High toughness hot rolled steel plate and manufacturing method thereof

A steel composition and microstructure optimized with controlled cooling and hot rolling address the challenges of high toughness, weldability, and strength in high-strength steels, achieving high Charpy impact energy and tensile strength with good weldability.

JP7559064B2Active Publication Date: 2024-10-01ARCELORMITTAL SA
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022530235
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-19
Filing Date
2020-12-17
Publication Date
2024-10-01
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Existing high-strength steels face challenges in achieving high toughness, weldability, and uniform elongation while maintaining high tensile strength, due to issues like brittleness and complex manufacturing processes.

Method used

A steel composition with specific elements (C, Mn, Si, B, Ti, Nb, Mo, Al, Cr) and microstructure (martensite, lath bainite, austenite) is developed, optimized through controlled cooling and hot rolling, ensuring high Charpy impact energy, tensile strength, and good weldability.

Benefits of technology

The solution achieves a steel plate with 0.50 J/mm² Charpy impact energy, 1450 MPa tensile strength, and 5% uniform elongation, with excellent weldability and processing ease.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559064000001
    Figure 0007559064000001
  • Figure 0007559064000002
    Figure 0007559064000002
  • Figure 0007559064000003
    Figure 0007559064000003
Patent Text Reader

Abstract

The present invention relates to a hot-rolled steel sheet, which contains, by weight percent, C: 0.10 to 0.25%, Mn: 3.5 to 5.0%, Si: 0.80 to 1.60%, B: 0.0003 to 0.004%, S≦0.010%, P≦0.020%, N≦0.008%, with the remainder being iron and unavoidable impurities resulting from smelting, and which has a surface fraction of between 50% and 80% lath bainite, less than 30% granular bainite, and the remainder being martensite, island martensite-austenite, and austenite film, and has a thickness of 1 μm. 2 Maximum length L of larger particles max and the maximum width of the particle W max The present invention relates to a hot-rolled steel sheet having a microstructure containing less than 20% martensite and islands of MA, with a product of:
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a high strength steel plate having high toughness and good weldability and a method for obtaining such a steel plate. [Background technology]

[0002] It is known to use steel sheets made from DP (Dual Phase) steels or TRIP (Transformation Induced Plasticity) steels to manufacture various items such as body structural members and body panel parts for automobiles.

[0003] One of the main challenges in the automotive industry is to reduce the weight of vehicles to improve their fuel efficiency in terms of global environmental conservation, without neglecting safety requirements. To meet these requirements, new high-strength steels are continuously developed by the steelmaking industry to have steel plates with improved yield strength and tensile strength, as well as good ductility and formability.

[0004] One of the developments that has been made to improve the mechanical properties is to increase the manganese content in the steel. The presence of manganese helps to make the steel more ductile by stabilizing the austenite. However, these medium manganese steels exhibit a weakness of brittleness.

[0005] Publication WO2007101921 describes a method for obtaining a "multiphase" hot-rolled steel sheet, in particular with a manganese content comprised between 1% and 3%. The microstructure consists of at least 75% bainite, an amount of retained austenite of at least 5% and at least 2% martensite. 2 In order to obtain a Charpy V-notch fracture energy exceeding 0.05 mm (corresponding to 0.05 mm) and the desired microstructure, the cooling of the hot rolled steel sheet must be controlled. Two cooling stages are actually required to obtain the desired properties, which complicates the manufacturing process. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2007 / 101921 Summary of the Invention [Problem to be solved by the invention]

[0007] Therefore, an object of the present invention is to solve the above-mentioned problems and to provide a thermal shock absorber having a thermal shock absorber capacity of 0.50 J / mm at 20° C. 2 It is an object of the present invention to provide a steel plate having a higher Charpy impact energy, a tensile strength TS of 1450 MPa or more, a high uniform elongation of 5% or more, and high toughness which can be easily processed by conventional process routes.It is another object of the present invention to provide a steel plate having good weldability. [Means for solving the problem]

[0008] The object of the present invention is achieved by providing a steel sheet according to claim 1. The steel sheet may also comprise the features according to any one of claims 2 to 6. Another object is achieved by providing a method according to claim 7. Another object of the present invention is achieved by providing a steel sheet comprising the features according to claim 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The invention will now be described in detail and illustrated by examples without introducing any limitations.

[0010] Hereinafter, Ms denotes the martensitic transformation start temperature, i.e. the temperature at which austenite begins to transform into martensite on cooling. This temperature can be calculated from the following formula, based on the weight percentages of the corresponding elements:

[0011] Ms=560-(30*%Mn+13*%Si-15*%Al+12*%Mo)-600*(1-exp(-0,96*%C))

[0012] The composition of the steel according to the invention is now described and the contents expressed as percentages by weight.

[0013] The carbon content is comprised between 0.10% and 0.25%. If the carbon content is too high, the weldability of the steel sheet is insufficient. If the carbon content is less than 0.10%, the austenite fraction is not stabilized enough to obtain the targeted properties. In a preferred embodiment of the present invention, the carbon content is comprised between 0.15% and 0.20%.

[0014] The manganese content is comprised between 3.5% and 5.0%. If the addition exceeds 5.0%, the risk of central segregation increases and the toughness is impaired. Below 3.5%, the final structure contains an insufficient fraction of retained austenite to obtain the desired properties. In a preferred embodiment of the invention, the manganese content is comprised between 3.5% and 4.5%.

[0015] According to the invention, the silicon content is comprised between 0.80% and 1.60%. A silicon addition of at least 0.80% helps to stabilize a sufficient amount of retained austenite. Above 1.60%, silicon is detrimental to toughness. Moreover, silicon oxide forms on the surface, impairing the coatability of the steel. In a preferred embodiment of the invention, the silicon content is between 1.00% and 1.60%.

[0016] According to the invention, the boron content is comprised between 0.0003% and 0.004%. The presence of boron delays the bainite transformation to lower temperatures, and the bainite formed at low temperatures has a lath morphology that enhances toughness. In addition, boron improves the weldability of the steel sheet. Above 0.004%, the formation of boron carbides at the prior austenite grain boundaries is promoted, making the steel more brittle. Below 0.0003%, there is not a sufficient concentration of free B to segregate at the prior austenite grain boundaries and enhance the toughness of the steel. In a preferred embodiment of the invention, the boron content is between 0.001% and 0.003%.

[0017] Optionally, certain elements can be added to the composition of the steel according to the invention.

[0018] Titanium may optionally be added up to 0.04% to provide precipitation strengthening. Preferably, a minimum of 0.01% titanium is added in addition to boron to protect the boron from the formation of BN.

[0019] Niobium may be added up to 0.05% to refine the austenite grains and provide precipitation strengthening during hot rolling. Preferably, the minimum amount of niobium added is 0.0010%.

[0020] Molybdenum may be added optionally with a maximum limit of 0.3%. Molybdenum stabilizes austenite and increases the toughness of the steel. In addition, molybdenum improves the weldability of the steel plate. Above 0.3%, the addition of molybdenum becomes costly and ineffective considering the properties required.

[0021] Aluminum can be added optionally up to 0.90%, since it is a very effective element for deoxidizing steel in the liquid phase during refining. Furthermore, aluminum improves the weldability of the steel sheet. The aluminum content is less than 0.90% to avoid the occurrence of inclusions and to avoid oxidation problems. Preferably, the aluminum content is comprised between 0.10% and 0.90%. More preferably, the aluminum content is comprised between 0.20% and 0.90%. More preferably, the aluminum content is comprised between 0.30% and 0.90%, or even between 0.40% and 0.90%.

[0022] According to the invention, a maximum of 0.80% chromium is permitted, beyond which saturation effects become significant and chromium addition becomes useless and expensive.

[0023] The balance of the steel composition is iron and impurities resulting from smelting. In this respect, at least P, S and N are considered as residual elements, which are unavoidable impurities. Their contents are less than 0.010% for S, less than 0.020% for P and less than 0.008% for N.

[0024] In particular, phosphorus segregates at grain boundaries and, at a phosphorus content exceeding 0.020%, the toughness of the steel decreases.

[0025] Next, the microstructure of the hot-rolled steel sheet according to the present invention will be described. Hereinafter, the aspect ratio is defined as the maximum length L max The maximum width W of the particle measured at 90° to said maximum length max is the ratio of.

[0026] The hot rolled steel sheet has a microstructure consisting of between 50% and 80% lath bainite, less than 30% granular bainite, and the balance being martensite, martensite-austenite islands (MA) and austenite film, the sum of which is comprised between 15% and 35%. Furthermore, less than 20% of the martensite and the MA islands are within 1 μm. 2 Maximum length L of larger particles max and the maximum width of the particle W max It has a product with.

[0027] The lath bainite morphology is obtained due to the presence of boron which retards the bainite transformation and low temperature coiling. According to the invention, lath bainite is bainite with an aspect ratio of 3 or more. The presence of between 50% and 80% lath bainite is beneficial for the toughness of hot rolled steel. Granular bainite exhibits an aspect ratio of less than 3.

[0028] The balance of the microstructure includes martensite, MA islands, and austenite film, the sum of which is included in the range of 15% to 35% to ensure a uniform elongation of more than 5%. If the sum of martensite, MA islands, and austenite film exceeds 35%, the austenite in the MA islands and austenite film becomes unstable and transforms into martensite, leading to a decrease in elongation.

[0029] The martensite and island-like MA portions are less than 20%. 2 Bigger L max and W maxIf it exceeds 20%, the island-like MA transforms into fresh martensite, resulting in a decrease in elongation.

[0030] Martensite-austenite (MA) islands have an aspect ratio of 2 or less. These MA islands are generated during coiling. Part of the austenite transforms in the lath bainite as described above. Part of the austenite transforms to martensite and creates MA islands during coiling. The last part of the austenite remains in the final microstructure. Austenite films are the austenite between the bainite laths with an aspect ratio of 2 or more. Both MA islands and austenite films are beneficial to the toughness of hot rolled steel plates.

[0031] The hot-rolled steel sheet according to the invention has a hardness of 0.50 J / mm at 20° C., measured according to standards ISO 148-1:2006(F) and ISO 148-1:2017(F). 2 The hot rolled steel sheet according to the invention has a tensile strength TS of more than or equal to 1450 MPa and a uniform elongation UE of more than or equal to 5%. Preferably, the hot rolled steel sheet according to the invention has a total elongation TE of more than or equal to 7%. TS, UE and TE are measured according to the ISO standard ISO 6892-1.

[0032] The steel sheet according to the invention can be manufactured by any suitable manufacturing method, which the person skilled in the art can define, however it is preferable to use a method according to the invention comprising the following steps:

[0033] Further, a semi-finished product capable of being hot rolled is provided with the above-mentioned steel composition. The semi-finished product is heated to a temperature comprised between 1150°C and 1300°C to facilitate hot rolling, the final hot rolling temperature FRT being comprised between 750°C and 900°C. Preferably, the FRT is comprised between 800°C and 900°C. If the FRT is higher than 900°C, the bainite transformation rate is significantly reduced during coiling, leading to the formation of a high fraction of martensite, islands of MA and austenite in the final microstructure. Furthermore, a 1 μm2 Bigger L max *W max The presence of a large fraction of martensite having the above structure and MA islands leads to a decrease in elongation.

[0034] The hot-rolled steel is then cooled to a temperature T between (Ms-100°C) and 550°C. coil and wind it up.

[0035] The hot rolled steel sheet is then cooled to room temperature.

[0036] After coiling, the steel sheet may be pickled to remove oxidation.

[0037] Another object of the present invention is to provide a steel plate having good weldability.

[0038] The welded assembly is produced by fabricating two pieces of hot rolled steel sheet and resistance spot welding the two steel parts together.

[0039] Spot welding under standard ISO 18278-2 conditions is carried out on hot-rolled steel sheets.

[0040] In the test used, the specimen consists of two steel sheets, in identical cross-welded configuration. A force is applied to break the weld. This force is known as the cross tensile strength (CTS) and is expressed in daN. It depends on the diameter of the weld and on the thickness of the metal, i.e. the thickness of the steel and of the metal coating. It makes it possible to calculate a coefficient α, which is the ratio of the value of CTS to the product of the diameter of the weld multiplied by the thickness of the base material. This coefficient is expressed in daN / mm 2 It is expressed as:

[0041] The plug ratio is equal to the plug diameter divided by the molten zone diameter.

[0042] The resistance spot weld joining the first steel sheet to the second steel sheet is characterized by a high resistance in a cross tension test, defined by an α value of at least 50 daN / mm2 and a plug ratio of at least 80%.

[0043] The present invention will now be illustrated by the following examples, which are not intended to be limiting in any way. EXAMPLES

[0044] [Example 1] Four grades, whose compositions are summarized in Table 1, were cast into semi-finished products and processed into steel plates.

[0045] The compositions tested are summarized in the following table, with elemental contents expressed as weight percent.

[0046] [Table 1]

[0047] The as-cast steel semi-finished products were reheated at 1200°C, hot rolled and coiled. The following specific conditions were applied:

[0048] [Table 2]

[0049] Then, the hot-rolled steel plates were analyzed, and the corresponding microstructural elements, mechanical properties and welding properties were summarized in Tables 3, 4 and 5, respectively.

[0050] The phase ratios in the microstructure of the obtained hot-rolled steel sheets were determined.

[0051] [Table 3]

[0052] The surface fraction of the phases in the microstructure is determined through the following method: a specimen is cut from the hot roll, polished and etched with per se known reagents to expose the microstructure. The section is then examined through a scanning electron microscope, for example a scanning electron microscope equipped with a field emission gun ("FEG-SEM"), at a magnification of more than 5000 times, in secondary electron mode.

[0053] The surface fraction of the austenite film and the islands of MA is determined by SEM observation after Nital or Picral / Nital reagent etching.

[0054] According to the present invention, lath bainite is bainite having an aspect ratio of 3 or more. According to the present invention, island MA has an aspect ratio of 2 or less.

[0055] The mechanical properties of the tested samples were determined and are summarized in the following table.

[0056] [Table 4]

[0057] The weld properties of several samples were determined and are summarized in the following table.

[0058] [Table 5]

[0059] These examples show that the steel sheets according to the invention, ie, Examples 1 to 3, are unique in that they exhibit all the targeted properties due to their specific composition and microstructure.

[0060] In test 4, the steel sheet was hot rolled at 910°C FRT to obtain a high fraction of martensite and island-like MA, which results in a uniform elongation of less than 5%.

[0061] In tests 5 and 6, the absence of boron in steels C and D leads to lower levels of Charpy impact energy and reduces the fracture toughness of the steels due to the formation of more than 30% granular bainite. With regard to the weldability parameters, the absence of boron, molybdenum and aluminum is detrimental to α and plug ratio.

Claims

1. 1. A hot rolled steel sheet having the following composition, in weight percent: C: 0.10-0.25% Mn: 3.5-5.0% Si: 0.80~1.60% B: 0.0003-0.004% S≦0.010% P≦0.020% N≦0.008% 0.01≦Ti≦0.04% 0.20≦Mo≦0.3% 0.10≦Al≦0.90% and Optionally, the following elements, in weight percent: Nb≦0.05% Cr≦0.80% and The balance of the composition is iron and inevitable impurities resulting from smelting; It is made of steel having The steel plate has a surface fraction of - 50% to 80% lath bainite with an aspect ratio of 3 or more; - less than 30% granular bainite with an aspect ratio of less than 3; the balance being martensite, martensite-austenite islands MA with an aspect ratio of less than or equal to 2, and an austenite film, the sum of which is between 15% and 35%; - and 1 μm 2 The maximum length of the larger particle L max and the maximum width of the particle W max and the martensite and the islands M-A A hot-rolled steel sheet having a microstructure comprising:

2. 2. The hot rolled steel sheet according to claim 1, wherein the manganese content is between 3.5% and 4.5%.

3. 3. The hot rolled steel sheet according to claim 1, wherein the silicon content is between 1.00% and 1.60%.

4. The hot-rolled steel sheet has a compressive strength of 0.50 J / mm at 20°C. 2 The hot rolled steel sheet according to any one of claims 1 to 3, having a more strictly high Charpy impact energy.

5. The hot-rolled steel sheet according to any one of claims 1 to 4, wherein the hot-rolled steel sheet has a tensile strength TS of 1450 MPa or more.

6. The hot-rolled steel sheet according to any one of claims 1 to 5, wherein the hot-rolled steel sheet has a uniform elongation UE of 5% or more.

7. 2. A method for producing a hot rolled steel sheet according to claim 1, comprising the following successive steps: - casting a steel to obtain a semi-finished product, said semi-finished product having a composition according to claim 1, the semi-finished product at a temperature T comprised between 1150 ° C. and 1300 ° C. reheat reheating the mixture with - hot rolling the semi-finished product at a finish hot rolling temperature between 750°C and 900°C to obtain a hot rolled steel sheet; - cooling the hot-rolled steel sheet; The hot-rolled steel sheet is wound at a coiling temperature T between (Ms-100°C) and 550°C. coil The process of winding the steel sheet A manufacturing method comprising:

8. A resistance spot weld of two steel parts of a hot rolled steel sheet according to any one of claims 1 to 6 or obtained by the method according to claim 7, wherein the resistance spot weld has a strength of at least 50 daN / mm 2 and a plug ratio of at least 80%.

Citation Information

Patent Citations

  • Spot welding method of high-strength steel sheet

    JP2005271033A

  • High intensity resistance-welding joint and manufacturing method thereof

    JP2014180698A

  • Process for manufacturing steel sheet having very high strength, ductility and toughness characteristics, and sheet thus produced

    WO2007101921A1

  • Bainite-containing high-strength hot-rolled steel plate with excellent isotropic workability and process for producing same

    WO2012133636A1

  • High-strength cold-rolled steel sheet with excellent local formability, and manufacturing method therefor

    WO2012141265A1