Ferrite sintered magnet, ferrite particles, bonded magnet, and rotating electric machine
By optimizing the atomic ratios and composition of metal elements in ferrite magnets, particularly with Ca and controlled Si and B contents, the magnets exhibit superior Br and HcJ at room temperature with reduced temperature sensitivity.
Patent Information
- Application Number
- JP2021512075
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2020-03-27
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-03-27
AI Technical Summary
Existing sintered ferrite magnets face challenges in achieving high residual magnetic flux density (Br) and coercive force (HcJ) at room temperature, despite efforts to enhance these properties through element substitution.
The ferrite sintered magnets and particles are formulated with specific atomic ratios of metal elements A, R, Fe, Co, Zn, and B, with Ca as a primary component, and controlled Si and B contents to optimize Br and HcJ, while maintaining a magnetoplumbite crystal structure.
The solution results in ferrite magnets with enhanced Br and HcJ at room temperature, along with a reduced temperature coefficient of HcJ, demonstrating improved magnetic performance.
Smart Images

Figure 0007557458000005 
Figure 0007557458000006 
Figure 0007557458000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to sintered ferrite magnets, ferrite particles, bonded magnets, and rotating electric machines. [Background technology]
[0002] Known magnetic materials used in sintered ferrite magnets include Ba ferrite, Sr ferrite, and Ca ferrite, which have a hexagonal crystal structure. Known crystal structures of such ferrite include magnetoplumbite type (M type) and W type. Among these, magnetoplumbite type (M type) ferrite is mainly used as a magnet material for motors, etc. M type ferrite is usually made of AFe 12 O 19 It is expressed by the general formula:
[0003] Residual magnetic flux density (Br) and coercive force (HcJ) are generally used as indicators of the magnetic properties of sintered ferrite magnets. In the past, attempts have been made to add various elements different from the constituent elements of ferrite in order to improve Br and HcJ. For example, Patent Document 1 attempts to improve the magnetic properties by substituting some of the elements in the A site with Ca and rare earth elements (R) and some of the elements in the B site with Co. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2018 / 117261 Summary of the Invention [Problem to be solved by the invention]
[0005] However, there is a demand for higher Br and HcJ at room temperature.
[0006] In view of the above, one object of the present invention is to provide a sintered ferrite magnet or the like that is excellent in Br and HcJ at room temperature. [Means for solving the problem]
[0007] The sintered ferrite magnet according to the present invention has a ferrite phase with a magnetoplumbite crystal structure. This magnet contains at least metal element A, metal elements R, Fe, Co, Zn, and B. The metal element A is at least one element selected from the group consisting of Sr, Ba, Ca, and Pb, and necessarily contains Ca. The metal element R is at least one element selected from the group consisting of rare earth elements including Y and Bi, and necessarily includes La. When the atomic ratio of the metal elements is expressed by formula (1), this sintered ferrite magnet has the following: r, x, y, and z satisfy the following formulas (2) to (5). A 1-r R r Fe x Co y Zinc z (1) 0.40≦r≦0.70 (2) 8.20≦x≦9.34 (3) 0.05 <y≦0.50 (4) 0 <z≦0.20 (5) Furthermore, this sintered ferrite magnet has a Si content of 0 to 0.60 mass % calculated as SiO2, and a B content of 0.01 to 0.70 mass % calculated as B2O3.
[0008] Here, the Si content may be 0.01 to 0.40 mass % in terms of SiO2, and the B content may be 0.20 to 0.70 mass % in terms of B2O3. In the sintered ferrite magnet, 95 atomic % or more of the metal element A can be Ca.
[0009] A rotating electric machine of the present invention includes any one of the sintered ferrite magnets described above.
[0010] The ferrite particles according to the present invention are ferrite particles having a ferrite phase with a magnetoplumbite crystal structure. The ferrite particles contain at least a metal element A, a metal element R, Fe, Co, Zn, and B. The metal element A is at least one element selected from the group consisting of Sr, Ba, Ca, and Pb, and necessarily contains Ca. The metal element R is at least one element selected from the group consisting of rare earth elements including Y and Bi, and necessarily includes La. When the atomic ratio of metal elements is expressed by formula (1), ferrite particles are r, x, y, and z satisfy the following formulas (2) to (5). A 1-r R r Fe x Co y Zinc z (1) 0.40≦r≦0.70 (2) 8.20≦x≦9.34 (3) 0.05 <y≦0.50 (4) 0 <z≦0.20 (5) Furthermore, the ferrite particles have a Si content of 0 to 0.60 mass % calculated as SiO2, and a B content of 0.01 to 0.70 mass % calculated as B2O3.
[0011] Here, the Si content may be 0.01 to 0.40 mass % in terms of SiO2, and the B content may be 0.20 to 0.70 mass % in terms of B2O3. In the ferrite particles, Ca may account for 95 atomic % or more of the metal element A.
[0012] The bonded magnet according to the present invention contains any of the ferrite particles described above. A rotating electrical machine according to the present invention includes the bonded magnet described above.
[0013] Another sintered ferrite magnet or ferrite particle according to the present invention is a sintered ferrite magnet or ferrite particle having a ferrite phase with a magnetoplumbite type crystal structure, Contains at least a metal element A, a metal element R, Fe, Co, Zn, Si, and B; The metal element A is at least one element selected from the group consisting of Sr, Ba, Ca, and Pb, and must contain Ca; The metal element R is at least one element selected from the group consisting of rare earth elements including Y and Bi, and must include La; When the atomic ratio of metal elements is expressed by formula (1), r, x, y, and z satisfy the following formulas (2) to (5): A 1-r R r Fe x Co y Zinc z (1) 0.300 <r<0.800 (2) 8.200 <x≦9.340 (3) 0 <y<0.500 (4) 0 <z<0.200 (5) The Si content is 0.010 to 0.400 mass % in terms of SiO2, and the B content is 0.200 to 0.700 mass % in terms of B2O3. Effect of the Invention
[0014] According to the present invention, there are provided sintered ferrite magnets and the like that are excellent in Br and HcJ at room temperature. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic cross-sectional view of a sintered ferrite magnet. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an embodiment of the motor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Several embodiments of the present invention are described in detail below.
[0017] The sintered ferrite magnet and ferrite particles according to the embodiments of the present invention are sintered ferrite magnets having a ferrite phase with a magnetoplumbite type crystal structure. The sintered ferrite magnet and ferrite particles contain at least the metal element A, the metal elements R, Fe, Co, Zn, and B. The metal element A is at least one element selected from the group consisting of Sr, Ba, Ca, and Pb, and necessarily contains Ca.
[0018] From the viewpoint of suppressing the temperature coefficients of Br and HcJ, the atomic ratio of Ca in the metal element A can be 50 atomic % or more, 70 atomic % or more, 90 atomic % or more, 95 atomic % or more, 97 atomic % or more, 99 atomic % or more, or even 100 atomic %. There is no particular limitation on the ratio of atoms other than Ca in the metal element A.
[0019] The metal element R is at least one element selected from the group consisting of rare earth elements including Y and Bi, and necessarily includes La.
[0020] The rare earth elements are yttrium (Y), scandium (Sc), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0021] The metal element R preferably contains one or more elements selected from the group consisting of La (lanthanum), Pr (praseodymium), and Nd (neodymium), and more preferably necessarily contains La. The metal element R may contain 50 atomic % or more of La, 95 atomic % or more of La, 99 atomic % or more of La, or even 100 atomic % of La.
[0022] In the sintered ferrite magnet and ferrite particles according to the embodiments of the present invention, when the atomic ratio of metal elements is expressed by formula (1), r, x, y, and z satisfy the following formulas (2) to (5). A 1-r R r Fe x Co y Zinc z (1) 0.40≦r≦0.70 (2) 8.20≦x≦9.34 (3) 0.05 <y≦0.50 (4) 0 <z≦0.20 (5)
[0023] In the general formula (1), r may be 0.45 or more from the viewpoint of further increasing Br and HcJ, and from the same viewpoint, r may be 0.60 or less, or 0.55 or less.
[0024] In general formula (1), x may be 8.3 or more, or may be 8.5 or more, from the viewpoint of further increasing Br. In general formula (1), x may be 9.3 or less, 9.2 or less, or may be 9.15 or less, from the viewpoint of further increasing Br and HcJ.
[0025] From the viewpoint of further increasing Br, y in general formula (1) may be 0.45 or less, or may be 0.4 or less. From the same viewpoint, y in general formula (1) may be 0.1 or more, or may be 0.2 or more.
[0026] In order to further increase Br and HcJ, z in general formula (1) may be 0.001 or more, 0.002 or more, 0.003 or more, 0.005, 0.01 or more, or 0.05 or more. In order to increase HcJ and decrease the absolute value of the temperature coefficient of HcJ, z in general formula (1) may be 0.15 or less, or 0.1 or less.
[0027] The Si content in the sintered ferrite magnet and ferrite particles according to the embodiment of the present invention is 0 to 0.60 mass% or may be 0.01 to 0.40 mass% in terms of SiO2, and the B content is 0.01 to 0.70 mass% or may be 0.20 to 0.70 mass% in terms of B2O3. The sintered ferrite magnet does not have to contain Si.
[0028] From the viewpoint of further increasing Br and HcJ, the Si content in the sintered ferrite magnet and ferrite particles, calculated as Si in terms of SiO2, may be, for example, 0.01 mass% or more, 0.02 mass% or more, 0.05 mass% or more, 0.1 mass% or more, or 0.2 mass% or more. From the same viewpoint, the Si content in the sintered ferrite magnet and ferrite particles, calculated as Si in terms of SiO2, may be 0.5 mass% or less, 0.4 mass% or less, or 0.35 mass% or less.
[0029] The B content in the sintered ferrite magnet and ferrite particles may be 0.1 mass% or more, 0.2 mass% or more, 0.3 mass% or more, or 0.4 mass% or more, calculated as B2O3, from the viewpoint of increasing Br and HcJ. From the same viewpoint, the B content may be 0.65 mass% or less, or 0.6 mass% or less.
[0030] The ferrite sintered magnet and ferrite particles of this embodiment may further contain other subcomponents in addition to Bi and Si as subcomponents. For example, the ferrite sintered magnet of this embodiment may contain Ca as a subcomponent. However, as described above, the ferrite sintered magnet of this embodiment contains Ca as a component constituting the ferrite phase, which is the main phase. Therefore, when Ca is contained as a subcomponent, for example, the amount of Ca analyzed from the sintered body is the total amount of the main phase and the subcomponents. Therefore, when Ca is used as a subcomponent, the atomic ratio of Ca in the metal element A in formula (1) is a value including the subcomponent. The range of the atomic ratio of Ca is specified based on the composition analyzed after sintering, so it can be applied to both cases where Ca is included as a subcomponent and where it is not included.
[0031] In addition to the above-mentioned components, the sintered ferrite magnet and ferrite particles may contain impurities contained in the raw materials or unavoidable components derived from the manufacturing equipment. Examples of such components include Ti (titanium), Cr (chromium), Mn (manganese), Mo (molybdenum), V (vanadium), and Al (aluminum). These components may be contained in the sintered ferrite magnet and ferrite particles as their respective oxides or composite oxides. The auxiliary components may segregate at the grain boundaries of the ferrite crystal grains in the sintered ferrite magnet to form a different phase.
[0032] The content ratio of metal elements in the sintered ferrite magnet and the ferrite particles can be measured by fluorescent X-ray analysis.
[0033] The contents of metalloid elements such as B (boron) and Si (silicon) in the sintered ferrite magnet and ferrite particles can be measured by inductively coupled plasma optical emission spectrometry (ICP optical emission spectrometry).
[0034] Fig. 1 is a cross-sectional schematic diagram of a sintered ferrite magnet (ferrite particle) 100 according to an embodiment of the present invention. As shown in Fig. 1, the sintered ferrite magnet (ferrite particle) 100 according to the embodiment of the present invention has a ferrite phase (crystal grains) 4 having a magnetoplumbite-type (M-type) crystal structure, and a grain boundary phase 6 existing between the ferrite phase (crystal grains) 4.
[0035] M-type ferrite has a hexagonal crystal structure. An example of M-type ferrite is the ferrite represented by the following formula (III): MX 12 O 19 (III) M necessarily contains Ca and may contain Sr and / or Ba. M may contain R. X contains Fe and may contain Co and Zn. In addition, the ratio of M (A site) and X (B site) and the ratio of oxygen (O) in the above formula (III) may deviate slightly from the above-mentioned ranges in reality.
[0036] From the viewpoint of sufficiently enhancing magnetic properties, the sintered ferrite magnet and ferrite particles preferably have the ferrite phase 4 as the main phase. In this specification, "as the main phase" refers to the crystal phase having the largest mass ratio in the sintered ferrite magnet and ferrite particles. The sintered ferrite magnet and ferrite particles may have a crystal phase (heterogeneous phase) different from the main phase. The ratio of the main phase may be 70 mass% or more, 80 mass% or more, 90 mass% or more, or 95 mass% or more.
[0037] The average grain size of the ferrite phase (crystal grains) in the ferrite sintered magnet may be, for example, 5 μm or less, 4.0 μm or less, or 0.5 to 3.0 μm. By having such an average grain size, the coercive force can be further increased. The average grain size of the ferrite phase (crystal grains) can be obtained using an observation image of a cross section by TEM or SEM. Specifically, the cross-sectional area of each main phase particle in a cross section of an SEM or TEM containing several hundred ferrite phases (crystal grains) is obtained by image analysis, and the diameter of a circle having the cross-sectional area (equivalent circle diameter) is defined as the grain size of the main phase particle in the cross section to measure the grain size distribution. From the measured grain size distribution based on the number, the average grain size based on the number of grains of the ferrite phase (crystal grains) is calculated. The average grain size measured in this manner is the average grain size of the ferrite phase.
[0038] The grain boundary phase 6 is mainly composed of oxides. Specifically, examples of oxides include oxides having at least one selected from Si (silicon), B (boron), Ca (calcium), Sr (strontium), Ba (barium), Fe (iron), Mn (manganese), Co, cobalt, Cr (chromium), Zn (zinc), and Al (aluminum), and composite oxides of two or more of these. Examples of such oxides include SiO2, B2O3, CaO, BaO, SrO, Fe2O3, Co3O4, ZnO, Al2O3, MnO, and Cr2O3. In addition, silicate glass may be included. The mass ratio of the oxides can be 90% or more, can be 95% or more, and can be 97% or more.
[0039] In the cross section of the sintered ferrite magnet, the area ratio of the grain boundary phase 6 to the total area of the ferrite phase 4 and the grain boundary phase 6 can be 0.1 to 5%.
[0040] There are no particular limitations on the shape of the sintered ferrite magnet, and it can have a variety of shapes, such as an arc segment shape (C-shape) with curved end faces forming an arc shape, or a flat plate shape.
[0041] The ferrite particles can be obtained, for example, by a pulverization process described later. The average particle size of the ferrite particles is, for example, 0.1 to 7 μm. The average particle size of the ferrite particles can be determined, in the same manner as the average particle size of the crystal grains of the ferrite sintered magnet, by using an image of the ferrite particles observed by a TEM or SEM. Specifically, the area of each main phase particle of an SEM or TEM containing several hundred ferrite particles is determined by image analysis, and the diameter of a circle having this area (equivalent circle diameter) is defined as the particle size of the ferrite particles, and the particle size distribution is measured. From the measured particle size distribution based on the number, the average particle size based on the number of ferrite particles is calculated. The average value thus measured is taken as the average particle size of the ferrite particles.
[0042] The coercive force of the sintered ferrite magnet at 20° C. can be, for example, 4000 Oe or more, and can exceed 4700 Oe. The residual magnetic flux density of the sintered ferrite magnet at 20° C. can be 4000 G or more, and can be 4400 G or more. It is preferable that the sintered ferrite magnet is excellent in both coercive force (HcJ) and residual magnetic flux density (Br).
[0043] The ferrite particles may have a residual magnetic flux density Br of 40 emu / g or more and a coercive force HcJ of 3000 Oe or more at 20°C.
[0044] The absolute value of the temperature coefficient of HcJ of the sintered ferrite magnet and the ferrite particles may be 0.15 [% / °C] or less, or may be 0.1 [% / °C] or less.
[0045] Here, the temperature coefficient β of HcJ is (20℃) is the measured value of HcJ at 20℃ (unit: Oe), (100℃) is defined as follows, assuming that HcJ is the actual measured value (unit: Oe) at 100°C.
[0046] HcJ temperature coefficient β(% / ℃)=[HcJ (100℃) -HcJ (20℃) ] / 80(℃) / HcJ (20℃) ×100
[0047] (action) The sintered ferrite magnet and ferrite particles according to this embodiment contain metal element R, metal element A, Fe, Co, Zn, Si, and B within specified ranges, and therefore can increase both the coercive force and residual magnetic flux density at 20°C.
[0048] The reason for this is believed to be that Zn substitutes for the B site of ferrite, improving Br. It is also believed that the addition of metal element R increases HcJ and Br. It is also believed that the addition of Si and / or Ca densifies the structure and improves density. It is also believed that the addition of B improves HcJ.
[0049] Furthermore, with the sintered ferrite magnet and ferrite particles according to this embodiment, the absolute value of the temperature coefficient of HcJ can be kept low. In particular, the smaller the proportion of Zn (e.g., z is 0.1 or less), the smaller the temperature coefficient of HcJ tends to be (e.g., 0.105% / °C or less).
[0050] (bonded magnet) Next, an embodiment of a bonded magnet will be described below. The bonded magnet of this embodiment contains the above ferrite particles and a resin. Examples of the resin include thermosetting resins such as epoxy resins, phenolic resins, resins having polyaromatic rings, and resins having triazine rings (triazine resins); thermoplastic resins such as styrene-based, olefin-based, urethane-based, polyester-based, and polyamide-based elastomers such as nylon, ionomers, ethylene propylene copolymers (EPM), and ethylene-ethyl acrylate copolymers.
[0051] From the viewpoint of achieving both excellent magnetic properties and excellent shape retention, the resin content in the bonded magnet may be, for example, 0.5 to 10% by mass, or may be 1 to 5% by mass. The resin content in the bonded magnet can be adjusted by changing the resin concentration in the resin-containing solution used during production, or the molding pressure during the production of the compact. From the same viewpoint, the ferrite particle content in the bonded magnet may be, for example, 90 to 99.5% by mass, or may be 95 to 99% by mass.
[0052] There is no particular limitation on the shape of the bonded magnet, and it can be the same as that of a sintered ferrite magnet.
[0053] The sintered ferrite magnets and bonded magnets according to the present embodiment can be used as magnetic field generating components for rotating electric machines such as motors and generators, magnets for speakers and headphones, magnetron tubes, magnetic field generators for MRI, clampers for CD-ROMs, sensors for distributors, sensors for ABS, fuel and oil level sensors, magnet latches, isolators, etc. They can also be used as targets (pellets) when forming the magnetic layer of a magnetic recording medium by a deposition method, a sputtering method, etc.
[0054] (Rotating Electric Machines) 2 shows a motor 200 according to an embodiment of the present invention. The motor 200 includes a stator 31 and a rotor 32. The rotor 32 has a shaft 36 and a rotor core 37. In the motor 200 of this embodiment, a C-shaped sintered ferrite magnet or bonded magnet 100, which is a permanent magnet, is provided in the stator 31, and an electromagnet (coil) is provided in the rotor core 37 of the rotor 32.
[0055] The motor may have a rotor with a sintered ferrite magnet and a stator with an electromagnet (coil). There is no particular limitation on the form of the motor. Another example of a rotating electric machine is a generator having a rotor and a stator. The sintered ferrite magnet can be provided in the rotor or the stator.
[0056] (Manufacturing method of sintered ferrite magnets, etc.) Next, an example of a method for producing ferrite particles, sintered ferrite magnets, and bonded magnets will be described. The manufacturing method described below includes a compounding step, a calcining step, a pulverizing step, a molding step, and a sintering step. Each step will be described in detail below.
[0057] The blending step is a step of preparing a mixed powder for calcination. The mixed powder for calcination may contain ferrite constituent elements, such as metal element A, metal element R, Fe, Co, and Zn. In the blending step, it is preferable to mix and pulverize the mixture of powders containing each element for about 1 to 20 hours using an attritor or a ball mill, etc., to obtain a mixed powder.
[0058] The additive elements such as B and Si may be contained in the powder beforehand, or a separate powder containing the additive elements may be added in the blending step to obtain the mixed powder for calcination. Examples of the separate powder include a powder containing B and a powder containing Si.
[0059] Examples of powders containing each element include the simple substance, oxide, hydroxide, carbonate, nitrate, silicate, and organometallic compound of each element. One powder may contain two or more metal elements, or one powder may substantially contain only one metal element.
[0060] Examples of powders containing Ca are CaCO3 and CaO. Examples of powders containing Sr are SrCO3 and SrO. Examples of powders containing R are La2O3 and La(OH)3. An example of a powder containing Fe is Fe2O3. An example of a powder containing Co is Co3O4. An example of a powder containing Zn is ZnO. An example of a powder containing B is B2O3. An example of a powder containing Si is SiO2.
[0061] The average particle size of the raw material powder is not particularly limited and is, for example, 0.1 to 2.0 μm.
[0062] After the blending step, it is preferable to dry the raw material composition and remove coarse particles using a sieve, if necessary.
[0063] In the calcination step, the raw material composition obtained in the blending step is calcined. Calcination is preferably performed in an oxidizing atmosphere such as air. The calcination temperature may be, for example, 1100 to 1400°C, or 1100 to 1300°C. The calcination time may be, for example, 1 minute to 10 hours, or 1 minute to 3 hours. The ratio of the ferrite phase (M phase) in the calcined powder (ferrite particles) obtained by calcination may be, for example, 70 mass% or more, or 75 mass% or more. This ratio of the ferrite phase can be determined in the same manner as the ratio of the ferrite phase in a ferrite sintered magnet.
[0064] In the pulverization step, the calcined powder that has become granular or lumpy in the calcination step is pulverized. In this way, ferrite particles are obtained. The pulverization step may be performed in two stages, for example, by pulverizing the calcined powder into a coarse powder (coarse pulverization step) and then pulverizing the coarse powder further into fine powder (fine pulverization step).
[0065] The coarse pulverization can be carried out, for example, using a vibration mill or the like until the average particle size of the calcined powder becomes 0.1 to 5.0 μm.
[0066] In the fine pulverization, the coarse powder obtained by the coarse pulverization is further pulverized by a wet attritor, a ball mill, a jet mill, or the like. In the fine pulverization, pulverization is performed so that the average particle size of the obtained fine powder (ferrite particles) is, for example, about 0.08 to 2.0 μm. The specific surface area of the fine powder (measured, for example, by the BET method) is, for example, 7 to 12 m. 2The preferred grinding time varies depending on the grinding method, for example, 30 minutes to 10 hours in the case of a wet attritor, and 10 to 50 hours in the case of wet grinding using a ball mill. The specific surface area of the ferrite particles can be measured using a commercially available BET specific surface area measuring device (manufactured by Mountech, product name: HM Model-1210).
[0067] In the fine grinding process, in order to increase the degree of magnetic orientation of the sintered body obtained after sintering, for example, n (OH) n H n+2 In the general formula, n may be, for example, 4 to 100, or 4 to 30. As the polyhydric alcohol, for example, sorbitol may be mentioned. Furthermore, two or more kinds of polyhydric alcohols may be used in combination. Furthermore, in addition to the polyhydric alcohol, other known dispersing agents may be used in combination.
[0068] When polyhydric alcohol is added, the amount of the polyhydric alcohol added may be, for example, 0.05 to 5.0% by mass, or 0.1 to 3.0% by mass, based on the target material (e.g., coarse powder). The polyhydric alcohol added in the fine pulverization step is thermally decomposed and removed in the firing step described below.
[0069] It is preferable not to mix all of the raw powders in the blending step, but to add some of the raw powders, for example, some of the CaCO3 powder and some or all of the SiO2 powder, in the coarse grinding step and / or fine grinding step. By adding powders containing such components after calcination, it is possible to improve the sinterability in the firing step and improve the magnetic properties. These subcomponents may flow out together with the solvent in the slurry when wet molding, so they can be blended in amounts larger than the target content in the ferrite sintered magnet 100. For example, when a portion of the powder containing Ca is added after calcination, the amount of Ca added, calculated as CaCO3, may be 0.01 mass % or more and 1.60 mass % or less with respect to the entire ferrite magnet.
[0070] In the molding step, the ferrite particles obtained in the pulverization step are molded in a magnetic field to obtain a molded body. The molding can be performed by either dry molding or wet molding. From the viewpoint of increasing the degree of magnetic orientation, it is preferable to perform the wet molding.
[0071] In the case of forming by wet forming, for example, after obtaining a slurry by performing the above-mentioned fine pulverization process in a wet manner, the slurry is concentrated to a predetermined concentration to obtain a slurry for wet forming. Forming can be performed using this slurry for wet forming. The slurry can be concentrated by centrifugation or a filter press. The content of the ferrite particles in the slurry for wet forming is, for example, 30 to 80 mass %. In the slurry, the dispersion medium for dispersing the ferrite particles can be, for example, water. A surfactant such as gluconic acid, a gluconate salt, or sorbitol may be added to the slurry. A non-aqueous solvent may be used as the dispersion medium. An organic solvent such as toluene or xylene may be used as the non-aqueous solvent. In this case, a surfactant such as oleic acid may be added. The slurry for wet forming may be prepared by adding a dispersion medium or the like to the ferrite particles in a dry state after fine pulverization.
[0072] In the wet compaction, the slurry for wet compaction is then compacted in a magnetic field. In this case, the compaction pressure is, for example, 9.8 to 196 MPa (0.1 to 2.0 ton / cm 2 The magnetic field to be applied is, for example, 398 to 1194 kA / m (5 to 15 kOe).
[0073] In the firing (main firing) step, the compact obtained in the compacting step is fired to obtain a sintered ferrite magnet. The compact can be fired in an oxidizing atmosphere such as air. The firing temperature may be, for example, 1050 to 1270°C, or 1080 to 1240°C. The firing time (the time to hold at the firing temperature) is, for example, 0.5 to 3 hours.
[0074] In the firing step, before the sintering temperature is reached, the molded body may be heated, for example, from room temperature to about 100°C at a heating rate of about 0.5°C / min. This allows the molded body to be sufficiently dried before sintering proceeds. Also, the surfactant added in the molding step can be sufficiently removed. These treatments may be performed at the beginning of the firing step, or may be performed separately before the firing step.
[0075] In this way, a ferrite sintered magnet can be manufactured. When manufacturing a bonded magnet instead of a ferrite sintered magnet, the molded body obtained in the above molding process is impregnated with resin and heated to harden the resin, thereby obtaining a bonded magnet. Specifically, the molded body is immersed in a resin-containing solution prepared in advance, and the resin-containing solution is degassed by reducing the pressure in a closed container, allowing the resin-containing solution to penetrate into the voids in the molded body. Thereafter, the molded body is removed from the resin-containing solution, and the excess resin-containing solution adhering to the surface of the molded body is removed. A centrifuge or the like may be used to remove the excess resin-containing solution.
[0076] By placing the molded body in a sealed solution before immersing it in the resin-containing solution and immersing it in a solvent such as toluene while maintaining a reduced pressure atmosphere, degassing is promoted, making it possible to increase the amount of resin impregnated and reduce voids in the molded body.
[0077] The manufacturing methods of the ferrite particles, sintered ferrite magnets, and bonded magnets are not limited to the above examples. For example, when manufacturing a bonded magnet, after carrying out the above-mentioned crushing process, the obtained ferrite particles and resin may be mixed, and the mixture may be molded in a magnetic field to obtain a bonded magnet containing the ferrite particles and resin.
[0078] Also, for example, the molding step and the firing step may be performed in the following order. That is, the molding step may be performed by CIM (Ceramic Injection Molding) molding method or PIM (Powder Injection Molding, a type of powder injection molding). In the CIM molding method, first, dried ferrite particles are heated and kneaded together with a binder resin to form a pellet. This pellet is injection molded in a mold to which a magnetic field is applied to obtain a preform. This preform is subjected to a binder removal treatment to obtain a green body. Next, in the firing step, the binder-removed green body is sintered in the atmosphere at a temperature of preferably 1100 to 1250°C, more preferably 1160 to 1230°C, for about 0.2 to 3 hours to obtain a sintered ferrite magnet. EXAMPLES
[0079] The present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0080] [Manufacturing of sintered ferrite magnets] (Examples 1 to 37 and Comparative Examples 1 to 17) As raw materials, powders of calcium carbonate (CaCO3), barium carbonate (BaCO3), strontium carbonate (SrCO3), lanthanum hydroxide (La(OH)3), iron oxide (Fe2O3), cobalt oxide (Co3O4), and zinc oxide (ZnO) were prepared. These raw material powders were blended so that the atomic ratios were as shown in Tables 1 to 3. However, as described later, a part of calcium carbonate was added during the grinding process, and this amount was deducted in advance. A predetermined amount of boron oxide (B2O3) was added to the blend obtained in this way so that the amount in the ferrite sintered magnet was the amount shown in Tables 1 to 2, and the mixture was mixed and ground using a wet attritor and a ball mill to obtain a slurry (blending process). In each of the examples and comparative examples, the blending ratios of each raw material were changed as shown in Tables 1 to 2 so that ferrite sintered magnets having different compositions were obtained.
[0081] This slurry was dried, and the coarse particles were removed, and then calcined at 1280°C in air to obtain a calcined powder (calcination step). The calcined powder obtained was coarsely pulverized using a small rod vibration mill to obtain a coarse powder. To this coarse powder, silicon oxide (SiO2) powder in an amount of 0.3% by mass relative to the mass of the ferrite sintered magnet, calcium carbonate (CaCO3) powder in an amount of 0.7% by mass, and sorbitol in an amount of 1% by mass were added. After that, the mixture was finely pulverized using a wet ball mill to obtain a slurry containing ferrite particles (pulverization step).
[0082] The water content of the slurry obtained after fine pulverization was adjusted to obtain a slurry for wet compaction. This slurry for wet compaction was compacted using a wet magnetic field molding machine in an applied magnetic field of 796 kA / m (10 kOe) to obtain a cylindrical compact with a diameter of 30 mm and a thickness of 15 mm (compacting step). The compact obtained was dried in air at room temperature, and then sintered in air at 1170°C (sintering (main sintering) step). In this way, a cylindrical ferrite sintered magnet was obtained.
[0083] (Examples 38 and 39) The composition was mixed as shown in Table 3, and the same procedure as in Example 1 was carried out except that the firing (main firing) temperature was 1150°C.
[0084] [Evaluation of sintered ferrite magnets 1] <Evaluation of magnetic properties> After processing the top and bottom surfaces of the sintered ferrite magnets, the Br and HcJ were measured at 20°C using a BH tracer with a maximum applied magnetic field of 29 kOe. In addition, for some of the sintered ferrite magnets, the HcJ was measured at 100°C using a vibrating sample magnetometer, and the temperature coefficient β of HcJ was calculated.
[0085] <Composition analysis> The B (boron) and Si (silicon) contents in sintered ferrite magnets were measured using the following procedure. 0.1 g of a sample of sintered ferrite magnet was mixed with 1 g of sodium peroxide and 1 g of sodium carbonate, and then heated to melt. The melt was dissolved in a solution of 40 ml of pure water and 10 ml of hydrochloric acid, and then pure water was added to make a 100 ml solution. Using this solution, the boron content calculated as B2O3 and the silicon content calculated as SiO2 were determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). A Shimadzu analyzer (instrument name: ICPS 8100CL) was used for the ICP atomic emission spectrometry, and matrix matching was performed for the measurements. The r, x, y, and z in the ferrite were measured by X-ray fluorescence analysis. The results are shown in Tables 1 to 3.
[0086] [Table 1]
[0087] [Table 2]
[0088] [Table 3]
[0089] As shown in Tables 1 to 3, ferrite magnets that satisfy formulas (2) to (5) and have Si and B contents within the specified ranges exhibited excellent Br and HcJ at 20° C. Furthermore, especially when the amount of Zn was small (e.g., z was 0.1 or less), the absolute value of the temperature coefficient β of HcJ was kept low (e.g., 0.105% / ° C. or less).
[0090] The sintered ferrite magnets of Comparative Example 10 and Examples 11, 24, and 28 were also pulverized to particles with an average particle size of about 10 μm, and the Br and HcJ at 20° C. and HcJ at 100° C. were measured using a vibrating sample magnetometer in the same manner as above, and the temperature coefficient β of HcJ was calculated. The results are shown in Table 4. Even in the particulate state, the Br and HcJ at 20° C. were excellent, and when the amount of Zn was small, the absolute value of the temperature coefficient β of HcJ was kept particularly low.
[0091] [Table 4] [Explanation of symbols]
[0092] 4...ferrite phase (main phase), 6...grain boundary phase, 31...stator (stator cover), 32...rotor, 36...shaft, 37...rotor core, 100...ferrite sintered magnet or bonded magnet, 200...motor.
Claims
1. A sintered ferrite magnet having a ferrite phase with a magnetoplumbite type crystal structure, Contains at least a metal element A, a metal element R, Fe, Co, Zn, and B; The metal element A is at least one element selected from the group consisting of Sr, Ba, Ca, and Pb, and must contain Ca; The metal element R is at least one element selected from the group consisting of rare earth elements including Y and Bi, and always includes La; When the atomic ratio of metal elements is expressed by formula (1), r, x, y, and z satisfy the following formulas (2) to (5), A 1-r R r Fe x Co y Zn z (1) 0.40≦r≦0.70 (2) 8.20≦x≦9.2 (3) 0.05<y≦0.50 (4) 0.01≦z≦0.1 (5) The content of Si is SiO 2 In terms of mass%, this is 0 to 0.60% by mass. The content of B is B 2 O 3 This is calculated as 0.20 to 0.70 mass%. A sintered ferrite magnet in which 95 atomic % or more of the metal element A is Ca.
2. The content of Si is SiO 2 The sintered ferrite magnet according to claim 1, wherein the content is 0.01 to 0.40 mass % in terms of total mass.
3. A rotating electrical machine comprising the sintered ferrite magnet according to claim 1 or 2.
4. Ferrite particles having a ferrite phase having a magnetoplumbite type crystal structure, Contains at least a metal element A, a metal element R, Fe, Co, Zn, and B; The metal element A is at least one element selected from the group consisting of Sr, Ba, Ca, and Pb, and must contain Ca; The metal element R is at least one element selected from the group consisting of rare earth elements including Y and Bi, and always includes La; When the atomic ratio of metal elements is expressed by formula (1), r, x, y, and z satisfy the following formulas (2) to (5), A 1-r R r Fe x Co y Zn z (1) 0.40≦r≦0.70 (2) 8.20≦x≦9.2 (3) 0.05<y≦0.50 (4) 0.01≦z≦0.1 (5) The content of Si is SiO 2 In terms of mass%, this is 0 to 0.60% by mass. The content of B is B 2 O 3 This is calculated as 0.20 to 0.70 mass%. Ferrite particles in which Ca accounts for 95 atomic % or more of the metal element A.
5. The content of Si is SiO 2 The ferrite particles according to claim 4, wherein the content is 0.01 to 0.40 mass% in terms of total mass.
6. A bonded magnet comprising the ferrite particles according to claim 4 or 5.
7. A rotating electrical machine comprising the bonded magnet according to claim 6.
Citation Information
Patent Citations
La-Co-Ca-Zn-Mg-Bi permanent magnetic ferrite material and preparation method thereof
CN106587980A
Sintered magnet and motor
JP1999154604A
Manufacturing method of oxidized magnetic material, ferrite grain, bonded magnet, and sintered magnet, and magnetic recording media made of these materials
JP2000223307A
Oxide magnetic material and sintered magnet
JP2006104050A
Ferrite sintered magnet
JP2009246243A