A novel battery system based on a dual-additive electrolyte system containing 1,2,6-oxodithiane-2,2,6,6-tetraoxide
A dual-additive electrolyte system with VC and ODTO, or FEC and ODTO, combined with NMC and graphite electrodes, addresses the challenge of synergistic interactions in lithium-ion batteries, enhancing performance and longevity for rapid charging and discharging applications.
Patent Information
- Application Number
- JP2023043694
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-08-07
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2038-08-31
AI Technical Summary
Existing rechargeable lithium-ion battery systems face challenges in achieving synergistic interactions between electrolyte additives and electrodes, leading to suboptimal performance and longevity, particularly in applications requiring rapid charging and discharging, and there is a need for simpler yet effective electrolyte systems that can be predictably formulated.
A dual-additive electrolyte system comprising vinylene carbonate (VC) combined with 1,2,6-oxodithian-2,2,6,6-tetraoxide (ODTO), or fluoroethylene carbonate (FEC) combined with ODTO, along with a lithium nickel manganese cobalt oxide (NMC) positive electrode and a graphite negative electrode, enhances battery performance and reduces costs.
The dual-additive electrolyte system improves cycle life and reduces gas production, maintaining high energy efficiency and capacity retention, making it suitable for grid and automotive applications.
Smart Images

Figure 0007559122000005 
Figure 0007559122000006 
Figure 0007559122000007
Abstract
Description
[Technical field]
[0001] The present disclosure relates to rechargeable battery systems, and more particularly to the chemistry of such systems, including working electrolyte additives and electrodes, for improving the performance of rechargeable lithium-ion battery systems. [Background technology]
[0002] Rechargeable batteries are essential components in energy storage systems for electric vehicles and grid storage (e.g., for backup power during power outages, as part of a microgrid, etc.). Depending on the application, different properties are required for the energy storage system. Trade-offs in the battery system chemistry may need to be made to create a system suitable for a particular application. For example, in automotive applications, and especially electric vehicle applications, the ability to charge and discharge quickly is a key property of the system. Electric vehicle owners may need to accelerate quickly in traffic, which requires the ability to discharge the system quickly. Furthermore, because rapid charging and discharging places demands on the system, the system's components may also need to be selected to provide sufficient lifetime under such operating conditions.
[0003] Electrolyte additives are operative and have been shown to improve the life and performance of lithium-ion based batteries. For example, in Non-Patent Document 1, five unique and undisclosed electrolyte additives were shown to extend cycle life compared to electrolyte systems containing no or only one additive. Other studies have focused on improving the performance of electrolyte systems containing three or four additives, as described in Patent Document 1. However, researchers usually do not understand the interactions between different additives that allow the electrolyte and a particular positive and negative electrode to work together synergistically. Therefore, the composition of the additive blend for a particular system is often based on trial and error and cannot be predicted in advance.
[0004] Previous studies have not identified a two-additive electrolyte system that can be combined with a lithium-ion battery system to produce a robust system with sufficient properties for grid or automotive applications. As discussed in U.S. Patent No. 5,399,636, the two-additive systems studied (e.g., 2% VC+1% allyl methanesulfonate and 2% PES+1% TTSPi) typically performed less well than three- and four-additive electrolyte systems. (See, e.g., Tables 1 and 2 of U.S. Patent No. 5,399,636.) U.S. Patent No. 5,399,636 discloses that a third compound, often tris(-trimethyl-silyl)-phosphate (TTSP) or tris(-trimethyl-silyl)-phosphite (TTSPi), at a concentration of 0.25% to 3% by weight was required to produce a robust lithium-ion battery system. (See, e.g., paragraph 72 of U.S. Patent No. 5,399,636.) However, because of the potentially expensive and difficult to include additives in Li-ion batteries at a manufacturing scale, there is a need for simpler, yet effective electrolytes, including those with fewer additives. Summary of the Invention [Means for solving the problem]
[0005] This disclosure encompasses novel battery systems with fewer working electrolyte additives that can be used in a variety of energy storage applications, such as vehicle and grid storage. More specifically, this disclosure includes a dual-additive electrolyte system that improves the performance and life of Li-ion batteries while simultaneously reducing the cost of other systems that rely on more additives. This disclosure also describes effective cathode and anode additives that work in conjunction with the disclosed dual-additive electrolyte system to provide further systemic improvements. and a negative electrode.
[0006] A working additive electrolyte system is disclosed that includes vinylene carbonate (VC) in combination with 1,2,6-oxodithiane-2,2,6,6-tetraoxide (ODTO), where ODTO has the following formula (I): TIFF0007559122000001.tif44111
[0007] Also disclosed are fluoroethylene carbonate (FEC) in combination with ODTO and LiPO2F2 (herein referred to as LFO) in combination with ODTO. Systems including VC, LFO and at least two combinations of VC and ODTO are also disclosed.
[0008] Since VC and FEC provide similar improvements (and are believed to function similarly), a mixture of VC and FEC can be considered a single effective electrolyte. That is, another disclosed dual-acting additive electrolyte system includes a mixture of VC and FEC in combination with ODTO. When used as part of a larger battery system (including electrolyte, electrolyte solvent, cathode and anode), these dual-acting additive electrolyte systems produce desirable properties for energy storage applications, including vehicle and grid applications. In addition, LFO effectively acts as a primary additive and can be combined with FEC and / or VC to create an additive system that can be further improved by LFO.
[0009] More specifically, a lithium nickel manganese cobalt oxide (NMC) cathode, a graphite anode, a lithium salt dissolved in an organic or non-aqueous solvent that may include methyl acetate (MA), and two additives can form a battery system with desirable properties for various applications. The electrolyte solvent can be any of the following solvents, alone or in combination: ethylene carbonate (EC), ethyl methyl carbonate (EMC), methyl acetate, propylene carbonate, dimethyl carbonate, diethyl carbonate, another carbonate solvent (cyclic or non-cyclic), another organic solvent, and / or another non-aqueous solvent. The solvent is present at a higher concentration than the additive, typically greater than 6% by weight. The solvent can be combined with the disclosed two-additive pairs (such as VC and ODTO, FEC and ODTO, LFO and ODTO, a mixture of VC and FEC and ODTO, or another combination) to form a battery system with desirable properties for various applications. The positive electrode may be coated with a material such as aluminum oxide (Al2O3), titanium dioxide (TiO2), or another coating material. Additionally, to save cost, the negative electrode may be formed from natural graphite, although depending on pricing structures, synthetic graphite may be cheaper than natural graphite in certain instances.
[0010] The disclosure herein is supported by experimental data showing the symbiotic nature of the two-additive electrolyte system and selected electrodes. An exemplary battery system includes two additives (e.g., FEC, LFO or VC, ODTO), a graphite anode (either naturally occurring graphite or man-made synthetic graphite), an NMC cathode, a lithium electrolyte (e.g., formed from a lithium salt such as lithium hexafluorophosphate having the chemical composition LiPF6), and an organic or non-aqueous solvent. In a further embodiment, the first additive is a combination of at least two of VC, LFO, and FEC.
[0011] An exemplary embodiment of the present application is a method for preparing a lithium salt, a non-aqueous solvent, a first working additive selected from vinylene carbonate, LiPO2F2 (LFO), fluoroethylene carbonate, or any combination thereof, and a compound represented by the following formula (I): and a mixture including a second working type additive of 1,2,6-oxodithiane-2,2,6,6-tetraoxide having TIFF0007559122000002.tif44111.
[0012] In another exemplary embodiment, the concentration of the first actuating additive ranges from 0.25% to 6% by weight.
[0013] In another exemplary embodiment, the concentration of the second actuating additive ranges from 0.25% to 5% by weight.
[0014] In another exemplary embodiment, the concentration of the first working type additive is 2 wt % (for VC or FEC) and 1 wt % (for LFO), and the concentration of the second working type additive is 1 wt %.
[0015] In another exemplary embodiment, the first working additive is fluoroethylene carbonate.
[0016] In another exemplary embodiment, the first working additive is vinylene carbonate.
[0017] In another exemplary embodiment, the first working additive is LiPO2F2.
[0018] In another exemplary embodiment, the non-aqueous solvent is a carbonate solvent.
[0019] In another exemplary embodiment, the non-aqueous solvent is at least one selected from ethylene carbonate and ethyl methyl carbonate.
[0020] In another exemplary embodiment, the electrolyte further comprises a second non-aqueous solvent.
[0021] Another exemplary embodiment of the present application is a battery comprising a negative electrode, a positive electrode, lithium ions dissolved in a first non-aqueous solvent, and a first working additive selected from fluoroethylene carbonate, LiPO2F2, and vinylene carbonate, or any combination thereof, and a lithium ion-containing electrolyte having the following formula (I): and a non-aqueous electrolyte comprising an additive mixture of 1,2,6-oxodithiane-2,2,6,6-tetraoxide having a second working type additive of TIFF0007559122000003.tif44111.
[0022] In another exemplary embodiment, the volume of gas produced in the lithium ion battery is comparable to the volume of gas produced in a lithium ion battery containing only the first working type additive.
[0023] In another exemplary embodiment, the lithium ion battery has 95% retention of initial capacity after 200 cycles between 3.0V and 4.3V at a charge rate of C / 3CCCV at 40°C.
[0024] In another exemplary embodiment, the lithium ion battery has 95% retention of initial capacity after 300 cycles between 3.0V and 4.3V at a charge rate of C / 3CCCV at 40°C.
[0025] In another exemplary embodiment, the lithium ion battery has 95% retention of initial capacity after 400 cycles between 3.0V and 4.3V at a charge rate of C / 3CCCV at 40°C.
[0026] In another exemplary embodiment, the lithium ion battery has 95% retention of initial capacity after 500 cycles between 3.0V and 4.3V at a charge rate of C / 3CCCV at 40°C.
[0027] In another exemplary embodiment, the lithium ion battery has 95% retention of initial capacity after 600 cycles between 3.0V and 4.3V at a charge rate of C / 3CCCV at 40°C.
[0028] In another exemplary embodiment, the lithium ion battery has 95% retention of initial capacity after 700 cycles between 3.0V and 4.3V at a charge rate of C / 3CCCV at 40°C.
[0029] In another exemplary embodiment, the lithium ion battery has 95% retention of initial capacity after 800 cycles from 3.0V to 4.3V at a charge rate of C / 3CCCV at 40°C.
[0030] In another exemplary embodiment, the lithium ion battery has 95% retention of initial capacity after 900 cycles from 3.0V to 4.3V at a charge rate of C / 3CCCV at 40°C.
[0031] Another exemplary embodiment of the present application is an electric vehicle equipped with a rechargeable battery, a traction motor, a gearbox, electronics, and the battery system described herein. [Brief description of the drawings]
[0032] [Figure 1] FIG. 1 is a schematic diagram of a vehicle equipped with a storage battery system.
[0033] [Diagram 2] FIG. 1 is a schematic diagram of an exemplary battery storage system.
[0034] [Diagram 3] FIG. 1 is a schematic diagram of a lithium ion battery cell system.
[0035] [Figure 4A-4B] 1 shows the passivation effect of various electrolyte compositions in different types of cells. [Fig. 4C-4D] 1 shows the passivation effect of various electrolyte compositions in different types of cells. [Figure 4E] 1 shows the passivation effect of various electrolyte compositions in different types of cells.
[0036] FIG. 4A illustrates the passivation effect by showing dQ / dV versus V during formation cycling of uncoated NMC532 / synthetic graphite cells containing electrolytes with ethylene carbonate (EC):ethyl methyl carbonate (EMC) (control) and EC:EMC with 2% VC, 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, and 1% LFO (LiPO2F2)+1% ODTO.
[0037] FIG. 4B illustrates the passivation effect by showing dQ / dV versus V during formation cycles for coated NMC532 / synthetic graphite cells containing electrolytes with ethylene carbonate (EC):ethyl methyl carbonate (EMC) (control) and EC:EMC with 2% VC, 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, and 1% LFO+1% ODTO.
[0038] FIG. 4C illustrates the passivation effect by showing dQ / dV versus V during formation cycles for Al2O3-coated NMC622 / synthetic graphite cells containing electrolytes with 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, and 2% VC.
[0039] FIG. 4D illustrates the passivation effect by showing dQ / dV vs. V during formation cycles for NMC622 / synthetic graphite cells coated with aluminum, fluorine and oxygen (AFO) polycrystalline coating material containing electrolytes with ethylene carbonate (EC):ethyl methyl carbonate (EMC) (control) and EC:EMC with 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, and 2% VC.
[0040] FIG. 4E illustrates the passivation effect by showing dQ / dV versus V during formation cycling of lithium-ion battery cells containing electrolytes with 2% VC, 2% VC+1% ODTO, and 2% VC+3% ODTO.
[0041] [Figure 5A-5B] Electrochemical Impedance Spectroscopy (EIS) spectra of different types of cells with various electrolyte compositions. [Fig. 5C-5D] Electrochemical Impedance Spectroscopy (EIS) spectra of different types of cells with various electrolyte compositions. [Figure 5E] Electrochemical Impedance Spectroscopy (EIS) spectra of different types of cells with various electrolyte compositions.
[0042] FIG. 5A shows EIS spectra of different electrolyte systems including 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, 2% FEC, and 1% LFO in a cell with an uncoated NMC532 cathode and a synthetic graphite anode.
[0043] FIG. 5B shows EIS spectra of different electrolyte systems including 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 1% LFO+1% ODTO+1% VC, 1% LFO+1% ODTO+1% FEC, 1% LFO+1% ODTO+1% TTSPi, 2% VC, 2% FEC, and 1% LFO in a cell with a coated NMC532 cathode and a synthetic graphite anode.
[0044] FIG. 5C shows EIS spectra of different electrolyte systems including 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, and 2% FEC in a cell with an Al2O3-coated NMC622 cathode and a synthetic graphite anode.
[0045] FIG. 5D shows EIS spectra of different electrolyte systems including 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, and 2% FEC in a cell with an AFO-coated NMC622 cathode and a synthetic graphite anode.
[0046] FIG. 5E shows the EIS spectra of different electrolyte systems including 2% VC, 2% VC+1% ODTO, and 2% FEC+3% ODTO in a lithium-ion battery cell.
[0047] [Figure 6A] 1 illustrates the charge transfer resistance (Rct) of different types of cells with various electrolyte compositions measured after formation cycling. [Figure 6B] 1 illustrates the charge transfer resistance (Rct) of different types of cells with various electrolyte compositions measured after formation cycling. [Figure 6C] 1 illustrates the charge transfer resistance (Rct) of different types of cells with various electrolyte compositions measured after formation cycling. [Figure 6D] 1 illustrates the charge transfer resistance (Rct) of different types of cells with various electrolyte compositions measured after formation cycling. [Figure 6E] 1 illustrates the charge transfer resistance (Rct) of different types of cells with various electrolyte compositions measured after formation cycling.
[0048] FIG. 6A shows the R of different electrolyte systems containing 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, 2% FEC, and 1% LFO in a cell with an uncoated NMC532 cathode and a synthetic graphite anode. ct is illustrated.
[0049] FIG. 6B shows the R of different electrolyte systems containing 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, 2% FEC, and 1% LFO in a cell with a coated NMC532 cathode and a synthetic graphite anode. ct is illustrated.
[0050] FIG. 6C shows the R of different electrolyte systems including 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, and 2% FEC in a cell with an Al2O3-coated NMC622 cathode and an artificial graphite anode. ct is illustrated.
[0051] FIG. 6D shows the R of different electrolyte systems including 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, and 2% FEC in cells with coated NMC622 positive and synthetic graphite negative electrodes. ct is illustrated.
[0052] FIG. 6E shows the R of different electrolyte systems containing 2% VC, 2% VC+1% ODTO, and 2% VC+3% ODTO in a lithium-ion battery cell with a coated NMC622 cathode and an artificial graphite anode. ct is illustrated.
[0053] [Figure 7A] The experimental data of the volume of formation gas produced during cell formation for different electrolyte systems is summarized. [Figure 7B]The experimental data of the volume of formation gas produced during cell formation for different electrolyte systems is summarized. [Figure 7C] The experimental data of the volume of formation gas produced during cell formation for different electrolyte systems is summarized. [Figure 7D] The experimental data of the volume of formation gas produced during cell formation for different electrolyte systems is summarized. [Figure 7E] The experimental data of the volume of formation gas produced during cell formation for different electrolyte systems is summarized.
[0054] FIG. 7A is a plot summarizing experimental data of the volume of formation gas produced during cell formation for electrolyte systems containing 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, 2% FEC, and 1% LFO in cells with uncoated NMC532 positive electrodes and synthetic graphite negative electrodes.
[0055] FIG. 7B is a plot summarizing experimental data of the volume of formation gas produced during cell formation for electrolyte systems containing 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, 2% FEC, and 1% LFO in cells with coated NMC532 positive electrodes and synthetic graphite negative electrodes.
[0056] FIG. 7C is a plot summarizing experimental data of the volume of formation gas produced during cell formation for electrolyte systems containing 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, and 2% FEC in cells with an Al2O3-coated NMC622 cathode and a synthetic graphite anode.
[0057] FIG. 7D is a plot summarizing experimental data of the volume of formation gas produced during cell formation for electrolyte systems containing 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, and 2% FEC in cells with AFO-coated NMC622 cathodes and synthetic graphite anodes.
[0058] FIG. 7E is a plot summarizing experimental data of the volume of formation gas produced during cell formation for electrolyte systems containing 2% VC, 2% VC+1% ODTO, and 2% VC+3% ODTO in a lithium-ion battery cell.
[0059] [Figure 8A-8B] 1 illustrates voltage versus time during high temperature storage for different NMC622 / synthetic graphite cells with various electrolyte systems.
[0060] FIG. 8A illustrates voltage versus time during high temperature storage for different electrolyte systems including 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, and 1% LFO+1% ODTO in a cell with an Al2O3 coated NMC622 positive electrode and a synthetic graphite negative electrode.
[0061] FIG. 8B illustrates voltage versus time during high temperature storage for different electrolyte systems including 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, and 1% LFO+1% ODTO in a cell with a coated NMC622 positive electrode and a synthetic graphite negative electrode.
[0062] [Figure 9] FIG. 9 illustrates the parasitic heat flow in experiments involving various electrolyte additive systems in a lithium-ion battery cell.
[0063] [Figure 10A]Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10B] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10C] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10D] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10E] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10F] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10G] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10H]Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10I] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10J] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10K] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Fig. 10L-10M] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10N] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10O] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10P]Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10Q] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10R] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10S] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10T] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10U] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10V] Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown. [Figure 10W]Experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments for various electrolyte systems are shown.
[0064] 10A-10I show the normalized discharge capacity (DCAP) data collected during cycling experiments of various additive electrolyte systems using coated NMC532 cathodes and synthetic graphite anodes. Experimental data is plotted, including discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (the difference between the average charge voltage and the average discharge voltage).
[0065] 10J-10K illustrate experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling and ultra-precision cycling experiments of various electrolyte systems using uncoated NMC532 cathodes and synthetic graphite anodes.
[0066] 10L-10R illustrate experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments of various electrolyte systems using Al2O3-coated and AFO-coated NMC622 positive electrodes and synthetic graphite negative electrodes.
[0067] FIG. 10S illustrates experimental data including discharge capacity, normalized discharge capacity (or fade rate), and ΔV (the difference between the average charge voltage and the average discharge voltage) collected during cycling experiments of various electrolyte systems using lithium-ion battery cells.
[0068] FIG. 10T illustrates experimental data including discharge capacity, normalized discharge capacity (or fade rate), and ΔV (the difference between the average charge voltage and the average discharge voltage) collected during cycling experiments of various electrolyte systems using lithium-ion battery cells.
[0069] FIG. 10U illustrates experimental data including discharge capacity, normalized discharge capacity (or fade rate), charge endpoint capacity, coulombic efficiency, and ΔV (difference between average charge voltage and average discharge voltage) collected during cycling experiments of various electrolyte systems using lithium-ion battery cells.
[0070] FIG. 10V illustrates experimental data, including discharge capacity, normalized discharge capacity (or fade rate), and ΔV (difference between average charge voltage and average discharge voltage), collected during cycling experiments of various electrolyte systems using coated and uncoated NMC532 positive electrodes and synthetic graphite negative electrodes, and Al2O3-coated and AFO-coated NMC622 positive electrodes and synthetic graphite negative electrodes.
[0071] FIG. 10W illustrates experimental data, including discharge capacity, normalized discharge capacity (or fade rate), and ΔV (difference between average charge voltage and average discharge voltage), collected during cycling experiments of various electrolyte systems using coated and uncoated NMC532 positive electrodes and synthetic graphite negative electrodes, and Al2O3-coated and AFO-coated NMC622 positive electrodes and synthetic graphite negative electrodes.
[0072] [Figure 11] Illustrates coulomb inefficiency per hour versus cycle number, partial charge endpoint capacity shift per hour versus cycle number, and partial capacity fade per hour versus cycle number for electrolyte systems containing 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, and 2% FEC using an uncoated NMC532 cathode and synthetic graphite anode cycling from 3.0 V to 4.3 V.
[0073] [Figure 12] Illustrates coulomb inefficiency per hour versus cycle number, partial charge endpoint capacity shift per hour versus cycle number, and partial capacity fade per hour versus cycle number for electrolyte systems containing 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, 2% FEC, and 1% LFO using coated NMC532 cathodes and synthetic graphite anodes cycled from 3.0 V to 4.3 V.
[0074] [Figure 13] Illustrates coulomb inefficiency per hour versus cycle number, partial charge endpoint capacity shift per hour versus cycle number, and partial capacity fade per hour versus cycle number for electrolyte systems containing 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, and 2% FEC using an Al2O3 coated NMC622A cathode and synthetic graphite anode cycled from 3.0 V to 4.3 V.
[0075] [Figure 14] Illustrates coulomb inefficiency per hour versus cycle number, partial charge endpoint capacity shift per hour versus cycle number, and partial capacity fade per hour versus cycle number for electrolyte systems containing 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, and 2% FEC using AFO coated NMC622B cathode and synthetic graphite anode cycling from 3.0 V to 4.3 V.
[0076] [Figure 15] 1 illustrates the average parasitic heat flow per cycle in experiments involving various electrolyte additive systems in lithium-ion battery cells.
[0077] [Figure 16] 1 illustrates the change in voltage and gas capacity over time for experiments involving various electrolyte additive systems in a lithium-ion battery cell.
[0078] [Figure 17] 1 illustrates the parasitic heat flow in experiments involving various electrolyte additive systems in a lithium-ion battery cell. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0079] FIG. 1 illustrates basic components of a battery-powered electric vehicle (EV) 100. The EV 100 includes at least one drive motor (traction motor) 102A and / or 102B, at least one gearbox 104A and / or 104B coupled to the corresponding drive motor 102A and / or 102B, battery cells 106, and electronics 108. In general, the battery cells 106 power the EV 100's electronics and provide electrical power to propel the EV 100 using the drive motor 102A and / or 102B. The EV 100 includes numerous other components not described herein but known to those skilled in the art. Although the EV 100 configuration of FIG. 1 is shown as having four wheels, different EVs may have fewer or more than four wheels. Different types of EVs 100, including motorcycles, aircraft, trucks, boats, and train engines, among other types of vehicles, may incorporate the inventive concepts described herein. Certain components made using embodiments of the present disclosure may be used in vehicle 100.
[0080] FIG. 2 shows a schematic diagram of an exemplary energy storage system 200 showing various components. The energy storage system 200 typically includes a modular housing with at least a base 202 and four side walls 204 (only two are shown in the figure). The modular housing is typically electrically isolated from the enclosed battery cells 206. This may occur by physical separation, by an electrically insulating layer, by selection of insulating material for the modular housing, any combination thereof, or otherwise. The base 202 may be an electrically insulating layer on a metal sheet, or a non-conductive / electrically insulating material such as polypropylene, polyurethane, polyvinyl chloride, another plastic, a non-conductive composite, or insulating carbon fiber. The sidewalls 204 may also include an insulating layer or may be formed from a non-conductive or electrically insulating material, such as polypropylene, polyurethane, polyvinyl chloride, another plastic, a non-conductive composite, or insulated carbon fiber. One or more interconnect layers 230 may be disposed over the battery cells 206, and the top plate 210 is disposed over the interconnect layers 230. The top plate 210 may be a single plate or may be formed from multiple plates.
[0081] The individual battery cells 106 and 206 are often lithium-ion battery cells with a positive electrode and a negative electrode, including an electrolyte containing lithium ions. Figure 3 shows a schematic diagram of a lithium-ion cell 300. Lithium ions 350 are dispersed throughout an electrolyte 320 within a container 360. The container 360 may be part of the battery cell. The lithium ions 350 migrate between a positive electrode 330 and a negative electrode 340. A separator 370 separates the negative and positive electrodes. A circuit 310 connects the negative and positive electrodes.
[0082] New research by the inventors has identified novel electrolyte and battery systems for use in grid and electric vehicle applications. These systems are based on dual-additive electrolyte systems that combine solvents and electrodes including vinylene carbonate (VC) in combination with 1,2,6-oxodithiane-2,2,6,6-tetraoxide (ODTO), LiPO2F2 in combination with ODTO, and fluoroethylene carbonate (FEC) in combination with ODTO. These dual-additive electrolyte systems are based on LNi x Mn y Co z The cathode is paired with a cathode made from lithium nickel manganese cobalt oxide having a composition of NMCxyz (commonly abbreviated as NMC or NMCxyz, where x, y, and z are the molar ratios of nickel, manganese, and cobalt, respectively). In certain embodiments, the cathode is formed from NMC111, NMC532, NMC811, or NMC622. In certain embodiments, NMC532 cathodes formed from single crystal, micrometer-sized grains resulting in electrodes with micrometer-sized areas of continuous crystal lattice (or coarse grains) have been shown to be particularly robust, due in part to the materials and processing conditions that result in larger grain sizes than when using conventional materials and processing conditions.
[0083] Typical processing conditions result in NMC electrodes with nanometer-sized particles packed into larger micrometer-sized aggregates, creating grain boundaries on the nanometer scale. Grain boundaries are defects that tend to reduce desirable properties (e.g., electrical properties), so it is generally desirable to reduce the number of coarse grains and increase the grain size. Processing can create larger domains on the micrometer-sized scale, thus reducing the number of grain boundaries in the NMC electrode and improving electrical properties. The improved properties result in a more robust battery system. In certain embodiments, other NMC electrodes can be processed to create larger domain sizes (micrometer-sized scale or larger), e.g., NMC111, NMC811, NMC622, or another NMC compound, to create a more robust system.
[0084] The positive electrode may be coated with a material such as aluminum oxide (Al2O3), titanium dioxide (TiO2), or another coating material. A coating material on the positive electrode is advantageous because it may help reduce interfacial phenomena at the positive electrode, such as parasitic reactions or other phenomena that may degrade a cell containing the coated material. The negative electrode may be made from natural graphite, synthetic graphite, or other materials.
[0085] The electrolyte may be a lithium salt (such as LiPF6) dissolved in a combination of organic or non-aqueous solvents, including ethylene carbonate, ethyl methyl carbonate, methyl acetate, propylene carbonate, dimethyl carbonate, diethyl carbonate, another carbonate solvent (cyclic or non-cyclic), another organic solvent, and / or another non-aqueous solvent. The solvent may be an additive. The additive is present in a higher concentration, typically greater than 5% or greater than 6% by weight. The experimental data was generated using an electrolyte solvent containing EC:EMC:DMC at 25:5:70 by volume (with or without methyl acetate (MA)), but these solvents are only examples of other carbonate solvents, particularly other non-aqueous solvents. To understand the effect of the additive and the electrode, the EC and EMC solvents were used in the experiments to control the system tested. Thus, the electrolyte system can use other carbonate solvents and / or other non-carbonate solvents, including propylene carbonate, ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, other carbonate solvents (cyclic or non-cyclic), other organic solvents, and / or another non-aqueous solvent. The solvent is present in a higher concentration, typically greater than 5% or greater than 6% by weight, than the additive.
[0086] In a binary mixture of FEC+ODTO, the concentration of FEC is preferably 0.5% to 6% by weight and the concentration of ODTO is preferably 0.25% to 5% by weight. In a binary mixture of VC+ODTO, the concentration of VC is preferably 0.5% to 6% by weight and the concentration of ODTO is preferably 0.25% to 5% by weight. In a binary mixture of LFO+ODTO, the concentration of LFO is preferably 0.5% to 1.5% by weight and the concentration of ODTO is preferably 0.25% to 5% by weight.
[0087] These particular new battery systems can be used in energy storage applications, as well as automotive applications (including energy storage in electric vehicles), where the speed of charge and discharge, as well as the lifetime when rapidly charged and discharged, are important.
[0088] Pre-experiment configuration Although the battery system itself may be packaged separately according to the present disclosure, the experimental setup typically uses a machined "sealed cell" to systematically evaluate battery systems using a common setup, including a dual-additive electrolyte system and specific materials for use in the positive and negative electrodes. All percentages referred to within this disclosure are by weight unless otherwise specified. Those skilled in the art will appreciate that the type of additive used and the concentration employed will depend on the most desirable and improved properties, as well as the other components and design used in the lithium-ion battery being fabricated, and will be apparent from this disclosure.
[0089] Sealed Battery Cell The NMC / graphite sealed cells used in the experimental setup contained 1M LiPF6 in the solvent with the additive. The electrolyte consisted of 1M LiPF6 in 30% EC and 70% EMC. The concentrations of the electrolyte components can be modified to include MA and / or DMC. To this electrolyte, the additive components were added at the weight percentages specified.
[0090] The sealed battery cells used in the experimental setup contained an electrolyte solvent consisting of 1.2 M LiPF6 added to EC, EMC, and DMC in a volume ratio of 25:5:70. To this electrolyte, additive components were added at the weight percentages specified.
[0091] Sealed NMC / graphite cells used positive electrodes made of coarse micrometer-sized NMC532 (sometimes called monocrystalline NMC532) and negative electrodes made of synthetic graphite unless otherwise specified. Other positive electrodes and negative electrodes (containing natural graphite) were used to test specific battery systems, including standard NMC532 (smaller grain size than the coarse micrometer-sized NMC) and NMC622.
[0092] Before filling the electrolyte, the sealed cells were cut open below the heat seal and vacuum dried at 100°C for 12 hours to remove residual moisture. The cells were then immediately transferred to an argon-filled glove box for filling and vacuum sealing before filling with the electrolyte. After filling, the cells were placed in a vacuum-sealed evaporator. The vacuum seal was performed.
[0093] After sealing, the sealed cells were placed in a temperature box at 40.0 + / - 0.1 °C and held at 1.5 V for 24 hours to complete wetting. The sealed cells were then subjected to a formation process. Unless otherwise stated, the formation process for NMC / graphite cells consisted of charging the sealed cells to 4.2 V at 11 mA (C / 20) and discharging to 3.8 V. C / x indicates that if the cell has an initial capacity, it will take x hours to charge or discharge the cell at the selected current. For example, C / 20 indicates that it will take 20 hours to charge or discharge. After formation, the cells were transferred to a glove box, cut open to release evolved gases, and vacuum sealed again for appropriate experiments.
[0094] The formation process of the battery cells for cycling and storage experiments consisted of charging the sealed cells at C / 2 at 40 °C for 1 h, storing the cells at 60 °C for 22 h, charging the cells at C / 2 at 40 °C to 4.2 V, and discharging to 3.8 V. After formation, the cells were transferred to a glove box, cut open to release evolved gases, and vacuum sealed again to perform the appropriate experiments.
[0095] The formation process of the battery cells for the charging profile and in-situ gas capacity measurement experiments consisted of charging the sealed cells at C / 20 at 40° C. to 4.2 V and discharging at C / 20 at 40° C. to 3.8 V while the cells were connected to the in-situ gas measurement equipment.
[0096] Passivation effect The passivation effect of various electrolyte compositions in different types of cells is shown in Figures 4A-4E. As can be seen from the data in Figures 4A-4E, ODTO shows similar passivation effect in five different types of cells. The first and second cells (Figures 4A-4B) show a comparison of the passivation effect of ethylene carbonate (EC); ethyl methyl carbonate (EMC) (control), 2% VC, 1% ODTO, 3% ODTO, 5% ODTO, 2% VC + 1% ODTO, 2% FEC + 1% ODTO, and 1% LFO + 1% ODTO in a cell with an uncoated NMC532 positive electrode (Figure 4A) and an artificial graphite electrode, and a cell with a coated NMC532 positive electrode (Figure 4B) and an artificial graphite electrode. The third and fourth cells (FIGS. 4C-4D) show the passivation effect of 2% VC, 1% LFO+1% ODTO, 2% FEC+1% ODTO, 2% VC+1% ODTO, 1% ODTO, 3% ODTO and 5% ODTO in the cell with Al2O3-coated NMC622 / artificial graphite electrodes (FIG. 4C) and the cell with AFO-coated NMC622 electrodes (FIG. 4D). And the fifth cell (FIG. 4E) shows the passivation effect of EC:EMC:DMC, 2% VC, 2% VC+1% ODTO and 2% VC+3% ODTO. The peak at approximately 2.3 V corresponds to the decrease in ODTO in the presence of 1% ODTO (passivation peak). The effect of the 1% ODTO additive is independent of the type of cathode used, as demonstrated by similar peaks in Figures 4C-E for the data for the Al2O3-coated NMC622 cathode, the AFO-coated NMC622 cathode, and the electrode found in the battery cell.
[0097] Cell Impedance The dual additive electrolyte system and novel battery system disclosed herein have low cell impedance. It is desirable to minimize cell impedance because it reduces the energy efficiency of the cell. Conversely, lower impedance allows for higher possible charge rates and greater energy efficiency.
[0098] Cell impedance was measured using electrochemical impedance spectroscopy (EIS). The cells were charged or discharged to 3.80 V before being transferred to a temperature box at 10.0 + / - 0.1 °C. AC impedance spectra were collected at 10 points per 10 min from 100 kHz to 10 mHz with a signal amplitude of 10 mV at 10.0 + / - 0.1 °C. The charge transfer resistance (R ct ) was calculated and plotted.
[0099] In certain embodiments, a dual-additive electrolyte system, with each additive having a concentration of about 0.25% to 6%, forms part of the battery system. 5A-5E show the results of the experiments with 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, 2% FEC, and 1% LFO in cells with uncoated NMC532 positive electrodes and synthetic graphite negative electrodes (FIG. 5A); 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 1% LFO+1% ODTO+1% VC, 1% LFO+1% ODTO+1% FEC, 1% LFO+1% ODTO+1% TTSPi, 2% VC, 2% FEC, and 1% LFO in cells with coated NMC532 positive electrodes and synthetic graphite negative electrodes (FIG. 5B); The experimental data are shown for cell charge transfer impedance experiments of dual additive electrolyte systems consisting of 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, and 2% FEC in cells with AFO-coated NMC622 positive electrodes and synthetic graphite negative electrodes (FIG. 5C); 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC, and 2% FEC in cells with AFO-coated NMC622 positive electrodes and synthetic graphite negative electrodes (FIG. 5D); and 2% VC, 2% VC+1% ODTO, 2% FEC+3% ODTO in another lithium-ion battery cell (FIG. 5E). A synthetic graphite negative electrode was used in each of these electrochemical cells.
[0100] In addition, the charge transfer impedance (R ct ) was investigated for these cells. As shown in the data in Figures 6A-6E, the cell charge transfer impedance is reduced with 1% ODTO alone or 1% ODTO in combination with 2% FEC, 2% VC, or 1% LFO compared to electrolytes containing 3% ODTO or 5% ODTO. Thus, these novel dual-additive electrolyte systems do not sacrifice significant charge transfer impedance performance with the inclusion of ODTO.
[0101] Gas volume measurement The formation process is carried out before the cells are used in their intended application, such as grid storage or energy storage in vehicles such as electric vehicles. During formation, the cells are subjected to precisely controlled charge-discharge cycles, which are intended to activate the electrodes and electrolyte for use in their intended application. Gases are generated during formation. If sufficient amounts of gas are generated (depending on the specific tolerances tolerated by the cell and the packaging of the cell), it may be necessary to release the gas after the formation process and before use in the application. This usually requires the additional steps of breaking the seal and then resealing. Although these steps are common in many battery systems, it is desirable to eliminate these steps, if possible, by choosing a system that produces less gas.
[0102] Gas capacity experiments proceeded as follows: Ex-situ (static) gas measurements were used to measure gas evolution during formation and cycling. Measurements were performed by suspending the cell from a balance while submerged in liquid using Archimedes' principle. The change in cell weight suspended in the fluid before and after the test is directly related to the volume change due to the change in buoyancy. The change in mass Δm of a cell suspended in a fluid of density ρ is related to the change in cell volume Δv by Δv=-Δm / ρ. Gases generated during charge / discharge and high potential hold periods were analyzed using the method described by Aiken et al. (CP Aiken, J. Xia, David Yaohui Wang, DA Stevens, S. Trussler and JR Dahn, J. Electrochem. Soc. 2014). The measurements were performed using an in-situ gas measurement apparatus described by the authors (Frank et al., 2014 volume 161, A1548-A1554).
[0103] In certain embodiments, a two-additive electrolyte system, with a concentration of each additive between about 0.25% and 6%, forms part of the battery system. Figures 7A-7E show the results of the electrolyte solutions of 1% ODTO, 3% ODTO, 5% ODTO, 2% VC + 1% ODTO, 2% FEC + 1% ODTO, 1% LFO + 1% ODTO, 2% VC, 2% FEC, and 1% LFO in cells with uncoated NMC532 positive electrodes and synthetic graphite negative electrodes (Figure 7A); 1% ODTO, 3% ODTO, 5% ODTO, 2% VC + 1% ODTO, 2% FEC + 1% ODTO, 1% LFO + 1% ODTO, 2% VC, 2% FEC, and 1% LFO in cells with coated NMC532 positive electrodes and synthetic graphite negative electrodes (Figure 7B); The results of gas generation experiments are shown in two-additive electrolyte systems consisting of 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC and 2% FEC (Figure 7C); 1% ODTO, 3% ODTO, 5% ODTO, 2% VC+1% ODTO, 2% FEC+1% ODTO, 1% LFO+1% ODTO, 2% VC and 2% FEC (Figure 7D) in cells with coated NMC622 positive electrodes and synthetic graphite negative electrodes; and 2% VC, 2% VC+1% ODTO and 2% VC+3% ODTO in separate lithium-ion battery cells (Figure 7E). A synthetic graphite negative electrode was used in each of these electrochemical cells. In each of these cells, the amount of gas produced was measured according to the procedure described above. As shown in Figures 7A-7E, significant amounts of gas were produced in cells with 1% ODTO or 1% LFO+1% ODTO. However, gas production was significantly reduced in cells with 2% VC + 1% ODTO and 2% FEC + 1% ODTO.
[0104] Energy storage experiment After formation, the cells were discharged twice to 3 V and charged to 4.4 V at a current corresponding to C / 10. The cells were then held at 4.4 V for 24 h and then transferred to a storage box at 60° C. The open circuit voltage was automatically recorded every 6 h for 500 h. Figures 8A and 8B show that the cells incorporating 2VC+1ODTO exhibited the lowest self-discharge under these conditions.
[0105] Ultra-Precision Cycling To study the effectiveness of the disclosed battery system, including the working electrolyte additive and electrodes, ultrahigh precision cycling (UHPC) was performed. The standard UHPC procedure consisted of cycling the cell from 3.0V to 4.3V at 40°C for 15 cycles using a current corresponding to C / 20 to generate data. For coulombic efficiency, UPHC is used to measure coulombic efficiency, charge endpoint capacity shift, and other parameters to an accuracy of 30 ppm. Details of the UHPC procedure are described in TM Bond, JC Burns, DA Stevens, HM Dahn, and JR Dahn, Journal of the Electrochemical Society, 160, A521 (2013), which is incorporated herein in its entirety.
[0106] Metrics measured and / or determined from UHPC measurements of particular interest include coulombic efficiency, normalized coulombic efficiency, normalized charge endpoint capacity shift, normalized discharge capacity (i.e., fade rate), and delta V. Coulombic efficiency is related to discharge capacity (Q d ) to the charge capacity of the previous cycle (Q c ) Coulombic efficiency tracks the parasitic reactions occurring in a Li-ion cell and includes contributions from both the positive and negative electrodes. A higher CE value indicates less degradation of the electrolyte in the cell. Coulombic efficiency per hour (CIE / h) is the normalized coulombic efficiency (per hour), where coulombic efficiency is defined as 1-CE. The CIE / h is calculated by taking 1-CE and dividing by the cycle time for which CE is measured. The movement (or drift) of the charge endpoint capacity tracks the parasitic reactions occurring at the positive electrode as well as the mass loss of the positive electrode material, if any. Less movement is better and is associated with less oxidation of the electrolyte. Normalized discharge capacity, or fade rate, is another important metric, with lower fade rates being more desirable and usually indicating a longer life for the battery system. ΔV is calculated as the difference between the average charge voltage and the average discharge voltage. The change in ΔV is closely related to the growth of polarization, and as cycling occurs, the change in ΔV becomes smaller. UHPC measurements are particularly well suited for comparing electrolyte compositions, as the metric can be tracked accurately with greater precision and various degradation mechanisms can be assessed relatively quickly.
[0107] Here, UHPC experiments were performed using 1% ODTO, 3% ODTO, 5% ODTO, 1% ODTO+2% VC, 1% ODTO+2% FEC, 1% ODTO+1% LFO, 2% VC, 2% FEC, 2% VC, 20% MA+2% VC, 20% MA+2% VC+1% ODTO and 1% LFO. The five different cell cathode materials investigated include uncoated (FIG. 11) and coated (FIG. 12) NMC532, as well as Al2O3-coated NMC622 (FIG. 13) and AFO-coated NMC622 (FIG. 14), and other lithium-ion battery cell active materials. The raw data for the coated NMC532 cell is shown in FIG. 10D and FIG. 10E. The raw data for the uncoated NMC532 cell is shown in FIG. 10J and FIG. 10K. The raw data for the Al2O3-coated NMC622 cell is shown in FIG. 10O and FIG. 10P. The raw data for the AFO coated NMC622 cell is shown in Figure 10Q and Figure 10R, while the raw data for the other lithium-ion battery cells is shown in Figure 10U.
[0108] In certain embodiments, a dual-additive electrolyte system, with a concentration of each additive of about 0.25% to 6%, forms part of the battery system. The battery system may also include a positive electrode made from NMC111, NMC532, NMC811, NMC622, or another NMC composition (NMCxyz). In certain embodiments, positive electrodes made from micrometer-scale coarse-grained NMC532 have been shown to be particularly robust, in part because processing conditions create larger grain sizes than normal processing conditions produce.
[0109] Typical processing conditions result in NMC electrodes with nanometer-sized particles packed into larger micrometer-sized aggregates, creating grain boundaries at the nanometer scale. Grain boundaries are defects that tend to reduce desirable properties (e.g., electrical properties), so it is generally desirable to reduce the number of coarse grains and increase the grain size. Current processing can create larger domains at the micrometer-sized scale, reducing the number of grain boundaries in the NMC electrode and improving electrical properties. The improved properties result in a more robust battery system. In certain embodiments, other NMC electrodes can be processed to create larger domain sizes (micrometer-sized scale or larger), such as NMC111, NMC811, NMC622, or another NMC compound, to create a more robust system.
[0110] Long-term cycling The lifetime of a battery system is an important characteristic of the battery system. The rates of charging and discharging can affect the lifetime. Long-term cycling experiments help determine the aging behavior of a resilient battery system under expected operating conditions. It is important to select a battery system with sufficient lifetime for the desired application.
[0111] Embodiments of the present disclosure demonstrate desirable long-term cycling for a variety of applications, including grid and vehicle energy storage. In particular, the VC+ODTO, LFO+ODTO, and FEC+ODTO dual additive electrolyte systems are particularly well suited for applications where the charge and discharge rates are typically consistent with those of grid energy storage applications. This is relevant for automotive applications (especially energy storage in electric vehicles), where the costs are higher than in the past.
[0112] In the long-term cycling experiments, monocrystalline NMC532 and NMC622 were typically used as the positive electrodes and synthetic graphite was used as the negative electrode (unless otherwise specified). Prior to the long-term cycling experiments, the sealed cells were subjected to a formation process as described above for each cell type. After formation, the cells were cycled in a Neware charging system.
[0113] In some experiments, the cells were stored in a temperature controlled box at 40° C. + / - 0.2° C. The cells were cycled between a top of charge (4.2V or 4.3V) with a current of 3.0V and C / 3 (3 hour half cycle) and a constant voltage step at the beginning of charge until the current fell below C / 20. Every 50 cycles, the cells underwent one complete cycle at C / 20. Results from such experiments for coated NMC532 are shown in Figures 10A, 10B, 10C, 10V(b), and 10W(b), uncoated NMC532 is shown in Figures 10V(a) and 10W(a), Al2O3-coated NMC622 is shown in Figures 10L, 10V(c), and 10W(c), AFO-coated NMC622 is shown in Figures 10M, 10N, 10V(d), and 10W(d), and another lithium-ion battery cell is shown in Figure 10T(b).
[0114] In some experiments, the cells were placed in a temperature controlled box at 55°C + / - 0.2°C. The cells were cycled between a top of charge (4.2V or 4.3V) with a current of 3.0V and C / 3 (3 hour half cycle) and a constant voltage step at the beginning of charge until the current fell below C / 20. Every 50 cycles, the cells went through one complete cycle at C / 20. Results from such experiments for the coated NMC532 are shown in Figures 10F and 10G, and for other lithium-ion battery cells in Figures 10S and 10T(c).
[0115] In some experiments, the cells were stored in a temperature controlled box at 20°C + / - 0.2°C. The cells were cycled between a top of charge (4.2V or 4.3V) with a current of 3.0V and C / 3 (3 hour half cycle) and a constant voltage step at the beginning of charge until the current fell below C / 20. Every 50 cycles, the cells went through one complete cycle at C / 20. The results of such an experiment for the coated NMC532 are shown in Figure 10H, and the results for other lithium-ion battery cells are shown in Figure 10T(a).
[0116] In some experiments, the cells were stored in a temperature controlled box at 20° C. + / - 0.2° C. The cells were cycled between the top of charge (4.2V or 4.3V) with a current of 3.0V and 1C (one hour to charge and one hour to discharge) and a constant voltage step at the beginning of charge until the current fell below C / 20. Every 50 cycles, the cells went through one complete cycle at C / 20. Results from such an experiment for coated NMC532 are shown in FIG. 10I.
[0117] The experimental data shows that the dual-additive electrolyte systems (ODTO+FEC, ODTO+LFO, and DTD+VC) have less capacity loss upon cycling to 4.2 V or 4.3 V, and also have lower polarization growth compared to the single-additive electrolyte systems of VC or FEC, and cycling is similar to 2%VC+1%DTD and 1%LFO+2FEC.
[0118] Other studies were performed on other lithium-ion battery cells, including average parasitic heat flow per cycle studies (FIGS. 15, 17, and 9) and in-situ gassing assessment during charge hold shown in FIG. 16.
[0119] Gas capacity experiments proceeded as follows: Ex-situ (static) gas measurements were used to measure gas evolution during formation and cycling. Measurements were performed by suspending the cell from a balance while submerged in liquid using Archimedes' principle. The change in cell weight suspended in fluid before and after the test is directly related to the volume change due to the change in buoyancy. The change in mass Δm of a cell suspended in a fluid of density ρ is related to the change in cell volume Δv by Δv=-Δm / ρ. Gases generated during charge / discharge and high potential hold periods were measured using an in-situ gas measurement apparatus described by Aiken et al. (CPA Aiken, J. Xia, David Yaohui Wang, DA Stevens, S. Trussler and JR Ahhn, J. Electrochem. Soc. 2014 volume 161, A1548-A1554).
[0120] The results in FIG. 16 showed that ODTO was beneficial in suppressing gassing at high voltages with and without 20% MA during charging / holding. Microcalorimetry
[0121] Microcalorimetry measures the heat flow to a cell during operation. The heat flow to the cell is a combination of three different effects: (1) ohmic heating, (2) entropy changes due to Li insertion at the electrodes, and (3) parasitic reactions (degradation of the electrolyte with additives at either electrode). Because the test cells contain the same physical design differing only in the electrolyte, the difference in heat flow is primarily due to differences in parasitic heat flow. Nevertheless, the parasitic heat flow can be extracted from the total heat flow using procedures developed by Downie et al. (Journal of the Electrochemical Society, 161, A1782-A1787 (2014)) and Glazier et al. (Journal of the Electrochemical Society, 164(4) A567-A573 (2017)). Both of these references are incorporated herein in their entirety. Cells with less parasitic heat flow during cycling will have a longer life. The voltage dependence of the parasitic reaction rate can be observed by plotting the measured parasitic heat flow as a function of the cell voltage.
[0122] Microcalorimetry procedure: Two cells of each electrolyte were connected to a Maccor charger and inserted into a TAMIII microcalorimeter (TA Instruments, stability + / - 0.0001 °C, accuracy + / - 1 μW, precision + / - 1 nW) at 40.0 °C. Baseline drift during the experiment did not exceed + / - 0.5 μW. All specifications and information regarding microcalorimetry calibration, cell connections, and operating procedures have been described previously (e.g., Downie et al, ECS Electrochemical Letters 2, A106-A109 (2013)). Cells were cycled four times at a C / 20 rate from 3.0 V to 4.2 V to ensure a properly formed and stable SEI, and then charged between different upper cutoffs of 4.0 V and 3.7 mA (C / 100) to investigate performance and parasitic heat flow at various voltage ranges. Each pair of cells performed nearly identically, so only one set of heat flow data is presented for each electrolyte.
[0123] The 3.7mA cycling protocol was as follows: Charge to 14.0V, discharge to 3.9V, repeat Charge to 2.4.1V, discharge to 3.9V (repeated) Charge to 3.4.2V, discharge to 3.9V (repeated) 6. Charge to 4.0V, discharge to 3.9V (repeated)
[0124] The experimental data shown in Figures 15, 17 and 9 were used for other lithium-ion battery cells containing electrolyte additives 2VC, 2VC+1ODTO, 2VC with 20% MA and 2VC+1ODTO with 20% MA. The cells were tested at 3.9V to 4.2V. The usefulness of ODTO is observed when 1% ODTO is added to the battery. In this situation, parasitic heat flow is reduced, suggesting that other Li-ion cells containing 1% ODTO will last longer when charged to 4.2V (full charge). This is important for extending the life of the battery pack to several years or miles of driving.
[0125] In certain embodiments, the cathode is formed from NMC111, NMC532, NMC822, NMC622, and / or NMCxyz. In particular, cathodes made from single crystal NMC532 have been shown to be particularly robust, in part due to the larger grain size of NMC532 compared to the grain size of other standard NMC materials, which are more polycrystalline and smaller grained.
[0126] The above disclosure is not intended to limit the disclosure to the exact form or specific field of use disclosed. Therefore, it is contemplated that various alternative embodiments and / or modifications to the disclosure are possible in light of the disclosure, whether or not expressly described or implied herein. Although the embodiments of the disclosure have been described in this manner, those skilled in the art will recognize that changes can be made in form and detail without departing from the scope of the disclosure. Therefore, the disclosure is limited only by the claims. References to additives in this specification generally refer to working additives, unless otherwise stated in this specification.
[0127] In the foregoing specification, the present disclosure has been described with reference to specific embodiments. However, as will be understood by those skilled in the art, the various embodiments disclosed herein may be modified or embodied in various other ways without departing from the spirit and scope of the present disclosure. Thus, this description should be considered as illustrative and is intended to teach those skilled in the art how to make and use the various embodiments of the disclosed battery system. It should be understood that the forms of the disclosure shown and described herein should be construed as representative embodiments. Equivalent elements or materials may be substituted for those typically illustrated and described herein. Furthermore, certain features of the present disclosure may be utilized independently of the use of other features, either of which will become apparent to those skilled in the art after having the benefit of this description of the present disclosure. The terms "including," "comprising," "incorporating," "consisting of," "having," and the like, used to describe and claim the present disclosure, should be construed in a non-exclusive manner, i.e., there may be items, components, or elements not expressly described. References to the singular should also be construed to relate to the plural. References to "about" or "approximately" should be construed to mean plus or minus 10%. Similarly, references to any percentage of an additive should be construed to mean plus or minus 10%.
[0128] Furthermore, the various embodiments disclosed herein should be construed in an illustrative and explanatory sense, and should not be construed as limiting the present disclosure in any way. All connector references (e.g., attached, affixed, coupled, connected, etc.) are used only to aid the reader's understanding of the present disclosure, and cannot create limitations with respect to the position, orientation, or use of the systems and / or methods disclosed herein in particular. Thus, connector references, if any, should be interpreted broadly. Moreover, such connector references do not necessarily infer that two elements are directly connected to each other.
[0129] Additionally, all absolute numbers, such as, but not limited to, "first," "second," "third," "primary, major," "secondary," "main," or other conventional terms and / or absolute numbers, are intended to be taken only as identifiers to aid the reader in understanding the various elements, embodiments, variations and / or modifications of the present disclosure, and in particular are not intended to limit the order or priority of any element, embodiment, variation and / or modification to or relative to another element, embodiment, variation and / or modification. It is not possible to set up
[0130] It is also understood that one or more elements shown in the drawings / figures may be implemented in a more separate or integrated manner, or even deleted or rendered inoperative in certain cases, as may be useful depending on the particular application. [Prior art documents] [Patent documents]
[0131] [Patent Document 1] US Patent Application Publication No. 2017 / 0025706 [Non-patent literature]
[0132] [Non-Patent Document 1] J.C. Burns et al., Journal of the Electrochemical Society, 160, A1451 (2013)
Claims
1. A lithium ion battery, A cathode; A positive electrode and 1. A non-aqueous electrolyte consisting essentially of lithium ions dissolved in a non-aqueous solvent and an additive mixture, the additive mixture comprising: a first working additive selected from the group consisting of fluoroethylene carbonate, LiPO 2 F 2 , vinylene carbonate, and combinations thereof; and The following formula (I) a second working additive which is 1,2,6-oxodithiane-2,2,6,6-tetraoxide having the formula: The concentration of the first working type additive is in the range of 0.25% to 6% by weight, and the concentration of the second working type additive is in the range of 0.25% to 5% by weight; The lithium ion battery has at least 95% retention of initial capacity after 200 cycles between 3.0V and 4.3V at a charge rate of C / 3 CCCV at 40° C.
2. A lithium ion battery as described in claim 1, wherein the concentration of the first working type additive is at least 1 weight % and the concentration of the second working type additive is at least 1 weight %.
3. The lithium ion battery of claim 1, wherein the first working additive is fluoroethylene carbonate.
4. The lithium ion battery of claim 1, wherein the first working additive is vinylene carbonate.
5. The lithium ion battery of claim 1, wherein the first working additive is LiPO 2 F 2 .
6. The lithium ion battery of claim 1, wherein the non-aqueous solvent is selected from the group consisting of ethylene carbonate, ethyl methyl carbonate, and combinations thereof.
7. The lithium ion battery of claim 6, further comprising a second non-aqueous solvent.
8. The lithium-ion battery of claim 1, wherein the positive electrode comprises lithium nickel manganese cobalt oxide (NMC) active material.
9. The lithium-ion battery of claim 8, wherein the positive electrode comprises at least one lithium nickel manganese cobalt oxide ("NMC") selected from the group consisting of NMC111, NMC532, NMC811 and NMC622.
10. The lithium ion battery of claim 1, wherein the negative electrode comprises a graphite active material.
11. A lithium ion battery as described in claim 1, wherein the volume of gas produced in the lithium ion battery is comparable to the volume of gas produced in a lithium ion battery containing only the first working type additive.
12. The lithium ion battery of claim 1, wherein the lithium ion battery has at least 95% retention of initial capacity after 800 cycles from 3.0V to 4.3V at a charge rate of C / 3 CCCV at 40°C.
13. An electric vehicle equipped with a rechargeable battery, A drive motor; The gearbox and Electronics and An electric vehicle comprising the lithium ion battery according to claim 1.
Citation Information
Patent Citations
Secondary battery
JP2009038018A
Electrolyte and secondary battery
JP2010165542A
Electrolyte for secondary battery, secondary battery, electric tool, electric vehicle, and power storage system
JP2012054156A
Electrolyte additives for lithium ion batteries
US20170025706A1