Polyimide film manufacturing method
The described method for polyimide film production using a multi-zone tenter heating process with controlled temperature settings addresses the challenge of orientation anisotropy, achieving more uniform films by balancing bowing strains.
Patent Information
- Application Number
- JP2020173048
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-14
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-10-14
AI Technical Summary
Conventional methods for producing polyimide films struggle to adequately control orientation anisotropy, particularly when using rigid monomers or materials with low elastic modulus at high temperatures, leading to uneven deformation and non-uniform properties.
A method involving a tenter heating process with a heating furnace composed of multiple zones, including hot air and radiant heating, where the temperature of the first hot air oven is set between 270 to 360°C, and the maximum temperature is between 330 to 420°C, with controlled temperature differences between adjacent furnaces to balance positive and negative bowing strains.
This approach effectively reduces orientation anisotropy by offsetting bowing strains, resulting in more uniform polyimide films with improved molecular orientation.
Smart Images

Figure 0007557333000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polyimide film. [Background technology]
[0002] Polyimide films are produced continuously by casting an organic solvent solution of polyamic acid, the precursor of polyimide, onto a rotating support such as a metal drum, drying and curing it until it is self-supporting to obtain a gel film, which is then peeled off and, while fixing both ends to maintain or expand the width of the gel film, transported to a heating furnace and heated for further drying and curing.
[0003] The tenter system as described above is a well-known technology suitable for maintaining or stretching the width of the gel film while resisting the curing shrinkage of the gel film during the drying and curing process in a heating oven, but it is difficult to make the transverse physical properties of the product film uniform. The reason for this is that in the tenter, both ends of the film are held by clips or pin sheets, so that the longitudinal stretching stress and shrinkage stress are restrained, whereas the center of the film is less affected by the holding means and has a weaker restraining force, so that it is more susceptible to the longitudinal stretching stress and shrinkage stress, and as a result, the directions of the stress received at both ends and the center of the film are different, leaving uneven deformation. This phenomenon is called the bowing phenomenon, and this bowing phenomenon causes the transverse physical properties of the film to be non-uniform.
[0004] The anisotropy of the width direction of a polyimide film has been a long-standing issue, and various attempts have been made to improve the anisotropy. For example, in a method for producing a polyimide film, which includes a step of casting and applying an organic solvent solution of polyamic acid onto a rotating support, drying and curing the solution until it has self-supporting properties to obtain a gel film, peeling the gel film off, fixing both ends of the gel film to maintain or expand its width while transporting the gel film to a heating furnace and heating the film, there is a method for controlling the orientation by focusing on the shrinkage phenomenon of the gel film on the support, the amount of remaining volatile components in the gel film, and the heating start temperature in the heating furnace (Patent Document 1). In addition, in a tenter heating step in which the ends of the gel film are fixed and heated, it is known that the orientation can be controlled by determining the tension applied to the gel film, the maximum baking temperature in the heating furnace, and the amount of remaining volatile components in the gel film based on the relationship between the elastic modulus of the gel film, the elastic modulus in the first zone of the tenter heating furnace, and the elastic modulus in the second zone of the tenter heating furnace (Patent Document 2). Furthermore, in the tenter heating step of the above-mentioned method for producing a polyimide film, a method is known in which the initial heating temperature is set to 180°C or higher, and heating is performed within a certain temperature range in the initial heating stage without changing the distance between the gripping members at both ends, thereby producing a film with a small degree of orientation anisotropy, and in a temperature range exceeding 220°C, stretching is performed in the width direction to control the linear expansion coefficient within a desired range (Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2003-165850 A [Patent Document 1] JP 2008-12776 A [Patent Document 2] WO2011 / 145696 publication Summary of the Invention [Problem to be solved by the invention]
[0006] Conventional methods for manufacturing polyimide that control the orientation anisotropy are effective in controlling the anisotropy to a certain extent. However, in order to meet the high level of performance required for recent FPCs, even higher characteristics are required for polyimide films, and the options for raw materials for the polyimide used are expanding accordingly. However, when rigid monomers are used as raw materials or raw materials that give the film a low elastic modulus at high temperatures are selected, conventional methods may not be able to adequately control the orientation, leaving room for improvement. Therefore, an object of the present invention is to provide a method for producing a polyimide film that can control the orientation anisotropy of the film, even when a rigid monomer is used as a raw material for the polyimide film, or when a raw material that reduces the elastic modulus of the film at high temperatures is selected. [Means for solving the problem]
[0008] The present invention relates to A polyamic acid organic solvent solution is cast or coated on a support and dried until it becomes self-supporting. 、 forming a gel film that is a partially imidized and / or partially dried polyamic acid film; peeling the gel film from the support; and The method for producing a polyimide film includes a tenter heating step of fixing the ends of the gel film and subjecting it to a heat treatment. (However, this does not include a process for heating the film in a state where the edges of the film are released after the tenter heating process.) In the tenter heating process, heat treatment is performed in a heating furnace consisting of at least three furnaces connected in the longitudinal direction of the film. do. The heating furnace is composed of a hot air heating zone in which two or more hot air stoves are arranged, and a radiant heat heating zone in which one or more radiant heat heater furnaces are arranged, which is arranged next to the hot air heating zone. There are. The temperature of the first hot air oven through which the gel film first passes in the tenter heating process is set in the range of 270 to 360°C, and the minimum temperature in the tenter heating process is 270°C or higher, and the maximum oven temperature is set in the range of 330 to 420°C. 。 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] The embodiment of the present invention will be described below. First, the polyimide film according to the present invention will be described based on one example of the embodiment, but the present invention is not limited thereto. In this specification, unless otherwise specified, "A to B" representing a numerical range means "A or more (including A and larger than A) and B or less (including B and smaller than B)".
[0031] The present invention relates to a method for producing a polyimide film, which includes at least a step of casting or applying a polyamic acid organic solvent solution onto a support and drying the polyamic acid to form a gel film, which is a polyamic acid film that has been partially imidized and / or partially dried until it has self-supporting properties, a step of peeling the gel film from the support, and a tenter heating step of fixing the ends of the gel film and subjecting it to a heat treatment, wherein the tenter heating step involves subjecting the film to a heat treatment in a heating furnace having at least three furnaces connected in the longitudinal direction of the film, the heating furnace comprising a hot air heating zone having two or more hot air furnaces and a radiant heat ray heating zone having one or more radiant heat ray heater furnaces arranged subsequent to the hot air heating zone, the temperature of the first hot air furnace through which the gel film first passes in the tenter heating step is set in the range of 270 to 360°C, the minimum temperature in the tenter heating step is 270°C or higher, and the temperature of the furnace set to the maximum temperature is in the range of 330 to 420°C. In addition, in the present specification, the expression "set", such as "the temperature is set in the range of 270 to 360° C.", is used, but it means "controlled" or "to control".
[0032] In the present invention, the tenter heating step involves heating in a hot air heating zone and heating in a radiant heat ray heating zone, and the temperature of the first hot air oven through which the gel film passes first is set to a relatively high temperature of 270 to 360°C. It is preferable that the temperatures of the multiple ovens subsequent to the first hot air oven are not increased significantly, and the temperature difference between adjacent ovens is set to a range of 100°C or less. Furthermore, the maximum temperature of the multiple ovens is set to a relatively low temperature of 330 to 420°C. This was set by the present inventors after verification based on the following hypothesis.
[0033] Generally, a film produced by a tenter is considered to have a positive bowing strain. When the orientation of a polyimide film in the width direction is measured, it is possible to determine whether the film has a positive or negative bowing strain, and the degree of the strain, by checking whether the orientation angle of the end portion is negative or positive with respect to the direction of travel. When the orientation angle of the end portion of various polyimide films produced through the tenter heating process, including existing long polyimide films, was checked, it was confirmed that all of the films had a positive bowing strain. Since the film produced in the end has a positive bowing strain, the inventors set the temperature of the above-mentioned multiple furnaces by assuming the bowing phenomenon that occurs in each baking furnace.
[0034] That is, the inventors first distinguished the bowing phenomenon occurring in each firing furnace into a bowing phenomenon in which the center lags behind the ends (hereinafter also referred to as positive bowing) and a bowing phenomenon in which the ends lag behind the center (hereinafter also referred to as negative bowing).
[0035] It was considered that the dominant factors of negative bowing were shrinkage stress caused by the volatilization of the solvent contained in the gel film and curing shrinkage caused by the chemical reaction of the precursor polyamic acid to polyimide. In other words, it is considered that negative bowing occurs especially in the first half of the continuous baking furnace, such as the first zone of the tenter heating furnace. In addition, it was considered that positive bowing is closely related to the decrease in elastic modulus when the film is exposed to high temperatures, and is caused by the difference in elastic modulus within the tenter. In other words, it is considered that it is particularly likely to occur in the second half of the continuous baking furnace where the maximum baking temperature is reached, and then in the baking furnace with a relatively high temperature where the residual solvent has been sufficiently volatilized. Therefore, it was considered that the anisotropy of the polyimide film finally manufactured can be improved by balancing (offsetting) the strain caused by positive bowing and the strain caused by negative bowing. Based on this idea, the temperature of the first hot air furnace through which the gel film first passes in the tenter heating process, the temperature difference between adjacent furnaces arranged in the heating furnace, and the temperature of the furnace set to the maximum temperature were set within specific ranges, and a surprising effect of suppressing the orientation anisotropy was confirmed. Such an effect is also exhibited in the case of a general-purpose polyimide film that is originally difficult to orient. However, in recent years, the raw material monomers and film-forming conditions selected to meet the various film properties required for FPCs have become complicated, and even if a film that meets those properties is obtained, the result may be a film that is easy to orient. A particularly excellent effect is exhibited in a polyimide film that is easy to orient. Hereinafter, the steps of forming a gel film, which is a polyamic acid film that is partially imidized and / or partially dried until it has self-supporting properties, by casting or applying a polyamic acid organic solvent solution onto a support and drying it, the step of peeling the gel film from the support, and the tenter heating step of fixing the ends of the gel film and performing heat treatment will be described in this order.
[0036] <A process of casting or coating a polyamic acid organic solvent solution on a support and drying it to form a gel film, which is a polyamic acid film that is partially imidized and / or partially dried to a self-supporting property> In the method for producing a polyimide film of the present invention, a solution of a polyamic acid, which is a polyimide precursor, in an organic solvent is cast and coated, and the polyimide film is partially dried and / or imidized to have self-supporting properties. The raw material monomers used in the present invention may be diamines and acid dianhydrides that are commonly used in the synthesis of polyamic acids.
[0037] The aromatic diamine is not particularly limited as long as it can exhibit the effects of the present invention, and examples thereof include 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 4,4'-oxydianiline, 3,3'-oxydianiline, 3,4'-oxydianiline, 4,4'-diaminodiphenyldiethylsilane, 4,4'-diaminodiphenylsilane, 4,4'-diaminodiphenylethylphosphine oxide, 4,4'-diaminodiphenyl N-methylamine, 4,4'-diaminodiphenyl Examples of the aminophenylamine include N-phenylamine, 1,4-diaminobenzene (p-phenylenediamine), bis{4-(4-aminophenoxy)phenyl}sulfone, bis{4-(3-aminophenoxy)phenyl}sulfone, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 2,2-bis(4-aminophenoxyphenyl)propane, 1,3-bis(4-aminophenoxy)benzene, and 4,4'-diamino-2,2'-dimethylbiphenyl. These may be used alone or in combination.
[0038] In addition, the acid dianhydride compound that can be used as a raw material monomer for polyamic acid is not particularly limited as long as it can exhibit the effects of the present invention, and examples thereof include pyromellitic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 4,4'-oxyphthalic dianhydride, 3,4'-oxyphthalic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propanoic dianhydride, 3, Examples of the dianhydride include 4,9,10-perylenetetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)propanoic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)ethane dianhydride, oxydiphthalic dianhydride, bis(3,4-dicarboxyphenyl)sulfonic dianhydride, p-phenylene bis(trimellitic acid monoester anhydride), ethylene bis(trimellitic acid monoester anhydride), bisphenol A bis(trimellitic acid monoester anhydride), and the like.
[0039] In the present invention, a film that is easily oriented in-plane exhibits a more excellent effect, and examples of such polyimide films include a film having a polyimide resin with a biphenyl skeleton or a terphenyl skeleton structure. Among them, a polyimide resin made from an acid dianhydride containing 3,3',4,4'-biphenyltetracarboxylic dianhydride and / or 2,2',3,3'-biphenyltetracarboxylic dianhydride and a diamine containing 4,4'-diaminobenzophenone as raw materials, or a polyimide resin made from an acid dianhydride containing 3,3',4,4'-biphenyltetracarboxylic dianhydride and / or 2,2',3,3'-biphenyltetracarboxylic dianhydride and 4,4'-diamino-2,2'-dimethylbiphenyl as raw materials exhibits an excellent effect.
[0040] The polyamic acid of the present invention can be produced by any known method, for example, by the following steps (Aa) to (Ac). Step (Aa): A step of reacting an aromatic diamine with an aromatic acid dianhydride in an organic polar solvent with the aromatic diamine in an excess state to obtain a prepolymer having amino groups at both ends; Step (Ab): A step of additionally adding an aromatic diamine having a structure different from that used in step (Aa); Step (Ac): A step of polymerizing by further adding an aromatic acid dianhydride having a structure different from that used in step (Aa) such that the aromatic diamine and the aromatic acid dianhydride are substantially equimolar in all steps.
[0041] Alternatively, it is also possible to obtain polyamic acid through the following steps (Ba) to (Bc). Step (Ba): a step of reacting an aromatic diamine with an aromatic acid dianhydride in an organic polar solvent in a state where the aromatic acid dianhydride is in excess to obtain a prepolymer having acid anhydride groups at both ends; Step (Bb): A step of additionally adding an aromatic acid dianhydride having a structure different from that used in step (Ba); Step (Bc): A step of polymerizing by further adding an aromatic diamine having a structure different from that used in step (Ba) such that the aromatic diamine and the aromatic acid dianhydride in all steps are substantially equimolar.
[0042] In the present invention, a synthesis method in which the order of addition is determined so that a specific diamine or acid dianhydride is selectively bonded to any diamine or acid dianhydride (for example, steps (Aa) to (Ac) and (Ba) to (Bc)) is called sequence polymerization. In contrast, in the present invention, a synthesis method in which the order of addition of the diamine and acid dianhydride to be bonded is not selected is called random polymerization.
[0043] The solids concentration of the polyamic acid of the present invention is not particularly limited, and is usually 5 to 35 wt %, preferably 10 to 30 wt %. When the concentration is within this range, appropriate molecular weight and solution viscosity are obtained.
[0044] The polyamic acid of the present invention may contain various additives such as fillers, heat stabilizers, antioxidants, ultraviolet absorbers, antistatic agents, flame retardants, pigments, dyes, fatty acid esters, and organic lubricants (e.g., wax). In addition, thermosetting resins such as epoxy resins and phenoxy resins, and thermoplastic resins such as polyether ketone and polyether ether ketone may be mixed within a range that does not impair the properties of the resulting polyimide film. As a method for adding these resins, if they are soluble in a solvent, they may be added to polyamic acid, which is a precursor of polyimide. If the polyimide is also soluble, they may be added to a polyimide solution. If they are insoluble in a solvent, they may be imidized first as a precursor of the non-imide, and then compounded by melt kneading. However, since the solder heat resistance and heat shrinkage rate of the resulting flexible metal-clad laminate may be deteriorated, it is preferable not to use a meltable polyimide in the present invention. Therefore, it is preferable to use a soluble resin to be mixed with polyimide.
[0045] The organic solvent used in the production of polyamic acid can be any solvent that dissolves polyamic acid. For example, amide solvents, i.e., N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, etc. are preferred, and N,N-dimethylformamide and N,N-dimethylacetamide are more preferred. The solid content concentration of polyamic acid is not particularly limited, and if it is within the range of 5% by weight to 35% by weight, a polyamic acid having sufficient mechanical strength when made into a polyimide film can be obtained.
[0046] The order of addition of the raw materials, that is, the aromatic diamine and aromatic acid dianhydride, is not particularly limited, and it is possible to control the properties of the resulting polyimide not only by controlling the chemical structures of the raw materials but also by controlling the order of addition.
[0047] A filler can be added to the polyamic acid for the purpose of improving various film properties such as sliding properties, thermal conductivity, electrical conductivity, corona resistance, loop stiffness, etc. Any filler can be used, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc.
[0048] Thermosetting resins such as epoxy resins and phenoxy resins, and thermoplastic resins such as polyether ketone and polyether ether ketone may be mixed within a range that does not impair the properties of the resulting polyimide film. As a method for adding these resins, if they are soluble in a solvent, they may be added to polyamic acid, which is a precursor of polyimide. If the polyimide is also soluble, they may be added to a polyimide solution. If they are insoluble in a solvent, they may be first imidized as a precursor of polyimide, polyamic acid, and then compounded by melt kneading. However, since the solder heat resistance and heat shrinkage rate of the resulting flexible metal-clad laminate may be deteriorated, it is preferable not to use a meltable polyimide in the present invention. Therefore, it is preferable to use a soluble resin to be mixed with polyimide.
[0049] The polyamic acid organic solvent solution thus obtained is cast or coated onto a support and dried to form a gel film, which is a polyamic acid film that has been partially imidized and / or partially dried to the point of being self-supporting.
[0050] There are two known methods for producing polyimide films: thermal imidization and chemical imidization. The thermal imidization method is a method in which a polyamic acid organic solvent solution is cast onto a support as a film-forming dope without using a dehydrating ring-closing agent, and the imidization is promoted by simply heating. On the other hand, the chemical imidization method is a method in which a polyamic acid organic solvent solution to which at least one of a dehydrating ring-closing agent and a catalyst is added as an imidization promoter is used as a film-forming dope to promote imidization. Either method may be used, but the chemical imidization method is more productive. In addition, in the present invention, a film that is easily oriented in-plane exhibits a more excellent effect, so that a more remarkable effect is exhibited when a chemical imidization method is used in which a polyamic acid organic solvent solution to which at least one of a dehydrating ring-closing agent and a catalyst is added as an imidization promoter is used as a film-forming dope. This is because a polyimide film produced by the chemical imidization method is more easily oriented in-plane.
[0051] As the dehydrating ring-closing agent, an acid anhydride such as acetic anhydride can be preferably used. As the catalyst, a tertiary amine such as an aliphatic tertiary amine, an aromatic tertiary amine, or a heterocyclic tertiary amine can be preferably used.
[0052] As the support for casting the polyamic acid organic solvent solution, a glass plate, an aluminum foil, an endless stainless steel belt, a stainless steel drum, etc. can be suitably used.
[0053] The method of the present invention can be applied not only to the production of a monolayer polyimide film by casting or applying one polyamic acid organic solvent solution onto a support and drying it to obtain a gel film, but also to a method of producing a multilayer polyimide film by casting and / or applying a plurality of polyamic acid organic solvent solutions onto a support by coextrusion and drying it to obtain a multilayer gel film.
[0054] <Step of Peeling Off the Gel Film from the Support> After the resin layer is heated on the support to form a self-supporting gel film, the process of peeling the gel film from the support involves setting heating conditions according to the final thickness of the film to be obtained and the production speed, and after at least one of partial imidization and drying is performed, the film is peeled off from the support to obtain a polyamic acid film (hereinafter referred to as the gel film).
[0055] The gel film thus obtained is partially dried and contains solvent, but the residual solvent ratio is (A-B) x 100 / B (%) (In the formula, A and B represent the following.) A: Weight of gel film B: Weight of gel film after heating at 350°C for 10 minutes It is calculated from:
[0056] In the present invention, in order to actively generate the negative bowing phenomenon as described later in detail, the temperature of the first hot air furnace through which the gel film first passes in the tenter heating process is set to a relatively high temperature. However, as one of the means for increasing the negative bowing strain, it is also effective to increase the amount of remaining volatile components in the gel film, and from this viewpoint, the preferable lower limit of the amount of remaining volatile components in the gel film is 60%, more preferably 70%, and particularly preferably 80%. This is because the more solvent contained in the gel film, the more the shrinkage stress acting in the negative direction due to the sudden evaporation of the solvent can be increased.
[0057] On the other hand, the upper limit is preferably 110%, more preferably 100%, and particularly preferably 90%. If the amount of residual volatile components in the gel film exceeds 110%, the gel film has poor self-supporting properties, and may stretch or break as soon as the gel film is transported to a tenter heating furnace, making it difficult to produce the gel film stably.
[0058] <Tenter heating process for fixing the ends of the gel film and subjecting it to heat treatment> The gel film peeled off from the support is then conveyed to the tenter heating step, with both ends held by pin sheets or clips laid on the tenter rails while applying an appropriate tension to the gel film. In the tenter heating step of the present invention, the film is subjected to heat treatment in a heating furnace having at least three furnaces connected in the longitudinal direction of the film. The heating furnace is composed of a hot air heating zone having two or more hot air furnaces and a radiant heat ray heating zone having one or more radiant heat ray heater furnaces arranged subsequent to the hot air heating zone. In this step, the gel film is heated stepwise in the multiple furnaces to complete the volatilization of the remaining volatile components in the gel film and the imidization reaction.
[0059] In the tenter heating process, shrinkage due to the evaporation of the residual solvent, increase in rigidity due to the imidization reaction, and decrease in rigidity due to exposure to high temperatures all work together to produce various expansion and contraction behaviors in each heating zone. After hypothesizing and verifying various factors that may affect the orientation of the film in the tenter heating process, in the present invention, the temperature of the first hot air oven through which the gel film first passes in the tenter heating process is set to the range of 270 to 360°C.
[0060] It has been known for some time that the so-called bowing phenomenon that occurs in the manufacturing process of polyimide films is related to the anisotropic orientation in the width direction of the polyimide film, and in particular, the orientation in the diagonal direction of approximately 45° at the ends has been a problem. In order to suppress the bowing phenomenon as much as possible, after a polyamic acid organic solvent solution is cast or applied on a support and dried to obtain a gel film, the gel film is held at both ends in the width direction and transported to a heating furnace and heated, and the initial heating should be gentle, that is, the difference between the heating on the support and the initial heating temperature in the heating furnace should not be too large. Therefore, for example, in Patent Document 1, the initial heating temperature when transported to the heating furnace is controlled to be 100°C or less than the atmospheric temperature on the support and 150 to 250°C. It is considered that this is intended to suppress the sudden shrinkage of the gel film containing the remaining volatile components in the tenter heating furnace.
[0061] However, in the present invention, on the contrary, the temperature of the first hot air oven through which the gel film passes first in the tenter heating process is set to a higher temperature. According to the conventional thinking, if the gel film is suddenly exposed to a high temperature, the orientation will progress further, so this is a method that should be avoided. However, in the present invention, under the assumption that a negative bowing phenomenon occurs in the first half of the tenter heating process, where both ends of the gel film are fixed and transported through the heating oven, and a positive bowing phenomenon occurs as the film is exposed to a higher temperature to complete imidization, the temperature pattern of each furnace is set to offset the negative bowing strain and the positive bowing strain, so that the positive bowing phenomenon that occurs later is taken into consideration in advance, and rather the first furnace is actively generated to generate a negative bowing strain. Therefore, in the present invention, the initial heating in the tenter heating process is set to a high temperature in order to generate a shrinkage stress due to the volatilization of the solvent and a hardening shrinkage due to the chemical reaction of polyamic acid to polyimide.
[0062] In addition, it is clear from, for example, Patent Document 2 that the storage modulus decreases when the film is exposed to high temperatures in the tenter heating process. However, the technical idea of considering this in relation to the cause of the positive bowing phenomenon and offsetting it with the negative bowing phenomenon that occurs in the first half of the tenter heating process described above is a new one that was discovered independently by the present inventors.
[0063] As a specific means for increasing the negative bowing, as described above in the process of peeling the gel film from the support, in addition to the method of increasing the amount of remaining volatile components in the gel film, means such as increasing the temperature of the first hot air stove are effective, but in consideration of the effects on other physical properties, it is particularly effective to increase the temperature of the first hot air stove. The reason why increasing the temperature of the first hot air stove is effective is that the solvent contained in the gel film rapidly evaporates, thereby increasing the shrinkage stress associated with the evaporation that acts in the negative direction.
[0064] In the first heating zone, the shrinkage of the film due to the evaporation of the residual solvent and the hardening of the film, i.e., the increase in rigidity, due to the progress of imidization are thought to be dominant, and it is thought that negative bowing, in which the center of the film is pulled, occurs toward the latter half.
[0065] The negative bowing caused by the shrinkage of the film is insufficient, and when the temperature exceeds 360°C, the remaining solvent evaporates without sufficient progress of imidization, so that the imidization rate of the obtained film is insufficient and sufficient mechanical strength tends to be not guaranteed. Also, the minimum temperature in the tenter heating step of the present invention is 270°C or higher. In the present invention, the temperature of the furnace installed in the heating furnace refers to the atmospheric temperature whether it is a hot air furnace or a radiant heat heater furnace.
[0066] In the present invention, the heating furnace is composed of a hot air heating zone in which two or more hot air stoves including the first hot air stove are arranged, and a radiant heat ray heating zone in which one or more radiant heat ray heater furnaces are arranged subsequent to the hot air heating zone, and heating is performed stepwise using a plurality of furnaces. However, it is preferable to set the temperature difference between adjacent hot air stoves arranged in the hot air heating zone to 100°C or less, since this further enhances the effects of the present invention. The temperature difference is preferably 70°C or less, more preferably 50°C or less, and even more preferably 30°C or less. After negative bowing strain is generated in the first hot air stove, it is considered that the decrease in rigidity due to the exposure of the film to high temperatures is dominant in the subsequent second hot air stove and onwards, and it is considered that positive bowing (a phenomenon in which the central part of the film is pulled toward the front furnace where rigidity is thought to be relatively maintained) occurs, in which the center part lags behind the ends. Since this positive bowing strain is unavoidable, the temperature difference between adjacent furnaces is reduced from the second hot air stove onwards, so that the positive bowing balances with the negative bowing strain. In other words, it suppresses an excessive increase in positive bowing.
[0067] In order to reduce the positive bowing, it is effective to set the temperature of the latter half of the multiple furnaces arranged in the heating furnace to a relatively low temperature. The present invention is also characterized in that the maximum temperature during stepwise heating is set to 330 to 420°C. In the method for producing a polyimide film of the present invention, heating at the maximum temperature can be performed by a radiant heat ray heating zone in which one or more radiant heat ray heater furnaces are arranged subsequent to the hot air heating zone. Therefore, it is preferable that the maximum temperature in the radiant heat ray heater is 330 to 420°C. The reason why it is most effective to set the maximum temperature as low as 330 to 420°C in this way is that the film can be transported without the elastic modulus of the film decreasing too much. The maximum temperature is preferably 330 to 390°C, more preferably 330 to 360°C.
[0068] After heating in stages in this way until it is finally heated to the highest temperature, it passes through a slow cooling zone and the tenter heating process is completed, finally obtaining a polyimide film. Although the conversion to polyimide is almost complete by heating at this highest temperature, it is considered that the film is no longer elastic but exhibits viscoelastic behavior due to exposure to high temperatures.
[0069] More preferred examples of the heating furnace used in the tenter heating step of the present invention are shown below. First, the number of hot air furnaces in the hot air heating zone must be at least two in terms of efficient heating, but it is preferable that the furnace consists of three hot air furnaces. Of course, it is not prohibited to have four or more hot air furnaces. Also, the number of radiant heat ray heater furnaces in the radiant heat ray heating zone must be at least one, but it is preferable that the furnace consists of two radiant heat ray heater furnaces. Of course, it is not prohibited to have three or more radiant heat ray heater furnaces. The radiant heat ray heater furnace is preferably a far-infrared heater furnace.
[0070] From the viewpoint of suppressing orientation anisotropy, it is preferable to reduce the temperature difference between adjacent furnaces in all hot air furnaces and radiant heat ray heater furnaces arranged in the heating furnace, but from the viewpoint of satisfying the basic properties of the film, a certain degree of temperature difference may be provided between the hot air heating zone and the radiant heat ray heating zone. However, when two or more radiant heat ray heater furnaces are arranged in the radiant heat ray heating zone, it is preferable that the temperature difference between adjacent radiant heat ray heater furnaces is 70° C. or less.
[0071] In the following, a more preferred heating method will be described in detail using an example in which a hot air zone consisting of three hot air furnaces and a radiant heat ray heating zone consisting of two radiant heat ray heater furnaces are arranged, which is the most preferred configuration of the heating furnace in the tenter heating process.
[0072] The hot air heating zone, which consists of three hot air stoves, Brazier , First Heat Brazier The second heat adjacent to Brazier and the second heat Brazier The third heat adjacent to Brazier This is expressed as follows.
[0073] An example of a preferred hot air zone is the first hot air zone. Brazier The temperature of the second heat is 290 to 310 degrees Celsius. Brazier The temperature of the third heat is 340-360℃. Brazier The temperature is 340 to 360° C. In this example, the temperature difference between the first and second hot stoves is preferably 50° C. or less, and the temperature difference between the second and third hot stoves is preferably 30° C. or less.
[0074] Another preferred example is a first heat Brazier The temperature of the second heat is 270 to 290 degrees Celsius. Brazier The temperature of the third heat is 290 to 310 degrees Celsius. Brazier The temperature is 340 to 360° C. In this example, the temperature difference between the first and second hot stoves is preferably 50° C. or less, and the temperature difference between the second and third hot stoves is preferably 30° C. or less.
[0075] Another preferred example is a first heat Brazier The temperature of the second heat is 270 to 290 degrees Celsius. Brazier The temperature of the third heat is 290 to 310 degrees Celsius. Brazier The temperature is 290 to 310° C. In this example, the temperature difference between the first and second hot stoves is preferably 50° C. or less, and the temperature difference between the second and third hot stoves is preferably 30° C. or less.
[0076] Another preferred example is a first heat Brazier The temperature of the second heat is 290 to 310 degrees Celsius. Brazier The temperature of the third heat is 290 to 310 degrees Celsius. BrazierThe temperature is 290 to 310° C. In this example, the temperature difference between the first and second hot stoves is preferably 50° C. or less, and the temperature difference between the second and third hot stoves is preferably 30° C. or less.
[0077] Another preferred example is a first heat Brazier The temperature of the second heat is 310-330℃. Brazier The temperature of the third heat is 290 to 310 degrees Celsius. Brazier The temperature is 290 to 310° C. In this example, the temperature difference between the first and second hot stoves is preferably 50° C. or less, and the temperature difference between the second and third hot stoves is preferably 30° C. or less.
[0078] Another preferred example is a first heat Brazier The temperature of the second heat is 340-360℃. Brazier The temperature of the third heat is 290 to 310 degrees Celsius. Brazier The temperature is 290 to 310° C. In this example, the temperature difference between the first and second hot stoves is preferably 50° C. or less, and the temperature difference between the second and third hot stoves is preferably 30° C. or less.
[0079] Another preferred example is a first heat Brazier The temperature of the second heat is 270 to 310 degrees Celsius. Brazier The temperature of the third heat is 370-390℃. Brazier The temperature is 250 to 370° C. In this example, the temperature difference between the first and second hot stoves is preferably 50° C. or less, and the temperature difference between the second and third hot stoves is preferably 30° C. or less.
[0080] A radiant heat heating zone consisting of two radiant heat heater furnaces is referred to as a first radiant heat heater furnace and a second radiant heat heater furnace adjacent to the first radiant heat heater furnace.
[0081] Next, in one preferred example of a radiant heat ray heating zone, the temperature of the first radiant heat ray heater furnace is 340 to 390° C., and the temperature of the second radiant heat ray heater furnace is 340 to 390° C. In this example, the temperature difference between the first radiant heat ray heater furnace and the second radiant heat ray heater furnace is preferably 30° C. or less.
[0082] In another preferred example of the radiant heat heating zone, the temperature of the first radiant heat heater furnace is 330 to 380° C., and the temperature of the second radiant heat heater furnace is 370 to 420° C. In this example, the temperature difference between the first radiant heat heater furnace and the second radiant heat heater furnace is preferably 30° C. or less.
[0083] In yet another preferred example of the radiant heat heating zone, the temperature of the first radiant heat heater furnace is 370 to 420° C., and the temperature of the second radiant heat heater furnace is 330 to 380° C. In this example, the temperature difference between the first radiant heat heater furnace and the second radiant heat heater furnace is preferably 30° C. or less.
[0084] As explained in detail above, in the manufacturing process of the polyimide film, the polyimide film is subjected to various thermal histories, and therefore the deformation due to bowing changes from moment to moment in each zone.
[0085] In the present invention, it was found that controlling the direction and magnitude of the bowing strain in each heating furnace is essential to suppress orientation anisotropy, and that the strong orientation anisotropy that occurs at the ends can be improved by controlling the temperature of each heating furnace so that these ultimately cancel each other out.
[0086] Based on the above-mentioned concept, the temperature of each furnace in the tenter heating process is set, so that the effect of the present invention is more excellent in the production of polyimide films that are assumed to have a large positive bowing strain. The elastic modulus is high in the relatively low temperature state in the first half of the heating furnace, and tends to decrease as the temperature increases toward the second half of the heating furnace. Due to such a difference in elastic modulus in the conveying direction, the downstream film with a lower elastic modulus is pulled by the upstream film with a higher elastic modulus, resulting in a bowing phenomenon in which the center lags behind the ends. An example of such a film is a polyimide film having a storage elastic modulus of 0.5 GPa or less at 350°C when the dynamic viscoelasticity of the finally obtained polyimide film is measured. A polyimide film having a storage elastic modulus of 0.3 GPa or less exhibits a more excellent effect, and a polyimide film having a storage elastic modulus of 0.2 GPa or less exhibits an even more excellent effect. In a film that is expected to have a large positive bowing strain, the orientation anisotropy of the resulting film can be suppressed by increasing the negative bowing to offset this and suppressing the positive bowing as much as possible.
[0087] Furthermore, the production method of the present invention is more effective in films that are easily oriented in-plane, and examples of such polyimide films include films having a polyimide resin with a biphenyl skeleton or a terphenyl skeleton. EXAMPLES
[0088] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.
[0089] The MOR-c of the polyimide films in the Synthesis Examples, Examples, and Comparative Examples was evaluated as follows.
[0090] (Method for evaluating MOR-c of polyimide film) The polyimide films obtained in the examples and comparative examples were cut into 50 mm x 50 mm pieces from the center, 70 mm from the left end, and 70 mm from the right end, and the molecular orientation state was evaluated. The measurement device was a microwave molecular orientation meter MOA-6015A manufactured by Oji Measurement Instruments Co., Ltd., and MOR-c was obtained. Here, MOR-c is a value obtained by converting the obtained molecular orientation degree MOR into the thickness of the test piece. The obtained results are shown in Table 1.
[0091] (Measurement of storage modulus) Using the obtained monolayer film of the adhesive layer, dynamic viscoelasticity was measured under an air atmosphere using a DDMS6100 manufactured by SII Nanotechnology, and a graph was created in which the storage modulus and loss modulus were plotted against the measurement temperature.The storage modulus and loss modulus at 350°C were read from the graph. Sample measurement range: width 9mm, gripping distance 20mm Measurement temperature range: 0℃~440℃ Heating rate: 3℃ / min Strain amplitude: 10μm ·Measurement frequency; 5Hz Minimum tension / compression force: 100mN Tension / Compression Gain: 1.5 Initial force amplitude: 100mN
[0092] (Synthesis Example 1) 72.1 kg of p-phenylenediamine (hereinafter also referred to as PDA) and 26.5 kg of 1,3-bis(4-aminophenoxy)benzene (hereinafter also referred to as TPE-R) were added to 1785.0 kg of N,N-dimethylformamide (hereinafter also referred to as DMF) and stirred for 5 minutes, and then 176.4 kg of 3,3',4,4'-biphenyltetracarboxylic dianhydride (hereinafter also referred to as BPDA) was gradually added while stirring under a nitrogen atmosphere. After visually confirming that BPDA had dissolved, 30.8 kg of pyromellitic dianhydride (hereinafter also referred to as PMDA) was gradually added and stirred for 30 minutes. Finally, a solution was prepared by dissolving 3.8 kg of PMDA in DMF to a solid concentration of 7.2%, and this solution was gradually added to the above reaction solution while paying attention to the increase in viscosity. When the viscosity at 23°C reached 2000 poise, the addition and stirring were stopped to obtain a polyamic acid solution.
[0093] (Synthesis Example 2) To 1892.0 kg of DMF, 120.0 kg of TPE-R and 37.4 kg of 4,4'-diamino-2,2'-dimethylbiphenyl (hereinafter also referred to as m-TB) were added, and 86.4 kg of BPDA was gradually added while stirring under a nitrogen atmosphere. After visually confirming that BPDA had dissolved, 41.0 kg of PMDA was added and stirred for 30 minutes. A solution was prepared by dissolving 3.8 g of PMDA in DMF to a solid content concentration of 7.2%, and this solution was gradually added to the above reaction solution while paying attention to the increase in viscosity, and polymerization was terminated when the viscosity reached 800 poise.
[0094] Comparative Example 1 Using a three-layer coextrusion three-layer die, the polyamic acid solution obtained in Synthesis Example 2 / polyamic acid solution obtained in Synthesis Example 1 / polyamic acid solution obtained in Synthesis Example 2 were cast on an endless belt at 120°C in a three-layer structure, and the resulting solution was heated and dried for 180 seconds to form a self-supporting gel film with a residual volatile content of 62%. Just before feeding the polyamic acid solution obtained in Synthesis Example 1 into the three-layer die, 40 g of a curing agent (chemical dehydrating agent and imidization catalyst) consisting of acetic anhydride / isoquinoline / DMF (weight ratio 303 / 153 / 144) was added per 100 g of the polyamic acid, and mixed in a mixer. The self-supporting gel film was then peeled off from the support, and both lateral ends were fixed with a tenter and heated for 23 seconds in a first hot air oven at 200°C, 22 seconds in a second hot air oven at 350°C, and 18 seconds in a third hot air oven at 350°C. The film was then heated in a first far-infrared heater furnace at 390°C for 23 seconds and in a second far-infrared heater furnace at 390°C for 22 seconds, and then passed through a slow cooling zone and an end slitting process to obtain a multilayer polyimide film having a width of 2150 mm and thicknesses of 4 μm / 17 μm / 4 μm. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end. The storage modulus of the multilayer polyimide film was 0.2 GPa.
[0095] Comparative Example 2 A multilayer polyimide film having a thickness of 4 μm / 17 μm / 4 μm was obtained in the same manner as in Comparative Example 1, except that the temperature of the first hot air oven was 230° C. However, the amount of remaining volatile components in the gel film was 63% in this comparative example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0096] Example 1 A multilayer polyimide film having a thickness of 4 μm / 17 μm / 4 μm was obtained in the same manner as in Comparative Example 1, except that the temperature of the first hot air furnace was 280° C. However, the amount of remaining volatile components in the gel film was 63% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end. The storage modulus of the multilayer polyimide film was 0.2 GPa.
[0097] Example 2 A multilayer polyimide film having a thickness of 4 μm / 17 μm / 4 μm was obtained in the same manner as in Comparative Example 1, except that the temperature of the first hot air oven was 300° C. However, the amount of remaining volatile components in the gel film was 63% in this comparative example.
[0098] Example 3 Using a three-layer coextrusion three-layer die, the polyamic acid solution obtained in Synthesis Example 2 / polyamic acid solution obtained in Synthesis Example 1 / polyamic acid solution obtained in Synthesis Example 2 were cast onto an endless belt at 100°C in a three-layer structure, and the resulting solution was heated and dried for 180 seconds to form a self-supporting gel film with a residual volatile content of 98%. Just before feeding the polyamic acid solution obtained in Synthesis Example 1 into the three-layer die, 40 g of a curing agent (chemical dehydrating agent and imidization catalyst) consisting of acetic anhydride / isoquinoline / DMF (weight ratio 303 / 153 / 144) was added per 100 g of the polyamic acid, and the mixture was mixed in a mixer. The self-supporting gel film was then peeled off from the support, and both lateral ends were fixed with a tenter and heated for 23 seconds in a first hot air oven at 300°C, 22 seconds in a second hot air oven at 300°C, and 18 seconds in a third hot air oven at 300°C. The film was then heated in a first far-infrared heater furnace at 400°C for 23 seconds and in a second far-infrared heater furnace at 380°C for 22 seconds, and then passed through a slow cooling zone and an edge slitting process to obtain a multilayer polyimide film having a width of 2150 mm and thicknesses of 4 μm / 17 μm / 4 μm. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0099] Example 4 A multilayer polyimide film having a thickness of 4 μm / 17 μm / 4 μm was obtained in the same manner as in Example 3, except that the temperature of the second hot air oven was 350° C. and the temperature of the third hot air oven was 380° C. However, the amount of remaining volatile components in the gel film was 99% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0100] Example 5 Using a three-layer coextrusion three-layer die, the polyamic acid solution obtained in Synthesis Example 2 / polyamic acid solution obtained in Synthesis Example 1 / polyamic acid solution obtained in Synthesis Example 2 were cast on an endless belt at 120°C in a three-layer structure, and the gel film was heated and dried for 180 seconds to form a self-supporting gel film with a residual volatile content of 62%. Just before feeding the polyamic acid solution obtained in Synthesis Example 1 into the three-layer die, 40 g of a curing agent (chemical dehydrating agent and imidization catalyst) consisting of acetic anhydride / isoquinoline / DMF (weight ratio 303 / 153 / 144) was added per 100 g of the polyamic acid, and mixed with a mixer. The self-supporting gel film was then peeled off from the support, and both lateral ends were fixed with a tenter and heated for 23 seconds in a first hot air oven at 280°C, 22 seconds in a second hot air oven at 350°C, and 18 seconds in a third hot air oven at 350°C. The film was then heated in a first far-infrared heater furnace at 390°C for 23 seconds and in a second far-infrared heater furnace at 390°C for 22 seconds, and then passed through a slow-cooling zone and an edge slitting process to obtain a multilayer polyimide film having a width of 2150 mm and thicknesses of 4 μm / 17 μm / 4 μm. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0101] Example 6 A multilayer polyimide film having a thickness of 4 μm / 17 μm / 4 μm was obtained in the same manner as in Example 5, except that the temperature of the second hot air oven was 380° C. The MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end is shown in Table 1. However, the amount of remaining volatile components in the gel film was 61% in this example.
[0102] (Reference example 1) Using a three-layer coextrusion three-layer die, the polyamic acid solution obtained in Synthesis Example 2 / polyamic acid solution obtained in Synthesis Example 1 / polyamic acid solution obtained in Synthesis Example 2 were cast on an endless belt at 120°C in a three-layer structure, and the resulting solution was heated and dried for 180 seconds to form a self-supporting gel film with a residual volatile content of 62%. Just before feeding the polyamic acid solution obtained in Synthesis Example 1 into the three-layer die, 40 g of a curing agent (chemical dehydrating agent and imidization catalyst) consisting of acetic anhydride / isoquinoline / DMF (weight ratio 303 / 153 / 144) was added per 100 g of the polyamic acid, and mixed in a mixer. The self-supporting gel film was then peeled off from the support, and both lateral ends were fixed with a tenter and heated for 23 seconds in a first hot air oven at 200°C, 22 seconds in a second hot air oven at 350°C, and 18 seconds in a third hot air oven at 350°C. The film was then heated in a first far-infrared heater furnace at 370°C for 23 seconds and in a second far-infrared heater furnace at 370°C for 22 seconds, and then passed through a slow cooling zone and an edge slitting process to obtain a multilayer polyimide film having a width of 2150 mm and thicknesses of 4 μm / 17 μm / 4 μm. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0103] (Reference example 2) A multilayer polyimide film having a thickness of 4 μm / 17 μm / 4 μm was obtained in the same manner as in Reference Example 1, except that the temperature of the first far-infrared heater furnace was 420° C. and the temperature of the second far-infrared heater furnace was 420° C. The amount of remaining volatile components in the gel film was 61% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0104] Example 7 Using a three-layer coextrusion three-layer die, the polyamic acid solution obtained in Synthesis Example 2 / polyamic acid solution obtained in Synthesis Example 1 / polyamic acid solution obtained in Synthesis Example 2 were cast onto an endless belt at 90°C in a three-layer structure, and the resulting solution was heated and dried for 240 seconds to form a self-supporting gel film with a residual volatile content of 81%. Just before feeding the polyamic acid solution obtained in Synthesis Example 1 into the three-layer die, 40 g of a curing agent (chemical dehydrating agent and imidization catalyst) consisting of acetic anhydride / isoquinoline / DMF (weight ratio 303 / 153 / 144) was added per 100 g of the polyamic acid, and the mixture was mixed in a mixer. The self-supporting gel film was then peeled off from the support, and both lateral ends were fixed with a tenter and heated for 31 seconds in a first hot air oven at 300°C, 29 seconds in a second hot air oven at 300°C, and 24 seconds in a third hot air oven at 300°C. The film was then heated in a first far-infrared heater furnace at 350°C for 37 seconds and in a second far-infrared heater furnace at 350°C for 36 seconds, and then passed through a slow cooling zone and an edge slitting process to obtain a multilayer polyimide film having a width of 2150 mm and thicknesses of 4 μm / 17 μm / 4 μm. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0105] Example 8 A multilayer polyimide film having a thickness of 4 μm / 17 μm / 4 μm was obtained in the same manner as in Example 7, except that the temperature of the first far-infrared heater furnace was 370° C. and the temperature of the second far-infrared heater furnace was 370° C. However, the amount of remaining volatile components in the gel film was 80% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0106] Example 9 A multilayer polyimide film having a thickness of 4 μm / 17 μm / 4 μm was obtained in the same manner as in Example 7, except that the temperature of the first far-infrared heater furnace was 390° C. and the temperature of the second far-infrared heater furnace was 390° C. However, the amount of remaining volatile components in the gel film was 82% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0107] Example 10 Using a three-layer coextrusion three-layer die, a three-layer structure of polyamic acid solution obtained in Synthesis Example 2 / polyamic acid solution obtained in Synthesis Example 1 / polyamic acid solution obtained in Synthesis Example 2 was cast on an endless belt at 150°C, and heated and dried for 320 seconds to form a self-supporting gel film with a residual volatile content of 60%. Just before feeding the polyamic acid solution obtained in Synthesis Example 1 into the three-layer die, 40g of a curing agent (chemical dehydrating agent and imidization catalyst) consisting of acetic anhydride / isoquinoline / DMF (weight ratio 303 / 153 / 144) was added to 100g of this polyamic acid, and mixed with a mixer. The self-supporting gel film was then peeled off from the support, and both lateral ends were fixed with a tenter and heated for 41 seconds in a first hot air oven at 280°C, 39 seconds in a second hot air oven at 300°C, and 32 seconds in a third hot air oven at 300°C. The film was then heated in a first far-infrared heater furnace at 370°C for 48 seconds and in a second far-infrared heater furnace at 370°C for 47 seconds, and then passed through a slow-cooling zone and an edge slitting process to obtain a multilayer polyimide film having a width of 2150 mm and thicknesses of 8 μm / 34 μm / 8 μm. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0108] Example 11 A multilayer polyimide film having a thickness of 8 μm / 34 μm / 8 μm was obtained in the same manner as in Example 10, except that the temperature of the third hot air oven was 350° C. The amount of remaining volatile components in the gel film was 60% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0109] Example 12 A multilayer polyimide film having a thickness of 8 μm / 34 μm / 8 μm was obtained in the same manner as in Example 10, except that the temperature of the third hot air oven was 380° C. The amount of remaining volatile components in the gel film was 60% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0110] (Example 13) Using a three-layer coextrusion three-layer die, the polyamic acid solution obtained in Synthesis Example 2 / polyamic acid solution obtained in Synthesis Example 1 / polyamic acid solution obtained in Synthesis Example 2 were cast onto an endless belt at 120°C in a three-layer structure, and the resulting solution was heated and dried for 320 seconds to form a self-supporting gel film with a residual volatile content of 70%. Just before feeding the polyamic acid solution obtained in Synthesis Example 1 into the three-layer die, 40 g of a curing agent (chemical dehydrating agent and imidization catalyst) consisting of acetic anhydride / isoquinoline / DMF (weight ratio 303 / 153 / 144) was added per 100 g of the polyamic acid, and the mixture was mixed in a mixer. The self-supporting gel film was then peeled off from the support, and both lateral ends were fixed with a tenter and heated for 41 seconds in a first hot air oven at 280°C, 39 seconds in a second hot air oven at 300°C, and 32 seconds in a third hot air oven at 300°C. The film was then heated in a first far-infrared heater furnace at 370°C for 48 seconds and in a second far-infrared heater furnace at 370°C for 47 seconds, and then passed through a slow-cooling zone and an edge slitting process to obtain a multilayer polyimide film having a width of 2150 mm and thicknesses of 8 μm / 34 μm / 8 μm. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0111] Example 14 A multilayer polyimide film having a thickness of 8 μm / 34 μm / 8 μm was obtained in the same manner as in Example 13, except that the temperature of the first hot air oven was 300° C. The amount of remaining volatile components in the gel film was 70% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0112] Example 15 Using a three-layer coextrusion three-layer die, the polyamic acid solution obtained in Synthesis Example 2 / polyamic acid solution obtained in Synthesis Example 1 / polyamic acid solution obtained in Synthesis Example 2 were cast onto an endless belt at 90°C in a three-layer structure, and the resulting solution was heated and dried for 480 seconds to form a self-supporting gel film with a residual volatile content of 99%. Just before feeding the polyamic acid solution obtained in Synthesis Example 1 into the three-layer die, 40 g of a curing agent (chemical dehydrating agent and imidization catalyst) consisting of acetic anhydride / isoquinoline / DMF (weight ratio 303 / 153 / 144) was added per 100 g of the polyamic acid, and the mixture was mixed in a mixer. The self-supporting gel film was then peeled off from the support, and both lateral ends were fixed with a tenter and heated for 62 seconds in a first hot air oven at 300°C, 58 seconds in a second hot air oven at 300°C, and 48 seconds in a third hot air oven at 300°C. The film was then heated in a first far-infrared heater furnace at 380°C for 73 seconds and in a second far-infrared heater furnace at 350°C for 73 seconds, and then passed through a slow cooling zone and an edge slitting process to obtain a multilayer polyimide film having a width of 2150 mm and thicknesses of 8 μm / 34 μm / 8 μm. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0113] (Example 16) A multilayer polyimide film having a thickness of 8 μm / 34 μm / 8 μm was obtained in the same manner as in Example 15, except that the temperature of the first hot air oven was 320° C. However, the amount of remaining volatile components in the gel film was 91% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0114] (Example 17) Using a three-layer coextrusion three-layer die, the polyamic acid solution obtained in Synthesis Example 2 / polyamic acid solution obtained in Synthesis Example 1 / polyamic acid solution obtained in Synthesis Example 2 were cast on an endless belt at 100°C in a three-layer structure, and the resulting solution was heated and dried for 480 seconds to form a gel film having self-supporting properties with a residual volatile content of 80%. Just before feeding the polyamic acid solution obtained in Synthesis Example 1 into the three-layer die, 40 g of a curing agent (chemical dehydrating agent and imidization catalyst) consisting of acetic anhydride / isoquinoline / DMF (weight ratio 303 / 153 / 144) was added per 100 g of the polyamic acid, and mixed in a mixer. The self-supporting gel film was then peeled off from the support, and both lateral ends were fixed with a tenter and heated for 62 seconds in a first hot air oven at 300°C, 58 seconds in a second hot air oven at 300°C, and 48 seconds in a third hot air oven at 300°C. The film was then heated in a first far-infrared heater furnace at 380°C for 73 seconds and in a second far-infrared heater furnace at 380°C for 73 seconds, and then passed through a slow-cooling zone and an edge slitting process to obtain a multilayer polyimide film having a width of 2150 mm and thicknesses of 8 μm / 34 μm / 8 μm. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0115] (Example 18) A multilayer polyimide film having a thickness of 8 μm / 34 μm / 8 μm was obtained in the same manner as in Example 17, except that the temperature of the first hot air oven was 320° C. However, the amount of remaining volatile components in the gel film was 81% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0116] (Example 19) Using a three-layer coextrusion three-layer die, the polyamic acid solution obtained in Synthesis Example 2 / polyamic acid solution obtained in Synthesis Example 1 / polyamic acid solution obtained in Synthesis Example 2 were cast onto an endless belt at 90°C in a three-layer structure, and the resulting solution was heated and dried for 120 seconds to form a self-supporting gel film with a residual volatile content of 73%. Just before feeding the polyamic acid solution obtained in Synthesis Example 1 into the three-layer die, 40 g of a curing agent (chemical dehydrating agent and imidization catalyst) consisting of acetic anhydride / isoquinoline / DMF (weight ratio 303 / 153 / 144) was added per 100 g of the polyamic acid, and the mixture was mixed in a mixer. The self-supporting gel film was then peeled off from the support, and both lateral ends were fixed with a tenter and heated for 16 seconds in a first hot air oven at 300°C, 15 seconds in a second hot air oven at 300°C, and 12 seconds in a third hot air oven at 300°C. The film was then heated in a first far-infrared heater furnace at 350°C for 19 seconds and in a second far-infrared heater furnace at 350°C for 18 seconds, and then passed through a slow cooling zone and an edge slitting process to obtain a multilayer polyimide film having a width of 2150 mm and thicknesses of 2 μm / 8.5 μm / 2 μm. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0117] (Example 20) A multilayer polyimide film having a thickness of 2 μm / 8.5 μm / 2 μm was obtained in the same manner as in Example 19, except that the temperature of the first far-infrared heater furnace was 370° C. and the temperature of the second far-infrared heater furnace was 370° C. The amount of remaining volatile components in the gel film was 73% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0118] Example 21 A multilayer polyimide film having a thickness of 2 μm / 8.5 μm / 2 μm was obtained in the same manner as in Example 19, except that the temperature of the first far-infrared heater furnace was 400° C. and the temperature of the second far-infrared heater furnace was 380° C. However, the amount of remaining volatile components in the gel film was 74% in this example. Table 1 shows the MOR-c at the center of the obtained multilayer polyimide film, at a position 70 mm from the left end, and at a position 70 mm from the right end.
[0119] From the results of Comparative Examples 1 and 2 and Examples 1 to 21 in Table 1, it can be seen that the molecular orientation of the resulting multilayer polyimide film is excellent when the temperature of the first hot stove is relatively high, such as 270 to 360° C. This is believed to be because the negative bowing can be increased by increasing the temperature of the first hot stove, thereby offsetting the positive bowing.
[0120] Furthermore, from the results of Examples 3 and 4 and Examples 5 and 6 in Table 1, it can be seen that when the temperature difference between adjacent hot stoves is small, and the temperature of the second hot stove in particular is low, the molecular orientation of the resulting multilayer polyimide film is excellent. This is believed to be because the positive bowing generated in the second hot stove can be reduced.
[0121] Furthermore, the results of Examples 10, 11, and 12 in Table 1 show that when the temperature difference between adjacent hot stoves is small, and the temperature of the third hot stove in particular is low, the molecular orientation of the resulting multilayer polyimide film is excellent. This is believed to be because the positive bowing generated in the third hot stove can be reduced.
[0122] Furthermore, from the results of Examples 7, 8, and 9 in Table 1, it can be seen that the lower the temperature of the far-infrared heater furnace set to the maximum temperature, the better the molecular orientation of the resulting multilayer polyimide film. The same can be seen from the results of Examples 19, 20, and 21 in Table 1. This is thought to be because the positive bowing generated in the furnace can be reduced by lowering the temperature of the far-infrared heater furnace set to the maximum temperature. In addition, from the results of Reference Examples 1 and 2, the effect of improving the orientation anisotropy of the film by lowering the temperature set to the maximum temperature can be clearly confirmed. [Table 1]
Claims
1. A gel film preparation process comprising casting or coating a polyamic acid organic solvent solution onto a support and drying to form a gel film which is a polyamic acid film that has been partially imidized and / or partially dried until it has self-supporting properties; peeling the gel film from the support; and a tenter heating step in which the gel film is subjected to a heat treatment while fixing the ends of the gel film and applying tension in the width direction; In a method for producing a polyimide film comprising the steps of: In the tenter heating step, the film is heat-treated in a heating furnace having at least three furnaces connected in the longitudinal direction of the film, The heating furnace is composed of a hot air heating zone in which two or more hot air stoves are arranged, and a radiant heat ray heating zone in which one or more radiant heat ray heater furnaces are arranged subsequent to the hot air heating zone, The temperature of the first hot air oven through which the gel film first passes in the tenter heating process is set in the range of 270 to 360°C, the minimum temperature in the tenter heating process is 270°C or higher, and the temperature of the oven set to the maximum temperature is in the range of 330 to 420°C. A method for producing a polyimide film.
2. A method for producing a polyimide film as described in claim 1, characterized in that the temperature difference between adjacent hot air furnaces arranged in the hot air heating zone is 100°C or less.
3. 2. The method for producing a polyimide film according to claim 1, wherein the temperature difference between adjacent hot air ovens arranged in the hot air heating zone is 70° C. or less.
4. A method for producing a polyimide film described in any one of claims 1 to 3, characterized in that the furnace set to the highest temperature in the tenter heating process is a radiant heat heater furnace.
5. 5. The method for producing a polyimide film according to claim 1, wherein the hot air heating zone has the first hot air stove, a second hot air stove adjacent to the first hot air stove, and a third hot air stove adjacent to the second hot air stove.
6. 6. The method for producing a polyimide film according to claim 5, wherein the temperature of the first hot air oven is in the range of 290 to 310°C, the temperature of the second hot air oven is in the range of 340 to 360°C, and the temperature of the third hot air oven is in the range of 340 to 360°C.
7. 6. The method for producing a polyimide film according to claim 5, wherein the temperature of the first hot air oven is in the range of 270 to 290°C, the temperature of the second hot air oven is in the range of 290 to 310°C, and the temperature of the third hot air oven is in the range of 340 to 360°C.
8. 6. The method for producing a polyimide film according to claim 5, wherein the temperature of the first hot air oven is in the range of 270 to 290°C, the temperature of the second hot air oven is in the range of 290 to 310°C, and the temperature of the third hot air oven is in the range of 290 to 310°C.
9. 6. The method for producing a polyimide film according to claim 5, wherein the temperature of the first hot air oven is in the range of 290 to 310°C, the temperature of the second hot air oven is in the range of 290 to 310°C, and the temperature of the third hot air oven is in the range of 290 to 310°C.
10. 6. The method for producing a polyimide film according to claim 5, wherein the temperature of the first hot air oven is in the range of 310 to 330°C, the temperature of the second hot air oven is in the range of 290 to 310°C, and the temperature of the third hot air oven is in the range of 290 to 310°C.
11. 6. The method for producing a polyimide film according to claim 5, wherein the temperature of the first hot air oven is in the range of 340 to 360°C, the temperature of the second hot air oven is in the range of 290 to 310°C, and the temperature of the third hot air oven is in the range of 290 to 310°C.
12. 6. The method for producing a polyimide film according to claim 5, wherein the temperature of the first hot air oven is in the range of 270 to 310°C, the temperature of the second hot air oven is in the range of 370 to 390°C, and the temperature of the third hot air oven is in the range of 350 to 370°C.
13. 13. The method for producing a polyimide film according to claim 1, wherein the radiant heat ray heating zone has a first radiant heat ray heater furnace and a second radiant heat ray heater furnace adjacent to the first radiant heat ray heater furnace.
14. The method for producing a polyimide film according to claim 13, wherein the temperature difference between the first radiant heat heater furnace and the second radiant heat heater furnace is in the range of 0 to 70°C.
15. The method for producing a polyimide film according to claim 13, wherein the temperature of the first radiant heat heater furnace is in the range of 340 to 390°C, and the temperature of the second radiant heat heater furnace is in the range of 340 to 390°C.
16. The method for producing a polyimide film according to claim 13, wherein the temperature of the first radiant heat heater furnace is in the range of 330 to 380°C, and the temperature of the second radiant heat heater furnace is in the range of 370 to 420°C.
17. The method for producing a polyimide film according to claim 13, wherein the temperature of the first radiant heat heater furnace is in the range of 370 to 420°C, and the temperature of the second radiant heat heater furnace is in the range of 330 to 380°C.
18. A method for producing a polyimide film described in any one of claims 1 to 17, characterized in that the radiant heat ray heater furnace is a far-infrared heater furnace.
19. The method for producing a polyimide film according to any one of claims 1 to 18, characterized in that the storage modulus at 350°C when the dynamic viscoelasticity of the polyimide film is measured is 0.5 GPa or less.
20. The method for producing a polyimide film according to any one of claims 1 to 19, wherein the polyimide film comprises a polyimide resin having a biphenyl skeleton or a terphenyl skeleton structure.
21. The method for producing a polyimide film according to any one of claims 1 to 20, further comprising a step of mixing a curing agent containing an imidization catalyst and a dehydrating agent prior to casting or coating the polyamic acid organic solvent solution on a support.
22. The method for producing a polyimide film according to any one of claims 1 to 21, characterized in that the gel film preparation step comprises casting and / or coating a plurality of polyamic acid organic solvent solutions onto a support by a co-extrusion method, and drying the resulting solution.
Citation Information
Patent Citations
Polyimide film and method for producing the same
JP2003165850A
Method for producing polyimide film
JP2008012776A
Method for producing adhesive film
JP2013032532A
Adhesive film, flexible metal-clad laminate, and processes for producing these
WO2005111164A1
Process for production of polyimide film, polyimide film, and laminate produced using the polyimide film
WO2011145696A1