Lithium ion battery positive electrode lithium supplement additive and preparation method thereof and lithium ion battery
The method improves the purity and scalability of Li2NiO2 production by using a composite lithium salt and controlled sintering, addressing the limitations of existing methods and enhancing battery performance.
Patent Information
- Application Number
- JP2023504719
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-29
- Filing Date
- 2020-10-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-10-09
AI Technical Summary
Existing methods for preparing positive electrode lithium replenishment materials for lithium-ion batteries face challenges such as low purity, complex processes, environmental pollution, and high residual alkali content, which hinder industrial scalability and battery performance.
A method involving the preparation of a composite lithium salt, mixing with a nickel source, sintering, and crushing under controlled atmospheres to produce a high-purity Li2NiO2 additive with <3% residual alkali, using specific temperature and atmosphere conditions to enhance purity and safety.
The method achieves a Li2NiO2 additive with >95% purity, 420-465 mAh/g first charge capacity, and 260-340 mAh/g irreversible capacity, facilitating cost-effective, environmentally friendly, and scalable battery production.
Smart Images

Figure 0007559211000003 
Figure 0007559211000004 
Figure 0007559211000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a lithium ion battery material and its preparation method and a lithium ion battery, in particular to a positive electrode additive material for a lithium ion battery and its preparation method and a lithium ion battery. [Background technology]
[0002] Lithium-ion batteries (batteries) are widely used in various electronic products due to their characteristics of high energy density and long cycle life. With the rapid development of large-scale mobile power sources such as electric vehicles, electric machines, and drones, there are higher requirements for high energy and high power.
[0003] The most effective way to meet the design requirements of high specific energy batteries is to select high specific capacity positive and negative electrode materials, such as silicon, tin, aluminum, and oxide as new negative electrode materials. However, during the first charging process of a lithium battery, some of the lithium released from the positive electrode will form an irreversible lithium-containing passivation film (SEI) on the surface of the negative electrode, causing the loss of active lithium, which reduces the available energy of the battery.
[0004] The prior art method for compensating for this portion of lithium loss is to pre-replenish lithium to the positive or negative electrode. The lithium supplementation of the negative electrode is generally made by reacting metallic lithium powder, foil, or sheet with the negative electrode material. However, this method has the problem that the chemical stability of the lithiation reagent is poor, and the active lithium powder has a large safety concern. The lithium supplementation of the positive electrode is generally made by mixing the lithium supplementation material with the positive electrode material in proportion, forming a slurry, and then forming a battery core, and during the first charging process, the lithium supplementation is completed by releasing the excess lithium and forming an SEI film on the surface of the negative electrode to replenish the consumed lithium. Compared with the lithium supplementation of the negative electrode, the lithium supplementation of the positive electrode does not need to change the traditional battery manufacturing process, so it has the characteristics of low cost, simple and high safety, and has a wider industrial application prospect. However, the preparation method of the positive electrode lithium supplementation material in the prior art has the problem that the process is complicated, and it is necessary to go through multiple mixing, crushing, and sintering processes, and the obtained positive electrode lithium supplementation material has a low purity and cannot meet the requirements of industrialized manufacturing.
[0005] The lithium replenishment material Li disclosed in the Chinese patent with publication number 108735526A 2 NiO 2 As the preparation method of Li 2 NiO 2 The lithium-ion capacitor uses Li 2 The raw materials are O and NiO, which are ball-milled under a protective atmosphere, sintered at high temperature, and then Al 2 O 3 Then, the ball milling is continued under a protective atmosphere, followed by high-temperature sintering to obtain the target Li 2 NiO 2 This method obtains Li 2 O, NiO and Al 2 O 3 Li prepared by high temperature sintering using 2 NiO 2 Such synthesis is difficult, and the Li 2 NiO 2 However, there are many impurities and it is difficult to improve the synthesis purity.
[0006] In addition, the Chinese patent with publication number 109786746A discloses a positive electrode sheet, a positive electrode lithium supplement material for lithium ion batteries and a preparation method thereof, which uses ethanol as a solvent to mix a positive electrode lithium supplement material matrix and a carbon source to obtain a mixed solution, which is then volatilized to remove the solvent, and then baked under an inert atmosphere to obtain a positive electrode lithium supplement material for lithium ion batteries having a carbon coating on its surface. This method involves the steps of: 2 CO 3 It is very difficult to prepare lithium oxide with a purity of >99.9% using this as a raw material, and the reproducibility is very poor. 2 CO 3 It has a high lithium content and can be used as a lithium source. 2 NiO 2 The preparation of the battery results in a high carbonate ion content, which has adverse effects on both the battery processing and battery performance.
[0007] In addition, the lithium replenishment material Li disclosed in the Chinese patent with publication number 110218078A 2 NiO 2 and its preparation method and use, the preparation method is Li 2 O, Ni 2 CO 3 , Al(OH) 3 The raw material is mixed with acetone as a solvent, and then ball milled under a protective atmosphere (S1); the ball milled product is baked to obtain a powder (S2); the powder is pre-sintered at a low temperature under a protective atmosphere (S3); the pre-sintered product is ball milled under a protective atmosphere, and the ball milled product is taken out and pressed into a sheet (S4); and the product obtained in step S4 is sintered at a high temperature to obtain the target lithium replenishment material Li. 2 NiO 2 This method requires multiple sintering steps to prepare the powder, and uses an organic solvent, acetone, which makes the process complicated and difficult to mass-produce, and is prone to environmental pollution. Summary of the Invention
[0008] The object of the present invention is to provide a positive electrode lithium replenishing additive for a lithium-ion battery, a preparation method thereof, and a lithium-ion battery. The problem to be solved is to improve the purity of Li 2 NiO 2 and reduce the cost.
[0009] The present invention adopts the following technical solutions. A positive electrode lithium replenishing additive for a lithium-ion battery, wherein the purity of Li 2 NiO 2 is > 95%, the total amount of residual alkali is < 3%, the gram capacity of the first charge is 420 - 465 mAh / g, and the irreversible capacity is 260 - 340 mAh / g.
[0010] The positive electrode lithium replenishing additive for a lithium-ion battery of the present invention is characterized in that it is obtained by using a preparation method including the following steps. Step 1, preparation of a composite lithium salt At room temperature, the lithium raw material is heated to 400 - 950 °C at a vacuum degree < 100 Pa and a heating rate of 1 - 10 °C / min, held for 15 - 480 min, and naturally cooled to room temperature in the furnace. Using zirconium balls with a diameter of 5 mm, the mass ratio of the balls to the lithium raw material is 10 - 15:1, and ball milling is performed at a rotation speed of 700 rpm for 0.5 h to obtain a composite lithium salt xLiOH·yLi 2 O·zLi 2 CO 3 ·wH 2 O, where x, y, z are mass fractions, 0 < x < 0.5, 0.5 ≤ y < 1.0, 0 < z < 0.5, x + y + z = 1, w represents the crystal water content, and 0 ≤ w ≤ 1. The lithium raw material is one or more of a lithium hydroxide - lithium oxide - lithium carbonate composite, a lithium hydroxide - lithium oxide - lithium oxalate composite, a lithium hydroxide - lithium peroxide - lithium carbonate composite, a lithium hydroxide - lithium peroxide - lithium oxalate composite, a lithium hydride - lithium oxide - lithium carbonate composite, a lithium hydride - lithium oxide - lithium oxalate composite, a lithium hydride - lithium peroxide - lithium carbonate composite, and a lithium hydride - lithium peroxide - lithium oxalate composite. Step 2, Mixing the composite lithium salt and nickel source The composite lithium salt is mixed with the lithium source and the nickel source in a molar ratio of 1.5-2.2:1.0 under an argon or nitrogen protective atmosphere, the rotation speed is 500-1000 rpm, and the time is 0.5-6.0 h, to obtain a mixed powder of the composite lithium salt and the nickel source; the nickel source is at least one of nickel(II) oxide, nickel trioxide, nickel dioxide, nickel hydroxide, nickel oxyhydroxide, nickel carbonate, nickel oxalate, and nickel acetate; Step 3: Sintering The mixed powder of the composite lithium salt and the nickel source is heated to 100-300°C at a heating rate of 1-10°C / min in a protective atmosphere or an oxidizing atmosphere, and then the temperature is maintained for 0.5-5.0 hours, and then the temperature is increased to 600-800°C at a heating rate of 1-10°C / min, and the temperature is maintained for 5.0-20.0 hours, followed by high-temperature sintering, and then the temperature is naturally lowered to room temperature in the furnace to obtain a sintered material. Step 4: Crushing The sintered material is dispersed and pulverized under an argon or nitrogen protective atmosphere at a rotation speed of 800-1000 rpm for 15-30 min, and then sieved through a 350-400 mesh sieve to obtain a pulverized material with a particle size D50 of 5.0-15.0 μm and Dmax<25.0 μm; Step 5: Demagnetization The ground material is demagnetized to obtain a magnetic substance content <50ppb, and the positive electrode lithium supplement additive for lithium-ion batteries is obtained.
[0011] In the step 1, the mass purity of the lithium raw material is >99%, in the step 2, the purity of the argon or nitrogen is >99.995% and the flow rate is 6 L / min, in the step 3, the protective atmosphere is one or more of argon or nitrogen, the gas purity is >99.995%, and the flow rate is 6 L / min, and the oxidizing atmosphere is a protective atmosphere with an oxygen content of 50 to 200 ppm, and in the step 4, the purity of the argon or nitrogen is >99.995%, and the flow rate is 6 L / min.
[0012] In step 4, the mixture is sieved through a 350 to 400 mesh sieve to have a particle size D50 of 5.0 to 15.0 μm and Dmax<25.0 μm.
[0013] A method for preparing a lithium supplement additive for the positive electrode of a lithium-ion battery, comprising the following steps: Step 1, preparation of a composite lithium salt At room temperature, the lithium raw material is heated to 400-950 °C at a heating rate of 1-10 °C / min under a vacuum of <100 Pa, held for 15-480 min while maintaining the vacuum, and then naturally cooled to room temperature in the furnace and taken out, crushed to obtain a composite lithium salt xLiOH·yLi 2 O·zLi 2 CO 3 ·wH 2 O, where x, y, and z are mass fractions, 0 < x < 0.5, 0.5 ≤ y < 1.0, 0 < z < 0.5, x + y + z = 1, w represents the crystal water content, and 0 ≤ w ≤ 1. The lithium raw material is one or more of a lithium hydroxide-lithium oxide-lithium carbonate composite, a lithium hydroxide-lithium oxide-lithium oxalate composite, a lithium hydroxide-lithium peroxide-lithium carbonate composite, a lithium hydroxide-lithium peroxide-lithium oxalate composite, a lithium hydride-lithium oxide-lithium carbonate composite, a lithium hydride-lithium oxide-lithium oxalate composite, a lithium hydride-lithium peroxide-lithium carbonate composite, and a lithium hydride-lithium peroxide-lithium oxalate composite. Step 2, mixing of the composite lithium salt and the nickel source The composite lithium salt is mixed at a molar ratio of lithium source to nickel source of 1.5-2.2:1.0 under an argon or nitrogen protection atmosphere, with a rotation speed of 500-1000 rpm and a time of 0.5-6.0 h to obtain a mixed powder of the composite lithium salt and the nickel source. The nickel source is one or more of nickel(II) oxide, nickel sesquioxide, nickel dioxide, nickel hydroxide, nickel oxyhydroxide, nickel carbonate, nickel oxalate, and nickel acetate. Step 3, sintering The mixed powder of the composite lithium salt and the nickel source is heated to 100-300°C at a heating rate of 1-10°C / min in a protective atmosphere or an oxidizing atmosphere, and then heated to 600-800°C at a heating rate of 1-10°C / min, and then kept at the same temperature for 5.0-20.0 hours. The temperature is then naturally lowered to room temperature in a furnace to obtain a sintered material. Step 4: Crushing The sintered material is dispersed and pulverized under argon or nitrogen protective atmosphere at a rotation speed of 800-1000 rpm for 15-30 min, and then sieved through a 350-400 mesh sieve to obtain the positive electrode lithium supplement additive for lithium ion batteries.
[0014] After step 4 of the method of the present invention, the material is demagnetized to a magnetic content of <50 ppb.
[0015] The crushing in step 1 of the method of the present invention is carried out by ball milling using zirconium balls having a diameter of 5 mm, with a mass ratio of balls to lithium raw material of 10 to 15:1, and at a rotation speed of 700 rpm for 0.5 hours.
[0016] In the method of the present invention, the mass purity of the lithium raw material in step 1 is >99%, the purity of argon or nitrogen in step 2 is >99.995% and the flow rate is 6L / min, the protective atmosphere in step 3 is one or more of argon or nitrogen, the gas purity is >99.995%, and the flow rate is 6L / min, the oxidizing atmosphere is a protective atmosphere with an oxygen content of 50-200ppm, and the purity of argon or nitrogen in step 4 is >99.995% and the flow rate is 6L / min.
[0017] In step 4 of the method of the present invention, the mixture is sieved through a 350-400 mesh sieve, with a particle size D50 of 5.0-15.0 μm and Dmax<25.0 μm.
[0018] A lithium ion battery is provided with a positive electrode, and a lithium supplement additive is added to the positive electrode active material of the positive electrode, and the lithium supplement additive is the positive electrode lithium supplement additive of the lithium ion battery of the present invention.
[0019] Compared with the prior art, the present invention uses a composite lithium salt as the lithium raw material, including mixing, sintering, and crushing, and the obtained Li 2 NiO 2 has a purity > 95%, a total residual alkali content < 3%, a gram capacity of 420 - 465 mAh / g for the first charge, an irreversible capacity of 260 - 340 mAh / g, a simple preparation method, easy control, low cost, environmental friendliness, and contributes to industrialized production.
Brief Description of the Drawings
[0020] [Figure 1] It is the XRD diagram of the composite lithium salt of Example 1 of the present invention. [Diagram 2] It is the XRD diagram of the positive electrode lithium supplement additive of the lithium ion battery of Example 1 of the present invention. [Diagram 3] It is the SEM diagram of the positive electrode lithium supplement additive of the lithium ion battery of Example 1 of the present invention. [Figure 4] It is the charge - discharge curve diagram of Example 1 of the present invention.
Modes for Carrying Out the Invention
[0021] Hereinafter, the present invention will be described in more detail with reference to the drawings and examples. The preparation method of the positive electrode lithium supplement additive Li 2 NiO 2 of the lithium ion battery of the present invention includes the following steps.
[0022] Step 1, Preparation of composite lithium salt The composite lithium salt is the mixture xLiOH·yLi 2 O·zLi 2 CO 3 ·wH 2 O, where x, y, z are mass fractions, 0 < x < 0.5, 0.5 ≤ y < 1.0, 0 < z < 0.5, x + y + z = 1, w represents the crystal water content, and 0 ≤ w ≤ 1. The lithium raw material is one or more of lithium hydroxide-lithium oxide-lithium carbonate complex, lithium hydroxide-lithium oxide-lithium oxalate complex, lithium hydroxide-lithium peroxide-lithium carbonate complex, lithium hydroxide-lithium peroxide-lithium oxalate complex, lithium hydride-lithium oxide-lithium carbonate complex, lithium hydride-lithium oxide-lithium oxalate complex, lithium hydride-lithium peroxide-lithium carbonate complex, lithium hydride-lithium peroxide-lithium oxalate complex, with mass purity of >99%. Complex refers to mechanical mixture. The lithium raw material in the embodiment of the present invention adopts battery grade lithium raw material from Ganfeng Lithium Co., Ltd. At room temperature (20°C), the lithium raw material was heated to 400-950°C at a rate of 1-10°C / min under a vacuum of <100 Pa, and then kept at that temperature for 15-480 min. The vacuum was maintained, and the temperature was naturally lowered to room temperature in the furnace before being removed. The sample was a block-shaped solid, which was crushed and ball-milled with 5 mm diameter zirconium balls at a mass ratio of 10-15:1 to the lithium raw material at a rotation speed of 700 rpm for 0.5 h to obtain a composite lithium salt xLiOH yLi 2 O·zLi 2 CO 3 ·wH 2 I got an O. By controlling the temperature and time of the heat retention, the lithium raw material is decomposed and converted into a composite lithium salt (lithium source) containing lithium oxide, lithium hydroxide, and lithium carbonate that meets the ratio requirements. During the sintering process in step 3, the Li 2 O+NiO=Li 2 NiO 2 This is also the key to preparing the positive electrode lithium supplement additive for lithium-ion batteries by sintering. In step 3, sintering, when the temperature is >450°C, the lithium hydroxide dissolves into liquid, which brings a certain fluidity to the mixed composite lithium salt and nickel source, leading to the diffusion of the composite lithium salt, and increasing the contact between the composite lithium salt and the nickel source, thereby Li 2 O+NiO=Li 2 NiO 2, LiOH+NiO=Li 2 NiO 2 +H 2 Reactions such as O became more efficient, and the presence of a trace amount of lithium carbonate contributed to the synergistic diffusion of lithium hydroxide and lithium oxide during the sintering process.
[0023] Step 2, Mixing the composite lithium salt and nickel source Complex lithium salt xLiOH yLi 2 O·zLi 2 CO 3 ·wH 2 O was mixed with the lithium source and the nickel source in a molar ratio of 1.5 to 2.2:1.0 under an argon or nitrogen protective atmosphere, the mixing speed was 500 to 1000 rpm, and the mixing time was 0.5 to 6.0 h to obtain a mixed powder of the composite lithium salt and the nickel source. The nickel source is one or more of nickel(II) oxide, nickel trioxide, nickel dioxide, nickel hydroxide, nickel oxyhydroxide, nickel carbonate, nickel oxalate, and nickel acetate. The purity of argon or nitrogen is >99.995% and the flow rate is 6L / min. By thoroughly mixing the lithium source and the nickel source, a uniform distribution of the lithium and nickel components can be obtained, and the degree of the diffusion reaction between lithium and nickel during the sintering process can be improved, thereby improving the purity of the positive electrode lithium supplement additive for lithium ion batteries.
[0024] Step 3: Sintering In order to remove moisture and volatile matter remaining in the mixed powder and reduce residual alkali, the mixed powder of the composite lithium salt and nickel source is heated to 100-300°C at a heating rate of 1-10°C / min in a protective or oxidizing atmosphere and kept at that temperature for 0.5-5.0 hours. Then, the temperature is raised to 600-800°C at a heating rate of 1-10°C / min and kept at that temperature for 5.0-20.0 hours for high-temperature sintering to ensure sufficient reaction between the composite lithium salt and the nickel source, and the temperature is naturally lowered to room temperature in a furnace in a protective or oxidizing atmosphere to obtain a sintered material. The protective atmosphere is one or more of argon or nitrogen, with a gas purity of >99.995% and a flow rate of 6L / min. The oxidizing atmosphere is a protective atmosphere with an oxygen content of 50-200ppm. During the sintering process, when the temperature is >450°C, lithium hydroxide dissolves and becomes liquid, which brings a certain fluidity to the mixed powder, leading to the diffusion of the lithium source, and increases the contact between the lithium oxide and the nickel source, which makes the reaction more sufficient. The presence of a trace amount of lithium carbonate contributes to the synergistic diffusion of lithium hydroxide and lithium oxide during the sintering process. Meanwhile, the reasons why it is necessary to prepare a composite lithium salt in step 1 are as follows: (1) Simply Li 2 If O is used as the lithium source, Li 2 Because O is an inorganic oxide, its melting point is as high as 1567°C, and it is in a solid state throughout the entire sintering process. The lithium provided can only react through solid-state diffusion, which makes the reaction kinetically slow and limited in extent. (2) If LiOH is simply used as the raw material, a large amount of moisture will be released during the sintering process, resulting in a large amount of Li in the final product. 2 NiO 2 The blocking of Li in the final product is severe and difficult to process. 2 NiO 2 The purity of Li is significantly reduced, which leads to an increase in the residual alkali content. (3) The Li 2 O+LiOH+Li 2 CO 3 If a simple mixture of the above is used as the lithium raw material, the Li 2 O, LiOH, Li 2 CO 3 During the sintering process, the material is still separate, which does not have a good synergistic effect. After LiOH is dissolved, the diffusion surface of the lithium source due to the flow is limited, and Li 2 The lithium source provided by O remains in a solid-state diffusion state.
[0025] Step 4: Crushing The sintered material was crushed using a 1000-type high-speed mixer from Wuxi Xinguang Powder Technology Co., Ltd. under an argon or nitrogen protective atmosphere, dispersed at a rotation speed of 800-1000 rpm for 15-30 min, and then crushed using a 350-type mechanical crusher from Yixing Jingxin Powder Machinery Equipment Co., Ltd. under an argon or nitrogen protective atmosphere, and sieved through a 350-400 mesh sieve using a vibration sieve from Xinxiang Weiliang Sieving Machinery Co., Ltd. to obtain a crushed material with a particle size D50 of 5.0-15.0 μm and Dmax<25.0 μm. The purity of argon or nitrogen is >99.995% and the flow rate is 6L / min.
[0026] Step 5: Demagnetization Using a demagnetizer, demagnetize the crushed material so that the magnetic content is <50ppb, put the demagnetized crushed material into an aluminum laminate bag, and package it using a vacuum sealer to make it into the positive electrode lithium supplement additive Li for lithium-ion batteries. 2 NiO 2 obtained.
[0027] For the positive electrode lithium supplement additive of the lithium ion battery prepared by the method of the present invention, the topography is observed using the US FEIinspectF50 scanning electron microscope (SEM), and the XRD diagram is obtained and the phase composition is measured using the X'pertPro type X-ray diffractometer of the Dutch PANalytical Company, and then the composition content is detailed and quantitatively analyzed using the tool GSAS software, and the purity and impurity content of the product are calculated, and the residual alkali content of the material is measured using the Mettler G20S titration device, and the grain size of the material is measured using the Sympatec dry grain size analyzer, and the magnetic material content is measured by ICP test.
[0028] The lithium ion battery positive electrode lithium supplement additive obtained in the embodiment and the lithium supplement additive of the comparative example are used as the positive electrode material, and the lithium sheet is used as the negative electrode sheet to manufacture a CR2032 button battery, and the gram capacity and coulombic efficiency of the first charge and discharge are measured.The lower the coulombic efficiency, the higher the irreversible capacity, which shows that the effect of using lithium supplement is better.
[0029] A lithium ion battery positive electrode lithium supplement additive or lithium supplement additive:conductive agent SP:adhesive PVDF=85:5:10 mass ratio was prepared, and an N-methylpyrrolidone NMP solution with a solid content of 30% was prepared, uniformly stirred to obtain a positive electrode slurry, which was uniformly applied to an aluminum foil, dried in a vacuum at 120°C for 10h, and punched into a circular sheet with a diameter of 10mm to obtain a positive electrode sheet. The positive electrode sheet, the negative electrode sheet metal lithium sheet with a diameter of 16mm, the separator Celgard2400 microporous polypropylene film, and LiPF6 / EC+DMC were assembled into a CR2032 button battery in an argon glove box with a volume ratio of 1:1 and an electrolyte of 1mo1 / L.
[0030] The battery was kept at a constant temperature of 25°C, the voltage range was 3.0 to 4.3 V, and the battery was charged at a constant current and voltage of 0.05 C. The gram capacity of the charge and discharge of the CR2032 button battery was measured, the irreversible capacity (initial charge capacity - initial discharge capacity = irreversible capacity) was calculated, and the initial coulombic efficiency was calculated.
[0031] The positive electrode lithium supplement additive of the lithium ion battery of the present invention is Li 2 NiO 2 Mass purity >95%, total residual alkali (residual lithium) <3%, first charge gram capacity is 420~465mAh / g, irreversible capacity is 260~340mAh / g.
[0032] Example 1 Step 1, Preparation of complex lithium salts Lithium raw material 0.8LiOH-0.1Li 2 O-0.1Li 2 CO 3The mixture was heated to 650°C at a heating rate of 6°C / min under a vacuum environment of 30 Pa, kept at that temperature for 240 min, and cooled to room temperature while maintaining the vacuum. It was then taken out and ball milled with 5 mm zirconium balls at a ball to lithium raw material ratio of 10:1 at a rotation speed of 700 rpm for 0.5 h to obtain a composite lithium salt. The composition content of the composite lithium salt was detailed and quantitatively analyzed by XRD test and GSAS software, and the purity was calculated. The ratio of the composite lithium salt was 0.193LiOH·0.788Li 2 O 0.019Li 2 CO 3 It is.
[0033] As shown in Figure 1, XRD tests showed that LiOH, Li 2 O and Li 2 CO 3 A complex lithium salt phase of the formula (101) appears, where 2θ=32.58° corresponds to the (101) plane of LiOH, and 2θ=33.61° corresponds to the (102) plane of LiOH. 2 O (111) plane, and 2θ=31.94° corresponds to Li 2 CO 3 This corresponds to the (002) surface of the
[0034] Step 2, Mixing the composite lithium salt and nickel source The molar ratio of the lithium source to the nickel source was 2.0:1.0. 327.3 g of composite lithium salt and 746.9 g of nickel (II) oxide were weighed and mixed under a nitrogen protective atmosphere. The mixing speed was 500 rpm and the mixing time was 0.5 h to obtain a mixed powder of composite lithium salt and nickel source.
[0035] Step 3: Sintering The mixed powder of the composite lithium salt and nickel source was heated to 100°C at a rate of 1°C / min in a nitrogen atmosphere, kept at that temperature for 0.5 h, then heated to 600°C at a rate of 1°C / min, kept at that temperature for 20.0 h, and then allowed to cool naturally to room temperature in a furnace in a nitrogen atmosphere to obtain a sintered material.
[0036] Step 4: Crushing The sintered material was dispersed under a nitrogen protective atmosphere at a rotation speed of 800 rpm for 15 min, pulverized under a nitrogen protective atmosphere, and sieved through a 400 mesh sieve to obtain a pulverized material with a particle size D50 of 8.0 μm and Dmax of 21.0 μm.
[0037] Step 5: Demagnetization Using a demagnetizer, demagnetize the crushed material so that the total amount of magnetic material is 15ppb. Put the demagnetized crushed material into an aluminum laminate bag and package it using a vacuum sealer. Then, use it as a lithium ion battery positive electrode lithium supplement additive Li 2 NiO 2 obtained.
[0038] The positive electrode lithium supplement additive Li of the lithium ion battery of Example 1 2 NiO 2 As shown in Figure 2, the XRD test showed that the oxide was mainly composed of Li. 2 NiO 2 where 2θ=25.75° is the diffraction peak of Li 2 NiO 2 The (101) plane of LiO corresponds to the (101) plane of LiO, and 2θ=43.38° corresponds to the (200) plane of NiO. The composition content was detailed and quantitatively analyzed using the tool GSAS software, and the Li 2 NiO 2 The content of the components is 97.5%. As shown in Figure 3, the topography is single crystal spherical or rod-like particles, and the particle size is about 8.0 μm. The total residual alkali content was analyzed by titration equipment as 1.055%. The test results are shown in Table 1.
[0039] As shown in Figure 4, the test results show that the first charge gram capacity of Example 1 is 430mAh / g, the first discharge gram capacity is 105mAh / g, the available irreversible capacity is 325mAh / g, and the first coulombic efficiency is 24.4%. The test results are shown in Table 1.
[0040] Example 2 Step 1, Preparation of complex lithium salts Lithium raw material 0.8LiOH-0.1Li 2 O-0.1Li 2 C2 O 4 The mixture was heated to 950°C at a heating rate of 5°C / min under a vacuum environment of 90 Pa, kept at that temperature for 15 minutes, and cooled to room temperature while maintaining the vacuum. It was then taken out and ball milled with 5 mm zirconium balls at a ball to lithium raw material ratio of 15:1 at a rotation speed of 700 rpm for 0.5 hours to obtain a composite lithium salt. The composition content of the composite lithium salt was detailed and quantitatively analyzed by XRD test and GSAS software, and the purity was calculated. The ratio of the composite lithium salt was 0.068LiOH·0.900Li 2 O 0.032Li 2 CO 3 It is.
[0041] Step 2, Mixing the composite lithium salt and nickel source The molar ratio of the lithium source to the nickel source was 2.1:1.0. 335.7 g of composite lithium salt and 926.9 g of nickel hydroxide were weighed and mixed under an argon protective atmosphere. The mixing speed was 1000 rpm and the mixing time was 2.0 h to obtain a mixed powder of composite lithium salt and nickel source.
[0042] Step 3: Sintering The mixed powder of the composite lithium salt and nickel source was heated to 300°C at a heating rate of 5°C / min in an argon atmosphere, kept at that temperature for 2.0 hours, then heated to 750°C at a heating rate of 5°C / min, kept at that temperature for 20.0 hours, and then allowed to cool naturally to room temperature in a furnace in an argon atmosphere to obtain a sintered material.
[0043] Step 4: Crushing The sintered material was dispersed under an argon protective atmosphere at a rotation speed of 1000 rpm for 30 min, pulverized under an argon protective atmosphere, and sieved through a 350 mesh sieve to obtain a pulverized material with particle sizes D50=5.0 μm and Dmax=20.0 μm.
[0044] Step 5: Demagnetization Using a demagnetizer, demagnetize the crushed material so that the total amount of magnetic material is 20 ppb. Put the demagnetized crushed material into an aluminum laminate bag and package it using a vacuum sealer. Then, use it as a lithium ion battery positive electrode lithium supplement additive Li2 NiO 2 obtained.
[0045] The positive electrode lithium supplement additive Li of the lithium ion battery of Example 2 2 NiO 2 Li 2 NiO 2 The content of the components is 97.9%. The total residual alkali content was analyzed by titration apparatus as 2.119%. The test results are shown in Table 1.
[0046] According to the test, the first charge gram capacity of Example 2 is 435mAh / g, the first discharge gram capacity is 150mAh / g, the available irreversible capacity is 285mAh / g, and the first coulombic efficiency is 34.5%. The test results are shown in Table 1.
[0047] Example 3 Step 1, Preparation of complex lithium salts Lithium raw material 0.8LiOH-0.1Li 2 O 2 -0.1Li 2 CO 3 The mixture was heated to 800°C at a heating rate of 3°C / min under a vacuum environment of 40 Pa, kept at that temperature for 60 minutes, and cooled to room temperature while maintaining the vacuum. It was then taken out and ball milled with 5 mm zirconium balls at a ball to lithium raw material ratio of 15:1 at a rotation speed of 700 rpm for 0.5 hours to obtain a composite lithium salt. The composition content of the composite lithium salt was detailed and quantitatively analyzed by XRD test and GSAS software, and the purity was calculated. The ratio of the composite lithium salt was 0.100LiOH·0.895Li 2 O 0.005Li 2 CO 3 It is.
[0048] Step 2, Mixing the composite lithium salt and nickel source The molar ratio of the lithium source to the nickel source was 2.2:1.0. 341.6 g of composite lithium salt and 827.0 g of nickel trioxide were weighed and mixed under an argon protective atmosphere. The mixing speed was 900 rpm and the mixing time was 1.0 h to obtain a mixed powder of composite lithium salt and nickel source.
[0049] Step 3: Sintering The mixed powder of the composite lithium salt and nickel source was heated to 200°C at a heating rate of 2°C / min in an argon atmosphere, kept at that temperature for 1.0 h, then heated to 700°C at a heating rate of 2°C / min and kept at that temperature for 15.0 h. The temperature was then allowed to naturally decrease to room temperature in a furnace in an argon atmosphere to obtain a sintered material.
[0050] Step 4: Crushing The sintered material was dispersed under an argon protective atmosphere at a rotation speed of 900 rpm for 20 min, pulverized under an argon protective atmosphere, and sieved through a 400 mesh sieve to obtain a pulverized material with particle sizes D50=13.0 μm and Dmax=23.0 μm.
[0051] Step 5: Demagnetization Using a demagnetizer, the crushed material is demagnetized so that the total amount of magnetic material is 18 ppb. The demagnetized crushed material is placed in an aluminum laminate bag and packaged using a vacuum sealer. The Lithium-ion battery positive electrode lithium supplement additive Li 2 NiO 2 obtained.
[0052] The positive electrode lithium supplement additive Li of the lithium ion battery of Example 3 2 NiO 2 Li 2 NiO 2 The content of the components is 98.2%. The total residual alkali content was analyzed by titration to be 1.786%. The test results are shown in Table 1.
[0053] According to the test, the first charge gram capacity of Example 3 is 465mAh / g, the first discharge gram capacity is 125mAh / g, the available irreversible capacity is 340mAh / g, and the first coulombic efficiency is 26.9%. The test results are shown in Table 1.
[0054] Example 4 Step 1, Preparation of complex lithium salts Lithium raw material 0.8LiOH-0.1Li 2 O-0.1Li 2C 2 O 4 The mixture was heated to 700°C at a heating rate of 10°C / min under a vacuum environment of 20 Pa, kept at that temperature for 120 min, and cooled to room temperature while maintaining the vacuum. It was then taken out and ball milled with 5 mm zirconium balls at a ball to lithium raw material ratio of 11:1 at a rotation speed of 700 rpm for 0.5 h to obtain a composite lithium salt. The composition content of the composite lithium salt was detailed and quantitatively analyzed by XRD test and GSAS software, and the purity was calculated. The ratio of the composite lithium salt was 0.116LiOH·0.852Li 2 O 0.032Li 2 CO 3 It is.
[0055] Step 2, Mixing the composite lithium salt and nickel source The molar ratio of the lithium source to the nickel source was 1.5:1.0, and 243.6 g of composite lithium salt and 906.9 g of nickel dioxide were weighed and mixed under a nitrogen protective atmosphere. The mixing speed was 800 rpm and the mixing time was 3.0 hours to obtain a mixed powder of composite lithium salt and nickel source.
[0056] Step 3: Sintering The mixed powder of the composite lithium salt and nickel source was heated to 150°C at a heating rate of 10°C / min in a nitrogen atmosphere, kept at that temperature for 3.0 hours, then heated to 850°C at a heating rate of 10°C / min, kept at that temperature for 5.0 hours, and then allowed to cool naturally to room temperature in a furnace in a nitrogen atmosphere to obtain a sintered material.
[0057] Step 4: Crushing The sintered material was dispersed in a nitrogen protective atmosphere at a rotation speed of 850 rpm for 20 min, pulverized in a nitrogen protective atmosphere, and sieved through a 350 mesh sieve to obtain a pulverized material with D50=10.0 μm and Dmax=24.0 μm.
[0058] Step 5: Demagnetization Using a demagnetizer, demagnetize the crushed material so that the total amount of magnetic material is 30 ppb. Put the demagnetized crushed material into an aluminum laminate bag and package it using a vacuum sealer. Then, use it as a lithium ion battery positive electrode lithium supplement additive Li 2 NiO2 obtained.
[0059] The positive electrode lithium supplement additive Li of the lithium ion battery of Example 4 2 NiO 2 Li 2 NiO 2 The content of the components is 96.3%. The total residual alkali content was analyzed by titration apparatus as 2.785%. The test results are shown in Table 1.
[0060] According to the test, the first charge gram capacity of Example 4 is 423mAh / g, the first discharge gram capacity is 110mAh / g, the available irreversible capacity is 313mAh / g, and the first coulombic efficiency is 26.0%. The test results are shown in Table 1.
[0061] Example 5 Step 1, Preparation of complex lithium salts Lithium raw material 0.4LiH-0.1Li 2 O-0.5Li 2 CO 3 The mixture was heated to 400°C at a heating rate of 1°C / min under a vacuum environment of 10 Pa, kept at that temperature for 480 min, and cooled to room temperature while maintaining the vacuum. It was then taken out and ball milled with 5 mm zirconium balls at a ball to lithium raw material ratio of 13:1 at a rotation speed of 700 rpm for 0.5 h to obtain a composite lithium salt. The composition content of the composite lithium salt was detailed and quantitatively analyzed by XRD test and GSAS software, and the purity was calculated. The ratio of the composite lithium salt was 0.075LiOH·0.500Li 2 O 0.425Li 2 CO 3 1H 2 It is O.
[0062] Step 2, Mixing the composite lithium salt and nickel source The molar ratio of the lithium source to the nickel source was 1.8:1.0. 450.1 g of the composite lithium salt and 916.9 g of nickel oxyhydroxide were weighed and mixed under a nitrogen protective atmosphere. The mixing speed was 600 rpm and the mixing time was 4.0 hours to obtain a mixed powder of the composite lithium salt and the nickel source.
[0063] Step 3: Sintering The mixed powder of the composite lithium salt and nickel source was heated to 250°C at a heating rate of 3°C / min in a nitrogen atmosphere, maintained at that temperature for 4.0 hours, then heated to 690°C at a heating rate of 3°C / min, maintained at that temperature for 8.0 hours, and then allowed to cool naturally to room temperature in a furnace in a nitrogen atmosphere to obtain a sintered material.
[0064] Step 4: Crushing The sintered material was dispersed in a nitrogen protective atmosphere at a rotation speed of 950 rpm for 15 min, pulverized in a nitrogen protective atmosphere, and sieved through a 375 mesh sieve to obtain a pulverized material with D50=12.0 μm and Dmax=20.0 μm.
[0065] Step 5: Demagnetization Using a demagnetizer, demagnetize the crushed material so that the total amount of magnetic material is 25 ppb. Put the demagnetized crushed material into an aluminum laminate bag and package it using a vacuum sealer. Then, use it as a lithium ion battery positive electrode lithium supplement additive Li 2 NiO 2 obtained.
[0066] The positive electrode lithium supplement additive Li of the lithium ion battery of Example 5 2 NiO 2 Li 2 NiO 2 The content of the components is 97.2%. The total residual alkali content was analyzed by titration as 1.901%. The test results are shown in Table 1.
[0067] According to the test, the first charge gram capacity of Example 5 is 429mAh / g, the first discharge gram capacity is 125mAh / g, the available irreversible capacity is 304mAh / g, and the first coulombic efficiency is 29.1%. The test results are shown in Table 1.
[0068] Example 6 Step 1, Preparation of complex lithium salts Lithium raw material 0.8LiH-0.1Li 2 O-0.1Li 2 C 2 O4 The mixture was heated to 550°C at a heating rate of 8°C / min under a vacuum environment of 70 Pa, kept at the temperature for 550 min, and cooled to room temperature while maintaining the vacuum. It was then taken out and ball milled with 5 mm zirconium balls at a ball to lithium raw material ratio of 14:1 at a rotation speed of 700 rpm for 0.5 h to obtain a composite lithium salt. The composition content of the composite lithium salt was detailed and quantitatively analyzed by XRD test and GSAS software, and the purity was calculated. The ratio of the composite lithium salt was 0.418LiOH·0.550Li 2 O 0.032Li 2 CO 3 0.5H 2 It is O.
[0069] Step 2, Mixing the composite lithium salt and nickel source The molar ratio of the lithium source to the nickel source was 1.6:1.0, and 291.3 g of composite lithium salt and 1187.0 g of nickel carbonate were weighed and mixed under an argon protective atmosphere. The mixing speed was 700 rpm and the mixing time was 5.0 h, and a mixed powder of composite lithium salt and nickel source was obtained.
[0070] Step 3: Sintering The mixed powder of the composite lithium salt and nickel source was heated to 280°C at a heating rate of 4°C / min in an argon atmosphere, maintained at that temperature for 5.0 hours, then heated to 780°C at a heating rate of 4°C / min, maintained at that temperature for 10.0 hours, and then allowed to cool naturally to room temperature in a furnace in an argon atmosphere to obtain a sintered material.
[0071] Step 4: Crushing The sintered material was dispersed under an argon protective atmosphere at a rotation speed of 800 rpm for 20 min, pulverized under an argon protective atmosphere, and sieved through a 400 mesh sieve to obtain a pulverized material with D50=15.0 μm and Dmax=20.0 μm.
[0072] Step 5: Demagnetization Using a demagnetizer, demagnetize the crushed material so that the total amount of magnetic material is 45ppb. Put the demagnetized crushed material into an aluminum laminate bag and package it using a vacuum sealer. Then, use it as a lithium ion battery positive electrode supplement additive Li2 NiO 2 obtained.
[0073] The positive electrode lithium supplement additive Li of the lithium ion battery of Example 6 2 NiO 2 Li 2 NiO 2 The content of the components is 98.1%. The total residual alkali content was analyzed by titration apparatus as 2.538%. The test results are shown in Table 1.
[0074] According to the test, the first charge gram capacity of Example 6 is 455mAh / g, the first discharge gram capacity is 137mAh / g, the available irreversible capacity is 318mAh / g, and the first coulombic efficiency is 30.1%. The test results are shown in Table 1.
[0075] Example 7 Step 1, Preparation of complex lithium salts Lithium raw material 0.8LiH-0.1Li 2 O 2 -0.1Li 2 CO 3 The mixture was heated to 780°C at a heating rate of 4°C / min under a vacuum environment of 80 Pa, kept at the temperature for 150 min, and cooled to room temperature while maintaining the vacuum. It was then taken out and ball milled with 5 mm zirconium balls at a ball to lithium raw material ratio of 10:1 at a rotation speed of 700 rpm for 0.5 h to obtain a composite lithium salt. The composition content of the composite lithium salt was detailed and quantitatively analyzed by XRD test and GSAS software, and the purity was calculated. The ratio of the composite lithium salt was 0.120LiOH·0.875Li 2 O 0.005Li 2 CO 3 It is.
[0076] Step 2, Mixing the composite lithium salt and nickel source The molar ratio of the lithium source to the nickel source was 1.7:1.0, and 265.7 g of composite lithium salt and 1,467.1 g of nickel oxalate were weighed and mixed under a nitrogen protective atmosphere. The mixing speed was 650 rpm and the mixing time was 6.0 hours to obtain a mixed powder of composite lithium salt and nickel source.
[0077] Step 3: Sintering The mixed powder of the composite lithium salt and nickel source was heated to 160°C at a heating rate of 6°C / min in an oxygen atmosphere, kept at that temperature for 1.5 hours, then heated to 660°C at a heating rate of 6°C / min, kept at that temperature for 12.0 hours, and allowed to cool naturally to room temperature in a furnace in an oxygen atmosphere to obtain a sintered material. The oxygen content of the oxidizing atmosphere was 100 ppm.
[0078] Step 4: Crushing The sintered material was dispersed in a nitrogen protective atmosphere at a rotation speed of 1000 rpm for 30 min, pulverized in a nitrogen protective atmosphere, and sieved through a 400 mesh sieve to obtain a pulverized material with D50=6.0 μm and Dmax=21.0 μm.
[0079] Step 5: Demagnetization Using a demagnetizer, demagnetize the crushed material so that the total amount of magnetic material is 35 ppb. Put the demagnetized crushed material into an aluminum laminate bag and package it using a vacuum sealer. Then, use it as a lithium ion battery positive electrode lithium supplement additive Li 2 NiO 2 obtained.
[0080] The positive electrode lithium supplement additive Li of the lithium ion battery of Example 7 2 NiO 2 Li 2 NiO 2 The content of the components is 95.9%. The total residual alkali content was analyzed by titration apparatus as 2.177%. The test results are shown in Table 1.
[0081] According to the test, the first charge gram capacity of Example 7 is 420mAh / g, the first discharge gram capacity is 160mAh / g, the available irreversible capacity is 260mAh / g, and the first coulombic efficiency is 38.1%. The test results are shown in Table 1.
[0082] Example 8 Step 1, Preparation of complex lithium salts Lithium raw material 0.8LiH-0.1Li 2 O-0.1Li2 C 2 O 4 The mixture was heated to 900°C at a heating rate of 2°C / min under a vacuum environment of 50 Pa, kept at that temperature for 30 minutes, and cooled to room temperature while maintaining the vacuum. It was then taken out and ball milled with 5 mm zirconium balls at a ball to lithium raw material ratio of 15:1 at a rotation speed of 700 rpm for 0.5 hours to obtain a composite lithium salt. The composition content of the composite lithium salt was detailed and quantitatively analyzed by XRD test and GSAS software, and the purity was calculated. The ratio of the composite lithium salt was 0.048LiOH·0.950Li 2 O 0.002Li 2 CO 3 It is.
[0083] Step 2, Mixing the composite lithium salt and nickel source The molar ratio of the lithium source to the nickel source was 1.9:1.0, and 288.9 g of composite lithium salt and 1768.4 g of nickel acetate were weighed and mixed under a nitrogen protective atmosphere. The mixing speed was 850 rpm and the mixing time was 2.5 hours, and a mixed powder of composite lithium salt and nickel source was obtained.
[0084] Step 3: Sintering The mixed powder of the composite lithium salt and nickel source was heated to 230°C at a heating rate of 8°C / min in a nitrogen atmosphere, maintained at that temperature for 2.5 hours, then heated to 730°C at a heating rate of 8°C / min, maintained at that temperature for 18.0 hours, and then allowed to cool naturally to room temperature in a furnace in a nitrogen atmosphere to obtain a sintered material.
[0085] Step 4: Crushing The sintered material was dispersed in a nitrogen protective atmosphere at a rotation speed of 95,000 rpm for 25 min, pulverized in a nitrogen protective atmosphere, and sieved through a 400 mesh sieve to obtain a pulverized material with D50=7.0 μm and Dmax=22.0 μm.
[0086] Step 5: Demagnetization Using a demagnetizer, the crushed material is demagnetized so that the total amount of magnetic material is 42 ppb. The demagnetized crushed material is placed in an aluminum laminate bag and packaged using a vacuum sealer. The Lithium-ion battery positive electrode lithium supplement additive Li2 NiO 2 obtained.
[0087] The positive electrode lithium supplement additive Li of the lithium ion battery of Example 8 2 NiO 2 Li 2 NiO 2 The content of the components is 96.7%. The total residual alkali content was analyzed by titration to be 1.393%. The test results are shown in Table 1.
[0088] According to the test, the first charge gram capacity of Example 8 is 428mAh / g, the first discharge gram capacity is 157mAh / g, the available irreversible capacity is 271mAh / g, and the first coulombic efficiency is 36.7%. The test results are shown in Table 1.
[0089] Comparative Example 1 Using battery-grade lithium oxide with a purity of 99.9% as the lithium raw material, 50.27 g of lithium oxide and 228.47 g of nickel (II) oxide were taken, mixed into powder, heated to 200°C at a heating rate of 2°C / min under a nitrogen atmosphere, kept at that temperature for 1 hour, then heated to 750°C at a heating rate of 2°C / min and kept at that temperature for 10 hours, and cooled to room temperature after that to obtain the lithium replenishment additive of Comparative Example 1.
[0090] The lithium supplement additive of Comparative Example 1 was Li 2 NiO 2 The content of the components was 85.6% and the total residual alkali content was analyzed by titration as 9.019%. The test results are shown in Table 1.
[0091] According to the test, the lithium supplement additive of Comparative Example 1 has a first charge gram capacity of 350mAh / g, a first discharge gram capacity of 130mAh / g, an available irreversible capacity of 220mAh / g, and an initial coulombic efficiency of 37.1%. The test results are shown in Table 1.
[0092] Comparative Example 2 Using battery-grade lithium hydroxide with a purity of 99.9% as the lithium raw material, 240.38 g of lithium hydroxide and 357.13 g of nickel (II) oxide were mixed into powder, and the mixture was heated to 100°C at a heating rate of 3°C / min under a nitrogen atmosphere, kept at that temperature for 1.5 hours, then heated to 680°C at a heating rate of 2°C / min and kept at that temperature for 10 hours. After that, the mixture was cooled to room temperature to obtain the lithium replenishment additive of Comparative Example 2.
[0093] The lithium supplement additive of Comparative Example 2 was Li 2 NiO 2 The content of the components was 62.3% and the total residual alkali content was analyzed by titration as 12.846%. The test results are shown in Table 1.
[0094] According to the test, the lithium supplement additive of Comparative Example 2 has a first charge gram capacity of 290mAh / g, a first discharge gram capacity of 120mAh / g, an available irreversible capacity of 170mAh / g, and an initial coulombic efficiency of 41.4%. The test results are shown in Table 1.
[0095] Test Example 1 The positive electrode lithium supplement additive Li of the lithium ion battery of Example 1 2 NiO 2Select NCM811 as the lithium supplementary additive, and select NCM812 as the positive electrode active material. The amount of lithium supplementary additive added is 3 wt% of the mass of the positive electrode active material, and added to the positive electrode. The whole is used as a composite positive electrode active material. In a low humidity room with a dew point of -10°C, prepare an N-methylpyrrolidone NMP solution with a solid content of 70% in a mass ratio of composite positive electrode active material:conductive agent SP:adhesive PVDF = 97.2:1.5:1.3, and stir evenly to obtain a positive electrode slurry. The aluminum foil is coated with the solution, and the solution is dried in a vacuum at 120°C for 10 hours, slit and pressed to obtain a positive electrode sheet. A negative electrode active material (silicon monoxide, capacity 500mAh / g, initial efficiency 90%): An aqueous solution with a solid content of 45% was prepared in a mass ratio of SP:CMC:SBR=96:1:1:2, and stirred uniformly to obtain a negative electrode slurry. The slurry was applied to a copper foil, dried in a vacuum at 120°C for 10 minutes, slit and pressed to obtain a negative electrode sheet. A soft-pack lithium-ion battery was manufactured and obtained by the steps of winding, sealing, baking, liquid injection, pre-sealing, aging, chemical conversion, secondary sealing and volume fractionation using a positive electrode sheet, a negative electrode sheet, a separator Celgard2400 microporous polypropylene film and LiPF6 / EC+DMC in a volume ratio of 1:1, electrolyte 1mo1 / L, winding, sealing, baking, liquid injection, pre-sealing, aging, chemical conversion, secondary sealing and volume fractionation. The initial charge / discharge gram capacities were 208 and 160mAh / g, respectively, and the initial efficiency was 76.9%. The test results are shown in Table 2. The positive electrode lithium supplement additive Li of the lithium-ion battery obtained in the example 2 NiO 2 The residual alkali content of LiOH and Li 2 CO 3 The content of is low, the prepared positive electrode slurry has good fluidity and is less likely to gel, and the amount of gas generated in the soft-pack battery is small.
[0096] Test Example 2 The positive electrode lithium supplement additive Li of the lithium ion battery of Example 4 2 NiO 2 The lithium supplement additive Li was selected as the positive electrode of the lithium ion battery obtained in the embodiment, and the lithium supplement additive Li was used to manufacture a soft-pack lithium ion battery in the same manner as in the embodiment. The initial charge / discharge capacity was 206 and 158 mAh / g, respectively, and the initial efficiency was 76.7%. The test results are shown in Table 2.2 NiO 2 The residual alkali content of LiOH and Li 2 CO 3 The content of is low, the prepared positive electrode slurry has good fluidity and is less likely to gel, and the amount of gas generated in the soft-pack battery is small.
[0097] Test Example 3 The lithium supplement additive of Comparative Example 1 was selected as the lithium supplement additive, and a soft-pack lithium ion battery was manufactured and tested using the same method as in Test Example 1, obtaining initial charge / discharge gram capacities of 195 and 169 mAh / g, respectively, and an initial efficiency of 86.7%. The test results are shown in Table 2. The residual alkali content of the lithium supplement additive of Comparative Example was higher than that of the Example, and the amount of LiOH and Li 2 CO 3 The content of is high, and the prepared positive electrode slurry has normal fluidity and is prone to gelation.
[0098] [Table 1]
[0099] From the data comparison in Table 1, the positive electrode lithium supplement additive Li of the lithium ion battery of the present invention 2 NiO 2 When using the positive electrode lithium supplement additive Li of the lithium ion battery, compared with the preparation method of the comparative example, 2 NiO 2 It was found that the purity of the lithium-ion battery was significantly improved, the residual alkaline content was significantly reduced, and the gram capacity of the lithium-ion battery on first charge was significantly improved.
[0100] [Table 2]
[0101] From the data comparison in Table 2, the positive electrode lithium supplement additive Li of the lithium ion battery of the present invention 2 NiO 2was used in a soft-pack lithium-ion battery, and the gram capacity of the first charge was compared with that of the comparative lithium supplement additive, and it was found that the gram capacity of the first charge was significantly improved, but the gram capacity of the first discharge remained at the same level, so that the available irreversible capacity was greater. The greater the initial efficiency loss caused by the lithium supplement additive, the more lithium can be supplemented to the negative electrode material, and the better the lithium supplement effect.
Claims
1. A positive electrode lithium supplement additive for a lithium ion battery, comprising: Li 2 NiO 2 The purity is >95%, the total amount of residual alkali is <3%, the gram capacity of the first charge is 420-465 mAh / g, and the irreversible capacity is 260-340 mAh / g; The measurement conditions for the gram capacity and irreversible capacity of the first charge are as follows: The lithium ion battery positive electrode lithium supplement additive is used as a positive electrode material, and a lithium sheet is used as a negative electrode sheet to manufacture a CR2032 button battery, and the battery is kept at a constant temperature of 25°C, and the voltage range is 3.0-4.3V, and the battery is charged at a constant current and voltage of 0.05C. The gram capacity of the first charge and first discharge of the CR2032 button battery is measured, and the irreversible capacity (first charge capacity-first discharge capacity=irreversible capacity) is calculated.
2. A method for preparing a lithium ion battery positive electrode lithium supplement additive, comprising the steps of: Step 1: Preparation of complex lithium salt At room temperature, the lithium raw material is heated to 400 to 950 ° C. at a rate of 1 to 10 ° C. / min under a vacuum degree of < 100 Pa, and the temperature is maintained for 15 to 480 min. The vacuum degree is maintained, and the temperature is naturally lowered to room temperature in the furnace. Then, the material is taken out and crushed to obtain a composite lithium salt xLiOH.yLi. 2 O.zLi 2 CO 3 ・wH 2 O, where x, y, and z are mass fractions, 0<x<0.5, 0.5≦y<1.0, 0<z<0.5, x+y+z=1, and w represents the content of water of crystallization, 0≦w≦1; the lithium raw material is one or more of a lithium hydroxide-lithium oxide-lithium carbonate complex, a lithium hydroxide-lithium oxide-lithium oxalate complex, a lithium hydroxide-lithium peroxide-lithium carbonate complex, a lithium hydroxide-lithium peroxide-lithium oxalate complex, a lithium hydride-lithium oxide-lithium carbonate complex, a lithium hydride-lithium oxide-lithium oxalate complex, a lithium hydride-lithium peroxide-lithium carbonate complex, a lithium hydride-lithium peroxide-lithium oxalate complex, a lithium hydride-lithium peroxide-lithium carbonate complex, and a lithium hydride-lithium peroxide-lithium oxalate complex; Step 2: Mixing the composite lithium salt with the nickel source Mix the composite lithium salt with the lithium source and the nickel source in a molar ratio of 1.5 to 2.2:1.0 under an argon or nitrogen protective atmosphere at a rotation speed of 500 to 1000 rpm for 0.5 to 6.0 hours to obtain a mixed powder of the composite lithium salt and the nickel source; the nickel source is one or more of nickel(II) oxide, nickel trioxide, nickel dioxide, nickel hydroxide, nickel oxyhydroxide, nickel carbonate, nickel oxalate, and nickel acetate; Step 3: Sintering The mixed powder of the composite lithium salt and the nickel source is heated to 100-300°C at a heating rate of 1-10°C / min in a protective atmosphere or an oxidizing atmosphere, and is kept at the same temperature for 0.5-5.0 hours. Then, the mixed powder is heated to 600-800°C at a heating rate of 1-10°C / min, and is kept at the same temperature for 5.0-20.0 hours. The mixed powder is then naturally cooled to room temperature in a furnace to obtain a sintered material. Step 4: Crushing The sintered material is dispersed and pulverized under argon or nitrogen protective atmosphere at a rotation speed of 800-1000 rpm for 15-30 min, and then sieved through a 350-400 mesh sieve to obtain the positive electrode lithium supplement additive for lithium ion battery.
3. The method for preparing the lithium supplement additive for positive electrode of lithium ion battery as claimed in claim 2, characterized in that after step 4, the additive is demagnetized so that the magnetic content is <50ppb.
4. The method for preparing the positive electrode lithium supplement additive of lithium ion battery according to claim 2 or 3, characterized in that in step 1, crushing is carried out by ball milling with zirconium balls of diameter 5mm, balls and lithium raw material mass ratio of 10-15:1, and rotation speed of 700 rpm for 0.5 h.
5. The preparation method of lithium ion battery positive electrode lithium supplement additive as claimed in claim 2 or 3, characterized in that: in step 1, the mass purity of lithium raw material is >99%, in step 2, the purity of argon or nitrogen is >99.995%, and the flow rate is 6L / min; in step 3, the protective atmosphere is one or more of argon or nitrogen, the gas purity is >99.995%, and the flow rate is 6L / min; the oxidizing atmosphere is the protective atmosphere with oxygen content of 50-200ppm; in step 4, the purity of argon or nitrogen is >99.995%, and the flow rate is 6L / min.
6. The preparation method of the positive electrode lithium supplement additive of lithium ion battery according to claim 2 or 3, characterized in that in step 4, the sieve is sieved through 350-400 mesh, and the particle size D50 is 5.0-15.0 μm, Dmax < 25.0 μm.
7. A lithium ion battery comprising a positive electrode and a lithium supplement additive added to a positive electrode active material of the positive electrode, The lithium ion battery positive electrode lithium supplement additive of claim 1 is used.
Citation Information
Patent Citations
Positive electrode for ultrafast charging lithium ion battery and a preparation method and application thereof
CN108987672A
Method for producing irreversible additive contained in cathode material for lithium secondary battery, cathode material containing irreversible additive produced by the method, and lithium secondary battery containing the cathode material
JP2020516039A
A forming method of cathode active material layer of a lithium secondary battery developing coating uniformity, and a cathode of lithium secondary battery formed therefrom and a lithium ...
KR1020080108723A
Positive active material for rechargeable lithium battery and rechargeable lithium battery comprising same
KR1020100036896A
Lithium compound, nickel-based cathode active material, method for preparing lithium oxide, method for preparing nickel-based cathode active material, and secondary battery using same
WO2020096212A1