Adhesives and adhesive tapes
The adhesive tape, composed of an acrylic polymer with an acid functional group and a crystalline resin, addresses adhesive strength loss from oil and alcohol contact by enhancing adhesion and resistance, providing durable bonding across diverse surfaces.
Patent Information
- Application Number
- JP2020074819
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-26
- Filing Date
- 2020-04-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-04-20
AI Technical Summary
Adhesive tapes experience a decrease in adhesive strength when coming into contact with oil or alcohol components, leading to peeling issues.
The adhesive tape incorporates an acrylic polymer with an acid functional group and a crystalline resin with a melting point of 25°C or higher, which includes a polyolefin resin, maleic anhydride-modified polyolefin resin, or acrylic modified polyolefin resin, along with additives like C5 and C9 petroleum resins, to enhance adhesive properties and resistance to oils and alcohols.
The adhesive tape maintains strong adhesion to both metallic and non-metallic surfaces, exhibits excellent heat and chemical resistance, and prevents adhesive strength degradation from contact with oils and alcohols, ensuring reliable bonding in various applications.
Smart Images

Figure 0007558677000004 
Figure 0007558677000001 
Figure 0007558677000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive and an adhesive tape. [Background technology]
[0002] Conventionally, adhesive tapes and double-sided tapes have been used for surface protection, insulation protection, component joining or fixing, etc., by being attached to various components. However, when used in applications that involve human hands, secretions such as sebum and fingerprints, chemicals such as cosmetics, hair styling products, moisturizing creams, and sunscreens, and oils contained in foods, etc., are likely to adhere through the fingertips. In addition to oils, alcohol components such as ethanol contained in perfumes, disinfectant sheets, and disinfectant alcohol are also components that are likely to adhere when used in a living environment. In such a usage form, if components such as oils and alcohols come into contact with the adhesive layer of the adhesive sheet, the adhesive strength will decrease, and problems such as peeling may occur. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-215355 A [Patent Document 2] JP 2013-100485 A [Patent Document 3] JP 2017-132911 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made to solve the problems in the related art, and an object of the present invention is to provide an adhesive tape that is inhibited from losing adhesive strength when it comes into contact with oil or alcohol components. [Means for solving the problem]
[0005] The pressure-sensitive adhesive of the present invention is an adhesive that exhibits adhesiveness through pressure-sensitive adhesion, and contains an acrylic polymer having an acid functional group and a crystalline resin having a melting point of 25° C. or higher. In one embodiment, the pressure-sensitive adhesive exhibits adhesiveness upon heating. In one embodiment, the acrylic polymer having an acid functional group has a structural unit a derived from a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 4 or more carbon atoms. In one embodiment, the content of the structural unit a is 50 parts by weight or more based on 100 parts by weight of the acrylic polymer having an acid functional group. In one embodiment, the crystalline resin is a polyolefin resin. In one embodiment, the polyolefin resin is a maleic anhydride-modified polyolefin resin, a maleic acid-modified polyolefin resin, or an acrylic-modified polyolefin resin. In one embodiment, the adhesive comprises a C5-based petroleum resin and / or a C9-based petroleum resin. According to another aspect of the present invention, there is provided an adhesive tape comprising the above-mentioned adhesive. In one embodiment, the pressure-sensitive adhesive tape comprises a substrate and a pressure-sensitive adhesive layer disposed on at least one side of the substrate, the pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive. In one embodiment, the substrate is formed from at least one selected from polyacrylate, polyurethane, polyimide, aramid, polyamide, ethylene-vinyl alcohol copolymer, polyetherimide, polyvinylidene fluoride, polyester, polypropylene, polyethylene, and polyphenylene sulfide. In one embodiment, the pressure-sensitive adhesive tape has a release film provided on the side of the pressure-sensitive adhesive layer opposite to the substrate. Effect of the Invention
[0006] According to the present invention, it is possible to provide an adhesive that suppresses the decrease in adhesive strength when it comes into contact with oil or alcohol, and an adhesive tape containing the adhesive. The adhesive of the present invention also exhibits excellent adhesion to both metallic and non-metallic adherends. Furthermore, the adhesive of the present invention has excellent heat resistance and chemical resistance, and can exhibit excellent adhesion and bonding properties in various applications. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic cross-sectional view of an adhesive tape according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] A. Adhesive The adhesive of the present invention is an adhesive that exhibits adhesiveness by pressure bonding, and includes an acrylic polymer having an acid functional group and a crystalline resin having a melting point of 25° C. or higher. In the present invention, by using an acrylic polymer having an acid functional group in combination with the crystalline resin, an adhesive that is excellent in heat resistance and chemical resistance and suppresses a decrease in adhesive strength when contacted with oil or alcohol components can be obtained. In addition, if the adhesive of the present invention is used in a double-sided adhesive tape, it can be suitably used for bonding metal materials to metal materials, bonding nonmetal materials to nonmetal materials, and bonding metal materials to nonmetal materials.
[0009] The pressure-sensitive adhesive may be an adhesive that exhibits adhesiveness at room temperature (25° C.), or an adhesive that exhibits adhesiveness upon heating (for example, 100° C. to 200° C.). An adhesive that exhibits adhesiveness upon heating may exhibit adhesiveness in a state cooled to room temperature after heating.
[0010] A-1. Acrylic polymers with acid functional groups Examples of acrylic polymers having an acid functional group include acrylic polymers containing one or more types of constituent units derived from (meth)acrylic acid alkyl esters, and constituent units derived from monomers having an acid functional group.
[0011] In the above adhesive, the content of the acrylic polymer having an acid functional group is preferably 7 parts by weight to 95 parts by weight, more preferably 15 parts by weight to 90 parts by weight, further preferably 20 parts by weight to 85 parts by weight, and particularly preferably 40 parts by weight to 85 parts by weight, based on 100 parts by weight of the solid content in the adhesive. The content of the acrylic polymer having an acid functional group can be an appropriate amount depending on the desired adhesiveness, etc. In addition, the above adhesive may contain an acrylic polymer not having an acid functional group in addition to the acrylic polymer having an acid functional group, or may not contain an acrylic polymer not having an acid functional group.
[0012] The content of the structural unit derived from the (meth)acrylic acid alkyl ester is preferably 50 to 99 parts by weight, more preferably 70 to 98 parts by weight, and even more preferably 80 to 98 parts by weight, relative to 100 parts by weight of the acrylic polymer having an acid functional group.
[0013] Preferably, the (meth)acrylic acid alkyl ester has a linear or branched alkyl group having 1 to 24 carbon atoms (more preferably 3 to 20, even more preferably 4 to 12, and particularly preferably 4 to 8).
[0014] Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, and eicosyl (meth)acrylate.
[0015] In one embodiment, the acrylic polymer having an acid functional group has a structural unit a derived from a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 4 or more carbon atoms (preferably 4 to 12, more preferably 4 to 8), and the content of the structural unit a is 50 parts by weight or more (preferably 50 parts by weight to 99 parts by weight, more preferably 70 parts by weight to 98 parts by weight, and even more preferably 80 parts by weight to 98 parts by weight) relative to 100 parts by weight of the acrylic polymer having an acid functional group. By using an acrylic polymer having an acid functional group containing a predetermined amount or more of the structural unit a, a pressure-sensitive adhesive having excellent heat resistance and chemical resistance and suppressing a decrease in adhesive strength when contacted with oil or alcohol components can be obtained.
[0016] In one embodiment, a (meth)acrylic acid alkyl ester having a branched alkyl group is used as the (meth)acrylic acid alkyl ester. By using a (meth)acrylic acid alkyl ester having a branched alkyl group, a pressure-sensitive adhesive tape having excellent chemical resistance can be obtained. The number of carbon atoms in the branched alkyl group is preferably 4 or more, more preferably 4 to 12, and even more preferably 4 to 8. A (meth)acrylic acid alkyl ester having a linear alkyl group and a (meth)acrylic acid alkyl ester having a branched alkyl group may be used in combination. Also, a (meth)acrylic acid alkyl ester having a branched alkyl group may be used alone as the (meth)acrylic acid alkyl ester.
[0017] In one embodiment, in the acrylic polymer having an acid functional group, the content of the structural units derived from an alkyl (meth)acrylate having a branched alkyl group is preferably 50 to 100 parts by weight, more preferably 70 to 100 parts by weight, and even more preferably 80 to 100 parts by weight, per 100 parts by weight of the structural units derived from an alkyl (meth)acrylate (i.e., 100 parts by weight of the total amount of the alkyl (meth)acrylate having a linear alkyl group and the alkyl (meth)acrylate having a branched alkyl group).
[0018] Examples of (meth)acrylic acid alkyl esters having a branched alkyl group include isobutyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, and 2-methylbutyl (meth)acrylate. Among these, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, or isodecyl (meth)acrylate is preferred, and 2-ethylhexyl (meth)acrylate is more preferred. By using 2-ethylhexyl (meth)acrylate, it is possible to obtain a pressure-sensitive adhesive that is suppressed from decreasing in adhesive strength when it comes into contact with oil or alcohol components.
[0019] Examples of the acid functional group of the acrylic polymer having an acid functional group include a carboxyl group, an acid anhydride group, a phosphoric acid group, and a sulfonic acid group. Therefore, examples of the monomer having the acid functional group include a carboxyl group-containing monomer, an acid anhydride group-containing monomer, a phosphoric acid group-containing monomer, and a sulfonic acid group-containing monomer. Among them, a carboxyl group-containing monomer is preferable. If a carboxyl group-containing monomer is used, the adhesive strength to the metal plate is easily expressed, and in terms of design and production, it is easy to copolymerize with other acrylic monomers, and the polymer produced by the copolymerization is easy to crosslink.
[0020] Examples of the carboxyl group-containing monomer include (meth)acrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, etc. Of these, acrylic acid is preferred.
[0021] The content of the structural unit derived from the monomer having an acid functional group is preferably 1.5 to 20 parts by weight, more preferably 1.8 to 15 parts by weight, and even more preferably 2 to 10 parts by weight, relative to 100 parts by weight of the acrylic polymer having an acid functional group.
[0022] The acrylic polymer having an acid functional group may contain, as necessary, a structural unit derived from another monomer copolymerizable with the (meth)acrylic acid alkyl ester and / or the monomer having an acid functional group, for the purpose of modifying cohesive strength, heat resistance, crosslinkability, etc. Examples of such other monomers include hydroxyl group-containing monomers such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxydecyl (meth)acrylate, hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl methacrylate; (N-substituted) amide monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, and N-methylolpropane(meth)acrylamide; (meth)acrylamide such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; ) Aminoalkyl acrylate monomers; (meth)acrylic acid alkoxyalkyl monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide and N-laurylitaconimide; succinimide monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide;Vinyl monomers such as vinyl acetate, vinyl propionate, N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, N-vinyl carboxylic acid amides, styrene, α-methylstyrene, and N-vinylcaprolactam; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing acrylic monomers such as glycidyl (meth)acrylate; glycol-based acrylic ester monomers such as polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate; tetrahydrofuran (meth)acrylate Examples of the monomers include acrylic acid ester monomers having heterocyclic rings, halogen atoms, silicon atoms, etc., such as furfuryl, fluorine (meth)acrylate, and silicone (meth)acrylate; polyfunctional monomers such as hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; olefin monomers such as isoprene, butadiene, and isobutylene; and vinyl ether monomers such as vinyl ether. These monomer components may be used alone or in combination of two or more.
[0023] The content of the structural units derived from the other monomers is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, and even more preferably 5 parts by weight or less, based on 100 parts by weight of the acrylic polymer having an acid functional group.
[0024] The weight average molecular weight of the acrylic polymer having an acid functional group is preferably from 300,000 to 2,000,000, and more preferably from 500,000 to 1,500,000. The weight average molecular weight can be measured by GPC (solvent: THF).
[0025] A-2. Crystalline resin As described above, the pressure-sensitive adhesive of the present invention contains a crystalline resin. The crystalline resin refers to a resin that has a clear endothermic peak (half-value width within 15° C.) in a differential calorimeter curve measured by a differential scanning calorimeter (DSC).
[0026] The content of the crystalline resin in the adhesive is preferably 3 to 90 parts by weight, more preferably 10 to 85 parts by weight, and even more preferably 15 to 80 parts by weight, per 100 parts by weight of the solid content in the adhesive.
[0027] The melting point of the crystalline resin is 25° C. or higher, more preferably 40° C. or higher, further preferably 60° C. to 120° C., and particularly preferably 60° C. to 100° C. Within such a range, a pressure-sensitive adhesive with little stickiness can be obtained. The melting point can be measured by differential scanning calorimetry (DSC).
[0028] The weight average molecular weight of the crystalline resin is preferably from 50,000 to 1.5 million, and more preferably from 70,000 to 1 million.
[0029] The crystallinity of the crystalline resin is preferably 10% or more, more preferably 20% or more. The crystallinity can be typically measured by differential scanning calorimetry (DSC).
[0030] In one embodiment, the crystalline resin is a polyolefin-based resin. Examples of the polyolefin-based resin include ethylene homopolymer, ethylene-propylene copolymer, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer, ethylene-1-heptene copolymer, ethylene-1-octene copolymer, ethylene-1-nonene copolymer, ethylene-1-decene copolymer, ethylene-1-undecene copolymer, ethylene-1-dodecene copolymer, ethylene-1-tridecene copolymer, ethylene-1-tetradecene copolymer, ethylene-1-pentadecene copolymer, and ethylene-1-hexadecene copolymer. ethylene-α-olefin copolymers such as ethylene-1-heptadecene copolymer, ethylene-1-octadecene copolymer, ethylene-1-nanodecene copolymer, and ethylene-1-eicosene copolymer; ethylene-vinyl ester copolymers such as ethylene-vinyl acetate copolymer and ethylene-vinyl propionate copolymer; ethylene-unsaturated carboxylic acid alkyl ester copolymers such as ethylene-methyl methacrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-butyl acrylate copolymer; and propylene-based resins.
[0031] In one embodiment, a crystalline polypropylene-based resin is used as the crystalline resin. The crystalline polypropylene-based resin may be a homopolymer or a copolymer obtained from propylene and a monomer copolymerizable with propylene. Examples of the monomer copolymerizable with propylene include α-olefins such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 4-methyl-1-pentene, and 3-methyl-1-pentene. In the crystalline polypropylene-based resin, the content of the propylene-derived structural unit is preferably 60 mol% to 99 mol%, more preferably 65 mol% to 99 mol%, and even more preferably 70 mol% to 99 mol%. In the crystalline polypropylene-based resin, the content of the α-olefin-derived structural unit is preferably 1 mol% to 15 mol%, and more preferably 1 mol% to 10 mol%.
[0032] In one embodiment, a modified polyolefin resin is used as the crystalline resin. By using a modified polyolefin resin, phase separation between the crystalline resin and the acrylic polymer having an acid functional group is suppressed, and an adhesive layer that is less prone to bleeding and has excellent transparency can be obtained. As the modified polyolefin resin, maleic anhydride-modified polyolefin resin, maleic acid-modified polyolefin resin, acrylic-modified polyolefin resin, etc. can be preferably used. Specifically, resins obtained by modifying the above-mentioned polyolefin resin with maleic anhydride, maleic acid, or acrylic can be mentioned. Among them, maleic anhydride polyolefin resin is preferable, and maleic anhydride-modified propylene resin is more preferable. A specific example of the maleic anhydride-modified propylene resin is a resin obtained by modifying the above-mentioned crystalline polypropylene resin with maleic anhydride. The modification rate of the modified polyolefin resin is preferably 1% by weight to 5% by weight, more preferably 1.5% by weight to 2% by weight.
[0033] A-3. Additives The pressure-sensitive adhesive may contain any suitable additive, if necessary. Examples of the additive include crosslinkers, tackifiers, plasticizers (e.g., trimellitic acid ester plasticizers, pyromellitic acid ester plasticizers), pigments, dyes, fillers, antioxidants, conductive materials, UV absorbers, light stabilizers, release regulators, softeners, surfactants, flame retardants, antioxidants, solvents, etc. The pressure-sensitive adhesive may also contain any suitable solvent.
[0034] As the tackifier, any appropriate tackifier can be used. As the tackifier, for example, a tackifier resin can be used. Specific examples of tackifier resins include rosin-based tackifier resins (e.g., unmodified rosin, modified rosin, rosin phenol-based resins, rosin ester-based resins, etc.), terpene-based tackifier resins (e.g., terpene-based resins, terpene phenol-based resins, styrene-modified terpene-based resins, aromatic modified terpene-based resins, hydrogenated terpene-based resins), hydrocarbon-based tackifier resins (e.g., aliphatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aromatic hydrocarbon resins (e.g., styrene-based resins, xylene-based resins, etc.), aliphatic and aromatic petroleum resins, aliphatic and alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone-based resins, coumarone-indene resins, etc.), phenol-based tackifier resins (e.g., alkylphenol-based resins, xylene formaldehyde-based resins, resols, novolacs, etc.), ketone-based tackifier resins, polyamide-based tackifier resins, epoxy-based tackifier resins, elastomer-based tackifier resins, etc.
[0035] In one embodiment, the pressure-sensitive adhesive contains a C5 petroleum resin and / or a C9 petroleum resin as a tackifier, which can provide good adhesion to non-polar adherends such as polypropylene.
[0036] The softening point of the tackifier is preferably 70° C. to 200° C., and more preferably 80° C. to 190° C. Within such a range, a pressure-sensitive adhesive layer with appropriately adjusted storage modulus and loss modulus can be obtained.
[0037] The content of the tackifier is preferably 5 to 50 parts by weight, and more preferably 10 to 40 parts by weight, per 100 parts by weight of the total amount of the acrylic polymer having an acid functional group and the crystalline resin having a melting point of 25°C or higher.
[0038] Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, as well as urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, amine-based crosslinking agents, etc. Among these, isocyanate-based crosslinking agents, epoxy-based crosslinking agents, and metal chelate-based crosslinking agents are preferred.
[0039] Specific examples of the isocyanate-based crosslinking agent include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate and xylylene diisocyanate; and isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate HX"). The content of the isocyanate-based crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength and elastic modulus, and is typically 0.1 to 20 parts by weight, and more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the total amount of the acrylic polymer having an acid functional group and the crystalline resin having a melting point of 25°C or higher.
[0040] Examples of the epoxy crosslinking agent include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Company, Inc., product name "Tetrad C"), 1,6-hexanediol diglycidyl ether (manufactured by Kyoeisha Chemical Company, Inc., product name "Epolite 1600"), neopentyl glycol diglycidyl ether (manufactured by Kyoeisha Chemical Company, Inc., product name "Epolite 1500NP"), ethylene glycol Licor diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., product name "Epolite 40E"), propylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., product name "Epolite 70P"), polyethylene glycol diglycidyl ether (manufactured by Nippon Oil & Fats Co., Ltd., product name "Epiol E-400"), polypropylene glycol diglycidyl ether (manufactured by Nippon Oil & Fats Co., Ltd., product name "Epiol P-200"), sorbitol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, product name "Denacol" Examples of the epoxy resins include glycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-611"), glycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-314"), pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-512"), sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. The content of the epoxy-based crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength and elastic modulus, and is typically 0.01 to 10 parts by weight, and more preferably 0.03 to 5 parts by weight, per 100 parts by weight of the total amount of the acrylic polymer having an acid functional group and the crystalline resin having a melting point of 25°C or higher.
[0041] As the metal chelate crosslinking agent, for example, a metal chelate compound in which the metal atom is aluminum, zirconium, titanium, zinc, iron, tin, etc., can be used. Among them, an aluminum chelate compound or a titanium chelate compound is preferable.
[0042] Examples of aluminum chelate compounds include diisopropoxyaluminum monooleyl acetoacetate, monoisopropoxyaluminum bisoleyl acetoacetate, monoisopropoxyaluminum monooleate monoethyl acetoacetate, diisopropoxyaluminum monolauryl acetoacetate, diisopropoxyaluminum monostearyl acetoacetate, diisopropoxyaluminum monoisostearyl acetoacetate, monoisopropoxyaluminum mono-N-lauroyl-β-alanate monolauryl acetoacetate, aluminum tris(acetylacetonate), acetylacetonate aluminum bis(ethyl acetoacetate), monoacetylacetonate aluminum bis(isobutyl acetoacetate) chelate, monoacetylacetonate aluminum bis(2-ethylhexyl acetoacetate) chelate, monoacetylacetonate aluminum bis(dodecyl acetoacetate) chelate, and monoacetylacetonate aluminum bis(oleyl acetoacetate) chelate.
[0043] Examples of titanium chelate compounds include titanium diisopropoxybis(acetylacetonate), titanium tetra-n-butylate, titanium tetra-2-ethylhexanoate, titanium tetraacetylacetonate, titanium diisopropoxybis(ethylacetoacetate), and titanium octylene glycolate.
[0044] Other examples of the metal chelate compounds include zirconium tetraacetylacetonate and zirconium tributoxymonoacetylacetonate.
[0045] The above metal chelate crosslinking agents may be used alone or in combination of two or more.
[0046] The content of the metal chelate crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength and elastic modulus, and is typically 0.01 to 10 parts by weight, more preferably 0.03 to 7 parts by weight, and even more preferably 0.05 to 5 parts by weight, relative to 100 parts by weight of the total amount of the acrylic polymer having an acid functional group and the crystalline resin having a melting point of 25°C or higher.
[0047] B. Adhesive tape 1 is a schematic cross-sectional view of an adhesive tape according to one embodiment of the present invention. The adhesive tape 100 comprises a substrate 10 and an adhesive layer 20 disposed on at least one side (both sides in the illustrated example) of the substrate 10. The adhesive layer 20 contains the adhesive described in section A above. Although not illustrated, the adhesive tape may be provided with a release film on the outer side of the adhesive layer (i.e., the surface of the adhesive layer opposite the substrate) for the purpose of protecting the adhesive surface until use.
[0048] The pressure-sensitive adhesive tape may be an adhesive tape that exhibits adhesiveness at room temperature (25° C.), or may be an adhesive tape that exhibits adhesiveness upon heating. The pressure-sensitive adhesive tape that exhibits adhesiveness upon heating may exhibit adhesiveness in a state where it is cooled to room temperature after heating.
[0049] The adhesive strength at 25°C when the adhesive layer of the adhesive tape of the present invention is applied to an aluminum plate is preferably 0.5N / 10mm or more, more preferably 0.8N / 10mm to 20N / 10mm, and even more preferably 1N / 10mm to 10N / 10mm. In this specification, the adhesive strength is an adhesive strength measured by a method according to JIS Z 0237:2000, and is measured by applying an adhesive tape to an adherend by one reciprocation of a 2kg roller, leaving it at 25°C for 30 minutes, and then peeling off the adhesive tape under the conditions of a peel angle of 180° and a peel speed (tensile speed) of 300mm / min. In addition, when the adhesive tape is an adhesive tape that develops adhesiveness by heating, the adhesive tape and the adherend are bonded by an adhesion operation (for example, 130°C, 0.4MPa, 5 minutes) at a temperature at which the adhesive tape shows adhesiveness, and the adhesive strength measured after cooling to 25°C corresponds to the above adhesive strength.
[0050] The adhesive strength at 25° C. when the adhesive layer of the adhesive tape of the present invention is adhered to an aluminum plate is preferably 0.3 N / 10 mm or more, more preferably 0.5 N / 10 mm to 20 N / 10 mm, and even more preferably 1 N / 10 mm to 10 N / 10 mm.
[0051] The thickness of the pressure-sensitive adhesive tape is preferably 5 μm to 200 μm, more preferably 15 μm to 150 μm, and further preferably 30 μm to 100 μm.
[0052] B-1. Adhesive layer The adhesive layer comprises an adhesive as described in section A above.
[0053] The thickness of the pressure-sensitive adhesive layer is preferably 1 μm to 100 μm, more preferably 3 μm to 80 μm, and even more preferably 5 μm to 50 μm.
[0054] The pressure-sensitive adhesive layer preferably has a probe tack value of 500 g or less, more preferably 400 g or less, further preferably 340 g or less, and particularly preferably 10 g to 300 g at 25° C. The method for measuring the probe tack value will be described later.
[0055] B-2. Base material As the substrate, a resin film is preferably used. Examples of the resin constituting the resin film include polyacrylate, polyurethane, polyimide, aramid, polyamide, ethylene-vinyl alcohol copolymer, polyetherimide, polyvinylidene fluoride, polyester, polypropylene, polyethylene, polyphenylene sulfide, etc. These resins may be used alone or in combination of two or more.
[0056] The thickness of the substrate is preferably from 1 μm to 100 μm, more preferably from 5 μm to 70 μm, and further preferably from 15 μm to 50 μm. EXAMPLES
[0057] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are by weight unless otherwise specified.
[0058] <<Single-sided adhesive tape>> [Example 1] A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with 2-ethylhexyl acrylate / acrylic acid (95 parts by weight / 5 parts by weight), 0.2 parts by weight of benzoyl peroxide as an initiator, and 120 parts by weight of ethyl acetate. Nitrogen gas was introduced while gently stirring, and a polymerization reaction was carried out for about 6 hours while maintaining the liquid temperature in the flask at around 60°C, thereby obtaining an acrylic copolymer (1) having a weight average molecular weight of 1.3 million. To 75 parts by weight of the acrylic copolymer (1), 25 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L", weight average molecular weight 75,000, melting point 70°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (1) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (1).
[0059] [Example 2] In the same manner as in Example 1, an acrylic copolymer (1) was obtained. To 75 parts by weight of the acrylic copolymer (1), 25 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L", weight average molecular weight 75,000, melting point 70°C) as a modified olefin resin, 30 parts by weight of a hydrogenated derivative of C9 petroleum resin (manufactured by Arakawa Chemical Industries Co., Ltd., product name "Arcon P-125", hydrogenation rate: 95%, softening point: 125°C), and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") were added, and the mixture was diluted with toluene to prepare an adhesive (2) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (2).
[0060] [Example 3] In the same manner as in Example 1, an acrylic copolymer (1) was obtained. To 75 parts by weight of the acrylic copolymer (1), 25 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-T", weight average molecular weight: 75,000, melting point: 90°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (3) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 12 μm) so that the adhesive layer had a thickness of 20 μm after drying, to obtain an adhesive tape (3).
[0061] [Example 4] In the same manner as in Example 1, an acrylic copolymer (1) was obtained. To 85 parts by weight of the acrylic copolymer (1), 15 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-T", weight average molecular weight: 75,000, melting point: 90°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (4) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 12 μm) so that the adhesive layer had a thickness of 5 μm after drying, to obtain an adhesive tape (4).
[0062] [Example 5] An adhesive tape (5) was produced in the same manner as in Example 4, except that a 50 μm thick polyester film (manufactured by Toray Industries, Inc., product name "Lumirror") was used as the substrate and the thickness of the adhesive layer was set to 20 μm.
[0063] [Example 6] A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with 2-ethylhexyl acrylate / acrylic acid (90 parts by weight / 10 parts by weight), 0.2 parts by weight of benzoyl peroxide as an initiator, and 120 parts by weight of ethyl acetate. Nitrogen gas was introduced while gently stirring, and a polymerization reaction was carried out for about 6 hours while maintaining the liquid temperature in the flask at around 60°C, thereby obtaining an acrylic copolymer (2) having a weight average molecular weight of 1.2 million. To 85 parts by weight of the acrylic copolymer (2), 15 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L", weight average molecular weight: 75,000, melting point: 70°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (5) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polyimide film, manufactured by Toray Industries, Inc., product name "Kapton 100H", thickness: 25 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (6).
[0064] [Example 7] An adhesive tape (7) was produced in the same manner as in Example 6, except that a 50 μm thick polyester film (manufactured by Toray Industries, Inc., product name "Lumirror") was used as the substrate and the thickness of the adhesive layer was set to 50 μm.
[0065] [Example 8] In the same manner as in Example 1, an acrylic copolymer (1) was obtained. To 75 parts by weight of the acrylic copolymer (1), 25 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-Lz", weight average molecular weight: 100,000, melting point: 70°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (6) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (8).
[0066] [Example 9] A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with 2-ethylhexyl acrylate / acrylic acid (100 parts by weight / 2 parts by weight), 0.2 parts by weight of benzoyl peroxide as an initiator, and 230 parts by weight of ethyl acetate. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was kept at around 60°C to carry out a polymerization reaction for about 6 hours, thereby obtaining an acrylic copolymer (3) having a weight average molecular weight of 650,000. To 70 parts by weight of the acrylic copolymer (3), 30 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L", weight average molecular weight: 75,000, melting point: 70°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (7) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (9).
[0067] [Example 10] A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with n-butyl acrylate / ethyl acrylate / acrylic acid (70 parts by weight / 25 parts by weight / 5 parts by weight), 0.2 parts by weight of benzoyl peroxide as an initiator, and 120 parts by weight of ethyl acetate. Nitrogen gas was introduced while gently stirring, and a polymerization reaction was carried out for about 6 hours while maintaining the liquid temperature in the flask at around 60°C, to obtain an acrylic copolymer (4) having a weight average molecular weight of 700,000. To 85 parts by weight of the acrylic copolymer (4), 15 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L", weight average molecular weight: 75,000, melting point: 70°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (8) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (10).
[0068] [Example 11] A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with n-butyl acrylate / acrylic acid (95 parts by weight / 5 parts by weight), 0.2 parts by weight of 2,2'-azobisisobutyronitrile as an initiator, and 233 parts by weight of ethyl acetate. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was kept at around 60°C to carry out a polymerization reaction for about 6 hours, thereby obtaining an acrylic copolymer (5) having a weight average molecular weight of 700,000. To 85 parts by weight of the acrylic copolymer (5), 15 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L", weight average molecular weight: 75,000, melting point: 70°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (9) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, Inc., product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 15 μm after drying, to obtain an adhesive tape (11).
[0069] [Example 12] In the same manner as in Example 6, an acrylic copolymer (2) was obtained. To 25 parts by weight of the acrylic copolymer (2), 75 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L", weight average molecular weight: 75,000, melting point 70°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (10) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 12 μm) so that the adhesive layer had a thickness of 3 μm after drying, to obtain an adhesive tape (12).
[0070] [Example 13] In the same manner as in Example 1, an acrylic copolymer (1) was obtained. To 25 parts by weight of the acrylic copolymer (1), 75 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L", weight average molecular weight: 75,000, melting point 70°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (11) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polyester film, manufactured by Toray Industries, product name "Lumirror", thickness: 50 μm) so that the adhesive layer had a thickness of 25 μm after drying, to obtain an adhesive tape (13).
[0071] [Example 14] In the same manner as in Example 1, an acrylic copolymer (1) was obtained. To 15 parts by weight of the acrylic copolymer (1), 85 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-T", weight average molecular weight: 75,000, melting point: 90°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (12) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (14).
[0072] [Example 15] In the same manner as in Example 1, an acrylic copolymer (1) was obtained. To 85 parts by weight of the acrylic copolymer (1), 15 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L" weight average molecular weight 75,000, melting point 70°C) as a modified olefin resin and 0.5 parts by weight of an aluminum chelate crosslinking agent (product name "Aluminum Chelate A" manufactured by Kawaken Fine Chemical Co., Ltd.) were added, and the mixture was diluted with toluene to prepare a pressure-sensitive adhesive (13) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 20 μm after drying, to obtain an adhesive tape (15).
[0073] [Example 16] In the same manner as in Example 1, an acrylic copolymer (1) was obtained. To 15 parts by weight of the acrylic copolymer (1), 85 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L" weight average molecular weight 75,000, melting point 70°C) as a modified olefin resin and 0.2 parts by weight of an aluminum chelate crosslinking agent (product name "Aluminum Chelate A" manufactured by Kawaken Fine Chemical Co., Ltd.) were added, and the mixture was diluted with toluene to prepare a pressure-sensitive adhesive (14) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, Inc., product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 5 μm after drying, to obtain an adhesive tape (16).
[0074] [Example 17] In the same manner as in Example 1, an acrylic copolymer (1) was obtained. To 25 parts by weight of the acrylic copolymer (1), 75 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-T" weight average molecular weight 75,000, melting point 90°C) as a modified olefin resin and 0.1 parts by weight of an epoxy crosslinking agent (manufactured by Mitsubishi Gas Chemical Co., Ltd., product name "TETRAD C") were added, and the mixture was diluted with toluene to prepare a pressure-sensitive adhesive (15) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 5 μm after drying, to obtain an adhesive tape (17).
[0075] [Comparative Example 1] In the same manner as in Example 1, an acrylic copolymer (1) was obtained. To 100 parts by weight of the acrylic copolymer (1), 18 parts by weight of a modified rosin resin (manufactured by Harima Chemicals, product name "Hariestar KT-3") and 2 parts by weight of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") were added, and the mixture was diluted with toluene to prepare an adhesive (C1) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (C1).
[0076] [Comparative Example 2] In the same manner as in Example 1, an acrylic copolymer (1) was obtained. 0.5 parts by weight of an epoxy crosslinking agent (manufactured by Mitsubishi Gas Chemical Co., Ltd., product name "Tetrad C") was added to 100 parts by weight of the acrylic copolymer (1), and the mixture was diluted with toluene to prepare a pressure-sensitive adhesive (C2) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (C2).
[0077] [Comparative Example 3] In the same manner as in Example 11, an acrylic copolymer (5) was obtained. To 100 parts by weight of the acrylic copolymer (5), 30 parts by weight of a terpene phenol resin (manufactured by Yasuhara Chemical Co., Ltd., product name "YS Polystar S-145", softening point: approximately 145°C), 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), and 0.03 parts by weight of an epoxy crosslinking agent (manufactured by Mitsubishi Gas Chemical Co., Ltd., product name "Tetrad C") were added, and the mixture was diluted with toluene to prepare a pressure-sensitive adhesive (C3) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (C3).
[0078] [Comparative Example 4] A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with 2-ethylhexyl acrylate / 2-hydroxyethyl acrylate (100 parts by weight / 4 parts by weight), 0.2 parts by weight of 2,2'-azobisisobutyronitrile as an initiator, and 233 parts by weight of ethyl acetate. Nitrogen gas was introduced while gently stirring, and a polymerization reaction was carried out for approximately 6 hours while maintaining the liquid temperature in the flask at around 60°C, to obtain an acrylic copolymer (6) having a weight average molecular weight of 550,000. To 85 parts by weight of the acrylic copolymer (6), 15 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L", weight average molecular weight: 75,000, melting point 70°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (C4) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (C4).
[0079] [Comparative Example 5] In the same manner as in Comparative Example 4, an acrylic copolymer (6) was obtained. To 25 parts by weight of the acrylic copolymer (6), 75 parts by weight of a maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L", weight average molecular weight: 7.5, melting point 70°C) as a modified olefin resin and 2 parts by weight of an isocyanate crosslinking agent (manufactured by Tosoh Corporation, product name "CORONATE L") were added, and the mixture was diluted with toluene to prepare an adhesive (C5) with a solid content of 15%. The obtained adhesive was applied onto a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (C5).
[0080] [Comparative Example 6] As a modified olefin resin, 100 parts by weight of maleic anhydride modified propylene-butene copolymer resin (manufactured by Toyobo Co., Ltd., product name "TOYOTAC PMA-L", weight average molecular weight: 75,000, melting point: 70°C) was dissolved in toluene to prepare an adhesive (C6) with a solid content of 15%. The obtained adhesive was coated on a substrate (polypropylene film, manufactured by Toray Industries, product name "Treyfan", thickness: 30 μm) so that the adhesive layer had a thickness of 10 μm after drying, to obtain an adhesive tape (C6).
[0081] <Evaluation> The obtained single-sided adhesive tape was subjected to the following evaluations, and the results are shown in Tables 1 and 2.
[0082] (1) Adhesive strength (to aluminum plate) Test specimens were obtained by attaching the adhesive tapes obtained in the Examples and Comparative Examples to the surface of an aluminum plate under the following conditions. Note that the adhesive tapes in Examples 12, 13, 14, 16, 17, Comparative Examples 5 and 6 were heat-bonding type adhesive tapes and therefore were pressed only by heating (130°C), while the other adhesive tapes were pressed at room temperature (25°C) and at heating (130°C). For the obtained test specimens, a precision universal testing machine (product name "Autograph AG-I", manufactured by Shimadzu Corporation) was used to measure the force (N / 10 mm) required to peel the adhesive tape from the surface of the aluminum plate under the following conditions, and this was taken as the adhesive strength of the adhesive tape. (Crimping conditions) Room temperature pressing: Pressed with a 2kg roller going back and forth once. Heating and compression bonding: The bonding device surface temperature is set to 130°C and compression is performed at 0.4 MPa for 5 minutes. (Peeling conditions) Temperature: Normal temperature (25℃) Peeling speed: 300mm / min Peel angle: 180°
[0083] (2) Adhesive strength (against polypropylene board) The adhesive strength of the adhesive tape was measured in the same manner as in the above evaluation (1), except that the aluminum plate was replaced with a polypropylene plate.
[0084] (3) Oil resistance Test specimens were obtained in the same manner as in (1) and (2) above. The obtained test specimens were immersed in oleic acid at 60°C for 72 hours, and the presence or absence of lifting and peeling of the adhesive tape was visually confirmed. Furthermore, for test specimens where the adhesive tape did not peel off, the oleic acid was wiped off, and the test specimens were left to stand for 30 minutes in an environment of 23°C and 50% RH. Thereafter, the adhesive strength of the adhesive tape (adhesive strength after immersion in oleic acid) was measured using the same method as in (1) above. Note that oleic acid was used as a pseudo-sebum.
[0085] (4) Alcohol resistance Test specimens were obtained in the same manner as in (1) and (2) above. The obtained test specimens were immersed in ethanol at 60°C diluted to 75% by weight with distilled water for 72 hours, and the presence or absence of lifting and peeling of the adhesive tape was visually confirmed. Furthermore, for the test specimens where the adhesive tape did not peel off, the oleic acid was wiped off and the specimens were left to stand for 30 minutes in an environment of 23°C and 50% RH. Thereafter, the adhesive strength of the adhesive tape (adhesive strength after immersion in ethanol) was measured by the same method as in (1) above. Note that ethanol was used as a pseudo-rubbing alcohol.
[0086] (5) Haze value The haze value of the adhesive tape was measured using a haze meter (model number: HM-150, manufactured by Murakami Color Laboratory) by irradiating light from the adhesive layer side.
[0087] (6) Retention strength test The adhesive tapes obtained in the Examples and Comparative Examples were laminated to a SUS304BA plate under the following conditions to obtain test specimens (bonding area: 10 mm x 20 mm). The adhesive tapes in Examples 12, 13, 14, 16, 17, Comparative Examples 5 and 6 were heat-bonded adhesive tapes, and were bonded at elevated temperature (130°C). The other adhesive tapes were bonded at room temperature (25°C) and at elevated temperature (130°C). The adhesive tapes using polypropylene film as the substrate were lined with a PET adhesive tape (manufactured by Nitto Denko Corporation, product name "No. 315") to prepare test specimens. (Crimping conditions) Room temperature pressing: Pressed with a 2kg roller going back and forth once. Heating and compression bonding: The bonding device surface temperature is set to 130°C and compression is performed at 0.4 MPa for 5 minutes. The test specimen prepared as described above was set up vertically, and a load of 500 g was applied downward at an environmental temperature of 130° C. The holding power was evaluated from the amount of slippage of the adhesive tape after one hour. The amount of slippage is also shown in Table 1.
[0088] [Table 1]
[0089] [Table 2]
[0090] <<Double-sided adhesive tape>> [Example 18] In the same manner as in Example 1, a pressure sensitive adhesive (1) was obtained. The obtained adhesive was coated on a release film (silicone-treated release film, manufactured by Toray Industries, trade name "Therapeel", thickness: 38 μm) so that the adhesive layer had a thickness of 10 μm after drying. The adhesive layer with the release film obtained as described above was attached to both sides of a substrate (polyester film, manufactured by Toray Industries, product name "Lumirror", thickness 38 μm) to obtain a double-sided adhesive tape (18).
[0091] [Example 19] In the same manner as in Example 13, a pressure sensitive adhesive (11) was obtained. The obtained pressure-sensitive adhesive (11) was applied to one side of a substrate (polyimide film, manufactured by Toray DuPont Co., Ltd., product name "Kapton 100H", thickness 25 μm) so that the thickness of the pressure-sensitive adhesive layer after drying was 5 μm. Next, the same procedure as in Example 1 was carried out to obtain a pressure sensitive adhesive (1). The obtained pressure-sensitive adhesive (1) was coated on a release film (silicone-treated release film, manufactured by Toray Industries, trade name "Therapeel", thickness: 38 μm) so that the thickness of the pressure-sensitive adhesive layer after drying was 10 μm. The adhesive layer with the release film thus obtained was attached to the other side of the above-mentioned substrate to obtain a double-sided adhesive tape (19).
[0092] [Example 20] In the same manner as in Example 16, a pressure sensitive adhesive (14) was obtained. The obtained pressure-sensitive adhesive (14) was applied to one side of a substrate (polypropylene film, manufactured by Toray Industries, trade name "Torayfan", thickness: 30 μm) so that the thickness of the pressure-sensitive adhesive layer after drying was 5 μm. Next, in the same manner as in Example 1, a pressure sensitive adhesive (1) was obtained. The obtained adhesive blend liquid (1) was coated on a release film (silicone-treated release film, manufactured by Toray Industries, Inc., product name "Therapeel", thickness: 38 μm) so that the adhesive layer would have a thickness of 10 μm after drying. The adhesive layer with the release film thus obtained was attached to the other side of the above-mentioned substrate to obtain a double-sided adhesive tape (20).
[0093] [Comparative Example 7] In the same manner as in Comparative Example 1, a pressure sensitive adhesive (15) was obtained. The obtained adhesive was coated on a release film (silicone-treated release film, manufactured by Toray Industries, trade name "Therapeel", thickness: 38 μm) so that the adhesive layer had a thickness of 10 μm after drying. The pressure-sensitive adhesive layer with release film obtained as described above was attached to both sides of a substrate (polyester film, manufactured by Toray Industries, product name "Lumirror", thickness 38 μm) to obtain a double-sided pressure-sensitive adhesive tape (C7).
[0094] <Evaluation> The obtained double-sided pressure-sensitive adhesive tape was subjected to the following evaluations, and the results are shown in Table 3.
[0095] (7) Oil resistance evaluation A polypropylene plate was placed on one side of the double-sided adhesive tape, an aluminum plate was placed on the other side, and the two were pressed together at 0.4 MPa for 5 minutes with a surface temperature of the laminating device set to 130° C. to prepare a test specimen. In the double-sided adhesive tapes of Examples 19 and 20, the polypropylene plate was placed on the side of the adhesive layer formed from adhesives (11) and (14). The obtained test specimen was immersed in oleic acid at 60° C. for 72 hours, and the presence or absence of lifting or peeling of the adhesive tape was visually confirmed.
[0096] (8) Alcohol resistance evaluation Test pieces were prepared in the same manner as in the above evaluation (7). The obtained test specimen was immersed in ethanol diluted to 75% by weight with distilled water at 60° C. for 72 hours, and the presence or absence of lifting or peeling of the adhesive tape was visually confirmed.
[0097] [Table 3] [Explanation of symbols]
[0098] 10 Base material 20 Adhesive layer 100 Adhesive Tape
Claims
1. A pressure-sensitive adhesive that exhibits adhesiveness through pressure-sensitive adhesive bonding, The composition comprises an acrylic polymer having an acid functional group and a crystalline resin having a melting point of 25° C. or higher, the acrylic polymer having an acid functional group contains a constituent unit derived from a monomer having an acid functional group, and the content of the constituent unit derived from the monomer having an acid functional group is 1.5 parts by weight to 20 parts by weight based on 100 parts by weight of the acrylic polymer having an acid functional group; the acrylic polymer having an acid functional group contains a structural unit derived from an alkyl (meth)acrylate ester having a branched alkyl group, the content of the structural unit derived from an alkyl (meth)acrylate having a branched alkyl group is 50 parts by weight to 100 parts by weight relative to 100 parts by weight of the structural unit derived from an alkyl (meth)acrylate in the acrylic polymer having an acid functional group, the crystalline resin is a polyolefin resin, The polyolefin resin is a maleic anhydride modified polyolefin resin, a maleic acid modified polyolefin resin, or an acrylic modified polyolefin resin. Adhesive.
2. The pressure-sensitive adhesive according to claim 1 , which exhibits adhesive properties upon heating.
3. The pressure-sensitive adhesive according to claim 1 or 2, wherein the acrylic polymer having an acid functional group has a structural unit a derived from a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 4 or more carbon atoms.
4. The pressure-sensitive adhesive according to claim 3 , wherein the content of the structural unit a is 50 parts by weight or more based on 100 parts by weight of the acrylic polymer having an acid functional group.
5. The pressure-sensitive adhesive according to claim 1 , comprising a C5 petroleum resin and / or a C9 petroleum resin.
6. An adhesive tape comprising the adhesive according to any one of claims 1 to 5.
7. A substrate and a pressure-sensitive adhesive layer disposed on at least one side of the substrate, The pressure-sensitive adhesive layer comprises the pressure-sensitive adhesive according to any one of claims 1 to 5. The adhesive tape according to claim 6.
8. 8. The pressure-sensitive adhesive tape according to claim 7, wherein the substrate is formed from at least one selected from the group consisting of polyacrylate, polyurethane, polyimide, aramid, polyamide, ethylene-vinyl alcohol copolymer, polyetherimide, polyvinylidene fluoride, polyester, polypropylene, polyethylene, and polyphenylene sulfide.
9. The pressure-sensitive adhesive tape according to claim 7 or 8, further comprising a release film provided on the pressure-sensitive adhesive layer on the opposite side to the substrate.
Citation Information
Patent Citations
Skin pack packaging multilayer film
JP1999310265A
Flexible multi-layered film
JP2000128112A
Adhesive composition and adherent article
JP2002338934A
Aqueous emulsion composition of chlorinated polyolefin and water-based coating produced by using the same
JP2004182896A
Adhesive composition
JP2005281338A