Internal oxidation start temperature estimation device, internal oxidation layer thickness estimation device, internal oxidation start temperature estimation method, and program
The internal oxidation start temperature estimation device accurately determines the thickness of internal oxidation layers in hot rolled steel sheets by calculating the internal oxidation start temperature based on Si, Mn, and Al concentrations, enhancing pickling process efficiency.
Patent Information
- Application Number
- JP2022560781
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-06
- Filing Date
- 2021-11-02
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2041-11-02
AI Technical Summary
Existing methods fail to accurately estimate the thickness of the internal oxidation layer in hot rolled steel sheets, which affects the efficiency of the pickling process due to the formation of excessive internal oxidation layers, particularly in high-tensile steel.
An internal oxidation start temperature estimation device and method that calculates the internal oxidation start temperature based on the concentrations of Si, Mn, and Al in the steel, using a cumulative temperature formula to accurately determine the thickness of the internal oxidation layer.
Enables precise estimation of the internal oxidation start temperature and layer thickness, improving the efficiency of the pickling process by optimizing winding completion temperatures and reducing processing time.
Smart Images

Figure 0007557146000010 
Figure 0007557146000012 
Figure 0007557146000017
Abstract
Description
[Technical field]
[0001] The present invention relates to an internal oxidation onset temperature estimation device, an internal oxidation layer thickness estimation device, an internal oxidation onset temperature estimation method, and a program. This application claims priority based on Japanese Patent Application No. 2020-185640, filed on November 6, 2020, the contents of which are incorporated herein by reference. [Background technology]
[0002] Hot-rolled steel sheets produced by hot rolling of a slab are often cooled after being wound into a coil. During this cooling process, an internal oxide layer is formed in the base steel portion directly below the scale layer. The internal oxide layer is a layer in which metal oxides are dispersed at the grain boundaries and within the grains. The metal oxides are mainly composed of oxides of elements less noble than iron (e.g., Si, Mn, Al, Cr, etc.). The scale layer is relatively easily removed by the pickling process after the cooling process, but the internal oxide layer is difficult to remove in the pickling process. For this reason, excessive generation of the internal oxide layer causes a problem of significantly slowing down the speed of the pickling process. This problem is particularly noticeable in steel materials that contain a large amount of elements less noble than iron, such as high-tensile steel (high-tensile steel), because the internal oxide layer is easily generated. Therefore, a method for controlling the appropriate thickness of the internal oxide layer is required. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2013-103235 [Patent Document 2] Japanese Patent Publication No. 9-256066 [Patent Document 3] Japanese Patent Publication No. 2005-281793 [Non-patent literature]
[0004] [Non-Patent Document 1] Kobayashi et al., "Improvement of cold rolling properties of hot-rolled steel sheets for cold rolling 980MPa super high-tensile strength steels", Tetsu-to-Haganen, Vol. 100 (2014), No. 5, P616-624 Summary of the Invention [Problem to be solved by the invention]
[0005] It is widely accepted that the thickness of the scale layer follows the so-called parabolic law, which states that the thickness of the scale layer is proportional to the square root of time. On the other hand, although Non-Patent Document 1 and Patent Document 1 provide information on the thickness of the internal oxide layer, these findings could not accurately estimate the thickness of the internal oxide layer.
[0006] Specifically, Non-Patent Document 1 discloses that there is a temperature at which the generation of the internal oxide layer substantially starts (in other words, the minimum temperature required for the internal oxide layer to grow, i.e., the internal oxidation onset temperature Tcr), and that the internal oxide layer is not formed in a temperature range below the internal oxidation onset temperature. In addition, the thickness of the internal oxide layer is considered to be proportional to time. However, as will be described in detail later, the thickness of the internal oxide layer is not simply proportional to time.
[0007] Patent Document 1 discloses Formula A, in which the thickness of the internal oxide layer is proportional to the square root of the time integral of the Aurhenius type growth rate. However, Formula A does not reflect the existence of the internal oxidation start temperature, and the integration is performed below that temperature down to room temperature, so there is a problem with the estimation accuracy.
[0008]
number
[0009] Patent Documents 2 and 3 disclose techniques for adjusting the coiling completion temperature of a hot-rolled steel sheet in accordance with the components of the hot-rolled steel sheet, taking into consideration the properties of the scale layer (adhesion, peeling resistance). However, the techniques disclosed in Patent Documents 2 and 3 do not control the thickness of the scale layer.
[0010] According to the description in Non-Patent Document 1, the internal oxidation layer is formed in a temperature range higher than the internal oxidation onset temperature. Therefore, in order to estimate the thickness of the internal oxidation layer with high accuracy, it is necessary to estimate the internal oxidation onset temperature with high accuracy.
[0011] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide an internal oxidation onset temperature estimation device, an internal oxidation layer thickness estimation device, an internal oxidation onset temperature estimation method, and a program capable of estimating the internal oxidation onset temperature with higher accuracy. [Means for solving the problem]
[0012] In order to solve the above problems, according to one aspect of the present invention, there is provided an internal oxidation start temperature estimation device that estimates an internal oxidation start temperature, which is the minimum temperature required for an internal oxidation layer to grow on the surface of a hot-rolled steel sheet containing easily oxidizable elements including at least one of Si, Mn, and Al, and is characterized in that the internal oxidation start temperature estimation device includes an internal oxidation start temperature estimation unit that estimates the internal oxidation start temperature based on the concentrations of Si, Mn, and Al contained in the hot-rolled steel sheet containing easily oxidizable elements.
[0013] Here, the internal oxide layer may be formed when the hot-rolled steel sheet containing an easily oxidizable element is cooled in a coiled state.
[0014] In addition, the internal oxidation start temperature estimation unit may determine the temperature at which an internal oxidation layer begins to form on the surface of the easily oxidizable element-containing hot-rolled steel sheet as the internal oxidation start temperature based on the actual measured value of the thickness of the internal oxidation layer formed on the easily oxidizable element-containing hot-rolled steel sheet.
[0015] Furthermore, the easily oxidizable element-containing hot rolled steel sheet is wound into a coil, and the internal oxidation start temperature estimation unit may generate a thickness-coiling temperature correlation graph showing a correspondence relationship between a coiling completion temperature, which is the temperature at the time when the coiling of the easily oxidizable element-containing hot rolled steel sheet is completed, and an actual measured value of the thickness of the internal oxidation layer, for each of a plurality of types of easily oxidizable element-containing hot rolled steel sheets differing in at least one of Si, Mn, and Al concentration, and may extrapolate the thickness-coiling temperature correlation graph to determine the coiling completion temperature at which the thickness of the internal oxidation layer becomes zero as the internal oxidation start temperature.
[0016] In addition, the internal oxidation start temperature estimation unit may determine the internal oxidation start temperature for each of multiple types of easily oxidizable element-containing hot-rolled steel sheets having different concentrations of at least one of Si, Mn, and Al, so that the correlation between the actual measured thickness of the internal oxidation layer and the cumulative temperature defined by the following formula (1) is maximized.
[0017]
number
[0018] In formula (1), S T is the cumulative temperature, T is the temperature of the portion of the hot-rolled steel sheet containing easily oxidizable elements that is the target of estimating the thickness of the internal oxide layer, Tcr is the internal oxidation start temperature, t0 is the estimation start point for starting to estimate the thickness of the internal oxide layer, and t1 is the estimation evaluation point. In the integral interval where T-Tcr is 0 or less, T-Tcr is set to 0.
[0019] In addition, the internal oxidation start temperature estimation unit may determine the internal oxidation start temperature for each of multiple types of easily oxidizable element-containing hot-rolled steel sheets having different concentrations of at least one of Si, Mn, and Al, so that the sum of squared deviations is minimized when a quadratic function of the cumulative temperature is fitted to the actual measured thickness of the internal oxidation layer.
[0020] According to another aspect of the present invention, there is provided an internal oxidation layer thickness estimation device, comprising an internal oxidation layer thickness estimation unit that estimates the thickness of an internal oxidation layer formed in a hot-rolled steel sheet containing an easily oxidizable element based on the internal oxidation start temperature estimated by the above-mentioned internal oxidation start temperature estimation device and the following formula (2). H = α × S T +H0(2) In formula (2), H is the thickness of the internal oxide layer, S T is the cumulative temperature, α is a proportionality constant, and H0 is the initial value of the thickness of the internal oxide layer.
[0021] According to another aspect of the present invention, there is provided an internal oxidation start temperature estimation method for estimating an internal oxidation start temperature, which is the minimum temperature required for an internal oxidation layer to grow on the surface of a hot-rolled steel sheet containing easily oxidizable elements including at least one of Si, Mn, and Al, the method comprising an internal oxidation start temperature estimation step of estimating the internal oxidation start temperature based on the concentrations of Si, Mn, and Al contained in the hot-rolled steel sheet containing easily oxidizable elements.
[0022] According to another aspect of the present invention, there is provided a program for causing a computer to estimate an internal oxidation start temperature, which is the minimum temperature required for an internal oxidation layer to grow on the surface of a hot-rolled steel sheet containing easily oxidizable elements including at least one of Si, Mn, and Al, characterized in that the program causes the computer to execute an internal oxidation start temperature estimation step of estimating the internal oxidation start temperature based on the concentrations of Si, Mn, and Al contained in the hot-rolled steel sheet containing easily oxidizable elements. Effect of the Invention
[0023] According to the above-mentioned aspect of the present invention, the internal oxidation start temperature, which is the minimum temperature required for an internal oxidation layer to grow on the surface of a hot-rolled steel sheet containing easily oxidizable elements including at least one of Si, Mn, and Al, is estimated based on the concentrations of Si, Mn, and Al contained in the hot-rolled steel sheet containing easily oxidizable elements, so that it is possible to estimate the internal oxidation start temperature with higher accuracy. [Brief description of the drawings]
[0024] [Figure 1] 1 is a thickness-coiling temperature correlation graph showing the correspondence relationship between the coiling completion temperature of a hot-rolled steel sheet and the measured thickness of an internal oxide layer for each composition of the hot-rolled steel sheet. [Diagram 2] 1 is a graph for explaining the correlation between the measured thickness of the internal oxide layer and the accumulated temperature. [Diagram 3] 1 is a graph showing that the correlation between the measured thickness of the internal oxidation layer and the cumulative temperature varies depending on the internal oxidation start temperature Tcr. [Figure 4] 1 is a graph showing the correlation between the holding time and the thickness of the internal oxide layer when the hot-rolled steel sheet is held at 600° C. for each composition of the hot-rolled steel sheet. [Diagram 5] 4 is a graph showing an example of the correlation between the measured thickness of the internal oxide layer and the formula (2) according to the present embodiment. [Figure 6] FIG. 2 is a functional block diagram showing the configuration of a processing device according to the present embodiment. [Figure 7] 4 is a flowchart showing a flow of processing by the processing device according to the present embodiment. [Figure 8] FIG. 2 is a hardware configuration diagram of the internal oxide layer thickness estimation device according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] A preferred embodiment of the present invention will be described in detail below with reference to the accompanying drawings. The present inventors have conducted extensive research into parameters that are highly correlated with the thickness of the internal oxidation layer in order to estimate the internal oxidation start temperature and, in turn, the thickness of the internal oxidation layer. As a result, the present inventors have found that the cumulative temperature described below has a very high correlation with the thickness of the internal oxidation layer. Furthermore, the present inventors have found that the internal oxidation start temperature, which affects the cumulative temperature, varies depending on the composition of the hot-rolled steel sheet, particularly the Si, Mn, and Al concentrations. The processing device according to this embodiment (a combination of an internal oxidation start temperature estimation device and an internal oxidation layer thickness estimation device) has been made based on these findings.
[0026] <1. Types of hot-rolled steel sheets> The hot-rolled steel sheet to be treated by the treatment device according to this embodiment (the internal oxidation start temperature and the thickness of the internal oxidation layer are estimated by this treatment device) is a hot-rolled steel sheet on which an internal oxidation layer can be formed. Specifically, it is an easily oxidized element-containing hot-rolled steel sheet containing at least one of Si, Mn, and Al, for example, Si is 0.2 mass% or more, Mn is 0.5 mass% or more, and Al is 0.01 mass% or more. Of course, the content of each element is not limited to this example. All elements are elements less noble than iron. That is, the "easily oxidized element" in this embodiment means an element that is "easier to oxidize (easily oxidized) than Fe". The easily oxidized element-containing hot-rolled steel sheet may further contain other elements, such as Cr. Examples of easily oxidized element-containing hot-rolled steel sheets include high-tensile steel (high-tensile steel). In particular, high-tensile steel is a preferred example for application of this embodiment because an internal oxidation layer is easily formed in the high-tensile steel. Hereinafter, unless otherwise specified, "hot-rolled steel sheet" refers to "easily oxidized element-containing hot-rolled steel sheet".
[0027] The thermal history of the hot-rolled steel sheet is not particularly limited. For example, after being wound into a coil, the hot-rolled steel sheet is cooled by any cooling method such as air cooling or water cooling (cooling process). In such a cooling process, an internal oxide layer is formed directly under the scale layer. In this case, the thermal history of the hot-rolled steel sheet follows a relatively simple cooling process. Of course, the thermal history of the hot-rolled steel sheet is not limited to this example. For example, the hot-rolled steel sheet may be cooled to a certain temperature in the cooling process after being wound into a coil, and then soaked or reheated for the purpose of annealing, etc. Furthermore, the hot-rolled steel sheet may be stretched into a flat plate and then subjected to the above-mentioned cooling, annealing, etc. Furthermore, the hot-rolled steel sheet may be cooled to a temperature equal to or lower than the internal oxidation start temperature Tcr described later, and then reheated to a temperature equal to or higher than the internal oxidation start temperature Tcr. In other words, in the calculation of the cumulative temperature described later, there may be an integral interval in which the temperature T of the estimation target portion is equal to or lower than Tcr. As will be described in detail later, in this integral interval, T-Tcr may be set to 0.
[0028] <2. Overall configuration of the processing device> FIG. 6 is a functional block diagram showing the overall configuration of the processing apparatus 10 according to this embodiment. The processing apparatus 10 has both functions of an internal oxidation start temperature estimation device and an internal oxidation layer thickness estimation device. That is, the processing apparatus 10 has an internal oxidation start temperature estimation unit 11 and an internal oxidation layer thickness estimation unit 12. Of course, these components may be built into separate device configurations. As shown in FIG. 8, the processing apparatus 10 includes a CPU 20, a ROM 21, a RAM 22, a hard disk 23, various input devices (keyboard, mouse, etc.) 24, and various output devices (display, etc.) 25 as a hardware configuration. The ROM stores programs and the like that cause the processing apparatus 10 to execute the internal oxidation start temperature estimation unit 11 and the internal oxidation layer thickness estimation unit 12. The CPU reads and executes the programs. The RAM serves as a working area for the CPU. An operator can input various information to the processing apparatus 10 using the input device. The processing apparatus 10 also outputs various information to the output device. Below, the processing performed by each component and the accumulated temperature, which is an important parameter in this embodiment, will be described.
[0029] <3. Processing performed by the internal oxidation start temperature estimation unit> As described above, the internal oxidation start temperature Tcr is the minimum temperature required for the internal oxidation layer to grow on the surface of the hot-rolled steel sheet. The inventors have found that the internal oxidation start temperature Tcr depends on the composition of the hot-rolled steel sheet, particularly on the Si, Mn, and Al concentrations. In this embodiment, the Si, Mn, and Al concentrations are mass% of each component with respect to the total mass of the base steel. The concentrations of these components may be measured by a general analysis method. For example, these components can be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Therefore, the Si, Mn, and Al concentrations in this embodiment are average concentrations with respect to the entire hot-rolled steel sheet. The internal oxidation start temperature estimation unit according to this embodiment estimates the internal oxidation start temperature Tcr based on the Si, Mn, and Al concentrations. If the internal oxidation start temperature Tcr can be estimated, the cumulative temperature can be calculated based on the internal oxidation start temperature Tcr, and the thickness of the internal oxidation layer can be estimated based on this cumulative temperature. Below, examples of methods for estimating the internal oxidation onset temperature Tcr will be explained, but any test can be performed offline.
[0030] (3-1. First estimation method) In the first estimation method, an operator prepares a plurality of types of hot-rolled steel sheets having at least one of Si, Mn, and Al concentrations, preferably different Si and Mn concentrations. A scale layer is formed on the surface of these hot-rolled steel sheets, and an internal oxide layer is not formed. For example, a hot-rolled steel sheet immediately after hot rolling (and before coiling) satisfies such a condition. If the hot-rolled steel sheet is left in this state, an unintended internal oxide layer may be formed. Therefore, it is preferable to rapidly cool the hot-rolled steel sheet (to a temperature at which an internal oxide layer is clearly not formed, for example, room temperature) immediately after hot rolling. The room temperature in this embodiment may be approximately 25°C ± 5°C. Rapid cooling may be performed by a method such as water cooling. The "rapid cooling" described below may also be performed by a similar method. This makes it possible to prepare a hot-rolled steel sheet without an internal oxide layer formed on the surface of the base steel sheet (base steel) (even if an internal oxide layer is formed, only a thin internal oxide layer that does not affect the test is formed). Next, the operator uses a heating device to heat these hot-rolled steel sheets under conditions that allow the formation of an internal oxidation layer. The temperature at which the internal oxidation layer starts to form on the surface of the hot-rolled steel sheet may be determined as the internal oxidation start temperature. The operator inputs the internal oxidation start temperature into the processing device. The internal oxidation start temperature estimation unit identifies the input temperature as the internal oxidation start temperature. In other words, the internal oxidation start temperature estimation unit determines the temperature at which the internal oxidation layer starts to form on the surface of the hot-rolled steel sheet as the internal oxidation start temperature based on the actual measured value of the thickness of the internal oxidation layer formed on the hot-rolled steel sheet.
[0031] Here, it is generally said that the internal oxide layer is formed in a state where a scale layer is formed and the steel sheet is isolated from the outside air (oxygen-containing atmosphere). For example, when a hot-rolled steel sheet wound into a coil (hereinafter, the hot-rolled steel sheet in such a state is also simply referred to as a "coil") is cooled, a scale layer is formed on each measurement target portion of the hot-rolled steel sheet and the measurement target portion is isolated from the outside air. Therefore, it is considered that the internal oxide layer is formed during the coil cooling process.
[0032] The isolation from the outside air can also be reproduced by, for example, placing the hot-rolled steel sheet on which the scale layer is formed in a non-oxidizing atmosphere. However, the internal oxide layer may not be formed simply by heating the hot-rolled steel sheet in a non-oxidizing gas atmosphere (for example, a nitrogen gas atmosphere). For example, a space may be generated between the scale layer and the base steel sheet due to the difference in contraction between them during cooling, and the internal oxide layer may not be formed. Conditions under which the internal oxide layer can be formed include, for example, conditions under which the hot-rolled steel sheet is heated in a non-oxidizing gas + water vapor atmosphere. In this case, the dew point may be within a range of, for example, about -20°C to +20°C.
[0033] The above operation actually results in the formation of an internal oxide layer, and the inventors believe that this is because the moisture that has entered the interface (space) between the scale layer and the base steel (base steel sheet) is reduced by Si, Mn, and Al in the base steel. In other words, it is believed that Si, Mn, and Al in the base steel are oxidized by oxygen in the moisture, and these oxides form the internal oxide layer. In addition, hydrogen (hydrogen gas) produced by the reduction of moisture reduces iron oxide in the scale layer to produce moisture. This moisture is reduced by Si, Mn, and Al in the base steel, and the formation of the internal oxide layer progresses.
[0034] Next, the worker heats the hot-rolled steel sheet at an arbitrary holding temperature for 1 hour. Next, the worker quenches the hot-rolled steel sheet to room temperature and measures the thickness of the internal oxide layer. For example, the hot-rolled steel sheet is cut parallel to the thickness direction, and the cut surface is etched with nital and then observed with a scanning electron microscope + energy dispersive X-ray analyzer (SEM-EDS) or the like. In the region where the internal oxide layer is formed, metal oxides present at the grain boundaries (grain boundary oxides) and metal oxides present within the grains (intragranular oxides) are observed. Therefore, the precipitates in the cross section are analyzed by EDS, and when at least one of Si, Mn, and Al is detected from the precipitates and O is also detected at the same time, the precipitates are determined to be metal oxides (grain boundary oxides). When metal oxides are observed at the grain boundaries and within the grains, such regions are determined to be internal oxide layers. Then, the distance from the surface of the base steel to the maximum depth of the internal oxide layer at each measurement point in the cross section (the number of measurement points is not limited, but may be set to about three points, for example) is measured, and the arithmetic average value of these distances is taken as the thickness of the internal oxide layer. The minimum holding temperature when the thickness of the internal oxide layer is formed to an average thickness of, for example, about 1 to 2 μm (i.e., the temperature at which the internal oxide layer begins to form on the surface of the hot-rolled steel sheet) may be taken as the internal oxidation start temperature. The temperature of the hot-rolled steel sheet may be measured using a thermocouple or the like. The temperature of the hot-rolled steel sheet here means the temperature of the base steel (base steel sheet) part immediately below the scale layer. If the hot-rolled steel sheet is thin (for example, about 2 to 5 mm) and the temperature of the estimation target part can be considered to be uniform in the thickness direction, the temperature of the hot-rolled steel sheet may be the temperature of any part in the thickness direction, or may be the temperature of the surface part of the base steel. When the temperature varies in the thickness direction, the temperature of the hot-rolled steel sheet is preferably the temperature of the surface of the base steel. From the viewpoint of measuring the thickness of the internal oxide layer as accurately as possible, it is preferable to heat the hot-rolled steel sheet to the holding temperature in as short a time as possible, and therefore the heating rate is preferably, for example, 10° C. / sec (=600° C. / min).
[0035] Another example of the condition that allows the internal oxide layer to be formed is a condition in which the scale layer and the base steel are pressure-bonded in a non-oxidizing atmosphere. This is based on the assumption that the hot-rolled steel sheet on which the scale layer is formed is wound into a coil. Even if a space is generated between the scale layer and the base steel sheet due to the difference in contraction between them during cooling, such a space can be removed and the scale layer and the base steel sheet can be tightly attached to each other. The pressure bonding method is not particularly limited, and for example, pressure bonding can be performed using a clamp or the like. The pressing force during pressure bonding is not particularly limited, but for example, when the clamp is tightened with a screw, the tightening torque value may be 25 N·m or more. In this state, the hot-rolled steel sheet is heated to an arbitrary holding temperature, and whether or not an internal oxide layer is formed is observed and judged. The specific observation and judgment methods are as described above.
[0036] Another example of the condition under which the internal oxide layer can be formed is a condition in which an iron oxide sample (e.g., Fe3O4 powder) is sandwiched between a plurality of hot-rolled steel sheets (each hot-rolled steel sheet has the same composition) from which the scale layer and the internal oxide layer have been removed by mechanical grinding or the like, and then pressed against each other. The method of pressing is not particularly limited, and for example, pressing may be performed using a clamp or the like. The pressing force during pressing is not particularly limited, but for example, when the clamp is tightened with a screw, the tightening torque value may be 25 N·m or more. In this state, the hot-rolled steel sheet is heated to an arbitrary holding temperature, and whether or not an internal oxide layer is formed is observed and judged. The specific observation method and judgment method are as described above. The data obtained by the above steps are summarized, for example, as shown in Table 1. That is, the operator inputs these data into the processing device 10. Although specific values are not given in Table 1, as described later, if the composition of the hot-rolled steel sheet (particularly the concentration of at least one of Si, Mn, and Al) is different, the internal oxidation start temperature is also different.
[0037] [Table 1]
[0038] Next, the internal oxidation start temperature estimation unit 11 obtains a regression equation using the internal oxidation start temperature obtained above as the objective variable and at least one of the Si, Mn, and Al concentrations of the hot-rolled steel sheet as the explanatory variable. For example, the regression equation is obtained by performing multiple regression analysis on the data summarized in Table 1. The regression equation shows the correlation between at least one of the Si, Mn, and Al concentrations of the hot-rolled steel sheet and the estimated value of the internal oxidation start temperature. The regression equation may include at least one of the Si, Mn, and Al concentrations as variables, but it is preferable that the Si concentration and the Mn concentration among these concentrations are included as variables, and it is more preferable that all concentrations are included as variables. Furthermore, it is preferable to replace at least one of the Si concentration and the Mn concentration in the regression equation with the Si / Mn concentration ratio. An example of the regression equation is as follows. Tcr(℃)=s0+s1×(%Si)+s2×(%Mn)+s3×(%Al) (A) Tcr(℃)=s0+s1×(%Si) / (%Mn)+s2×(%Mn)+s3×(%Al) (B) Tcr(℃)=s0+s1×(%Si)+s2×(%Mn) (C) Tcr(℃)=s0+s1×(%Si) / (%Mn)+s2×(%Mn) (D) In the regression equations (A) to (D), s0 to s3 are regression constants determined by regression analysis, and the element symbols indicate the mass percentage of each element.
[0039] Next, the internal oxidation start temperature estimation unit 11 determines the internal oxidation start temperature Tcr based on the regression equation obtained above. Specifically, an operator measures the Si concentration, Mn concentration, and Al concentration of a hot-rolled steel sheet to be actually manufactured, and inputs these concentrations into the processing device 10. Next, the internal oxidation start temperature estimation unit 11 determines the internal oxidation start temperature Tcr by substituting the input values into the regression equation obtained above. (3-2. Second estimation method) In the second estimation method, the hot-rolled steel sheet is wound into a coil shape, and a thickness-coiling temperature correlation graph is generated for each of a plurality of types of hot-rolled steel sheets having different concentrations of at least one of Si, Mn, and Al, preferably different concentrations of Si and Mn, which shows a correlation between a coiling completion temperature, which is a temperature at the time when the coiling of the hot-rolled steel sheet is completed, and an actual measured value of the thickness of the internal oxide layer.
[0040] Specifically, the worker arbitrarily changes the coiling completion temperature of the hot-rolled steel sheet and cools it to room temperature. Next, the worker measures the thickness of the internal oxide layer for each coiling completion temperature. There are no particular limitations on the location for measuring the coiling completion temperature and the thickness of the internal oxide layer, but it is preferable to measure it at the center (center part) in the sheet width direction of the hot-rolled steel sheet. As will be described in detail later, the internal oxide layer formed in this part tends to be particularly thick and shows a high correlation with the accumulated temperature. The coiling completion temperature may be actually measured using a thermocouple or a radiation thermometer installed immediately before the down coiler, or may be derived by a simulation (heat conduction calculation) such as that typified by Non-Patent Document 1. When the coiling completion temperature is actually measured using a thermocouple, it is sufficient to measure the temperature of the base steel (base steel sheet) part immediately below the scale layer. If the hot-rolled steel sheet is thin (for example, about 2 to 5 mm) and the temperature of the part where the coiling completion temperature is measured can be considered to be uniform in the sheet thickness direction, the coiling completion temperature may be the temperature of any part in the sheet thickness direction or the temperature of the surface part of the base steel. When the temperature varies in the thickness direction, the coiling completion temperature is preferably the temperature of the surface of the base steel. When a radiation thermometer is used, the measurement value of the radiation thermometer can be taken as the coiling completion temperature as is. The method for measuring the thickness of the internal oxide layer is as described above, but the measurement location may be, for example, the center part located 100 m from the tip of the coil (the end wound most inwardly).
[0041] Next, the operator inputs the multiple measurement points obtained by the above process into the processing device 10. The internal oxidation start temperature estimation unit 11 generates a thickness-coiling temperature correlation graph from the input measurement points. An example of the thickness-coiling temperature correlation graph is shown in FIG. 1. The horizontal axis of FIG. 1 indicates the coiling completion temperature (°C), and the vertical axis indicates the actual measured value of the thickness of the internal oxide layer (μm). Point P10 indicates the coiling completion temperature and the actual measured value of the thickness of the internal oxide layer of a hot-rolled steel sheet containing 0.5 mass% Si, 2.3 mass% Mn, and 0.18 mass% Al. Graph L10 is a thickness-coiling temperature correlation graph corresponding to point P10, and is obtained by performing regression analysis on point P10. In the example of FIG. 1, regression is performed with a quadratic function. The same applies to graphs L11 and L12 described below.
[0042] Point P11 indicates the actual measured values of the coiling completion temperature and the thickness of the internal oxide layer of a hot-rolled steel sheet containing 0.6 mass% Si, 2.0 mass% Mn, and 0.03 mass% Al. Graph L11 is a thickness-coiling temperature correlation graph corresponding to point P11, and is obtained by performing regression analysis on point P11.
[0043] Point P12 indicates the actual measured values of the coiling completion temperature and the thickness of the internal oxide layer of a hot-rolled steel sheet containing 1.0 mass% Si, 2.3 mass% Mn, and 0.02 mass% Al. Graph L12 is a thickness-coiling temperature correlation graph corresponding to point P12, and is obtained by performing regression analysis on point P12.
[0044] As is clear from Fig. 1, even if the coiling end temperature is the same, the thickness of the internal oxidation layer differs if the composition of the hot-rolled steel sheet is different. In the second estimation method, the internal oxidation start temperature estimation unit 11 extrapolates the thickness-coiling temperature correlation graph to obtain the coiling end temperature at which the thickness of the internal oxidation layer becomes zero as the internal oxidation start temperature. In the example of Fig. 1, the internal oxidation start temperature Tcr of the hot-rolled steel sheet with Si: 1.0 mass%, Mn: 2.3 mass%, and Al: 0.02 mass% was the lowest at 461°C, the internal oxidation start temperature Tcr of the hot-rolled steel sheet with Si: 0.5 mass%, Mn: 2.3 mass%, and Al: 0.18 mass% was the second lowest at 467°C, and the internal oxidation start temperature Tcr of the hot-rolled steel sheet with Si: 0.6 mass%, Mn: 2.0 mass%, and Al: 0.03 mass% was the highest at 481°C. As described above, it is found that the internal oxidation start temperature Tcr differs when the composition of the hot-rolled steel sheet (particularly at least one of the concentrations of Si, Mn, and Al) differs. The internal oxidation start temperature estimation unit 11 summarizes the data obtained by the above steps, for example, as shown in Table 1.
[0045] Note that the coiling test performed in the second estimation method is basically performed using an actual machine, but the test given as the second example of the first estimation method (a test in which the scale layer and the base steel are pressure-bonded in a non-oxidizing atmosphere) may be used instead. In this case, the operator regards the holding temperature as the coiling completion temperature and measures the thickness of the internal oxidation layer for a plurality of holding temperatures. Next, the internal oxidation start temperature estimation unit 11 generates a thickness-coiling temperature correlation graph in the same manner as above. Next, the internal oxidation start temperature estimation unit 11 extrapolates the thickness-coiling temperature correlation graph to determine the coiling completion temperature at which the thickness of the internal oxidation layer becomes zero as the internal oxidation start temperature.
[0046] Next, the internal oxidation start temperature estimation unit 11 obtains a regression equation using the internal oxidation start temperature obtained above as a response variable and at least one of the Si, Mn, and Al concentrations of the hot-rolled steel sheet as an explanatory variable. The method for obtaining the regression equation is as described above, and for example, regression equations (A) to (D) can be obtained.
[0047] Next, the internal oxidation start temperature estimation unit 11 determines the internal oxidation start temperature Tcr based on the regression equation obtained above. Specifically, an operator measures the Si concentration, Mn concentration, and Al concentration of a hot-rolled steel sheet to be actually manufactured, and inputs these concentrations into the processing device 10. Next, the internal oxidation start temperature estimation unit 11 determines the internal oxidation start temperature Tcr by substituting the input values into the regression equation obtained above.
[0048] (3-3. Third estimation method) The third estimation method is to determine the internal oxidation start temperature Tcr, which is the objective variable, so that the correlation between the actual value of the thickness of the internal oxide layer and the cumulative temperature is maximized when the internal oxidation start temperature Tcr is varied as a variable parameter. As described above, the cumulative temperature is a parameter that has a very high correlation with the thickness of the internal oxide layer. First, the cumulative temperature will be described.
[0049] (3-3-1. Cumulative temperature) The accumulated temperature is expressed by the following equation (1).
[0050]
number
[0051] In formula (1), S T is the accumulated temperature and S T ≧0. T is the temperature of the portion of the hot-rolled steel sheet that is the target of estimating the thickness of the internal oxide layer, Tcr is the internal oxidation start temperature, t0 is the estimation start time when estimation of the thickness of the internal oxide layer begins, and t1 is the estimation evaluation time. In the integral interval where T-Tcr is 0 or less, T-Tcr is set to 0. That is, the thickness of the internal oxide layer is estimated, for example, by the following formula (2), which will be described in detail later. H = α × S T +H0(2)
[0052] In equation (2), H is the thickness of the internal oxide layer (estimated value), α is a proportionality constant, and S Tis the cumulative temperature, and H0 is the initial value of the thickness of the internal oxide layer. Therefore, it can be said that formula (2) shows the correlation between the cumulative temperature and the estimated value of the thickness of the internal oxide layer. As will be described in detail later, the cumulative temperature has a very high correlation with the thickness of the internal oxide layer, so the thickness of the internal oxide layer can be estimated with high accuracy.
[0053] Therefore, the accumulated temperature is a very important parameter in this embodiment. The accumulated temperature is expressed by the above-mentioned formula (1). Therefore, each parameter constituting the accumulated temperature will be described in detail.
[0054] T is the temperature of the estimation target portion of the hot-rolled steel sheet, which is the target for estimating the thickness of the internal oxidation layer. Here, since a scale layer is formed on the hot-rolled steel sheet, the "temperature of the estimation target portion" here means the temperature of the base steel (base steel sheet) portion immediately below the scale layer. If the hot-rolled steel sheet is thin (for example, about 2 to 5 mm) and the temperature of the estimation target portion can be considered to be uniform in the thickness direction, the temperature of the estimation target portion may be the temperature of any portion in the thickness direction, or may be the temperature of the surface portion of the base steel. If the temperature varies in the thickness direction, it is preferable that the temperature of the estimation target portion is the surface temperature of the base steel. The temperature of the estimation target portion may be actually measured using a thermocouple or the like (in this case, the operator only needs to input the output value of the thermocouple to the processing device 10. The internal oxidation start temperature estimation unit 11 identifies the input temperature as the temperature of the estimation target portion), or may be derived by a simulation (heat conduction calculation) as typified by, for example, Non-Patent Document 1 (in this case, the internal oxidation start temperature estimation unit 11 only needs to perform the simulation). In this simulation, the thermal history of the hot-rolled steel sheet described above is taken into consideration.
[0055] Tcr is the internal oxidation start temperature (as will be described later, in this estimation method, the internal oxidation start temperature is first set to an arbitrary value). Therefore, the cumulative temperature is a value obtained by integrating the difference between the temperature T of the estimation target part and the internal oxidation start temperature Tcr with respect to time. In this embodiment, it is considered that an internal oxidation layer is formed (or grows) when the temperature of the estimation target part exceeds the internal oxidation start temperature Tcr. In other words, when the temperature of the estimation target part is equal to or lower than the internal oxidation start temperature Tcr, the internal oxidation layer is not formed (if the internal oxidation layer has already formed, its growth stops). The internal oxidation start temperature Tcr is a constant specific to the steel type. Therefore, an appropriate internal oxidation start temperature Tcr is assigned to the steel material to which the present invention is applied. A specific method of assigning the temperature will be described later.
[0056] t0 is the estimation start time point at which estimation of the thickness of the internal oxide layer is started. The estimation start time point is set to any time point during the process in which the internal oxide layer is assumed to be formed. As described above, it is generally said that the internal oxide layer is formed in a state in which a scale layer is formed and is isolated from the outside air (oxygen-containing atmosphere). For example, when cooling a hot-rolled steel sheet (i.e., a coil) wound into a coil, a scale layer is formed on each measurement target portion in the hot-rolled steel sheet, and the measurement target portion is isolated from the outside air. Therefore, it is considered that the internal oxide layer is formed in the coil cooling process. The coil cooling process starts from the completion of winding the hot-rolled steel sheet. Therefore, the estimation start time point t0 may be the completion of winding the hot-rolled steel sheet. Of course, the estimation start time point t0 may be set to any time point during the cooling process, and when annealing or the like is performed during the cooling process, the estimation start time point t0 may be set to the time period during which annealing or the like is performed. For example, the estimation start time t0 may be the start time of annealing (the time when the estimation target part of the hot-rolled steel sheet reaches the entrance of the annealing furnace), or may be the midway point of annealing. As described above, in the cooling process, an integral interval may exist in which the temperature T of the estimation target part is lower than the internal oxidation start temperature Tcr. In this case, for example, the estimation target part is cooled to the internal oxidation start temperature Tcr or lower in the middle of the cooling process, and the estimation target part is reheated to the internal oxidation start temperature Tcr or higher by the above-mentioned annealing.
[0057] t1 is the estimated evaluation time point. Therefore, it can be said that the internal oxide layer thickness estimating unit 12 according to the present embodiment estimates the thickness of the internal oxide layer at the estimated evaluation time point t1. The estimated evaluation time point t1 is set to a time point after the estimation start time point t0. For example, any time point during the coil cooling process may be the estimated evaluation time point t1. More specifically, when annealing or the like is performed during the coil cooling process, the annealing end time point (the time point when the estimation target part of the hot-rolled steel sheet reaches the outlet of the annealing furnace) may be the estimated evaluation time point t1, or a time point in the middle of the annealing may be the estimated evaluation time point t1. Furthermore, any time point during the cooling process after the annealing end may be the estimated evaluation time point t1. In this case, the time point when the temperature T of the estimation target part finally reaches the internal oxidation start temperature Tcr in the coil cooling process (after all the above-mentioned annealing or the like is performed) may be the estimated evaluation time point t1. A subsequent time point (i.e., the time point when the temperature T of the estimation target part is further cooled) may be the estimated evaluation time point t1. As described above, in the integral interval after the temperature T of the estimation target portion reaches the internal oxidation start temperature Tcr, T-Tcr becomes 0 or less. However, since T-Tcr is set to 0 in this integral interval, the estimation accuracy is not affected.
[0058] In calculating the cumulative temperature, the temperature T of the measurement target portion may be actually measured, or may be calculated by a simulation that takes into account the thermal history of the hot-rolled steel sheet. In the former case, the operator may input the actual measured value to the processing device 10, and in the latter case, the internal oxidation start temperature estimation unit 11 may perform a simulation. Although details will be described later, in calculating the cumulative temperature, the internal oxidation start temperature Tcr is first set to an arbitrary value. If T-Tcr is 0 or less in any integral interval, T-Tcr is set to 0 in that integral interval. In addition, the integral operation may be performed by dividing the integral interval (t0 to t1) into minute intervals Δt and calculating the cumulative temperature by summing up the discrete values of the cumulative temperature in each Δt interval. The operator may input t0 and t1 to the processing device 10. The internal oxidation start temperature estimation unit 11 identifies the inputted value as t0 and t1 in formula (1). Alternatively, t0 and t1 may be set in advance as specified values.
[0059] In the third estimation method, the internal oxidation start temperature estimation unit 11 estimates the internal oxidation start temperature Tcr using such a cumulative temperature. First, the internal oxidation start temperature estimation unit 11 sets the internal oxidation start temperature Tcr to an arbitrary value (for example, an arbitrary value within the range of 200 to 1000 ° C). Next, measurement target portions are set at a plurality of positions on the surface of the hot-rolled steel sheet, and the cumulative temperatures of these measurement target portions are calculated based on the above-mentioned mathematical formula (1). The measurement target portions may be set by the internal oxidation start temperature estimation unit 11 or by an operator. In the former case, the internal oxidation start temperature estimation unit 11 may display the measurement target portions on a display or the like. In the latter case, the operator may input the measurement target portions into the processing device 10. The measurement target portions may be set for the entire length in the rolling direction and the entire width in the sheet width direction of the hot-rolled steel sheet, or may be set for a part of the entire length and the entire width. In the example described below, the measurement target portions are set for the entire length and the entire width. In addition, it is preferable that the measurement target portions are set at the sheet width center and quarter portions. As described later, the accumulated temperature in the widthwise center and quarter sections has a high correlation with the measured thickness of the internal oxide layer. Here, the widthwise center and quarter sections refer to the region within the range from the center (center) of the hot-rolled steel sheet in the width direction to the quarter sections that are 1 / 4 of the sheet width away from both ends in the width direction (i.e., the region between the quarter sections at one end and the quarter sections at the other end in the width direction).
[0060] Meanwhile, the operator actually measures the thickness of the internal oxide layer of the measurement target portion and inputs the measured value into the processing device 10. The method for measuring the thickness of the internal oxide layer is as described above. In this manner, the actual measured values of the cumulative temperature and the thickness of the internal oxide layer are obtained for a plurality of measurement target portions. This test may be performed as an offline test.
[0061] Next, the internal oxidation start temperature estimation unit 11 plots the obtained cumulative temperature and the measured values of the thickness of the internal oxidation layer as measurement points on an xy plane with the cumulative temperature and the thickness of the internal oxidation layer as the xy axis. An example is shown in FIG. 2. The horizontal axis of FIG. 2 indicates the thickness of the internal oxidation layer (μm), and the vertical axis indicates the cumulative temperature (℃·min). In this example, the internal oxidation start temperature Tcr is 500℃. Points P1 and P2 indicate the measured values of the cumulative temperature and the thickness of the internal oxidation layer at each measurement target portion. Point P1 indicates the value at the measurement target portion set within the center / quarter portion of the plate width of the hot-rolled steel plate, and point P2 indicates the value at the measurement target portion set at the edge portion (end portion) in the plate width direction of the hot-rolled steel plate.
[0062] Next, the internal oxidation start temperature estimation unit 11 performs regression analysis on a plurality of measurement points to calculate an approximation equation (temperature determination correlation equation) for these measurement points. The regression analysis may be, for example, a simple regression analysis using the least squares method. Here, it is preferable that the measurement target portion is set within the width center / quarter portion. This is because there is a high correlation between the accumulated temperature within the width center / quarter portion and the actual measured value of the thickness of the internal oxidation layer. Furthermore, the width center / quarter portion, especially the center portion, is prone to forming a particularly thick internal oxidation layer. In this respect, it is also preferable that the measurement target portion is set within the width center / quarter portion. In the example of FIG. 2, the internal oxidation start temperature estimation unit 11 performs simple regression analysis on the measurement point P1 (width center / quarter portion) to obtain a graph L1 (temperature determination correlation equation). The degree of freedom determination coefficient R of the graph L1 2 In the example of Figure 2, when the measurement points P1 and P2 (edges) are subjected to regression analysis, the coefficient of freedom of the correlation equation for determining the temperature, R 2 is approximately 0.88. The temperature drop at the edge is greater than at the center and quarter of the sheet width, and the variation is also greater. For this reason, it is thought that the correlation between the cumulative temperature and the measured thickness of the internal oxide layer at the edge is somewhat lower. In other words, when a regression analysis is performed including the cumulative temperature at the edge, the degree of freedom determination coefficient R of the correlation equation for determining the temperature is 2 will be slightly lower.
[0063] Next, the internal oxidation start temperature estimation unit 11 determines the internal oxidation start temperature Tcr based on the correlation between the actual measured value of the thickness of the internal oxidation layer and the cumulative temperature when the internal oxidation start temperature Tcr is changed. For example, the internal oxidation start temperature estimation unit 11 derives the above-mentioned temperature determination correlation equation by setting the internal oxidation start temperature Tcr to various different values, and calculates the degree of freedom determination coefficient R 2 Then, the internal oxidation start temperature estimation unit 11 calculates the degree of freedom determination coefficient R of the temperature determination correlation equation. 2 is selected. The internal oxidation start temperature Tcr is selected when the internal oxidation start temperature Tcr is highest (i.e., when the correlation between the measured thickness of the internal oxidation layer and the cumulative temperature is highest).
[0064] FIG. 3 shows a specific example of the degree of freedom determination coefficient R 2 3 is a graph showing that the internal oxidation start temperature Tcr (i.e., the correlation between the actual measured value of the thickness of the internal oxidation layer and the cumulative temperature) varies depending on the internal oxidation start temperature Tcr. The horizontal axis of FIG. 3 shows the internal oxidation start temperature Tcr (°C), and the vertical axis shows the degree of freedom determination coefficient R 2 The plotted points P3 and P4 are the internal oxidation start temperature Tcr and the degree of freedom determination coefficient R of the correlation equation for temperature determination. 2 The graphs L2 and L3 are curve graphs connecting points P3 and P4, respectively. However, point P3 corresponds to the coefficient of freedom of determination R of the correlation equation for temperature determination obtained by regression analysis of the cumulative temperature in the width center quarter part (width center quarter part over the entire length). 2 The point P4 indicates the degree of freedom of the correlation equation for temperature determination obtained by regression analysis of the cumulative temperatures in the center and quarter parts and edge parts (full length and full width) of the strip width. 2 As is clear from Figure 3, the coefficient of determination R 2 is the coefficient of determination R 2 Therefore, the cumulative temperature in the width center and quarter areas shows a high correlation with the measured thickness of the internal oxide layer.
[0065] Both graphs L2 and L3 have peaks. Graph L2 has a peak at an internal oxidation start temperature Tcr of 500°C, while graph L3 has a peak at 450°C. The temperature at the edge is lower than the temperature at the center and quarter sections of the sheet width, and there is also a large variation, which is thought to be why this tendency appears. In any case, the peak of graph L3 is lower than the peak of graph L2. Therefore, in the example of Figure 3, it can be seen that it is preferable to set the internal oxidation start temperature Tcr to 500°C.
[0066] The operator and the internal oxidation start temperature estimation unit 11 perform the above process for at least one of the concentrations of Si, Mn, and Al, preferably for each of a plurality of types of hot-rolled steel sheets having different concentrations of Si and Mn, to obtain the internal oxidation start temperature Tcr as the objective variable. Next, the internal oxidation start temperature estimation unit 11 obtains a regression equation using the internal oxidation start temperature obtained above as the objective variable and at least one of the concentrations of Si, Mn, and Al of the hot-rolled steel sheet as the explanatory variables. The method of obtaining the regression equation is as described above, and for example, regression equations (A) to (D) can be obtained.
[0067] Next, the internal oxidation start temperature estimation unit 11 determines the internal oxidation start temperature Tcr based on the regression equation obtained above. Specifically, an operator measures the Si concentration, Mn concentration, and Al concentration of a hot-rolled steel sheet to be actually manufactured, and inputs the Si concentration, Mn concentration, and Al concentration into the processing device 10. Next, the internal oxidation start temperature estimation unit 11 determines the internal oxidation start temperature Tcr by substituting these concentrations into the regression equation obtained above.
[0068] (3-4. Fourth estimation method) The fourth estimation method is similar to the third estimation method, but differs from the third estimation method in that it fits a quadratic function of the cumulative temperature to the actual measured value of the thickness of the internal oxide layer (a linear function in the third estimation method).
[0069] Specifically, first, the internal oxidation start temperature estimation unit 11 sets the internal oxidation start temperature Tcr to an arbitrary value (for example, an arbitrary value within the range of 200 to 1000 ° C). Next, the internal oxidation start temperature estimation unit 11 sets measurement target parts at multiple positions on the surface of the hot-rolled steel sheet, and calculates the cumulative temperature of these measurement target parts based on the above-mentioned formula (1). The measurement target parts may be set by the internal oxidation start temperature estimation unit 11 or by an operator. In the former case, the internal oxidation start temperature estimation unit 11 may display the measurement target parts on a display or the like. In the latter case, the operator may input the measurement target parts into the processing device 10. The measurement target parts may be set for the entire length in the rolling direction and the entire width in the sheet width direction of the hot-rolled steel sheet, or may be set for a part of the entire length and the entire width. In the example described below, the measurement target parts are set for the entire length and the entire width. In addition, it is preferable that the measurement target parts are set at the sheet width center and quarter parts. As mentioned above, the cumulative temperature in the width center quarter area has a high correlation with the actual measured thickness of the internal oxide layer. The definition of the width center quarter area is as mentioned above.
[0070] Meanwhile, the operator actually measures the thickness of the internal oxide layer of the measurement target portion. The method for measuring the thickness of the internal oxide layer is as described above. In this manner, the internal oxidation start temperature estimation unit 11 obtains the actual measured values of the cumulative temperature and the thickness of the internal oxide layer for the multiple measurement target portions. This test may be performed as an offline test.
[0071] Next, the internal oxidation start temperature estimation unit 11 plots the obtained actual values of the accumulated temperature and the thickness of the internal oxide layer as measurement points on an xy plane with the accumulated temperature and the thickness of the internal oxide layer as the xy axes.
[0072] Next, the internal oxidation start temperature estimation unit 11 calculates an approximation equation (temperature determination correlation equation) for a plurality of measurement points by performing regression analysis with a quadratic function of the accumulated temperature. The regression analysis may be, for example, a simple regression analysis using the least squares method. Here, the measurement target portion is preferably set within the width center / quarter portion. This is because there is a high correlation between the accumulated temperature within the width center / quarter portion and the actual measured value of the thickness of the internal oxide layer. Furthermore, the internal oxide layer is likely to be formed particularly thickly in the width center / quarter portion, especially in the center portion. In this respect, it is also preferable that the measurement target portion is set within the width center / quarter portion. Then, the internal oxidation start temperature estimation unit 11 fits the quadratic function of the accumulated temperature to the actual measured value of the thickness of the internal oxide layer to calculate the sum of squares of the deviation.
[0073] Next, the internal oxidation onset temperature estimation unit 11 performs a similar process by varying the internal oxidation onset temperature Tcr as a variable parameter, and determines the internal oxidation onset temperature Tcr so that the sum of squares of the deviation is minimized when a quadratic function of the cumulative temperature is fitted to the actual measured value of the thickness of the internal oxidation layer.
[0074] The operator and the internal oxidation start temperature estimation unit 11 perform the above process for at least one of the concentrations of Si, Mn, and Al, preferably for each of a plurality of types of hot-rolled steel sheets having different concentrations of Si and Mn, to obtain the internal oxidation start temperature Tcr as the objective variable. Next, the internal oxidation start temperature estimation unit 11 obtains a regression equation using the internal oxidation start temperature obtained above as the objective variable and at least one of the concentrations of Si, Mn, and Al of the hot-rolled steel sheet as the explanatory variables. The method of obtaining the regression equation is as described above, and for example, regression equations (A) to (D) can be obtained.
[0075] Next, the internal oxidation start temperature estimation unit 11 determines the internal oxidation start temperature Tcr based on the regression equation obtained above. Specifically, an operator measures the Si concentration, Mn concentration, and Al concentration of a hot-rolled steel sheet to be actually manufactured, and substitutes these concentrations into the regression equation obtained above to determine the internal oxidation start temperature Tcr.
[0076] <4. Processing performed by the internal oxide layer thickness estimation unit> Next, a process performed by the internal oxidation layer thickness estimation unit 12 according to the present embodiment will be described. The internal oxidation layer thickness estimation unit 12 according to the present embodiment estimates the thickness of the internal oxidation layer based on the internal oxidation start temperature estimated by the internal oxidation start temperature estimation unit 11 and the following formula (2). H = α × S T +H0(2)
[0077] In formula (2), S T is the cumulative temperature, and H0 is the initial value of the thickness of the internal oxide layer. The initial value H0 of the thickness of the internal oxide layer means the thickness of the internal oxide layer at the estimation start time t0. The initial value H0 of the thickness of the internal oxide layer can be measured by an operator quenching the hot-rolled steel sheet to the internal oxidation start temperature Tcr or lower at the estimation start time t0 and then observing the cross section. If it is clear that no internal oxide layer has been formed at the estimation start time t0, the initial value H0 may be set to 0 without performing such a measurement.
[0078] α is a proportionality constant. The proportionality constant α can be determined by the internal oxide layer thickness estimating unit 12 through regression analysis based on a plurality of sets of actual measurement data of the cumulative temperature and the actual measurement value of the thickness of the internal oxide layer. However, the proportionality constant α may also be determined by the method described below.
[0079] Specifically, the worker prepares hot-rolled steel sheets having at least one of Si, Mn, and Al concentrations, preferably a plurality of types of hot-rolled steel sheets having different Si and Mn concentrations. Next, these hot-rolled steel sheets are coiled and then held at a predetermined holding temperature. The holding temperature is not particularly limited, but is preferably about 600 to 700°C, for example. This is because the internal oxidation phenomenon appears significantly in this temperature range.
[0080] Then, the worker measures the thickness of the internal oxide layer every time the preset holding time has elapsed. The method for measuring the thickness of the internal oxide layer is as described above. The position for measuring the thickness of the internal oxide layer is not particularly limited, but is preferably, for example, the center (center part) in the sheet width direction of the hot-rolled steel sheet. The data obtained by the above steps is summarized, for example, as shown in Table 2. The data in Table 2 is created for each prepared hot-rolled steel sheet. The worker inputs the data in Table 2 into the processing device 10. In Table 2, Δt is the holding time (the time elapsed after the temperature of the coil reaches the holding temperature), and H is the thickness of the internal oxide layer. It is preferable to obtain five or more pieces of data for each hot-rolled steel sheet. This is to accurately estimate the proportionality constant α.
[0081] [Table 2]
[0082] An example of a graph of the data in Table 2 is shown in Figure 4. The horizontal axis of Figure 4 shows the holding time (hr), and the vertical axis shows the actual thickness of the internal oxide layer (μm). Point P20 shows the holding time and the actual thickness of the internal oxide layer for a hot-rolled steel sheet containing 1.02 mass% Si, 2.28 mass% Mn, and 0.02 mass% Al. Graph L20 is an approximation curve of point P20.
[0083] Point P21 indicates the holding time and the thickness of the internal oxide layer of a hot-rolled steel sheet containing 0.45 mass% Si, 2.58 mass% Mn, and 0.03 mass% Al. Graph L21 is an approximation curve of point P21.
[0084] Point P22 indicates the holding time and the thickness of the internal oxide layer of a hot-rolled steel sheet containing 0.60 mass% Si, 2.08 mass% Mn, and 0.03 mass% Al. Graph L22 is an approximation curve of point P22.
[0085] Point P23 indicates the holding time and the thickness of the internal oxide layer of a hot-rolled steel sheet containing 0.37 mass% Si, 2.41 mass% Mn, and 0.39 mass% Al. Graph L23 is an approximation curve of point P23.
[0086] As is clear from FIG. 4, the proportionality constant α can vary if the composition of the hot-rolled steel sheet is different.
[0087] Since the holding temperature is constant, equations (1) and (2) can be replaced by the following equation (3). H = α(Te-Tcr)△t (3) In equation (3), Te is the holding temperature and Δt is the holding time. Therefore, the internal oxidation layer thickness estimation unit 12 can obtain the proportional constant α for each hot-rolled steel sheet by performing a simple regression analysis on the data in Table 2. The value determined by the above method may be used as the internal oxidation start temperature Tcr in the formula (3). For example, for the steel type A corresponding to the point P20 in Fig. 4, the data shown in the following Table 3 is obtained.
[0088] [Table 3]
[0089] A simple regression analysis of the data in Table 3 yielded an intercept of 1.27 and a slope of 1.78×10 -4 Therefore, the proportionality constant α corresponding to steel type A is α = 1.78 × 10 -4 The internal oxide layer thickness estimation unit 12 compiles the data obtained by the above steps, for example, as shown in Table 4.
[0090] [Table 4]
[0091] Next, the internal oxide layer thickness estimation unit 12 measures the cumulative temperature of the measurement target portion for which the thickness of the internal oxide layer is desired based on the formula (1). The temperature T of the measurement target portion may be measured by the above-mentioned simulation or actual measurement. Furthermore, the internal oxidation start temperature Tcr estimated by the above-mentioned method is used. Next, the internal oxide layer thickness estimation unit 12 can estimate the thickness of the internal oxide layer of the portion by applying the measured cumulative temperature to the formula (2). Here, the internal oxide layer thickness estimation unit 12 may use, as the proportionality constant α in the formula (2), the proportionality constant α corresponding to the composition closest to the composition of the hot-rolled steel sheet to be measured, among the data summarized in Table 4. Alternatively, as described above, the internal oxide layer thickness estimation unit 12 can determine the proportionality constant α by regression analysis based on multiple sets of actual measurement data of the cumulative temperature and the actual measurement value of the thickness of the internal oxide layer. Although details will be described later in the examples, there is a high correlation between the cumulative temperature and the actual measurement value of the thickness of the internal oxide layer, and the coefficient of freedom of determination R of the formula (2) 2 The internal oxidation start temperature Tcr also increases. Therefore, the thickness of the internal oxidation layer can be estimated with high accuracy based on the formula (2). Furthermore, since the internal oxidation start temperature Tcr varies based on the concentrations of Si, Mn, and Al in the hot-rolled steel sheet, in this embodiment, the internal oxidation start temperature estimation unit 11 determines (estimates) the internal oxidation start temperature Tcr based on these concentrations. Therefore, the internal oxidation start temperature Tcr can be determined with high accuracy, and the thickness of the internal oxidation layer can be estimated with high accuracy. By estimating the internal oxidation start temperature with high accuracy, the estimation accuracy of the thickness of the internal oxidation layer is improved, and appropriate manufacturing conditions can be determined. Specifically, the coiling temperature conditions are optimized so that the thickness of the internal oxidation layer after coiling and cooling is equal to or less than a predetermined value, thereby improving the efficiency of the next process, the pickling process.
[0092] For example, since the cumulative temperature varies depending on the winding completion temperature, the thickness of the internal oxide layer also varies. Therefore, the internal oxide layer thickness estimation unit 12 can also estimate the winding completion temperature for obtaining a desired thickness of the internal oxide layer. In other words, the thickness of the internal oxide layer can be controlled by the winding completion temperature.
[0093] <5. Processing procedure performed by the processing device> Next, the procedure of the process performed by the processing device according to this embodiment will be described with reference to the flowchart shown in Fig. 7. Note that since the detailed process has been described above, only the outline will be described here.
[0094] In step S10, the internal oxidation start temperature estimation unit 11 estimates the internal oxidation start temperature based on the concentrations of Si, Mn, and Al contained in the hot-rolled steel sheet. Specifically, the internal oxidation start temperature estimation unit 11 estimates the internal oxidation start temperature based on any one of the above-mentioned first to fourth estimation methods.
[0095] In step S20, the internal oxidation layer thickness estimation unit 12 estimates the thickness of the internal oxidation layer based on the internal oxidation start temperature estimated by the internal oxidation start temperature estimation unit 11 and the above-mentioned formula (2). EXAMPLES
[0096] Next, an example of this embodiment will be described. In this example, the following experiment was performed to confirm the effect of this embodiment. Of course, the present invention is not limited to the example described below. It is clear that a person with ordinary knowledge in the technical field to which the present invention belongs can think of various modified or revised examples within the scope of the technical idea described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.
[0097] First, the steel types A to D shown in Table 5 were prepared as test pieces of hot-rolled steel sheets. Next, the steel types A to D were each coiled at a coiling completion temperature of 600°C, and then air-cooled to room temperature. At this time, the internal oxidation start temperatures Tcr of the steel types A to D were determined by the second estimation method described above. The results are also shown in Table 5. Next, the data in Table 5 were subjected to multiple regression analysis to calculate the regression equations (A1) and (B1) shown below. Tcr=813.65-143.4×(%Si)-118.63×(%Mn)+155.01×(%Al) (A1) Tcr=895.12-336.73×(%Si) / (%Mn)-155.39×(%Mn)+151.39×(%Al) (B1)
[0098] [Table 5]
[0099] Next, the composition of steel type A was substituted into regression equation (B1). As a result, the internal oxidation start temperature Tcr was 395.6 (℃), which was confirmed to be almost the same as the internal oxidation start temperature Tcr determined by the second estimation method. When the internal oxidation start temperature Tcr of steel type A was estimated by another estimation method, the internal oxidation start temperature Tcr was approximately 400℃.
[0100] Next, the cumulative temperature of any measurement part of steel type A was calculated, with t0 being the time when coiling was completed and t1 being the time when the temperature T of the measurement part reached the internal oxidation start temperature Tcr. The internal oxidation start temperature Tcr was 395.6 (°C). Furthermore, the thickness of the internal oxide layer of these measurement parts was actually measured. These values were then subjected to simple regression analysis to determine the proportionality constant α. H0 was set to 0. The proportionality constant α was 2×10 -5 μm / (℃·min) The results are shown in Figure 5.
[0101] P30 in Fig. 5 shows the measured cumulative temperature and thickness of the internal oxide layer for each measurement part of steel type A. Graph L30 shows the correlation between the above-obtained formula (2), i.e., the cumulative temperature and the estimated thickness of the internal oxide layer. As is clear from Fig. 5, formula (2) has an extremely high correlation with the measured thickness of the internal oxide layer. The coefficient of determination R2 of the degree of freedom of formula (2) was 0.9989. In addition, when the internal oxidation start temperature Tcr was estimated using regression formula (A1), almost the same results were obtained, but the coefficient of determination of the degree of freedom of formula (2) was slightly lower. In addition, the correlation formula is described here starting from a cumulative temperature of 40,000°C·min, but this is merely an example, and the method of determining the correlation formula is not limited to this example.
[0102] Therefore, since the internal oxidation start temperature Tcr is determined based on the composition of the hot-rolled steel sheet, the internal oxidation start temperature Tcr can be estimated with high accuracy. Furthermore, since the thickness of the internal oxidation layer is estimated based on the internal oxidation start temperature Tcr estimated with high accuracy and the formula (2) (i.e., the cumulative temperature that has a high correlation with the thickness of the internal oxidation layer), the thickness of the internal oxidation layer can be estimated with high accuracy.
[0103] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or amended examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally fall within the technical scope of the present invention. [Explanation of symbols]
[0104] P1, P30 Measurement points showing the actual values of the cumulative temperature and the thickness of the internal oxide layer P3, P4 Measurement points showing the correlation between the internal oxidation start temperature Tcr, the actual thickness of the internal oxide layer, and the cumulative temperature P10~P12 Measurement points showing the actual values of the winding completion temperature and the thickness of the internal oxide layer Graph showing correlation between cumulative temperature and estimated thickness of internal oxide layer for L1 and L30 L10~L12 Thickness-winding temperature correlation graph 10 Processing equipment 11 Internal oxidation start temperature estimation section 12. Internal oxide layer thickness estimation section
Claims
1. An internal oxidation start temperature estimation device for estimating an internal oxidation start temperature, which is a minimum temperature required for an internal oxidation layer to grow on a surface of a hot-rolled steel sheet containing easily oxidizable elements including at least one of Si, Mn, and Al, An internal oxidation start temperature estimation unit that estimates the internal oxidation start temperature based on concentrations of Si, Mn, and Al contained in the easily oxidizable element-containing hot-rolled steel sheet, The internal oxidation start temperature estimation unit estimates the internal oxidation start temperature of the easily oxidizable element-containing hot-rolled steel plate using a correlation between the internal oxidation start temperature of the test hot-rolled steel plate and the concentrations of Si, Mn, and Al of the test hot-rolled steel plate; The internal oxidation start temperature of the test hot-rolled steel sheet is obtained based on the actual measured value of the thickness of the internal oxide layer formed on the test hot-rolled steel sheet. An internal oxidation start temperature estimation device.
2. The internal oxidation start temperature estimation device according to claim 1, characterized in that the internal oxidation layer is formed when the hot-rolled steel sheet containing an easily oxidizable element is cooled in a coiled state.
3. 3. The internal oxidation start temperature estimation device according to claim 1, characterized in that the internal oxidation start temperature estimation unit determines the temperature at which the internal oxidation layer begins to form on the surface of the test hot-rolled steel sheet based on an actual measurement value of the thickness of the internal oxidation layer formed on the test hot-rolled steel sheet as the internal oxidation start temperature.
4. The test hot-rolled steel sheet is wound into a coil, The internal oxidation start temperature estimation unit is For each of the plurality of types of the test hot-rolled steel sheets having different concentrations of at least one of Si, Mn, and Al, a thickness-coiling temperature correlation graph is generated that shows a correspondence relationship between a coiling completion temperature, which is a temperature at the time when coiling of the test hot-rolled steel sheet is completed, and an actual measured value of the thickness of the internal oxide layer of the test hot-rolled steel sheet; 3. The internal oxidation start temperature estimation device according to claim 1, wherein the thickness-coiling temperature correlation graph is extrapolated to determine the coiling completion temperature at which a thickness of the internal oxidation layer of the test hot-rolled steel sheet becomes zero as the internal oxidation start temperature.
5. The internal oxidation start temperature estimation unit determines the internal oxidation start temperature for each of a plurality of types of the test hot-rolled steel sheets having different concentrations of at least one of Si, Mn, and Al, such that a correlation between an actual measured value of the thickness of the internal oxidation layer of the test hot-rolled steel sheet and an accumulated temperature of the test hot-rolled steel sheet defined by the following mathematical formula (1) is maximized. [0010] In the formula (1), S T is the cumulative temperature of the test hot-rolled steel plate, T is the temperature of an estimation target portion of the test hot-rolled steel plate that is the target for estimating the thickness of the internal oxidation layer of the test hot-rolled steel plate, Tcr is the internal oxidation start temperature, t0 is an estimation start point at which estimation of the thickness of the internal oxidation layer of the test hot-rolled steel plate is started, and t1 is an estimation evaluation point, and T-Tcr is set to 0 in an integral interval where T-Tcr is 0 or less.
6. The internal oxidation start temperature estimation unit determines the internal oxidation start temperature for each of a plurality of types of the test hot-rolled steel sheets having different concentrations of at least one of Si, Mn, and Al, such that a deviation square sum is minimized when a quadratic function of the accumulated temperature of the test hot-rolled steel sheet is fitted to the actual measured value of the thickness of the internal oxidation layer of the test hot-rolled steel sheet. The internal oxidation start temperature estimation device according to claim 5,
7. 7. An internal oxidation layer thickness estimation device, comprising: an internal oxidation layer thickness estimation unit that estimates a thickness of the internal oxidation layer formed in the easily oxidizable element-containing hot-rolled steel sheet based on the internal oxidation start temperature of the easily oxidizable element-containing hot-rolled steel sheet estimated by the internal oxidation start temperature estimation device described in claim 5 or 6 and the following formula (2). H=α×S T +H 0 (2) In the formula (2), H is the thickness of the internal oxide layer of the easily oxidizable element-containing hot-rolled steel sheet, S T is the cumulative temperature of the hot-rolled steel sheet containing easily oxidizable elements, α is a proportionality constant, H 0 is the initial value of the thickness of the internal oxide layer of the easily oxidizable element-containing hot-rolled steel sheet.
8. A method for estimating an internal oxidation start temperature, which is a minimum temperature required for an internal oxidation layer to grow on a surface of a hot-rolled steel sheet containing easily oxidizable elements including at least one of Si, Mn, and Al, comprising: An internal oxidation start temperature estimation step of estimating the internal oxidation start temperature based on the concentrations of Si, Mn, and Al contained in the easily oxidizable element-containing hot-rolled steel sheet, In the internal oxidation start temperature estimation step, the internal oxidation start temperature of the easily oxidizable element-containing hot-rolled steel sheet is estimated using a correlation between the internal oxidation start temperature of the test hot-rolled steel sheet and the concentrations of Si, Mn, and Al of the test hot-rolled steel sheet; The internal oxidation start temperature of the test hot-rolled steel sheet is obtained based on the actual measured value of the thickness of the internal oxide layer formed on the test hot-rolled steel sheet. A method for estimating an internal oxidation start temperature.
9. On the computer, A program for estimating an internal oxidation start temperature, which is a minimum temperature required for an internal oxidation layer to grow on a surface of a hot-rolled steel sheet containing easily oxidizable elements including at least one of Si, Mn, and Al, The computer includes: carrying out an internal oxidation start temperature estimation step of estimating the internal oxidation start temperature based on the concentrations of Si, Mn, and Al contained in the easily oxidizable element-containing hot-rolled steel sheet; In the internal oxidation start temperature estimation step, the internal oxidation start temperature of the easily oxidizable element-containing hot-rolled steel sheet is estimated using a correlation between the internal oxidation start temperature of the test hot-rolled steel sheet and the concentrations of Si, Mn, and Al of the test hot-rolled steel sheet; The internal oxidation start temperature of the test hot-rolled steel sheet is obtained based on the actual measured value of the thickness of the internal oxide layer formed on the test hot-rolled steel sheet. A program characterized by:
Citation Information
Patent Citations
Easy and quick method of estimating generation amount of internal oxide layer of electromagnetic steel plate
JP1991108639A
Surface condition measuring method for steel sheet and steel sheet temperature measuring method
JP1996219891A
Production of steel sheet for heat treatment excellent in peeling resistance of scale
JP1997256066A
Method of evaluating internal oxide layer of metallic material surface layer
JP2004020519A
Method for producing wire rod for steel wire, and wire rod for steel wire
JP2005281793A