Anode and zinc secondary battery
The asymmetrical negative electrode design and hydroxide ion conductive separator enhance ion conductivity and reactivity, addressing the cycle performance and dendrite-induced short circuits in zinc secondary batteries, thereby extending their life span.
Patent Information
- Application Number
- JP2023506736
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-15
- Filing Date
- 2021-11-18
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2041-11-18
AI Technical Summary
The charge/discharge cycle performance of zinc secondary batteries is not sufficient, and the formation of zinc dendrites leads to short circuits, reducing the battery's life span.
A negative electrode with an asymmetrical negative electrode active material layer arrangement, where the center of the layer is offset from the negative electrode current collector plate, and a hydroxide ion conductive separator is used to enhance ion conductivity and reactivity, reducing reaction resistance.
The asymmetrical arrangement improves ion conductivity and reactivity, extending the cycle life of the zinc secondary battery by shortening the migration distance of hydroxide ions and reducing reaction resistance.
Smart Images

Figure 0007557613000006 
Figure 0007557613000005 
Figure 0007557613000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative electrode and a zinc secondary battery. [Background technology]
[0002] In zinc secondary batteries such as nickel-zinc secondary batteries and air-zinc secondary batteries, it is known that metallic zinc precipitates in the form of dendrites from the negative electrode during charging, penetrates the voids in the separator such as nonwoven fabric, and reaches the positive electrode, resulting in a short circuit. Such a short circuit caused by zinc dendrites shortens the repeated charge-discharge life.
[0003] In order to address the above problems, a battery has been proposed that includes a layered double hydroxide (LDH) separator that selectively allows hydroxide ions to pass through while preventing the penetration of zinc dendrites. For example, Patent Document 1 (WO 2013 / 118561) discloses that an LDH separator is provided between the positive and negative electrodes in a nickel-zinc secondary battery. In addition, Patent Document 2 (WO 2016 / 076047) discloses a separator structure that includes an LDH separator fitted or joined to a resin outer frame, and that the LDH separator has such high density that it is gas impermeable and / or water impermeable. This document also discloses that the LDH separator can be composited with a porous substrate. Furthermore, Patent Document 3 (WO 2016 / 067884) discloses various methods for obtaining a composite material by forming an LDH dense membrane on the surface of a porous substrate. This method includes a step of uniformly attaching an initiator substance capable of providing an initiator for the crystal growth of LDH to a porous substrate, and subjecting the porous substrate to hydrothermal treatment in a raw aqueous solution to form a dense LDH membrane on the surface of the porous substrate. An LDH separator has also been proposed that achieves further densification by roll pressing a composite material of LDH / porous substrate produced through hydrothermal treatment. For example, Patent Document 4 (International Publication No. 2019 / 124270) discloses an LDH separator that includes a polymeric porous substrate and an LDH filled in the porous substrate, and has a linear transmittance of 1% or more at a wavelength of 1000 nm.
[0004] In addition, although they cannot be called LDH, LDH-like compounds are known as hydroxides and / or oxides with a layered crystal structure similar to LDH, and exhibit hydroxide ion conductive properties similar to LDH and can be collectively called hydroxide ion conductive layered compounds together with LDH. For example, Patent Document 5 (International Publication No. 2020 / 255856) discloses a hydroxide ion conductive separator comprising a porous substrate and a layered double hydroxide (LDH)-like compound that blocks the pores of the porous substrate, the LDH-like compound being a layered crystal structure hydroxide and / or oxide containing Mg and one or more elements including at least Ti selected from the group consisting of Ti, Y, and Al. This hydroxide ion conductive separator is said to have superior alkali resistance and to be able to more effectively suppress short circuits caused by zinc dendrites compared to conventional LDH separators.
[0005] Meanwhile, the negative electrode in a zinc secondary battery includes a negative electrode active material layer and a negative electrode current collector. For example, Patent Document 6 (JP 2020-170652 A) discloses a negative electrode for a zinc battery including a negative electrode current collector, a first negative electrode material layer (including a negative electrode active material) provided on one side of the negative electrode current collector, and a second negative electrode material layer (including a negative electrode active material) provided on the other side of the negative electrode current collector. In this negative electrode, the ratio of the thickness of the second negative electrode material layer to the thickness of the first negative electrode material layer is 0.7 to 1, and the difference in thickness between the two is small. With this configuration, it is possible to suppress the precipitation of ZnO unevenly on one negative electrode material layer, thereby ensuring smooth OH reaction with the opposing positive electrode. - This will enable the transfer of electricity, which is said to result in improved life performance in zinc batteries. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2013 / 118561 [Patent Document 2] International Publication No. 2016 / 076047 [Patent Document 3] International Publication No. 2016 / 067884 [Patent Document 4] International Publication No. 2019 / 124270 [Patent Document 5] International Publication No. 2020 / 255856 [Patent Document 6] JP 2020-170652 A Summary of the Invention
[0007] However, the charge-discharge cycle performance of existing zinc secondary batteries is not necessarily sufficient, and further improvement in the charge-discharge cycle performance is required.
[0008] The present inventors have now discovered that the cycle life of a zinc secondary battery can be extended by arranging the negative electrode active material layer at a thickness ratio that is asymmetric with respect to the negative electrode current collector so that the center of the thickness direction of the negative electrode active material layer is biased relative to a reference plane passing through the center of the thickness direction of the negative electrode current collector.
[0009] Therefore, an object of the present invention is to provide a negative electrode that can extend the cycle life of a zinc secondary battery.
[0010] According to one aspect of the present invention, there is provided a negative electrode for use in a zinc secondary battery, comprising: a negative electrode active material layer including at least one selected from the group consisting of zinc, zinc oxide, a zinc alloy, and a zinc compound, the negative electrode active material layer having a first surface and a second surface; a negative electrode current collector plate embedded in the negative electrode active material layer in parallel to the negative electrode active material layer; Equipped with the first surface is farther from the negative electrode current collector than the second surface, so that a center in a thickness direction of the negative electrode active material layer is biased with respect to a reference plane passing through a center in a thickness direction of the negative electrode current collector; A negative electrode is provided, in which T2 / T1, which is a ratio of a thickness T2 defined as the distance between the second surface and the reference surface to a thickness T1 defined as the distance between the first surface and the reference surface, is greater than 0 and is not greater than 0.5.
[0011] According to another aspect of the present invention, a positive electrode including a positive electrode active material layer and a positive electrode current collector; The negative electrode; a hydroxide ion conductive separator that separates the positive electrode and the negative electrode so as to be capable of conducting hydroxide ions; An electrolyte; wherein the negative electrode is disposed so that the second surface is closer to the hydroxide ion conducting separator. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an example of a negative electrode according to the present invention. [Diagram 2] FIG. 1 is a diagram conceptually illustrating the migration path of hydroxide ions (OH−) in a conventional negative electrode until they reach the surface of a negative electrode current collector plate. [Diagram 3] FIG. 2 is a diagram conceptually illustrating the migration path of hydroxide ions (OH−) in the negative electrode of the present invention until they reach the surface of the negative electrode current collector plate. [Figure 4] 1 is a cross-sectional photograph of the negative electrode (after charge / discharge evaluation) prepared in Example 1 (comparison). [Diagram 5] 1 is a cross-sectional photograph of the negative electrode prepared in Example 4 (after charge / discharge evaluation). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] negative electrode The negative electrode of the present invention is a negative electrode used in a zinc secondary battery. FIG. 1 shows one embodiment of the negative electrode according to the present invention. The negative electrode 10 shown in FIG. 1 includes a negative electrode active material layer 14 and a negative electrode current collector plate 16. The negative electrode active material layer 14 includes at least one selected from the group consisting of zinc, zinc oxide, zinc alloys, and zinc compounds. The negative electrode active material layer 14 has a first surface 14a and a second surface 14b. The negative electrode current collector plate 16 is embedded in the negative electrode active material layer 14 in parallel with the negative electrode active material layer 14. The first surface 14a of the negative electrode active material layer 14 is farther away from the negative electrode current collector plate 16 than the second surface 14b, so that the center of the negative electrode active material layer 14 in the thickness direction is biased with respect to a reference plane P passing through the center of the negative electrode current collector plate 16 in the thickness direction. In other words, the negative electrode active material layer 14 is arranged asymmetrically with respect to the negative electrode current collector plate 16. In particular, T2 / T1, which is the ratio of thickness T2 defined as the distance between second surface 14b of negative electrode active material layer 14 and reference surface P to thickness T1 defined as the distance between first surface 14a of negative electrode active material layer 14 and reference surface P, is greater than 0 and not greater than 0.5. By arranging negative electrode active material layer 14 with a thickness ratio asymmetric with negative electrode current collector 16 in this manner such that the center in the thickness direction of negative electrode active material layer 14 is biased with respect to reference surface P passing through the center in the thickness direction of negative electrode current collector 16, the cycle life of the zinc secondary battery can be extended.
[0014] It is believed that the effect of extending the cycle life is due to the above-mentioned unique asymmetric arrangement, which improves the ionic conductivity and reactivity at the negative electrode 10 and its vicinity. That is, according to the knowledge of the present inventors, in a conventional negative electrode in which the negative electrode active material layer is arranged so as to have an equal thickness ratio on both sides of the negative electrode current collector, the resistance in the battery reaction is higher than in an electrode in which this is not the case. The presumed mechanism for this is as follows. That is, in a conventional negative electrode, as illustrated in FIG. 2, the negative electrode active material 12 (which constitutes the negative electrode active material layer 14) is evenly present around the negative electrode current collector 16. For this reason, hydroxide ions (OH -) to reach the surface of the negative electrode current collector 16, the hydroxide ions must make a detour by weaving through the gaps between many negative electrode active materials 12, as shown by the movement path indicated by the arrow in the figure. In this way, in the conventional negative electrode, the movement distance of the hydroxide ions is long, so the reaction resistance increases and the discharge capacity is impaired. In other words, the discharge reaction ends in a state where the negative electrode active material 12 is not completely changed. If the next charge is performed in this state, the excess capacity is charged, causing irreversible side reactions and the like. As a result, it is considered that the number of times that the battery can be charged and discharged is reduced. In contrast, in the negative electrode 10 of the present invention, the negative electrode active material layer 14 is arranged asymmetrically with respect to the negative electrode current collector 16, as described above. In other words, as shown in FIG. 3, the amount of the negative electrode active material 12 present on one side of the negative electrode current collector 16 (the side closer to the second surface 14b of the negative electrode active material layer 14) is small. For this reason, the hydroxide ions (OH - ) can reach the surface of the negative electrode current collector 16 in a straight line. That is, in the negative electrode 10 of the present invention, the movement distance of the hydroxide ions is shortened, and as a result, the resistance in the battery reaction can be reduced. Therefore, it is considered that the ion conductivity and reactivity are improved in the zinc secondary battery, which makes it possible to extend the cycle life.
[0015] The negative electrode 10 has a ratio T2 / T1 of the thickness T2 to the thickness T1 that is greater than 0 and less than 0.5, preferably greater than 0 and less than 0.2, more preferably 0.01 to 0.1. As described above, this improves the ion conductivity and reactivity of the zinc secondary battery, and increases the cycle life. As described above, the thickness T1 is defined as the distance between the first surface 14a of the negative electrode active material layer 14 and the reference surface P. The thickness T2 is defined as the distance between the second surface 14b of the negative electrode active material layer 14 and the reference surface P. Therefore, the thicknesses T1 and T2 can be measured by cutting out and observing a cross section of the negative electrode 10, setting the reference surface P so as to pass through the center of the negative electrode current collector 16 in the thickness direction, and then measuring the distances from both surfaces (outermost surfaces) of the negative electrode active material layer 14 to the reference surface P. At this time, it goes without saying that the surface of the negative electrode active material layer 14 that is farther from the reference plane P becomes the first surface 14a, and the surface of the negative electrode active material layer 14 that is nearer from the reference plane P becomes the second surface 14b.
[0016] The difference between the thickness T1 and the thickness T2 of the negative electrode 10 is preferably 0.01 mm or more, more preferably 0.04 to 2.0 mm, still more preferably 0.10 to 2.0 mm, and particularly preferably 0.20 to 2.0 mm. This more effectively improves the ion conductivity and reactivity of the zinc secondary battery, and further extends the cycle life.
[0017] The thickness T2 is preferably 0.01 to 1.0 mm, more preferably 0.01 to 0.9 mm, further preferably 0.01 to 0.6 mm, and particularly preferably 0.01 to 0.3 mm. With such a thickness, hydroxide ions (OH - ) can reach the surface of the negative electrode current collector 16 in a more linear manner, and the resistance in the battery reaction can be further reduced. On the other hand, the thickness T1 may be larger than the thickness T2 so as to satisfy the above ratio T2 / T1, and the value is not particularly limited, but is typically 0.02 to 2.0 mm, more typically 0.10 to 2.0 mm, and further typically 0.30 to 2.0 mm.
[0018] The negative electrode 10 includes a negative electrode active material layer 14. The negative electrode active material 12 constituting the negative electrode active material layer 14 includes at least one selected from the group consisting of zinc, zinc oxide, zinc alloys, and zinc compounds. Zinc may be included in any form of zinc metal, zinc compound, or zinc alloy, so long as it has electrochemical activity suitable for a negative electrode. Preferred examples of the negative electrode material include zinc oxide, zinc metal, calcium zincate, and the like, and a mixture of zinc metal and zinc oxide is more preferred. The negative electrode active material 12 may be configured in a gel form, or may be mixed with an electrolyte 18 to form a negative electrode mixture. For example, a gelled negative electrode can be easily obtained by adding an electrolyte and a thickener to the negative electrode active material 12. Examples of the thickener include polyvinyl alcohol, polyacrylate, CMC, alginic acid, and the like, and polyacrylic acid is preferred because it has excellent chemical resistance to strong alkalis.
[0019] As the zinc alloy, a zinc alloy containing no mercury or lead, known as a mercury-free zinc alloy, can be used. For example, a zinc alloy containing 0.01 to 0.1 mass% indium, 0.005 to 0.02 mass% bismuth, and 0.0035 to 0.015 mass% aluminum is preferable because it has an effect of suppressing hydrogen gas generation. In particular, indium and bismuth are advantageous in terms of improving discharge performance. The use of a zinc alloy for the negative electrode can improve safety by suppressing hydrogen gas generation by slowing down the self-dissolution rate in an alkaline electrolyte.
[0020] The shape of the negative electrode material is not particularly limited, but it is preferably in powder form, which increases the surface area and allows for high-current discharge. The average particle size of the negative electrode material is preferably in the range of 3 to 100 μm in minor axis in the case of a zinc alloy, and within this range, the large surface area makes it suitable for high-current discharge, and it is easy to mix uniformly with the electrolyte and gelling agent, and is easy to handle when assembling a battery.
[0021] The negative electrode 10 includes a negative electrode current collector 16 embedded in the negative electrode active material layer 14 in parallel to the negative electrode active material layer 14. The negative electrode current collector 16 is a plate-shaped current collector, and therefore has a desired thickness. It is preferable to use a metal plate having a plurality (or a large number) of openings as the negative electrode current collector 16 from the viewpoint of active material adhesion. Preferred examples of such a negative electrode current collector 16 include expanded metal, punched metal, metal mesh, and combinations thereof, more preferably copper expanded metal, copper punched metal, and combinations thereof, and particularly preferably copper expanded metal. In this case, for example, a negative electrode active material sheet containing zinc oxide powder and / or zinc powder, and optionally a binder (e.g. polytetrafluoroethylene particles) can be pressed onto the copper expanded metal to preferably produce a negative electrode consisting of a negative electrode active material layer / negative electrode current collector. At that time, the ratio T2 / T1 can be controlled by pressing negative electrode active material sheets of different thicknesses onto both sides of the copper expanded metal. Expanded metal is a mesh-like metal plate made by expanding a metal plate while making staggered cuts in it using an expansion machine, and then forming the cuts into a diamond or tortoiseshell shape. Punched metal is also called perforated metal, and is made by punching holes in a metal plate. Metal mesh is a metal product with a wire mesh structure, and is different from expanded metal and punched metal.
[0022] Zinc secondary battery The negative electrode 10 of the present invention is preferably applied to a zinc secondary battery. Therefore, according to a preferred embodiment of the present invention, a zinc secondary battery is provided, which includes a positive electrode including a positive electrode active material layer and a positive electrode current collector, a negative electrode 10, a hydroxide ion conductive separator that separates the positive electrode and the negative electrode 10 so that hydroxide ions can be conducted, and an electrolyte 18. In this zinc secondary battery, the negative electrode 10 is arranged so that the second surface 14b of the negative electrode active material layer 14 is closer to the hydroxide ion conductive separator. With such an arrangement, the amount of the negative electrode active material 12 present between the negative electrode current collector 16 and the hydroxide ion conductive separator is reduced. This allows hydroxide ions that have permeated the hydroxide ion conductive separator to quickly reach the surface of the negative electrode current collector 16, thereby reducing the reaction resistance and lengthening the cycle life.
[0023] The zinc secondary battery of the present invention is not particularly limited as long as it is a secondary battery using the above-mentioned negative electrode 10 and the electrolyte 18 (typically an aqueous alkali metal hydroxide solution). Therefore, it can be a nickel-zinc secondary battery, a silver oxide zinc secondary battery, a manganese oxide zinc secondary battery, a zinc-air secondary battery, or any other type of alkaline zinc secondary battery. For example, it is preferable that the positive electrode active material layer contains nickel hydroxide and / or nickel oxyhydroxide, thereby making the zinc secondary battery a nickel-zinc secondary battery. Alternatively, the positive electrode active material layer may be an air electrode layer, thereby making the zinc secondary battery an air-zinc secondary battery.
[0024] The hydroxide ion conductive separator is not particularly limited as long as it is a separator capable of isolating the positive electrode and the negative electrode 10 in a hydroxide ion conductive manner, but is typically a separator that contains a hydroxide ion conductive solid electrolyte and selectively passes hydroxide ions solely by utilizing hydroxide ion conductivity. A preferred hydroxide ion conductive solid electrolyte is a layered double hydroxide (LDH) and / or an LDH-like compound. Therefore, the hydroxide ion conductive separator is preferably an LDH separator. In this specification, an "LDH separator" is defined as a separator that contains LDH and / or an LDH-like compound and selectively passes hydroxide ions solely by utilizing the hydroxide ion conductivity of LDH and / or an LDH-like compound. In this specification, an "LDH-like compound" is a hydroxide and / or oxide with a layered crystal structure similar to LDH, which may not be called LDH, and can be said to be equivalent to LDH. However, in a broad definition, "LDH" can also be interpreted as including not only LDH but also LDH-like compounds. The LDH separator is preferably composited with a porous substrate. Therefore, the LDH separator preferably further comprises a porous substrate, and is composited with the porous substrate in a form in which the pores of the porous substrate are filled with LDH and / or LDH-like compounds. That is, in a preferred LDH separator, the pores of the porous substrate are blocked with LDH and / or LDH-like compounds so as to exhibit hydroxide ion conductivity and gas impermeability (and therefore function as an LDH separator exhibiting hydroxide ion conductivity). The porous substrate is preferably made of a polymer material, and it is particularly preferred that the LDH is incorporated over the entire thickness of the porous substrate made of a polymer material. For example, known LDH separators as disclosed in Patent Documents 1 to 5 can be used. The thickness of the LDH separator is preferably 3 to 80 μm, more preferably 3 to 60 μm, and even more preferably 3 to 40 μm.
[0025] The electrolyte 18 preferably contains an aqueous solution of an alkali metal hydroxide. Examples of the alkali metal hydroxide include potassium hydroxide, sodium hydroxide, lithium hydroxide, and ammonium hydroxide, with potassium hydroxide being more preferred. Zinc oxide, zinc hydroxide, and the like may be added to the electrolyte to suppress self-dissolution of the zinc-containing material.
[0026] LDH-like compounds According to a preferred embodiment of the present invention, the LDH separator may contain an LDH-like compound. The definition of the LDH-like compound is as described above. Preferred LDH-like compounds are: (a) a hydroxide and / or oxide having a layered crystal structure containing Mg and one or more elements including at least Ti selected from the group consisting of Ti, Y, and Al, or (b) a hydroxide and / or oxide having a layered crystal structure containing (i) Ti, Y, and optionally Al and / or Mg, and (ii) an additional element M which is at least one selected from the group consisting of In, Bi, Ca, Sr, and Ba; or (c) A hydroxide and / or oxide having a layered crystal structure containing Mg, Ti, Y, and optionally Al and / or In, in which the LDH-like compound is present in the form of a mixture with In(OH)3.
[0027] According to a preferred embodiment (a) of the present invention, the LDH-like compound may be a hydroxide and / or oxide having a layered crystal structure containing Mg and one or more elements including at least Ti selected from the group consisting of Ti, Y, and Al. Thus, a typical LDH-like compound is a composite hydroxide and / or composite oxide of Mg, Ti, optionally Y, and optionally Al. The above elements may be replaced with other elements or ions to the extent that the basic properties of the LDH-like compound are not impaired, but it is preferable that the LDH-like compound does not contain Ni. For example, the LDH-like compound may further contain Zn and / or K. This can further improve the ionic conductivity of the LDH separator.
[0028] The LDH-like compound can be identified by X-ray diffraction. Specifically, when X-ray diffraction is performed on the surface of the LDH separator, a peak derived from the LDH-like compound is typically detected in the range of 5°≦2θ≦10°, more typically in the range of 7°≦2θ≦10°. As described above, LDH is a substance having an alternating laminate structure in which exchangeable anions and H2O exist as intermediate layers between stacked hydroxide basic layers. In this regard, when LDH is measured by X-ray diffraction, a peak due to the crystal structure of LDH (i.e., the (003) peak of LDH) is essentially detected at a position of 2θ=11 to 12°. In contrast, when an LDH-like compound is measured by X-ray diffraction, a peak is typically detected in the above-mentioned range shifted to the lower angle side from the above-mentioned peak position of LDH. In addition, the interlayer distance of the layered crystal structure can be determined by the Bragg formula using 2θ corresponding to the peak derived from the LDH-like compound in X-ray diffraction. The interlayer distance of the layered crystal structure constituting the LDH-like compound thus determined is typically 0.883 to 1.8 nm, and more typically 0.883 to 1.3 nm.
[0029] In the LDH separator according to the above aspect (a), the atomic ratio of Mg / (Mg+Ti+Y+Al) in the LDH-like compound determined by energy dispersive X-ray analysis (EDS) is preferably 0.03 to 0.25, more preferably 0.05 to 0.2. The atomic ratio of Ti / (Mg+Ti+Y+Al) in the LDH-like compound is preferably 0.40 to 0.97, more preferably 0.47 to 0.94. The atomic ratio of Y / (Mg+Ti+Y+Al) in the LDH-like compound is preferably 0 to 0.45, more preferably 0 to 0.37. The atomic ratio of Al / (Mg+Ti+Y+Al) in the LDH-like compound is preferably 0 to 0.05, more preferably 0 to 0.03. Within the above ranges, the alkali resistance is more excellent, and the effect of suppressing short circuits caused by zinc dendrites (i.e., dendrite resistance) can be more effectively realized. Regarding LDH separators, conventionally known LDHs have the general formula: M 2+ 1-x M3+ x (OH)2A n- x / n ·mH2O (in the formula, M 2+ is a divalent cation, M 3+ is a trivalent cation, and A n- is an n-valent anion, n is an integer of 1 or more, x is 0.1 to 0.4, and m is 0 or more). In contrast, the above atomic ratio in the LDH-like compound generally deviates from the above general formula of LDH. For this reason, it can be said that the LDH-like compound in this embodiment generally has a composition ratio (atomic ratio) different from that of conventional LDH. It is preferable to perform the EDS analysis using an EDS analyzer (e.g., X-act, manufactured by Oxford Instruments) by 1) capturing an image at an accelerating voltage of 20 kV and a magnification of 5,000 times, 2) performing three-point analysis with an interval of about 5 μm in the point analysis mode, 3) repeating the above 1) and 2) once more, and 4) calculating the average value of a total of six points.
[0030] According to another preferred embodiment (b) of the present invention, the LDH-like compound may be a hydroxide and / or oxide having a layered crystal structure, comprising (i) Ti, Y, and optionally Al and / or Mg, and (ii) an additional element M. Thus, a typical LDH-like compound is a composite hydroxide and / or composite oxide of Ti, Y, the additional element M, optionally Al, and optionally Mg. The additional element M is In, Bi, Ca, Sr, Ba, or a combination thereof. The above elements may be replaced with other elements or ions to the extent that the basic properties of the LDH-like compound are not impaired, but it is preferred that the LDH-like compound does not contain Ni.
[0031] In the LDH separator according to the above aspect (b), the atomic ratio of Ti / (Mg+Al+Ti+Y+M) in the LDH-like compound determined by energy dispersive X-ray analysis (EDS) is preferably 0.50 to 0.85, more preferably 0.56 to 0.81. The atomic ratio of Y / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0.03 to 0.20, more preferably 0.07 to 0.15. The atomic ratio of M / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0.03 to 0.35, more preferably 0.03 to 0.32. The atomic ratio of Mg / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0 to 0.10, more preferably 0 to 0.02. The atomic ratio of Al / (Mg+Al+Ti+Y+M) in the LDH-like compound is preferably 0 to 0.05, more preferably 0 to 0.04. Within the above range, the alkali resistance is more excellent, and the effect of suppressing short circuits caused by zinc dendrites (i.e., dendrite resistance) can be more effectively realized. Incidentally, LDHs conventionally known as LDH separators are represented by the general formula: M 2+ 1-x M 3+ x (OH)2A n- x / n ·mH2O (in the formula, M 2+ is a divalent cation, M 3+ is a trivalent cation, and A n- is an n-valent anion, n is an integer of 1 or more, x is 0.1 to 0.4, and m is 0 or more). In contrast, the above atomic ratio in the LDH-like compound generally deviates from the above general formula of LDH. For this reason, it can be said that the LDH-like compound in this embodiment generally has a composition ratio (atomic ratio) different from that of conventional LDH. It is preferable to perform the EDS analysis using an EDS analyzer (e.g., X-act, manufactured by Oxford Instruments) by 1) capturing an image at an accelerating voltage of 20 kV and a magnification of 5,000 times, 2) performing three-point analysis with an interval of about 5 μm in the point analysis mode, 3) repeating the above 1) and 2) once more, and 4) calculating the average value of a total of six points.
[0032] According to yet another preferred embodiment (c) of the present invention, the LDH-like compound is a hydroxide and / or oxide of a layered crystal structure containing Mg, Ti, Y, and optionally Al and / or In, and the LDH-like compound may be present in the form of a mixture with In(OH)3. The LDH-like compound of this embodiment is a hydroxide and / or oxide of a layered crystal structure containing Mg, Ti, Y, and optionally Al and / or In. Thus, a typical LDH-like compound is a composite hydroxide and / or composite oxide of Mg, Ti, Y, optionally Al, and optionally In. The In that may be contained in the LDH-like compound may not only be that which is intentionally added to the LDH-like compound, but may also be that which is inevitably mixed into the LDH-like compound due to the formation of In(OH)3 or the like. The above elements may be replaced with other elements or ions to the extent that the basic properties of the LDH-like compound are not impaired, but it is preferable that the LDH-like compound does not contain Ni. Incidentally, LDHs conventionally known for LDH separators are represented by the general formula: M 2+ 1-x M 3+ x (OH)2A n- x / n ·mH2O (in the formula, M 2+ is a divalent cation, M 3+ is a trivalent cation, and A n- is an n-valent anion, n is an integer of 1 or more, x is 0.1 to 0.4, and m is 0 or more). In contrast, the atomic ratio in the LDH-like compound generally deviates from the above general formula of LDH. Therefore, it can be said that the LDH-like compound in this embodiment generally has a composition ratio (atomic ratio) different from that of conventional LDH.
[0033] The mixture according to the above embodiment (c) contains not only an LDH-like compound but also In(OH)3 (typically composed of an LDH-like compound and In(OH)3). The inclusion of In(OH)3 can effectively improve the alkali resistance and dendrite resistance of the LDH separator. The content ratio of In(OH)3 in the mixture is preferably an amount that can improve the alkali resistance and dendrite resistance without substantially impairing the hydroxide ion conductivity of the LDH separator, and is not particularly limited. In(OH)3 may have a cubic crystal structure, or may have a structure in which In(OH)3 crystals are surrounded by the LDH-like compound. In(OH)3 can be identified by X-ray diffraction. EXAMPLES
[0034] The present invention will now be further illustrated by the following examples.
[0035] Examples 1-4 (1) Preparation of the positive electrode Paste-type nickel hydroxide positive electrode (capacity density: approx. 700 mAh / cm 3 ) was prepared.
[0036] (2) Preparation of the negative electrode The following various raw material powders were prepared. ZnO powder (Seido Chemical Industry Co., Ltd., JIS standard class 1 grade, average particle size D50: 0.2 μm) Metallic Zn powder (Mitsui Mining & Smelting Co., Ltd., doped with Bi and In, Bi: 1000 ppm by weight, In: 1000 ppm by weight, average particle size D50: 100 μm)
[0037] 100 parts by weight of ZnO powder was added with 5 parts by weight of metallic Zn powder, and 1.26 parts by weight of polytetrafluoroethylene (PTFE) dispersion solution (manufactured by Daikin Industries, Ltd., solid content 60%) was further added in terms of solid content, and kneaded with propylene glycol. The kneaded product was rolled with a roll press to obtain a plurality of negative electrode active material sheets with different thicknesses. The negative electrode active material sheets with different thicknesses were each pressure-bonded to both sides of a tin-plated copper expand metal to produce negative electrodes with different thickness ratios of the negative electrode active material layer.
[0038] (3) Preparation of electrolyte Ion-exchanged water was added to a 48% aqueous potassium hydroxide solution (special grade, manufactured by Kanto Chemical Co., Ltd.) to adjust the KOH concentration to 5.4 mol%, and then 0.42 mol / L of zinc oxide was dissolved therein by heating and stirring to obtain an electrolyte.
[0039] (4) Preparation of evaluation cell The positive and negative electrodes were wrapped in nonwoven fabric, and a current extraction terminal was welded to them. The positive and negative electrodes thus prepared were placed opposite each other via an LDH separator, sandwiched between a laminate film with a current extraction port, and three sides of the laminate film were heat-sealed. An electrolyte was added to the cell container with the top open in this way, and the electrolyte was allowed to fully penetrate the positive and negative electrodes by evacuation or the like. The remaining side of the laminate film was then heat-sealed to form a simple sealed cell.
[0040] (5) Evaluation Using a charge / discharge device (TOSCAT3100, manufactured by Toyo Systems Co., Ltd.), the simple sealed cell was subjected to formation by charging at 0.1C and discharging at 0.2C. Then, a 1C charge / discharge cycle was performed. The charge / discharge cycle was repeated under the same conditions, and the number of charge / discharge cycles until the discharge capacity of the prototype battery decreased to 70% of the discharge capacity of the first cycle was recorded. The number of charge / discharge cycles for each example is shown in Table 1 as a relative value when the number of charge / discharge cycles in Example 1 is set to 1.0, together with the evaluation results based on the following criteria. <Evaluation criteria> Rating A: Number of charge / discharge cycles (relative to the number in Example 1) is 2.0 or more Grade B: Number of charge / discharge cycles (relative value to the number of cycles in Example 1) is 1.5 or more and less than 2.0 Rating C: Number of charge / discharge cycles (relative value to the number of cycles in Example 1) is 1.2 or more and less than 1.5 Rating D: The number of charge / discharge cycles (relative to the number in Example 1) is less than 1.2
[0041] Figure 4 shows a cross-sectional photograph of the negative electrode (after charge / discharge evaluation) prepared in Example 1 (comparison), while Figure 5 shows a cross-sectional photograph of the negative electrode (after charge / discharge evaluation) prepared in Example 4. From the cross section of the negative electrode in each example, a reference plane passing through the center in the thickness direction of the negative electrode current collector plate was set, and the distance from both sides (outermost surfaces) of the negative electrode active material layer to the reference plane was measured to calculate the thickness T1, thickness T2, and ratio T2 / T1. The results are shown in Table 1.
[0042] [Table 1]
Claims
1. A negative electrode for use in a zinc secondary battery, a negative electrode active material layer including at least one selected from the group consisting of zinc, zinc oxide, a zinc alloy, and a zinc compound, the negative electrode active material layer having a first surface and a second surface; a negative electrode current collector plate embedded in the negative electrode active material layer in parallel to the negative electrode active material layer; Equipped with the first surface is farther from the negative electrode current collector than the second surface, so that a center in a thickness direction of the negative electrode active material layer is biased with respect to a reference plane passing through a center in a thickness direction of the negative electrode current collector; A thickness T defined as the distance between the first surface and the reference surface 1 a thickness T defined as the distance between the second surface and the reference surface, 2 T is the ratio of 2 / T 1 is greater than 0 and not greater than 0.
5.
2. The negative electrode according to claim 1 , wherein the negative electrode current collector plate is at least one selected from the group consisting of an expanded metal, a punched metal, and a metal mesh.
3. Said ratio T 2 / T 1 The negative electrode according to claim 1 or 2, wherein the anode current density is greater than 0 and is equal to or less than 0.
2.
4. Said T 1 and the above T 2 The negative electrode according to any one of claims 1 to 3, wherein the difference between the negative electrode thickness and the negative electrode thickness is 0.01 mm or more.
5. Said T 2 The negative electrode according to any one of claims 1 to 4, wherein the thickness is 0.01 to 1.0 mm.
6. a positive electrode including a positive electrode active material layer and a positive electrode current collector; The negative electrode according to any one of claims 1 to 5, a hydroxide ion conductive separator that separates the positive electrode and the negative electrode so as to be capable of conducting hydroxide ions; An electrolyte; wherein the negative electrode is disposed so that the second surface is closer to the hydroxide ion conductive separator.
7. 7. The zinc secondary battery of claim 6, wherein the hydroxide ion conducting separator is a layered double hydroxide (LDH) separator comprising an LDH and / or an LDH-like compound.
8. The zinc secondary battery described in claim 7, wherein the LDH separator further comprises a porous substrate, and the LDH and / or LDH-like compound is composited with the porous substrate in a form filled in the pores of the porous substrate.
9. The zinc secondary battery according to claim 8 , wherein the porous substrate is made of a polymeric material.
10. The zinc secondary battery according to any one of claims 6 to 9, wherein the positive electrode active material layer contains nickel hydroxide and / or nickel oxyhydroxide, thereby forming the zinc secondary battery into a nickel-zinc secondary battery.
11. The zinc secondary battery according to any one of claims 6 to 9, wherein the positive electrode active material layer is an air electrode layer, thereby forming the zinc secondary battery into an air zinc secondary battery.
Citation Information
Patent Citations
Multilayer zinc electrode and application of multilayer zinc electrode in zinc-air battery
CN111293314A
Cylindrical alkaline zinc storage battery
JP1986077255A
Secondary battery compensating capacity ratio of positive electrode and negative electrode
JP1999214027A
Negative plate for alkaline secondary battery, and alkaline secondary battery with the negative plate applied
JP2006156186A
Manufacturing method of negative electrode for zinc battery and negative electrode for zinc battery
JP2020170652A