Moisture-curable composition having good adhesive properties

A moisture-curable polyurethane composition with a specific polyether urethane polymer and hydrophobic polymer combination addresses adhesion issues on difficult substrates, ensuring long open time, excellent adhesion, and high weathering resistance, while maintaining elasticity and extrudability.

JP7558953B2Active Publication Date: 2024-10-01SIKA TECH AG

Patent Information

Application Number
JP2021542105
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-05
Filing Date
2020-04-02
Publication Date
2024-10-01
Estimated Expiration
2040-04-02

AI Technical Summary

Technical Problem

Existing one-component moisture-curable polyurethane compositions struggle with achieving good adhesion on difficult substrates like residual adhesive beads, particularly in automobile assembly, leading to issues such as water ingress, wind noise, and delamination, while using adhesion promoters like diisocyanate oligomers results in a loss of elasticity.

Method used

A moisture-curable composition comprising a polyether urethane polymer with high 1,2-propyleneoxy units and a hydrophobic polymer containing isocyanate groups, prepared separately and in specific ratios, allows for good adhesion to residual adhesive beads without compromising other properties like curing speed, weathering resistance, and elasticity.

Benefits of technology

The composition exhibits long open time, excellent adhesion to residual adhesive beads, high weathering resistance, and low carbon black leaching, with improved extrudability and sag resistance, maintaining desirable properties even at low temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558953000001
    Figure 0007558953000001
  • Figure 0007558953000002
    Figure 0007558953000002
  • Figure 0007558953000003
    Figure 0007558953000003
Patent Text Reader

Abstract

The present invention relates to a moisture-curable composition that is liquid at ambient temperature and optionally highly viscous, comprising: - at least one polyetherurethane polymer (P1) containing isocyanate groups and having a content of 1,2-propyleneoxy units in the polyether segments of at least 80% by weight, and at least one hydrophobic polymer (P2) containing isocyanate groups and liquid at ambient temperature, obtained by reacting at least one diisocyanate monomer with a hydrophobic diol having an OH number ranging from 28 to 120 mg KOH / g, Here, the polymers P1 and P2 are produced separately, and the weight ratio of the polymers P1 / P2 ranges from 70 / 30 to 98 / 2. Due to the presence of the hydrophobic polymer (P2), the compositions according to the invention exhibit improved properties in terms of open time, adhesion, application and weathering resistance, with unchanged good properties in terms of storage stability, hardening speed, strength, ductility, elasticity and hazardous material classification. This type of composition is particularly suitable for use as an elastic adhesive in replacement glass for vehicles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a moisture-curable polyurethane composition and its use as an elastic adhesive and / or sealant for construction and industrial applications, in particular for glass replacement in automobiles. [Background technology]

[0002] Curable compositions based on polyurethanes are often used as adhesives for elastic bonds, for example in automotive assembly, which require good properties, especially with regard to storage stability, applicability, open time, curing speed, adhesion, strength, elasticity, weather resistance and hazardous materials classification.

[0003] One-component moisture-curing systems are especially popular due to their ease of handling. In general, these systems show good adhesive properties. However, there are applications on certain substrates on which it is difficult to achieve good adhesion. An example of this is the bonding of replacement glass in automobiles, where the body flange as substrate has both areas with exposed paint and areas with residues of the old adhesive that are attached to the paint and have not been completely removed or left as a bonding substrate ("residual adhesive beads"). If the new adhesive does not completely adhere to the residual adhesive beads, the effects can be unwanted water ingress or wind noise, or even delamination of the panes. Moisture-curing adhesives available now without proper pretreatment on the residual adhesive beads often simply result in inadequate adhesion, especially when the old adhesive has aged considerably and therefore become hard or brittle. For the improvement of adhesion on the residual adhesive beads, it is possible to use known adhesion promoters, such as diisocyanate oligomers or their derivatives. However, this leads to a loss of elasticity of the adhesive after curing.

[0004] Hydrophobic diols are typically used in two-component polyurethanes, especially to improve low temperature flexibility or weathering stability, but they are rarely used in one-component moisture-curing polyurethanes.

[0005] WO 2017 / 103070 describes a moisture-curing polyurethane adhesive with high early strength, which is heated for application. It comprises a polymer containing isocyanate groups, which is a reaction product prepared in several stages from a polyol mixture containing a polyol based on dimer fatty acid from other reactants. This reaction product has a very high viscosity and its preparation is complicated. Due to its poor extrudability, it is not suitable for an adhesive that can be applied at room temperature, which does not allow the desired adhesion to the residual adhesive beads. Summary of the Invention [Problem to be solved by the invention]

[0006] It is an object of the present invention to provide a one-component moisture-curing polyurethane composition having good adhesion on difficult to bond substrates, e.g. residual adhesive beads, said composition having no disadvantages in further relevant product properties, in particular storage stability, applicability, cure speed, weather resistance, blistering, strength, extensibility, elasticity and harmful substances classification. [Means for solving the problem]

[0007] This object is achieved by a moisture-curing composition according to claim 1. The composition comprises a polyetherurethane polymer P1 containing isocyanate groups and having a content of 1,2-propyleneoxy units in the polyether segments of at least 80% by weight, and a hydrophobic polymer P2 containing isocyanate groups, based on a hydrophobic diol, in particular a polyester diol based on dimer fatty acid or on poly(1,2-butylene glycol), having an OH value in the range of 28 to 120 mg KOH / g. The polymers P1 and P2 are prepared separately from one another and are present in a weight ratio in the range of 70 / 30 to 98 / 2. They preferably each contain a low diisocyanate monomer content.

[0008] The compositions of the present invention have good processability at room temperature without loss in cure speed, strength, extensibility or other relevant product properties, surprisingly long open time, surprisingly good adhesion to residual adhesive beads and especially high weatherability compared to corresponding compositions without polymer P2. Furthermore, the carbon black filled compositions of the present invention have a surprisingly low tendency for the carbon black to leach out, so that the substrate does not stain even after prolonged use. Furthermore, the compositions of the present invention have a matte surface, which is highly desirable for many users in the case of visible adhesive bonds.

[0009] It is particularly surprising that the composition of the invention has unexpectedly good processing properties: even at low contents of hydrophobic polymer P2, it can be extruded from containers at room temperature and at low temperatures with particularly low forces, with good sag resistance and short thread formation unchanged compared to the corresponding composition without polymer P2.

[0010] To improve early strength, sag resistance and thread formation, moisture-curable polyurethane adhesives, especially for automotive assembly, often further comprise a meltable component, typically a small amount of room temperature solid polyurethane polymer based on crystalline polyester polyol.However, the meltable component increases the extrusion force for the adhesive at room temperature and under low temperature conditions, and the sag resistance is highly shear-dependent, which can lead to problems in production and application.Surprisingly, even when the composition of the present invention further comprises a meltable component, it is surprisingly easy to extrude, and the rheological properties are significantly less shear-dependent.More specifically, the composition of the present invention allows the adhesive to be used with a much smaller amount of meltable component or to be completely omitted.

[0011] The compositions of the present invention allow for moisture-curing elastic polyurethane sealants and adhesives that can be applied at room temperature and have improved bonding properties, in particular long open times on certain substrates, such as residual adhesive beads, improved application properties, in particular good extrudability even at low temperatures, in particular a small increase in the extrudability at 5°C from room temperature, a matte surface and particularly good weather resistance, coupled with good properties that do not change in terms of storage stability, curing speed, blister formation, strength, extensibility, elasticity and harmful substance classification, compared to corresponding compositions without polymer P2. Thus, the compositions are particularly suitable as elastic adhesives in automobile assembly, in particular for the replacement of defective elastically bonded windshields to automobiles.

[0012] Further aspects of the invention are the subject of further independent claims. Particularly preferred embodiments of the invention are the subject of the dependent claims. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention provides a moisture-curable composition that is liquid or pasty at room temperature, comprising: at least one polyetherurethane polymer P1 containing isocyanate groups and having a content of 1,2-propyleneoxy units in the polyether segments of at least 80% by weight, and at least one hydrophobic polymer P2 containing isocyanate groups and liquid at room temperature, obtained from the reaction of at least one diisocyanate monomer with a hydrophobic diol having an OH number in the range from 28 to 120 mg KOH / g, Here, the polymers P1 and P2 are prepared separately from each other and the polymer P1 / polymer P2 is present in a weight ratio ranging from 70 / 30 to 98 / 2.

[0014] "Diisocyanate monomer" refers to an organic compound having two isocyanate groups separated from each other by a divalent hydrocarbyl group having from 4 to 15 carbon atoms.

[0015] "Polyetherurethane polymer" refers to a polymer having ether groups as repeat units and further containing urethane groups.

[0016] "Dimer fatty acid-based polyester diol" refers to a polyester diol prepared from dimer fatty acid and / or dimer fatty alcohol.

[0017] "NCO content" refers to the content of isocyanate groups in weight percent based on total polymer.

[0018] "Molecular weight" refers to the molar mass (in g / mol) of a molecule or molecular residue. "Average molecular weight" refers to the number average molecular weight (M n ), which is determined by gel permeation chromatography (GPC) against polystyrene as a standard.

[0019] A substance or composition is said to be "storage stable" or "storable" when it can be stored in a suitable container at room temperature for an extended period of time, typically at least three to six months or more, without a change in its application or use characteristics to an extent that would be relevant to its use as a result of storage.

[0020] A composition referred to as a "one-component" composition is one in which all components of the composition are in the same container and are themselves storage stable.

[0021] "Room temperature" refers to a temperature of 23°C.

[0022] All industry standards mentioned herein relate to the version in effect as of the date of first filing.

[0023] Percentage by weight (wt %) refers to the proportion by mass of a component or molecule of a composition based on the entire composition or molecule, unless otherwise specified. The terms "mass" and "weight" are used synonymously herein.

[0024] The moisture-curable composition comprises at least one polyether urethane polymer P1 containing isocyanate groups and having a content of 1,2-propyleneoxy units in the polyether segments of at least 80% by weight.

[0025] The polyetherurethane polymer P1 preferably comprises from 80% to 100% by weight of 1,2-propyleneoxy units and from 0% to 20% by weight of 1,2-ethyleneoxy units in the polyether segments.

[0026] The polyetherurethane polymer P1 preferably has an average NCO functionality ranging from 1.8 to 3.5, preferably from 2 to 3.

[0027] The polyetherurethane polymer P1 preferably has an NCO content in the range from 1% to 5% by weight, in particular from 1% to 3% by weight.

[0028] The polyether urethane polymer P1 preferably has an average molecular weight M in the range of 2,000 to 20,000 g / mol, preferably 3,000 to 15,000 g / mol. n has.

[0029] The polyether urethane polymer P1 preferably has a viscosity in the range of 5 to 300 Pa·s, more preferably 5 to 200 Pa·s, in particular 5 to 100 Pa·s at 20° C. The viscosity is measured here at 50 s with a cone-plate viscometer having a cone diameter of 25 mm, a cone angle of 1°, and a cone tip-plate distance of 0.5 mm. -1 The shear rate is measured.

[0030] The preferred polyether urethane polymer P1 allows for efficiently processable moisture curable compositions having high elasticity and extensibility coupled with high strength.

[0031] The polyetherurethane polymer P1 containing isocyanate groups is obtained in particular from the reaction of at least one diisocyanate monomer and at least one suitable polyether polyol, the reaction being preferably carried out with the exclusion of moisture at temperatures ranging from 20 to 160° C., in particular from 40 to 140° C., optionally in the presence of a suitable catalyst.

[0032] The NCO / OH ratio is preferably in the range from 1.3 / 1 to 10 / 1. The diisocyanate monomers remaining in the reaction mixture after reaction of the OH groups can in particular be removed by distillation.

[0033] When excess diisocyanate monomer is removed by distillation, the NCO / OH ratio in the reaction mass is preferably in the range of from 3 / 1 to 10 / 1, in particular from 4 / 1 to 7 / 1, and the resulting polyetherurethane polymer containing isocyanate groups contains, after distillation, preferably not more than 0.5% by weight, more preferably not more than 0.3% by weight, of diisocyanate monomer.

[0034] If the excess diisocyanate monomer is not removed from the polyetherurethane polymer, the NCO / OH ratio in the reaction mass is preferably in the range of 1.3 / 1 to 2.5 / 1. Such polyetherurethane polymers in particular contain not more than 3% by weight, preferably not more than 2% by weight, of diisocyanate monomer.

[0035] Suitable diisocyanate monomers for the preparation of the polyether urethane polymers P1 are commercially available aromatic, aliphatic or cycloaliphatic diisocyanates, in particular diphenylmethane 4,4'-diisocyanate, optionally with a fraction of diphenylmethane 2,4'- and / or 2,2'-diisocyanate (MDI), tolylene 2,4-diisocyanate with tolylene 2,6-diisocyanate or mixtures thereof (TDI), phenylene 1,4-diisocyanate (PDI), naphthalene 1,5-diisocyanate (NDI), hexane 1,6-diisocyanate, isocyanatomethylcyclohexane (isophorone diisocyanate or IPDI), perhydro(diphenylmethane 2,4'- or 4,4'-diisocyanate) (HMDI), 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane, m- or p-xylylene diisocyanate (XDI), or mixtures thereof.

[0036] Of these, MDI, TDI, HDI or IPDI is preferred, with IPDI or MDI being particularly preferred.

[0037] Most preferred is MDI, especially diphenylmethane 4,4'-diisocyanate (4,4'-MDI), which is a solid at room temperature, especially those qualities that contain only small fractions of diphenylmethane 2,4'- and / or 2,2'-diisocyanate.

[0038] The isocyanate groups of the polyetherurethane polymer P1 thus preferably derive from diphenylmethane 4,4'-diisocyanate. Such polymers cure particularly quickly and allow particularly high strengths.

[0039] Suitable polyether polyols for the preparation of the polyether urethane polymers P1 are polyether polyols having at least 80% by weight of 1,2-propyleneoxy units in the polyether segments, in particular polyoxypropylene diols or triols, or so-called ethylene oxide-terminated (EO-capped or EO-tipped) polyoxypropylene diols or triols, the latter being polyoxyethylene / polyoxypropylene copolyols, which are in particular obtained by further alkoxylation of polyoxypropylene diols or triols with ethylene oxide, as a result of a propoxylation reaction, which results in them having primary hydroxyl groups.

[0040] Polyether polyols having an OH value in the range of 6 to 280 mg KOH / g, particularly 7.5 to 112 mg KOH / g, are preferred.

[0041] Average molecular weight M in the range of 400 to 20,000 g / mol, more preferably 1000 to 15,000 g / mol, in particular 2000 to 10,000 g / mol. n Preferred is a polyether polyol having the formula:

[0042] Polyether polyols with an average OH functionality in the range of 1.6 to 3 are preferred.

[0043] In the preparation of the polyetherurethane polymers P1 containing isocyanate groups, it is also possible to include a proportion of di- or polyfunctional alcohols.

[0044] More preferably, the polyetherurethane polymer P1 is obtained from the reaction of at least one diisocyanate monomer with at least one, optionally ethylene oxide-terminated, polyoxypropylene diol or triol having an OH number in the range from 7.5 to 112 mg KOH / g, in particular from 11 to 58 mg KOH / g.

[0045] In a preferred embodiment of the present invention, the polyetherurethane polymer P1 containing isocyanate groups contains a slightly low content of diisocyanate monomers, preferably less than 0.5% by weight, more preferably less than 0.3% by weight, in particular less than 0.2% by weight of diisocyanate monomers. Such polyetherurethane polymer P1 allows compositions with a particularly attractive hazard classification.

[0046] A preferred separation method for the removal of the diisocyanate monomer is a distillation method, particularly thin film distillation or short path distillation, preferably under reduced pressure.

[0047] Particularly preferred is a multi-stage process in which the diisocyanate monomer is removed in a short-path evaporator with a jacket temperature in the range of 120-200° C. and a pressure of 0.001-0.5 mbar.

[0048] In the case of 4,4'-MDI, which is preferred as diisocyanate monomer, removal by distillation is particularly demanding; for example, it must be ensured that the condensate does not solidify and block the system. It is preferred to operate at 0.001-0.5 mbar with a jacket temperature in the range of 160-200°C and to condense the removed monomer at a temperature in the range of 40-60°C.

[0049] It is preferred to react the diisocyanate monomer with the polyether polyol followed by removal of most of the diisocyanate monomer remaining in the reaction mixture without the use of a solvent or entraining agent.

[0050] It is preferred to subsequently reuse the diisocyanate monomer removed after the reaction, ie to use it again for the preparation of a polymer containing isocyanate groups.

[0051] Particularly preferred are polyetherurethane polymers P1 having an NCO content in the range of 1% to 2.5% by weight, in particular 1.3% to 2.1% by weight, and a diisocyanate monomer content of 0.3% by weight or less, which are obtained by reacting at least one diisocyanate monomer, in an NCO / OH ratio of at least 3 / 1, with a polyethertriol having an average OH functionality in the range of 2.2 to 3 and an OH number in the range of 20 to 42 mg KOH / g, followed by removal of most of the diisocyanate monomer using suitable separation methods. Preferred diisocyanate monomers are IPDI or 4,4'-MDI, in particular 4,4'-MDI.

[0052] More particularly preferred are linear polyetherurethane polymers P1 having an NCO content in the range of 1% to 2.5% by weight, in particular 1.3% to 2.1% by weight, and a diisocyanate monomer content of 0.3% by weight or less, which are obtained by reacting at least one diisocyanate monomer with a polyetherdiol having an OH value in the range of 13 to 38 mg KOH / g, in particular 22 to 32 mg KOH / g, in an NCO / OH ratio of at least 3 / 1, followed by removal of most of the diisocyanate monomer using suitable separation methods. Preferred diisocyanate monomers are IPDI or 4,4'-MDI, in particular 4,4'-MDI.

[0053] Mixtures of these two particularly preferred polyetherurethane polymers are further particularly preferred as polyetherurethane polymer P1.

[0054] The moisture-curable composition preferably contains 15% to 80% by weight, in particular 20% to 60% by weight, of the polyetherurethane polymer P1.

[0055] The moisture curable composition further comprises at least one room temperature liquid, hydrophobic polymer P2 containing isocyanate groups, obtained from the reaction of at least one diisocyanate monomer and a hydrophobic diol.

[0056] The polymer P2 preferably has a viscosity of 1000 Pa·s or less, in particular 500 Pa·s or less, at 20° C. The viscosity at 20° C. is preferably in the range of 10 to 1000 Pa·s, in particular 10 to 500 Pa·s. The viscosity is measured here in a cone-plate viscometer with a cone diameter of 25 mm, a cone angle of 1°, and a cone tip-plate distance of 0.5 mm, at a viscosity of 50 s. -1 The shear rate is measured.

[0057] The polymer P2 preferably has an NCO content in the range of 1.5% to 6% by weight, more preferably 1.8% to 5% by weight, particularly preferably 2% to 4% by weight, in particular 2.2% to 3.4% by weight, which allows an attractive combination of good extrudability, good adhesive properties and high strength.

[0058] The hydrophobic diols are preferably selected from the group consisting of polyester diols based on dimer fatty acids and poly(1,2-butylene glycols), which allow the moisture-curing composition to have particularly good properties in terms of processability, extensibility, elasticity, strength and adhesion to residual adhesive beads.

[0059] The hydrophobic diols have an OH number in the range of 28 to 120 mg KOH / g. Such diols have an average molecular weight M in the range of 950 to 4,000 g / mol. n These have a mostly linear structure and an average OH functionality of about 2.

[0060] The hydrophobic diols preferably have an OH number in the range of 34 to 120 mg KOH / g, in particular in the range of 52 to 60 mg KOH / g. Such diols have an average molecular weight M in the range of 950 to 3300 g / mol, in particular in the range of 1900 to 2200 g / mol. nThis allows for a particularly attractive combination of good extrudability, good adhesion properties and high strength.

[0061] In a preferred embodiment of the present invention, the hydrophobic diol is a polyester diol based on dimer fatty acid. It is preferably amorphous. Such hydrophobic diol allows compositions (especially also compositions filled with carbon black) to have particularly good processability in terms of thread formation and particularly good hydrolysis and weathering stability, and as a result, they have a significantly lower tendency for carbon black to leach out. This also allows a significantly matte surface.

[0062] Suitable dimer fatty acid-based polyester diols are obtained in particular from the esterification of at least one dimer fatty acid and / or at least one dimer fatty alcohol with a diol, such as diethylene glycol or butanediol, and / or a dicarboxylic acid, such as adipic acid, in such a stoichiometry that the product is amorphous, liquid at room temperature and has an OH number in the range of 28 to 120 mg KOH / g.

[0063] The polyester diols based on dimer fatty acids preferably contain a content of carbon atoms from renewable sources according to ASTM D6866, based on the total carbon content in the range of 50% to 100%, preferably 60% to 95%, in particular 70% to 90%. Such polyester diols are amorphous and hydrophobic, allowing the polymer P2 to have particularly good compatibility with the polyether urethane polymer P1.

[0064] Particularly suitable are commercially available polyester diols based on amorphous dimeric fatty acids, in particular the grades available under the trade name Priplast®: Priplast® 1837, 1838, 3187, 3196, 3197, 3199 or 3238 (from Croda). Of these, Priplast® 1838 is preferred.

[0065] In a further preferred embodiment of the present invention, the hydrophobic diol is poly(1,2-butylene glycol). It is obtained from the polymerization of 1,2-butylene oxide. The starter used for this purpose is typically water or a small diol, such as ethylene glycol or butane-1,2-diol. This allows the polymer P2 to have a particularly low viscosity, thus being particularly easy to handle, and the composition to have a particularly rapid cure.

[0066] Particularly suitable are commercially available grades, especially Vorapel® D3201 (from Dow).

[0067] Suitable diisocyanate monomers are the commercially available aromatic, aliphatic or cycloaliphatic diisocyanates already mentioned.

[0068] The diisocyanate monomers used for the reaction are preferably diphenylmethane 4,4'-diisocyanate (4,4'-MDI), diphenylmethane 2,4'-diisocyanate (2,4'-MDI), tolylene 2,4-diisocyanate with tolylene 2,6-diisocyanate or mixtures thereof (TDI), 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (IPDI) or hexane 1,6-diisocyanate (HDI). These diisocyanates are easily obtainable, inexpensive and allow good mechanical strength. It is also possible to use a combination of two or more of these diisocyanate monomers.

[0069] A particularly preferred diisocyanate monomer is IPDI.Such polymers P2 are particularly suitable in moisture-curable compositions having particularly high light stability.

[0070] Most preferred as diisocyanate monomer is 4,4'-MDI, especially those qualities which contain only small fractions of diphenylmethane 2,4'- and / or 2,2'-diisocyanate, which are solid at room temperature. Such polymers P2 allow particularly rapid curing and high strength.

[0071] The reaction of at least one diisocyanate monomer and a hydrophobic diol for the preparation of polymer P2 is preferably carried out with the exclusion of moisture at a temperature in the range of 20 to 160° C., in particular 40 to 140° C., optionally in the presence of a suitable catalyst.

[0072] The NCO / OH ratio is preferably in the range from 1.3 / 1 to 10 / 1. The diisocyanate monomers remaining in the reaction mixture after reaction of the OH groups can in particular be removed by distillation.

[0073] When excess diisocyanate monomer is removed by distillation, the NCO / OH ratio in the reaction mass is preferably in the range of 3 / 1 to 10 / 1, in particular 4 / 1 to 7 / 1, and the resulting polymer containing isocyanate groups contains, after distillation, preferably 0.5% by weight or less, more preferably 0.3% by weight or less of diisocyanate monomer.

[0074] If excess diisocyanate monomer is not removed from the polymer, the NCO / OH ratio in the reaction mass is preferably in the range of 1.3 / 1 to 2.5 / 1. Such polymers in particular contain not more than 3% by weight, preferably not more than 2% by weight, of diisocyanate monomer.

[0075] The polymer P2 preferably has a diisocyanate monomer content of less than or equal to 0.5% by weight and is obtained by reaction of at least one diisocyanate monomer and a hydrophobic diol in an NCO / OH ratio of at least 3 / 1, followed by removal of most of the diisocyanate monomer by suitable separation methods.

[0076] Such polymers P2 have a particularly low viscosity, which makes them easier to handle, and are particularly suitable for use in compositions having less than 0.1% by weight of diisocyanate monomers; they are safe to handle even without special safety precautions and can be sold in many countries without hazardous substance classification.

[0077] The NCO / OH ratio in the reactants is preferably in the range of from 3 / 1 to 10 / 1, more preferably from 3 / 1 to 8 / 1, in particular from 4 / 1 to 7 / 1.

[0078] The diisocyanate monomer content is preferably not more than 0.3% by weight, in particular not more than 0.2% by weight.

[0079] A preferred separation method for the removal of the diisocyanate monomer is a distillation method, particularly thin film distillation or short path distillation, preferably under reduced pressure.

[0080] Particularly preferred is a multi-stage process in which the diisocyanate monomer is removed in a short-path evaporator with a jacket temperature in the range of 120-200° C. and a pressure of 0.001-0.5 mbar.

[0081] It is preferred to react the diisocyanate monomer with a hydrophobic diol followed by removal of most of the diisocyanate monomer remaining in the reaction mixture without the use of a solvent or entraining agent.

[0082] It is preferred to subsequently reuse the diisocyanate monomer removed after the reaction, ie to use it again for the preparation of a polymer containing isocyanate groups.

[0083] The moisture-curable composition of the invention preferably contains from 1% to 15% by weight, preferably from 1% to 10% by weight, in particular from 2% to 8% by weight of polymer P2.

[0084] The polyetherurethane polymer P1 and the polymer P2 are prepared separately from one another and are thus mixed with one another only after preparation, in particular in the moisture-curable composition according to the invention.

[0085] The polyetherurethane polymer P1 and the polymer P2 are present in the moisture-curable composition of the invention in a weight ratio ranging from 70 / 30 to 98 / 2, preferably from 75 / 25 to 97 / 3, in particular from 80 / 20 to 95 / 5. Such compositions have particularly good processing properties, rapid curing and high extensibility coupled with high strength and good bonding properties.

[0086] The moisture-curable composition preferably comprises, besides the polymers P1 and P2, a further polymer which contains only small amounts of isocyanate groups, in particular not more than 20 parts by weight, preferably not more than 15 parts by weight, in particular not more than 10 parts by weight, of a further polymer which contains isocyanate groups, based on 100 parts by weight of the sum of the polymers P1 and P2.

[0087] The moisture curable composition preferably further comprises at least one additional component selected from meltable components, blocked amines, fillers, plasticizers, diisocyanate oligomers, catalysts and stabilizers.

[0088] In one embodiment of the present invention, the moisture curable composition preferably further comprises at least one meltable component.

[0089] Suitable meltable components are in particular the room temperature solid polyester urethane polymers containing isocyanate groups which result from the reaction of at least one diisocyanate monomer, in particular 4,4'-MDI, with at least one crystalline polyester diol or polycarbonate diol.

[0090] Suitable polyesterdiols are in particular OH-functional polyesters of adipic acid or sebacic acid or dodecanedicarboxylic acid with butane-1,4-diol or hexane-1,6-diol.

[0091] Suitable polycarbonate diols are especially the OH-functional polycarbonates of hexane-1,6-diol.

[0092] Such polymers are typically solid at room temperature and have at least partially crystalline characteristics.

[0093] Such meltable components are suitable for adhesives that are applied first in a heated state, for example at a temperature of about 60° C., and have a high initial strength very quickly after application, so that the joined parts are self-supporting and do not need to be fixed. The meltable components are now in molten form in the adhesive heated by application, and crystallize as the applied adhesive cools. Furthermore, such meltable components are suitable for adhesives that are applied at ambient temperature, where the meltable components are in crystallized form, resulting in increased sag resistance. However, meltable components are difficult to handle, and the sag resistance obtained thereby is highly shear dependent, which can lead to problems in production and application. Furthermore, the meltable components make it difficult to extrude the adhesive at room temperature and at low ambient or bonding temperatures.

[0094] Polymer P2 has a specific proportion of meltable components and allows for compositions with better extrudability at room temperature and under low temperature conditions.

[0095] Furthermore, polymer P2 allows for compositions with very good sag resistance, in which meltable components are used in much lower amounts or are completely free of meltable components.

[0096] In a further embodiment of the present invention, the moisture curable composition preferably further comprises at least one blocked amine.

[0097] Suitable blocked amines preferably have at least one aldimino or oxazolidino group, which upon contact with moisture can be hydrolyzed with release of an amino group and react with available isocyanate groups, promoting rapid blister-free curing, particularly non-sticky surfaces and / or particularly good mechanical properties.

[0098] Preferred oxazolidines are mono- or bis-oxazolidines, especially those derived from isobutyraldehyde, benzaldehyde or substituted benzaldehydes, especially benzaldehydes substituted in the para position with an optionally branched alkyl group having 10 to 14 carbon atoms.

[0099] Particularly preferred are monooxazolidines derived from N-alkylethanolamines, such as Nn-butylethanolamine, or bisoxazolidines from the reaction of OH-functional monooxazolidines derived from diethanolamine with diisocyanates, in particular hexane 1,6-diisocyanate.

[0100] Suitable aldimines are in particular di- or tri-aldimines from the reaction of commercially available primary di- or triamines with non-enolizable aldehydes, which are aldehydes that do not have a hydrogen atom in the alpha position to the carbon atom of the aldehyde group.

[0101] Preferred blocked amines are selected from aldimines of formula (I) and (II) below: [ka] During the ceremony, n is 2 or 3; A is an n-valent hydrocarbyl group optionally containing an ether oxygen and having a molecular weight in the range of 28 to 6,000 g / mol; R 1 and R 2are each independently a monovalent hydrocarbyl group having 1 to 12 carbon atoms or together a divalent hydrocarbyl group having 4 to 12 carbon atoms which is part of an optionally substituted carbocyclic ring having 5 to 8, preferably 6, carbon atoms; R 3 is hydrogen or a linear or branched alkyl, arylalkyl or alkoxycarbonyl group having 1 to 12 carbon atoms; R 4 is hydrogen or a monovalent hydrocarbyl group having 1 to 20 carbon atoms; R 5 is an alkyl or alkoxy group having 6 to 20 carbon atoms.

[0102] A is preferably an aliphatic, cycloaliphatic or arylaliphatic radical, in particular having a molecular weight in the range from 28 to 500 g / mol, in particular 1,6-hexylene, (1,5,5-trimethylcyclohexan-1-yl)methane-1,3,4(2)-methyl-1,3-cyclohexylene, 1,3-cyclohexylenebis(methylene), 1,4-cyclohexylenebis(methylene), 1,3-phenylenebis(methylene), 1,2-cyclohexylene, 1,3-cyclohexylene, 1,4-cyclohexylene, methylenebis(2-methylcyclohexan-4-yl), (bicyclo[2.2.1]heptane-2,5(2,6)-diyl)dimethylene, (tricyclo[5.2.1.0 ... 2,6 ]Decan-3(4),8(9)-diyl)dimethylene, average molecular weight M in the range of 170-500 g / mol n and an average molecular weight M in the range of 330 to 500 g / mol. n or glycerol-initiated tris(ω-polyoxypropylene) having the formula:

[0103] Preferably, R 1 and R 2 are each methyl.

[0104] Preferably, R3 is hydrogen.

[0105] Preferably, R 4 is methyl or undecyl.

[0106] Preferably, R 5 is an optionally branched alkyl group in the para position having 10 to 14 carbon atoms.

[0107] Particularly preferred blocked amines are N,N'-bis(2,2-dimethyl-3-lauroyloxypropylidene)hexylene-1,6-diamine, N,N'-bis(2,2-dimethyl-3-acetoxypropylidene)-3-aminomethyl-3,5,5-trimethylcyclohexylamine, N,N'-bis(2,2-dimethyl-3-lauroyloxypropylidene)-3-aminomethyl-3,5,5-trimethylcyclohexylamine, N,N'-bis(4-C 10~14 -alkylbenzylidene)-3-aminomethyl-3,5,5-trimethylcyclohexylamine, with average molecular weight M in the range of 450-880 g / mol n N,N'-bis(2,2-dimethyl-3-acetoxypropylidene)polyoxypropylenediamine having an average molecular weight M in the range of 750 to 1,050 g / mol n N,N'-bis(2,2-dimethyl-3-lauroyloxypropylidene)polyoxypropylenediamine having an average molecular weight M in the range of 680 to 1,100 g / mol n N,N'-bis(4-C 10~14 -alkylbenzylidene)polyoxypropylenediamine, with average molecular weight M in the range of 730-880 g / mol n N,N',N''-tris(2,2-dimethyl-3-acetoxypropylidene)polyoxypropylenetriamine having an average molecular weight M in the range of 1,150 to 1,300 g / mol n and N,N',N''-tris(2,2-dimethyl-3-lauroyloxypropylidene)polyoxypropylenetriamine having an average molecular weight M in the range of 1,000 to 1,350 g / mol. nN,N',N''-Tris(4-C 10~14 -alkylbenzylidene)polyoxypropylenetriamines.

[0108] Suitable fillers are in particular powdered or precipitated calcium carbonate, optionally coated with fatty acids, in particular stearic acid, barite, quartz flour, quartz sand, dolomite, wollastonite, calcined kaolin, sheet silicates, for example mica or talc, zeolites, aluminium hydroxide, magnesium hydroxide, silica, including finely divided silica from pyrolysis processes, cement, gypsum, fly ash, industrially produced carbon black, graphite, metal powders, for example of aluminium, copper, iron, silver or steel, PVC powder or lightweight fillers, for example hollow glass beads or gas-filled plastic spheres (microspheres), in particular the type available under the brand name Expancel® (from Akzo Nobel).

[0109] Calcium carbonate, calcined kaolin, micronized silica or industrially produced carbon black, optionally coated with fatty acids, in particular stearic acid, are preferred.

[0110] Suitable plasticizers are in particular carboxyl esters, such as phthalates, in particular diisononyl phthalate (DINP), diisodecyl phthalate (DIDP) or di(2-propylheptyl)phthalate (DPHP), hydrogenated phthalates or cyclohexane-1,2-dicarboxylates, in particular hydrogenated diisononyl phthalate or diisononyl cyclohexane-1,2-dicarboxylate (DINCH), terephthalates, in particular bis(2-ethylhexyl)terephthalate (DOTP) or diisononyl terephthalate (DINT), hydrogenated terephthalates or cyclohexane-1,4-dicarboxylates, in particular hydrogenated bis(2-ethylhexyl)terephthalate or bis(2-ethyl hexyl)cyclohexane-1,4-dicarboxylate, or hydrogenated diisononyl terephthalate or diisononyl cyclohexane-1,4-dicarboxylate, isophthalates, trimellitates, adipates, in particular dioctyl adipate, azelates, sebacates, benzoates, glycol ethers, glycol esters, plasticizers having a polyether structure, in particular polypropylene oxide mono-, di- or triols having hydroxyl groups blocked in the form of acetate groups, organic phosphates or sulfonates, polybutenes, polyisobutenes, or plasticizers derived from natural fats or oils, in particular epoxidized soybean oil or linseed oil.

[0111] Preferred plasticizers are those having a phthalate or polyether structure.

[0112] Suitable diisocyanate oligomers are, in particular, HDI biurets, such as Desmodur® N100 or N3200 (from Covestro AG), Tolonate® HDB or HDB-LV (from Vencorex) or Duranate® 24A-100 (from Asahi Kasei); HDI isocyanurates, such as Desmodur® N3300, N3600 or N3790BA (all from Covestro), Tolonate® HDT, HDT-LV or HDT-LV2 (from Vencorex), Duranate® TPA-100 or THA-100 (from Asahi Kasei) or Coronate® HX (from Tosoh Corp.); HDI uretdiones, such as Desmodur® N3400 (from Covestro); HDI iminooxadiazinediones, such as Desmodur® XP2410 (from Covestro); HDI allophanates, such as Desmodur® VP LS2102 (from Covestro); IPDI isocyanurates, either in solution, such as Desmodur® Z4470 (from Covestro), or in solid form, such as Vestanat® T1890 / 100 (from Evonik Industries); TDI oligomers, such as Desmodur® IL (from Covestro); or mixed isocyanurates based on TDI / HDI, such as Desmodur® HL (from Covestro).

[0113] Suitable catalysts are catalysts for accelerating the reaction of isocyanate groups, in particular organotin(IV) compounds, such as, in particular, dibutyltin diacetate, dibutyltin dilaurate, dibutyltin dichloride, dibutyltin diacetylacetonate, dimethyltin dilaurate, dioctyltin diacetate, dioctyltin dilaurate or dioctyltin diacetylacetonate, complexes of bismuth(III) or zirconium(IV) with ligands selected from alkoxides, carboxylates, 1,3-diketonates, oxinates, 1,3-ketoesterates and 1,3-ketoamidates, or compounds containing tertiary amino groups, such as, in particular, 2,2′-dimorpholinodiethyl ether (DMDEE).

[0114] If the moisture-curable composition contains a blocked amine, suitable catalysts are also catalysts for the hydrolysis of the blocked amino groups, in particular organic acids, in particular carboxylic acids such as 2-ethylhexanoic acid, lauric acid, stearic acid, isostearic acid, oleic acid, neodecanoic acid, benzoic acid, salicylic acid or 2-nitrobenzoic acid, organic carboxylic acid anhydrides such as phthalic anhydride, hexahydrophthalic anhydride or methylhexahydrophthalic anhydride, silyl esters of carboxylic acids, organic sulfonic acids such as methanesulfonic acid, p-toluenesulfonic acid or 4-dodecylbenzenesulfonic acid, sulfonic acid esters, other organic or inorganic acids, or mixtures of the abovementioned acids and acid esters. Particular preference is given to carboxylic acids, in particular aromatic carboxylic acids such as benzoic acid, 2-nitrobenzoic acid or in particular salicylic acid.

[0115] Also particularly suitable are combinations of different catalysts.

[0116] Suitable stabilizers are in particular stabilizers against oxidation, heat, light or UV light, in particular titanium dioxide, iron oxide, zinc oxide, benzophenones, benzotriazoles, compounds which have a 2,6-di-tert-butylphenol group (for example those known under the trade name Irganox® (from BASF)), compounds which have a 2,2,6,6-tetramethylpiperidine group (referred to as HALS (hindered amine light stabilizers), for example those known under the trade name Tinuvin® (from BASF)), or phosphorus-containing compounds (for example those known under the trade name Irgafos® (from BASF)).

[0117] The moisture-curable composition may further comprise additional additives, in particular inorganic or organic pigments, in particular titanium dioxide, chromium oxide or iron oxide; fibres, in particular glass fibres, carbon fibres, metal fibres, ceramic fibres, polymer fibres, for example polyamide fibres or polyethylene fibres, or natural fibres, for example wool, cellulose, hemp or sisal; - nanofillers, such as graphene or carbon nanotubes; - dye; - desiccant, in particular molecular sieve powder, calcium oxide, highly reactive isocyanates such as p-tosylisocyanate, monooxazolidines such as Incozol® 2 (from Incorez) or orthoformates; adhesion promoters, in particular organoalkoxysilanes, in particular epoxysilanes, such as, in particular, 3-glycidoxypropyltrimethoxysilane or 3-glycidoxypropyltriethoxysilane, (meth)acrylosilanes, anhydridosilanes, carbamatosilanes, alkylsilanes or iminosilanes, or oligomeric forms of these silanes, or titanates; - further catalysts which accelerate the reaction of isocyanate groups; rheology modifiers, in particular thickeners, in particular sheet silicates, for example bentonite, derivatives of castor oil, hydrogenated castor oil, polyamides, polyamide waxes, polyurethanes, urea compounds, fumed silica, cellulose ethers or hydrophobically modified polyoxyethylenes; solvents, in particular acetone, methyl acetate, tert-butyl acetate, 1-methoxy-2-propyl acetate, ethyl 3-ethoxypropionate, diisopropyl ether, diethylene glycol diethyl ether, ethylene glycol diethyl ether, ethylene glycol monobutyl ether, ethylene glycol mono-2-ethylhexyl ether, acetals such as propylal, butyral, 2-ethylhexylal, dioxolane, glycerol formal or 2,5,7,10-tetraoxaundecane (TOU), toluene, xylene, heptane, octane, naphtha, white spirit, petroleum ether or gasoline, in particular the Solvesso™ grades (from Exxon), and also propylene carbonate, dimethyl carbonate, butyrolactone, N-methylpyrrolidone, N-ethylpyrrolidone, p-chlorobenzotrifluoride or benzotrifluoride; natural resins, fats or oils, such as rosin, shellac, linseed oil, castor oil or soybean oil; - non-reactive polymers, in particular homo- or copolymers of unsaturated monomers from the group comprising ethylene, propylene, butylene, isobutylene, isoprene, vinyl acetate or alkyl (meth)acrylates, in particular polyethylene (PE), polypropylene (PP), polyisobutylene, ethylene / vinyl acetate copolymers (EVA) or atactic poly-α-olefins (APAO); - flame-retardant substances, in particular the aluminium hydroxide or magnesium hydroxide fillers already mentioned, and also in particular organic phosphates, such as, in particular, triethyl phosphate, tricresyl phosphate, triphenyl phosphate, diphenylcresyl phosphate, isodecyl diphenyl phosphate, tris(1,3-dichloro-2-propyl)phosphate, tris(2-chloroethyl)phosphate, tris(2-ethylhexyl)phosphate, tris(chloroisopropyl)phosphate, tris(chloropropyl)phosphate, isopropylated triphenyl phosphate, mono-, bis- or tris(isopropylphenyl)phosphates of different degrees of isopropylation, resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate) or ammonium polyphosphate; additives, in particular wetting agents, levelling agents, defoamers, air release agents or biocides; or further substances which are customarily used in moisture-curable polyurethane compositions. may contain

[0118] It may be advisable to chemically or physically dry certain materials before incorporating them into the composition.

[0119] Preferably, the compositions of the invention contain little solvent, in particular less than 5% by weight, preferably less than 2.5% by weight, of solvent. Most preferably, the compositions of the invention are essentially solvent-free.

[0120] The moisture curable composition preferably contains: - 20% to 60% by weight of a polyether urethane polymer P1, - 0.5% to 10% by weight of polymer P2, - 0% to 5% by weight of meltable components; - 20% to 60% by weight of a filler, - 0% to 35% by weight of a plasticizer, and Optionally further components, in particular blocked amines, diisocyanate oligomers, catalysts or stabilizers.

[0121] In a preferred embodiment of the invention, the moisture-curable composition comprises carbon black, in particular at least one industrially produced carbon black, in particular in an amount ranging from 5% to 40% by weight, preferably from 10% to 30% by weight. Such compositions are particularly suitable for bonding glass panes due to their high sag resistance, strength and stability, and have a particularly low tendency for the carbon black to leach out due to the hydrophobic polymer P2.

[0122] The moisture curable composition preferably contains less than 0.1% by weight of monomeric diisocyanate. Such compositions can be shipped and sold in many countries without hazardous material classification.

[0123] The moisture-curable composition is in particular produced with the exclusion of moisture and stored in a moisture-tight container at ambient temperature. Suitable moisture-tight containers are in particular drums, transport boxes, hobbocks, buckets, canisters, cans, bags, tubular bags, cartridges or tubes, in particular made of metal and / or plastic, optionally coated.

[0124] The moisture curable composition is preferably a one-component composition, which, given proper packaging and storage, is typically shelf stable for several months, up to a year or more.

[0125] Moisture-curable compositions begin to cure under the influence of moisture or water during and after application. To accelerate the cure, an accelerator component containing water and optionally a catalyst and / or a curing agent can be mixed into the composition upon application, or the composition can be contacted with such an accelerator component after its application.

[0126] During the curing process, the isocyanate groups react with each other under the influence of moisture. If the moisture curable composition contains a blocked amine, the isocyanate groups will further react with the blocked amino groups as they are hydrolyzed. The overall reaction of the isocyanate groups resulting in the curing of the composition is also referred to as crosslinking. This results in a cured composition.

[0127] The moisture required for the curing of the composition preferably enters the composition by diffusion from the air (atmospheric moisture). In this process, a solid layer of the cured composition ("skin") is formed on the surface of the composition, which is in contact with the air. The curing continues from the outside inwards in the direction of diffusion, and the skin becomes thicker and thicker, eventually surrounding the entire applied composition. Moisture can also enter the composition additionally or entirely from the substrate or substrates to which the composition is applied, and / or can come from accelerator components that are mixed into the composition during application or that come into contact with the composition after application, for example by painting or spraying.

[0128] The moisture-curable composition is preferably applied at ambient temperatures in the range of about -10 to 50°C, preferably in the range of -5 to 45°C, in particular in the range of 0 to 40°C.

[0129] If desired, the moisture-curable composition can also be applied in a heated state, for example at a temperature of about 60°C.

[0130] The moisture curable composition preferably cures at ambient temperature.

[0131] Moisture curable compositions have long processing times (open times) and rapid cure.

[0132] "Open time" refers to the period during which the composition can be worked or reworked after application without losing its ability to function. If the composition is used as an adhesive, the open time also refers in particular to the period within which bonding must be performed after its application in order for sufficient adhesion to develop. At least the open time has been exceeded when a skin is formed or when there is no longer sufficient adhesion to the substrate.

[0133] The moisture-curable compositions are preferably used as elastic adhesives and / or sealants, in particular for bonding or sealing applications in the construction and manufacturing industries or in automotive assembly, in particular for parquet bonding, assembly, bonding of installable components, module bonding, pane bonding, joint sealing, body sealing, seam sealing or cavity sealing.

[0134] Elastic connections in automotive assembly are, for example, the bonding attachment of parts, such as plastic covers, trim strips, flanges, fenders, cabs or other installable components to the painted body of an automobile, or the bonding of panes to a vehicle body, said automobile being in particular a car, truck, bus, rail vehicle or ship.

[0135] Particularly preferred is the use as an adhesive for automotive glass installation, especially for glass replacement in automobiles.

[0136] The moisture-curable composition is preferably formulated to have a paste-like consistency with structurally viscous properties at room temperature. This type of composition is applied using a suitable device, for example from a commercially available cartridge or barrel or hob, in particular in the form of beads which may have an essentially circular or triangular cross-sectional area.

[0137] Suitable substrates that can be bonded and / or sealed with the moisture curable composition are, in particular: - glass, glass-ceramic or screen-printed ceramic-coated glass or polycarbonate; - surface-finished metals or alloys, for example galvanized or chrome-plated metals, for example aluminium, copper, iron, steel, non-ferrous metals; - coated or painted substrates, in particular powder-coated metals or alloys or painted metal sheets; - paints or varnishes, in particular automotive topcoats; - cured adhesives, in particular based on polyurethanes, silane-modified polymers or polysulfides, in particular aged adhesives (residual adhesive beads) or body flanges with residual adhesive beads throughout or in places; - plastics, such as rigid or flexible PVC, polycarbonate, polystyrene, polyester, polyamide, PMMA, ABS, SAN, epoxy resins, phenolic resins, PUR, POM, TPO, PE, PP, EPM or EPDM, in each case untreated or surface-treated, for example by means of plasma, corona or flame; - fibre reinforced plastics, such as carbon fibre reinforced plastics (CFP), glass fibre reinforced plastics (GFP) and sheet moulding compounds (SMC); - repair or levelling compounds based on PCC (polymer modified cement mortar) or ECC (epoxy resin modified cement mortar); - insulating foams, in particular made of EPS, XPS, PUR, PIR, rock wool, mineral wool or expanded glass; - concrete, mortar, cement screed, fibre cement, in particular fibre cement boards, bricks, tiles, gypsum, in particular gypsum boards or anhydrous screeds, or natural stone, for example granite or marble, painted tiles or painted concrete, asphalt or bitumen; Leather, textiles, paper, wood, resins, e.g. wood materials bonded with phenolic, melamine or epoxy resins, resin / textile composites or further materials referred to as polymer composites. It is.

[0138] If necessary, the substrate can be pre-treated prior to application, especially by physical and / or chemical cleaning methods or by application of an activator or primer.

[0139] It is possible to bond and / or seal two identical or two different substrates.

[0140] The present invention further provides a method of bonding or sealing comprising: (i) a moisture-curable composition as described above, - applying to a first substrate and contacting the composition with the second substrate within the open time of the composition; or - applied to a first and a second substrate and bonding the two substrates within the open time of the composition; or - application between two substrates, (ii) curing the composition by contact with moisture.

[0141] At least one of the substrates is preferably selected from the group consisting of glass, glass ceramic, screen printed and ceramic coated glass or polycarbonate, metals, alloys, powder coated metals or alloys, paints and varnishes and cured adhesives, in particular residual adhesive beads, and / or metal sheets painted with automotive topcoats.

[0142] Application and curing of the moisture curable composition, or a bonding or sealing method, results in an article bonded or sealed with the composition, which may be an erected structure or part thereof, in particular an erected structure above or below ground level in civil engineering, a bridge, a roof, a staircase or a facade, or it may be an industrial or consumer item, in particular a window, a pipe, a rotor blade of a wind turbine, a domestic appliance or a means of transport, such as, in particular, a car, a bus, a truck, a rail car, a ship, an airplane or a helicopter, or an installable component thereof.

[0143] Thus, the present invention further provides articles resulting from the described methods of bonding or sealing.

[0144] It is particularly preferred to use this method of bonding for the elastic bonding of glass panes to motor vehicles, in particular for glass replacement, where good adhesion to the residual adhesive beads is of particular importance.

[0145] The moisture-curing composition has advantageous properties, particularly good bonding properties coupled with a long open time, particularly good application properties coupled with a high sag resistance, particularly good extrudability, a non-glossy surface coupled with good set, strength, extensibility, elasticity and hazardous materials classification that do not change, and particularly good weatherability. Thus, the composition is particularly suitable as an elastic adhesive in automobile assembly, in particular for the replacement of defective elastically bonded windshields of automobiles. EXAMPLES

[0146] Examples intended to clarify the invention as described are presented herein below, the invention being of course not limited to these described examples.

[0147] "Standard climatic conditions" (SCC) refers to a temperature of 23±1°C and a relative air humidity of 50±5%.

[0148] Unless otherwise stated, chemicals used were from Sigma-Aldrich Chemie GmbH.

[0149] Polyols used: Desmophen® 5031 BT: glycerol initiated ethylene oxide terminated polyoxypropylene triol, OH value 28 mg KOH / g (from Covestro) Acclaim® 4200: Polyoxypropylene diol, OH value 28 mg KOH / g (from Covestro) Priplast® 1838: amorphous polyester diol based on dimer fatty acids, OH value 56 mg KOH / g, liquid at room temperature (from Croda) (=hydrophobic diol) Priplast® 1837: amorphous polyester diol based on dimeric fatty acids, OH value 110 mg KOH / g, liquid at room temperature (from Croda) (=hydrophobic diol) Priplast® 3196: amorphous polyester diol based on dimeric fatty acids, OH value 37 mg KOH / g, liquid at room temperature (from Croda) (=hydrophobic diol) Priplast® 3197: amorphous polyester diol based on dimeric fatty acids, OH value 56 mg KOH / g, liquid at room temperature (from Croda) (=hydrophobic diol) Vorapel® D3201: Poly(1,2-butylene glycol), OH value 56 mg KOH / g, liquid at room temperature (from Dow) (=hydrophobic diol) Dynacoll® 7360: room temperature solid semi-crystalline polyester diol, OH value 34 mg KOH / g (from Evonik)

[0150] Preparation of polymers containing isocyanate groups: Viscosity was measured using a thermostated Rheotec RC30 cone-plate viscometer (cone diameter 25 mm, cone angle 1°, cone tip-plate distance 0.5 mm, shear rate 50 s -1 ) was measured.

[0151] The diisocyanate monomer content was determined using HPLC (photodiode array detection; 0.04 M sodium acetate / acetonitrile as mobile phase) after prior derivatization with N-propyl-4-nitrobenzylamine.

[0152] Polymer P1-1: 725.0 g of Desmophen® 5031BT and 275.0 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted by known methods to give a polyether urethane polymer with an NCO content of 7.6 wt. %, a viscosity of 6.5 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 20 wt. %.

[0153] Subsequently, most of the volatile constituents, especially diphenylmethane 4,4'-diisocyanate, were removed by distillation in a short-path evaporator (jacket temperature 180 °C, pressure 0.1-0.005 mbar, condensation temperature 47 °C). The polyether urethane polymer thus obtained had an NCO content of 1.7 wt.%, a viscosity of 19 Pa·s at 20 °C, and a diphenylmethane 4,4'-diisocyanate content of 0.04 wt.%.

[0154] Polymer P1-2: 727.0 g of Acclaim® 4200 and 273.0 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted by known methods to give a polyether urethane polymer having an NCO content of 7.6 wt. %, a viscosity of 5.2 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 18 wt. %.

[0155] Subsequently, most of the volatile constituents, in particular the diphenylmethane 4,4'-diisocyanate, were removed as described for polymer P1-1. The polyetherurethane polymer thus obtained had an NCO content of 1.8% by weight, a viscosity of 15.2 Pa s at 20°C, and a diphenylmethane 4,4'-diisocyanate content of 0.08% by weight.

[0156] Polymer P2-1: 597.5 g of Priplast® 1838 and 402.5 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted at 80° C. to give a polymer with an NCO content of 11.0 wt. %, a viscosity of 36 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 26 wt. %.

[0157] Subsequently, most of the volatile constituents, in particular the diphenylmethane 4,4'-diisocyanate, were removed as described for polymer P1-1. The polymer thus obtained was slightly turbid and of liquid, viscous consistency at room temperature. It had an NCO content of 2.8% by weight, a viscosity of 312 Pa·s at 20°C or 11.5 Pa·s at 60°C, and a diphenylmethane 4,4'-diisocyanate content of 0.09% by weight.

[0158] Polymer P2-2: 445.0 g Priplast® 1837 and 555.0 g diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted at 80° C. to give a polymer with an NCO content of 14.8 wt. %, a viscosity of 6.5 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 35 wt. %.

[0159] Subsequently, most of the volatile constituents, especially the diphenylmethane 4,4'-diisocyanate, were removed as described for polymer P1-1. The polymer thus obtained was slightly turbid and of a liquid, viscous consistency at room temperature. It had an NCO content of 4.8% by weight, a viscosity of 11 Pa·s at 60°C, and a diphenylmethane 4,4'-diisocyanate content of 0.06% by weight.

[0160] Polymer P2-3: 663.0 g Priplast® 3196 and 337.0 g diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted at 80° C. to give a polymer with an NCO content of 9.4 wt. %, a viscosity of 57 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 23 wt. %.

[0161] Subsequently, most of the volatile constituents, in particular the diphenylmethane 4,4'-diisocyanate, were removed as described for polymer P1-1. The polymer thus obtained was slightly turbid and of liquid, viscous consistency at room temperature. It had an NCO content of 2.2% by weight, a viscosity of 17 Pa·s at 60°C, and a diphenylmethane 4,4'-diisocyanate content of 0.06% by weight.

[0162] Polymer P2-4: 600.0 g of Priplast® 3197 and 400.0 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted at 80° C. to give a polymer with an NCO content of 10.7 wt. %, a viscosity of 28 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 25 wt. %.

[0163] Subsequently, most of the volatile constituents, especially the diphenylmethane 4,4'-diisocyanate, were removed as described for polymer P1-1. The polymer thus obtained was of a slightly turbid, liquid, viscous consistency at room temperature. It had an NCO content of 2.8% by weight, a viscosity of 16 Pa·s at 60°C, and a diphenylmethane 4,4'-diisocyanate content of 0.08% by weight.

[0164] Polymer P2-5: 601.1 g of Vorapel® D3201 and 398.9 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted at 80° C. to give a polymer with an NCO content of 10.7 wt. %, a viscosity of 3.5 Pa·s at 20° C., and a diphenylmethane 4,4′-diisocyanate content of about 24 wt. %.

[0165] Subsequently, the majority of the volatile constituents, in particular the diphenylmethane 4,4'-diisocyanate, were removed as described for polymer P1-1. The polymer thus obtained had an NCO content of 3.0% by weight, a viscosity of 26 Pa·s at 20° C., and a diphenylmethane 4,4'-diisocyanate content of 0.06% by weight.

[0166] Polymer M: 1000 g of Dynacoll® 7360 and 142 g of diphenylmethane 4,4′-diisocyanate (Desmodur® 44MC L, from Covestro) were reacted at 80° C. to give a room temperature solid polymer with an NCO content of 2.0 wt. % and a diphenylmethane 4,4′-diisocyanate content of 2.3 wt. %.

[0167] Polymers P1-1 and P1-2 are polyether urethane polymer P1. Polymers P2-1 to P2-5 are hydrophobic polymer P2. Polymer M is a room temperature solid polymer, which was used as the meltable component.

[0168] Moisture-curing composition: Compositions Z1~Z6: For each composition, the specific ingredients in Table 1 were thoroughly mixed in the specific amounts (in parts by weight) using a planetary mixer under reduced pressure with the exclusion of moisture, and the compositions were dispensed into tubular bags with airtight seals and stored at room temperature.

[0169] For rapid hardening, a water-containing accelerator component was added to the composition at the time of application. For this purpose, the composition was applied from a PowerCure dispenser (available from Sika Schweiz AG) with the metered addition of 2% by weight of water-containing paste into the composition by squeezing and mixing with a dynamic mixer.

[0170] The adhesion to the residual adhesive bead was determined on the cured and aged adhesive layer. For this purpose, a commercially available polyurethane adhesive for bonding glass panes (Sikaflex®-250SV-3, from Sika Automotive Hamburg GmbH) was applied to the glass body in the form of a triangular bead with a width of about 8 mm and a height of about 10 mm, covered with a silicone-coated release paper, pressed to a layer thickness of about 5 mm, cured under standard climatic conditions for 7 days, the release paper was removed and the compressed adhesive bead was aged for 14 days at 80° C. Subsequently, the cured and aged adhesive bead was cut from the glass body to a layer thickness of about 1 mm.

[0171] The accelerated composition was then applied under standard climatic conditions from a PowerCure dispenser in the form of a triangular bead about 8 mm wide and about 10 mm high to a strip of silicone-coated release paper. In each case, after the waiting time specified in Table 1, the triangular bead applied to the release paper was turned over and placed on the residual adhesive bead remaining on the glass body with the release paper on top and the composition in contact with the residual adhesive bead. The composition was subsequently pressed to a layer thickness of about 5 mm and cured under standard climatic conditions for 7 days, then the release paper was removed and the adhesion of the cured composition on the residual adhesive bead was tested by making an incision in the cured composition at the narrow end directly above the bonding surface, holding the incised end of the composition with rounded tweezers and trying to pull the composition away from the substrate (=residual adhesive bead). The composition was then cut again to the substrate, the cut part was rolled up with rounded tweezers and an attempt was made to pull the composition away from the substrate again. In this way, the composition was cut away from the substrate by pulling it away. The bonds were subsequently assessed for failure profile using the following scale: "Very good" represents greater than 95% cohesive failure; "Good" represents 75% to 95% cohesive failure; "Moderate" represents 50%-75% cohesive failure; "Poor" refers to less than 50% cohesive failure; "No adhesion" represents 0% cohesive failure or 100% adhesive failure.

[0172] The results are reported in Table 1.

[0173] The composition labeled "(Reference)" is a comparative example.

[0174] [Table 1]

[0175] Compositions Z7 and Z8: Each composition was prepared as described for composition Z1 using the components identified in Table 2 in the amounts (in parts by weight) identified, dispensed into aluminum cartridges with airtight seals, and stored at room temperature.

[0176] Each composition was applied and pressed between two silicone-coated release papers to obtain a film with a thickness of 2 mm, and stored under standard climatic conditions for 14 days. After removing the release paper, a square test specimen (75×150 mm) was cut from the cured film and tested in a QUV weathering apparatus for the time specified in Table 2, and then the weathered surface was tested for carbon black staining by first manually pressing a transparent adhesive tape onto the surface and then attaching it to a white printer paper. Carbon black staining was rated as "no" if a light gray stain was visible, rated as "moderate" if the carbon black stain was a dark gray stain, and rated as "severe" if the carbon black stain was a black stain.

[0177] The results are reported in Table 2.

[0178] The composition labeled "(Reference)" is a comparative example.

[0179] [Table 2]

[0180] Compositions Z9~Z18: Each composition was prepared as described for composition Z1 using the components specified in Tables 3 and 4 in the amounts specified (in parts by weight), dispensed into aluminum cartridges with airtight seals, and stored at room temperature.

[0181] Each composition was tested as follows: The measures determined for the processability or applicability of the composition are compression force, sag resistance and thread formation. Low compression force, high sag resistance and short thread formation are representative of good processability or applicability.

[0182] The compression force was determined at 23° C. and 5° C. The first closed cartridge was stored for 7 days at 23° C., the second for 6 days at 23° C. and then for 24 hours at 5° C. The compression force was then measured in each case using an extrusion device (Zwick / Roell Z005) by screwing a nozzle with an internal diameter of 5 mm onto the cartridge and then measuring the force required to extrude the composition through the nozzle at an extrusion speed of 60 mm / min. The reported value is the average of the forces measured after compression distances of 22 mm, 24 mm, 26 mm and 28 mm.

[0183] The sag resistance of each composition was determined by applying triangular beads approximately 8 mm wide and 20 mm high to a vertical corrugated cardboard surface under standard climatic conditions in such a way that the triangular beads were arranged as a horizontal strip 8 mm wide with a protruding height (=tip) of 20 mm. After curing under standard climatic conditions, an assessment was made as to whether and how the position of the applied beads changed. More specifically, the extent to which the tip, measured from a horizontal position, sagged downwards was determined. A sag of less than 1 mm was rated as "very good", 1-3 mm as "good", 4-7 mm as "average" and 8 mm or more as "poor". A "liquid" composition is defined as one in which the applied material moves downwards, i.e. sags downwards, not only at the tip of the applied triangular bead, but also at the base.

[0184] Thread formation was determined for several compositions by measuring the length of the thread formed by moving the application cartridge away from the triangular bead that was applied for sag resistance determination.

[0185] The measure determined for the processing time (open time) was the skin time (ST). For this purpose, a few grams of the composition were applied under standard climatic conditions to a cardboard in a layer thickness of about 2 mm, and the period was determined after which no residues remained any more on an LDPE pipette used to gently tap the surface of the composition.

[0186] For the determination of the mechanical properties, each composition was pressed between two silicone-coated release papers to obtain a film 2 mm thick and stored under standard climatic conditions for 14 days. After removing the release papers, several test specimens were punched out and tested as described below.

[0187] For the determination of the tensile strength (TS), elongation at break (EaB) and modulus at an elongation of 0.5-5%, the films were die-cut into dumbbells having a length of 75 mm with a bar length of 30 mm and a bar width of 4 mm, which were tested according to DIN EN53504 at a strain rate of 200 mm / min.

[0188] Some test specimens were also punched out for the determination of the tear propagation resistance and tested according to DIN ISO 34 at a strain rate of 500 mm / min.

[0189] Appearance and gloss were determined visually on the films produced for the determination of mechanical properties. "Satisfactory" was used to describe a non-tacky flat film with no blistering.

[0190] To determine the strength of the adhesive bond, the overlap shear strength (LSS) for some compositions was determined on glass. For this purpose, composite specimens were produced by bonding two glass plates, degreased with isopropanol and pretreated with Sika® Aktivator 100 (from Sika Schweiz), in such a way that the overlapping adhesive bond had dimensions of 12×25 mm and a thickness of 4 mm, with the glass plates protruding at the tips. After storing the composite specimens under standard climatic conditions for 14 days, the overlap shear strength was tested according to DIN EN 1465 at a strain rate of 20 mm / min. As a measure of the thermal and hydrolytic stability of the bond, further test specimens were further stored in an air-circulating oven at 100° C. or at 70° C. / 100% relative humidity for 7 days, cooled under standard climatic conditions and tested in the same way. The results are indicated with the addition "14d SCC" or "7d 100° C." or "7d 70 / 100".

[0191] The results are reported in Tables 3 and 4.

[0192] The composition labeled "(Reference)" is a comparative example.

[0193] [Table 3]

[0194] [Table 4]

Claims

1. A moisture-curable composition that is liquid or pasty at room temperature, comprising: at least one polyether urethane polymer P1 containing isocyanate groups and having a content of 1,2-propyleneoxy units in the polyether segments of at least 80% by weight, and at least one hydrophobic polymer P2, liquid at room temperature, containing isocyanate groups, obtained from the reaction of at least one diisocyanate monomer with a hydrophobic diol having an OH number in the range from 28 to 120 mg KOH / g, wherein the hydrophobic diol is selected from the group consisting of dimer fatty acid based polyester diols and poly(1,2-butylene glycol); wherein the polymers P1 and P2 are prepared separately from each other and the polymer P1 / polymer P2 is present in a weight ratio ranging from 70 / 30 to 98 / 2, Moisture curable compositions.

2. 2. The moisture-curing composition according to claim 1, characterized in that the polymer P1 has an NCO content ranging from 1% to 5% by weight.

3. 3. A moisture-curing composition according to claim 1, characterized in that the isocyanate groups of polymer P1 are derived from diphenylmethane 4,4'-diisocyanate.

4. 4. The moisture-curing composition according to claim 1 , characterized in that the polymer P1 is obtained from the reaction of at least one monomeric diisocyanate with at least one, optionally ethylene oxide-terminated, polyoxypropylene diol or triol having an OH number ranging from 7.5 to 112 mg KOH / g.

5. 5. The moisture-curable composition according to claim 1, wherein the polymer P1 has a diisocyanate monomer content of less than or equal to 0.5% by weight.

6. 6. The moisture-curing composition according to claim 1, wherein the polymer P2 has an NCO content ranging from 1.5% to 6% by weight.

7. 7. The moisture-curing composition according to claim 1, wherein the hydrophobic diol is a polyester diol based on an amorphous dimeric fatty acid.

8. 8. The moisture-curing composition according to any one of claims 1 to 7, characterized in that the polymer P2 has a diisocyanate monomer content of less than or equal to 0.5% by weight and is obtained from the reaction of at least one diisocyanate monomer with said hydrophobic diol in an NCO / OH ratio of at least 3 / 1, followed by the removal of most of the diisocyanate monomer by suitable separation methods.

9. Polymer P2 was measured for 50 s in a cone-plate viscometer having a cone diameter of 25 mm, a cone angle of 1°, and a cone tip-plate distance of 0.5 mm. -1 The moisture-curable composition according to any one of claims 1 to 8, characterized in that it has a viscosity in the range of 10 to 1000 Pa·s at 20°C, measured at a shear rate of 1000 Pa·s.

10. 10. The moisture-curable composition according to any one of claims 1 to 9, characterized in that at least one further component is further present, selected from meltable components, blocked amines, fillers, plasticizers, diisocyanate oligomers, catalysts and stabilizers.

11. 11. The moisture-curable composition of claim 10, comprising: - from 20% to 60% by weight of polymer P1, - 0.5% to 10% by weight of polymer P2, - 0% to 5% by weight of meltable components, - from 20% to 60% by weight of a filler, - 0% to 35% by weight of a plasticizer, and Optionally further components, in particular blocked amines, diisocyanate oligomers, catalysts, or stabilizers.

12. 12. The moisture-curable composition according to claim 10 or 11, further comprising carbon black.

13. A moisture-curable composition according to any one of claims 1 to 12, characterized in that it contains less than 0.1% by weight of diisocyanate monomers.

14. Methods of bonding or sealing, including: (i) a moisture-curable composition according to any one of claims 1 to 13, - applying to a first substrate and contacting said composition with a second substrate within the open time of said composition; or - applied to a first and a second substrate and bonding the two substrates within the open time of the composition; or - application between two substrates; (ii) curing said composition by contact with moisture.

15. 15. An article obtained from the method of claim 14.

Citation Information

Patent Citations

  • Single-component moisture-curable polyurethane sealant and method for preparing same

    CN108048025A

  • Polyurethane resin composition

    JP1989132662A

  • Bonding of tile

    JP1989132675A

  • Polyurethane adhesive composition

    JP1989167389A

  • Thermoplastic moisture cure polyurethanes

    US6355317B1

Cited By

  • Polyurethane pre-polymer, method of obtention and uses thereof

    WO2026074401A1