carbon atoms, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, and a sec-butyl group. The number of carbon atoms in the compound having an aromatic fused ring is preferably 9 to 40, more preferably 9 to 20, and even more preferably 9 to 12.
[0023] Examples of compounds having an aromatic fused ring include compounds having an indene ring, an indane ring, a phenanthrene ring, an acenaphthylene ring, a fluorene ring, etc. At least one carbon atom of these aromatic fused rings may have a substituent. From the viewpoint of dielectric properties and flame retardancy, the compound having an aromatic fused ring is preferably a compound having an indene ring or a derivative thereof, more preferably substituted or unsubstituted indene, and even more preferably unsubstituted indene. The compound having an aromatic fused ring may be used alone or in combination of two or more in the reaction of the polyfunctional vinylbenzyl compound.
[0024] (Biphenylene group-containing compound) The unit derived from the biphenylene group-containing compound can introduce a biphenylene group into the polyfunctional vinylbenzyl compound, thereby contributing to flame retardancy. Furthermore, since this polyfunctional vinylbenzyl compound has a biphenylene group-containing unit, it can improve the dielectric properties of the cured resin composition.
[0025] The compound having a biphenylene group is preferably a compound having one biphenylene group and two reactive groups. For example, the compound having a biphenylene group is preferably a compound having one biphenylene group and one reactive group on each of the two benzene rings of the biphenylene group, and more preferably a compound having one biphenylene group and one reactive group on each of the 4- and 4'-positions of the biphenylene group. The reactive group is preferably a haloalkyl group. The haloalkyl group preferably has 1 to 12 carbon atoms, more preferably 1 to 8 carbon atoms, and even more preferably 1 to 4 carbon atoms. The haloalkyl group is preferably an alkyl group in which at least one hydrogen atom has been substituted with a halogen atom, and the halogen atom is preferably a chlorine atom or a bromine atom, and the number of halogen atoms substituted is preferably one. Examples of haloalkyl groups include a chloromethyl group, a chloroethyl group, a bromomethyl group, and a bromoethyl group.
[0026] In compounds having a biphenylene group, the biphenylene group may be substituted or unsubstituted. The substituent may be an alkyl group or the like. The alkyl group as the substituent may have 1 to 30, 1 to 12, or 1 to 4 carbon atoms, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, and a sec-butyl group. The compound having a biphenylene group may contain a functional group containing a heteroatom as a substituent, but from the viewpoint of dielectric properties, it is preferable that the compound does not contain a functional group containing a heteroatom. However, the compound having a biphenylene group may contain a halogen atom contained as the reactive group. Note that the compound having a biphenylene group is a compound different from a compound having an aromatic fused ring and does not have an aromatic fused ring.
[0027] The compound having a biphenylene group preferably includes 4,4'-bis(haloalkyl)biphenyl. Examples of the compound having a biphenylene group include 4,4'-bis(chloromethyl)biphenyl, 3,4'-bis(chloromethyl)biphenyl, 3,3'-bis(chloromethyl)biphenyl, 4,4'-bis(bromomethyl)biphenyl, 3,4'-bis(bromomethyl)biphenyl, and 3,3'-bis(bromomethyl)biphenyl. The compound having a biphenylene group may be used alone or in combination of two or more in the reaction of the polyfunctional vinylbenzyl compound.
[0028] (Compound having a vinylbenzyl group) The unit derived from the compound having a vinylbenzyl group provides a polymerizable functional group in the polyfunctional vinylbenzyl compound, and can contribute to thermosetting. In addition, the polyfunctional vinylbenzyl compound can also contribute to the dielectric properties and flame retardancy of the cured product of the resin composition by introducing a polymerizable functional group derived from the compound having a vinylbenzyl group.
[0029] In the polyfunctional vinylbenzyl compound, the vinylbenzyl group of the compound having a vinylbenzyl group is preferably bonded to the aromatic fused ring of the compound having an aromatic fused ring, and more specifically, the vinylbenzyl group of the compound having a vinylbenzyl group is preferably directly bonded to a carbon atom on the aromatic fused ring of the compound having an aromatic fused ring. From this viewpoint, the compound having a vinylbenzyl group is preferably a vinylbenzyl halide. The halogen atom of the vinylbenzyl halide is preferably a chlorine atom or a bromine atom. For example, the vinylbenzyl halide may be, for example, vinylbenzyl chloride or vinylbenzyl bromide, and preferably vinylbenzyl chloride.
[0030] The vinylbenzyl group may be any of o-vinylbenzyl, m-vinylbenzyl, and p-vinylbenzyl groups, with m-vinylbenzyl or p-vinylbenzyl groups being preferred, and p-vinylbenzyl groups being more preferred. Examples include 4-vinylbenzyl chloride. When a compound containing a p-vinylbenzyl group is used, a mixture of a compound containing a p-vinylbenzyl group and a compound containing an m-vinylbenzyl group may be used. In this mixture, the mass ratio of the compound containing a p-vinylbenzyl group to the compound containing an m-vinylbenzyl group may be 20 to 80:20 or 40:60 to 60:40.
[0031] In a compound having a vinylbenzyl group, the vinylbenzyl group may be substituted or unsubstituted. The substituent may be an alkyl group or the like. The alkyl group as the substituent may have 1 to 30, 1 to 12, or 1 to 4 carbon atoms, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, and a sec-butyl group. Note that a compound having a vinylbenzyl group is a compound different from a compound having an aromatic fused ring and a compound having a biphenylene group, and does not have an aromatic fused ring or a biphenylene group.
[0032] The compound having a vinylbenzyl group may be used alone or in combination of two or more in the reaction of the polyfunctional vinylbenzyl compound.
[0033] The method for reacting a compound having an aromatic fused ring, a compound having a biphenylene group, and a compound having a vinylbenzyl group is not particularly limited. For example, the reaction can be carried out by mixing the compound having an aromatic fused ring, the compound having a biphenylene group, and the compound having a vinylbenzyl group, and heating and stirring as necessary. The reaction can be carried out in a solvent, and the solvent is not particularly limited and may be appropriately selected from the organic solvents exemplified as solvents for the resin composition described below. The reaction temperature is preferably 20 to 80°C. Additives such as a phase transfer catalyst and a polymerization inhibitor may also be added to the mixture during the reaction.
[0034] The phase transfer catalyst is used in a reaction system containing an organic solvent and water. The organic solvent is preferably one that is incompatible with water, such as toluene. Examples of the phase transfer catalyst include quaternary ammonium salts such as tetra-n-butylammonium chloride, tetra-n-butylammonium bromide, tetraethylammonium chloride, tetraethylammonium bromide, tetrapropylammonium chloride, tetrapropylammonium bromide, benzyltrimethylammonium chloride, benzyltrimethylammonium bromide, benzyltributylammonium chloride, benzyltributylammonium bromide, benzyldimethyltetradecylammonium chloride, tricaprylmethylammonium chloride, tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide, trioctylmethylammonium chloride, and tetra-n-butylammonium hydrogen sulfate; and quaternary phosphonium salts such as tetra-n-butylphosphonium chloride, tetra-n-butylphosphonium bromide, tetraphenylphosphonium chloride, tetraphenylphosphonium bromide, benzyltriphenylphosphonium chloride, and benzyltriphenylphosphonium bromide. The phase transfer catalyst may be used alone or in combination of two or more.
[0035] The polymerization inhibitor is added to the reaction system to adjust the degree of polymerization of the polyfunctional vinylbenzyl compound. Examples of the polymerization inhibitor include hydroquinone, methylhydroquinone, tert-butylhydroquinone, 2,6-di-tert-butylhydroquinone, 2,5-di-tert-butylhydroquinone, hydroquinone monomethyl ether, 1,4-benzoquinone, 2-tert-butyl-1,4-benzoquinone, 2-tert-butylphenol, 2,4-di-tert-butylphenol, 2,6-di-tert-butylphenol, cresol, catechol, and 4-tert-butylcatechol. Chole, pyrogallol, 4-methoxyphenol, thiodiphenylamine, phenothiazine, 3,7-dioctylphenothiazine, 3,7-dicumylphenothiazine, 2,2,6,6-tetramethylpiperidine-1-oxyl, 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine-1-oxyl, bis(2,2,6,6-tetramethyl-1-piperidinyloxy-4-yl)sebacate, and the like.
[0036] Furthermore, from the viewpoint of reaction control, the reaction can be carried out under basic conditions. For example, a basic compound may be added to the mixture. Examples of basic compounds include alkali metal hydroxides and alkali metal alkoxides, and specific examples include sodium hydroxide. The product obtained by the reaction may be purified, if necessary, by known methods such as concentration, reprecipitation, and washing.
[0037] The polyfunctional vinylbenzyl compound preferably has a partial structure in which a unit (A) having an aromatic fused ring and a unit (B) having a biphenylene group are bonded as in ABA by reacting a compound having an aromatic fused ring, a compound having a biphenylene group, and a compound having a vinylbenzyl group. It is more preferable that a vinylbenzyl group is bonded to the aromatic fused ring of at least one of the two A's in this ABA partial structure. For example, the polyfunctional vinylbenzyl compound is preferably a compound represented by ABA, in which a vinylbenzyl group is bonded to each of the aromatic fused rings of the two A's. These structures improve dielectric properties, particularly a low dielectric tangent, and provide flame retardancy.
[0038] The polyfunctional vinylbenzyl compound may be an equimolar reaction of a compound having an aromatic fused ring and a compound having a biphenylene group, or may be a reaction in which, in terms of molar ratio, 100 molar parts of the compound having an aromatic fused ring and 100 molar parts of the compound having a biphenylene group are reacted in an amount of 100 molar parts or less, 80 molar parts or less, 60 molar parts or less, or 50 molar parts or less. More specifically, the polyfunctional vinylbenzyl compound may be a reaction in which, in terms of molar ratio, 100 molar parts of the compound having an aromatic fused ring and 10 to 100 molar parts, 20 to 80 molar parts, 30 to 60 molar parts, or 40 to 50 molar parts of the compound having a biphenylene group are reacted in an amount of 10 to 100 molar parts, 20 to 80 molar parts, 30 to 60 molar parts, or 40 to 50 molar parts. In the reaction, the degree of polymerization can be increased by increasing the proportion of the compound having a biphenylene group, but this proportion may be limited from the perspective of accelerating the reaction. Note that when the molecular weight of the polyfunctional vinylbenzyl compound is small, it is preferable that the terminal structure be a unit derived from the compound having an aromatic fused ring. From this perspective, it is also desirable to satisfy these molar ratio ranges.
[0039] The polyfunctional vinylbenzyl compound may be an equimolar reaction of a compound having an aromatic fused ring with a compound having a vinylbenzyl group, or may be a reaction in which, in terms of molar ratio, 200 parts by weight or less, 140 parts by weight or less, 120 parts by weight or less, or 100 parts by weight or less of a compound having a vinylbenzyl group is reacted with 100 parts by weight of a compound having an aromatic fused ring. More specifically, in terms of molar ratio, 50 to 200 parts by weight, 60 to 140 parts by weight, 80 to 120 parts by weight, or 90 to 100 parts by weight of a compound having a vinylbenzyl group is reacted with 100 parts by weight of a compound having an aromatic fused ring. In the reaction, by introducing one or more vinylbenzyl groups per aromatic fused ring, better curing acceleration of the resin composition can be obtained.
[0040] Another embodiment provides a polyfunctional vinylbenzyl compound comprising a unit having an aromatic fused ring and a unit having a biphenylene group, wherein the aromatic fused rings are bonded to two carbon atoms on the biphenylene group ring either directly or via a linking group, and the linking group has a structure of a divalent hydrocarbon group, and the polyfunctional vinylbenzyl compound comprises a vinylbenzyl group bonded directly to a carbon atom on the aromatic fused ring ring. In this polyfunctional vinylbenzyl compound, it is preferred that the unit having an aromatic fused ring has an indene ring, and the vinylbenzyl group is directly bonded to at least one carbon atom among the 1-, 2-, and 3-positions of the indene ring.
[0041] The polyfunctional vinylbenzyl compound according to this embodiment is not limited by its synthesis method, but can be obtained, for example, by reacting the above-described compound having an aromatic fused ring, a compound having a biphenylene group, and a compound having a vinylbenzyl group.
[0042] (Still Another Embodiment) According to still another embodiment, there is provided a polyfunctional vinylbenzyl compound, which is a compound represented by the following formula (1):
[0043]
[0044] (In formula (1), R 1are each independently a monovalent group having 1 to 30 carbon atoms or a hydrogen atom, 2 are each independently a monovalent group having 1 to 30 carbon atoms, a hydrogen atom, or a bonding position to another structure; each X is independently an alkylene group having 1 to 4 carbon atoms or a single bond; and n is an integer of 1 or greater.
[0045] The polyfunctional vinylbenzyl compound according to this embodiment is not limited by its synthesis method, but can be obtained, for example, as described above, by reacting substituted or unsubstituted indene, substituted or unsubstituted 4,4'-bis(haloalkyl)biphenyl, and substituted or unsubstituted vinylbenzyl halide. 1 or R 2 It is a group represented by the following formula:
[0046] In formula (1), R 1 are each independently a monovalent group having 1 to 30 carbon atoms or a hydrogen atom. 1 The monovalent group represented by R is preferably a saturated or unsaturated, chain or cyclic hydrocarbon group. 1 The monovalent group represented by may have 1 to 30, 1 to 12, or 1 to 4 carbon atoms. 1 The monovalent group represented by the formula (1) may specifically be an alkyl group, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, and a sec-butyl group. 1 may be all the same or some or all may be different. 1 is preferably a hydrogen atom in part or in whole.
[0047] In formula (1), R 2 are each independently a monovalent group having 1 to 30 carbon atoms, a hydrogen atom, or a bonding position to another structure. 2 are each independently R 1 Alternatively, R 2 may be a bonding site with a unit having a biphenyl group, a unit having a vinylbenzyl group, etc. 2may be all the same or some or all may be different. 2 One or both are R 1 Preferably, it is a group represented by the following formula: and more preferably a hydrogen atom.
[0048] In formula (1), X's are each independently an alkylene group having 1 to 4 carbon atoms or a single bond. Examples include a methylene group, an ethylene group, a trimethylene group, an isopropylene group, an n-butylene group, an isobutylene group, a tert-butylene group, and a sec-butylene group. In formula (1), multiple X's may all be the same, or some or all may be different. In formula (1), it is preferable that some or all of X's are methylene groups or single bonds, and a methylene group is more preferable.
[0049] In formula (1), n is an integer of 1 or more. n is an integer of preferably 1 to 10, more preferably 1 to 5, and still more preferably 1 to 4. n may be 1. Furthermore, in formula (1), n may be an integer appropriately determined depending on the weight average molecular weight (Mw) of the polyfunctional vinylbenzyl compound, which will be described later.
[0050] In formula (1), the bonding site between the indene ring and the vinylbenzyl group is preferably position 1 of the indene ring. Furthermore, the bonding site between the indene ring and X is preferably position 1 or 2 of the indene ring. Furthermore, the vinylbenzyl group may be any of an o-vinylbenzyl group, an m-vinylbenzyl group, and a p-vinylbenzyl group, with a p-vinylbenzyl group being more preferred. In formula (1), it is preferred that some or all of the vinylbenzyl groups are p-vinylbenzyl groups.
[0051] The polyfunctional vinylbenzyl compound represented by formula (1) is preferably a compound containing a partial structure represented by the following formula (2).
[0052]
[0053] In formula (2), R 3 are each independently a monovalent group having 1 to 30 carbon atoms, a hydrogen atom, or a bonding position to another structure. 3 For details, see R in formula (1). 2The other configurations are as explained in the formula (1).
[0054] In formula (2), a plurality of R 3 may be all the same or some or all may be different. 3 is one or both of R of formula (1) 1 Preferably, it is a group represented by the following formula: and more preferably a hydrogen atom.
[0055] The polyfunctional vinylbenzyl compound represented by formula (1) contains repeating units of units having an aromatic fused ring and units having a biphenylene group, and therefore the molar ratio of the units having a biphenylene group may be 50 to 150 molar parts, 50 to 100 molar parts, 50 to 80 molar parts, or 50 to 60 molar parts per 100 parts of the units having an aromatic fused ring. When the molecular weight of the polyfunctional vinylbenzyl compound is small, it is preferable that the terminal structure is a unit derived from a compound having an aromatic fused ring. From this perspective, it is also desirable to satisfy these molar ratio ranges.
[0056] The polyfunctional vinylbenzyl compound represented by formula (1) contains a structure in which a unit having a vinylbenzyl group is bonded to a unit having an aromatic fused ring, and therefore the molar ratio of the unit having a vinylbenzyl group may be 50 to 200 parts by mole, 100 to 150 parts by mole, or 100 to 120 parts by mole per 100 parts by mole of the unit having an aromatic fused ring.
[0057] The weight average molecular weight (Mw) of the polyfunctional vinylbenzyl compound will be described below. The weight average molecular weight (Mw) of the polyfunctional vinylbenzyl compound may be 100,000 or less, 50,000 or less, 10,000 or less, 5,000 or less, or 2,000 or less. Within these ranges, the resin composition can have better solvent solubility and coatability, and the coating film, semi-cured product, and cured product can have better moldability and flexibility. The weight average molecular weight (Mw) of the polyfunctional vinylbenzyl compound may be 400 or more, 500 or more, 800 or more, or 1,000 or more. Within these ranges, the resin composition can have better solvent solubility and coatability, and the coating film, semi-cured product, and cured product can have better moldability and flexibility. For example, the weight average molecular weight (Mw) of the polyfunctional vinylbenzyl compound may be 400 to 100,000, 400 to 50,000, 500 to 10,000, 800 to 5,000, or 1,000 to 2,000.
[0058] "Resin Composition" The resin composition according to one embodiment contains a polyfunctional vinylbenzyl compound. Details of the polyfunctional vinylbenzyl compound are as described above.
[0059] The resin composition may contain a polyfunctional vinylbenzyl compound obtained by reacting a compound having an aromatic fused ring, a compound having a biphenylene group, and a compound having a vinylbenzyl group. The polyfunctional vinylbenzyl compound may be contained as a reaction product. In this case, the resin composition may contain multiple types of polyfunctional vinylbenzyl compounds having different molecular weights and molecular structures.
[0060] The resin composition is not limited to a synthesis method of a polyfunctional vinylbenzyl compound, and may include a polyfunctional vinylbenzyl compound that includes a unit having an aromatic fused ring and a unit having a biphenylene group, in which the aromatic fused rings are bonded to two carbon atoms on the ring of the biphenylene group, respectively, directly or via a linking group, and the linking group is a divalent hydrocarbon group, and has a vinylbenzyl group bonded directly to a carbon atom on the ring of the aromatic fused ring, or may include a compound represented by formula (1).
[0061] A resin composition containing such a polyfunctional vinylbenzyl compound can have excellent dielectric properties and flame retardancy in the cured product.
[0062] The resin composition may further contain, in addition to the polyfunctional vinylbenzyl compound, at least one of a thermosetting resin and a thermoplastic resin as another resin component.
[0063] Examples of thermosetting resins include epoxy resins, maleimide compounds, modified polyphenylene ether resins, phenolic resins, polyimide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, and melamine resins. Thermosetting resins can undergo polymerization and / or curing reactions when heated, optionally in the presence of a polymerization initiator or the like. Thermosetting resins may be used singly or in combination of two or more.
[0064] The thermoplastic resin may contain an elastomer. Examples of the elastomer include diene-based elastomers, olefin-based elastomers, polysulfide-based elastomers, silicone-based elastomers, fluorine-based elastomers, urethane-based elastomers, and ether-based elastomers. More specifically, examples of the diene-based elastomers include styrene-butadiene rubber (SBR), butadiene rubber (BR), styrene-isoprene rubber, isoprene rubber (IR), chloroprene rubber (CR), and acrylonitrile-butadiene rubber (NBR). Examples of the olefin-based elastomers include butyl rubber (IIR), ethylene-propylene rubber, ethylene-vinyl acetate rubber, chlorosulfonated polyethylene, and acrylic rubber. These elastomers may be non-hydrogenated or hydrogenated. The elastomers may be used alone or in combination.
[0065] The polyfunctional vinylbenzyl compound may be present in an amount of 10 to 100% by mass, 30 to 90% by mass, 50 to 80% by mass, or 60 to 80% by mass relative to the total mass of the resin components of the resin composition. In the present disclosure, the total mass of the resin components of the resin composition is the total mass of the polymer, and the polymerizable oligomer and monomer.
[0066] The total mass of the polyfunctional vinylbenzyl compound and other thermosetting resins may be 10 to 100% by mass, 30 to 90% by mass, 50 to 80% by mass, or 60 to 80% by mass, based on the total mass of the resin components of the resin composition. The total mass of the thermoplastic resins may be 1 to 90% by mass, 10 to 70% by mass, or 20 to 50% by mass, based on the total mass of the resin components of the resin composition. The total mass of the resin components may be 10 to 80% by mass, 30 to 70% by mass, or 40 to 60% by mass, based on the total mass of the resin composition.
[0067] The resin composition may be a solvent-free composition, or may contain a solvent. The solvent can adjust the viscosity of the resin composition and further improve the coatability. The solvent is preferably an organic solvent.
[0068] Examples of organic solvents include alcohol-based solvents such as ethanol, propanol, butanol, methyl cellosolve, ethylene glycol monobutyl ether, and propylene glycol monomethyl ether; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether-based solvents such as tetrahydrofuran; aromatic hydrocarbon-based solvents such as toluene, xylene, and mesitylene; nitrogen-containing solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; sulfur-containing solvents such as dimethyl sulfoxide; and ester-based solvents such as γ-butyrolactone. The organic solvents may be used alone or in combination of two or more.
[0069] When the resin composition contains a solvent, the components other than the solvent are considered to be solids, and the amount of solids may be 10 to 80 mass %, 30 to 70 mass %, or 40 to 60 mass % relative to the total mass of the resin composition. Note that the solvent does not include compounds containing polymerizable functional groups.
[0070] The resin composition may contain an inorganic filler as an optional component. Examples of the inorganic filler include silica (SiO 2 ), alumina (Al 2 O 3 ), titanium oxide, barium titanate, strontium titanate, potassium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, aluminum borate, silicon carbide, mica, beryllia, clay, talc, etc.
[0071] The shape and size of the inorganic filler are not particularly limited. The average particle diameter of the inorganic filler may be, for example, 0.01 to 20 μm, or 0.1 to 10 μm. Here, the average particle diameter of the inorganic filler is the particle diameter at a point corresponding to an integrated value of 50% in a volume-based particle distribution measured by a laser diffraction scattering method.
[0072] The inorganic filler may be used alone or in combination of two or more. The inorganic filler may be used in an amount of 10 to 80% by volume, 30 to 70% by volume, or 50 to 60% by volume relative to the solid content of the resin composition.
[0073] The resin composition may further contain a curing catalyst to promote curing of the polyfunctional vinylbenzyl compound. A radical polymerization initiator can be used as the curing catalyst. The radical polymerization initiator may be a thermal radical polymerization initiator or a photoradical polymerization initiator, but a thermal radical polymerization initiator is preferred. The radical polymerization initiator is not particularly limited, and examples thereof include an azo-based polymerization initiator and an organic peroxide-based polymerization initiator.
[0074] The amount of the curing catalyst used may be adjusted as appropriate, and may be, for example, 0.01 to 5 parts by mass, 0.1 to 4 parts by mass, or 0.5 to 2 parts by mass relative to 100 parts by mass of the polyfunctional vinylbenzyl compound.
[0075] The resin composition may further contain a flame retardant. Examples of flame retardants include phosphorus-based flame retardants, metal hydrates, and halogen-based flame retardants. From the viewpoint of environmental issues, phosphorus-based flame retardants are preferred. The phosphorus-based flame retardant may be either an inorganic phosphorus-based flame retardant or an organic phosphorus-based flame retardant, but an organic phosphorus-based flame retardant is preferred. Examples of inorganic phosphorus-based flame retardants include red phosphorus; ammonium phosphates such as monoammonium phosphate, diammonium phosphate, triammonium phosphate, and ammonium polyphosphate; inorganic nitrogen-containing phosphorus compounds such as phosphoric acid amide; phosphoric acid; and phosphine oxide. Examples of organic phosphorus-based flame retardants include aromatic phosphate esters, monosubstituted phosphonic acid diesters, disubstituted phosphinic acid esters; metal salts of disubstituted phosphinic acids, organic nitrogen-containing phosphorus compounds, and cyclic organic phosphorus compounds. Examples of metal salts of disubstituted phosphinic acids include lithium salts, sodium salts, potassium salts, calcium salts, magnesium salts, aluminum salts, titanium salts, and zinc salts.
[0076] The amount of the flame retardant may be 0.1 to 30 parts by mass, 1 to 20 parts by mass, or 5 to 10 parts by mass per 100 parts by mass of the total mass of the resin components of the resin composition.
[0077] The resin composition may further contain additives other than the above components, such as a curing accelerator, an antioxidant, a heat stabilizer, an antistatic agent, an ultraviolet absorber, a pigment, a colorant, and a lubricant, as long as the effects of the present invention are not impaired.
[0078] The method for producing the resin composition is not particularly limited. In one example of the method for producing the resin composition, optional components are added to a polyfunctional vinylbenzyl compound as needed and mixed to obtain a resin composition. More specifically, the polyfunctional vinylbenzyl compound is dissolved or dispersed in a solvent, and additives and the like are added as needed and mixed to obtain a resin composition. The conditions for mixing the components, such as the order, temperature, and time, are not particularly limited and may be appropriately adjusted depending on the type of raw material, production scale, production equipment, etc.
[0079] The cured product of the resin composition preferably has a heat residue ratio, expressed as the mass after heating at 800°C relative to the mass before heating, of 25% by mass or more, more preferably 28% by mass or more, and even more preferably 30% by mass or more. Within these ranges, a product with excellent flame retardancy can be provided.
[0080] In particular, it is preferable that the heat residue ratio is in the above range in a cured product of a resin composition that contains a polyfunctional vinylbenzyl compound but does not contain other solid components.
[0081] In the present disclosure, the heat residue ratio of the cured product of the resin composition is determined by the following method: -1 ), temperature rise rate (10 ° C. min -1 The mass change can be determined by measuring the mass change when a cured product of the resin composition is heated to 800° C. under the conditions of (1) and (2). As the measuring device, for example, a TG / DTA device manufactured by Hitachi High-Tech Science Corporation can be used.
[0082] The sample pieces for measuring the heating residual amount are prepared by curing the resin composition to a C-stage state according to JIS K 6800 (1985). Specifically, the resin composition is semi-cured to a B-stage state, and the semi-cured product is crushed to prepare a resin powder. The resin powder is filled into a mold, subjected to vacuum heating and pressure molding at a temperature of 150°C, a pressure of 1.5 to 2.0 MPa, and a time of 120 minutes, and further subjected to heating and molding at a temperature of 180°C for 300 minutes to form a 1 mm-thick plate-shaped cured product.
[0083] The cured product of the resin composition preferably has a dielectric dissipation factor (Df) at 25°C and 10 GHz of 0.0020 or less, more preferably 0.0019 or less, and even more preferably 0.0017 or less. The lower the dielectric dissipation factor (Df) at 25°C and 10 GHz of the cured product of the resin composition, the better. There is no particular restriction on the lower limit, but taking into consideration the balance with other physical properties, it may be, for example, 0.0001 or more, 0.0005 or more, or 0.0010 or more. For example, the cured product of the resin composition preferably has a dielectric dissipation factor (Df) at a frequency of 10 GHz at a measurement temperature of 25°C of 0.0001 to 0.0020, 0.0005 to 0.0019, or 0.0010 to 0.0017.
[0084] The cured product of the resin composition preferably has a dielectric constant (Dk) at 25°C and 10 GHz of 4.0 or less, more preferably 3.0 or less, even more preferably 2.7 or less, and even more preferably 2.6 or less. The lower the dielectric constant (Dk) at 25°C and 10 GHz of the cured product of the resin composition, the better, and there is no particular restriction on the lower limit, but taking into consideration the balance with other physical properties, it may be, for example, 2.3 or more, or 2.4 or more. For example, the cured product of the resin composition preferably has a dielectric constant (Dk) at a measurement temperature of 25°C and a frequency of 10 GHz of 2.3 to 4.0, 2.3 to 3.0, 2.4 to 2.7, or 2.4 to 2.6.
[0085] In particular, it is preferable that the dielectric loss tangent (Df) and the relative dielectric constant (Dk) at 25°C and 10 GHz of a cured product of the resin composition containing the polyfunctional vinylbenzyl compound but not containing any other solid content are within the above ranges.
[0086] In the present disclosure, the dielectric loss tangent (Df) and the relative permittivity (Dk) are measured in the 10 GHz band at 25° C. in accordance with the cavity resonator perturbation method. The measurement device may be a “PNA Network Analyzer N5222B” (product name) from Agilent Technologies.
[0087] The sample pieces for measuring the dielectric loss tangent (Df) and the relative dielectric constant (Dk) were prepared by curing the resin composition to a C-stage state according to JIS K 6800 (1985). Specifically, the resin composition was semi-cured to a B-stage state, and the semi-cured product was crushed to prepare a resin powder. The resin powder was filled into a mold, subjected to vacuum heating and pressure molding at a temperature of 150°C, a pressure of 1.5 to 2.0 MPa, and a time of 120 minutes, and further subjected to heating and molding at a temperature of 180°C for 300 minutes to form a 1 mm-thick plate-shaped cured product.
[0088] "Prepreg" According to one embodiment, a prepreg formed using a resin composition and a fiber base material can be provided. Details of the resin composition are as described above.
[0089] Prepreg refers to a fiber substrate impregnated with a resin composition. In the prepreg, the resin composition may be in an uncured state, or may be partially or entirely semi-cured. For example, a molded product such as a laminate can be assembled using this prepreg, and then cured by heat treatment or the like to obtain a cured product.
[0090] Prepregs can be obtained, for example, by coating a fiber substrate with a resin composition and drying it. Alternatively, prepregs can be obtained by impregnating a fiber substrate with a resin composition and then drying the fiber substrate impregnated with the resin composition. Drying is preferably carried out at a temperature at which volatile components such as solvents that may be contained in the resin composition are removed or higher, and may be carried out at a temperature at which the resin composition contained in the resin composition is semi-cured or higher depending on the application. Furthermore, drying is preferably adjusted so that the resin composition is not completely cured. From this perspective, the drying temperature may be 80 to 200°C, and the drying time may be 1 to 30 minutes depending on the drying temperature, drying equipment, its scale, etc.
[0091] In the present disclosure, one index of a semi-cured product is the B-stage state according to JIS K 6800 (1985).
[0092] The fiber substrate may be any of woven fabric, knitted fabric, and nonwoven fabric. The fiber substrate may be provided in the form of chopped strand mat, roving, etc. The fiber material may be any of inorganic fiber and organic fiber. Examples of inorganic fibers include glass fiber and carbon fiber. Examples of glass fibers include E-glass, NE-glass, D-glass, S-glass, Q-glass, etc. Examples of organic fibers include polyimide, polyester, tetrafluoroethylene, etc. The fiber substrate may be a single fiber of these, or a blend of two or more types of fibers. From the viewpoints of dielectric properties and flame retardancy, the fiber substrate is preferably an inorganic fiber, and more preferably a glass fiber. Prepregs using inorganic fibers are also excellent in heat resistance and dimensional stability.
[0093] The fiber substrate may be selected appropriately depending on the application of the prepreg, but a sheet-like fiber substrate is preferred. Examples of the sheet-like fiber substrate include various sheet-like fiber substrates used in known laminates for electrical insulating materials. The thickness of the sheet-like fiber substrate is not particularly limited, but is preferably 0.02 to 0.5 mm, for example. Here, the thickness is measured at five points at equal distances across the entire surface of the sheet-like fiber substrate, and the arithmetic average value of the five measurements is used.
[0094] In the prepreg, the total mass of the thermosetting resin containing the polyfunctional vinylbenzyl compound and the thermoplastic resin may be 20 to 90 mass% or 30 to 80 mass% based on the total mass of the prepreg. Within these ranges, the resin impregnation coating of the fiber substrate in the prepreg can be more easily performed. Furthermore, the process of assembling the prepreg into a molded article and curing it can be more easily performed.
[0095] "Resin Film" According to one embodiment, a resin film formed using a resin composition can be provided. Details of the resin composition are as described above.
[0096] The term "resin film" refers to a resin composition formed into a film. In the resin film, the resin composition may be in an uncured state, or may be in a partially or entirely semi-cured state. A cured product can be obtained by curing the resin film by heat treatment or the like.
[0097] The resin film can be obtained, for example, by applying a resin composition to a substrate and drying it. Drying can be performed, for example, in the same manner as in the above-mentioned prepreg manufacturing method. After drying the resin film on the substrate, a product can be provided as a combination of the resin film and the substrate. For example, this method can provide a resin film to form an insulating layer or the like on the substrate in electronic devices, etc. In another method, after drying the resin film on the substrate, the resin film can be peeled off from the substrate and provided as a product.
[0098] The substrate to be coated may be either an inorganic substrate or an organic substrate, and examples thereof include glass substrates, metal substrates such as metal foils and metal plates, plastic substrates such as plastic plates and plastic films, and paper substrates. The substrate to be coated may be a fiber substrate as described above for the prepreg, or may be a prepreg. A substrate to be coated having a release layer formed on its surface may be used so that the resin film can be peeled off from the substrate.
[0099] "Metal-clad laminate" According to one embodiment, a metal-clad laminate formed using a prepreg and a metal foil can be provided. According to another embodiment, a metal-clad laminate including a cured resin layer and a metal foil can be provided. The cured resin layer may be a cured product of a resin composition or a cured product of a prepreg. Details of the resin composition and the prepreg are as described above.
[0100] The metal-clad laminate preferably includes a cured resin layer containing a cured resin and a metal foil formed on at least one side of the cured resin layer. The cured resin layer includes a cured product of a resin composition, but may also be the cured product of the prepreg described above. A more useful application involves forming a metal foil on at least one side of the cured prepreg, more preferably on both sides of the cured prepreg. The metal-clad laminate may be manufactured by forming a metal foil on at least one side of a single sheet-like prepreg, or by laminating two or more sheet-like prepregs and forming a metal foil on at least one of the outermost surfaces of the laminate. A more useful application involves laminating two or more sheet-like prepregs and forming a metal foil on both sides of the laminate. Specifically, the metal-clad laminate can be manufactured, for example, by placing a metal foil on one or both sides of a sheet-like prepreg and then hot-pressing and molding it. This hot-pressing and molding process causes the curing reaction of the sheet-like prepreg to proceed, resulting in a metal-clad laminate containing a cured prepreg. When hot-press molding is performed, only one prepreg may be used, or two or more prepregs may be laminated together. For hot-press molding, for example, an autoclave molding machine, a multi-stage press, a multi-stage vacuum press, a continuous molding machine, etc. The conditions for hot-press molding are not particularly limited, but can be, for example, a temperature of 100 to 300°C, a time of 10 to 300 minutes, and a pressure of 1.5 to 5 MPa.
[0101] The metal for the metal foil is not particularly limited, and examples thereof include copper, nickel, aluminum, gold, silver, platinum, molybdenum, ruthenium, tungsten, iron, titanium, chromium, and alloys containing two or more of these metal elements. Industrially, the metals copper, nickel, and aluminum are preferred. By using copper as the metal foil, a copper-clad laminate can be provided.
[0102] The dielectric properties of the cured resin in the assembled metal-clad laminate with the metal foil removed (also simply referred to as the dielectric properties of the metal-clad laminate) are preferably as follows: By using a resin composition containing a polyfunctional vinylbenzyl compound according to one embodiment, a metal-clad laminate with excellent dielectric properties can be provided.
[0103] The metal-clad laminate preferably has a dielectric loss tangent (Df) of 0.0001 to 0.0020, 0.0005 to 0.0019, or 0.0010 to 0.0017 at a frequency of 10 GHz at a measurement temperature of 25° C. The metal-clad laminate preferably has a relative dielectric constant (Dk) of 2.3 to 4.0, 2.3 to 3.0, 2.4 to 2.7, or 2.4 to 2.6 at a frequency of 10 GHz at a measurement temperature of 25° C. The dielectric loss tangent (Df) and relative dielectric constant (Dk) of the metal-clad laminate may be measured in accordance with the measurement of the dielectric loss tangent (Df) and relative dielectric constant (Dk) of the cured product of the resin composition described above.
[0104] "Printed Wiring Board" According to one embodiment, a printed wiring board including a cured product of the resin composition can be provided. Details of the resin composition are as described above.
[0105] In the printed wiring board, the cured product of the resin composition can be produced using a resin composition, a prepreg, a resin film, a metal-clad laminate, or a combination thereof. For example, a printed wiring board can be provided by using a metal-clad laminate containing a cured product of the resin composition as the substrate of the printed wiring board and forming a conductor circuit by a known method. Details of the prepreg, resin film, and metal-clad laminate are as described above. The printed wiring board may be either a single-layer printed wiring board or a multilayer printed wiring board.
[0106] "Semiconductor Package" According to one embodiment, a semiconductor package can be provided that includes a printed wiring board containing a cured resin product and a semiconductor element, wherein the cured resin product is a cured product of a resin composition. Details of the resin composition are as described above. Details of the cured product of the resin composition and the printed wiring board are also as described above. The semiconductor package can be manufactured, for example, by mounting a semiconductor element, a memory, etc. on a printed wiring board by a known method. The cured resin product may be used as an insulating material, a sealing material, etc. for the semiconductor package.
[0107] Examples of embodiments are listed below. The present invention is not limited to the following embodiments. <1> A polyfunctional vinylbenzyl compound obtained by reacting a compound having an aromatic fused ring, a compound having a biphenylene group, and a compound having a vinylbenzyl group.
[0108] <2> The polyfunctional vinylbenzyl compound according to <1>, wherein the compound having an aromatic fused ring includes indene.
[0109] <3> The polyfunctional vinylbenzyl compound according to <1> or <2>, wherein the compound having a biphenylene group includes 4,4'-bis(haloalkyl)biphenyl.
[0110] <4> The polyfunctional vinylbenzyl compound according to any one of <1> to <3>, wherein the compound having a vinylbenzyl group includes a vinylbenzyl halide.
[0111] <5> A polyfunctional vinylbenzyl compound comprising a unit having an aromatic fused ring and a unit having a biphenylene group, wherein the aromatic fused ring is bonded to two carbon atoms on the ring of the biphenylene group directly or via a linking group, and the linking group has a structure that is a divalent hydrocarbon group, and wherein the polyfunctional vinylbenzyl compound has a vinylbenzyl group that is bonded directly to a carbon atom on the ring of the aromatic fused ring.
[0112] <6> The polyfunctional vinylbenzyl compound according to <5>, wherein the unit having an aromatic fused ring has an indene ring, and the vinylbenzyl group is directly bonded to at least one carbon atom among the 1st, 2nd, and 3rd positions of the indene ring.
[0113] <7> A polyfunctional vinylbenzyl compound, which is a compound represented by the following formula (1):
[0114]
[0115] (In formula (1), R 1 are each independently a monovalent group having 1 to 30 carbon atoms or a hydrogen atom, 2 are each independently a monovalent group having 1 to 30 carbon atoms, a hydrogen atom, or a bonding position to another structure; each X is independently an alkylene group having 1 to 4 carbon atoms or a single bond; and n is an integer of 1 or greater.
[0116] <8> The polyfunctional vinylbenzyl compound according to <7>, which contains a partial structure represented by the following formula (2):
[0117]
[0118] (In formula (2), R 3 are each independently a monovalent group having 1 to 30 carbon atoms, a hydrogen atom, or a bonding position to another structure.
[0119] <9> A resin composition containing the polyfunctional vinylbenzyl compound according to any one of <1> to <8> above.
[0120] <10> The resin composition according to <9>, wherein the cured product of the resin composition has a heating residue ratio, expressed as the mass after heating at 800°C to the mass before heating, of 25 mass% or more.
[0121] <11> The resin composition according to <9> or <10>, wherein a cured product of the resin composition has a dielectric loss tangent of 0.0001 to 0.0020 at a frequency of 10 GHz when measured at a temperature of 25°C.
[0122] <12> A prepreg formed using a resin composition containing the polyfunctional vinylbenzyl compound according to any one of <1> to <8> above and a fiber substrate.
[0123] <13> A metal-clad laminate formed using the prepreg <12> and a metal foil.
[0124] <14> A resin film formed using a resin composition containing the polyfunctional vinylbenzyl compound according to any one of <1> to <8> above.
[0125] <15> A printed wiring board comprising a cured product of a resin composition containing the polyfunctional vinylbenzyl compound according to any one of <1> to <8> above.
[0126] <16> A semiconductor package comprising: a printed wiring board containing a cured resin; and a semiconductor element, wherein the cured resin is a cured resin composition containing the polyfunctional vinylbenzyl compound according to any one of <1> to <8>.
[0127] Specific examples of the present invention will be described below with reference to examples, but the present invention is not limited to the following examples.
[0128] "Method for measuring weight-average molecular weight (Mw)" The weight-average molecular weight (Mw) was measured by the following procedure. The weight-average molecular weight (Mw) was calculated by gel permeation chromatography (GPC) from a calibration curve using standard polystyrene. The calibration curve was approximated by a cubic equation using standard polystyrene: TSKstandard POLYSTYRENE (Types: A-500, A-2500, A-5000, F-2, F-2, F-4, F-40, F-128, F-288) [manufactured by Tosoh Corporation, trade name]. The GPC measurement conditions are shown below.
[0129] Apparatus: High-speed GPC apparatus HLC-8320GPC Detector: Ultraviolet absorption detector UV-8320 [manufactured by Tosoh Corporation] Column: Guard column: TSKgel guard column Super (HZ)-M + Column: TSKgel SuperMultipore HZ-M (2 columns), Reference column: TSKgel Super H-RC (2 columns) (all manufactured by Tosoh Corporation, trade names) Column size: 4.6 x 20 mm (guard column), 4.6 x 150 mm (column), 6.0 x 150 mm (reference column) Eluent: Tetrahydrofuran Sample concentration: 10 mg / 1 mL Injection volume: 2 μL Flow rate: 0.35 mL / min Measurement temperature: 40°C
[0130] "Preparation of polyfunctional vinylbenzyl compounds" (Production Examples 1 to 4) Table 1 shows the formulations of polyfunctional vinylbenzyl compounds. The blend amounts shown in the table are in parts by mass. A 500 mL reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet was charged with indene, 4,4'-bis(chloromethyl)biphenyl, chloromethylstyrene, a phase transfer catalyst, a polymerization inhibitor, pure water, and toluene as a solvent in the amounts shown in Table 1, and the mixture was heated and stirred at 40°C while blowing in nitrogen at a flow rate of 50 mL / min.
[0131] Next, a 48% by mass aqueous solution of sodium hydroxide (NaOH) (Kanto Chemical Co., Inc.) was added dropwise over 20 minutes as a basic compound in the amount shown in Table 1, and the mixture was stirred at 60°C for a further 9 hours. Nitrogen was continuously blown in during the reaction. The mixture was cooled to room temperature (25°C) and neutralized with a 10% aqueous hydrochloric acid solution, then washed three times with pure water, and the organic phase was precipitated in methanol to obtain polyfunctional vinylbenzyl compounds 1 to 4.
[0132] The chloromethylstyrene used was "CMS-P" (trade name: a mixture of m- and p-isomers, with an m-isomer content of approximately 50% by mass and a p-isomer content of approximately 50% by mass) manufactured by AGC Seimi Chemical Co., Ltd. The phase transfer catalyst used was tetra-n-butylammonium bromide (Kanto Chemical Co., Inc.). The polymerization inhibitor used was phenothiazine.
[0133] The weight average molecular weights (Mw) of the polyfunctional vinylbenzyl compounds 1 to 4 are shown in Table 1.
[0134]
[0135] Examples 1 to 4 The polyfunctional vinylbenzyl compounds 1 to 4 obtained in the Production Examples were each dissolved in toluene to obtain resin compositions of Examples 1 to 4 having a solid content concentration of about 60% by mass.
[0136] Comparative Examples 1 to 3 In Comparative Examples 1 to 3, the following compounds 1 to 3 were dissolved in toluene, respectively, to obtain resin compositions of Comparative Examples 1 to 3 having a solid concentration of about 60% by mass.
[0137] Compound 1: 1-ethenyl-4-[2-(4-ethenylphenyl)ethyl]benzene (Shandong Xingshun New Materials Co., Ltd.), Compound 2: Xylylene-type vinylbenzyl-modified resin (Nippon Kayaku Co., Ltd., trade name: STR-2000), Compound 3: Oligophenylene ether vinylbenzyl-modified resin (Mitsubishi Gas Chemical Co., Ltd., trade name: OPE-2St).
[0138] The structural formulae of compounds 1 to 3 are shown below.
[0139] Compound 1
[0140] Compound 2
[0141] Compound 3
[0142] "Preparation of Resin Plate" Each of the resin compositions obtained above was coated onto a 38 μm thick polyethylene terephthalate (PET) film (manufactured by Teijin Limited, product name: G2000) and dried by heating at 110°C for 5 minutes to prepare a B-stage resin film. This resin film was peeled off from the PET film and then pulverized to produce a resin powder. Note that, since Compound 1 is a powder, it was used as a resin powder without being heated, dried, or pulverized. Next, the resin powder was placed on a Teflon (registered trademark) sheet die-cut to a size of 1 mm thick x 50 mm long x 30 mm wide, and 18 μm thick low-profile copper foil (manufactured by Mitsui Mining & Smelting Co., Ltd., product name: SI-VSP) was placed on top and bottom of the sheet with its S-side (glossy side) in contact with the resin powder. The resin composition was then cured by vacuum heating and pressure molding at a temperature of 150°C, a pressure of 1.5 to 2.0 MPa, and a time of 120 minutes, followed by heat molding at a temperature of 180°C for 300 minutes. The copper foil on both sides was then removed to obtain a resin plate (thickness of the resin plate: 1 mm).
[0143] "Evaluation Method" The resin plates obtained above were subjected to the following evaluations. The results are shown in Table 2.
[0144] (Dielectric Loss Tangent (Df)) The resin plate obtained above was cut to prepare a 1 mm x 50 mm test piece. Next, the dielectric loss tangent (Df) of the test piece was measured in the 10 GHz band at an ambient temperature of 25°C according to the cavity resonator perturbation method. Measuring device: "PNA Network Analyzer N5222B" from Agilent Technologies.
[0145] (Heating Residue Amount Ratio) The resin plate obtained above was cut out to prepare a test piece. This test piece was heated under a nitrogen gas flow (100 ml min ) using a TG / DTA device. -1 ), temperature rise rate (10 ° C. min -1 The heating residue ratio (mass%) was calculated from the ratio of the mass of the test piece after heating to the mass of the test piece before heating. Measuring device: Hitachi High-Tech Science "TG / DTA7300"
[0146]
[0147] As shown in the table, Examples 1 to 4 all exhibit high flame retardancy due to the large ratio of the amount of heat residue, and exhibit excellent dielectric properties due to the low dielectric loss tangent (Df).
[0148] The disclosure of this application relates to the subject matter described in Japanese Patent Application No. 2023-074727, filed April 28, 2023, the entire disclosure of which is incorporated herein by reference. It should be noted that, in addition to what has already been described, various modifications and variations may be made to the above-described embodiments without departing from the novel and advantageous features of the present disclosure. Accordingly, all such modifications and variations are intended to be included within the scope of the appended claims.
Claims
1. A polyfunctional vinylbenzyl compound obtained by reacting a compound having an aromatic condensed ring, a compound having a biphenylene group, and a compound having a vinylbenzyl group.
2. The polyfunctional vinylbenzyl compound according to claim 1, wherein the compound having an aromatic condensed ring comprises indene.
3. The polyfunctional vinylbenzyl compound according to claim 1, wherein the compound having a biphenylene group includes 4,4'-bis(haloalkyl)biphenyl.
4. The polyfunctional vinylbenzyl compound according to claim 1, wherein the compound having a vinylbenzyl group includes a vinylbenzyl halide.
5. A polyfunctional vinylbenzyl compound comprising a unit having an aromatic fused ring and a unit having a biphenylene group, wherein the aromatic fused ring is bonded directly or via a linking group to each of two carbon atoms on the ring of the biphenylene group, and the linking group has a structure that is a divalent hydrocarbon group, and wherein the polyfunctional vinylbenzyl compound has a vinylbenzyl group bonded directly to a carbon atom on the ring of the aromatic fused ring.
6. The polyfunctional vinylbenzyl compound according to claim 5, wherein the unit having an aromatic fused ring has an indene ring, and the vinylbenzyl group is directly bonded to at least one carbon atom among the 1-, 2-, and 3-positions of the indene ring.
7. A polyfunctional vinylbenzyl compound represented by the following formula (1): (In formula (1), R 1 are each independently a monovalent group having 1 to 30 carbon atoms or a hydrogen atom; 2 are each independently a monovalent group having 1 to 30 carbon atoms, a hydrogen atom, or a bonding position to another structure; each X is independently an alkylene group having 1 to 4 carbon atoms or a single bond; and n is an integer of 1 or greater.
8. The polyfunctional vinylbenzyl compound according to claim 7, which contains a partial structure represented by the following formula (2): (In formula (2), R 3 are each independently a monovalent group having 1 to 30 carbon atoms, a hydrogen atom, or a bonding position to another structure.
9. A resin composition comprising the polyfunctional vinylbenzyl compound according to any one of claims 1 to 8.
10. A resin composition according to claim 9, wherein the cured product of the resin composition has a heating residue ratio, expressed as the mass after heating at 800°C relative to the mass before heating, of 25 mass% or more.
11. The resin composition according to claim 9, wherein a cured product of the resin composition has a dielectric loss tangent of 0.0001 to 0.0020 at a measurement temperature of 25° C. and a frequency of 10 GHz.
12. A prepreg formed using a resin composition containing the polyfunctional vinylbenzyl compound according to any one of claims 1 to 8 and a fiber substrate.
13. A metal-clad laminate formed using the prepreg according to claim 12 and a metal foil.
14. A resin film formed using a resin composition containing the polyfunctional vinylbenzyl compound according to any one of claims 1 to 8.
15. A printed wiring board comprising a cured product of a resin composition containing the polyfunctional vinylbenzyl compound according to any one of claims 1 to 8.
16. A semiconductor package comprising a printed wiring board containing a resin cured product and a semiconductor element, wherein the resin cured product is a cured product of a resin composition containing the polyfunctional vinylbenzyl compound described in any one of claims 1 to 8.
Citation Information
Patent Citations
Thermosetting resin composition, prepreg using the same, metal foil with resin, and board
JP2005325197A
Thermosetting resin composition and electronic part using the same
JP2007119531A
Organic light-emitting devices
JP2020537826A
Compound for organic electronic element, organic electronic element using the same, and an electronic device thereof
KR1020160035448A
Cited By
Resin, curable resin material, prepreg, resin film, metal-clad laminate, printed wiring board, and semiconductor package
WO2026126551A1
Resin, resin production method, curable resin material, prepreg, resin film, metal-clad laminate, printed wiring board, and semiconductor package
WO2026126848A1
Prepreg, metal-clad laminate, printed wiring board, and semiconductor package
WO2026126968A1
Curable composition, prepreg, metal-clad laminate, printed circuit board and semiconductor package
WO2026126995A1
Resin composition, prepreg, resin-equipped film, resin-equipped metal foil, metal-clad laminated sheet, and wiring board
WO2026205337A1