Sacrificial capping layer for passivation using plasma-based implantation process
A sacrificial capping layer on semiconductor workpieces mitigates etching during plasma-based implantation, ensuring device reliability and enabling deeper ion penetration, thus addressing the etching challenges in advanced transistors.
Patent Information
- Application Number
- JP2023504155
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-22
- Filing Date
- 2021-06-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-06-24
AI Technical Summary
Plasma-based implantation processes for semiconductor workpieces face challenges due to excessive etching caused by radicals and excited species, which adversely affect device performance and reliability, particularly in advanced transistors with high germanium concentration SiGe films.
A sacrificial capping layer is applied on the workpiece surface to protect it from etching during ion implantation, using materials like silicon dioxide, silicon nitride, or silicon oxynitride, which are etched at a slower rate than the underlying workpiece, allowing passivating ions to penetrate while minimizing surface damage.
The sacrificial capping layer effectively reduces etching of the workpiece surface, preserving the integrity of the semiconductor devices and enabling deeper implantation of passivating ions without significant time or cost addition to the manufacturing process.
Smart Images

Figure 0007559209000001 
Figure 0007559209000002 
Figure 0007559209000003
Abstract
Description
[Technical field]
[0001] This application claims priority to U.S. Patent Application No. 16 / 935,774, filed July 22, 2020, the disclosure of which is incorporated herein by reference in its entirety.
[0002] Embodiments of the present disclosure relate to systems and methods for passivating a workpiece using a plasma chamber, and more particularly to passivating a workpiece using implantation while minimizing etching of the workpiece. [Background technology]
[0003] Semiconductor workpieces are often implanted with dopant species to produce desired electrical conductivity. Plasma implantation is an effective method of doping or otherwise modifying the surface of semiconductor devices to form devices such as transistors.
[0004] As feature sizes continue to get smaller, new issues arise that affect the performance and reliability of these smaller transistors. For example, for advanced transistors, gate reliability, specifically negative bias temperature instability (NBTI), is one of the critical parameters for device performance and reliability. Gate oxide reliability issues become even more critical as the industry moves to more advanced channel materials, such as high germanium concentration SiGe films.
[0005] Gate oxide reliability is primarily related to defects and trap states at the gate oxide interface, and performance can be enhanced by passivating these defects. For example, these defects can be passivated using nuclear species such as hydrogen, deuterium, and fluorine.
[0006] These species can be introduced using a number of different processes. In certain embodiments, ion implantation is used to introduce these species. There are several advantages to this approach because high doping levels can be achieved at high dose rates, which allows for cost of ownership advantages, especially at low implant energies.
[0007] However, implantation of workpieces using plasma-based processes can be a challenge due to the presence of radicals and excited species along with ions during the implantation process, which can lead to excessive etching of the surface layer and thus adversely affecting device performance.
[0008] It would therefore be beneficial to have an apparatus and method that allows for the implantation of species to passivate a workpiece without etching the surface of the workpiece, and further, it would be beneficial if the method did not add a significant amount of time or cost to the overall semiconductor manufacturing process. Summary of the Invention
[0009] An apparatus and method for processing a workpiece is disclosed in which a sacrificial capping layer is created on the top surface of the workpiece. The workpiece is then subjected to an ion implantation process in which select species are used to passivate the workpiece. While the implantation process is ongoing, radicals and excited species etch the sacrificial capping layer. This reduces the amount of etching the workpiece experiences. In certain embodiments, the thickness of the sacrificial capping layer is selected based on the total time used for the implantation process and the etch rate. The total time used for the implantation process may be a function of the desired dose, bias voltage, plasma power, and other parameters. In some embodiments, the sacrificial capping layer is applied prior to the implantation process. In other embodiments, material is added to the sacrificial capping layer during the implantation process.
[0010] According to one embodiment, a method for passivating a portion of a workpiece is disclosed. The method includes placing a workpiece in a plasma chamber; applying a sacrificial capping layer to an upper surface of the workpiece; generating a plasma in the plasma chamber including a passivating species, the passivating species being selected from the group consisting of hydrogen, deuterium, fluorine, and a mixed gas containing hydrogen, deuterium, or fluorine as a diluent or primary process gas; generating the plasma in which ions, radicals, and excited molecules of the passivating species are generated; performing an implantation process in which ions of the passivating species are implanted through the sacrificial capping layer into the portion by applying a bias voltage to the workpiece, during the implantation process, the radicals and excited molecules etch the sacrificial capping layer; and terminating the implantation process when a desired dose of the passivating species has been implanted, wherein at the end of the implantation process, the thickness of the sacrificial capping layer is less than 5 angstroms or all of the sacrificial capping layer has been completely removed and less than 10 angstroms of the workpiece has been etched. In certain embodiments, the sacrificial capping layer is applied in the plasma chamber during the capping period by introducing a capping species and generating a plasma containing the capping species while the bias voltage is disabled. In some embodiments, the capping period precedes the implantation process. In some embodiments, an additional sacrificial capping layer is applied during the implantation process by flowing the capping species into the plasma chamber. In some further embodiments, the flow of the capping species is continuous throughout the implantation process. In some further embodiments, the flow of the capping species is pulsed during the implantation process. In some further embodiments, the bias voltage is varied as the capping species is flowing into the plasma chamber during the implantation process.In certain embodiments, the implantation process is terminated after a predetermined time, the predetermined time being determined based on the passivating species and the desired dose of the passivating species. In some embodiments, an alarm is generated if the output of the metrology system indicates that the workpiece is being etched. In certain embodiments, the implantation process is terminated based on the output from the metrology system indicating that the workpiece is being etched. In certain embodiments, the initial thickness of the sacrificial capping layer is determined based on the etch rate of the sacrificial capping layer and the total duration of the implantation process. In some further embodiments, the initial thickness is adjusted based on chamber metrology, the number of workpieces processed, or the hours of operation to compensate for varying etch rates. In certain embodiments, the thickness of the sacrificial capping layer is between 5 Angstroms and 100 Angstroms. In certain embodiments, when a bias voltage is applied, the bias voltage is a pulsed DC voltage between 0.1 kV and 10 kV.
[0011] According to another embodiment, a method of passivating a portion of a workpiece is disclosed. The method includes applying a sacrificial capping layer on an upper surface of the workpiece in a chamber, the sacrificial capping layer having a thickness between 5 angstroms and 100 angstroms; placing the workpiece in a plasma chamber, the plasma chamber being different from the above-mentioned chamber; generating a plasma in the plasma chamber including a passivating species, the passivating species being selected from the group consisting of hydrogen, deuterium, fluorine, and a gas mixture containing hydrogen, deuterium, or fluorine as a diluent or primary process gas, generating the plasma in which ions, radicals, and excited molecules of the passivating species are generated; performing an implantation process in which ions of the passivating species are implanted through the sacrificial capping layer into the above-mentioned portion by applying a bias voltage to the workpiece, during the implantation process the radicals and excited molecules etch the sacrificial capping layer; and terminating the implantation process when a desired dose of the passivating species has been implanted. In certain embodiments, the chamber heats the workpiece to a temperature near the temperature of the implantation process and grows a sacrificial capping layer by flowing gas while the workpiece is heated.
[0012] According to another embodiment, a method of passivating a portion of a workpiece is disclosed. The method includes flowing a capping species into a plasma chamber in which a workpiece is disposed; flowing the capping species; energizing the capping species to generate a plasma, wherein no bias voltage is applied to the workpiece during the capping period to produce a sacrificial capping layer on an upper surface of the workpiece; energizing the capping species; flowing a passivating species into the plasma chamber, wherein the passivating species is selected from the group consisting of hydrogen, deuterium, fluorine, and gas mixtures containing hydrogen, deuterium, or fluorine as diluents or primary process gases; flowing the passivating species; and performing an implantation process to implant passivating ions into the workpiece, the implantation process being defined as a period of time during which a bias voltage is applied to the workpiece while a plasma containing the passivating species is generated; performing the implantation process; adding material to the sacrificial capping layer by flowing the capping species into the plasma chamber during the implantation process; and terminating the implantation process. In certain embodiments, the implantation process is terminated when a desired dose of passivating ions is implanted. In certain embodiments, at the end of the implantation process, the thickness of the sacrificial capping layer is less than 5 angstroms, or all of the sacrificial capping layer has been completely removed and less than 10 angstroms of the workpiece has been etched. In certain embodiments, the flow of the capping species is continuous throughout the implantation process. In certain embodiments, the flow of the capping species is pulsed during the implantation process. In some further embodiments, the bias voltage is varied as the capping species is flowing into the plasma chamber during the implantation process. In certain embodiments, the amount of material added is varied based on chamber metrology, number of workpieces being processed, or number of hours of operation to compensate for varying etch rates.In some further embodiments, the capping species flows into the plasma chamber through a mass flow controller, and the amount of material is manipulated by adjusting the flow rate of the capping species, the frequency at which the mass flow controller is operated, or the duty cycle of the mass flow controller.
[0013] For a better understanding of the present disclosure, reference is made to the accompanying drawings, which are incorporated herein by reference. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 illustrates an ion source according to one embodiment. [Diagram 2] FIG. 2 illustrates the interactions between a sacrificial capping layer, ions, and radicals. [Figure 3A] 13A-13C show timing diagrams for capping periods and injection processes according to different embodiments. [Figure 3B] 13A-13C show timing diagrams for capping periods and injection processes according to different embodiments. [Figure 3C] 13A-13C show timing diagrams for capping periods and injection processes according to different embodiments. [Figure 4] FIG. 13 shows a flow chart that may be used to determine the initial thickness of a sacrificial capping layer. [Figure 5A] FIG. 1 illustrates an exemplary transistor that may utilize a sacrificial capping layer. [Figure 5B] FIG. 1 illustrates an exemplary transistor that may utilize a sacrificial capping layer. [Figure 6] FIG. 13 shows a timing diagram for an implantation process for an embodiment in which a sacrificial capping layer is applied outside the plasma chamber. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] FIG. 1 shows a cross-section of an embodiment of a plasma chamber 105 of an ion source 100 that may be used according to the present disclosure. The ion source 100 includes a plasma chamber 105 defined by a number of plasma chamber walls 107 that may be constructed of aluminum, graphite, or another suitable material. The plasma chamber 105 may be supplied with one or more feed gases stored in one or more feed gas containers 170a, 170b that enter the plasma chamber 105 through a gas baffle 175. Mass flow controllers 171a, 171b may be used to regulate the flow of feed gas from the feed gas containers 170a, 170b, respectively, into the plasma chamber 105. The feed gas may be energized by an RF antenna 120 or another plasma generating mechanism. The RF antenna 120 is in electrical communication with an RF power supply 121 that provides power to the RF antenna 120. A dielectric window 125, such as a quartz or alumina window, may be disposed between the RF antenna 120 and the interior of the plasma chamber 105.
[0016] The workpiece 10 is disposed in the plasma chamber 105 on a platen 130. The platen 130 is in electrical communication with a bias power supply 135 that is used to negatively bias the platen 130 for a certain period of time such that positive ions are attracted toward the workpiece 10.
[0017] Additionally, the platen 130 may also be heated. In one embodiment, a heated fluid may flow through channels embedded in the platen 130. In another embodiment, a heating element, such as a resistive element, may be embedded in the platen to heat it.
[0018] A controller 160 may be in communication with the bias power supply 135, the RF power supply 121, and mass flow controllers 171a, 171b that control the flow of feed gas into the plasma chamber 105. The controller 160 may include a processing unit, such as a microcontroller, a personal computer, a special purpose controller, or another suitable processing unit. The controller 160 may further include a non-transitory computer-readable storage element, such as a semiconductor memory, a magnetic memory, or another suitable memory. The non-transitory storage element may contain instructions and other data that enable the controller 160 to perform the functions described herein.
[0019] As discussed above, when using a plasma chamber such as the plasma chamber shown in FIG. 1, it is possible that the surface of the workpiece will be etched by radicals and / or excited species when ions are injected into the workpiece 10. This has the effect of removing material from the surface of the workpiece 10, which may result in reduced performance. When a feed gas is introduced into the plasma chamber and the RF antenna 120 is energized, a portion of the feed gas is ionized into a plasma. These ions are exposed to an electric field and can thus be controlled and manipulated. However, some molecules of the feed gas are excited but not ionized. Other molecules are disrupted into radicals.
[0020] Both the excited molecules and the radicals are highly reactive and tend to react with any surface. Thus, if the radicals come into contact with the surface of the workpiece 10, the radicals react with the material of the workpiece 10, typically silicon, and the material is removed. Thus, while ions are beneficially implanted into the workpiece 10 to passivate it, the radicals and excited molecules are detrimentally etching the surface of the workpiece.
[0021] To preserve the benefits of implanting passivating ions while resisting the etching effects of the radicals and excited molecules, a sacrificial capping layer may be provided on top of the workpiece, as shown in Figure 2. As can be seen, the radicals and excited molecules 200 may react with the sacrificial capping layer 210 disposed on top of the workpiece 10. At the same time, passivating ions 220 travel through the sacrificial capping layer 210 and are implanted into the workpiece 10.
[0022] The sacrificial capping layer 210 comprises a material that is resistant to the etching effects of the radicals and excited molecules 200. In other words, the etch rate of the sacrificial capping layer 210 is less than the etch rate of the lower workpiece 10. In some embodiments, the etch rate of the sacrificial capping layer 210 may be 5 to 10 times slower than the etch rate of the lower workpiece. In certain embodiments, the etch rate of the sacrificial capping layer 210 may be more than 10 times slower than the etch rate of the lower workpiece. In certain embodiments, the sacrificial capping layer is made of a material such as silicon dioxide (SiO2), silicon nitride (Si x N y ), or silicon oxynitride (Si x O y N z ) may be the case.
[0023] The sacrificial capping layer 210 may be between 5 Angstroms and 100 Angstroms in thickness. In other embodiments, the sacrificial capping layer 210 may be between 10 Angstroms and 100 Angstroms. In other embodiments, the sacrificial capping layer 210 may be between 20 Angstroms and 100 Angstroms. The thickness is selected such that the passivating ions 220 can still travel through the sacrificial capping layer 210. Furthermore, the thickness is selected such that the sacrificial capping layer 210 may be completely or nearly completely etched by the radicals and excited molecules 200 during the implantation of the passivating ions 220. Thus, the thickness of the sacrificial capping layer 210 may be determined based on the implantation time as well as the etch rate of the sacrificial capping layer 210.
[0024] This sacrificial capping layer 210 may be applied in a number of different ways. For example, the sacrificial capping layer 210 may be applied either in the plasma chamber used to perform the ion implantation or in a separate chamber.
[0025] When the sacrificial capping layer is grown in the same plasma chamber that is used to perform the passivating ion implantation, there are a number of different sequences that can be used.
[0026] FIG. 3A shows a first embodiment. In this figure, the vertical axis is used to represent process parameter values. Line 300 represents the flow rate of the capping species. The capping species includes any species that may be used to grow a sacrificial capping layer, including oxygen (O2) and nitrogen (N2). Other species, such as nitric oxide (NO) or nitrogen dioxide (NO2), may also be used to grow a sacrificial capping layer. All of these species may be referred to as capping species, since they are used for the growth of a sacrificial capping layer. Line 301 represents the flow rate of the passivating species. Line 302 represents the bias voltage applied by the bias power supply 135 (see FIG. 1). The operation of the RF power supply 121 is shown in line 303.
[0027] In this embodiment, the RF power supply 121 is activated at approximately the same time as the introduction of the capping species. The capping species may be stored in a feed gas container 170a. Then, to introduce the capping species, the controller 160 may activate the mass flow controller 171a to allow a desired flow rate of the capping species into the plasma chamber 105. The activation of the RF power supply 121 ionizes the capping species, thereby allowing a sacrificial capping layer 210 to be grown on the top surface of the workpiece. A bias voltage is not enabled during this time so that the ionized capping species is not implanted into the workpiece. The period during which the RF power supply 121 is activated, the mass flow controller 171a is activated, and no bias voltage is enabled may be referred to as a capping period. As a sacrificial capping layer is being grown during the capping period, a flow of passivating species may begin as shown in line 301. The passivating species may be hydrogen, deuterium, fluorine, or a mixture of gases containing hydrogen, deuterium, or fluorine as a diluent or primary process gas. The passivating species may be stored in a feed gas container 170b, and the controller 160 may operate the mass flow controller 171b to enable the flow of the passivating species into the plasma chamber 105. Of course, the rate at which the passivating species is introduced may differ from the rate shown in FIG. 3A. After the flow of the capping species is stopped, such as by disabling the mass flow controller 171a, a bias voltage may be applied by the bias power supply 135, as shown in line 302. Although FIGS. 3A-3C show the bias voltage as appearing positive, it is understood that a negative bias voltage is used to attract positive ions. The bias voltage may be a pulsed DC voltage having an amplitude between 0.1 kV and 10 kV, depending on the passivating species.For example, a heavier passivating species, such as fluorine, may utilize a bias voltage that is greater than a lighter passivating species, such as hydrogen. The amplitude of the bias voltage is selected to allow the passivating ions to travel through the sacrificial capping layer and stop at the portion of the workpiece 10 that is to be passivated.
[0028] In certain embodiments, this portion may be the interface between polysilicon and another material, such as at the gate of a transistor. Examples of two different semiconductor structures utilizing a sacrificial capping layer during the passivation process are found in Figures 5A-5B. In Figure 5A, a transistor is shown having a source 500 and a drain 510 that are created in a silicon substrate. A gate 520 is then formed on the silicon substrate between the source 500 and the drain 510. The gate 520 may include a gate oxide 521 and a polycrystalline silicon (polysilicon) layer 522 disposed on the gate oxide 521. On top of the polysilicon layer is a sacrificial capping layer 210.
[0029] In Figure 5B, a transistor with a metal gate is shown. The transistor has a source 530 and a drain 540 that are produced in a silicon substrate. A gate 550 is then formed on the silicon substrate between the source 530 and the drain 540. The gate 550 comprises an interfacial layer 551, a high dielectric constant layer 552, a metal gate 553, and a polysilicon layer 554. On top of the polysilicon layer is a sacrificial capping layer 210.
[0030] The RF power supply 121 may remain activated while the passivating species are flowed into the plasma chamber 105. When the bias power supply 135, the RF power supply 121, and the mass flow controller 171b are all activated, implantation of the workpiece occurs. This period of time may then be referred to as the implantation process. The implantation process continues until the desired dose is implanted into the workpiece. The desired dose may be 1E15 / cm. 3 From 3E17 / cm 3 Sometimes it can be between.
[0031] During the implantation process, the radicals and excited molecules 200 etch the sacrificial capping layer 210. The thickness of the sacrificial capping layer 210 can be such that the sacrificial capping layer 210 is completely or mostly etched away during the implantation process. For example, in one embodiment, when the implantation process is completed, the dose in the implanted portion of the workpiece 10 can be within a desired range, with 5 Angstroms or less of the sacrificial capping layer 210 remaining. In another embodiment, when the implantation process is completed, the dose in the implanted portion of the workpiece 10 can be within a desired range, with the sacrificial capping layer 210 being completely etched away and 10 Angstroms or less of the workpiece 10 being etched away.
[0032] Thus, the thickness of the sacrificial capping layer 210 applied during the capping period prior to the implantation process is determined by the implantation time and the etch rate of the sacrificial capping layer 210. The etch rate of the sacrificial capping layer 210 may be determined based on the material, passivating species, and other process parameters used to create the sacrificial capping layer 210. The implantation time may be determined by the power supplied by the RF power supply 121, the bias voltage, and the desired dose.
[0033] In other words, in one embodiment, the injection time is calculated based on the parameters discussed above. Once the injection time is determined, the initial thickness of the sacrificial capping layer 210 can be determined based on the injection time and the etch rate. It should be noted that in certain embodiments, the etch rate of the sacrificial capping layer 210 can vary as a function of the number of hours of operation since the last cleaning. For example, the etch rate can change as the walls of the plasma chamber become coated with material generated during an earlier process. Thus, in certain embodiments, the controller 160 can monitor the number of hours of operation since the last cleaning and adjust the etch rate based on this monitored value. In certain embodiments, the controller 160 can monitor the number of workpieces processed since the last cleaning and adjust the etch rate based on this monitored value. In another embodiment, the controller 160 can rely on a metrology system to determine the actual etch rate of the sacrificial capping layer. Thus, in these embodiments, the controller monitors parameters such as the number of hours of operation, the number of workpieces processed, or the output from the metrology system to compensate for the varying etch rate that occurs over time.
[0034] The controller 160 may then execute the following sequence: First, the passivating species and the desired dose of the passivating species may be determined or provided to the controller 160, as shown in box 400 of FIG. 4. Based on this information, the controller 160 may determine an implant time that may be used to deliver the desired dose, as shown in box 410. The controller 160 may then determine or provide a capping species to be selected, as shown in box 420. Next, the controller optionally determines the amount of time the plasma chamber 105 has been operating since the last cleaning, as shown in box 430. Alternatively, the controller 160 may determine the number of workpieces that have been processed since the last cleaning. The controller 160 then determines an estimated etch rate of the sacrificial capping layer 210 based on the passivating species, the capping species, the power applied by the RF power supply, and optionally the number of hours of operation of the plasma chamber or the number of workpiece processes, as shown in box 440. In another embodiment, the controller 160 may utilize measurements to determine the change in etch rate as a result of chamber usage. Based on the etch rate and the implantation time, the controller 160 calculates a desired initial thickness of the sacrificial capping layer 210, as shown in box 450. The initial thickness may be calculated as the product of the etch rate and the total implantation time. Using this information, the controller 160 may calculate the duration of the capping period during which the mass flow controller 171a is activated to form the sacrificial capping layer, as shown in box 460. In other words, the initial thickness of the sacrificial capping layer 210 is calculated as a function of the subsequent implantation time, which is a function of the passivating species and the desired dose.
[0035] If desired, the sequence shown in Figure 3A may be repeated multiple times. Figure 3A shows a sequence in which a sacrificial capping layer 210 is created and then an implantation process is performed until the sacrificial capping layer 210 is etched away.
[0036] Thus, in certain embodiments, a thinner sacrificial capping layer may be grown and a shorter implantation process may be performed. After the thin sacrificial capping layer is etched away, the sequence shown in FIG. 3A may be repeated. The sequence of capping periods followed by implantation processes may then be repeated multiple times. This may add time to the total manufacturing process, but it may allow for a thinner initial sacrificial capping layer than would be used if the sequence of FIG. 4 were simply performed once. This may allow the passivating ions 220 to travel to a greater depth, particularly at the beginning of the implantation process.
[0037] FIG. 3B shows another embodiment. In this figure, the vertical axis is used to represent process parameter values. Line 310 represents the flow rate of the capping species. Capping species includes any species that may be used to grow a sacrificial capping layer, including oxygen (O2) and nitrogen (N2). Other species, such as nitric oxide (NO) or nitrogen dioxide (NO2), may also be used to grow a sacrificial capping layer. All of these species may be referred to as capping species, since they are used for the growth of a sacrificial capping layer. Line 311 represents the flow rate of the passivating species. Line 312 represents the bias voltage applied by the bias power supply 135 (see FIG. 1). As explained above, the bias voltage appears positive, however, it is understood that a negative bias voltage is used to attract positive ions. The operation of the RF power supply 121 is shown in line 313.
[0038] In this embodiment, the mass flow controller 171a is operated to enable the flow of the capping species. As explained above, during the capping period, the bias voltage is disabled so that ions of the capping species are not implanted. After a predetermined amount of time, the flow of the passivating species may begin as shown in line 311. The passivating species may be hydrogen, deuterium, fluorine, or a mixture of gases containing hydrogen, deuterium, or fluorine as a diluent or primary process gas. The passivating species may be stored in a feed gas container 170b, and the controller 160 may operate the mass flow controller 171b to enable the flow of the passivating species into the plasma chamber 105. Of course, the rate at which the passivating species is introduced may differ from the rate shown in FIG. 3B. After the flow of the capping species is stopped, such as by disabling the mass flow controller 171a, a bias voltage may be applied by the bias power supply 135, as shown at line 312. The bias voltage may be a pulsed DC voltage having an amplitude between 0.1 kV and 10 kV, depending on the passivating species. The amplitude of the bias voltage is selected to allow the passivating ions 220 to travel through the sacrificial capping layer 210 and stop at a portion of the workpiece to be passivated. In some embodiments, this portion may be an interface between polysilicon and another material, as shown in Figures 5A-5B. The RF power supply 121 may remain activated while the passivating species is flowed into the plasma chamber 105. When the bias power supply 135, the RF power supply 121, and the mass flow controller 171b are all activated, the implantation process occurs. The implantation process continues until the desired dose is implanted into the workpiece 10. The desired dose is 1E15 / cm 3 From 3E17 / cm 33A , periodically, the controller 160 operates the mass flow controller 171a to enable the flow of the capping species during the implantation process. In certain embodiments, the capping species is much heavier than the passivating species. For example, the capping species may be oxygen or nitrogen, while the passivating species is hydrogen or deuterium. Thus, even if ions of the capping species are implanted, they will travel to a much shallower depth than the passivating ions 220. Furthermore, the presence of the sacrificial capping layer 210 may further slow down these ions of the capping species. In certain embodiments, the bias voltage (not shown) may be reduced during the time when the capping species is flowing into the plasma chamber 105 during the implantation process. This may further serve to reduce the number of ions of the capping species that are implanted and the depth to which these ions are implanted.
[0039] In this embodiment, the sacrificial capping layer 210 may be etched by the radicals and excited molecules 200 of the passivating species during the implantation process, but the sacrificial capping layer 210 is also grown during the implantation process. This effectively reduces the etching rate of the sacrificial capping layer 210. This allows a thinner initial sacrificial capping layer to be grown prior to the implantation process, as compared to the embodiment of FIG. 3A. This may allow the passivating ions to travel to a greater depth, especially at the beginning of the implantation process.
[0040] Thus, FIG. 3B shows a sequence in which the sacrificial capping layer 210 is created during the capping period and then the implantation process is performed, in which periodically, during the implantation process, the sacrificial capping layer is grown by activating the mass flow controller 171a. Note that FIG. 3B shows that the line 310 behaves like a periodic function during the implantation process in that the line 310 has a constant amplitude, frequency, and duty cycle. However, other embodiments are also possible. For example, the duty cycle at which the mass flow controller 171a is activated may decrease or increase as the implantation process progresses. Additionally, the frequency at which the mass flow controller 171a is activated may decrease or increase as the implantation process progresses.
[0041] 3B, the flow rate of the capping species is shown to be constant whenever the mass flow controller 171a is activated. However, in certain embodiments, the flow rate of the capping species may be lower during the implantation process than the flow rate during the capping period.
[0042] In this embodiment, the controller calculates the initial thickness of the sacrificial capping layer 210. However, unlike the previous embodiment, the controller 160 also takes into account that material will be added to the sacrificial capping layer during the implantation process. The amount of material added to the sacrificial capping layer is a function of the flow rate of the mass flow controller 171a during the implantation process as well as the duty cycle and frequency of the mass flow controller 171a. The etch rate may be calculated as described above. In addition, the total amount of the sacrificial capping layer etched may be determined as described above. Furthermore, the controller 160 may use information such as the number of hours of operation since the last cleaning, the number of workpieces processed since the last cleaning, or the output of the metrology system to determine the change in the etch rate over time. Based on this revised etch rate, the controller 160 may vary the flow rate of the mass flow controller 171a or shift the frequency or duty cycle of the mass flow controller 171a to compensate for the varying etch rate.
[0043] Therefore, in this embodiment, the initial thickness of the sacrificial capping layer 210 may be calculated as the product of the etch rate of the sacrificial capping layer and the total implantation time minus the amount of material added to the sacrificial capping layer during the implantation process. Thus, the initial thickness of the sacrificial capping layer is thinner in the embodiment shown in Figure 3B than in the embodiment shown in Figure 3A. This may allow the passivating ions to travel to a greater depth, especially at the beginning of the implantation process.
[0044] FIG. 3C shows a third embodiment, which is similar to FIG. 3B. In this figure, the vertical axis is used to represent process parameter values. Line 320 represents the flow rate of the capping species. Capping species includes any species that may be used to grow a sacrificial capping layer, including oxygen (O2) and nitrogen (N2). Other species, such as nitric oxide (NO) or nitrogen dioxide (NO2), may also be used to grow a sacrificial capping layer. All of these species may be referred to as capping species, since they are used for the growth of a sacrificial capping layer. Line 321 represents the flow rate of the passivating species. Line 322 represents the bias voltage applied by the bias power supply 135 (see FIG. 1). Again, the bias voltage appears positive, however, it is understood that a negative bias voltage is used to attract positive ions. The operation of the RF power supply 121 is shown in line 323.
[0045] In this embodiment, rather than pulsing the mass flow controller 171a during the implantation process, the flow of the capping species is always enabled during the implantation process. In certain embodiments, such as the embodiment shown in FIG. 3C, the flow rate of the capping species may be constant throughout the implantation process. However, in other embodiments, the flow rate may increase or decrease throughout the implantation process. In addition, the flow rate of the capping species during the implantation process may be less than the flow rate during the capping period.
[0046] Additionally, the controller 160 may use information such as the number of hours of operation since the last clean, the number of workpieces processed since the last clean, or the output of a metrology system to determine changes in etch rate over time. Based on this revised etch rate, the controller 160 may vary the flow rate of the mass flow controller 171a or shift the frequency or duty cycle of the mass flow controller 171a to compensate for the varying etch rate.
[0047] Thus, in certain embodiments, a semiconductor processing apparatus is disclosed. The apparatus includes a plasma chamber 105. The apparatus further includes a feed gas container 170a containing a capping species, a mass flow controller 171a regulating the flow of the capping species from the feed gas container 170a to the plasma chamber 105, a feed gas container 170b containing a passivating species, and a mass flow controller 171b regulating the flow of the passivating species from the feed gas container 170b to the plasma chamber 105. In addition, the apparatus includes an RF power supply 121 providing power to the RF antenna 120. A platen 130 is disposed within the plasma chamber 105. The platen 130 is in electrical communication with a bias power supply 135. The apparatus further includes a controller 160 in communication with the RF power supply 121, the bias power supply 135, and the mass flow controllers 171a, 171b. The controller 160 comprises instructions that enable the controller 160 to perform the functions described above and shown in FIGS. 3A-3C. The controller 160 thus controls the device to generate a capping period and an injection process. As described above, the controller 160 may perform a capping period before and / or during the injection process. Additionally, in certain embodiments, the controller 160 is in communication with a metrology system. The controller 160 may terminate the injection process based on the output of the metrology system. In other embodiments, the controller 160 may issue an alert based on the output of the metrology system.
[0048] While Figures 3A-3C show an embodiment in which the sacrificial capping layer is applied in the same plasma chamber as the implantation process, in other embodiments, the sacrificial capping layer is applied outside of the plasma chamber used to perform the implantation process. For example, in one embodiment, the workpiece may be placed in a heated chamber, such as above 600°C, and capping species may be introduced. Due to the presence of these species in the heated chamber, the capping layer will grow in this environment without the use of any bias voltage.
[0049] In another embodiment, the workpiece may be placed in a preheat chamber having a temperature between 200° C. and 600° C. A capping species may be introduced into the preheat chamber. A sacrificial capping layer may be grown in these circumstances. In a variation of this embodiment, a remote plasma generator is used to generate a plasma using one or more capping species. This plasma is then introduced into the preheat chamber.
[0050] In another embodiment, the sacrificial capping layer may be grown using a plasma deposition process (PVD). In PVD, a plasma is created using one or more capping species in a chamber containing the workpiece. Ions or molecules from the plasma are then deposited on the workpiece to create the sacrificial capping layer.
[0051] It is further noted that there are other methods and apparatus that may be used to produce the sacrificial capping layer, and the present disclosure is not limited to the embodiments disclosed above. Furthermore, in certain embodiments, the chamber used to apply the sacrificial capping layer may also be used to heat the workpiece, such as to a temperature used during the passivating process.
[0052] In each of these embodiments in which the sacrificial capping layer is applied outside the plasma chamber, the flow chart shown in FIG. 4 may be used to determine the initial thickness of the sacrificial capping layer. Additionally, the sequence used in the plasma chamber 105 for these embodiments is shown in FIG. 6. In this figure, the vertical axis is used to represent process parameter values. Line 331 represents the flow rate of the passivating species. Line 332 represents the bias voltage applied by the bias power supply 135 (see FIG. 1). Again, the bias voltage appears positive, however, it is understood that a negative bias voltage is used to attract positive ions. The operation of the RF power supply 121 is shown in line 333. The flow rate of the passivating species may differ from the flow rate shown in FIG. 6. Note that FIG. 6 is similar to FIG. 3A, except that the capping period is performed outside the plasma chamber 105.
[0053] Further, while the disclosure above describes an implantation process that is terminated based on a predetermined time, other embodiments are also possible. For example, in one example as shown in FIG. 1, a metrology system such as an optical emission spectroscopy (OES) system 180 may be disposed within the plasma chamber 105.
[0054] In certain embodiments, the OES system 180 may be used to terminate the implantation process. Specifically, while the sacrificial capping layer 210 is being etched, the spectrum detected by the OES system 180 will show the presence of oxygen or nitrogen (depending on the composition of the sacrificial capping layer). The spectrum may also show peaks that indicate the presence of silicon. However, once the sacrificial capping layer 210 is completely etched away, the spectrum will show a much larger peak for silicon, and the peaks associated with oxygen and / or nitrogen will disappear. Thus, in one embodiment, rather than using a predetermined time for the implantation process, the OES system 180 is used to detect when the sacrificial capping layer has disappeared. The implantation process is then terminated based on this detection. This approach may be advantageous when the final device parameters are relatively insensitive to dose, but very sensitive to any etching of the surface.
[0055] In certain embodiments, OES system 180 may be used as a warning system. For example, the implantation process may be a timed process of a predetermined duration. However, if OES system 180 detects an increase in the emission of silicon before the predetermined duration has expired, controller 160 may terminate the implantation process prematurely.
[0056] In addition to OES systems, other metrology systems may be used. For example, absorption spectroscopy may be used to monitor the plasma. Alternatively, Fourier transform infrared spectroscopy (FTIR), reflectrometry, or ellipsometry may be used to monitor the sacrificial cap.
[0057] The embodiments described in this disclosure may have many advantages. For example, it is useful to implant ions into a semiconductor substrate to passivate the semiconductor substrate. The use of implantation allows the passivating ions to be delivered deeper into the substrate than can be achieved using other processes. The creation of a sacrificial capping layer allows this passivating implantation to be achieved without the detrimental etching that sometimes accompanies implantation processes. Thus, these embodiments expand the process space available with a given configuration, thereby allowing greater energies and / or doses to be utilized.
[0058] Although the disclosure above describes implants used to passivate the workpiece, the disclosure is not limited to this embodiment. For example, the implants may be used to shift the conductivity of the workpiece or to dope the workpiece for bulk deformation. For example, the implants may be dopant species, such as Group 3, 4, or 5 species. Thus, in certain embodiments, the implant species may be a passivating species. In other embodiments, the implants may be dopant species.
[0059] The present disclosure should not be limited in scope by the specific embodiments described herein. Moreover, various other embodiments of the present disclosure and modifications thereto, in addition to the embodiments and modifications described herein, will be apparent to those skilled in the art from the foregoing description and the accompanying drawings. Thus, such other embodiments and modifications are intended to fall within the scope of the present disclosure. Furthermore, although the present disclosure has been described herein in the context of a particular implementation in a particular environment for a particular purpose, those skilled in the art will recognize that the usefulness of the present disclosure is not limited to that implementation, and that the present disclosure may be beneficially implemented in any number of environments for any number of purposes. Thus, the claims discussed below should be construed in light of the full breadth and spirit of the present disclosure as described herein.
Claims
1. 1. A method of passivating a portion of a workpiece, comprising: placing the workpiece in a plasma chamber; applying a sacrificial capping layer to an upper surface of the workpiece; generating a plasma in the plasma chamber that includes a passivating species, the passivating species being selected from the group consisting of hydrogen, deuterium, fluorine, and a gas mixture containing hydrogen, deuterium, or fluorine as a diluent or primary process gas, and generating a plasma in which ions, radicals, and excited molecules of the passivating species are generated; performing an implantation process in which the ions of the passivating species are implanted through the sacrificial capping layer and into the portion by applying a bias voltage to the workpiece, wherein the radicals and excited molecules etch the sacrificial capping layer during the implantation process; terminating the implantation process when a desired dose of the passivating species has been implanted, where at the end of the implantation process, the thickness of the sacrificial capping layer is less than 5 Angstroms or all of the sacrificial capping layer has been completely removed and less than 10 Angstroms of the workpiece has been etched; A method comprising:
2. 10. The method of claim 1, wherein the sacrificial capping layer is applied in the plasma chamber during a capping period by introducing a capping species and generating a plasma containing the capping species while the bias voltage is disabled.
3. The method of claim 2 , wherein the capping period precedes the implantation process.
4. 4. The method of claim 3, wherein an additional sacrificial capping layer is applied during the implantation process by flowing the capping species into the plasma chamber.
5. 5. The method of claim 4, wherein the flow of the capping species is continuous throughout the implantation process.
6. 5. The method of claim 4, wherein the flow of the capping species is pulsed during the implantation process.
7. 7. The method of claim 6, wherein the bias voltage is varied as the capping species is flowing into the plasma chamber during the implantation process.
8. 2. The method of claim 1, wherein the implantation process is terminated after a predetermined time, the predetermined time being determined based on the passivating species and the desired dose of the passivating species.
9. 9. The method of claim 8, wherein an alert is generated if an output of a metrology system indicates that the workpiece is being etched.
10. The method of claim 1 , wherein the implantation process is terminated based on an output from a metrology system indicating that the workpiece is being etched.
11. The method of claim 1 , wherein an initial thickness of the sacrificial capping layer is determined based on an etch rate of the sacrificial capping layer and a total duration of the implantation process.
12. 12. The method of claim 11, wherein the initial thickness is adjusted based on chamber metrology, number of workpieces processed, or number of operating hours to compensate for varying etch rates.
13. The method of claim 1 , wherein the sacrificial capping layer has a thickness between 5 Angstroms and 100 Angstroms.
14. 2. The method of claim 1, wherein when the bias voltage is applied, the bias voltage is a pulsed DC voltage having an amplitude between 0.1 kV and 10 kV.
15. 1. A method of passivating a portion of a workpiece, comprising: applying a sacrificial capping layer to an upper surface of the workpiece in a chamber, the sacrificial capping layer having a thickness between 5 Angstroms and 100 Angstroms; placing the workpiece in a plasma chamber separate from the chamber; generating a plasma in the plasma chamber that includes a passivating species, the passivating species being selected from the group consisting of hydrogen, deuterium, fluorine, and gas mixtures containing hydrogen, deuterium, or fluorine as diluents or primary process gases, and generating a plasma in which ions, radicals, and excited molecules of the passivating species are generated; performing an implantation process in which the ions of the passivating species are implanted through the sacrificial capping layer and into the portion by applying a bias voltage to the workpiece, wherein the radicals and excited molecules etch the sacrificial capping layer during the implantation process; terminating said implantation process when a desired dose of said passivating species has been implanted. A method comprising:
16. The chamber comprises: heating the workpiece to a temperature near a temperature of the implantation process; growing the sacrificial capping layer by flowing a gas while the workpiece is heated; The method of claim 15.
17. 1. A method of passivating a portion of a workpiece, comprising: flowing a capping species into a plasma chamber in which the workpiece is disposed; energizing the capping species to generate a plasma, wherein no bias voltage is applied to the workpiece during a capping period to produce a sacrificial capping layer on an upper surface of the workpiece; flowing a passivating species into the plasma chamber, the passivating species being selected from the group consisting of hydrogen, deuterium, fluorine, and gas mixtures containing hydrogen, deuterium, or fluorine as diluents or primary process gases; performing an implantation process to implant passivating ions into the workpiece, the implantation process being defined as a period of time during which the bias voltage is applied to the workpiece while a plasma containing the passivating species is generated; adding material to a sacrificial capping layer by flowing the capping species into the plasma chamber during the implantation process; Terminating the injection process. A method comprising:
18. 20. The method of claim 17, wherein the implantation process is terminated when a desired dose of the passivating ions has been implanted.
19. 20. The method of claim 17, wherein at the conclusion of the implantation process, the sacrificial capping layer has a thickness of less than 5 Angstroms, or all of the sacrificial capping layer has been completely removed and less than 10 Angstroms of the workpiece has been etched.
20. 20. The method of claim 17, wherein the flow of the capping species is continuous throughout the implantation process.
21. 20. The method of claim 17, wherein the flow of the capping species is pulsed during the implantation process.
22. 22. The method of claim 21, wherein the bias voltage is varied as the capping species is flowing into the plasma chamber during the implantation process.
23. 20. The method of claim 17, wherein the amount of material added is varied based on chamber metrology, number of workpieces processed, or number of operating hours to compensate for varying etch rates.
24. 24. The method of claim 23, wherein the capping species flows into the plasma chamber through a mass flow controller, and the amount of material is manipulated by adjusting the flow rate of the capping species, the frequency at which the mass flow controller is operated, or the duty cycle of the mass flow controller.
Citation Information
Patent Citations
Ion implantation device and ion implantation method
JP2006221941A
Dose monitor using optical radiation spectrum for field use
JP2008244444A
Systems and processes for contact doping and annealing for nanowire thin films
JP2008522404A
Safe handling of low-energy, high-dose arsenic, phosphorus, and boron-implanted wafers
JP2010514166A
Adjusting the doping profile in the P3i process
JP2012507867A