Nitride epitaxial structures and semiconductor devices
Patent Information
- Application Number
- JP2023519134
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-25
- Filing Date
- 2021-09-14
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2041-09-14
Smart Images

Figure 0007557056000009 
Figure 0007557056000010 
Figure 0007557056000012
Abstract
Description
[Technical field]
[0002] This application relates to the field of semiconductor technology, and in particular to nitride epitaxial structures and semiconductor devices. [Background technology]
[0003] Gallium nitride (GaN) materials have advantages such as large band gap and high mobility, and are therefore widely used in electronic power devices, radio frequency devices, and photoelectric devices. High electron mobility transistors (HEMTs) are the most widely used. Gallium nitride materials are usually obtained by epitaxial growth on silicon substrates. However, there is a large lattice mismatch and a thermal expansion coefficient mismatch of over 17% between GaN and silicon. Therefore, large stress is generated in silicon-based gallium nitride, which causes warping in epitaxy and affects the uniformity and reliability of GaN epitaxial wafers. In addition, as the size of the substrate increases, the impact of warping becomes more and more significant. Currently, in the prior art, the stress is mainly adjusted using graded AlGaN structures and superlattice structures. However, the graded AlGaN structure has the disadvantages of low dynamic performance and low crystal quality. Although the stress control ability and crystal quality of the superlattice structure are better than those of the graded AlGaN structure, it is difficult to balance the voltage endurance performance and crystal quality. Summary of the Invention [Means for solving the problem]
[0004] In view of this, the embodiments of the present application provide a nitride epitaxial structure and a semiconductor device. In order to effectively relieve and release the stress generated between the substrate and the epitaxial layer due to lattice mismatch and thermal mismatch, a buffer layer with a specific structure is disposed between the substrate and the epitaxial layer, which reduces the warpage during and after epitaxy, and improves the uniformity and reliability of the nitride epitaxial structure. Furthermore, the crystal quality and voltage endurance performance of the epitaxial layer can be improved, thereby effectively improving the performance of the semiconductor device.
[0005] in general The first aspect of the embodiment of the present application is A substrate; a nucleation layer formed on a substrate, the nucleation layer being an aluminum nitride layer or a gallium nitride layer; a buffer layer formed on the nucleation layer, the buffer layer comprising K stacked III-nitride bilayer structures, K≧3, each bilayer structure comprising a stacked upper layer and lower layer, a band gap of the upper layer material being larger than a band gap of the lower layer material, a band gap difference of each bilayer structure being the difference between the band gap of the upper layer material and the band gap of the lower layer material, the band gap differences of the K bilayer structures generally exhibiting a gradient trend along a thickness direction of the buffer layer; an epitaxial layer formed on the buffer layer, the material of the epitaxial layer comprising a Group III nitride; The present invention provides a nitride epitaxial structure comprising:
[0006] The nucleation layer can provide a nucleation center for the subsequent growth of the nitride epitaxial layer to alleviate the lattice mismatch between the substrate and the epitaxial layer, and can further effectively prevent the impurities brought by the substrate from affecting the subsequent growth of the nitride epitaxial layer, thereby improving the crystal quality of the epitaxial layer. In order to effectively alleviate and release the stress caused between the substrate and the epitaxial layer due to the lattice mismatch and thermal mismatch, a buffer layer is disposed between the substrate and the epitaxial layer, which reduces the warpage during and after epitaxy, and improves the uniformity and reliability of the nitride epitaxial structure. In addition, the buffer layer is disposed by stacking a plurality of III-nitride bilayer structures with graded band gap differences, which results in good dynamic performance, effectively balances the crystal quality and voltage resistance performance, and reduces the risk of leakage current, thereby effectively improving the performance of the semiconductor device. In addition, two-layer structures with different band gap differences are adaptively used in different locations, so that the advantages of filtering dislocations and improving voltage resistance performance can both be achieved, and the balance between the two aspects of performance can be achieved according to actual requirements. Dynamic performance usually refers to the recovery ability of a transistor after electrical stress is increased, and can be measured using an index such as Dron (dynamic resistance).
[0007] In one embodiment of the present application, in each bilayer structure, the upper layer material and the lower layer material are each selected from one of GaN, AlN, InN, or a combination thereof, ie, AlGaN, InGaN, InAlN, or InAlGaN. in general The material combinations of the upper and lower layers of the bilayer structure can be AlN / GaN, AlGaN / GaN, AlN / AlGaN, or AlGaN / AlGaN.
[0008] In one embodiment of the present application, the thickness of the underlayer is greater than twice the thickness of the overlayer. A thick underlayer and a thick overlayer are arranged, so that lattice relaxation can be effectively avoided. For heteroepitaxy, when the thickness of the overlayer is smaller, the material is in a strained state, specifically, after the material of the overlayer is stretched or compressed by the material of the underlayer, the lattice constant of the material of the overlayer becomes the same as that of the material of the underlayer, so that the superlattice can function effectively; or, when the thickness of the overlayer is larger, the material recovers to the lattice constant of the material, causing lattice relaxation.
[0009] In one embodiment of the present application, the band gap difference of the K bilayer structures gradually decreases from one side of the nucleation layer to one side of the epitaxial layer. When the band gap difference is large, the difference between the lattice constants of the materials of the bilayer structure is large, thereby helping to filter dislocations. However, the polarization effect is also strong, so leakage current is likely to occur. Conversely, when the band gap difference is small, this helps to reduce leakage current, but does not help to filter dislocations. The bilayer structure with a large band gap difference is placed closer to the nucleation layer, thereby helping to remove dislocations in the early stage of epitaxy and reducing the effect of leakage current. The bilayer structure with a small band gap difference is placed closer to the epitaxial layer, thereby helping to reduce leakage current and improve voltage endurance performance.
[0010] In one embodiment of the present application, the difference between the maximum band gap difference and the minimum band gap difference in the K bilayer structure is greater than 20% of the band gap difference between the III nitride with the maximum band gap and the III nitride with the minimum band gap constituting the bilayer structure. The difference between the maximum band gap difference and the minimum band gap difference of the K bilayer structures of the entire buffer layer is controlled within a suitable range, so that the crystal quality and the voltage resistance performance can be better balanced and adjusted.
[0011] In one embodiment of the present application, the K bilayer structures include two types of group III nitrides, i.e., GaN and AlN, and the average Al content in each bilayer structure is 5%-50%. The average Al content is the average molar percentage of Al element among the group III metal elements in each bilayer structure. The Al content in each bilayer structure is controlled within a suitable range to ensure that the buffer layer has good crystal quality.
[0012] In one embodiment of the present application, the average Al content in each two-layer structure is the same. The Al content remains unchanged. Therefore, when pre-compensation is designed for high temperature warpage, only the effect of the thickness of the membrane layer needs to be considered, and the effect of the change of the Al content does not need to be considered, thereby simplifying the parameter design.
[0013] In one embodiment of the present application, the average Al content of the K bilayer structures exhibits a gradient trend along the thickness direction of the buffer layer. The average Al content of the multiple bilayer structures is designed to be gradient, thereby facilitating stress tuning.
[0014] In one embodiment of the present application, in the K bilayer structures, any two adjacent bilayer structures may have different band gap differences, or some adjacent bilayer structures may have the same band gap difference. The repeat periodicity of the bilayer structures stacked adjacently and having the same band gap difference may be 1 to 10.
[0015] In one embodiment of the present application, the thickness of each bilayer is set to less than 100 nm to avoid relaxation.
[0016] In one embodiment of the present application, the material of the epitaxial layer includes one or more of GaN, AlN, InN, AlGaN, InGaN, InAlN, and InAlGaN.
[0017] In one embodiment of the present application, the thickness of the epitaxial layer is 300 nm or more. The thickness of a conventional gallium nitride epitaxial layer is usually small due to stress limitations. However, the nitride epitaxial wafer in the embodiment of the present application can fully remove stress, and therefore can have theoretically infinite thickness. In some embodiments of the present application, the thickness of the epitaxial layer can be 5 μm or more, or 10 μm or more.
[0018] In one embodiment of the present application, the substrate comprises a silicon substrate, a sapphire substrate, a silicon-on-insulator substrate (SOI substrate), a gallium nitride substrate, a gallium arsenide substrate, an indium phosphide substrate, an aluminum nitride substrate, a silicon carbide substrate, a quartz substrate, or a diamond substrate.
[0019] In one embodiment of the present application, the thickness of the nucleation layer is from 10 nm to 300 nm.
[0020] In one embodiment of the present application, the nitride epitaxial structure further includes a transition layer disposed between the nucleation layer and the epitaxial layer, and the material of the transition layer is AlGaN. In one embodiment of the present application, the material of the transition layer is the same as that of the nucleation layer. In one embodiment of the present application, the thickness of the transition layer is 10 nm to 300 nm.
[0021] In one embodiment of the present application, the nitride epitaxial structure further includes other functional layers disposed on the epitaxial layer. The other functional layers can be disposed according to the requirements of practical applications; in general , an AlN insertion layer, an AlGaN barrier layer, a P-type GaN layer, and the like.
[0022] According to a second aspect, an embodiment of the present application further provides a semiconductor device including the nitride epitaxial structure according to the first aspect of the embodiment of the present application, the semiconductor device being a power device, a radio frequency device, or a photovoltaic device. in general For example, the semiconductor device may be a field effect transistor, a light emitting diode, or a laser diode.
[0023] In the nitride epitaxial structure provided in the embodiment of the present application, a nucleation layer is disposed on the substrate, and a buffer layer is disposed on the nucleation layer, which effectively relieves and releases the stress generated between the substrate and the epitaxial layer due to lattice mismatch and thermal mismatch, reduces the warpage during and after epitaxy, improves the uniformity and reliability of the nitride epitaxial structure, and further improves the performance of the semiconductor device. Since the nitride epitaxial structure provided in the embodiment of the present application is used in the semiconductor device provided in the embodiment of the present application, a large-sized thick nitride epitaxial layer device can be obtained, which can effectively reduce the device cost and improve the device performance. [Brief description of the drawings]
[0024] [Figure 1] 1 is a schematic diagram of a nitride epitaxial structure according to one embodiment of the present application; [Diagram 2] FIG. 2 is a schematic diagram of a nitride epitaxial structure according to another embodiment of the present application. [Diagram 3] FIG. 2 is a schematic diagram of a nitride epitaxial structure according to yet another embodiment of the present application. [Figure 4] FIG. 2 is a schematic diagram of the structure of a buffer layer according to one embodiment of the present application. [Diagram 5] 1 is a schematic diagram of a nitride epitaxial structure according to one embodiment of the present application; [Figure 6] 1 is a flow chart of a process for fabricating a nitride epitaxial structure according to one embodiment of the present application. [Figure 7A] 11 is a TEM (Transmission Electron Microscope) graph of a two-layer structure of a buffer layer close to a substrate side in a nitride epitaxial structure according to embodiment 2. [Figure 7B]11 is an EDS (Energy Dispersive Spectroscopy) graph of a two-layer structure of a buffer layer close to a substrate side in a nitride epitaxial structure according to the second embodiment. [Figure 8A] 11 is a TEM graph of a two-layer structure of a buffer layer close to an epitaxial layer side in a nitride epitaxial structure according to the second embodiment. [Figure 8B] 11 is an EDS graph of a two-layer structure of a buffer layer close to an epitaxial layer side in a nitride epitaxial structure according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The following describes embodiments of the present application with reference to the accompanying drawings in the embodiments of the present application.
[0026] As shown in FIG. 1 and FIG. 2 , an embodiment of the present application provides a nitride epitaxial structure 100, including a substrate 10, a nucleation layer 20, a buffer layer 30, and an epitaxial layer 40. The nucleation layer 20 is an AlN layer or a GaN layer, and is formed on the substrate 10. The buffer layer 30 is formed on the nucleation layer 20. The epitaxial layer 40 is formed on the buffer layer 30. The material of the epitaxial layer 40 includes a group III nitride. The buffer layer 30 includes K stacked group III nitride bilayer structures 200, where K≧3. Each bilayer structure 300 includes an underlayer 30. 2 and the top 30 1 In order to generate a band gap difference, the upper layer 30 1 The band gap of the material is the lower 30 2 The band gap difference of each bilayer 300 is greater than the band gap of the material of the upper layer 30. 1 Band gap of the material and the lower layer 2is the difference between the band gaps of the materials of K and K. The band gap difference of the K bilayer structure generally shows a gradient trend along the thickness direction of the buffer layer 30. The nitride epitaxial structure provided in this embodiment of the present application has an epitaxial layer with good uniformity and high crystal quality, and can be used in semiconductor devices to improve device performance. The nitride epitaxial structure can have a nitride epitaxial layer with a large size of at least 6 inches and a thickness of at least 5 micrometers to meet the requirements of large epitaxial structures.
[0027] It should be noted that in this application, the terms "top" and "bottom" do not refer to any particular orientation when referring to the top and bottom layers of a bilayer structure. In the art, for superlattice bilayer structures, the layer with the larger bandgap is usually written as the top layer and the layer with the smaller bandgap as the bottom layer. This does not change if the two layers are swapped in order during actual growth.
[0028] In one embodiment of the present application, the substrate 10 may be a silicon substrate, a sapphire substrate, a silicon-on-insulator substrate (SOI substrate), a gallium nitride substrate, a gallium arsenide substrate, an indium phosphide substrate, an aluminum nitride substrate, a silicon carbide substrate, a quartz substrate, or a diamond substrate, or may be any known conventional substrate that can be used to fabricate a film of a group III nitride. The crystal orientation of the silicon substrate is not limited, for example, it may be a silicon substrate with a crystal facet index of (111), or it may be a silicon substrate with a crystal facet index of (100), or it may be a silicon substrate with another crystal facet index.
[0029] In one embodiment of the present application, the nucleation layer 20 is a layer of aluminum nitride or gallium nitride film, and the nucleation layer 20 completely covers the substrate 10. In order to reduce lattice defects, reduce dislocation density, and improve the crystal quality of the nitride epitaxial layer, the nucleation layer 20 can provide nucleation centers for the subsequent growth of the nitride epitaxial layer, relieve the stress caused by the lattice mismatch between the substrate 10 and the epitaxial layer 40, and more effectively prevent the impurities brought by the substrate 10 from affecting the subsequent growth of the nitride epitaxial layer. In addition, the nucleation layer 20 is thin and monocrystalline or quasi-monocrystalline. Therefore, the stress caused by the lattice mismatch between the substrate 10 and the epitaxial layer 40 can be relieved without affecting the crystal quality of the subsequent nitride epitaxial layer, and the cost can also be effectively controlled. In some embodiments of the present application, the thickness of the nucleation layer 20 can be 10 nm to 300 nm. In some other embodiments of the present application, the thickness of the nucleation layer 20 can be from 20 nm to 200 nm. Alternatively, in some other embodiments of the present application, the thickness of the nucleation layer 20 can be from 50 nm to 150 nm.
[0030] In one embodiment of the present application, the nucleation layer 20 can be fabricated by the method of metal-organic chemical vapor deposition or molecular beam epitaxy. Metal-organic chemical vapor deposition (MOCVD) is a chemical vapor deposition technique that uses the thermal decomposition reaction of organometallic compounds to grow films by vapor phase epitaxy. in general In order to grow a film of a group III-V or group II-VI compound on a substrate using a thermal decomposition reaction, an organic compound of a group III or group II element, a hydride of a group V or group VI element, etc. may be used as a source for crystal growth of a metal-organic compound. Nitride Epitaxial Layer The subsequent crystal quality can be improved.
[0031] In one embodiment of the present application, the buffer layer 30 includes K stacked III-nitride bilayer structures 300. In some embodiments, the value of K can be between 3 and 100. In some other embodiments, the value of K can be between 10 and 60. Alternatively, in some other embodiments, the value of K can be between 20 and 50. In each bilayer structure, the upper layer 30 1 Material and bottom layer 30 2 Each of the materials may be selected from one of GaN, AlN, InN, or combinations thereof, i.e., AlGaN, InGaN, InAlN, or InAlGaN. AlGaN is a combination of two III-nitrides, i.e., GaN and AlN. InGaN is a combination of two III-nitrides, i.e., GaN and InN. InAlN is a combination of two III-nitrides, i.e., AlN and InN. InAlGaN is a combination of three III-nitrides, i.e., GaN, AlN, and InN. The band gap of GaN is 3.4 eV, the band gap of AlN is 6.2 eV, and the band gap of InN is 0.7 eV. in general The material combinations of the upper and lower layers of the bilayer structure 300 can be AlN / GaN, AlGaN / GaN, AlN / AlGaN, or AlGaN / AlGaN.
[0032] In one embodiment of the present application, the thickness of the buffer layer 30 can be set based on the withstand voltage level. For example, when the withstand voltage level is 100V, the buffer layer should usually be arranged to be 2 μm to 3 μm, or when the withstand voltage level is 600V, the buffer layer should be arranged to be greater than 5 μm. In some embodiments of the present application, the thickness of the buffer layer 30 is greater than 300 nm. The thickness of each bilayer structure is less than 100 nm. in general The thickness of each bilayer structure may be between 10 nm and 80 nm, or between 20 nm and 60 nm. The appropriate thickness of the bilayer structure helps to avoid relaxation. In each bilayer structure 300, the lower layer 30 2 The thickness of the upper layer is 30 1The thickness of the K bilayer structure 300 is greater than twice the thickness of the K bilayer structure 300. A thick underlayer and a thick overlayer are arranged, so that lattice relaxation can be effectively avoided. For heteroepitaxy, when the thickness of the overlayer is smaller, the material is in a strained state, specifically, after the overlayer material is stretched or compressed by the underlayer material, the lattice constant of the overlayer material becomes the same as that of the underlayer material, so that the superlattice can function effectively; or when the thickness of the overlayer is larger, the material recovers to the lattice constant of the material, causing lattice relaxation. In the K bilayer structure 300, the thickness of all the overlayers may be the same, and the thickness of all the underlayers may be the same.
[0033] In some embodiments of the present application, the band gap difference of the K bilayer structures 300 gradually decreases from one side of the nucleation layer 200 to one side of the epitaxial layer 400. When the band gap difference is large, the difference between the lattice constants of the materials of the bilayer structure is large, thereby helping to filter dislocations. However, the polarization effect is also strong, so leakage current is likely to occur. Conversely, when the band gap difference is small, this helps to reduce leakage current, but does not help to filter dislocations. The bilayer structure with the large band gap difference is placed on the side closer to the nucleation layer, thereby helping to filter dislocations. In addition, since the bilayer structure is away from the AlGaN barrier layer and the channel layer, the adverse effects caused by leakage current are small. The bilayer structure with the small band gap difference is placed on the side closer to the epitaxial layer, thereby helping to reduce the polarization effect and improve the voltage endurance performance. Alternatively, in some other embodiments, the K bilayer structures 300 may be arranged in a manner such that the band gap difference gradually increases from one side of the nucleation layer 200 to one side of the epitaxial layer 400 according to requirements.
[0034] In one embodiment of the present application, the difference between the maximum band gap difference and the minimum band gap difference in the K bilayer structure is greater than 20% of the band gap difference between the group III nitride having the maximum band gap and the group III nitride having the minimum band gap, which constitute the bilayer structure. For example, in the K AlGaN / AlGaN bilayer structure, the group III nitrides constituting the bilayer structure include GaN and AlN, the band gap of GaN is 3.4 eV, and the band gap of AlN is 6.2 eV. In this case, 20% of the band gap difference between the group III nitride having the maximum band gap and the group III nitride having the minimum band gap, which constitute the bilayer structure, is 20%×(6.2−3.4) eV. As another example, in the K InAlGaN / InAlGaN bilayer structure, the group III nitrides constituting the bilayer structure include InN, GaN, and AlN, the band gap of InN is 0.7 eV, the band gap of GaN is 3.4 eV, and the band gap of AlN is 6.2 eV. In this case, 20% of the band gap difference between the group III nitride having the largest band gap and the group III nitride having the smallest band gap, which constitute the two-layer structure, is 20%×(6.2−0.7) eV.
[0035] In some embodiments of the present application, the K bilayer structures 200 include two types of III-nitrides, namely GaN and AlN, and the combination of the upper and lower layers of the bilayer structure is Al. x Ga 1-x N / A y Ga 1-y N(0<x≦1、y> 0). In the two-layer structure, the gradient of the band gap difference can be equivalent to the gradient of the Al content difference. The band gap change trend and the Al content in AlGaN Trend of change It is approximately linearly related to AlGaN. Specifically, the higher the Al content in AlGaN, the larger the band gap. Therefore, the slope trend of the band gap difference of the two-layer structure can be equivalent to the slope trend of the Al content difference of the two-layer structure. It should be noted that the Al content in this application is the mole percent of Al element in the group III metal elements. Alx Ga 1-x The band gap of N may be approximately equal to [6.2x+(1-x)3.4] eV. Thus, the Al component content in the upper and lower layers of each bilayer structure can be controlled to result in a gradient in the Al component content difference of the bilayer structure, and thus the band gap difference of the K bilayer structures can be gradient. For example, as shown in FIG. 2 and FIG. 3, K bilayer structures 200 include a first bilayer structure Al x1 Ga 1-x1 N / A y1 Ga 1-y1 N and the second two-layer structure Al x2 Ga 1-x2 N / A y2 Ga 1-y2 N and the third two-layer structure Al x3 Ga 1-x3 N / A y3 Ga 1-y3 N, ..., Kth two-layer structure Al xk Ga 1-xk N / A yk Ga 1-yk N. When the band gap difference gradually decreases from the first bi-layer structure to the Kth bi-layer structure, x1-y1>x2-y2>x3-y3>...>xk-yk, that is, the Al component content difference gradually decreases from the first bi-layer structure to the Kth bi-layer structure. In this embodiment, any two adjacent bi-layer structures have different band gap differences. in general , any two adjacent bilayer structures have different components. In some other embodiments of the present application, in the K bilayer structures, some adjacent bilayer structures may have the same band gap difference. The repeat periodicity of bilayer structures stacked adjacently and having the same band gap difference can be 1 to 10. The repeat periodicity of bilayer structures having different band gap differences can be the same or different. For example, as shown in FIG. 4, Al x Ga 1-x N / A y Ga 1-yIn the buffer layer composed of N, the repeating periodicity of the bilayer structures having different band gap differences is the same, that is, all 2. This can be as follows, that is, band gap difference of the first bilayer structure = band gap difference of the second bilayer structure > band gap difference of the third bilayer structure = band gap difference of the fourth bilayer structure ... > band gap difference of the Kth bilayer structure. The repeating periodicity of the bilayer structures having different band gap differences is different, for example, band gap difference of the first bilayer structure = band gap difference of the second bilayer structure = band gap difference of the third bilayer structure > band gap difference of the fourth bilayer structure = band gap difference of the fifth bilayer structure > band gap difference of the sixth bilayer structure ... > band gap difference of the Kth bilayer structure.
[0036] In one embodiment of the present application, the K bilayer structures include two types of group III nitrides, i.e., GaN and AlN, and the average Al content in each bilayer structure can be 5%-50%. In some embodiments, the average Al content in each bilayer structure is 8%-38%. In some other embodiments, the average Al content in each bilayer structure is 15%-30%. In some other embodiments, the average Al content in each group III nitride bilayer structure is 20%-25%. The average Al content is the average mole percent of Al element among the group III metal elements in each bilayer structure. The average Al content in each bilayer structure is controlled within a suitable range to ensure that the buffer layer has good crystal quality. Al x Ga 1-x N / A y Ga 1-y For the two-layer structure of N, the average Al content in each two-layer structure is [(T upper ×x+T lower ×y) / (T upper +T lower )] × 100%, T upper and T lowerdenotes the thickness of the upper layer and the lower layer of the bilayer structure, respectively, and x and y denote the Al content of the upper layer and the lower layer, respectively. In some embodiments of the present application, the average Al content in each bilayer structure is the same. The Al content remains unchanged. Therefore, when pre-compensation is designed for high temperature warpage, only the effect of the membrane layer thickness needs to be considered, and the effect of the change in the Al content does not need to be considered, thereby simplifying the parameter design. In some other embodiments of the present application, the average Al content of the K bilayer structures shows a gradient trend along the thickness direction of the buffer layer. The average Al content of the multiple bilayer structures is designed to be gradient, thereby facilitating stress tuning.
[0037] In addition, in the present application, the band gap difference of the K bilayer structures generally exhibiting a gradual trend along the thickness direction of the buffer layer may mean that the band gap difference strictly exhibits a gradually increasing or gradually decreasing change along the thickness direction of the buffer layer, or that the band gap difference generally exhibits a gradually increasing or gradually decreasing change, but there are a few special cases in which the change is opposite to the overall gradual trend, e.g., there are a few bilayer structures in which the band gap difference gradually decreases among the buffer layers in which the band gap difference generally gradually increases.
[0038] In one embodiment of the present application, the material of the epitaxial layer includes one or more of GaN, AlN, InN, AlGaN, InGaN, InAlN, and InAlGaN. In one embodiment of the present application, the material of the epitaxial layer 40 includes a III-nitride; in general, for example, one or more of GaN, AlN, InN, AlGaN, InGaN, InAlN, and InAlGaN. The thickness of the epitaxial layer 40 is 300 nm or more. The thickness of a conventional gallium nitride epitaxial layer is usually small due to stress limitations. However, the nitride epitaxial structure in this embodiment of the present application can fully remove stress, and thus is applicable to the fabrication of thick epitaxial layers, which can have theoretically infinite thickness. In some embodiments of the present application, the thickness of the epitaxial layer can be 5 μm or more, or 10 μm or more, for example, 15 μm to 100 μm. The epitaxial layer 40 can completely cover the nucleation layer 20, or can partially cover the nucleation layer 20.
[0039] In one embodiment of the present application, different nitride epitaxial layers are applicable to different semiconductor devices, for example, GaN, AlGaN, AlN are applicable to power devices, and In-containing nitride epitaxial layers are applicable to photovoltaic devices.
[0040] In this embodiment of the present application, other elements may alternatively be added to the epitaxial layer 40 to meet the serviceability requirements, for example, carbon may be added to improve the insulation properties, and carbon may be added to achieve high resistivity and improve voltage endurance performance.
[0041] 5, the nitride epitaxial structure 100 further includes a transition layer 50 disposed between the nucleation layer 30 and the epitaxial layer 40, which may be an AlGaN layer. The thickness of the transition layer may be between 10 nm and 300 nm. The transition layer 50 is disposed to help adjust the stress applied to the epitaxial structure.
[0042] In one embodiment of the present application, as shown in FIG. 5, the nitride epitaxial structure 100 further includes another functional layer 60 disposed on the epitaxial layer 40. The specific structural composition of the other functional layer 60 can be arranged according to the actual application requirements. In one embodiment of the present application, the other functional layer 60 includes an AlN insertion layer 61, an AlGaN barrier layer 62, and a P-type GaN layer 63, which are sequentially disposed on the epitaxial layer 40. general Alternatively, in some other embodiments, other functional layer 60 may have another structure.
[0043] As shown in FIG. 6, an embodiment of the present application further provides a method for fabricating a nitride epitaxial structure, including the following steps.
[0044] S01: A nucleation layer is formed on a substrate, the nucleation layer being an AlN layer or a GaN layer.
[0045] in general The nucleation layer 20 may be fabricated on the substrate 10 by the methods of metal organic chemical vapor deposition or molecular beam epitaxy. Prior to fabrication of the nucleation layer 20, the substrate 10 may be subjected to conventional cleaning.
[0046] In a specific embodiment of the present application, the nucleation layer 20 is fabricated on the substrate 10 by the method of metal organic chemical vapor deposition. The details may be as follows: to obtain the treated substrate 10, the substrate 10 is placed in a metal organic chemical vapor deposition reaction chamber, and hydrogen and ammonia are injected for 3 min to 5 min at a temperature of 900 ° C to 1100 ° C and a pressure of 30 to 60 Torr. Then, hydrogen, ammonia and an aluminum source or a gallium source are injected, and aluminum nitride or gallium nitride is deposited on the treated substrate 10 to obtain the nucleation layer 20. In this embodiment of the present application, the parameters in the deposition process are not limited to the aforementioned ranges. The gallium source includes, but is not limited to, trimethylgallium and triethylgallium. The aluminum source includes, but is not limited to, trimethylaluminum and triethylaluminum.
[0047] S02: A buffer layer is formed on the nucleation layer.
[0048] In one embodiment of the present application, the buffer layer 30 may be fabricated by a method of metal-organic chemical vapor deposition. in general , the substrate with the nucleation layer obtained in step S01 is placed in a metal organic chemical vapor deposition reaction chamber. Then, at a temperature of 900°C-1100°C and a pressure of 30-60 Torr, hydrogen, ammonia and a group III metal source are injected, and group III nitrides are obtained by epitaxial growth on the buffer layer 30 to obtain a buffer layer 30. The group III metal source is an organic compound containing a group III metal element, such as trimethylgallium, triethylgallium, trimethylaluminum, or triethylaluminum. To change the content of each group III nitride in the buffer layer, the flow of the group III metal source can be changed, and the deposition time can be controlled to obtain nitride layers of different thicknesses.
[0049] S03: To form an epitaxial layer, a group III nitride is epitaxially grown on the buffer layer.
[0050] In one embodiment of the present application, the epitaxial layer 40 may be fabricated by a method of metal-organic chemical vapor deposition. in general To obtain a processed substrate 10, the substrate 10 obtained in step S02 is placed in a metal organic chemical vapor deposition reaction chamber, and hydrogen and ammonia are injected for 3 min to 5 min at a temperature of 900°C to 1100°C and a pressure of 30 to 60 Torr. Then, hydrogen, ammonia and a group III metal source are injected, and a group III nitride is obtained by epitaxial growth on the buffer layer 30 to form an epitaxial layer 40. The group III nitride is in general The group III metal source may include one or more of the following: GaN, AlN, InN, AlGaN, InGaN, InAlN, and InAlGaN. The group III metal source may be an organic compound containing a group III metal element, such as trimethylgallium, triethylgallium, trimethylaluminum, or triethylaluminum.
[0051] In one embodiment of the present application, the fabrication method may further include a step of forming a transition layer 50 between the buffer layer 30 and the epitaxial layer 40. Specifically, before step S03, the transition layer 50 is first fabricated on the buffer layer 30, and then the epitaxial layer 40 is grown on the transition layer 50. The material of the transition layer 50 may be an AlGaN layer.
[0052] An embodiment of the present application further provides a semiconductor device including the aforementioned nitride epitaxial structure provided in the embodiment of the present application. The nitride epitaxial structure in the embodiment of the present application can be directly used as a part of a semiconductor device or can be used independently in a semiconductor device. The semiconductor device includes, but is not limited to, a power device (i.e., an electronic power device), a radio frequency device, or a photoelectric device. The power device or the radio frequency device can be a transistor, in general The photoelectric device may be, for example, a light emitting diode (LED) or a laser diode (LD), and the photoelectric device may be, for example, a field effect transistor, such as a high electron mobility transistor (HEMT). in general , a nitride-based light emitting diode, or a nitride-based quantum well laser diode.
[0053] The following further describes the embodiments of the present application using several embodiments.
[0054] EMBODIMENT 1 The nitride epitaxial structure includes a substrate, a nucleation layer, a buffer layer, an epitaxial layer, and other functional layers arranged in order on the substrate. The material of the substrate is Si, sapphire, GaN, SiC, diamond, SOI, etc. The nucleation layer is an AlN nucleation layer with a thickness of 50 nm to 400 nm. The buffer layer is a structural layer with a graded band gap difference, and the Al x Ga 1-xN / A y Ga 1-y The bilayer structure includes 11 bilayer structures having upper and lower layers of N. The average Al content of each bilayer structure is 20%. Table 1 shows the values of x and y in each bilayer structure, as well as the thickness T upper and T lower The epitaxial layer is a GaN layer, which may include carbon-doped structures such as GaN or AlGaN, with a thickness of 100 nm to 3 μm. The other functional layers may include the following layers arranged in order on the epitaxial layer: an AlN insertion layer with a thickness of 1 nm, an AlGaN barrier layer with an Al content range of 10% to 30% and a thickness of 10 nm to 30 nm, and a p-GaN layer, where the p-type impurity is implemented by Mg doping, with a thickness range of 30 nm to 120 nm.
[0055] [Table 1]
[0056] The bilayer structures with sequence numbers 1 to 11 are stacked and arranged in order. The bilayer structure with sequence number 1 is arranged near the epitaxial layer, and the bilayer structure with sequence number 11 is arranged near the nucleation layer. The periodicity 5 in Table 1 means that the bilayer structure with each sequence number is repeated 5 times. Specifically, the bilayer structures with different band gap differences have the same repeating periodicity to form 11 groups of bilayer structures, and each group includes five identical bilayer structures stacked. Specifically, the buffer layer is made up of five stacked Al 0.5 Ga 0.5 N / A 0.17 Ga 0.83 Two layers of N, five stacked Al 0.55 Ga 0.45 N / A 0.165 Ga 0.835N bilayer structure, etc. It can be learned from Table 1 that in the nitride epitaxial structure of embodiment 1, the Al component content difference of the bilayer structure of 11 groups of buffer layers gradually decreases from one side of the nucleation layer to one side of the epitaxial layer, that is, the band gap difference of the bilayer structure of 11 groups gradually decreases from one side of the nucleation layer to one side of the epitaxial layer. In addition, the average Al component content of each group of the bilayer structure of embodiment 1 is the same, which is 20%.
[0057] EMBODIMENT 2 The difference from the first embodiment is that the buffer layer is Al x Ga 1-x N / A y Ga 1-y The only difference is that the system includes 51 bilayer structures with N upper and lower layers. Table 2 lists the values of x and y in each bilayer structure, as well as the thickness T upper and the thickness of the lower layer T lower Shows.
[0058] [Table 2A] [Table 2B]
[0059] The bilayer structures with sequence numbers 1 to 51 are stacked and arranged in order. The bilayer structure with sequence number 1 is arranged near the epitaxial layer, and the bilayer structure with sequence number 51 is arranged near the nucleation layer. The periodicity 1 in Table 2 means that there is only one bilayer structure with each sequence number. It can be learned from Table 2 that in the nitride epitaxial structure of embodiment 2, the Al component content difference of the 51 bilayer structures of the buffer layer gradually decreases from one side of the nucleation layer to one side of the epitaxial layer, that is, the band gap difference of the 51 bilayer structures gradually decreases from one side of the nucleation layer to one side of the epitaxial layer. In addition, the average Al component content of each bilayer structure of embodiment 2 is the same, which is 20%. Compared with embodiment 1, the gradient interval between the band gap difference of the buffer layer of embodiment 2 is smaller, so that the stress between the substrate and the epitaxial layer can be better adjusted.
[0060] FIG. 7A is a TEM graph of a two-layer structure of a buffer layer close to the substrate side in a nitride epitaxial structure according to embodiment 2. FIG. 7B is an EDS graph of a two-layer structure of a buffer layer close to the substrate side in a nitride epitaxial structure according to embodiment 2. The two-layer structure in FIG. 7B corresponds to the three two-layer structures with sequence numbers 49 to 51 in Table 2. It can be learned from FIG. 7A and FIG. 7B that in the two-layer structure close to the substrate side, the Al component of the upper layer having a large band gap is close to 100%, and the Al component shows a tendency to gradually decrease toward the side away from the substrate. FIG. 8A is a TEM graph of a two-layer structure of a buffer layer close to the epitaxial layer side in a nitride epitaxial structure according to embodiment 2. FIG. 8B is an EDS graph of a two-layer structure of a buffer layer close to the epitaxial layer side in a nitride epitaxial structure according to embodiment 2. The two-layer structure in FIG. 8B corresponds to the three two-layer structures with sequence numbers 1 to 3 in Table 2. It can be learned from FIG. 7B and FIG. 8B that the Al content difference of the two-layer structure closer to the substrate side is larger than the Al content difference of the two-layer structure closer to the epitaxial layer side.
[0061] Note: The EDS graph contains curves for three elements, namely Ga, Al, and N. The N element accounts for about 50%. Therefore, the vertical coordinate value of each point on the curve for Al element multiplied by 2 is the Al content. Due to factors such as measurement error, the measured value may differ from the design value.
[0062] EMBODIMENT 3 The difference from the first embodiment is that the buffer layer is Al x Ga 1-x N / A y Ga 1-y The difference is that the bilayer structure includes 11 groups of bilayer structures with N upper and lower layers. Table 3 shows the values of x and y in each group of bilayer structures, as well as the thickness T upper and the thickness of the lower layer T lower Shows.
[0063] [Table 3]
[0064] The bilayer structures with sequence numbers 1 to 11 are stacked and arranged in order. The bilayer structure with sequence number 1 is arranged near the epitaxial layer, and the bilayer structure with sequence number 11 is arranged near the nucleation layer. The periodicity 5 in Table 1 means that the bilayer structure with each sequence number is repeated 5 times. Specifically, the bilayer structures with different band gap differences have the same repeating periodicity to form 11 groups of bilayer structures, and each group includes five identical bilayer structures stacked. In the nitride epitaxial structure of embodiment 3, the Al component content difference of the 11 groups of bilayer structures of the buffer layer gradually decreases from one side of the nucleation layer to one side of the epitaxial layer, i.e., 11 group It can be learned from Table 3 that the band gap difference of the two-layer structure of gradually decreases from one side of the nucleation layer to one side of the epitaxial layer. In addition, the average Al component content of the two-layer structure of 11 groups of embodiment 3 also gradually decreases from one side of the nucleation layer to one side of the epitaxial layer. [Explanation of symbols]
[0065] 10 Substrate 20 Nucleation layer 30 Buffer Layer 40 Epitaxial layer 50 Transition layer 60 Other functional layers 61 AlN insertion layer 62 AlGaN barrier layer 63 P-type GaN layer 100 Nitride epitaxial structure 300 (III-nitride) two-layer structure 301 Upper layer 302 Lower layer
Claims
1. A substrate; a nucleation layer formed on the substrate, the nucleation layer being an aluminum nitride layer or a gallium nitride layer; a buffer layer formed on the nucleation layer, the buffer layer comprising K stacked Group III nitride bilayer structures, K≧3, each bilayer structure comprising a stacked upper layer and lower layer, a bandgap of the material of the upper layer being larger than a bandgap of the material of the lower layer, a bandgap difference of each bilayer structure being the difference between the bandgap of the material of the upper layer and the bandgap of the material of the lower layer, the bandgap differences of the K bilayer structures exhibiting a graded trend along a thickness direction of the buffer layer; an epitaxial layer formed on the buffer layer, the material of the epitaxial layer comprising a Group III nitride; and Including, A nitride epitaxial structure, wherein the K bilayer structures include GaN and AlN, and the average Al content in each bilayer structure is between 5% and 50%.
2. 2. The nitride epitaxial structure of claim 1, wherein said material of said upper layer and said material of said lower layer are each selected from one of the following: GaN, AlN, InN, or combinations thereof.
3. The nitride epitaxial structure of claim 1 or 2, wherein the thickness of said underlayer is greater than twice the thickness of said overlayer.
4. 4. The nitride epitaxial structure of claim 1, wherein the band gap difference of the K bilayer structures gradually decreases from one side of the nucleation layer to one side of the epitaxial layer.
5. 5. The nitride epitaxial structure of claim 1, wherein the difference between the largest bandgap difference and the smallest bandgap difference in the K bilayer structures is greater than 20% of the bandgap difference between the largest and smallest bandgap group III nitrides constituting the bilayer structure.
6. The nitride epitaxial structure of claim 1 wherein the average Al content in each bilayer structure is the same.
7. The nitride epitaxial structure of claim 1 , wherein the average Al content of the K bilayer structures exhibits a graded trend along the thickness direction of the buffer layer.
8. 8. The nitride epitaxial structure of claim 1, wherein each bilayer structure has a thickness of less than 100 nm.
9. 9. The nitride epitaxial structure of claim 1, wherein the epitaxial layer material comprises one or more of GaN, AlN, InN, AlGaN, InGaN, InAlN and InAlGaN.
10. 10. The nitride epitaxial structure of claim 1, wherein the epitaxial layer has a thickness of 300 nm or more.
11. 11. The nitride epitaxial structure of claim 1, wherein the substrate comprises a silicon substrate, a sapphire substrate, a silicon-on-insulator substrate, a gallium nitride substrate, a gallium arsenide substrate, an indium phosphide substrate, an aluminum nitride substrate, a silicon carbide substrate, a quartz substrate, or a diamond substrate.
12. The nitride epitaxial structure of any one of claims 1 to 11, wherein the nucleation layer has a thickness of 10 nm to 300 nm.
13. A semiconductor device comprising the nitride epitaxial structure of any one of claims 1 to 12.
14. The semiconductor device of claim 13 , wherein the semiconductor device comprises a power device, a radio frequency device, or a photovoltaic device.
15. 15. The semiconductor device of claim 13 or 14, wherein the semiconductor device comprises a field effect transistor, a light emitting diode, or a laser diode.
Citation Information
Patent Citations
Group iii nitride epitaxial substrate and manufacturing method of the same
JP2014132607A
A semiconductor structure including a iii-v semiconductor layer having a hexagonal lattice crystal structure
JP2018503968A
LED Epitaxial Structure and Fabrication Method Thereof
US20150318448A1
Iii nitride epitaxial substrate and method of producing the same
US20150340230A1
Semiconductor structure having a group iii-v semiconductor layer comprising a hexagonal mesh crystalline structure