Manufacturing method of copper foam

The production of ultra-thin foamed copper with balanced porosity and structural strength addresses the need for efficient heat dissipation in miniaturized electronic components by applying copper paste to a release film, drying, peeling, and sintering processes.

JP7559092B2Active Publication Date: 2024-10-01AAC TECHNOLOGIES (NANJING) CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022577436
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-06-30
Filing Date
2022-07-20
Publication Date
2024-10-01
Estimated Expiration
2042-07-20

AI Technical Summary

Technical Problem

The challenge is to produce ultra-thin foamed copper with high water absorption performance to meet the demands of miniaturized electronic components that require efficient heat dissipation.

Method used

A method involving the application of copper paste to a release film, followed by drying, peeling off the film to form a preform, discharging adhesive, and sintering, resulting in foamed copper with a thickness of 30 to 120 μm and porosity of 50 to 80%, balancing porosity and structural strength for enhanced heat dissipation.

Benefits of technology

The method achieves reduced thickness and improved heat dissipation performance of foamed copper by ensuring a balance between porosity and structural strength, enhancing its water absorption capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559092000001
    Figure 0007559092000001
Patent Text Reader

Abstract

The present invention provides a method for producing foamed copper. [Solution] The method for producing foamed copper is to apply a copper paste to a release film to form a coating sheet having a thickness of 50 to 200 μm on the release film, then dry the release film on which the coating sheet is formed, and peel off the release film to obtain a foamed copper preform, then discharge an adhesive onto the foamed copper preform, and sinter it to obtain a foamed copper having a thickness of 30 to 120 μm and a porosity of 50 to 80%. In this way, the thickness of the foamed copper is reduced and a balance between the porosity and structural strength of the foamed copper is ensured, so that the foamed copper has good water absorption performance and effectively improves the heat dissipation performance of the foamed copper.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a heat dissipation material, and more particularly to a method for producing copper foam. [Background technology]

[0002] Due to the frequent use and rapid development of electronic components and integrated circuit technology, a large amount of heat is generated during the operation of electronic components. For example, the heat flow density of a computer CPU during operation is 60~100W / cm 2 The heat dissipation has become an important issue in the miniaturization of electronic products, because high heat flow greatly threatens the reliability of the normal operation of electronic components. In order to ensure that electronic components can operate normally, a heat sink is generally added to the electronic components to dissipate heat, and a temperature-equalizing plate with good thermal conductivity is added between the heat sink and the electronic components, so that the heat of the electronic components is evenly distributed and then dissipated through the heat sink.

[0003] The isothermal plate is a heat transfer assembly that realizes rapid heat transfer by relying on the phase change of the working fluid inside it, and mainly includes upper and lower cover plates or metal tubes, a seal head, an absorbent wick, and a heat transfer working medium. Here, the capillary structure of the absorbent wick directly affects the performance of the isothermal plate. The capillary structure is required to have strong capillary force and small water flow resistance. In the prior art, there are many types of absorbent wicks with capillary structures, such as foamed copper, copper mesh, composite copper mesh, and etched capillary structure.

[0004] With the continuous development of miniaturization of electronic products, the size of other electronic components is getting smaller and smaller, and they are required to be thinner and thinner, so the thickness of the temperature equalizing plate is more stringent. For example, ultra-thin temperature equalizing plates with a thickness of 280 μm or less (e.g., 240 μm) are born. While the ultra-thin temperature equalizing plate guarantees the heat transfer performance, thinner liquid absorbing cores are required, and for example, the production of liquid absorbing cores with a thickness of 80 μm or even 50 μm is planned.

[0005] Therefore, in order to solve the above problems, it is necessary to provide a method for manufacturing ultra-thin copper foam. Summary of the Invention [Problem to be solved by the invention]

[0006] SUMMARY OF THE DISCLOSURE Based on the above problems, the present invention provides a method for producing ultra-thin copper foam, which has a small thickness and high water absorption performance. [Means for solving the problem]

[0007] In order to achieve the above object, the present invention provides a method for producing foamed copper, the method comprising the steps of: applying a copper paste to a release film to form a coating sheet on the release film; a step of drying the release film on which the coating sheet is formed, and then peeling off the release film to obtain a foamed copper preform; and then discharging adhesive from the foamed copper preform and sintering the same to obtain foamed copper. The coating sheet has a thickness of 50 to 200 μm, and the foamed copper has a thickness of 30 to 120 μm and a porosity of 50 to 80%.

[0008] Preferably, the copper paste has a viscosity of 10,000 to 35,000 cps, and contains copper powder, an adhesive, a pore-forming agent, a solvent, a thickener, a dispersant, a leveling agent, and an antioxidant.

[0009] Preferably, the copper powder has an average particle size of 0.5 to 10 μm and a median diameter of 3 μm.

[0010] Preferably, the sintering is performed at a sintering temperature of 650 to 1050° C. for a sintering time of 0.5 to 24 hours in an ammonia gas atmosphere.

[0011] Preferably, the adhesive discharge temperature during the adhesive discharge is 350 to 450° C., and the adhesive discharge atmosphere is nitrogen gas.

[0012] Preferably, the release film is one selected from PET, PE and OPP, and the thickness of the release film is 75 to 120 μm.

[0013] Preferably, the adhesive contains one or more of PVA, epoxy resin, acrylic resin, phenolic resin, modified phenolic resin, hydroxymethyl cellulose, and ethyl cellulose, and the copper paste contains 0.1 to 30 wt % of the adhesive; The pore-forming agent includes one or more of ammonium chloride, urea, ammonium sulfate, citric acid, and benzoic acid, and the copper paste includes 5 to 50 wt % of the pore-forming agent.

[0014] Preferably, the solvent includes one or more of ethanol, propanol, isopropanol, acetone, toluene, xylene, terpineol, triethanolamine, isophorone, diacid ester, and water, and the copper paste includes 1 to 70 wt % of the solvent; The thickener includes one or more of natural rubber, styrene-butadiene rubber, chloroprene rubber, C5 petroleum resin, and C9 petroleum resin, and the copper paste includes 0.01 to 5 wt % of the thickener.

[0015] Preferably, the dispersant includes one or more of methylpentanol, a cellulose derivative, a polyacrylamide, and a fatty acid polyethylene glycol, and the copper paste includes 0.01 to 5 wt % of the dispersant.

[0016] Preferably, the leveling agent includes one or more of sodium dodecyl sulfate, sodium dodecylbenzenesulfonate, sodium tetradecylsulfonate, sodium cetylsulfonate, lecithin, triethanolamine, KH550, polyethylene glycol, and triethanolamine, and the copper paste includes 0.01 to 10 wt % of the leveling agent, The antioxidant includes one or more of citric acid, phytic acid, vitamins, oxalic acid, ascorbic acid, and glucose, and the copper paste includes 0.01 to 10 wt % of the antioxidant. Effect of the Invention

[0017] Compared with the related art, the manufacturing method of the foamed copper according to the present invention forms a coating sheet having a thickness of 50 to 200 μm on the release film by coating a copper paste on the release film, and then dries the release film on which the coating sheet is formed, and then peels off the release film to obtain a foamed copper preform. The foamed copper preform is then sequentially discharged with adhesive and sintered to obtain a foamed copper having a thickness of 30 to 120 μm and a porosity of 50 to 80%, thereby reducing the thickness of the foamed copper and ensuring a balance between the porosity and structural strength of the foamed copper, thereby having good water absorption performance and effectively improving the heat dissipation performance of the foamed copper. [Brief description of the drawings]

[0018] [Figure 1] 1 is a flowchart of a method for producing foamed copper in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The technical solutions of the present invention will be described clearly and completely below with reference to the drawings and specific embodiments.

[0020] As shown in FIG. 1, the present invention provides a method for producing foamed copper, which includes the following steps: Step 1: A copper paste is applied to a release film to form a coated sheet on the release film. Step 2: After the release film on which the coating sheet is formed is dried, the release film is peeled off to obtain a foamed copper preform. Step 3: The foamed copper preform is sequentially subjected to adhesive ejection and sintering, and then foamed copper is obtained.

[0021] In step 1, the copper paste includes copper powder, an adhesive, a pore-forming agent, a solvent, a thickener, a dispersant, a leveling agent, and an antioxidant.

[0022] The copper powder has an average particle size of 0.5 to 10 μm and a median diameter of 3 μm. Specifically, the copper powder having a wide distribution and fine particle size can be sufficiently contacted during the sintering process, and the produced foamed copper is guaranteed to have high structural strength even when it is thin.

[0023] The adhesive includes one or more of PVA, epoxy resin, acrylic resin, phenolic resin, modified phenolic resin, hydroxymethylcellulose, and ethylcellulose.

[0024] The pore-forming agent includes one or more of ammonium chloride, urea, ammonium sulfate, citric acid, and benzoic acid.

[0025] The solvent includes one or more of ethanol, propanol, isopropanol, acetone, toluene, xylene, terpineol, triethanolamine, isophorone, diacid esters, and water.

[0026] The thickener includes one or more of natural rubber, styrene butadiene rubber, chloroprene rubber, C5 petroleum resin, and C9 petroleum resin.

[0027] The dispersant includes one or more of methylpentanol, cellulose derivatives, polyacrylamides, and fatty acid polyethylene glycols.

[0028] The leveling agent includes one or more of sodium dodecyl sulfate, sodium dodecylbenzenesulfonate, sodium tetradecylsulfonate, sodium cetylsulfonate, lecithin, triethanolamine, KH550, polyethylene glycol, and triethanolamine.

[0029] The antioxidants include one or more of citric acid, phytic acid, vitamins, oxalic acid, ascorbic acid, and glucose.

[0030] After the above raw materials are selected, the pore-forming agent is put into a ball mill and ball milled for 4 to 24 hours or crushed by a crusher to obtain the pore-forming agent with a particle size of 20 to 200 μm. Next, the copper powder and the sieved pore-forming agent are thoroughly mixed in a material mixer for 1 to 12 hours to obtain a mixed powder material. The selected solvent, adhesive, dispersant, leveling agent, thickener and antioxidant are added to the mixed powder material, and the mixed powder material is mixed at 0.5° C. in a material mixer. The mixture is stirred thoroughly for 1.5 to 12 hours to obtain the copper paste having a viscosity of 10,000 to 35,000 cps. Specifically, the copper paste contains a certain amount of the copper powder, 0.1 to 30 wt% of the adhesive, 5 to 50 wt% of the pore-forming agent, 1 to 70 wt% of the solvent, 0.01 to 5 wt% of the thickener, 0.01 to 5 wt% of the dispersant, 0.01 to 10 wt% of the leveling agent, and 0.01 to 10 wt% of the antioxidant.

[0031] After preparing the copper paste, the copper paste is applied to the release film by rubbing or screen printing to form a coating sheet having a thickness of 50 to 200 μm on the release film. Specifically, the release film is one selected from PET, PE, and OPP, and the thickness of the release film is 75 to 120 μm, thereby ensuring that the release film to which the coating sheet is applied does not soften or undergo serious deformation in the subsequent sintering process, and the thickness is preferably the upper limit value.

[0032] In step 2, the drying process is generally carried out in an oven, and a programmable temperature rise and fall control is adopted in the drying process to ensure that the coating sheet on the release film does not crack during the drying process and the subsequent peeling process, thereby obtaining a complete foamed copper preform. Specifically, the drying process is generally carried out in a tunnel furnace or oven.

[0033] In step 3, the adhesive discharge temperature is 350 to 450°C, the adhesive discharge atmosphere is nitrogen gas, and in the adhesive discharge process, the adhesive and the pore-forming agent can volatilize, and in order to ensure the uniformity of the manufactured foamed copper structure, it is necessary to control the temperature in the adhesive discharge process to the same temperature range. In addition, since a certain amount of gas is generated in the adhesive discharge process, air needs to flow on both the top and bottom surfaces so that the uniformity of the top and bottom surfaces of the manufactured foamed copper is guaranteed. Therefore, in the adhesive discharge process, it is necessary to place the foamed copper preform on ceramic or quartz glass having a porous structure and discharge the adhesive, and it is also possible to avoid adhesion between the foamed copper preform and the porous ceramic or quartz glass that is the support plate. In addition, since a large amount of exhaust gas is generated in the adhesive discharge process, it is necessary to provide an exhaust gas absorption device in the device for discharging the adhesive. In general, the adhesive discharge process is generally performed in a sintering furnace.

[0034] The foamed copper preform is sintered after the adhesive is discharged, and the sintering temperature is 650 to 1050°C, the sintering time is 0.5 to 24 hours, and the sintering atmosphere is ammonia gas. Specifically, the sintering temperature is preferably 700 to 900°C, the sintering time is preferably 2 to 12 hours, and after the adhesive is discharged and sintered, the foamed copper preform produces a foamed copper having a thickness of 30 to 120 μm and a porosity of 50 to 80%.

[0035] As will be appreciated, the sintering temperature and sintering time may be adjusted to control the balance between porosity and structural strength of the produced copper foam.

[0036] The method for producing copper foam according to the present invention will be described in more detail below with reference to several examples.

[0037] Example 1 A copper powder having an average particle size of 10 μm and ammonium chloride particles having a particle size of 70-100 μm obtained by sieving after ball milling or pulverization are mixed in a mass ratio of 3:1 to obtain a mixed powder, and a xylene solution having a concentration of 25% is added to the mixed powder, and then mixed, and 0.5% of a thickener, 0.5% of a dispersant, 1% of an antioxidant, and a certain amount of a leveling agent are added in sequence, and the mixture is stirred for 0.5-6 hours to obtain a copper paste. The copper paste is applied to a PET release film having a thickness of 150 μm to form a coated sheet, and then placed in an oven at 90-110 ° C to dry for 20 minutes, and the PET release film is peeled off to obtain a foamed copper preform. The foamed copper preform obtained is placed in a sintering furnace, and N2 is first introduced, and adhesive is discharged at 400 ° C for 90 minutes, and then ammonia gas is introduced, and sintered at 700-850 ° C for 120 minutes, and finally a foamed copper having a thickness of 90 ± 10 μm and a porous capillary structure is obtained.

[0038] Example 2 Copper powder with an average particle size of 1 μm and ammonium chloride particles with a particle size of 70 to 100 μm obtained by sieving after ball milling or pulverization are mixed in a mass ratio of 3:1 to obtain a mixed powder material, which is then added to a xylene solution with a concentration of 25% and mixed, and 0.5% thickener, 0.5% dispersant, 1% antioxidant and a certain amount of leveling agent are added in sequence, and the mixture is stirred for 0.5 to 6 hours to obtain a copper paste. The copper paste is applied to a PET release film with a thickness of 120 μm to form a coated sheet, which is then placed in an oven at 90 to 110°C and dried for 30 minutes. The PET release film is then peeled off to obtain a foamed copper preform. The resulting foamed copper preform is placed in a sintering furnace, where N2 is first introduced and the adhesive is discharged at 400°C for 120 minutes. Ammonia gas is then introduced and sintered at 700 to 850°C for 90 minutes. Finally, a foamed copper having a porous capillary structure and a thickness of 75±10 μm is obtained.

[0039] Example 3 A copper powder having an average particle size of 10 μm and ammonium chloride particles having a particle size of 70-100 μm obtained by sieving after ball milling or pulverization are mixed in a mass ratio of 2:1 to obtain a mixed powder, and a xylene solution having a concentration of 25% is added to the mixed powder, and then mixed, and 0.5% of a thickener, 0.5% of a dispersant, 1% of an antioxidant, and a certain amount of a leveling agent are added in sequence, and the mixture is stirred for 0.5-6 hours to obtain a copper paste. The copper paste is applied to a PET release film having a thickness of 100 μm to form a coated sheet, and then placed in an oven at 90-110 ° C to dry for 20 minutes, and the PET release film is peeled off to obtain a foamed copper preform. The foamed copper preform obtained is placed in a sintering furnace, and N2 is first introduced, and adhesive is discharged at 400 ° C for 90 minutes, and then ammonia gas is introduced, and sintered at 700-850 ° C for 120 minutes, and finally a foamed copper having a thickness of 70 ± 10 μm and a porous capillary structure is obtained.

[0040] Example 4 A copper powder having an average particle size of 1 μm and ammonium chloride particles having a particle size of 70-100 μm obtained by sieving after ball milling or pulverization are mixed in a mass ratio of 2:1 to obtain a mixed powder, and a xylene solution having a concentration of 25% is added to the mixed powder, and then mixed, and 0.5% of a thickener, 0.5% of a dispersant, 1% of an antioxidant, and a certain amount of a leveling agent are added in sequence, and the mixture is stirred for 0.5-6 hours to obtain a copper paste. The copper paste is applied to a PET release film having a thickness of 80 μm to form a coated sheet, and then the sheet is placed in an oven at 90-110 ° C to dry for 20 minutes, and the PET release film is peeled off to obtain a foamed copper preform. The foamed copper preform obtained is placed in a sintering furnace, and N2 is first introduced, and adhesive is discharged at 400 ° C for 90 minutes, and then ammonia gas is introduced, and the mixture is sintered at 700-850 ° C for 120 minutes, and finally a foamed copper having a thickness of 50 ± 8 μm and a porous capillary structure is obtained.

[0041] Example 5 A copper powder having an average particle size of 10 μm and ammonium chloride particles having a particle size of 70-100 μm obtained by sieving after ball milling or pulverization are mixed in a mass ratio of 1:1 to obtain a mixed powder, and a xylene solution having a concentration of 25% is added to the mixed powder, and then mixed, and 0.5% of a thickener, 0.5% of a dispersant, 1% of an antioxidant, and a certain amount of a leveling agent are added in sequence, and the mixture is stirred for 0.5-6 hours to obtain a copper paste. The copper paste is applied to a PET release film having a thickness of 70 μm to form a coated sheet, and then the sheet is placed in an oven at 90-110 ° C to dry for 20 minutes, and the PET release film is peeled off to obtain a foamed copper preform. The foamed copper preform is placed in a sintering furnace, and N2 is first introduced, and adhesive is discharged at 450 ° C for 90 minutes, and then ammonia gas is introduced, and the mixture is sintered at 700-850 ° C for 120 minutes, and finally a foamed copper having a thickness of 45 ± 5 μm and a porous capillary structure is obtained.

[0042] Example 6 A copper powder having an average particle size of 1 μm and ammonium chloride particles having a particle size of 70-100 μm obtained by sieving after ball milling or pulverization are mixed in a mass ratio of 1:1 to obtain a mixed powder, and a xylene solution having a concentration of 25% is added to the mixed powder, and then mixed, and 0.5% of a thickener, 0.5% of a dispersant, 1% of an antioxidant, and a certain amount of a leveling agent are added in sequence, and the mixture is stirred for 0.5-6 hours to obtain a copper paste. The copper paste is applied to a PET release film having a thickness of 60 μm to form a coated sheet, and then placed in an oven at 90-110 ° C to dry for 20 minutes, and the PET release film is peeled off to obtain a foamed copper preform. The foamed copper preform obtained is placed in a sintering furnace, and N2 is first introduced, and adhesive is discharged at 450 ° C for 90 minutes, and then ammonia gas is introduced, and sintered at 700-850 ° C for 120 minutes, and finally a foamed copper having a thickness of 40 ± 5 μm and a porous capillary structure is obtained.

[0043] Example 7 A copper powder having an average particle size of 1 μm and ammonium chloride particles having a particle size of 70-100 μm obtained by sieving after ball milling or pulverization are mixed in a mass ratio of 3:1 to obtain a mixed powder, and a xylene solution having a concentration of 20% is added to the mixed powder, and then mixed, and 0.5% of a thickener, 0.5% of a dispersant, 1% of an antioxidant, and a certain amount of a leveling agent are added in sequence, and the mixture is stirred for 0.5-6 hours to obtain a copper paste. The copper paste is applied to a PET release film having a thickness of 50 μm to form a coated sheet, and then placed in an oven at 90-110 ° C to dry for 30 minutes, and the PET release film is peeled off to obtain a foamed copper preform. The foamed copper preform obtained is placed in a sintering furnace, and N2 is first introduced, and adhesive is discharged at 400 ° C for 90 minutes, and then ammonia gas is introduced, and sintered at 700-850 ° C for 120 minutes, and finally a foamed copper having a thickness of 30 ± 8 μm and a porous capillary structure is obtained.

[0044] Example 8 Copper powder with an average particle size of 1 μm and ammonium chloride particles with a particle size of 70 to 100 μm obtained by sieving after ball milling or pulverization are mixed in a mass ratio of 5:2 to obtain a mixed powder, and a xylene solution with a concentration of 20% is added to the mixed powder and mixed. Then, 0.5% thickener, 0.5% dispersant, 1% antioxidant and a certain amount of leveling agent are added in order, and the mixture is stirred for 0.5 to 6 hours to obtain a copper paste. The copper paste is applied to a PET release film with a thickness of 50 μm to form a coated sheet, which is then placed in an oven at 90 to 110°C and dried for 30 minutes. The PET release film is then peeled off to obtain a foamed copper preform. The foamed copper preform is then placed in a rubber discharge furnace, where N2 is first introduced and the adhesive is discharged at 400°C for 90 minutes. The foamed copper preform is then placed in a sintering furnace, where ammonia gas is introduced and sintered at 850 to 900°C for 120 minutes. Finally, a foamed copper having a porous capillary structure and a thickness of 30±5 μm is obtained.

[0045] Example 9 Copper powder with an average particle size of 1 μm and ammonium chloride particles with a particle size of 70 to 100 μm obtained by sieving after ball milling or pulverization are mixed in a mass ratio of 2:1 to obtain a mixed powder, and a xylene solution with a concentration of 20% is added to the mixed powder and mixed. Then, 0.5% thickener, 0.5% dispersant, 1% antioxidant and a certain amount of leveling agent are added in order, and the mixture is stirred for 0.5 to 6 hours to obtain a copper paste. The copper paste is applied to a PET release film with a thickness of 60 μm to form a coated sheet, which is then placed in an oven at 90 to 110°C and dried for 30 minutes. The PET release film is then peeled off to obtain a foamed copper preform. The foamed copper preform is then placed in a rubber discharge furnace, where N2 is first introduced and the adhesive is discharged at 450°C for 90 minutes. The foamed copper preform is then placed in a sintering furnace, where ammonia gas is introduced and sintered at 850 to 900°C for 120 minutes. Finally, a foamed copper having a porous capillary structure and a thickness of 40±5 μm is obtained.

[0046] Example 10 Copper powder with an average particle size of 1 μm and ammonium chloride particles with a particle size of 70 to 100 μm obtained by sieving after ball milling or pulverization are mixed in a mass ratio of 2.5:1 to obtain a mixed powder, a xylene solution with a concentration of 20% is added to the mixed powder, and then mixed. 0.5% thickener, 0.5% dispersant, 1% antioxidant and a certain amount of leveling agent are added in order, and the mixture is stirred for 0.5 to 6 hours to obtain a copper paste. The copper paste is applied to a PET release film with a thickness of 60 μm to form a coated sheet, which is then placed in an oven at 90 to 110°C and dried for 30 minutes. The PET release film is then peeled off to obtain a foamed copper preform. The foamed copper preform is then placed in a rubber discharge furnace, where N2 is first introduced and the adhesive is discharged at 450°C for 90 minutes. It is then placed in a sintering furnace, where ammonia gas is introduced and sintered at 850 to 900°C for 120 minutes. Finally, a foamed copper having a porous capillary structure and a thickness of 45±5 μm is obtained.

[0047] Compared with the related art, the manufacturing method of the foamed copper according to the present invention involves applying a copper paste to a release film to form a coating sheet having a thickness of 50 to 200 μm on the release film, drying the release film on which the coating sheet is formed, and then peeling off the release film to obtain a foamed copper preform. The foamed copper preform is then sequentially discharged with adhesive and sintered to obtain a foamed copper having a thickness of 30 to 120 μm and a porosity of 50 to 80%, thereby reducing the thickness of the foamed copper and ensuring a balance between the porosity and structural strength of the foamed copper, thereby having good water absorption performance and effectively improving the heat dissipation performance of the foamed copper.

[0048] The above is merely an embodiment of the present invention, and those skilled in the art may make modifications without departing from the spirit of the present invention, all of which are within the scope of protection of the present invention.

Claims

1. A method for producing foamed copper, comprising: applying a copper paste to a release film to form a coating sheet on the release film; a step of drying the release film on which the coating sheet is formed, and then peeling off the release film to obtain a foamed copper preform; and then discharging adhesive from the foamed copper preform and sintering the same to obtain foamed copper. The thickness of the coating sheet is 50 to 200 μm, the foamed copper has a thickness of 30 to 120 μm and a porosity of 50 to 80%, The sintering temperature of the sintering is 650 to 1050°C, the adhesive discharge temperature of the adhesive discharge is 350 to 450°C, and the adhesive discharge atmosphere is nitrogen gas; The method for producing foamed copper, wherein the release film is one selected from PE and OPP, and the thickness of the release film is 75 to 120 μm.

2. 2. The method for producing copper foam according to claim 1, wherein the viscosity of the copper paste is 10,000 to 35,000 cps, and the copper paste includes copper powder, an adhesive, a pore former, a solvent, a thickener, a dispersant, a leveling agent, and an antioxidant.

3. The method for producing copper foam according to claim 2, wherein the copper powder has an average particle size of 0.5 to 10 μm and a median diameter of 3 μm.

4. 2. The method for producing copper foam according to claim 1, wherein the sintering is performed for a period of 0.5 to 24 hours in an ammonia gas atmosphere.

5. The adhesive includes one or more of PVA, epoxy resin, acrylic resin, phenolic resin, modified phenolic resin, hydroxymethyl cellulose, and ethyl cellulose, and the copper paste includes 0.1 to 30 wt % of the adhesive; 3. The method for producing copper foam according to claim 2, wherein the pore-forming agent includes one or more of ammonium chloride, urea, ammonium sulfate, citric acid, and benzoic acid, and the copper paste includes 5 to 50 wt % of the pore-forming agent.

6. The solvent includes one or more of ethanol, propanol, isopropanol, acetone, toluene, xylene, terpineol, triethanolamine, isophorone, diacid ester, and water, and the copper paste includes 1 to 70 wt % of the solvent; The method for producing copper foam according to claim 2, characterized in that the thickener includes one or more of natural rubber, styrene-butadiene rubber, chloroprene rubber, C5 petroleum resin, and C9 petroleum resin, and the copper paste includes 0.01 to 5 wt % of the thickener.

7. 3. The method for producing copper foam according to claim 2, characterized in that the dispersant includes one or more of methylpentanol, cellulose derivatives, polyacrylamide, and fatty acid polyethylene glycol, and the copper paste includes 0.01 to 5 wt % of the dispersant.

8. The leveling agent includes one or more of sodium dodecyl sulfate, sodium dodecylbenzenesulfonate, sodium tetradecylsulfonate, sodium cetylsulfonate, lecithin, triethanolamine, KH550, polyethylene glycol, and triethanolamine, and the copper paste includes 0.01 to 10 wt % of the leveling agent; The method for producing copper foam according to claim 2, characterized in that the antioxidant includes one or more of citric acid, phytic acid, vitamins, oxalic acid, ascorbic acid, and glucose, and the copper paste includes 0.01 to 10 wt % of the antioxidant.

Citation Information

Patent Citations

  • Preparation method for foamy copper

    CN103526064A

  • Foam copper powder and preparation method thereof

    CN106180745A

  • Foaming body material, vibrating plate and loudspeaker

    CN110677783A

  • Capillary structure of heat dissipation element, heat dissipation element and preparation method of capillary structure

    CN114543570A

  • Method and apparatus for making sintered porous metal plate

    EP0765704A2