Method for manufacturing two-dimensional material laminate and laminate
The laminate structure with UV or heat-sensitive adhesive layers facilitates high transfer rates and improved productivity in two-dimensional material laminates, addressing scaling challenges and environmental issues in traditional transfer methods.
Patent Information
- Application Number
- JP2021501945
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-02-19
- Filing Date
- 2020-02-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-02-14
AI Technical Summary
The transfer of two-dimensional materials, such as graphene, is challenging due to low transfer rates and quality issues, particularly when scaling up, leading to increased costs and environmental concerns from etching waste, and adhesiveness control is difficult with existing methods.
A laminate structure is used, comprising a two-dimensional material bonded to an adhesive layer that reduces adhesive strength with UV or heat, allowing for high transfer rates by peeling the adhesive sheet from a substrate.
The method enables high transfer rates and improved productivity of two-dimensional material laminates, reducing defects and costs associated with traditional etching methods.
Smart Images

Figure 0007558517000005 
Figure 0007558517000006 
Figure 0007558517000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a two-dimensional material stack and to the stack. [Background technology]
[0002] Two-dimensional materials such as two-dimensional carbon materials are expected to have various applications such as wiring materials and transparent electrodes due to their excellent electrical and optical properties. 2 Graphene, a conductive planar crystal made of bonded carbon atoms, has high optical transmittance and electrical conductivity, and is expected to be used in transparent conductive films, transparent electrodes, transistors, and more. Graphene is produced by chemical vapor deposition (CVD) on the surface of a catalytic metal, etc. However, when using graphene in a device, a process is required to transfer the graphene formed on the surface of the catalytic metal to the surface of a substrate.
[0003] For example, Patent Document 1 describes a graphene formation step of forming graphene on a surface of a copper foil for producing graphene, and a graphene production method including laminating a transfer sheet on the surface of the graphene, etching the copper foil for producing graphene while transferring the graphene onto the transfer sheet, and then transferring the graphene to another substrate and peeling off the transfer sheet.
[0004] Furthermore, Patent Document 2 describes an adhesive for temporarily fixing fragile members, which contains as its main component a polyurethane resin obtained by curing an adhesive composition containing a polyol and a polyfunctional isocyanate compound, and is used for temporarily fixing fragile members such as graphene.
[0005] However, because graphene is a thin film, transferring large areas of graphene is not only technically difficult, but there is also the problem of quality degradation during transfer. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent No. 5850720 [Patent Document 2] Japanese Patent Publication No. 2014-172989 Summary of the Invention [Problem to be solved by the invention]
[0007] Two-dimensional materials such as graphene are thin films with thicknesses on the nanometer order, so there was a problem that the transfer rate during transfer decreased as the area became larger. As described in Patent Document 1, when transferring graphene from a catalytic metal to a substrate, if the catalytic metal is etched away, the graphene may be torn or have fine scratches, which is thought to lead to a decrease in yield and the performance of the graphene. In addition, according to the technology described in Patent Document 1, etching the catalytic metal requires high metal costs and the treatment of etching waste liquid, which poses a problem in productivity. Furthermore, when graphene is to be transferred to another substrate after etching, it is difficult to transfer the graphene to another substrate because the adhesiveness of the PET film described in Patent Document 1 cannot be controlled.
[0008] Therefore, an object of the present invention is to provide a laminate and a method for manufacturing a two-dimensional material laminate that are excellent in productivity and capable of transferring a two-dimensional material at a high transfer rate. [Means for solving the problem]
[0009] As a result of intensive research conducted by the present inventors in order to achieve the above object, the present inventors have found that the above problems in the conventional technology can be solved by using a laminate in which a two-dimensional material and a specific pressure-sensitive adhesive layer are laminated, and have completed the present invention. That is, the present invention is as follows.
[0010] [1] A step of transferring the two-dimensional material on the first substrate to a surface of an adhesive sheet having a base material and an adhesive layer whose adhesive strength is reduced by ultraviolet light or heat, thereby obtaining a laminate of the adhesive sheet and the two-dimensional material; placing the stack on a second substrate such that a surface of the stack facing the two-dimensional material is in contact with the second substrate; applying the ultraviolet light or heat to the laminate; and transferring the two-dimensional material onto the second substrate by peeling off the adhesive sheet; the adhesive strength A of the pressure-sensitive adhesive layer to a silicon wafer at 25° C. before the application of the ultraviolet light or heat is 1.0 N / 20 mm to 20.0 N / 20 mm when peeled at 180° at a pulling speed of 300 mm / min; the surface roughness of the adhesive surface of the pressure-sensitive adhesive layer after application of the ultraviolet rays or heat is 0.01 μm to 8.00 μm; A method for manufacturing a two-dimensional material stack. [2] The method for producing a two-dimensional material stack according to [1], wherein the two-dimensional material is a two-dimensional carbon material, molybdenum disulfide, tungsten disulfide, or hexagonal boron nitride. [3] The method for producing a two-dimensional material laminate according to [1] or [2], wherein an adhesive strength B of the pressure-sensitive adhesive layer to a silicon wafer at 25°C after exposure to the ultraviolet rays or heat is 0.01 N / 20 mm to 1.00 N / 20 mm when subjected to a 180° peel at a tensile speed of 300 mm / min. [4] The method for producing a two-dimensional material laminate according to [2], wherein the two-dimensional carbon material is graphene or a graphene derivative. [5] The method for producing a two-dimensional material laminate according to any one of [2] to [4], wherein the pressure-sensitive adhesive layer contains an ultraviolet-curable pressure-sensitive adhesive. [6] The method for producing a two-dimensional material laminate according to any one of [2] to [5], wherein the base material is ultraviolet ray transparent. [7] The method for manufacturing a two-dimensional material laminate according to [6], wherein the transfer rate of the two-dimensional material is 30% or more. [8] A laminate of a substrate, an adhesive sheet having an adhesive layer whose adhesive strength is reduced by ultraviolet light or heat, and a two-dimensional material, the adhesive strength A of the pressure-sensitive adhesive layer to a silicon wafer at 25° C. before application of ultraviolet light or heat is 1.0 N / 20 mm to 20.0 N / 20 mm when subjected to a 180° peel at a tensile speed of 300 mm / min; The laminate has a surface roughness of the adhesive surface of the adhesive layer after exposure to ultraviolet light or heat of 0.01 μm to 8.00 μm. [9] The laminate according to [8], wherein the two-dimensional material is a two-dimensional carbon material, molybdenum disulfide, tungsten disulfide, or hexagonal boron nitride.
[10] The laminate according to [9], wherein the adhesive strength B of the pressure-sensitive adhesive layer to a silicon wafer at 25°C after exposure to the ultraviolet light or heat is 0.01 N / 20 mm to 1.00 N / 20 mm when subjected to a 180° peel at a tensile speed of 300 mm / min.
[11] The laminate according to [9], wherein the two-dimensional carbon material is graphene or a graphene derivative.
[12] The laminate according to any one of [9] to
[11] , wherein the pressure-sensitive adhesive layer contains an ultraviolet-curable pressure-sensitive adhesive.
[13] The laminate according to any one of [9] to
[12] , wherein the substrate has ultraviolet light transmissibility. Effect of the Invention
[0011] According to the present invention, it is possible to provide a laminate which is excellent in productivity and capable of transferring a two-dimensional material at a high transfer rate, and a method for producing a two-dimensional material laminate using the laminate. [Brief description of the drawings]
[0012] [Figure 1]FIG. 1 is a schematic diagram for explaining a production method according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram for explaining the manufacturing method according to the embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view of a laminate according to an embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram for explaining a manufacturing method according to an embodiment of the present invention. [Diagram 5] FIG. 5 is a schematic diagram for explaining a manufacturing method according to an embodiment of the present invention. [Figure 6] FIG. 6 is a diagram showing image data for explaining an embodiment of the present invention. [Figure 7] FIG. 7 is a diagram showing image data for explaining an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described in detail. A method for producing a two-dimensional material laminate according to an embodiment of the present invention includes: A step of transferring the two-dimensional material on the first substrate to a surface of an adhesive sheet having a base material and an adhesive layer whose adhesive strength is reduced by ultraviolet light or heat, thereby obtaining a laminate of the adhesive sheet and the two-dimensional material; placing the stack on a second substrate such that a surface of the stack facing the two-dimensional material is in contact with the second substrate; applying the ultraviolet light or heat to the laminate; and transferring the two-dimensional material onto the second substrate by peeling off the adhesive sheet; the adhesive strength A of the pressure-sensitive adhesive layer to a silicon wafer at 25° C. before the application of the ultraviolet light or heat is 1.0 N / 20 mm to 20.0 N / 20 mm when peeled at 180° at a pulling speed of 300 mm / min; The surface roughness of the adhesive surface of the pressure-sensitive adhesive layer after the application of the ultraviolet rays or heat is 0.01 μm to 8.00 μm.
[0014] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. FIG. 1 is a schematic diagram showing a stack 101 comprising a two-dimensional material 30 on a first substrate 21 .
[0015] The first substrate 21 is not particularly limited, and may be any of a metal substrate, a ceramic substrate, a silicon substrate, a resin substrate, and the like. Examples of the first substrate 21 include metal substrates made of transition metals such as copper, nickel, cobalt, iron, chromium, gold, platinum, molybdenum, and tungsten; alloy metal substrates of these metals; single crystal substrates such as sapphire, magnesia, spinel, mica, SiC, SiN, and Si, and single crystal substrates whose surfaces have been oxidized; quartz substrates; substrates for forming films of two-dimensional materials on the surfaces of the above-mentioned transition metals, and substrates on the above-mentioned substrates on which two-dimensional materials are formed. The first substrate 21 is preferably a substrate for forming films of two-dimensional materials.
[0016] There is no particular limitation on the method for forming the two-dimensional material on the metal substrate for film formation, and the CVD method is preferably used. As the film formation method, for example, there are a thermal CVD method in which a raw material gas is introduced in the presence of a catalytic metal and processed by thermal decomposition of the raw material gas, and a surface wave microwave plasma chemical vapor deposition (CVD) method in which processing is performed by microwave plasma, etc., but it is sufficient as long as the two-dimensional material 30 can be formed on the first substrate 21.
[0017] The two-dimensional material 30 is a material having a two-dimensional layered structure made of a single type or two or more types of elements and having an extremely thin sheet structure. Graphene, which is a two-dimensional sheet made of carbon only, is a representative example. The two-dimensional material 30 may also be a ribbon-like film having a width in nanometer units. Examples of two-dimensional materials include two-dimensional carbon materials, transition metal chalcogenides, molybdenum disulfide, tungsten disulfide, hexagonal boron nitride (h-BN), black phosphorus, and derivatives thereof, and two-dimensional carbon materials, molybdenum disulfide, tungsten disulfide, or hexagonal boron nitride are preferred. As the two-dimensional carbon material, graphene or a graphene derivative is preferable. Graphene is a film formed by sp2 bonded carbon atoms with a thickness of one atom, forming a hexagonal lattice structure made of carbon atoms and their bonds. In this specification, multi-layer graphene, which is a stack of 2 to 100 layers of these films, is also called "graphene".
[0018] Examples of the graphene derivative include graphene oxide, sulfonated graphene oxide, graphene hydroxide, graphene carbonate, graphene nitride, and the like, with graphene oxide being preferred.
[0019] The laminate 101 may be subjected to a pretreatment of immersion in water. For example, when the two-dimensional material is graphene, and the graphene film-forming catalyst of the laminate 101 is Cu, the laminate 101 is immersed in water at 4 to 100° C. for 4 to 72 hours. This treatment causes water to be intercalated at the interface between graphene and Cu, and the Cu surface is oxidized. During the immersion, the water may be left to stand or stirred. Stirring the water makes the Cu surface more likely to be oxidized. There are also methods of adding a metal salt such as potassium chloride or sodium chloride to water to promote oxidation of Cu, and methods of oxidizing Cu by contacting it with water vapor, and in either case, water is intercalated at the interface between graphene and Cu, and the Cu surface is oxidized. This oxidation weakens the interaction between the graphene and Cu, allowing the graphene to be effectively transferred to the adhesive sheet 10.
[0020] 2 and 3 are schematic diagrams showing a process in which a two-dimensional material 30 on a first substrate 21 is laminated and transferred onto the adhesive layer side of an adhesive sheet 10 having a base material 11 and an adhesive layer 12 whose adhesive strength is reduced by ultraviolet light or heat, to obtain a laminate 103 of the adhesive sheet 10 and the two-dimensional material 30. When bonding adhesive sheet 10 to laminate 101 of first substrate 21 and two-dimensional material 30, adhesive sheet 10 can be placed on laminate 101 to form laminate 102. The laminate 102 may be formed by, for example, pressing the two-dimensional material 30 and the adhesive sheet 10 together using a roller or the like.
[0021] Since the two-dimensional material 30 adheres to the adhesive sheet 10, the two-dimensional material 30 is transferred from the first substrate 21 to the adhesive sheet 10 by peeling off the laminate 103 of the adhesive sheet 10 and the two-dimensional material 30 from the laminate 102. Alternatively, the laminate 103 in which the two-dimensional material 30 is transferred to the adhesive sheet 10 can be obtained by immersing the laminate 102 in an aqueous potassium hydroxide solution, an aqueous hydrochloric acid solution, or the like, and etching the surface of the first substrate 21 facing the two-dimensional material.
[0022] According to the laminate 103 obtained in this embodiment, for example, a two-dimensional material formed on a catalytic metal can be transferred onto another substrate with a high transfer rate.
[0023] 4 is a schematic diagram showing a step of placing the laminate 103 on the second substrate 40 so that the surface of the laminate 103 on the two-dimensional material side is in contact with the second substrate 40. The laminate 104 is obtained by laminating the second substrate 40 and the laminate 103. By applying ultraviolet light or heat to the laminate 103 (laminate 104), the adhesive strength of the adhesive layer 12 is reduced, making it easier to peel off the adhesive sheet 10. The step of applying ultraviolet light or heat to the laminate 103 may be performed before or after the step of placing the laminate 103 on the second substrate 40, but is preferably performed after. 5 is a schematic diagram showing a process of transferring two-dimensional material 30 onto second substrate 40 by peeling off adhesive sheet 10. By peeling off adhesive sheet 10 of laminate 104, two-dimensional material 30 is transferred onto second substrate 40, and two-dimensional material laminate 105 is obtained.
[0024] The pressure-sensitive adhesive sheet according to the embodiment of the present invention includes a substrate and a pressure-sensitive adhesive layer whose adhesive strength is reduced by ultraviolet light or heat. The adhesive strength of the pressure-sensitive adhesive layer is reduced by ultraviolet light or heat, so that the two-dimensional material can be transferred onto a second substrate with a high transfer rate. For example, the adhesive sheet exerts high adhesive strength when a two-dimensional material formed on a metal substrate is peeled off from the metal substrate and transferred to an adhesive layer. Then, after laminating a laminate of the adhesive sheet and the two-dimensional material onto another substrate, the adhesive strength of the adhesive layer is reduced by ultraviolet light or heat, and then the adhesive sheet is removed, thereby preventing the two-dimensional material from being torn, cracked, wrinkled, or the like, and allowing the material to be transferred at a high transfer rate.
[0025] The peel angle when peeling the laminate 103 from the laminate 102 is not particularly limited and is usually 180 degrees or less, but a small peel angle can prevent defects such as breakage and cracks from occurring in the two-dimensional material 30 due to changes in the shape of the laminate 103. For this reason, it is preferable that the peel angle is small, preferably 90 degrees or less, and more preferably 60 degrees or less. In addition, from the viewpoint of increasing the size of the peeling device itself, the peel angle is preferably 0 degrees or more. The peeling angle refers to the angle formed between first substrate 21 and the peeled portion of laminate 103 when laminate 103 is peeled from laminate 102.
[0026] The peeling speed when peeling the laminate 103 from the laminate 102 is not particularly limited, but if the peeling speed is high, the time for the shape of the laminate 103 to change is shortened, and therefore defects such as breakage and cracks can be prevented from occurring in the two-dimensional material 30. For this reason, the peeling speed is usually 10 mm / min or more, but is preferably high, preferably 1000 mm / min or more, and more preferably 2000 mm / min or more. In addition, from the viewpoint of stable operation of the device, the peeling speed is preferably 100,000 mm / min or less, and more preferably 90,000 mm / min or less. The peeling speed refers to the length of the laminate 103 peeled from the laminate 102 per unit time when the laminate 103 is peeled from the laminate 102 .
[0027] The transfer rate of the two-dimensional material is preferably 30% or more, more preferably 50% or more, and even more preferably 70% or more.
[0028] Here, the transfer rate of the two-dimensional material can be calculated as follows. For example, when the two-dimensional material is graphene, graphene is grown on the surface of a Cu / sapphire substrate by thermal CVD, and then the Cu is oxidized. When the Cu surface of the Cu / sapphire substrate is completely covered with graphene, the Cu is oxidized uniformly across the entire substrate. On the other hand, when the Cu surface is not completely covered with graphene, the Cu region directly below the graphene crystal grains (the Cu region covered with graphene) and the Cu region not covered with graphene undergo different oxidation patterns, allowing the graphene crystal grains to be clearly observed. Then, adhesive tape is applied to the graphene and peeled off, and the adhesive tape / graphene is attached to a 0.5 mm thick silicon substrate (e.g., manufactured by SUMCO) with a 300 nm oxide film, which is the material to be transferred. The adhesive tape / graphene / silicon substrate is irradiated with ultraviolet light or heated to reduce the adhesive strength of the adhesive tape, and then the adhesive tape is peeled off. When the Cu surface is completely covered with graphene, the adhesive tape is peeled off and the image of the graphene transferred to the surface of the transfer material is observed under a microscope. The area ratio of graphene in the image expressed as a percentage is taken as the transfer rate. When the Cu surface is not completely covered with graphene, the graphene crystal grain group on the Cu / sapphire substrate before the adhesive tape is applied and the graphene crystal grain group on the transfer material transferred by the adhesive tape are compared under a microscope, and the ratio, expressed as a percentage, of the area of the graphene crystal grain group on the Cu / sapphire substrate to the area of the crystal grain group transferred to the surface of the transfer material is taken as the transfer rate.
[0029] For example, a base material containing any resin selected from nylon, polyurethane, polyester, polyolefin, and olefin-based elastomer as a main component, or a crosslinked product thereof, etc. can be used as the base material 11. The base material 11 is preferably UV-transparent.
[0030] The substrate 11 may be a non-stretched film, or may be one that has been subjected to uniaxial or biaxial stretching treatment as necessary. The thickness of the substrate 11 is not particularly limited and can be appropriately selected, but is generally about 5 to 200 μm.
[0031] The adhesive strength of the adhesive layer 12 decreases due to ultraviolet rays or heat. From the viewpoint of the graphene transfer rate to the adhesive sheet, the adhesive strength A (initial adhesive strength) before application of ultraviolet rays or heat is preferably an adhesive strength to a silicon wafer at 25°C of 1.0 N / 20 mm or more, more preferably 1.5 N / 20 mm or more, even more preferably 2.0 N / 20 mm or more, preferably 20.0 N / 20 mm or less, more preferably 17.0 N / 20 mm or less, and even more preferably 15.0 N / 20 mm or less.
[0032] From the viewpoint of the graphene transfer rate from the adhesive sheet, the adhesive strength B of the adhesive layer after application of ultraviolet light or heat is preferably an adhesive strength to a silicon wafer at 25° C. of 0.01 N / 20 mm or more, more preferably 0.03 N / 20 mm or more, even more preferably 0.05 N / 20 mm or more, preferably 1.00 N / 20 mm or less, more preferably 0.50 N / 20 mm or less, and even more preferably 0.25 N / 20 mm or less. Here, adhesive strength A and adhesive strength B are the adhesive strengths when a 180° peel was performed on a silicon wafer at 25° C. and at a tensile speed of 300 mm / min. The adhesive strength after exposure to ultraviolet light or heat is preferably reduced to 30% or less, and more preferably to 10% or less, of the adhesive strength before exposure to ultraviolet light or heat.
[0033] When the pressure-sensitive adhesive layer is irradiated with ultraviolet light, crosslinking or polymerization of the resin contained in the pressure-sensitive adhesive layer can proceed, thereby reducing the adhesive strength of the pressure-sensitive adhesive layer. The adhesive layer also loses its adhesive strength due to heat such as heating or cooling. For example, the adhesive strength of the adhesive layer can be reduced by heating to promote crosslinking or polymerization of the resin contained in the adhesive layer. For example, a foaming agent may be added to the adhesive layer and foamed by heating to generate unevenness on the contact surface between the adhesive layer and the two-dimensional material, thereby reducing the adhesive strength of the adhesive layer. Even if unevenness is generated on the contact surface of the adhesive layer, the surface roughness of the adhesive surface of the adhesive layer needs to be 0.01 μm to 8.00 μm in order to prevent a decrease in the transfer rate.
[0034] In the pressure-sensitive adhesive layer according to the embodiment of the present invention, the surface roughness of the adhesive surface of the pressure-sensitive adhesive layer after exposure to ultraviolet light or heat is 0.01 μm to 8.00 μm. The surface roughness of the adhesive surface of the pressure-sensitive adhesive layer is preferably 0.03 μm or more, more preferably 0.05 μm or more, even more preferably 0.10 μm or more, and is preferably 5.00 μm or less, more preferably 4.00 μm or less, even more preferably 3.00 μm or less. If the surface roughness of the adhesive surface of the adhesive layer after exposure to ultraviolet light or heat is greater than 8.00 μm, the film of the two-dimensional material will be torn or scratched, resulting in a decrease in the transfer rate. Also, if the surface roughness of the adhesive surface of the adhesive layer is less than 0.01 μm, it will be difficult to create the adhesive surface itself. The surface roughness of the adhesive side of the adhesive layer can be measured using a white light confocal microscope (Lasertec OPTELICS HYBRID, manufactured by Lasertec Corporation) with a 20x objective lens and the software "LMeye7". The adhesive layer is attached to a silicon wafer separately, and then the adhesive strength is reduced by heat or ultraviolet light, and the adhesive surface is peeled off and measured by focusing on the outermost adhesive surface and scanning a range of 50 μm up and down. The measured image of a 750 μm square is also used with the software "LMeye7" to calculate Ra at five points on an arbitrary line in the surface roughness line profile, and the average value is taken as the surface roughness.
[0035] The adhesive layer 12 preferably contains an ultraviolet-curable adhesive, which can increase the degree of crosslinking by irradiation with ultraviolet light, thereby easily reducing the adhesive strength. The ultraviolet-curable adhesive preferably has an ultraviolet-curable functional group such as a radically reactive carbon-carbon double bond and exhibits adhesive properties. An example of the ultraviolet-curable adhesive is an additive type ultraviolet-curable adhesive in which an ultraviolet-curable monomer component or oligomer component is blended with an acrylic adhesive.
[0036] Examples of the acrylic polymer include acrylic polymers using one or more of (meth)acrylic acid alkyl esters (e.g., methyl ester, ethyl ester, propyl ester, isopropyl ester, butyl ester, isobutyl ester, sec-butyl ester, t-butyl ester, pentyl ester, isopentyl ester, hexyl ester, heptyl ester, octyl ester, 2-ethylhexyl ester, isooctyl ester, nonyl ester, decyl ester, isodecyl ester, undecyl ester, dodecyl ester, tridecyl ester, tetradecyl ester, hexadecyl ester, octadecyl ester, eicosyl ester, and other linear or branched alkyl esters having 1 to 30 carbon atoms, particularly 4 to 18 carbon atoms) and (meth)acrylic acid cycloalkyl esters (e.g., cyclopentyl ester, cyclohexyl ester, and the like) as monomer components. Note that (meth)acrylic acid ester refers to acrylic acid ester and / or methacrylic acid ester, and (meth) in the present invention has the same meaning in all cases.
[0037] The acrylic polymer contains, as an essential component, a hydroxyl group-containing monomer that is copolymerizable with the acrylic ester, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate.
[0038] The content of the hydroxyl group-containing monomer is preferably within a range of 10 to 30 mol % relative to the acrylic acid ester, and more preferably within a range of 15 to 25 mol %. When the content is 10 mol % or more, crosslinking after ultraviolet irradiation is sufficient, the transfer rate of the two-dimensional material is improved, and the productivity is increased.
[0039] The acrylic polymer may contain units corresponding to other monomer components copolymerizable with the acrylic acid alkyl ester or cycloalkyl ester, if necessary. Examples of such monomer components include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride monomers such as maleic anhydride and itaconic anhydride; sulfonic acid group-containing monomers such as styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid; phosphoric acid group-containing monomers such as 2-hydroxyethylacryloylphosphate; acrylamide, acrylonitrile, and the like. These copolymerizable monomer components can be used alone or in combination. The amount of these copolymerizable monomers used is preferably 40% by mass or less of the total monomer components. The amount of the carboxyl group-containing monomer used is preferably 0 to 3 mass % or less of the total monomer components. In addition, since the hydroxyl group-containing monomer and the glycidyl group-containing monomer can react with the epoxy group in the epoxy resin, it is preferable to use them in the same manner as the carboxyl group-containing monomer.
[0040] The acrylic polymer preferably contains an isocyanate compound having a radical reactive carbon-carbon double bond, such as methacryloyl isocyanate, 2-methacryloyloxyethyl isocyanate, 2-acryloyloxyethyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate, etc.
[0041] The content of the isocyanate compound having the radical reactive carbon-carbon double bond is preferably within a range of 50 to 90 mol %, more preferably within a range of 75 to 85 mol %, based on the hydroxyl group-containing monomer. If the content is 50 mol % or more, crosslinking after ultraviolet irradiation proceeds sufficiently, and the transfer rate of the two-dimensional material is increased, which is preferable.
[0042] The acrylic polymer is obtained by polymerizing a single monomer or a mixture of two or more monomers. The polymerization can be carried out by any method such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, etc. The weight average molecular weight of the acrylic polymer is preferably about 350,000 to 1,000,000, more preferably about 450,000 to 800,000.
[0043] The pressure-sensitive adhesive layer 12 may also contain a thermoplastic resin. Examples of the thermoplastic resin include natural or synthetic rubbers such as natural rubber, polyisobutylene, polyisoprene, chloroprene rubber, butyl rubber, and nitrile butyl rubber; olefin-based elastomers such as ethylene-propylene copolymer, ethylene-propylene-diene copolymer, ethylene-vinyl acetate copolymer, polybutene, and chlorinated polyethylene; styrene-based elastomers such as styrene-butadiene-styrene copolymer, styrene-isoprene-styrene copolymer, and hydrogenated products thereof; polyester-based elastomers; polyamide-based elastomers; and various thermoplastic elastomers such as polyurethane-based elastomers. These rubber components or thermoplastic elastomer components may be used alone or in combination of two or more.
[0044] In addition to the above resin, the pressure-sensitive adhesive layer 12 may contain a foaming agent. The foaming agents may be used alone or in combination of two or more kinds. The foaming agent is not particularly limited, but preferably includes inorganic substances.The above-mentioned inorganic substances include, for example, hydroxides such as aluminum hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide, etc.; clay (particularly hard clay); talc; silica; zeolite; alkaline earth metal carbonates such as calcium carbonate, magnesium carbonate, etc.; metal oxides such as zinc oxide, titanium oxide, alumina, etc.; metal powders such as various metal powders such as iron powder, copper powder, aluminum powder, nickel powder, zinc powder, titanium powder, etc., alloy powder, etc.; mica; carbon particles; glass fiber; carbon tube; layered silicate; glass, etc.
[0045] The thickness of the adhesive layer is not particularly limited, but from the viewpoint of exerting good adhesion to two-dimensional materials, it is preferably 2 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more, and from the viewpoint of forming a smooth adhesive layer, it is preferably 500 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less.
[0046] The second substrate 40 is a material to which a two-dimensional material is transferred. The second substrate 40 is preferably a substrate in which the adhesive strength between its transfer surface and the two-dimensional material 30 is stronger than the adhesive strength between the adhesive layer 12 and the two-dimensional material 30 after ultraviolet light or heat is applied. Such a second substrate 40 may have a strong interacting force by itself, or may have an interacting force imparted by surface processing. Examples of surface processing include, but are not limited to, the application of a curable resin, surface melting, formation of a fine structure, and surface chemical modification.
[0047] The second substrate 40 is not particularly limited and may be any of a metal substrate, a ceramic substrate, a silicon substrate, a resin substrate, etc. As the second substrate 40, for example, a SiO2 / Si substrate, a quartz substrate, a glass substrate, a PET substrate, a sapphire substrate, an ITO substrate, and a substrate on which two-dimensional materials are laminated are preferable, and a SiO2 / Si substrate is more preferable.
[0048] The thickness of the second substrate 40 is not particularly limited and can be selected as appropriate, but is preferably 1 μm or more, more preferably 10 μm or more, and even more preferably 100 μm or more, and from the viewpoint of handling, is preferably 100 mm or less, more preferably 20 mm or less, and even more preferably 5 mm or less.
[0049] The two-dimensional material laminate obtained by the method for producing a two-dimensional material laminate according to the embodiment of the present invention can be applied to transparent conductive films for touch panels, etc., semiconductor devices or electronic devices such as transistors and integrated circuits, transparent electrodes and electrochemical electrodes that require a large area, and the like. EXAMPLES
[0050] The present invention will be described below based on examples, but the present invention is not limited to these examples.
[0051] <Preparation of Adhesive Sheet 1> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer was charged with 75 parts by mass of n-butyl acrylate (hereinafter referred to as "BA"), 25 parts by mass of acryloylmorpholine (hereinafter referred to as "ACMO"), 20 parts by mass of 2-hydroxyethyl acrylate (hereinafter referred to as "HEA"), 0.2 parts by mass of benzoyl peroxide, and 65 parts by mass of toluene, and polymerized in a nitrogen stream at 61°C for 6 hours to obtain acrylic polymer A.
[0052] 2-methacryloyloxyethyl isocyanate (hereinafter referred to as "MOI") was added to this acrylic polymer A in an amount of 80 mol % based on HEA, and an addition reaction treatment was carried out in an air stream at 50°C for 48 hours to obtain acrylic polymer A'.
[0053] Next, 8 parts by mass of a polyisocyanate compound (product name "Coronate L", manufactured by Nippon Polyurethane Co., Ltd.) and 5 parts by mass of a photopolymerization initiator (product name "Irgacure 651", manufactured by Chiba Specialty Chemicals) were added to 100 parts by mass of acrylic polymer A' to prepare an adhesive solution.
[0054] The adhesive solution prepared above was applied onto the silicone-treated surface of a PET release liner, and crosslinked by heating at 120°C for 2 minutes to form an adhesive layer with a thickness of 17 μm. Next, an ethylene-vinyl acetate copolymer (EVA) film with a thickness of 115 μm was laminated onto the adhesive layer surface. After that, it was stored at 50°C for 24 hours, and then adhesive sheet 1 was produced.
[0055] <Preparation of Adhesive Sheet 2> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer was charged with 30 parts by mass of 2-ethylhexyl acrylate (hereinafter referred to as "2EHA"), 70 parts by mass of methyl acrylate (hereinafter referred to as "MA"), 10 parts by mass of acrylic acid (hereinafter referred to as "AA"), 0.2 parts by mass of benzoyl peroxide, and 65 parts by mass of toluene, and polymerized in a nitrogen stream at 61°C for 6 hours to obtain acrylic polymer B.
[0056] Next, 100 parts by mass of photopolymerizable oligomer UV-1700B (manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), 1 part by mass of melamine resin (product name "Super Beckamine J-820-60N", manufactured by Dainippon Ink Co., Ltd.), 1 part by mass of polyisocyanate compound (product name "Coronate L", manufactured by Nippon Polyurethane Co., Ltd.), and 3 parts by mass of photopolymerization initiator (product name "Irgacure 651", manufactured by Chiba Specialty Chemicals) were added to 100 parts by mass of acrylic polymer B to prepare an adhesive solution.
[0057] The adhesive solution prepared above was applied onto the silicone-treated surface of a PET release liner, and crosslinked by heating at 120°C for 2 minutes to form an adhesive layer having a thickness of 20 μm. A polyolefin film having a thickness of 150 μm was then laminated onto the adhesive layer surface. After that, the adhesive sheet 2 was produced after storing at 50°C for 24 hours.
[0058] <Preparation of Adhesive Sheet 3> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer was charged with 50 parts by mass of BA, 50 parts by mass of ethyl acrylate (hereinafter referred to as "EA"), 10 parts by mass of HEA, 0.2 parts by mass of benzoyl peroxide, and 65 parts by mass of toluene, and polymerized in a nitrogen stream at 61°C for 6 hours to obtain acrylic polymer C.
[0059] To this acrylic polymer C, 50 mol % of MOI based on HEA was added, and addition reaction was carried out in an air stream at 50° C. for 48 hours to obtain acrylic polymer C′.
[0060] Next, 8 parts by mass of a polyisocyanate compound (product name "Coronate L", manufactured by Nippon Polyurethane Co., Ltd.) and 5 parts by mass of a photopolymerization initiator (product name "Irgacure 651", manufactured by Chiba Specialty Chemicals) were added to 100 parts by mass of acrylic polymer C' to prepare an adhesive solution.
[0061] The adhesive solution prepared above was applied onto the silicone-treated surface of a PET release liner, and crosslinked by heating at 120°C for 2 minutes to form an adhesive layer with a thickness of 30 μm. Next, a PET film with a thickness of 50 μm was attached to the adhesive layer surface. After that, the adhesive sheet 3 was produced after storing at 50°C for 24 hours.
[0062] <Preparation of Adhesive Sheet 4> 20 parts by mass of EA, 80 parts by mass of BA, 10 parts by mass of AA, 0.2 parts by mass of benzoyl peroxide, and 65 parts by mass of toluene were placed in a reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer, and polymerization treatment was carried out in a nitrogen stream at 61° C. for 6 hours, thereby obtaining acrylic polymer D. 100 parts by mass of acrylic polymer D was uniformly mixed with 1 part by mass of an epoxy crosslinking agent (product name "Tetrad-C" manufactured by Mitsubishi Gas Chemical Co., Ltd.), 5 parts by mass of a rosin tackifier (product name "Tamanol 361" manufactured by Arakawa Chemical Co., Ltd.), 30 parts by mass of a foaming agent (thermally expandable microspheres; product name "Matsumoto Microsphere F-501D" manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd.; 120°C foaming and expansion type), and toluene. The resulting coating liquid was applied to one side of a 100 μm thick PET film so that the thickness after drying would be 50 μm, and the film was dried. The silicone-treated side of a PET release liner was then bonded to the film to produce adhesive sheet 4.
[0063] <Preparation of Adhesive Sheet 5> To 100 parts by mass of acrylic polymer B, 100 parts by mass of photopolymerizable oligomer UV-1700B (manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), 1 part by mass of melamine resin (product name "Super Beckamine J-820-60N", manufactured by Dainippon Ink Co., Ltd.), and 8 parts by mass of a polyisocyanate compound (product name "Coronate L", manufactured by Nippon Polyurethane Co., Ltd.) were added to prepare an adhesive solution.
[0064] The adhesive solution prepared above was applied onto the silicone-treated surface of a PET release liner, and crosslinked by heating at 120°C for 2 minutes to form an adhesive layer having a thickness of 20 μm. A polyolefin film having a thickness of 150 μm was then laminated onto the adhesive layer surface. After that, the adhesive sheet was stored at 50°C for 24 hours, and then an adhesive sheet 5 was produced.
[0065] <Preparation of Adhesive Sheet 6> Adhesive sheet 6 was prepared in the same manner as adhesive sheet 1, except that the MOI in the preparation of adhesive sheet 1 was changed to 50 mol % with respect to HEA.
[0066] <Preparation of Adhesive Sheet 7> Adhesive sheet 7 was prepared in the same manner as adhesive sheet 1, except that the amount of ACMO in the preparation of adhesive sheet 1 was changed to 30 parts by mass, and the MOI was changed to 50 mol % relative to HEA.
[0067] <Preparation of Adhesive Sheet 8> Adhesive sheet 8 was prepared in the same manner as adhesive sheet 1, except that the HEA used in the preparation of adhesive sheet 1 was changed to 4-hydroxybutyl acrylate (hereinafter referred to as "4HBA") and the MOI was changed to 50 mol % relative to 4HBA.
[0068] <Preparation of Adhesive Sheet 9> Adhesive sheet 9 was produced in the same manner as adhesive sheet 1, except that the EVA film used in the production of adhesive sheet 1 was changed to a nylon film having a thickness of 25 μm.
[0069] <Preparation of Adhesive Sheet 10> Adhesive sheet 10 was produced in the same manner as adhesive sheet 1, except that the EVA film used in the production of adhesive sheet 1 was changed to a polyolefin (biaxially oriented polypropylene) film having a thickness of 50 μm.
[0070] <Preparation of Adhesive Sheet 11> Adhesive sheet 11 was produced in the same manner as adhesive sheet 1, except that the EVA film used in the production of adhesive sheet 1 was changed to a polyolefin (poly-4-methylpentene-1) film having a thickness of 50 μm.
[0071] <Deposition of epitaxial metal films on single crystal substrate surfaces by sputtering> The c-plane (0001) of sapphire (α-Al2O3) purchased from Adamant Namiki Precision Jewel Co., Ltd. was used as a single crystal substrate. The above single crystal substrate was placed in the chamber of an RF magnetron sputtering device (Shibaura Mechatronics CFS-4ES), and Cu metal was sputtered onto the surface of the single crystal substrate (Ar atmosphere, standard vacuum level of 0.6 Pa). As a result, a Cu film with a thickness of 1000 nm was epitaxially deposited, resulting in a Cu / sapphire substrate.
[0072] <Graphene CVD deposition> The above Cu / sapphire substrate was placed inside a quartz tube (inner diameter 26 mmφ) set in a ceramic tubular furnace at Asahi Rika Seisakusho as a substrate for graphene deposition. A substrate size of 10 mm square was used. Then, under atmospheric pressure, the temperature was raised to a specified temperature (1000-1075°C) while flowing argon and hydrogen. After reaching the specified temperature, it was held under the same conditions for 0-3 hours to reduce and smooth the Cu surface. Then, 10-200 ppm of methane was added to carry out a chemical vapor reaction. After the reaction, it was cooled to room temperature (23°C), and the Cu / sapphire substrate on which single-layer graphene had been generated was removed from the quartz tube. Through this reaction, single-layer graphene with a crystal grain size of 10-200 μm was formed on the Cu surface. A continuous film (whole surface) covering the entire surface of the Cu was formed by a 90-minute chemical vapor reaction, and isolated graphene crystal grains were formed by a 30-minute chemical vapor reaction. Depending on the reaction time, it is possible to form anything from isolated graphene crystal grains to a continuous film covering the entire surface of the Cu. In addition, more than 90% of the area of the graphene formed is a single layer.
[0073] <Oxidation of graphene / Cu / sapphire substrate in water> 3 ml of ultrapure water (Milli-Q) was placed in a 50 ml sample tube, and the laminate 1a (all-surface and grain) in which graphene was formed on the Cu / sapphire substrate described above was immersed in the ultrapure water in the beaker. This was placed in a thermostatic chamber set at 40°C and left to stand for 4 to 72 hours to perform an oxidation treatment on the Cu surface.
[0074] Example 1 After the oxidation treatment of the Cu surface, adhesive sheet 1 was attached to the graphene side of laminate 1a using a roller (pressure of 2 kg / 10 mm), and the laminate was autoclaved at 50°C and 5 atmospheres for 30 minutes. After leaving the laminate at room temperature and normal pressure for 30 minutes, it was peeled off at a peel angle of 180 degrees and a peel speed of 300 mm / min to transfer the graphene from the Cu / sapphire substrate to the adhesive sheet 1, thereby obtaining laminate 1b. Thereafter, the graphene side of the laminate 1b was placed on a silicon substrate with an oxide film (SUMCO silicon (crystal plane (100)), surface thermal oxidation-oxide film thickness 300 nm) and attached with a roller (pressure of 2 kg / 10 mm) to obtain a laminate 1c. The laminate 1c was left to stand at room temperature and normal pressure for 30 minutes, and then irradiated with a UV irradiator (Nitto Seiki UM-810) at 450 mJ / cm from the substrate side of the adhesive sheet 1. 2 The adhesive sheet 1 was peeled off at a peel angle of 180 degrees and a peel speed of 300 mm / min, and the graphene of the laminate 1a was transferred to the silicon substrate to obtain a laminate of the silicon substrate and graphene of Example 1.
[0075] Example 2 The same operation as in Example 1 was carried out except that the adhesive sheet 1 in Example 1 was changed to adhesive sheet 2, thereby obtaining a laminate of a silicon substrate and graphene of Example 2.
[0076] Example 3 The same operation as in Example 1 was carried out except that the adhesive sheet 1 in Example 1 was changed to adhesive sheet 3, thereby obtaining a laminate of a silicon substrate and graphene of Example 3.
[0077] [Examples 4 to 7] Laminates of silicon substrate and graphene of Examples 4 to 7 were obtained in the same manner as in Example 1, except that the peel angle when transferring graphene from the Cu / sapphire substrate to the adhesive sheet was changed to the angle shown in Table 3 and the peel speed was changed to 1000 mm / min. The graphene transferred from the Cu / sapphire substrate to the adhesive sheet was observed. The graphene obtained in Examples 4 and 5 had almost no cracks and was relatively good. The graphene obtained in Examples 6 and 7 had cracks in a direction approximately perpendicular to the peeling direction (direction from the start of peeling to the end of peeling). The observation results are shown in Table 3.
[0078] [Examples 8 to 13] Laminates of silicon substrate and graphene for Examples 8 to 13 were obtained in the same manner as in Example 1, except that the peel angle when transferring graphene from the Cu / sapphire substrate to the adhesive sheet was changed to 20 degrees and the peel speed was changed to the speeds shown in Table 4. The graphene transferred from the Cu / sapphire substrate to the adhesive sheet was observed. The graphene obtained in Examples 8 and 9 had almost no cracks and was relatively good. The graphene obtained in Examples 10 to 12 had cracks and was broken overall. The graphene obtained in Example 13 had no cracks and was good. The observation results are shown in Table 4.
[0079] [Examples 14 to 19] The same operation as in Example 1 was carried out except that the adhesive sheet 1 in Example 1 was changed to adhesive sheets 6 to 11, thereby obtaining laminates of silicon substrates and graphene of Examples 14 to 19.
[0080] Example 20 (MoS2 CVD deposition) A sapphire substrate (c-face, manufactured by Kyocera Corporation) was placed inside a quartz tube (inner diameter 26 mmφ) set in a ceramic tubular furnace at Asahi Rika Seisakusho as a substrate for film formation of molybdenum disulfide (MoS2), a type of transition metal chalcogenide. In addition, a crucible containing molybdenum trioxide powder, the raw material, was placed in the upstream region of the gas flow relative to the film formation substrate inside the quartz tube, and a crucible containing sulfur powder was placed in the upstream region further upstream. The sapphire substrate used was 10 mm square, and 10 to 50 mg of molybdenum trioxide and 50 to 200 mg of sulfur were used. The distance between the sapphire substrate and each crucible was as follows: the sapphire substrate requiring the highest reaction temperature was placed at the center of the tubular furnace, the molybdenum trioxide crucible was placed 10 to 20 cm away from it, and the sulfur crucible was placed 15 to 25 cm away from the molybdenum trioxide crucible. Then, under atmospheric pressure, the sapphire substrate and each crucible were heated to a predetermined temperature (substrate: 850-950°C, molybdenum trioxide: 580-600°C, sulfur: 100-200°C) while flowing argon, and a chemical vapor reaction was carried out for 30 minutes. After the reaction, the substrate was cooled to room temperature (23°C), and the sapphire substrate on which isolated MoS2 crystal grains had been generated was removed from the quartz tube. Through this reaction, MoS2 with a crystal grain size of about 5-50 μm was formed on the surface of the sapphire substrate (laminate 20a (grain)).
[0081] (Method of peeling / transferring MoS2 grown on a sapphire substrate from the sapphire substrate) An adhesive sheet 1 was attached to the MoS2 side of the laminate 20a (grain) with a roller (2 kg / 10 mm pressure), autoclaved at 50° C. and 5 atm for 30 minutes, and then left to stand at room temperature and pressure for 30 minutes. Thereafter, the laminate 20b (adhesive sheet / MoS2 / sapphire substrate) was immersed in a potassium hydroxide aqueous solution with a concentration of 1 mol / L. As a result, the potassium hydroxide etched only the outermost surface of the sapphire substrate, and MoS2 was transferred from the sapphire substrate to the adhesive sheet 1, thereby obtaining a laminate 20c. Thereafter, the laminate 20c was placed so that the MoS2 side was in contact with a silicon substrate with an oxide film (SUMCO silicon (crystal surface (100)), surface thermally oxidized-oxide film thickness 300 nm) and was bonded with a roller (pressure of 2 kg / 10 mm) to obtain the laminate 20d. The laminate 20d is left to stand at room temperature and normal pressure for 30 minutes, and then is irradiated with a UV irradiator (UM-810 manufactured by Nitto Seiki Co., Ltd.) at 450 mJ / cm from the substrate side of the adhesive sheet 1. 2 The adhesive sheet 1 was peeled off at a peel angle of 180 degrees and a peel speed of 300 mm / min, and the MoS2 of the laminate 20c was transferred to the silicon substrate, thereby obtaining a laminate of the silicon substrate and MoS2 of Example 20.
[0082] Example 21 (CVD deposition of WS2) A sapphire substrate (c-face, manufactured by Kyocera Corporation) was placed inside a quartz tube (inner diameter 26 mmφ) set in a ceramic tubular furnace at Asahi Rika Seisakusho, as a substrate for deposition of tungsten disulfide (WS2), a type of transition metal chalcogenide. In addition, a crucible containing tungsten trioxide powder, the raw material, was placed in the upstream region of the gas flow relative to the deposition substrate inside the quartz tube, and a crucible containing sulfur powder was placed in the upstream region further upstream. The sapphire substrate used was 10 mm square, and 10 to 50 mg of tungsten trioxide and 50 to 200 mg of sulfur were used. The distance between the sapphire substrate and each crucible was as follows: the tungsten trioxide crucible, which requires the highest reaction temperature, was placed in the center of the tubular furnace, the sapphire substrate was placed 5 to 15 cm away from it, and the sulfur crucible was placed 15 to 25 cm away from the molybdenum trioxide crucible. Then, under atmospheric pressure, the sapphire substrate and each crucible were heated to a specified temperature (substrate: 900-1000°C, tungsten trioxide: 1050-1100°C, sulfur: 100-200°C) while flowing argon, and a chemical vapor reaction was carried out for 30 minutes. After the reaction, the substrate was cooled down to room temperature (23°C), and the sapphire substrate on which isolated WS2 crystal grains had been generated was removed from the quartz tube. By this reaction, WS2 having a crystal grain size of about 5 to 50 μm was formed on the surface of the sapphire substrate (laminate 21a (grain)).
[0083] (Method of peeling / transferring WS2 grown on a sapphire substrate from the sapphire substrate) Adhesive sheet 1 was attached to the WS2 side of laminate 21av with a roller (pressure of 2 kg / 10 mm), autoclaved at 50° C. and 5 atm for 30 minutes, and then left to stand at room temperature and normal pressure for 30 minutes. Thereafter, the laminate 21b (adhesive sheet / WS2 / sapphire substrate) was immersed in a 1 mol / L aqueous potassium hydroxide solution, whereby the potassium hydroxide etches only the outermost surface of the sapphire, transferring WS2 from the sapphire substrate to the adhesive sheet 1 to obtain a laminate 21c. Thereafter, the WS2 side surface of the laminate 21c was placed in contact with a silicon substrate with an oxide film (SUMCO silicon (crystal face (100)), surface thermal oxidation-oxide film thickness 300 nm) and was attached with a roller (pressure of 2 kg / 10 mm) to obtain a laminate 21d. The laminate 21d was left to stand at room temperature and normal pressure for 30 minutes, and then irradiated with 450 mJ / cm from the substrate side of the adhesive sheet 1 with a UV irradiator (Nitto Seiki UM-810). 2 The adhesive sheet 1 was peeled off at a peel angle of 180 degrees and a peel speed of 300 mm / min, and WS2 of the laminate 21c was transferred to the silicon substrate to obtain a laminate of the silicon substrate and WS2 of Example 21.
[0084] Example 22 (CVD deposition of h-BN) An iron-nickel alloy foil substrate (manufactured by Nilaco) was placed inside an alumina tube (inner diameter 39 mm) set in a ceramic tubular furnace at Asahi Rika Seisakusho Co., Ltd., as a substrate for forming an h-BN film. The iron-nickel alloy foil substrate used was 10 mm square. Then, the temperature was raised to the specified temperature (1000-1200°C) under reduced pressure (10-1000 Pa) while flowing argon and hydrogen. After reaching the specified temperature, the substrate was held under the same conditions for 0-3 hours to reduce and smooth the surface of the iron-nickel alloy substrate. Borazine was then added so that the partial pressure was 1 Pa or less, and a chemical vapor reaction was carried out for 30 minutes. After the reaction, the temperature was allowed to reach room temperature (23°C), and the iron-nickel alloy foil substrate on which the multi-layered h-BN had been formed was removed from the alumina tube. Through this reaction, a multi-layered h-BN film with a thickness of about 1 to 50 nm was formed on the entire surface of the iron-nickel alloy substrate (laminate 22a (entire surface)).
[0085] (Method of peeling off h-BN grown on a catalyst substrate from the catalyst) Adhesive sheet 1 was attached to the h-BN side of laminate 22a with a roller (2 kg / 10 mm pressure), autoclaved at 50° C. and 5 atm for 30 minutes, and then left to stand at room temperature and pressure for 30 minutes. Thereafter, the laminate 22b (adhesive sheet / h-BN / iron-nickel alloy foil) was immersed in hydrochloric acid with a concentration of 1 mol / L. As a result, the hydrochloric acid etches the surface of the iron-nickel alloy substrate, and hydrogen gas is generated between the iron-nickel alloy substrate and the h-BN, and the h-BN is transferred from the iron-nickel alloy substrate to the adhesive sheet 1 to obtain the laminate 22c. Thereafter, the laminate 22c was placed so that the h-BN side was in contact with a silicon substrate with an oxide film (SUMCO silicon (crystal surface (100)), surface thermal oxidation-oxide film thickness 90 nm) and was bonded with a roller (pressure of 2 kg / 10 mm) to obtain the laminate 22d. The laminate 22d is left to stand for 30 minutes at room temperature and normal pressure, and then is irradiated with a UV irradiator (UM-810 manufactured by Nitto Seiki Co., Ltd.) at 450 mJ / cm from the substrate side of the adhesive sheet 1. 2 The adhesive sheet 1 was peeled off at a peel angle of 180 degrees and a peel speed of 300 mm / min, and the h-BN of the laminate 22c was transferred to the silicon substrate to obtain a laminate of silicon substrate and h-BN of Example 22.
[0086] Comparative Example 1 A laminate of a silicon substrate and graphene of Comparative Example 1 was obtained by carrying out the same operation as in Example 1, except that the adhesive sheet 1 in Example 1 was changed to the adhesive sheet 4 and the UV treatment was changed to a heat treatment.
[0087] Comparative Example 2 A laminate of a silicon substrate and graphene of Comparative Example 2 was obtained by carrying out the same operation as in Example 1, except that the adhesive sheet 1 in Example 1 was changed to adhesive sheet 5 and no UV treatment was carried out.
[0088] The laminates obtained in Examples 1 to 3, 14 to 22, and Comparative Examples 1 and 2 are shown in Tables 1 and 2.
[0089] [Table 1]
[0090] [Table 2]
[0091] <Surface roughness> Each of the pressure-sensitive adhesive sheets 1 to 3 and 6 to 11 prepared above was cut to a width of 20 mm and a length of 10 cm, subjected to UV treatment, and the release liner was peeled off and removed. The adhesive sheet 4 prepared above was cut to a width of 20 mm and a length of 10 cm, and subjected to a heat treatment, and the release liner was peeled off and removed. The adhesive sheet 5 prepared above was cut to a width of 20 mm and a length of 10 cm, and the release liner was peeled off and removed.
[0092] The UV treatment was performed using a UV irradiator (Nitto Seiki UM-810) at 450 mJ / cm from the substrate side of the adhesive sheets 1 to 3. 2 The irradiation dose was 100 μg / kg. The heat treatment was carried out by placing the adhesive sheet 4 on a hot plate heated to 150° C. with the substrate side in contact with the hot plate, and after 1 minute, removing it and cooling it in air.
[0093] The surface roughness of the adhesive surface of the adhesive layer was measured using a white light confocal microscope (Lasertec OPTELICS HYBRID, manufactured by Lasertec Corporation) with a 20x objective lens and the software "LMeye7". The adhesive layer was attached to a separate silicon wafer, and then the adhesive strength was reduced by heat or ultraviolet light, and the adhesive surface was peeled off and measured by focusing on the top surface of the adhesive layer and scanning a range of 50 μm up and down. The measured image of 750 μm square was also used to calculate Ra at five points on an arbitrary line in the surface roughness line profile using the software "LMeye7", and the average value was taken as the adhesive surface roughness (μm) after triggering.
[0094] <Adhesive strength measurement> For the pressure-sensitive adhesive sheets 1 to 3 and 6 to 11 prepared above, the adhesive strength (initial) before UV treatment was measured. The adhesive strength was measured by cutting each of the adhesive sheets 1 to 3 and 6 to 11 to a width of 20 mm and a length of 10 cm, and then peeling off and removing the release liner. Next, the adhesive sheet of each example was attached to a silicon wafer (4-inch silicon mirror wafer) by pressing it back and forth once with a 2 kg roller. Using a tensile testing machine (AUTOGRAPH AGS-X, manufactured by Shimadzu Corporation), the force at a peel angle of 180 degrees and a peel speed of 300 mm / min was measured as adhesive strength (initial peel force at 180°C from silicon wafer) (N / 20 mm).
[0095] The adhesive strength after UV treatment (180°C peeling force from silicon wafer (after trigger)) (N / 20 mm) was measured using the same procedure as above, except that the adhesive sheet was pressed onto a silicon wafer (4-inch silicon mirror wafer) and then UV treatment was performed. The UV treatment was performed using a UV irradiator (Nitto Seiki UM-810) at 450 mJ / cm from the substrate side of the adhesive sheets 1-3 and 6-11. 2 The irradiation dose was 100 μg / kg.
[0096] The adhesive strength (initial) of the pressure-sensitive adhesive sheet 4 produced above before heat treatment was measured. The adhesive strength was measured by cutting the adhesive sheet 4 to a width of 20 mm and a length of 10 cm, and peeling off the release liner. Next, the adhesive sheet of each example was attached to a silicon wafer (4-inch silicon mirror wafer) by pressing it back and forth once with a 2 kg roller. Using a tensile tester (AUTOGRAPH AGS-X, manufactured by Shimadzu Corporation), the force at the time of peeling at a peel angle of 180 degrees and a peel speed of 300 mm / min was measured as adhesive strength (initial) (N / 20 mm).
[0097] The adhesive strength (after trigger) (N / 20 mm) after heat treatment was measured using the same procedure as above, except that the adhesive sheet was pressed onto a silicon wafer (4-inch silicon mirror wafer) and then heat treated. The heat treatment was carried out by placing the silicon wafer side on a hot plate heated to 150° C. so that the silicon wafer side was in contact with the hot plate, and after 1 minute, the silicon wafer was removed and cooled in air.
[0098] The adhesive strength (initial) of the pressure-sensitive adhesive sheet 5 produced above before heat treatment was measured. The adhesive strength was measured by cutting the adhesive sheet 5 to a width of 20 mm and a length of 10 cm, and then peeling off the release liner. Next, the adhesive sheet of each example was attached to a silicon wafer (4-inch silicon mirror wafer) by pressing it back and forth once with a 2 kg roller. Using a tensile tester (AUTOGRAPH AGS-X, manufactured by Shimadzu Corporation), the force at the time of peeling at a peel angle of 180 degrees and a peel speed of 300 mm / min was measured as adhesive strength (initial) (N / 20 mm).
[0099] <Transfer rate> (Graphene transfer rate (all over)) The images of graphene remaining on the surface of the transferred material of the laminate (whole surface) of the silicon substrate and graphene obtained in Examples 1 to 3, 14 to 19, and Comparative Examples 1 and 2 were obtained as digital images using a metal microscope (Nikon ME600) and a CCD camera (Nikon DS-Fi1). The digital images were observed with a 50x objective lens, with a field of view of 160 μm × 120 μm, and digital images of three arbitrary locations were obtained. Using the obtained digital images, RGB separation and binarization analysis of each component image were performed using the software "Win ROOF" (Mitani Shoji), and the area ratio of graphene in the corresponding digital image was calculated as a percentage. The average value of the area ratio of graphene in the digital images of the three locations was taken as the transfer rate (whole surface).
[0100] (Graphene transfer rate (grain)) After the laminate 1a (grain) in which graphene was formed on the Cu / sapphire substrate described above was oxidized in water, an observation image of the graphene (grain) on the Cu / sapphire substrate was obtained as a digital image using a metallurgical microscope (Nikon ME600) and a CCD camera (Nikon DS-Fi1) before the adhesive sheet 1 was attached. The digital images were observed with a 50x objective lens, with a field of view of 160 μm×120 μm, and digital images were taken at three random locations.
[0101] Next, an observation image of the graphene transferred to the surface of a transfer material in the laminate (grain) of the silicon substrate and graphene obtained in Example 1 was obtained as a digital image using a similar metallurgical microscope and CCD camera at a position corresponding to the previously obtained observation image of the graphene (grain) on the Cu / sapphire substrate.
[0102] From each digital image, the area ratio of the graphene (grain) on the Cu / sapphire substrate previously obtained to the graphene (grain) on the silicon substrate at the corresponding position was calculated as a percentage. The average value of the graphene area ratio in the digital images at three locations was taken as the transfer rate (grain).
[0103] FIG. 6 shows a group of graphene crystal grains on a Cu substrate before adhesive tape was attached. The image of the graphene crystal grains after the graphene / Cu / sapphire substrate of Example 1 was oxidized in water. The image was taken as a digital image using a metallurgical microscope (Nikon ME600) and a CCD camera (Nikon DS-Fi1). FIG. 7 shows an image of graphene on the surface of the laminate of silicon substrate and graphene in Example 1, as a two-dimensional material grain group on a transfer material transferred by adhesive tape, which was acquired as a digital image by a metallurgical microscope (Nikon ME600) and a CCD camera (Nikon DS-Fi1).
[0104] The graphene crystal grains in Figures 6 and 7 were compared by microscopic observation and image analysis was performed to calculate the transfer rate (grain). Similarly, image analysis was performed for Examples 2, 3, and 14 to 19, and Comparative Examples 1 to 3 to determine the grain transfer rates.
[0105] (Transfer rate (grain) of MoS2 and WS2) Before the adhesive sheet 1 was attached to the laminate 20a, an observation image of MoS2 on the sapphire substrate formed by CVD was obtained as a digital image using a metallurgical microscope (Nikon ME600) and a CCD camera (Nikon DS-Fi1). The digital image was an observation image with a 50x objective lens, with a field of view of 160 μm × 120 μm, and digital images were obtained at three arbitrary locations. Next, an image of MoS2 remaining on the surface of the transfer material (silicon substrate) of the laminate of silicon substrate and MoS2 obtained in Example 20 was obtained as a digital image by the same metal microscope and CCD camera at a position corresponding to the previously obtained observation image of MoS2 on the sapphire substrate. The area ratio of MoS2 on the silicon substrate at the position corresponding to the previously obtained MoS2 on the sapphire substrate was calculated as a percentage. The average value of the area ratio of MoS2 in the digital images at three points was taken as the transfer rate. The transcription rate (grain) of WS2 was determined by the same procedure.
[0106] (h-BN transfer rate (all over)) The transfer rate of h-BN (overall surface) was determined by the same procedure as for the transfer rate of graphene (overall surface).
[0107] [Table 3]
[0108] [Table 4] [Industrial Applicability]
[0109] According to the present invention, it is possible to provide a laminate and a method for manufacturing a two-dimensional material laminate, which are excellent in productivity and capable of transferring a two-dimensional material at a high transfer rate.
[0110] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made therein without departing from the spirit and scope of the invention. This application is based on a Japanese patent application (Patent Application No. 2019-027773) filed on February 19, 2019, the contents of which are incorporated herein by reference. [Explanation of symbols]
[0111] 101, 102, 103, 104: laminate 10: Adhesive sheet 11: Base material 12: Adhesive layer 21: First substrate 30: Two-dimensional materials 40: Second substrate 105: Two-dimensional material laminate
Claims
1. A step of transferring the two-dimensional material on the first substrate to a surface of an adhesive sheet having a base material and an adhesive layer whose adhesive strength is reduced by ultraviolet light, thereby obtaining a laminate of the adhesive sheet and the two-dimensional material; placing the laminate on a second substrate such that a surface of the laminate facing the two-dimensional material is in contact with the second substrate; exposing the laminate to the ultraviolet light; and transferring the two-dimensional material onto the second substrate by peeling off the adhesive sheet; the step of applying ultraviolet light to the laminate is performed after the step of placing the laminate on the second substrate; an adhesive strength A of the pressure-sensitive adhesive layer to a silicon wafer at 25° C. before exposure to the ultraviolet light is 1.0 N / 20 mm to 20.0 N / 20 mm when subjected to a 180° peel at a tensile speed of 300 mm / min; the adhesive strength B of the pressure-sensitive adhesive layer to a silicon wafer at 25° C. after exposure to the ultraviolet light is 0.01 N / 20 mm to 1.00 N / 20 mm when subjected to a 180° peel at a tensile speed of 300 mm / min; the surface roughness of the adhesive surface of the pressure-sensitive adhesive layer after the application of the ultraviolet rays is 0.01 μm to 8.00 μm; A method for manufacturing a two-dimensional material stack.
2. The method for producing a two-dimensional material stack according to claim 1 , wherein the two-dimensional material is a two-dimensional carbon material, molybdenum disulfide, tungsten disulfide, or hexagonal boron nitride.
3. The method for producing a two-dimensional material laminate according to claim 2 , wherein the two-dimensional carbon material is graphene or a graphene derivative.
4. The method for producing a two-dimensional material laminate according to claim 2 or 3, wherein the adhesive layer contains an ultraviolet-curable adhesive.
5. The method for producing a two-dimensional material laminate according to any one of claims 2 to 4, wherein the base material has ultraviolet light transmissibility.
6. The method for producing a two-dimensional material laminate according to claim 5, wherein the transfer rate of the two-dimensional material is 30% or more.
7. A laminate of a substrate, a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer whose adhesive strength is reduced by ultraviolet light, and a two-dimensional material, the adhesive strength A of the pressure-sensitive adhesive layer to a silicon wafer at 25° C. before exposure to ultraviolet light is 1.0 N / 20 mm to 20.0 N / 20 mm when subjected to a 180° peel at a tensile speed of 300 mm / min; the adhesive strength B of the pressure-sensitive adhesive layer to a silicon wafer at 25° C. after exposure to the ultraviolet light is 0.01 N / 20 mm to 1.00 N / 20 mm when subjected to a 180° peel at a tensile speed of 300 mm / min; The surface roughness of the adhesive surface of the adhesive layer after exposure to the ultraviolet light is 0.01 μm to 8.00 μm.
8. 8. The stack of claim 7, wherein the two-dimensional material is a two-dimensional carbon material, molybdenum disulfide, tungsten disulfide, or hexagonal boron nitride.
9. The laminate according to claim 8 , wherein the two-dimensional carbon material is graphene or a graphene derivative.
10. The laminate according to claim 8 or 9, wherein the pressure-sensitive adhesive layer comprises an ultraviolet-curable pressure-sensitive adhesive.
11. The laminate according to any one of claims 8 to 10, wherein the substrate has ultraviolet light transmissibility.
Citation Information
Patent Citations
Manufacture of shielded cast transformer
JP1983050720A
Thermally strippable pressure-sensitive adhesive sheet and method of recovering adherend
JP2008115273A
Energy-ray curing type polymer, energy-ray curing type adhesive composition, adhesive sheet, and processing method of semiconductor wafer
JP2009242733A
Adhesive member for temporarily fixing brittle member
JP2014172989A
Pellicle film for photolithography, and pellicle
JP2019008089A
Cited By