Hot Melt Composition

A hot melt composition with thermoplastic resin and plasticizer addresses discomfort and breakage issues in stretchable members by enhancing stretch recovery and compatibility with coating devices, suitable for absorbent articles.

JP7559177B2Active Publication Date: 2024-10-01SEKISUI FULLER CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023178252
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-06-04
Filing Date
2023-10-16
Publication Date
2024-10-01
Estimated Expiration
2039-06-04

AI Technical Summary

Technical Problem

Existing stretchable members in absorbent articles, such as rubber threads and thermoplastic elastomer films, cause discomfort due to linear pressure, breakage during manufacturing, and reduced stretchability when used in hot melt adhesive compositions.

Method used

A hot melt composition comprising a thermoplastic resin and a plasticizer, with specific dynamic viscoelasticity properties, allowing for improved stretch recovery and resistance to breakage even when heated and stretched, and compatible with normal hot melt coating devices.

Benefits of technology

The composition ensures excellent coating properties, maintains stretch recovery, and prevents breakage, making it suitable for use in absorbent articles like paper diapers and sanitary napkins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559177000001
    Figure 0007559177000001
Patent Text Reader

Abstract

To provide a hot-melt composition which suppresses lowering and breakage of elastic recovery even after being heated and held in an elongated state, and can be coated by a usual hot-melt coating device.SOLUTION: A hot-melt composition contains a thermoplastic resin (A) and a plasticizer (B), wherein a master curve obtained by performing dynamic viscoelasticity measurement under the conditions of a temperature of -20 to 120°C and a frequency (f) of -0.2 to 2.0 Hz, plotting a log (log(G')) of measured storage elastic modulus (G') and a log (log(G")) of measured storage elastic modulus (G") with respect to a log (log(f)) of the frequency (f), and setting a reference temperature at 40°C, (1) the value of the log(f) at a point with the maximum log(G") in a range of -6.0<log(f)<-1.0 is -2.5 or less, and (2) when the value of the log(f) is -4, the value of a log (log(tanδ)) of tanδ calculated by (G" / G') is 0 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hot melt composition. [Background technology]

[0002] In recent years, absorbent articles including sanitary materials such as paper diapers and sanitary napkins have been widely used. These absorbent articles use elastic laminates made of elastic members to prevent the absorbent articles from slipping off when worn.

[0003] Rubber thread, which is made of natural rubber or synthetic polymer in the form of a thread, is known as a stretchable member used in stretch laminates. Because rubber thread exhibits good stress when stretched, it is effective in preventing absorbent articles from slipping off when worn.

[0004] Also, a stretchable film containing a thermoplastic elastomer has been proposed as a stretchable member of a stretchable laminate provided in an absorbent article (see, for example, Patent Document 1). Patent Document 1 discloses a stretchable film containing a thermoplastic elastomer and a hydrophilic resin. This stretchable film provides a stretchable film with excellent moisture permeability and flexibility, suitable for absorbent articles such as sanitary napkins.

[0005] In addition, a hot melt stretchable adhesive composition has been proposed as a stretchable material that can be used in a hot melt adhesive applicator (see, for example, Patent Document 2). Patent Document 2 discloses a hot melt stretchable adhesive composition that contains a block copolymer containing an elastic polymer segment, which is one or more polymers selected from a butadiene polymer or a hydrogenated polymer of an isoprene polymer, or an ethylene propylene polymer, and a polystyrene polymer segment. This hot melt stretchable adhesive composition can be applied using a normal hot melt applicator, and since it itself has both adhesiveness and stretchability, a hot melt adhesive is provided that can easily form a gathered portion by laminating it with a substrate such as a nonwoven fabric. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2015-86367 A [Patent Document 2] Patent No. 2919385 Summary of the Invention [Problem to be solved by the invention]

[0007] However, when the above-mentioned rubber thread is used as a stretchable member for use in a stretch laminate, there is a problem that a linear pressure is applied to the human body, which may cause a feeling of pressure or a rash when worn. In addition, since multiple thin rubber threads are used in absorbent articles such as sanitary products, the rubber threads are prone to breaking during the manufacture of the absorbent article, which often makes it difficult to manufacture the absorbent article.

[0008] The stretchable film of Patent Document 1 solves the above-mentioned problems that arise when using rubber thread, since the human body is subjected to surface pressure. However, because the stretchable film is produced by molding resin using an extrusion device, it cannot be coated using a normal hot melt coating device, and there is a problem that the coatability (shape processability) is insufficient.

[0009] In addition, the hot melt elastic adhesive composition of Patent Document 2 can be applied using a normal hot melt coating device, improving the coatability of the elastic member, but the decrease in elasticity has not been sufficiently considered. When a sanitary material such as a disposable diaper is worn, the elastic member used in the sanitary material is kept in a stretched state at a temperature close to body temperature for a long time. Therefore, it is required that the decrease in elastic recovery is suppressed even when the elastic member is heated and kept in a stretched state.

[0010] In view of the above circumstances, the present invention aims to provide a hot melt composition that suppresses a decrease in stretch recovery and breakage even after being heated and held in an extended state, and has excellent coatability that can be coated with a normal hot melt coating device.

Means for Solving the Problems

[0011] As a result of intensive studies to achieve the above object, the present inventor has found that a hot melt composition containing a thermoplastic resin (A) and a plasticizer (B), which is subjected to dynamic viscoelasticity measurement under specific conditions, and in the master curve obtained with a reference temperature of 40°C, (1) the value of log(f) at the point where log(G'') is maximized in the range of -6.0 < log(f) < -1.0 is -2.5 or less, and (2) when the value of log(f) is -4, the value of the logarithm of tanδ (log(tanδ)) calculated by (G'' / G') is 0 or less. Based on this finding, the present invention has been completed.

[0012] That is, the present invention relates to the following hot melt composition. 1. A hot melt composition containing a thermoplastic resin (A) and a plasticizer (B), Dynamic viscoelasticity measurement is performed under the conditions of temperature -20 to 120°C and frequency (f) -0.2 to 2.0 Hz. For the logarithm of the measured storage modulus (G') (log(G')) and the logarithm of the measured loss modulus (G'') (log(G'')) with respect to the logarithm of the frequency (f) (log(f)), in the master curve obtained with a reference temperature of 40°C, (1) The value of log(f) at the point where log(G'') is maximized in the range of -6.0 < log(f) < -1.0 is -2.5 or less, and (2) When the value of log(f) is -4, the value of the logarithm of tanδ (log(tanδ)) calculated by (G'' / G') is 0 or less, A hot melt composition characterized by the above. 2. The hot melt composition according to item 1, having a melt viscosity at 180°C of 5,000 mPa·s or more and 45,000 mPa·s or less. 3. The hot melt composition according to item 1 or 2, wherein the content of the thermoplastic resin (A) is 40 to 75% by mass based on 100% by mass of the hot melt composition. 4. The hot melt composition according to any one of items 1 to 3, wherein the thermoplastic resin (A) is a styrene-based block copolymer. 5. The hot melt composition according to item 4, wherein the styrene-based block copolymer is a hydrogenated styrene-based block copolymer. 6. A stretchable laminate characterized in that a non-woven fabric is joined to at least one side of a film formed from the hot melt composition according to any one of items 1 to 5.

Advantages of the Invention

[0013] Even after the hot melt composition of the present invention is heated and held in an extended state, a decrease in stretch recovery and breakage are suppressed, and it can be applied with a normal hot melt coating apparatus and has excellent coatability.

Embodiments for Carrying Out the Invention

[0014] 1. Hot melt composition The hot melt composition of the present invention is a hot melt composition containing a thermoplastic elastomer (A) and a plasticizer (B), Dynamic viscoelasticity measurement is performed under the conditions of temperature -20 to 120°C and frequency (f) -0.2 to 2.0 Hz. For the logarithm (log(f)) of the frequency (f), the logarithm (log(G')) of the measured storage modulus (G') and the logarithm (log(G'')) of the measured loss modulus (G'') are plotted. In the master curve obtained with a reference temperature of 40°C, (1) The value of log(f) at the point where log(G'') is maximum in the range of -6.0 < log(f) < -1.0 is -2.5 or less, and (2) When the value of log(f) is −4, the value of the logarithm of tan δ (log(tan δ)) calculated by (G″ / G′) is equal to or less than 0. By virtue of having the above configurations (1) and (2), the hot melt composition of the present invention is able to suppress a decrease in stretch recovery even after it is heated and maintained in an elongated state, exhibit excellent stretch recovery, and is also able to suppress breakage.

[0015] The hot melt composition of the present invention can be suitably used as an elastic member for forming an elastic laminate for use in absorbent articles such as sanitary products.

[0016] In this specification, "warming" refers to bringing the temperature to about human body temperature, meaning about 35 to 42°C, preferably about 35.5 to 41.5°C, and more preferably about 36 to 41°C.

[0017] The master curve can be obtained by the following method. That is, the hot melt composition is heated and melted at 180°C, and dropped onto the release layer side of a release-treated PET film. Then, another release-treated PET film is laminated on the hot melt composition so that the release layer side is in contact with the hot melt composition. Then, the hot melt composition is compressed with a heat press heated to 120°C, and the thickness of the hot melt composition is adjusted to about 2 mm. After leaving the hot melt composition between the PET films at 23°C for 24 hours, the release film is removed to prepare a sample for dynamic viscoelasticity measurement.

[0018] Using this sample, dynamic viscoelasticity measurement is performed in the rotational shear mode of a dynamic viscoelasticity measuring device under the measurement conditions of a temperature range from -20°C to 120°C and a frequency range from 0.2 to 2.0 Hz. Specifically, under the condition of a constant temperature of -20°C, the storage modulus G' and the loss modulus G'' are measured in the rotational shear mode at a frequency range from 0.2 to 2.0 Hz. Similar measurements are performed every 10°C up to 120°C. The logarithms of the measured storage modulus G' and loss modulus G'' are taken and plotted against the logarithmic value of the frequency (log(f)). Next, with a reference temperature of 40°C, shift factors are set for log(G'), log(G''), and log(tanδ) (= log(G'' / G')), and while parallelly moving in the X-axis direction, master curves of log(G'), log(G''), and log(tanδ) are created such that they overlap each other.

[0019] In the obtained master curve of log(G''), the value of log(f) at the point where log(G'') becomes maximum in the range of -6.0 < log(f) < -1.0 is read and recorded. In the case where there is no point where log(G'') becomes maximum in the range of -6.0 < log(f) < -1.0 in the above master curve, the value of the point where log(G'') becomes maximum in the above range is read and recorded. Also, in the obtained master curve of log(tanδ), the value of log(tanδ) when log(f) is -4.0 and the value of log(tanδ) when log(f) is -4.0 are read and recorded.

[0020] Note that in the above master curve, the following relational expression holds between the frequency f (Hz) and the time s (seconds). f = 1 / 2πs Also, log(f) = -4.0 and log(f) = -3.0 correspond to 30 minutes and 3 minutes, respectively. The dynamic viscoelasticity measuring device is not particularly limited. For example, a rotational rheometer (trade name "AR-G2") manufactured by TA Instruments can be mentioned.

[0021] In the hot melt composition of the present invention, in the master curve obtained by the above method, the value of log(f) at the point where log(G'') is maximized in the range of -6.0 < log(f) < -1.0 is -2.5 or less. When the value of log(f) exceeds -2.5, the stretch recovery property of the hot melt composition after heating and holding decreases. The value of log(f) is preferably -2.7 or less, more preferably -2.9 or less. Further, the lower limit of the value of log(f) is not particularly limited, and in terms of further improving the coatability of the hot melt composition, it is preferably -6.0 or more, more preferably -5.8 or more.

[0022] In order to adjust the value of log(f) at the point where log(G'') is maximized in the range of -6.0 < log(f) < -1.0 to be smaller, the end block phase of the thermoplastic resin may be made stronger. Specifically, the value of log(f) can be adjusted to be smaller by methods such as using a thermoplastic resin with a high styrene content, reinforcing the styrene-based end block phase with an end block resin, and bonding the end block phases to each other. Further, the value of log(f) can also be adjusted to be smaller by methods such as using a thermoplastic resin with a high weight average molecular weight and increasing the content of the thermoplastic resin in the hot melt composition.

[0023] In the case where there is no point where log(G'') is maximized in the range of -6.0 < log(f) < -1.0 in the master curve, the value of log(f) at the point where log(G'') is maximized in the above range may be within the above range.

[0024] In the hot melt composition of the present invention, when the value of log(f) is −4 in the master curve obtained by the above method, the value of the logarithm of tan δ (log(tan δ)) calculated by (G″ / G′) is 0 or less. If the value of (log(tan δ)) exceeds 0, the stretch recovery property of the hot melt composition after heating and holding decreases. The value of (log(tan δ)) is preferably −0.05 or less, and more preferably −0.1 or less. There is no particular lower limit for the value of (log(tan δ)), and in terms of further improving the coatability of the hot melt composition, it is preferably −1.0 or more, and more preferably −0.9 or more.

[0025] When the value of log(f) is −4, the value of the logarithm of tan δ (log(tan δ)) calculated by (G″ / G′) can be adjusted to be smaller by making the end block phase of the thermoplastic resin stronger. Specifically, the value of the logarithm of tan δ (log(tan δ)) can be adjusted to be smaller by using a thermoplastic resin with a high styrene content, reinforcing the styrene-based end block phase with an end block resin, bonding the end block phases together, etc. Furthermore, the value of the logarithm of tan δ (log(tan δ)) can also be adjusted to be smaller by using a thermoplastic resin with a high weight average molecular weight, increasing the content of the thermoplastic resin in the hot melt composition, etc.

[0026] In the hot melt composition of the present invention, the difference between the value of log(tan δ) when log(f) is -4 and the value of log(tan δ) when log(f) is -3 is preferably 0.05 or more, more preferably 0.1 or more. By setting the difference within the above range, the stretch recovery property of the hot melt composition after heating and holding is further improved, and breakage is further suppressed. The upper limit of the difference is not particularly limited, and is preferably 0.6 or less, more preferably 0.5 or less, in that the deterioration of the stretch recovery property and the suppression of breakage of the hot melt composition are further improved.

[0027] (Thermoplastic resin (A)) The thermoplastic resin (A) is not particularly limited as long as the hot melt composition satisfies the above conditions (1) and (2), and is preferably a thermoplastic elastomer in terms of being more excellent in elasticity. In addition, a reactive thermoplastic resin can be used as the thermoplastic resin (A). An example of such a reactive thermoplastic resin is a thermoplastic resin containing a styrene-based block copolymer having a reactive polystyrene-based hard block in the molecule of the thermoplastic resin. By using such a thermoplastic resin and further containing a photopolymerization initiator, the hot melt composition can be irradiated with light such as ultraviolet light to react the reactive polystyrene-based hard block, crosslinking the molecules, and adjusting the properties such as dynamic viscoelasticity of the hot melt composition.

[0028] Examples of the thermoplastic elastomer include styrene-based block copolymers, olefin-based block copolymers, olefin-based random copolymers, urethane-based block copolymers, polyester-based block copolymers, etc. Among these, styrene-based block copolymers are preferred, and in particular, those containing hydrogenated styrene-based block copolymers, which are hydrogenated products of styrene-based block copolymers, are more preferred. The hydrogenated product of styrene-based block copolymers refers to block copolymers obtained by block copolymerizing vinyl aromatic hydrocarbons and conjugated diene compounds, and hydrogenating all or a part of the blocks based on the conjugated diene compounds in the resulting block copolymer.

[0029] Vinyl aromatic hydrocarbons are aromatic hydrocarbon compounds having vinyl groups.Specific examples of vinyl aromatic hydrocarbons include styrene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 1,3-dimethylstyrene, α-methylstyrene, vinylnaphthalene, vinylanthracene, etc., and among these, styrene is preferred.Vinyl aromatic hydrocarbons may be used alone or in combination of two or more.

[0030] The conjugated diene compound is a diolefin compound having at least one pair of conjugated double bonds.Specific examples of the conjugated diene compound include 1,3-butadiene, 2-methyl-1,3-butadiene (or isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene, and among these, 1,3-butadiene and 2-methyl-1,3-butadiene are preferred.The conjugated diene compound may be used alone or in combination of two or more.

[0031] In this specification, the hydrogenation ratio in a hydrogenated thermoplastic block copolymer, such as a hydrogenated product of a styrene-based block copolymer, is indicated by the "hydrogenation ratio". The "hydrogenation ratio" of a hydrogenated thermoplastic block copolymer refers to the ratio of ethylenically unsaturated double bonds that have been hydrogenated and converted to saturated hydrocarbon bonds, based on the total ethylenically unsaturated double bonds contained in the block based on a conjugated diene compound. The hydrogenation ratio can be measured by an infrared spectrophotometer, a nuclear magnetic resonance apparatus, or the like.

[0032] The hydrogenated styrene block copolymer may be a partially hydrogenated or fully hydrogenated product. Of these, a fully hydrogenated product is preferred. When the hydrogenated styrene block copolymer is fully hydrogenated, the heat stability of the hot melt composition is further improved. The hydrogenation rate of the hydrogenated styrene block copolymer is preferably about 100%.

[0033] The hydrogenated product of the styrene-based block copolymer is not particularly limited, and examples thereof include styrene-ethylene-butylene-styrene copolymer (SEBS), styrene-butylene-butadiene-styrene copolymer (SBBS), styrene-ethylene-butylene / styrene-styrene copolymer (SEB / SS), styrene-ethylene-propylene-styrene copolymer (SEPS), styrene-ethylene-ethylene-propylene-styrene copolymer (SEEPS), and styrene-ethylene-butylene-olefin crystalline copolymer (SEBC). By using the above-mentioned thermoplastic elastomer as the thermoplastic resin (A), the hot melt composition of the present invention is further suppressed from decreasing the elastic recovery and breaking even after being heated and held in an elongated state. Among these, styrene-ethylene-butylene-styrene copolymer and styrene-ethylene-butylene / styrene-styrene copolymer are preferred from the viewpoint of being more excellent in elastic recovery after being held at a temperature and being able to achieve both stress during elongation and good elongation.

[0034] The hydrogenated styrene block copolymers may be used alone or in combination of two or more.

[0035] The styrene-ethylene-butylene-styrene copolymer (SEBS) is a copolymer in which the terminal styrene units form the end block phase and the ethylene-butylene units form the midblock phase. By using a copolymer in which the midblock phase is a hydrogenated ethylene-butylene unit, the polarity difference with the styrene units in the endblock phase becomes more pronounced, and the styrene units in the endblock phase become stronger than in a copolymer in which the midblock phase is not hydrogenated. As a result, the stretch recovery of the hot melt composition can be further improved. Furthermore, since the midblock phase is hydrogenated, a hot melt composition with even better heat stability can be provided.

[0036] The styrene-ethylene-butylene-styrene copolymer may be a reactive styrene-ethylene-butylene-styrene copolymer containing a styrene-based block copolymer having a reactive polystyrene-based hard block in the molecule of the thermoplastic resin. By using a reactive styrene-ethylene-butylene-styrene copolymer and further containing a photopolymerization initiator, the hot melt composition can be irradiated with light such as ultraviolet light to react the reactive polystyrene-based hard block and crosslink the molecules, thereby adjusting the properties such as dynamic viscoelasticity of the hot melt composition. As such a reactive styrene-ethylene-butylene-styrene copolymer, a commercially available product can be used, and examples of the commercially available product include Septon V9827 manufactured by Kuraray Co., Ltd.

[0037] The styrene content of the styrene-ethylene-butylene-styrene copolymer is preferably 15 to 45% by mass, and more preferably 20 to 40% by mass, based on 100% by mass of the styrene-ethylene-butylene-styrene copolymer. When the lower limit of the styrene content is within the above range, the hot melt composition can have a further improved stretch recovery after elongation. When the upper limit of the styrene content is within the above range, the hot melt composition can be made softer and can exhibit even better elongation.

[0038] In this specification, the "styrene content" of a styrene-based block copolymer refers to the content (mass %) of the styrene block in the styrene-based block copolymer.

[0039] In the present specification, the method for calculating the styrene content in the styrene-based block copolymer is not particularly limited, and examples thereof include a method using proton nuclear magnetic resonance spectroscopy or infrared spectroscopy in accordance with JIS K6239.

[0040] The styrene-ethylene-butylene-styrene copolymer may be a commercially available product, such as G1650 manufactured by Kraton Polymers, MD1648 manufactured by Kraton Polymers, or Tuftec H1041 manufactured by Asahi Kasei Corporation.

[0041] The styrene-ethylene-butylene-styrene copolymer may be used alone or in combination of two or more. For example, a styrene-ethylene-butylene-styrene copolymer having a high styrene content and a styrene-ethylene-butylene-styrene copolymer having a low styrene content may be used in combination. When two or more types are used in combination, the styrene content of the entire styrene-ethylene-butylene-styrene copolymer may be calculated as an average value based on weight.

[0042] The styrene-ethylene-butylene / styrene-styrene copolymer (SEB / SS) is a styrene-ethylene-butylene-styrene copolymer in which the terminal styrene units form an end block phase and the ethylene-butylene units form a midblock phase, and in which styrene is also dispersed in the midblock phase. By using a copolymer in which styrene is dispersed in the midblock phase, even if the total styrene content of the styrene block copolymer is increased, the styrene block copolymer does not become too hard and exhibits good extensibility, so that a hot melt composition containing the styrene-ethylene-butylene / styrene-styrene copolymer can achieve both good extensibility and improved stress during elongation. Furthermore, by using a styrene-ethylene-butylene / styrene-styrene copolymer in which styrene is dispersed in the midblock phase for a hot melt composition, an increase in melt viscosity at low temperatures is suppressed, and the coatability of the hot melt composition can be further improved.

[0043] The method for preparing the styrene-ethylene-butylene / styrene-styrene copolymer is not particularly limited, and examples thereof include the method described in US Pat. No. 7,169,848.

[0044] The styrene content of the styrene-ethylene-butylene / styrene-styrene copolymer is preferably 20 to 60% by mass, more preferably 25 to 55% by mass, based on 100% by mass of the styrene-ethylene-butylene / styrene-styrene copolymer. When the lower limit of the styrene content is within the above range, the hot melt composition can have a further improved stretch recovery after elongation. When the upper limit of the styrene content is within the above range, the hot melt composition can be made softer and can exhibit even better elongation.

[0045] As the styrene-ethylene-butylene / styrene-styrene copolymer, commercially available products can be used, such as MD6951 and A1536 manufactured by Kraton Polymers.

[0046] The styrene-ethylene-butylene / styrene-styrene copolymer may be used alone or in combination of two or more. For example, a styrene-ethylene-butylene / styrene-styrene copolymer having a high styrene content and a styrene-ethylene-butylene / styrene-styrene copolymer having a low styrene content may be used in combination. When two or more types are used in combination, the styrene content of the entire styrene-ethylene-butylene / styrene-styrene copolymer may be calculated by the average value based on weight.

[0047] The styrene-ethylene-butylene-olefin crystalline copolymer (SEBC) is a block polymer of styrene-ethylene-butylene-olefin crystal. By using the styrene-ethylene-butylene-olefin crystalline copolymer, the hot melt composition has better elasticity recovery after heating and holding, and the coatability is improved, and the tensile strength and transparency are improved.

[0048] The method for producing the styrene-ethylene-butylene-olefin crystal copolymer is not particularly limited, and it can be produced by the following production method. That is, first, 1,3-butadiene is polymerized using an organolithium initiator, and then 1,3-butadiene is polymerized so that the 1,2-vinyl bond content is 30 to 70%, to produce block-shaped polybutadiene with different 1,2-vinyl bond contents. Next, a vinyl aromatic compound containing 90 mass% or more of styrene is added to the polybutadiene and polymerized to produce a block copolymer before hydrogenation. Next, the block copolymer before hydrogenation is hydrogenated by a known method to produce a styrene-ethylene-butylene-olefin crystal copolymer.

[0049] Examples of vinyl aromatic compounds include styrene, t-butylstyrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylstyrene, N,N-diethyl-p-aminoethylstyrene, and vinylpyridine. Among these, styrene and α-methylstyrene are preferred.

[0050] Examples of organolithium compounds used as organolithium initiators include n-butyllithium, sec-butyllithium, tert-butyllithium, propyllithium, amyllithium, and butyllithium / barium nonylphenoxide / trialkylaluminum / dialkylaminoethanol.

[0051] The styrene content of the styrene-ethylene-butylene-olefin crystalline copolymer is preferably 10 to 30% by mass, more preferably 15 to 25% by mass, based on 100% by mass of the styrene-ethylene-butylene-olefin crystalline copolymer. When the lower limit of the styrene content is within the above range, the hot melt composition can have a further improved stretch recovery after elongation. When the upper limit of the styrene content is within the above range, the hot melt composition can be made softer and can exhibit even better elongation.

[0052] As the styrene-ethylene-butylene-olefin crystalline copolymer, a commercially available product can be used, such as DYNARON 4600P manufactured by JSR Corporation.

[0053] The styrene-ethylene-butylene-olefin crystal copolymer may be used alone or in combination of two or more. For example, a styrene-ethylene-butylene-olefin crystal copolymer having a high styrene content and a styrene-ethylene-butylene-olefin crystal copolymer having a low styrene content may be used in combination. When two or more types are used in combination, the styrene content of the styrene-ethylene-butylene-olefin crystal copolymer may be calculated as an average value based on weight.

[0054] The content of the thermoplastic resin (A) in the hot melt composition of the present invention is preferably 40 to 75 mass%, more preferably 50 to 70 mass%, and more preferably 55 to 65 mass%, based on 100 mass% of the hot melt composition. By having the content of the thermoplastic resin (A) in the above range, the hot melt composition of the present invention has even better elasticity recovery after heating and is also excellent in coatability.

[0055] The styrene content of the thermoplastic resin (A) in the hot melt composition of the present invention is preferably 10 to 35 mass%, more preferably 12 to 25 mass%, based on 100 mass% of the thermoplastic resin (A). When the lower limit of the styrene content is within the above range, the hot melt composition can have a further improved stretch recovery after being kept at a temperature. When the upper limit of the styrene content is within the above range, the hot melt composition can be made softer and can exhibit a further improved extensibility.

[0056] The weight average molecular weight (Mw) of the thermoplastic resin (A) in the hot melt composition of the present invention is preferably 30,000 to 200,000, more preferably 40,000 to 150,000, and even more preferably 45,000 to 125,000. When the lower limit of the weight average molecular weight is in the above range, the hot melt composition can have a further improved stretch recovery after being kept at a temperature. When the upper limit of the weight average molecular weight is in the above range, the hot melt composition can be made softer and can exhibit a further improved extensibility.

[0057] The weight average molecular weight (Mw) of the thermoplastic resin is a measured value obtained by using a gel permeation chromatography measuring device and converting it into standard polystyrene.

[0058] The weight average molecular weight (Mw) in this specification can be measured, for example, using the following measuring device and under the following measuring conditions. Measurement device: Waters product name "ACQUITY APC" Measurement conditions: Column ·ACQUITY APCXT45 1.7μm×1 piece ·ACQUITY APCXT125 2.5μm×1 piece ·ACQUITY APCXT450 2.5μm×1 piece Mobile phase: Tetrahydrofuran 0.8mL / min Sample concentration: 0.2% by mass Detector: Refractive index (RI) detector Standard material: polystyrene (Waters, molecular weight: 266-1,800,000) Column temperature: 40°C RI detector temperature: 40℃

[0059] (Plasticizer (B)) The hot melt composition of the present invention contains a plasticizer (B). The plasticizer (B) is preferably liquid at 23°C. In this specification, "liquid" refers to a state exhibiting fluidity. The pour point of such a plasticizer (B) is preferably 23°C or lower, more preferably 10°C or lower.

[0060] In this specification, the pour point is a value measured by a measurement method in accordance with JIS K2269.

[0061] The plasticizer (B) is not particularly limited, and examples thereof include paraffinic process oil, naphthenic process oil, aromatic process oil, liquid paraffin oil, hydrocarbon synthetic oil, etc. Among them, paraffinic process oil, naphthenic process oil, liquid paraffin oil, and hydrocarbon synthetic oil are preferred from the viewpoint of excellent heat stability, and hydrocarbon synthetic oil is more preferred from the viewpoint of further improving the stretch recovery property of the hot melt composition after heating and holding.

[0062] As the paraffin-based process oil, commercially available products can be used, such as PW-32 and PS-32 manufactured by Idemitsu Kosan Co., Ltd.

[0063] As the naphthenic process oil, commercially available products can be used, such as Diana Fresia N28 manufactured by Idemitsu Kosan Co., Ltd., Diana Fresia U46 manufactured by Idemitsu Kosan Co., Ltd., and Nyflex 222B manufactured by Nynas Corporation.

[0064] As the liquid paraffin oil, commercially available products can be used, such as P-100 manufactured by MORESCO and Kaydol manufactured by Sonneborn.

[0065] As the synthetic hydrocarbon oil, commercially available products can be used, such as LUCANT HC-10 and LUCANT HC-20 manufactured by Mitsui Chemicals.

[0066] The above plasticizers may be used alone or in combination of two or more.

[0067] The content of the plasticizer (B) in the hot melt composition of the present invention is preferably 5 to 60 mass%, more preferably 10 to 50 mass%, and even more preferably 12 to 45 mass%, based on 100 mass% of the hot melt composition. By setting the upper limit of the content of the plasticizer (B) within the above range, the hot melt composition can have a further improved stretch recovery after being kept at a temperature. By setting the lower limit of the content of the plasticizer (B) within the above range, the melt viscosity of the hot melt composition can be further reduced, and the coatability of the hot melt composition can be further improved.

[0068] (Wax (C)) The hot melt composition of the present invention may contain a wax (C) having at least one group selected from the group consisting of a carbonyl group, a carboxyl group, and a carboxylic anhydride group in the molecule. The wax (C) is preferably solid at 23°C. In this specification, "solid" refers to a state that does not exhibit fluidity. The softening point of such wax (C) is preferably 23°C or higher, more preferably 30°C or higher, and even more preferably 40°C or higher.

[0069] In this specification, the softening point is a value measured by a measurement method in accordance with ASTM D-3954.

[0070] Waxes having at least one group selected from the group consisting of carbonyl groups, carboxyl groups, and carboxylic anhydride groups in the molecule have high polarity, and therefore have good compatibility with styrene-based block copolymers and good dispersion in the composition. Therefore, compared with waxes not having carbonyl groups, carboxyl groups, and carboxylic anhydride groups in the molecule, the heat stability of the hot melt composition can be further improved. Waxes (C) having at least one group selected from the group consisting of carbonyl groups, carboxyl groups, and carboxylic anhydride groups in the molecule are not particularly limited, and examples thereof include vinyl acetate wax, acrylic acid wax, and maleic anhydride modified wax. Among them, vinyl acetate wax is preferred from the viewpoint of better heat stability.

[0071] As the vinyl acetate wax, commercially available products can be used, such as AC-400 manufactured by Honeywell and AC-430 manufactured by Honeywell.

[0072] As the acrylic acid wax, commercially available products can be used, such as AC-540 and AC-580 manufactured by Honeywell.

[0073] As the maleic anhydride modified wax, commercially available products can be used, such as AC-573P and AC-577P manufactured by Honeywell, and MAW-0300 manufactured by Nippon Seiro Co., Ltd.

[0074] The wax having at least one group selected from the group consisting of a carbonyl group, a carboxyl group, and a carboxylic anhydride group in the molecule may be used alone or in combination of two or more kinds.

[0075] The content of the wax (C) in the hot melt composition of the present invention is preferably 5 to 40 mass%, more preferably 5 to 35 mass%, and even more preferably 10 to 30 mass%, based on 100 mass% of the hot melt composition. When the lower limit of the wax (C) content is within the above range, the stress of the hot melt composition when elongated twice is further improved. When the upper limit of the wax (C) content is within the above range, the stretch recovery property of the hot melt composition after heating and holding is further improved.

[0076] (Other additives) The hot melt composition of the present invention may contain other additives to the extent that the purpose of the present invention is not essentially hindered. Examples of the other additives include antioxidants, ultraviolet absorbers, tackifier resins, photopolymerization initiators, liquid rubbers, and fine particle fillers.

[0077] Antioxidants include 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(4'-hydroxy-3',5'-di-t-butylphenyl)propionate, 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 2,4-bis(octylthiomethyl)-o-cresol, 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2,4-di-t-amyl-6-[1-(3,5-di-t-amyl-2-hydroxyphenyl)ethyl ester, and 2,2'-methylenebis(4-ethyl-6-t-butylphenol). hindered phenol-based antioxidants such as 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)] acrylate, tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl) propionate] methane; sulfur-based antioxidants such as dilauryl thiodipropionate, lauryl stearyl thiodipropionate, pentaerythritol tetrakis(3-lauryl thiopropionate); phosphorus-based antioxidants such as tris(nonylphenyl) phosphite, tris(2,4-di-t-butylphenyl) phosphite, etc. The antioxidants may be used alone or in combination of two or more.

[0078] The content of the antioxidant in the hot melt composition of the present invention is preferably 0.01 to 2 mass%, more preferably 0.05 to 1.5 mass%, and even more preferably 0.1 to 1 mass%, based on 100 mass% of the hot melt composition. When the content of the antioxidant is 0.01 mass% or more, the thermal stability of the hot melt composition is further improved. When the content of the antioxidant is 2 mass% or less, the odor of the hot melt composition is reduced.

[0079] Examples of the ultraviolet absorbent include benzotriazole-based ultraviolet absorbents such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-t-butylphenyl)benzotriazole, and 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole; benzophenone-based ultraviolet absorbents such as 2-hydroxy-4-methoxybenzophenone; salicylic acid ester-based ultraviolet absorbents; cyanoacrylate-based ultraviolet absorbents; and hindered amine-based light stabilizers. The ultraviolet absorbent may be used alone or in combination of two or more.

[0080] The content of the ultraviolet absorber in the hot melt composition of the present invention is preferably 0.01 to 2 mass%, more preferably 0.05 to 1.5 mass%, and even more preferably 0.1 to 1 mass%, based on 100 mass% of the hot melt composition. When the content of the ultraviolet absorber is 0.01 mass% or more, the weather resistance of the hot melt composition is improved. When the content of the ultraviolet absorber is 2 mass% or less, the odor of the hot melt composition is reduced.

[0081] Examples of the tackifier resin include natural rosin, modified rosin, glycerol ester of natural rosin, glycerol ester of modified rosin, pentaerythritol ester of natural rosin, pentaerythritol ester of modified rosin, copolymer of natural terpene, three-dimensional polymer of natural terpene, hydrogenated derivative of copolymer of natural terpene, terpene resin, hydrogenated derivative of phenol-based modified terpene resin; petroleum resin such as C5-based petroleum resin, C9-based petroleum resin, C5C9-based petroleum resin, dicyclopentadiene-based petroleum resin, and partially hydrogenated petroleum resin and fully hydrogenated petroleum resin obtained by adding hydrogen to these petroleum resins. As the tackifier resin, petroleum resin, partially hydrogenated petroleum resin, and fully hydrogenated petroleum resin are preferred, and partially hydrogenated petroleum resin and fully hydrogenated petroleum resin are more preferred, in terms of excellent odor and thermal stability of the hot melt composition. These tackifier resins may be used alone or in combination of two or more.

[0082] The Ring and Ball softening point temperature of the tackifier resin is preferably 80° C. or higher, and more preferably 90° C. or higher, in order to provide a hot melt composition with even better elasticity and thermal stability. The Ring and Ball softening point temperature of the tackifier resin is preferably 125° C. or lower, and more preferably 120° C. or lower, in order to provide a hot melt composition with even better flexibility and to further suppress embrittlement. In this specification, the Ring and Ball softening point temperature of the tackifier resin is a value measured in accordance with JIS K2207.

[0083] The content of the tackifier resin in the hot melt composition of the present invention is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on 100% by mass of the hot melt composition. When the content of the tackifier resin is 30% by mass or less, the hot melt composition does not become too hard, and the stretch recovery after elongation is further improved.

[0084] Examples of the photopolymerization initiator include ultraviolet polymerization initiators. When the hot melt composition of the present invention contains a styrene-based block copolymer having a reactive polystyrene-based hard block in the molecule as the thermoplastic resin (A), the hot melt composition further contains a photopolymerization initiator, so that the hot melt composition can be irradiated with light such as ultraviolet light to react the reactive polystyrene-based hard block and crosslink the molecules, thereby adjusting the properties of the hot melt composition such as dynamic viscoelasticity. When the hot melt composition is irradiated with ultraviolet light, the irradiation intensity of the ultraviolet light is 50 to 1,000 mW / cm. 2 The cumulative light quantity is preferably about 1,000 to 15,000 mJ / cm 2 The photopolymerization initiator may be used alone or in combination of two or more kinds.

[0085] Examples of the liquid rubber include liquid polybutene, liquid polybutadiene, liquid polyisoprene, and hydrogenated resins thereof. The liquid rubber may be used alone or in combination of two or more kinds.

[0086] The content of the liquid rubber in the hot melt composition of the present invention is preferably 1 to 20% by mass, more preferably 2 to 15% by mass, and even more preferably 3 to 10% by mass, based on 100% by mass of the hot melt composition. When the content of the liquid rubber is 1% by mass or more, the melt viscosity of the hot melt composition decreases, and the coatability is further improved. When the content of the liquid rubber is 20% by mass or less, the hot melt composition does not become too soft, and the stretch recovery is further improved.

[0087] The particulate filler is not particularly limited, and examples thereof include calcium carbonate, kaolin, talc, titanium oxide, mica, styrene beads, etc. The particulate filler may be used alone or in combination of two or more kinds.

[0088] The hot melt composition of the present invention preferably has a melt viscosity at 180°C of 45,000 mPa·s or less, more preferably 28,000 mPa·s or less, and even more preferably 22,000 mPa·s or less. When the upper limit of the melt viscosity is within the above range, the coatability of the hot melt composition is further improved. In addition, the lower limit of the melt viscosity at 180°C of the hot melt composition is not particularly limited, and may be about 5,000 mPa·s.

[0089] In this specification, the "melt viscosity" refers to the viscosity of a hot melt composition in a molten state at a certain temperature. For example, the melt viscosity at 180°C may be measured by heating and melting the hot melt composition, and measuring the viscosity of the molten composition at 180°C using a Brookfield RVT viscometer (spindle No. 29).

[0090] The hot melt composition of the present invention is produced by a known method, for example, by feeding the thermoplastic resin (A), the plasticizer (B), and optionally wax and various additives into a twin-arm kneader heated to 150° C. and melt-kneading the mixture while heating.

[0091] The hot melt composition of the present invention is solid usually in the temperature range of 0 to 60° C., particularly at room temperature of 23° C., and exhibits elasticity, and therefore can be used for various applications as an elastic hot melt composition.

[0092] The applications of the hot melt composition of the present invention are not particularly limited, and examples thereof include absorbent articles including sanitary materials, hospital gowns, masks, etc. Specific examples of the sanitary materials include disposable diapers, sanitary napkins, etc.

[0093] The hot melt composition of the present invention is suitable for use as a stretchable film and a stretchable laminate including a stretchable member. For example, such a stretchable laminate includes a stretchable laminate having a nonwoven fabric bonded to at least one side of a film formed from the hot melt composition. Such a stretchable laminate is also one aspect of the present invention.

[0094] Applications of the elastic laminate are not particularly limited, and examples thereof include absorbent articles including sanitary materials, hospital gowns, masks, etc. Specific examples of the sanitary materials include disposable diapers, sanitary napkins, etc. EXAMPLES

[0095] Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0096] The raw materials used in the examples and comparative examples are as follows.

[0097] Styrenic block copolymer (A1) : Styrene-ethylene-butylene / styrene-styrene (SEB / SS) copolymer: Kraton Polymers MD6951 (styrene content 34% by mass, Mw=100,000) Styrene-based block copolymer (A2) : Styrene-ethylene-butylene-styrene (SEBS) copolymer: Kraton Polymers MD1648 (styrene content 20% by mass, Mw=54,000) Styrenic block copolymer (A3) : Styrene-ethylene-butylene-olefin crystalline copolymer (SEBC) JSR DYNARON 4600P (styrene content 20% by mass) Styrenic block copolymer (A4) : Styrene-ethylene-butylene-styrene (SEBS) copolymer: Asahi Kasei Corporation, Tuftec H1041 (styrene content 30% by mass, Mw=61,000) Styrenic block copolymer (A5) : Styrene-ethylene-butylene-styrene (SEBS) copolymer (Kuraray Co., Ltd. Septon V9827) (styrene content 30% by mass, contains reactive polystyrene hard blocks within the molecule)

[0098] Plasticizer (B) : ·Hydrocarbon synthetic oil (B1) Mitsui Chemicals LUCANT HC-10 (pour point -32.5℃) Liquid paraffin oil (B2) Kaydol manufactured by Sonneborn (pour point -21°C)

[0099] Tackifier : Endblock resin: Mitsui Chemicals FTR-0120

[0100] Photoinitiator Alkylphenone photoinitiator: BASF IRGACURE184

[0101] Antioxidants : Phenolic antioxidant: BASF IRGANOX1010

[0102] Examples and Comparative Examples The above-mentioned raw materials were charged into a stirring kneader equipped with a heating device in the amounts shown in Table 1. The materials were kneaded while being heated at 150°C for 90 minutes to produce a hot melt composition. Note that Example 5 and Comparative Example 2 have the same composition, but in Example 5, the hot melt composition was irradiated with ultraviolet light to react the reactive polystyrene hard block of the styrene block copolymer and crosslink the molecules to adjust the properties of the hot melt composition. The irradiation intensity of ultraviolet light in Example 5 was 500mW / cm. 2 , the cumulative light intensity is 1000mJ / cm 2 It was.

[0103] The properties of the obtained hot melt composition were evaluated under the following measurement conditions.

[0104] (180℃ Melt Viscosity) The hot melt composition was heated to melt, and the viscosity of the molten composition at 180° C. was measured using a Brookfield RVT viscometer (spindle No. 29).

[0105] (Coatability) The hot melt composition was put into a melt tank heated to 180 to 190°C, discharged from a slot nozzle heated to 180 to 190°C, and contact-coated onto a release-treated PET film. In Example 5, after contact coating, the hot melt composition was irradiated with ultraviolet light under the above conditions to crosslink the molecules, thereby adjusting the properties of the hot melt composition. The coatability of the hot melt composition was visually observed and evaluated according to the following evaluation criteria. ◎: Coating can be done evenly at a coating temperature of 180℃. ◯: Coating can be performed without unevenness at a coating temperature of 190°C. △: At a coating temperature of 190°C, some coating unevenness was observed, but this did not cause any problems in use. ×: Significant unevenness in application was observed, or the desired amount of hot melt composition was not dispensed.

[0106] (Return rate) Preparation of test specimens The hot melt composition was applied at a coating temperature of 180 to 190°C at a rate of 50 g / m2 onto the release layer side of a release-treated PET film. 2 The coating amount was 1000g. The coating width was 80mm. Next, the laminate was laminated with a release paper that had been subjected to a release treatment on one side to prepare a laminate. The obtained laminate was cut to a length of 85mm in the MD direction. The PET film and the release paper of the laminate were peeled off to prepare a test piece of the hot melt composition with a length of 85mm and a width of 80mm.

[0107] Measurement of return rate A test box with an open top was prepared. The length of the opening was 170 mm. The test piece prepared as described above was stretched in the length direction (MD direction) to a length of 170 mm, and both ends were fixed to the opening of the test box, and the test piece was held in the stretched state. The test box with both ends of the test piece fixed was placed in a thermostatic chamber at 40°C and left to stand for 1 hour. Next, the test piece was removed from the test box, and the length of the test piece after the test was measured. The return rate was calculated by the following formula. Return rate (%) = length of test piece after test (mm) / length of test piece before test (85 mm) x 100

[0108] (Viscoelasticity master curve) The hot melt composition was heated and melted at 180°C and dropped onto the release layer side of the release-treated PET film. Then, another release-treated PET film was laminated on the hot melt composition so that the release layer side was in contact with the hot melt composition. Then, it was compressed with a heat press heated to 120°C, and the thickness of the hot melt composition was adjusted to about 2 mm. After the hot melt composition was sandwiched between the PET films and left at 23°C for 24 hours, the release film was removed to prepare a sample for dynamic viscoelasticity measurement.

[0109] Using this sample, dynamic viscoelasticity measurements were performed in the rotational shear mode of a dynamic viscoelasticity measuring device under the measurement conditions of a temperature range from -20°C to 120°C and a frequency range from 0.2 to 2.0 Hz. Specifically, the storage modulus G' and the loss modulus G'' were measured in the rotational shear mode at a constant temperature of -20°C and a frequency range from 0.2 to 2.0 Hz. Similar measurements were performed every 10°C up to 120°C. The logarithms of the measured storage modulus G' and loss modulus G'' were plotted against the logarithm of the frequency value (log(f)). Next, with a reference temperature of 40°C, shift factors were set for log(G'), log(G''), and log(tanδ)(=log(G'' / G')), and while parallelly moving them in the X-axis direction, master curves of log(G'), log(G''), and log(tanδ) were created so that they overlapped each other.

[0110] In the obtained master curve of log(G''), the value of log(f) at the point where log(G'') in the range of -6.0 < log(f) < -1.0 reaches a maximum was read and recorded. Also, in the obtained master curve of log(tanδ), the value of log(tanδ) when log(f) is -4.0 and the value of log(tanδ) when log(f) is -4.0 were read and recorded.

[0111] Note that in the above master curve, the following relational expression holds between the frequency f (Hz) and the time s (seconds). f = 1 / 2πs Also, log(f) = -4.0 and log(f) = -3.0 correspond to 30 minutes and 3 minutes, respectively. Note that as the dynamic viscoelasticity measuring device, a rotational rheometer (trade name "AR-G2") manufactured by TA Instruments was used.

[0112] The results are shown in Table 1.

[0113]

Table 1

Claims

1. A hot melt composition comprising a thermoplastic resin (A) and a plasticizer (B), The thermoplastic resin (A) is at least one selected from the group consisting of styrene-ethylene-butylene-styrene copolymer (SEBS), styrene-ethylene-butylene / styrene-styrene copolymer (SEB / S-S), and styrene-ethylene-butylene-olefin crystalline copolymer (SEBC); The styrene content of the styrene-ethylene-butylene-styrene copolymer (SEBS) is 15 to 45% by mass, with the styrene-ethylene-butylene-styrene copolymer (SEBS) being 100% by mass, The styrene content of the styrene-ethylene-butylene / styrene-styrene copolymer (SEB / S-S) is 20 to 60 mass% based on 100 mass% of the styrene-ethylene-butylene / styrene-styrene copolymer (SEB / S-S), The styrene content of the styrene-ethylene-butylene-olefin crystalline copolymer (SEBC) is 10 to 30 mass%, assuming that the styrene-ethylene-butylene-olefin crystalline copolymer (SEBC) is 100 mass%, The plasticizer (B) is at least one selected from the group consisting of paraffinic process oil, naphthenic process oil, aromatic process oil, liquid paraffin oil, and hydrocarbon synthetic oil; The content of the thermoplastic resin (A) is 40 to 75% by mass, based on 100% by mass of the hot melt composition; The content of the plasticizer (B) is 5 to 60% by mass, based on 100% by mass of the hot melt composition. Dynamic viscoelasticity measurements were performed under conditions of a temperature of −20 to 120° C. and a frequency (f) of −0.2 to 2.0 Hz, and the logarithm (log(G')) of the measured storage modulus (G') and the logarithm (log(G'')) of the measured loss modulus (G'') were plotted against the logarithm (log(f)) of the frequency (f). In the master curve obtained with the reference temperature of 40° C., (1) The value of log(f) at the point where log(G″) is maximized in the range of −6.0<log(f)<−1.0 is −2.5 or less, and (2) When the value of log(f) is −4, the value of the logarithm of tan δ (log(tan δ)) calculated by (G″ / G′) is 0 or less. A hot melt composition comprising:

2. 2. The hot melt composition according to claim 1, having a melt viscosity at 180°C of 5,000 mPa·s or more and 45,000 mPa·s or less.

3. A hot melt composition as described in claim 1 or 2, wherein the total content of the thermoplastic resin (A) and the plasticizer (B) is 45 to 99.5 mass %, with the hot melt composition being 100 mass %.

4. 4. An elastic laminate comprising a film formed from the hot melt composition according to claim 1 and a nonwoven fabric bonded to at least one surface of the film.

Citation Information

Patent Citations

  • Hot-melt thermoplastic elastomer composition and article containing same

    JP2006502291A

  • Low applied temperature elastic adhesive

    JP2007525575A

  • Substrates containing adhesion-promoting additives and articles made therefrom

    JP2008505988A

  • Stretchable film lamination adhesive

    JP2014514390A

  • Stretchable film

    JP2015086367A