Method for manufacturing solid electrolyte membrane or anode, and solid electrolyte membrane or anode
By using fibrillated polytetrafluoroethylene as a binder in a powder mixture, the method addresses the challenges of high resistance and solvation in solid-state batteries, enabling the production of mechanically stable electrodes with reduced binder content, improving the performance of solid-state batteries.
Patent Information
- Application Number
- JP2021535235
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-18
- Filing Date
- 2019-12-17
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2039-12-17
AI Technical Summary
The fabrication of non-porous thin electrodes or solid electrolyte membranes in solid-state batteries is challenging due to high sintering temperatures and the use of binder solvent mixtures that lead to high electrical and ionic resistance, solvation of underlying layers, and undesirable side reactions.
A method involving a powder mixture of solid electrolyte material and polytetrafluoroethylene (PTFE) is used, with shear forces forming fibrillated PTFE as a binder, allowing for the production of flexible composite layers with reduced binder content, typically less than 1% by weight, which are then processed into solid electrolyte membranes and anode units.
This approach reduces electrical and ionic resistance, prevents binder degradation, and enables the production of self-supporting, mechanically stable electrodes suitable for direct contact with lithium or sodium, enhancing the performance and efficiency of solid-state batteries.
Smart Images

Figure 0007557466000008 
Figure 0007557466000003 
Figure 0007557466000016
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a solid electrolyte membrane or anode, and to a correspondingly produced solid electrolyte membrane or anode. [Background technology]
[0002] Solid-state batteries represent a very promising further development of lithium-ion batteries. In solid-state batteries, instead of a liquid electrolyte, a lithium-ion conductor present as a solid is used as the electrolyte. It simultaneously acts as an ion conductor between the active material particles and as an ion-conducting separator between the anode and the cathode. The key here is the possibility of large-area processing of the powdered electrode mixture and the formation of an intimate contact surface between the solid electrolyte and the active material with as many contact points as possible and as few hollow spaces as possible. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] US Patent Application Publication No. US2016 / 248120 Summary of the Invention [Problem to be solved by the invention]
[0004] Solid-state batteries can be classified in particular with reference to the electrolyte class used (oxide, sulfide, polymer-based). Oxide solid electrolytes have high chemical and mechanical stability. However, processing into non-porous thin electrodes or solid electrolyte membranes is a great challenge due to the high sintering temperatures. Sulfide electrolyte materials can also hardly be deposited on large areas. Different binder-solvent mixtures are used for the anode, cathode and electrolyte layers of the application, for example by wet chemical processes as described in US 2016 / 248120 A1. This is because otherwise solvation of the layers below could occur during the formation of the layers. The relatively high binder content of a few weight percent and the resulting higher electrical and ionic resistance are disadvantageous in such processes.
[0005] It is therefore an object of the present invention to develop components for solid-state batteries on the anode side and a method for their manufacture which avoids the above-mentioned drawbacks, i.e. which can be produced on a large area and which have as low an electrical and ionic resistance as possible. [Means for solving the problem]
[0006] This object is achieved according to the invention by a method according to claim 1, a solid electrolyte membrane according to claim 6 and an anode unit according to claim 7. Advantageous embodiments and further developments are set out in the dependent claims.
[0007] A method for producing a solid electrolyte membrane for a solid-state battery, preferably for an alkali-ion solid-state battery or for a lithium battery or for a sodium battery, includes the steps of producing a powder mixture of a solid electrolyte material and polytetrafluoroethylene (PTFE). By applying a shear force to the powder mixture, at least partially fibrillated polytetrafluoroethylene is formed. The powder mixture is then formed into a flexible composite layer as the solid electrolyte membrane. The powder mixture contains up to 1% by weight of polytetrafluoroethylene.
[0008] The use of fibrillated polytetrafluoroethylene as a binder allows the use of a reduced amount of binder, with the solid electrolyte membrane only needing a small amount of polytetrafluoroethylene, up to 1% by weight, which allows the use of polytetrafluoroethylene as a binder in these cell components, thus improving the electrical properties. Furthermore, the low binder content allows the manufacture and design of solid electrolyte membranes and anode units as battery components exposed to voltages typically below 0.1 V with respect to lithium. Otherwise, the degradation of the binder material PTFE would result in undesirable side reactions. The low binder content reduces the above-mentioned side reactions, allowing for a technically efficient manufacture and design. The core of the invention is the manufacture of solid electrolyte membranes or anode units as battery components exposed to electrochemical potentials close to the electrochemical potential of lithium or sodium, which may be in direct contact with the battery components. Despite the low binder content, a self-supporting and processable membrane can be manufactured. The binder usually degrades below a certain potential, which causes an irreversible loss of capacity (anode) and functionality of the cell components (membrane). The mechanical stability of the electrodes is provided by the outer casing for solid-state batteries after cell assembly and pressing. Thus, the function of the binder is no longer required in the final cell, but is only important during assembly.
[0009] The powder mixture ensures a simple process. Here, the material in the powder mixture is to be understood as a material present in granular form and consisting of a plurality of small particles having a size of up to 5 μm for solid electrolyte membranes and up to 15 μm for active material particles, or a granular or fragmented mixture or bulk material. The powder mixture can be present in dry form for ease of handling. In addition, the powder mixture also does not have flowability as defined in the standard of DIN EN ISO 6186. In the present specification, "dry" is to be understood as the components of the powder mixture being present in a solid form without materials present in a liquid or liquid aggregate state. The powder mixture can be solvent-free and can be prepared without solvent. A "flexible composite layer" is to be understood as a composite layer that can be bent, folded or unfolded up to 180° at room temperature without destruction. A bending radius of 90 to 100 μm is preferred, in particular 100 μm.
[0010] The formation of at least partially fibrillated or alternatively completely fibrillated polytetrafluoroethylene can be carried out by grinding, mixing in a worm shaft or calendar rolling device, kneading device, mortar device, or a combination thereof to ensure effective fibrillation. The formation of at least partially fibrillated polytetrafluoroethylene typically occurs at room temperature. However, in order to reach a binder content of less than 0.5% by weight, the formation is preferably carried out at an elevated temperature of 60 to 100°C, particularly preferably 90 to 100°C, in particular 100°C.
[0011] Forming the powder mixture into a flexible composite layer is typically accomplished by rolling, pressing, or extrusion, although a combination of these methods can also be used.
[0012] The polytetrafluoroethylene may be present in the composite layer as at least partially uniaxially and / or biaxially oriented polytetrafluoroethylene. However, the polytetrafluoroethylene may also be present as fully uniaxially or fully biaxially oriented polytetrafluoroethylene.
[0013] A powder mixture containing a solid electrolyte material at a concentration of 99 to 99.9% by weight and polytetrafluoroethylene at a concentration of 0.1 to 1% by weight can be provided. The powder mixture preferably contains less than 0.5% by weight of polytetrafluoroethylene, particularly preferably 0.1 to 0.4% by weight of polytetrafluoroethylene.
[0014] The solid electrolyte membrane includes a solid electrolyte material and polytetrafluoroethylene, and the solid electrolyte membrane includes up to 1% by weight of polytetrafluoroethylene.
[0015] The above-mentioned method can be used to produce the above-mentioned solid electrolyte membrane, i.e., the above-mentioned solid electrolyte membrane can be produced by the above-mentioned method.
[0016] The solid electrolyte electrode composite is formed from a first active layer and a first current collector, and includes a solid electrolyte membrane formed directly on, i.e., in direct contact with, a first electrode unit formed from a first active layer and a first current collector layer, typically made of a conductive material. The solid electrolyte membrane has the above-mentioned properties. Here, the material to which the term "conductive" is used has a conductivity of 10 at room temperature, e.g., 25° C. 5 It should be understood to be any material having a conductivity greater than S / m.
[0017] The solid electrolyte membrane and the first active layer may form a laminate, i.e. the solid electrolyte membrane may be laminated onto the first active layer.
[0018] The above method can also be used to manufacture an anode unit. In this case, a powder mixture of electrode material, solid electrolyte material, conductive additive and polytetrafluoroethylene is manufactured for the anode unit, and at least partially fibrillated polytetrafluoroethylene is formed by the action of shear forces on the powder mixture. The powder mixture is formed into a layer disposed on a current collector. The layer consists of a composite material of the anode unit, and the powder mixture contains up to 1% by weight of polytetrafluoroethylene.
[0019] The composite layer of the solid electrolyte membrane and the anode unit acting as the second active layer may form a stack, i.e. the solid electrolyte membrane may be stacked on the second active layer.
[0020] For example, an anode unit that can be produced by the methods described for lithium batteries or other solid-state batteries typically includes a conductive current collector and a layer of a composite material disposed on the current collector. The composite material includes an electrode material, a solid electrolyte material, a conductive additive, and polytetrafluoroethylene (PTFE) as a binder. The composite material includes 0.1-1 wt. % polytetrafluoroethylene, which is present as at least partially fibrillated polytetrafluoroethylene.
[0021] By using fibrillated polytetrafluoroethylene as a binder, the amount of binder used can be reduced, the amount of polytetrafluoroethylene used can be reduced, and the electrical properties can be improved. Here, the material for which the term "conductive" is used has a resistance of 10 at room temperature, e.g., 25°C. 6 It should be understood to be any material having a conductivity greater than S / m. The composite materials are typically solvent-free, which allows for simpler processing and simpler application.
[0022] The polytetrafluoroethylene in the composite can be present as at least partially uniaxially and / or biaxially oriented polytetrafluoroethylene to obtain the desired mechanical properties. Of course, the polytetrafluoroethylene can also be present as fully uniaxially oriented or fully biaxially oriented or oriented polytetrafluoroethylene.
[0023] The composite material may contain 60-99% by weight, preferably 100% by weight, of the conductive electrode material. The composite material typically contains at least 0.1% by weight of polytetrafluoroethylene, which is sufficient to be utilized as a binder. The composite material preferably contains less than 0.5% by weight, particularly preferably 0.1-0.4% by weight of polytetrafluoroethylene.
[0024] The conductive electrode materials are lithium, sodium, graphite, non-graphitic and / or non-graphitic carbon materials such as hard carbon, Li4Ti5O 12 , or a mixture of these materials.
[0025] The solid electrolyte material may include materials selected from the group consisting of Li2S-P2S5, Li2S-GeS2, Li2S-B2S3, Li2S-SiS2, Li5PS6Cl, Li2S-P2S5-LiX (X=Cl, Br, I), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-P2S5-Z m S n (wherein m and n are integers and M is selected from P, Si or Ge), Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q(wherein p and q are integers and M is selected from P, Si or Ge), Na2S-P2S5, Na2S-GeS2, Na2S-B2S3, Na6PS5Cl, Na2S-SiS2, Na2S-P2S5-NaX (X=Cl, Br, I), Na2S-P2S5-Na2O, Na2S-P2S5-Na2O-NaI, Na2S-SiS2-NaI, Na2S-SiS2-NaBr, Na2S-SiS2-NaCl, Na2S-SiS2-B2S3-NaI, Na2S-SiS2-P2S5-NaI, Na2S-P2S5-Z m S n (wherein m and n are integers and M is selected from P, Si or Ge), Na2S-SiS2-Na3PO4, Na2S-SiS2-Na p MO q where p and q are integers and M is selected from P, Si or Ge, or a mixture thereof. Lithium may generally be substituted by sodium in all compounds described in this application. The solid electrolyte material is typically present in the powder mixture at a concentration of 13-35% by weight. The composite may contain carbon nanotubes, black carbon, graphite, graphene, and / or carbon fibers as conductive additives at a concentration of 1-5% by weight. The solid electrolyte material is typically an electrochemically active material. The conductive additive may be an electrochemically inactive material.
[0026] The electrode material may include a protective layer formed on the particles of this material. This protective layer should prevent side reactions between the solid electrolyte material and the electrode material. The protective layer may include, for example, Li2O-ZrO2 or other metal oxides. All particles of the electrode material may have a protective layer, typically with a thickness of 2-5 nm. The conductive current collector of the anode unit typically comprises or is formed entirely of an electrically conductive material, preferably nickel, copper, stainless steel, or a corresponding alloy. Alternatively or additionally, the current collector can be formed as a current collector layer, in particular as an area collector or current collector film, preferably with a double-sided coating, as an expanded metal, as a foam, as a woven fabric, as a non-crimp woven fabric or as a current collector layer with a primer layer, where the primer layer can likewise be planar.
[0027] Preferably, the flexible composite layer is formed on a conductive current collector to form a cathode unit. The flexible composite layer and / or the current collector may then be compressed. The formation of the flexible composite layer on the conductive current collector layer is typically performed at a temperature of 60 to 120°C, preferably 80 to 100°C.
[0028] The solid-state battery includes a solid electrolyte electrode composite having the above-mentioned characteristics, in which a second electrode unit including a second active layer and a second carrier film is formed on a surface of the solid electrolyte membrane opposite the first electrode unit.
[0029] The material of the second carrier film is typically different from the material of the first carrier film. [Brief description of the drawings]
[0030] Embodiments of the invention are illustrated in the drawings and will be described below with reference to FIGS. [Figure 1] FIG. 2 is a schematic side view of an anode. [Diagram 2] 2 is a schematic diagram of an anode having a solid electrolyte membrane according to the present invention; [Diagram 3] An anode with a solid electrolyte membrane and a cathode, as shown corresponding to FIG. [Figure 4] Scanning electron micrograph of a dried composite film. [Diagram 5] Discharge voltage profile of the test cells with 0 wt. % binder content. [Figure 6] Discharge voltage profile of test cells with binder content of 0.1 wt % shown corresponding to FIG. [Figure 7]Discharge voltage profile of test cells with binder content of 0.3 wt % shown corresponding to FIG. [Figure 8] Discharge voltage profile of test cells with binder content of 0.7 wt % shown corresponding to FIG. [Figure 9] Discharge voltage profile of test cells with 1 wt. % binder content shown corresponding to FIG. [Figure 10] Nyquist plot of the internal resistance of the test cell. [Figure 11] Scanning electron micrograph of an anode containing graphite, corresponding to FIG. [Figure 12] Scanning electron microscope photograph of the solid electrolyte membrane corresponding to Figure 4. [Figure 13] FIG. 13 is a graph showing the voltage progression over time of a battery cell of a symmetric design. [Figure 14] FIG. 14 corresponds to FIG. 13 and shows the voltage progression of a symmetric battery cell using polytetrafluoroethylene as a binder. [Figure 15] Impedance spectrum of solid electrolyte material. [Figure 16] Voltage curves for the first charge of a graphite dry film electrode combined with an electrolyte dry film and a cathode dry film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] A conductive current collector layer 1 made of aluminum as a substrate or carrier film with a first electrode 2 as a first active layer forming a cathode unit is shown in a schematic side view in FIG. 1. The first electrode 2 is formed in this embodiment from a powdered composite material. The composite material comprises 85 wt. % Lithium Nickel Manganese Cobalt (NCM), 13 wt. % solid electrolyte material such as Li2S-P2S5 or Li6PS5Cl (argyrodite), 2 wt. % conductive carbon nanotubes as conductive additive, and 0.1 wt. % polytetrafluoroethylene as binder. The binder content here is related to the total mass with a ratio of NCM:C:SE of 85:2:13 (SE is the abbreviation for solid electrolyte). The obtained composite material is powdered, dry, solvent-free, but not flowable. The composite material can be mixed in a mortar. In this process, shear forces act on the mixture or powder mixture forming the composite material, which forms fibrils along the force vector. In the next step, the composite is rolled onto a plate with a roller to the desired layer thickness and laminated onto a carrier film 1, which has a thickness of less than 20 μm and may have a carbon primer. The final shaping of the cathode unit is done by stamping or laser cutting.
[0032] The composite material can alternatively be introduced directly into the calender gap as a powder mixture or bulk material without solvent addition. As described in German patent application DE 10 2017 208 220, different rotational speeds are used for the two calender rollers, for example in a ratio of 10:9 to 10:4. The ratio of the rotational speeds is 2:1, for example 10 mm / s:5 mm / s or 20 mm / s:10 mm / s are advantageous. This causes shear forces on the composite material in the gap, which leads to the formation of fibrils along the running direction of the roller. A layer formation occurs on the faster rotating roller. In the next step, the layer is laminated on the substrate film 1 and the final shaping is carried out by stamping or laser cutting. The film formation in the calendar gap furthermore allows a large compression of the included layers during film formation. For this, the particle size distribution of the powder materials used for the composite material is important, which should be adjusted to one another so that the gaps between the larger particles are filled as efficiently as possible with the smaller particles, keeping the porosity low. The density of the film before pressing is therefore 1.7-1.9 g / cm 3 This corresponds to a porosity of 50-55%. The density after pressing or compaction is typically 3.5 g / cm 3 and the porosity up to 10% approaches the ideal porosity of 0%.
[0033] The treatment is advantageously carried out at high temperatures of 60-100 ° C, which is the result of a considerable reduction in the required binder content or binder content. In addition, the solid electrolyte can also be treated at higher temperatures without binding. The cathode unit thus obtained has a layer sequence of substrate membrane 1-first electrode 2. The first electrode 2 typically has the following composition: cathode material: 60-99 wt. %, solid electrolyte material: 13-35 wt. %, conductive additive: 2-5 wt. %. Here, the binder (polytetrafluoroethylene) is 0.1-1 wt. % of the total mass. The above-mentioned pressing is typically carried out as a final step. This is carried out at a pressure of 290-450 MPa, preferably 300 MPa, to ensure the fluidity of the electrolyte. All treatment steps involving the solid electrolyte material are preferably carried out under a protective gas, for example a noble gas, preferably argon, or nitrogen, or dry air with a dew point below -50 ° C.
[0034] Instead of the cathode unit, the anode unit can also be manufactured by the above method. For example, a powder mixture consisting of 60-85% by weight of graphite, 13-35% by weight of solid electrolyte and 2-5% by weight of carbon nanotubes is used and processed as described above for this purpose. As the substrate or current collector layer 1, nickel or stainless steel membrane or copper is used. Polytetrafluoroethylene is added to the powder mixture in a proportion of 0.3-1% by weight of the total mass. Instead of graphite, hard carbon, lithium, lithium alloys, in particular lithium-indium alloys, or silicon can also be used for the anode.
[0035] A cathode unit consisting of a carrier membrane 1 and a first electrode 2 is shown in FIG. 2, which corresponds to FIG. 1, together with a solid electrolyte membrane 3 arranged directly against it. This solid electrolyte membrane 3 is arranged directly against the side or surface of the first electrode 2 opposite to the side or surface against which the carrier membrane 1 is attached directly as a current collector layer. The carrier membrane 1 and the first electrode 2 are arranged on top of each other in the same alignment, i.e. with identical dimensions except for their respective thicknesses, but the solid electrolyte membrane 3 is wider than the first electrode 2. Repeating elements are provided with the same reference numbers in this and the following figures.
[0036] FIG. 3 is a view corresponding to FIG. 1 and FIG. 2, and shows a solid-state battery in which, in addition to the structure shown in FIG. 2, an anode unit is attached to the side located opposite to the side of the solid electrolyte membrane 3. The anode unit is formed by directly contacting a second electrode 4 as a second active layer and a second substrate membrane 5 as a second current collecting layer. The second electrode 4 is directly contacted to the solid electrolyte membrane 3. The solid electrolyte membrane 3, the second electrode 4, and the second carrier membrane 5 are arranged on top of each other in the same alignment, the second carrier membrane 5 has the thinnest thickness, the second electrode 4 has the thickest thickness, and the thickness of the solid electrolyte membrane 3 is between the thickness of the second electrode 4 and the thickness of the second carrier membrane 5. The capacitance is typically adjusted to each other, and the thickness results therefrom. The first electrode can have a thickness of, for example, 100 μm, and the second electrode as a lithium anode is, for example, up to 10 μm. The thicknesses of the first carrier membrane 1 and the second carrier membrane 5 can also be the same.
[0037] The thickness of the first electrode 2 is greater than the thickness of the solid electrolyte membrane 3 and greater than the thickness of the first carrier membrane 1. Battery electrodes for primary and secondary batteries can be produced using the above-mentioned method, preferably with layers of lithium- or sodium-ion compounds, solid-state supercapacitor electrodes or moisture- or solvent-sensitive materials, i.e. with any kind of sulfide electrolyte.
[0038] Here, the solid electrolyte membrane 3 is also formed using the method described above. A powder mixture of more than 99.9% by weight of solid electrolyte and 0.1% by weight of polytetrafluoroethylene is processed in a manner similar to that of cathode production until a membrane is formed. This results in a solid electrolyte membrane having 99-99.9% by weight of solid electrolyte and 0.1-1% by weight of polytetrafluoroethylene.
[0039] The cell stack, shown in the schematic side view of FIG. 3, can be provided with a battery housing configured as a pouch bag or hard case. The stack is then compressed and tensioned to obtain a solid-state battery. This allows all layers of the solid-state battery to be formed with the same binder, to be stacked directly on top of each other, or to be connected in a different way. This allows for uniform and dense interfaces that do not impair the battery performance. Nevertheless, it is possible to combine components manufactured in different ways.
[0040] The above-mentioned method allows the production of electrodes without the addition of solvents: since solid-state batteries are ultimately highly mechanically tensioned for their operation, the binder function is only required for deposition and not for stabilization of the layers in the operation of the completed cell.
[0041] Figure 4 shows a scanning electron micrograph (SEM) of a dried membrane containing NCM, solid electrolyte (SE), and carbon fibers (CNF) in a mass ratio of 85:13:2, and polytetrafluoroethylene (PTFE) at 0.3 wt % of the total mass.
[0042] Figures 5 to 9 show the discharge voltage profiles of the test cells of the above-mentioned solid-state battery. Here, the respective voltages are recorded against the capacity. In Figure 5, the percentage of polytetrafluoroethylene is 0% by weight; in Figure 6, 0.1% by weight; in Figure 7, 0.3% by weight; in Figure 8, 0.7% by weight; and in Figure 10, 1% by weight.
[0043] The impedance measurements are shown in the Nyquist diagram in Figure 10, where the imaginary component is recorded against the real component. The measurement curves show test cells with binder contents of 0.1 wt%, 0.3 wt%, and 1 wt%. The internal resistance of each solid-state battery increases with increasing proportion of polytetrafluoroethylene.
[0044] Scanning electron micrographs are shown in Figures 11 and 12, which correspond to Figure 4. Figure 11 shows the second electrode 4 of the anode unit made from graphite, solid electrolyte material, and 0.7 wt% polytetrafluoroethylene. The solid electrolyte membrane 3 made of solid electrolyte material and 0.7 wt% polytetrafluoroethylene is shown in Figure 12.
[0045] A voltage profile of the symmetric battery cell is shown in Figure 13. The symmetric battery cell, which includes two lithium anodes and one film of solid electrolyte material, was charged at 0.1 mA / cm 2 The battery was charged and discharged for 30 minutes at a current density of 0.01 V for over 200 hours, i.e., galvanostatically cycled. The recorded voltage profile versus time shows that the applied voltage remained stable throughout the measurement.
[0046] The voltage course of a battery cell containing 0.7 wt. % polytetrafluoroethylene in the solid electrolyte dry film is shown in Fig. 14, which corresponds to Fig. 13. The measurement cycle corresponds to that described in relation to Fig. 13, and the applied voltage again remains stable during the measurement. It can be concluded that binder side reactions are negligible.
[0047] Figure 15 shows the impedance spectrum for the conductivity measurement at room temperature of the solid electrolyte material or solid electrolyte. The conductivity of the solid electrolyte film 3 is only slightly reduced due to the small binder weight of 0.7 wt. %. The wet chemical approach reduces the conductivity partially by a factor of 10.
[0048] FIG. 16 shows the voltage course of the first charge of a graphite dry film electrode combined with an electrolyte dry film as the solid electrolyte film 3. The continuous measurement curve is for a binder with a proportion of 0% by weight in the total components, the dashed curve is for a binder with a proportion of 0.3% by weight of polytetrafluoroethylene, and the dotted measurement curve is for a binder with a proportion of 0.7% by weight of polytetrafluoroethylene. The irreversible capacity at lower binder contents drops below 3.4 V. Conversely, more capacity can be stored up to a breakdown voltage of 4.25 V.
[0049] Only the embodiments disclosed in the examples can be combined with each other and claimed separately.
Claims
1. A method for producing a solid electrolyte membrane (3), comprising the steps of: Producing a powder mixture of a solid electrolyte material and polytetrafluoroethylene; forming at least partially fibrillated polytetrafluoroethylene by applying a shear force to the powder mixture; The powder mixture is formed into a flexible composite layer as the solid electrolyte membrane (3); The method, wherein the powder mixture comprises up to 0.7% by weight polytetrafluoroethylene.
2. 10. The method of claim 1, wherein the at least partially fibrillated polytetrafluoroethylene is formed by grinding, mixing in a worm shaft, or mixing in a calendering device, or a combination thereof.
3. 3. The method according to claim 1 or 2, characterized in that the powder mixture is formed into the flexible composite layer by rolling, pressing or extrusion.
4. The method according to any one of claims 1 to 3, characterized in that the powder mixture for the solid electrolyte membrane contains the solid electrolyte material at a concentration of 99.3 to 99.9 wt% and polytetrafluoroethylene at a concentration of 0.1 to 0.7 wt%.
5. The method according to any one of claims 1 to 4, characterized in that the polytetrafluoroethylene is present as fully uniaxially oriented or fully biaxially oriented polytetrafluoroethylene.
6. The method of claim 1, wherein at least partially fibrillated polytetrafluoroethylene is formed by applying a shear force to the powder mixture at a temperature of 60 to 100°C.
7. A method for producing an anode unit for a solid-state battery, comprising the steps of: Producing a powder mixture of an electrode material, a solid electrolyte material, a conductive additive, and polytetrafluoroethylene; forming at least partially fibrillated polytetrafluoroethylene by applying a shear force to the powder mixture; The powder mixture is placed on a current collector layer (5) and molded into a layer of the anode unit composite material (4); The method, wherein the powder mixture comprises up to 0.7% by weight polytetrafluoroethylene.
8. 8. The method of claim 7, wherein the at least partially fibrillated polytetrafluoroethylene is formed by grinding, mixing in a worm shaft, or mixing in a calendering device, or a combination thereof.
9. 9. The method according to claim 7 or 8, characterized in that the powder mixture is formed into the layer by rolling, pressing or extrusion.
10. The method of claim 7, wherein the powder mixture contains polytetrafluoroethylene at a concentration of 0.1 to 0.7% by weight.
11. 11. The method according to any one of claims 7 to 10, characterized in that the polytetrafluoroethylene is present as fully uniaxially oriented or fully biaxially oriented polytetrafluoroethylene.
12. The method of claim 7, wherein at least partially fibrillated polytetrafluoroethylene is formed by applying a shear force to the powder mixture at a temperature of 60 to 100°C.
13. A solid electrolyte membrane (3) comprising a solid electrolyte material and polytetrafluoroethylene, The solid electrolyte membrane (3) contains a maximum of 0.7% by weight of polytetrafluoroethylene, A solid electrolyte membrane, wherein the polytetrafluoroethylene is at least partially present as fibrillated polytetrafluoroethylene.
14. An anode unit comprising: an electrically conductive current collector layer (5); and a layer of a composite material (4) disposed on the current collector layer (5) and containing an electrode material, a solid electrolyte material, a conductive additive, and polytetrafluoroethylene as a binder, the composite material comprises up to 0.7 wt.% polytetrafluoroethylene; The anode unit, wherein the polytetrafluoroethylene is at least partially present as fibrillated polytetrafluoroethylene.
15. 15. The anode unit according to claim 14, wherein the composite material comprises at least 0.1% by weight of polytetrafluoroethylene.
16. 16. The anode unit according to claim 14 or 15, wherein the electrode material includes a protective layer formed on particles of the electrode material.
17. A solid electrolyte electrode composite, in which the solid electrolyte membrane (3) described in claim 13 is formed directly on a first electrode unit formed from a first active layer (2) and a first carrier membrane (1).
18. 18. A solid electrolyte electrode composite according to claim 17, characterized in that the solid electrolyte membrane (3) and the first active layer (2) form a laminate.
19. A solid-state battery comprising the solid electrolyte electrode composite of claim 17 or 18, a current collector layer (5) as a second carrier film and a layer made of a composite material (4) as a second active layer, the current collector layer (5) being formed on a surface of the solid electrolyte membrane (3) opposite to the first electrode unit.
20. 20. Solid-state battery according to claim 19, characterized in that the material of the second carrier film (5) is different from the material of the first carrier film (1).
Citation Information
Patent Citations
Solid electrolyte secondary cell
JP1987254367A
Coin-shaped all solid battery
JP2005056827A
All solid lithium secondary battery and method of manufacturing the same
JP2009164059A
Negative electrode body and lithium ion battery
JP2012164571A
Cathode for lithium-containing batteries and method for producing the same without solvents
JP2015508220A