Active energy ray curable composition, cured product, lens and camera module

The active energy ray-curable composition addresses productivity and thinness challenges in camera modules by forming lenses with high Abbe number, heat resistance, and crack-resistant inorganic layers, enhancing performance under thermal and humidity stress.

JP7559386B2Active Publication Date: 2024-10-02DIC CORP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2020118355
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-09
Publication Date
2024-10-02
Estimated Expiration
2040-07-09

AI Technical Summary

Technical Problem

Conventional methods for producing camera modules face limitations in productivity and thinness, with wafer-level lenses experiencing issues such as peeling, defects, and cracks due to thermal history, especially under high temperature and humidity conditions, and sedimentation of fine particles in resin compositions.

Method used

An active energy ray-curable composition containing specific polycarbonate diol di(meth)acrylate, compounds with (meth)acryloyl groups and multi-branched structures, and cyclic structures, which form lenses with high Abbe number, excellent heat and moisture resistance, and crack-resistant inorganic layers.

Benefits of technology

The composition allows for lenses with high Abbe number, reduced chromatic aberration, and improved heat and humidity resistance, preventing peeling and cracks, suitable for wafer-level lenses and camera modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559386000001
    Figure 0007559386000001
  • Figure 0007559386000002
    Figure 0007559386000002
  • Figure 0007559386000003
    Figure 0007559386000003
Patent Text Reader

Abstract

To provide an active energy ray-curable composition capable of producing a lens having a high Abbe number, heat resistance and moist heat resistance, and to provide a cured product, a lens and a camera module.SOLUTION: The active energy ray-curable composition is used which contains: a polycarbonate diol di(meth)acrylate (A) represented by general formula (1); a compound (B) having one or two (meth)acryloyl groups, an alkylene glycol structure and a cyclic structure in one molecule other than the polycarbonate diol di(meth)acrylate (A); and a compound (C) having six or more (meth)acryloyl groups and a multi-branched structure in one molecule other than the polycarbonate diol di(meth)acrylate (A) and the compound (B).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an active energy ray-curable composition, a cured product, a lens, and a camera module. [Background technology]

[0002] In recent years, the demand for small camera modules for electronic devices such as smartphones and mobile PCs has been rapidly expanding, and development aimed at improving the production efficiency of camera modules has been actively undertaken. In addition, as electronic devices have become thinner, the demand for thinner camera modules has also become stricter. Conventionally, camera modules have been produced by molding resin lenses by injection molding using thermoplastic resins such as cycloolefin polymers and assembling them into lens units. However, the conventional method has limitations in productivity and thinning. In response to such market trends, a production method for camera modules that achieves both productivity and thinning has been disclosed (Patent Document 1), in which wafer-level lenses molded by a replica method are stacked together to assemble a lens unit.

[0003] Generally, lens units are determined by their optical constants, mainly the refractive index (n d ) and Abbe number (ν d ) A plurality of lenses with different refractive indices are superimposed to correct chromatic aberration and realize high pixel count. As a material for the wafer-level lens, an active energy ray-curable resin composition is preferably used from the viewpoints of productivity, transparency, heat resistance, etc. In particular, a resin composition using polycarbonate diol (meth)acrylate having an aliphatic skeleton has been disclosed as a wafer-level lens material having an optical constant with a medium refractive index and a high Abbe number (Patent Document 2).

[0004] Since wafer level lenses are expected to be directly mounted on a substrate, they are required to have heat resistance that can withstand solder reflow (170°C to 260°C). Methods of adding thiol compounds or antioxidants have been disclosed to improve heat resistance (Patent Document 3, Patent Document 4). In addition, they are required to have moisture and heat resistance that can withstand a moist heat test (85°C-85% RH-1000h) to confirm reliability under high temperature and high humidity conditions according to the mode of use. However, there have been no reports of wafer level lenses that have excellent moisture and heat resistance without substrate peeling or defects inside the lens under harsh temperature and humidity test conditions of 85°C-85% RH. In particular, aliphatic skeletons that show optical constants with a medium refractive index and high Abbe number are hydrophobic and prone to abnormalities after moist heat tests.

[0005] It is common to provide an anti-reflection layer on the lens surface in order to improve the contrast during imaging. If a similar anti-reflection layer is provided on a wafer-level lens, there is a problem that cracks will occur in the anti-reflection layer after the solder reflow process after mounting. A method of blending silica fine particles has already been disclosed as a resin composition for lenses that has excellent crack resistance for the anti-reflection layer (Patent Document 5, Patent Document 6). However, the use of fine particles poses new problems, such as the sedimentation or aggregation of fine particles in the resin composition, and the deterioration of handleability in the manufacturing process due to the high viscosity of the resin composition.

[0006] Therefore, there has been a demand for a material capable of forming a lens having a high Abbe number and transmittance, excellent heat resistance and moist heat resistance, and capable of suppressing the occurrence of cracks due to thermal history in inorganic layers, such as an antireflection layer, laminated on the surface. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2009-251368 A [Patent Document 2] International Publication No. 2019 / 124156 [Patent Document 3] JP 2014-52424 A [Patent Document 4] International Publication No. 2018 / 030351 [Patent Document 5] International Publication No. 2019 / 142601 [Patent Document 6] International Publication No. 2019 / 167461 Summary of the Invention [Problem to be solved by the invention]

[0008] The problem to be solved by the present invention is to provide an active energy ray-curable composition capable of forming a lens having a high Abbe number and transmittance, little change in transmittance even after solder reflow, excellent heat resistance and moist heat resistance, and crack resistance such that no cracks occur even after the inorganic layer formed on the surface is subjected to a thermal history. [Means for solving the problem]

[0009] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that the above problems can be solved by using an active energy ray-curable composition containing a specific polycarbonate diol di(meth)acrylate, a specific compound having a (meth)acryloyl group, an alkylene glycol structure, and a cyclic structure, and a specific compound having a (meth)acryloyl group and a multi-branched structure, and have thus completed the present invention.

[0010] That is, the present invention relates to an active energy ray-curable composition, a cured product, a lens, and a camera module, which contain a polycarbonate diol di(meth)acrylate (A) represented by the following general formula (1), a compound (B) other than the polycarbonate diol di(meth)acrylate (A) having one or two (meth)acryloyl groups, an alkylene glycol structure, and a cyclic structure in one molecule, and a compound (C) having six or more (meth)acryloyl groups and a multibranched structure in one molecule.

[0011] [ka] (In the formula, R 1 each independently represents a hydrogen atom or a methyl group; R 2 each independently represents a hydrocarbon group having 1 to 10 carbon atoms, and n is an integer of 1 to 10. Effect of the Invention

[0012] The active energy ray-curable composition of the present invention can be easily cured by irradiation with active energy rays, and can be suitably used for producing lenses by photoimprinting.

[0013] The lens formed by the active energy ray curable composition of the present invention has a high Abbe number and can reduce chromatic aberration. In addition, the lens has heat resistance with a small change in transmittance before and after solder reflow, and can be suitably used as a wafer level lens. Furthermore, since the lens has moist heat resistance that does not cause peeling or defects from the substrate even under high temperature and high humidity, it can be suitably used as a wafer level lens with excellent long-term stability. In addition, since the inorganic layer formed on the lens surface is suppressed from cracking due to heat history, it can be suitably used as a wafer level lens equipped with an inorganic layer such as an antireflection layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The active energy ray-curable composition of the present invention contains a polycarbonate diol di(meth)acrylate (A) represented by general formula (1), a compound (B) other than the polycarbonate diol di(meth)acrylate (A) having one or two (meth)acryloyl groups, an alkylene glycol structure and a cyclic structure in one molecule, and a compound (C) having six or more (meth)acryloyl groups and a multi-branched structure in one molecule.

[0015] In the present invention, "(meth)acrylate" means acrylate and / or methacrylate. "(meth)acryloyl" means acryloyl and / or methacryloyl. "(meth)acrylic" means acrylic and / or methacrylic.

[0016] The polycarbonate diol di(meth)acrylate (A) represented by the general formula (1) (hereinafter, abbreviated as "component (A)") has a structure represented by the following general formula (1): By using the component (A), an active energy ray-curable composition capable of forming a lens having a high Abbe number and excellent heat resistance can be obtained.

[0017] [ka] (In the formula, R 1 each independently represents a hydrogen atom or a methyl group; R 2 each independently represents a hydrocarbon group having 1 to 10 carbon atoms, and n is an integer of 1 to 10.

[0018] As the component (A), among the compounds represented by the general formula (1), a compound represented by R 1 is preferably a hydrogen atom, and R 2 are each independently preferably a linear hydrocarbon group having 5 to 6 carbon atoms or a cyclic hydrocarbon group having 6 to 10 carbon atoms, and n is preferably an integer of 4 to 10. Furthermore, from the viewpoint of easily preventing crystallization and warping of the lens over time, R 2 More preferably, each independently has a linear hydrocarbon group having 5 to 6 carbon atoms, a cyclohexane structure, or an isosorbide structure, and n is more preferably an integer of 4 to 6.

[0019] In the general formula (1), R 2When a linear hydrocarbon group having 5 to 6 carbon atoms and a cyclic hydrocarbon group having 6 to 10 carbon atoms, and n is an integer of 4 to 6, is used, the mass ratio of the linear hydrocarbon group having 5 to 6 carbon atoms to the cyclic hydrocarbon group having 6 to 10 carbon atoms is preferably in the range of 10 / 90 to 90 / 10, more preferably in the range of 20 / 80 to 80 / 20, and particularly preferably in the range of 60 / 40 to 80 / 20.

[0020] The component (A) may, for example, be a reaction product of a polycarbonate diol with (meth)acrylic acid and / or a (meth)acrylic acid ester.

[0021] The polycarbonate diol may, for example, be a reaction product between a compound having two or more hydroxyl groups and a carbonate ester.

[0022] Examples of the compound having two or more hydroxyl groups include an alkylene diol having a linear structure, an alkylene diol having a branched structure, an alkylene diol having a cyclic structure, a diol having a heterocyclic structure, etc. These compounds can be used alone or in combination of two or more kinds.

[0023] Examples of the alkylene diol having a linear structure include 1,2-ethanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol.

[0024] Examples of the alkylene diol having a branched chain structure include 1,2-propanediol, 1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 2,2-dimethyl-1,3-propanediol, 3-methyl-1,3-butanediol, 2-methyl-1,3-butanediol, 1,2-hexanediol, 1,5-hexanediol, 2,5-hexanediol, 3-methyl-1,5-pentanediol, 2,3-dimethyl-2,3-butanediol, 2- Examples of the alkyl esters include ethyl-2-methyl-1,3-propanediol, 1,2-heptanediol, 2-methyl-2-propyl-1,3-propanediol, 2,4-dimethyl-2,4-pentanediol, 3,6-octanediol, 2,2,4-trimethyl-1,3-pentanediol, 2,5-dimethyl-2,5-hexanediol, 2-ethyl-1,3-hexanediol, 1,2-nonanediol, 1,8-nonanediol, 2,8-nonanediol, 2-butyl-2-ethyl-1,3-propanediol, 2,4-diethyl-1,5-pentanediol, 1,2-decanediol, and 2,2-diisobutyl-1,3-propanediol.

[0025] Examples of the alkylene diol having a cyclic structure include 1,2-cyclopentanediol, 1,3-cyclopentanediol, 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 1,3-adamantanediol, and 1-hydroxy-3-adamantylmethanol.

[0026] Examples of the diol having a heterocyclic structure include 3,4-tetrahydrofuran diol, 1,4-dioxane-2,3-diol, 1,1-bicyclohexyl-4,4-diol, and hexahydrofuro[3,2-b]furan-3,6-diol.

[0027] Examples of the carbonate ester include dimethyl carbonate, diethyl carbonate, diphenyl carbonate, ethylene carbonate, propylene carbonate, etc. These compounds can be used alone or in combination of two or more kinds.

[0028] Examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, etc. These (meth)acrylic acid esters can be used alone or in combination of two or more.

[0029] Commercially available products of the component (A) include, for example, "UH-100DA", "UM-90(1 / 3)DA", "UM-90(1 / 1)DA", "UM-90(3 / 1)DA", "UH-100DM", "UM-90(1 / 3)DM", "UM-90(1 / 1)DM", and "UM-90(3 / 1)DM" manufactured by Ube Industries, Ltd.

[0030] The content of the component (A) in the active energy ray-curable composition is preferably in the range of 5 to 70 mass %, more preferably in the range of 10 to 60 mass %, and particularly preferably in the range of 20 to 50 mass %, because an active energy ray-curable composition capable of forming a lens having a high Abbe number and excellent heat resistance and moist heat resistance can be obtained.

[0031] The compound (B) having one or two (meth)acryloyl groups, an alkylene glycol structure, and a cyclic structure in one molecule (hereinafter, abbreviated as "component (B)") essentially has one or two (meth)acryloyl groups, an alkylene glycol structure, and a cyclic structure in one molecule. By using the component (B), an active energy ray-curable composition capable of forming a lens having a high Abbe number, excellent heat resistance and moist heat resistance, and excellent crack resistance of the inorganic layer can be obtained.

[0032] Examples of the cyclic structure include single ring structures such as a cyclopentane structure, a cyclohexane structure, a cyclooctane structure, and a cyclodecane structure, a perhydroindene structure, a perhydroanthracene structure, a perhydrofluorene structure, a perhydrophenanthrene structure, a perhydroacenaphthene structure, a perhydrophenalene structure, a norbornane structure, an isobornane structure, an isobornyl structure, an adamantane structure, a bicyclo[3.3.0]octane structure, and a tricyclo[5.2.1.0]octane structure. 2,6 ] decane structure, tricyclo[6.2.1.0 2,7 ]undecane structure, dicyclopentanyl structure, dicyclopentenyl structure, and other polycyclic structures; tetrahydrofuran structure, 1,3-dioxolane structure, 1,3-dioxane structure, 1,4 dioxane structure, hexahydrofuro[3,2-b]furan structure, and other heterocyclic structures; benzene structure, naphthalene structure, fluorene structure, acenaphthene structure, phenalene structure, anthracene structure, phenanthrene structure, tetracene structure, chrysene structure, pyrene structure, triphenylene structure, pentacene structure, benzopyrene structure, perylene structure, and other aromatic ring structures. These cyclic structures may be present alone or in one molecule, or may have two or more kinds. Among these, cyclohexane structure, tricyclo[5.2.1.0]undecane structure, dicyclopentanyl structure, dicyclopentenyl structure, and other polycyclic structures are preferred, since they can provide an active energy ray-curable composition capable of forming a lens having a high Abbe number and excellent heat resistance. 2,6 ] The decane structure is preferred.

[0033] In the component (B), the cyclic structure and the (meth)acryloyl group may be bonded directly or via a linking group.

[0034] Examples of the linking group include an oxygen atom, a linear and / or branched hydrocarbon group having 1 to 10 carbon atoms, an alkylene oxide group having 1 to 10 repeating numbers, an alkyl ester group having 1 to 10 repeating numbers which is a ring-opening polymer of caprolactone, and an amide group.

[0035] Examples of the alkylene glycol structure include 1,2-ethanediol (ethylene glycol), 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,2-propanediol (propylene glycol), 1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 2,2-dimethyl-1,3-propanediol (neopentyl glycol), 3-methyl-1,3-butanediol, 2-methyl-1,3-butanediol, 1,2-hexanediol, ethanol, 1,5-hexanediol, 2,5-hexanediol, 3-methyl-1,5-pentanediol, 2,3-dimethyl-2,3-butanediol, 2-ethyl-2-methyl-1,3-propanediol, 1,2-heptanediol, 2-methyl-2-propyl-1,3-propanediol, 2,4-dimethyl-2,4-pentanediol, 3,6-octanediol, 2,2,4-trimethyl 1,3-pentanediol, 2,5-dimethyl-2,5-hexanediol, 2-ethyl-1,3-hexanediol, 1,2-nonanediol, 1,8-nonanediol, 2,8-nonanediol, 2-butyl-2-ethyl-1,3-propanediol, 2,4-diethyl-1,5-pentanediol, 1,2-decanediol, 2,2-diisobutyl-1,3-propanediol, etc. These alkylene glycol structures may be present in one molecule, or may have two or more types. Among these, ethylene glycol, propylene glycol, and neopentyl glycol are preferred because they can provide an active energy ray-curable composition capable of forming a lens having excellent heat resistance and moist heat resistance. Furthermore, the number of repeating units of the alkylene glycol structure is preferably 2 to 15, because they can provide an active energy ray-curable composition capable of forming a lens having better moist heat resistance and crack resistance.

[0036] Specific examples of the component (B) include cyclopentyl alkylene oxide-modified (meth)acrylate, 1-methylcyclopentyl alkylene oxide-modified (meth)acrylate, 1-ethylcyclopentyl alkylene oxide-modified (meth)acrylate, cyclohexyl alkylene oxide-modified (meth)acrylate, 1-methylcyclohexyl alkylene oxide-modified (meth)acrylate, 1-ethylcyclohexyl alkylene oxide-modified (meth)acrylate, trimethylcyclohexyl alkylene oxide-modified (meth)acrylate, Acrylate, 4-tertiary butylcyclohexyl alkylene oxide modified (meth)acrylate, 2-cyclohexylpropanyl alkylene oxide modified (meth)acrylate, hydrogenated bisphenol A alkylene oxide modified di(meth)acrylate, hydrogenated bisphenol F alkylene oxide modified di(meth)acrylate, benzyl alkylene oxide modified (meth)acrylate, phenyl alkylene oxide modified (meth)acrylate, nonylphenol alkylene oxide modified (meth)acrylate, phenoxybenzyl alkenyl alkylene oxide modified (meth)acrylate, phenylbenzyl alkylene oxide modified (meth)acrylate, biphenyl alkylene oxide modified (meth)acrylate, bisphenol A alkylene oxide modified di(meth)acrylate, bisphenol F alkylene oxide modified di(meth)acrylate, fluorene alkylene oxide modified di(meth)acrylate, isobornyl alkylene oxide modified (meth)acrylate, isobornyl alkylene oxide modified di(meth)acrylate, dicyclopentanyl alkylene oxide modified di(meth)acrylate Side-modified (meth)acrylate, dicyclopentenyl alkylene oxide-modified (meth)acrylate, tricyclodecane diol alkylene oxide-modified di(meth)acrylate, tricyclodecane dimethanol alkylene oxide-modified di(meth)acrylate, adamantyl alkylene oxide-modified (meth)acrylate, adamantyl alkylene oxide-modified di(meth)acrylate, 2-methyl adamantyl alkylene oxide-modified (meth)acrylate, 2-ethyl adamantyl alkylene oxide-modified (meth)acrylate,Examples of the alkylene oxide-modified (meth)acrylate include 2-isopropyladamantyl alkylene oxide-modified (meth)acrylate, (3-ethyloxetan-3-yl)methyl alkylene oxide-modified (meth)acrylate, tetrahydrofurfuryl alkylene oxide-modified (meth)acrylate, (2-oxo-1,3-dioxolan-4-yl)methyl alkylene oxide-modified (meth)acrylate, and isosorbide alkylene oxide-modified di(meth)acrylate. These compounds can be used alone or in combination of two or more. Among these, hydrogenated bisphenol A alkylene oxide-modified di(meth)acrylate and tricyclodecane dimethanol alkylene oxide-modified di(meth)acrylate are preferred because they can provide an active energy ray-curable composition capable of forming a lens having a high Abbe number, and excellent heat resistance, moist heat resistance, and crack resistance.

[0037] Commercially available products of the component (B) include, for example, Miramer M1142, Miramer M140, Miramer M141, Miramer M142, Miramer M144, Miramer M164, Miramer M166, Miramer M1602, Miramer M240, Miramer M241, Miramer M244, Miramer M245, Miramer M2100, Miramer M2101, Miramer M2200, Miramer M2300, Miramer M2301, and Miramer M290 manufactured by MIWON Co., Ltd.; and NK Ester AMP-10G, NK Ester AMP-20GY, NK Ester AMP-10G, NK Ester 702A, NK Ester A-LEN-10, NK Ester 401P, NK Ester A-BPEF, and NK Ester A-BPE-2", "NK Ester ABE-300", "NK Ester A-BPE-4", "NK Ester A-BPE-10", "NK Ester A-BPE-20", "NK Ester A-BPE-30", "NK Ester A-BPP-3", "NK Ester A-B1206PE", "NK Ester PHE-1G", "NK Ester PHE-2G", "NK Ester BPE-80N", "NK Ester BPE-100", "NK Ester BPE-200", "NK Ester BPE-300", "NK Ester BPE-500", "NK Ester BPE-900", "NK Ester BPE-1300N", Osaka Organic Chemical Industry Co., Ltd.'s "Viscoat #192", "Viscoat #700HV", "Viscoat #540", Kyoeisha Chemical Co., Ltd.'s "Light Ester PO", "Light Ester BP-2EMK", "Light Acrylate PO-A", "Light Acrylate P2H-A", "Light Acrylate P-200A", "Epoxy Ester M-600A", "Light Acrylate BP-4PA", Nippon Kayaku Co., Ltd.'s "KAYARAD R-128H", "KAYARAD R-551", "KAYARADR-712" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. "New Frontier PHE", "New Frontier PHE-2", "New Frontier PHE-2D", "New Frontier NP-1", "New Frontier NP-4", "New Frontier N-177E", "New Frontier N-PGA", "New Frontier OPPE", "New Frontier BPE-4", "New Frontier BPE-10", "New Frontier BPE-20", "New Frontier BPEM- 4," "New Frontier BPEM-10," "New Frontier HBPE-4," and "New Frontier HBPEM-10," as well as Hitachi Chemical Co., Ltd.'s "Fancryl FA-310A," "Fancryl FA-314A," "Fancryl FA-318A," "Fancryl FA-321A," "Fancryl FA-324A," "Fancryl FA-310M," "Fancryl FA-320M," "Fancryl FA321M," and "Fancryl FA-3218M."

[0038] The content of the component (B) in the active energy ray-curable composition is preferably in the range of 10 to 60 mass%, more preferably in the range of 15 to 55 mass%, and particularly preferably in the range of 20 to 50 mass%, because an active energy ray-curable composition capable of forming a lens having a high Abbe number and excellent heat resistance and moist heat resistance can be obtained.

[0039] The compound (C) having six or more (meth)acryloyl groups and a multi-branched structure in one molecule (hereinafter abbreviated as "component (C)") essentially has six (meth)acryloyloxy groups and a multi-branched structure in one molecule. By using the component (C), an active energy ray-curable composition capable of forming a lens having excellent crack resistance can be obtained.

[0040] The (meth)acryloyl groups in one molecule of the component (C) are preferably in the range of 6 to 96, more preferably in the range of 8 to 64, and particularly preferably in the range of 9 to 48, since this gives an active energy ray-curable resin composition having excellent crack resistance.

[0041] Examples of the multi-branched structure include a dendron structure, a dendritic structure (a branched structure), a hyperbranched structure (a hyperbranched structure), and a star structure. One molecule may have one or more of these multi-branched structures. Among these, the dendritic structure and the hyperbranched structure are preferred because they can provide an active energy ray-curable composition capable of forming a lens having particularly excellent crack resistance.

[0042] The method for producing the component (C) is not particularly limited, and it can be produced by a known method as appropriate. For example, the divergent method in which a branch is formed by bonding a molecule to a central core molecule for each generation, the convergent method in which a branch portion synthesized in advance is bonded to a core molecule, and a method of synthesis in one step using a monomer ABx having a branch portion having two or more reaction points B and a linking portion having another reaction point A in one molecule can be mentioned. Among them, the divergent method is preferred as one of the simple synthesis methods, and for example, a polyol compound having a multi-branched structure is obtained by esterifying a polyhydric alcohol and a compound having one or more carboxyl groups and two or more hydroxyl groups in one molecule. Then, it can be produced by an esterification reaction by dehydration condensation between the terminal hydroxyl group of the polyol compound and (meth)acrylic acid, an ester exchange reaction between the terminal hydroxyl group of the polyol compound and a (meth)acrylic acid ester, and an addition reaction between the terminal hydroxyl group of the polyol compound and an isocyanate compound having a (meth)acryloyl group, or the like.

[0043] Examples of the polyhydric alcohol include glycerin, trimethylolethane, ditrimethylolethane, trimethylolpropane, ditrimethylolpropane, 1,2,4-butanetriol, pentaerythritol, dipentaerythritol, tris(2-hydroxyethyl)isocyanurate, sorbitol, mannitol, and alkylene oxide adducts of these alcohols or ring-opening adducts of caprolactone, etc. These polyhydric alcohols can be used alone or in combination of two or more kinds.

[0044] Examples of the compound having one or more carboxyl groups and two or more hydroxyl groups in one molecule include 2,3-dihydroxypropionic acid, 2,2-dimethylolpropionic acid, 2,2-dimethylolbutanoic acid, tartaric acid, 2,3-dihydroxybenzoic acid, 2,4-dihydroxybenzoic acid, 2,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 3,5-bis(2-hydroxyethoxy)benzoic acid, 2,6-dihydroxy-4-methylbenzoic acid, 3,5-dihydroxy-4-methylbenzoic acid, citrazinic acid, 2,3-dihydroxyphenylacetic acid, 2,4-dihydroxyphenylacetic acid, 2,5-dihydroxyphenylacetic acid, 2,6-dihydroxyphenylacetic acid, 3,4-dihydroxyphenylacetic acid, 3,5-dihydroxyphenylacetic acid, and derivatives thereof. These compounds can be used alone or in combination of two or more kinds.

[0045] Commercially available examples of the polyol compound include "BOLTORN H20", "BOLTORN H30", "BOLTORN H40", "BOLTORN H311", "BOLTORN H2003", "BOLTORN H2004", "BOLTORN P500", "BOLTORN P501", and "BOLTORN P1000" manufactured by Perstorp.

[0046] In addition, examples of commercially available products of the component (C) include "Viscoat #1000LT" manufactured by Osaka Organic Chemical Industry Ltd., "Miramer SP1106" manufactured by MIWON, "CN2302", "CN2303", and "CN2304" manufactured by Arkema, and "Photomer 5500" manufactured by IGM.

[0047] The content of the component (C) in the active energy ray-curable composition is preferably in the range of 1 to 40 mass%, more preferably in the range of 5 to 35 mass%, and particularly preferably in the range of 10 to 30 mass%, because an active energy ray-curable composition capable of forming a lens having a high Abbe number and excellent heat resistance and moist heat resistance can be obtained.

[0048] In addition to the components (A), (B), and (C), the active energy ray-curable composition of the present invention may contain, if necessary, a compound (D) having one or two (meth)acryloyl groups in one molecule and at least one hydroxyl group in one molecule (hereinafter, abbreviated as "component (D)") for the purpose of further improving moist heat resistance.

[0049] Examples of the component (D) include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxy-1-methylethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-hydroxy-3-phenylphenolpropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 3-hydroxy-3-methylbutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, cyclohexanedimethanol mono(meth)acrylate, 3-hydroxy-1-adamantine, and the like. Examples of the hydroxyl groups include glycerin mono(meth)acrylate, 3,5-dihydroxy-1-adamantyl(meth)acrylate, glycerin mono(meth)acrylate, glycerin di(meth)acrylate, trimethylolpropane mono(meth)acrylate, trimethylolpropane di(meth)acrylate, ditrimethylolpropane mono(meth)acrylate, ditrimethylolpropane di(meth)acrylate, pentaerythritol mono(meth)acrylate, pentaerythritol di(meth)acrylate, dipentaerythritol mono(meth)acrylate, dipentaerythritol di(meth)acrylate, sorbitol mono(meth)acrylate, sorbitol di(meth)acrylate, mannitol mono(meth)acrylate, and mannitol di(meth)acrylate. In addition, compounds in which a part or all of the hydroxyl groups of the above-mentioned compounds are modified with alkylene oxide or caprolactone can also be used. These compounds can be used alone or in combination of two or more. Among these, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, cyclohexanedimethanol mono(meth)acrylate, and sorbitol ethylene oxide modified di(meth)acrylate are preferred from the viewpoint of obtaining higher Abbe number, heat resistance, and moist heat resistance.

[0050] In addition, the (D) component may be, for example, an epoxy (meth)acrylate such as a reaction product of a compound having one or two glycidyl groups in one molecule with (meth)acrylic acid, or a reaction product of a compound having a (meth)acryloyloxy group and a glycidyl group in one molecule with a carboxylic acid and / or a dicarboxylic acid anhydride.

[0051] Examples of the compound having one or two glycidyl groups in one molecule include dodecyl glycidyl ether, tetradecyl glycidyl ether, ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1.6-Hexanediol diglycidyl ether, glycerin diglycidyl ether, 1,2-epoxy-4-vinylcyclohexane, 3,4-epoxycyclohexylmethyl methacrylate, 1,4-cyclohexanedimethanol monoglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, 3,4,3,4-diepoxybicyclohexyl, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, ε-caprolactone-modified 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, bisphenol A monoglycidyl ether, bisphenol A diglycidyl ether, bisphenol A alkylene oxide-modified monoglycidyl ether, bisphenol A alkylene oxide-modified diglycidyl ether, bisphenol A caprolactone-modified monoglycidyl ether, bisphenol A caprolactone-modified diglycidyl ether, hydrogenated bisphenol A monoglycidyl ether, hydrogenated bisphenol A diglycidyl ether, Examples of the alkylene oxide-modified monoglycidyl ether include hydrogenated bisphenol A alkylene oxide-modified diglycidyl ether, hydrogenated bisphenol A caprolactone-modified monoglycidyl ether, hydrogenated bisphenol A caprolactone-modified diglycidyl ether, bisphenol F monoglycidyl ether, bisphenol F diglycidyl ether, bisphenol F alkylene oxide-modified monoglycidyl ether, bisphenol F alkylene oxide-modified diglycidyl ether, bisphenol F caprolactone-modified monoglycidyl ether, bisphenol F caprolactone-modified diglycidyl ether, hydrogenated bisphenol F monoglycidyl ether, hydrogenated bisphenol F diglycidyl ether, hydrogenated bisphenol F alkylene oxide-modified monoglycidyl ether, hydrogenated bisphenol F alkylene oxide-modified diglycidyl ether, hydrogenated bisphenol F caprolactone-modified monoglycidyl ether, hydrogenated bisphenol F alkylene oxide-modified diglycidyl ether, hydrogenated bisphenol F caprolactone-modified monoglycidyl ether, hydrogenated bisphenol F caprolactone-modified diglycidyl ether, and the like.

[0052] Examples of the compound having a (meth)acryloyl group and a glycidyl group in one molecule include glycidyl (meth)acrylate, 4-hydroxybutyl acrylate glycidyl ether, and 3,4-epoxycyclohexylmethyl (meth)acrylate.

[0053] Examples of the carboxylic acid and / or dicarboxylic anhydride include (meth)acrylic acid, 1,2-cyclohexanedicarboxylic anhydride, 4-methylcyclohexane-1,2-dicarboxylic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, bicyclo[2.2.1]heptane-2,3-dicarboxylic anhydride, methylbicyclo[2.2.1]heptane-2,3-dicarboxylic anhydride, succinic anhydride, octenylsuccinic anhydride, tetrapropene, and the like. Examples of such anhydrides include 3-dodecenyl succinic anhydride, 3-dodecenyl succinic anhydride, 3,3,4,4-tetrahydro-3,3-bifuran-2,2,5,5-tetraone, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid anhydride, trimellitic anhydride, and bis(1,3-dihydro-1,3-dioxo-5-isobenzofuran carboxylic acid) 2-acetyloxy-1,3-propanediyl.

[0054] Examples of commercially available products of the component (D) include Miramer M100 and Miramer M1051 manufactured by MIWON Co., Ltd., NK Ester 702A, NK Ester 401P, and NK Ester 701A manufactured by Shin-Nakamura Chemical Co., Ltd., HEA, HPA, 4-HBA, and Viscoat #540 manufactured by Osaka Organic Chemical Industry Ltd., Light Ester HO-250(N), Light Ester HOP(N), Light Ester HOP-A(N), Light Ester HOA(N), Light Ester HOB(N), Light Ester G-101P, Light Ester G-201P, Light Acrylate HOB-A, Epoxy Ester M-600A, and HOA-MPE(N) manufactured by Kyoeisha Chemical Co., Ltd., New Frontier PGA manufactured by Daiichi Kogyo Seiyaku Co., Ltd., and KAYARAD R-128H and KAYARAD Examples of such monomers include "R-167" manufactured by Toagosei Co., Ltd., "Aronix M-920" and "Aronix M-926" manufactured by Toa Gosei Co., Ltd., "4HBA" and "CHDMMA" manufactured by Mitsubishi Chemical Corporation, and "Resist Monomer HMA" and "Resist Monomer DHMA" manufactured by Daicel Corporation.

[0055] The content of the component (D) in the active energy ray-curable composition is preferably in the range of 1 to 30 mass %, and more preferably in the range of 5 to 20 mass %, because an active energy ray-curable composition capable of forming a lens having a high Abbe number and excellent heat resistance and moist heat resistance can be obtained.

[0056] The active energy ray-curable composition of the present invention may further contain, as necessary, other compounds in addition to the component (A), the component (B), the component (C), and the component (D).

[0057] Examples of the other compounds include (meth)acrylates having a hydroxyl group, etc. Examples of the (meth)acrylates having a hydroxyl group include pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, alkylene oxide-modified and / or caprolactone-modified compounds of the (meth)acrylates having a hydroxyl group, urethane acrylate, acrylic (meth)acrylate, polyester polyol (meth)acrylate, and epoxy acrylate.

[0058] Moreover, the active energy ray curable composition of the present invention can be irradiated with active energy rays to obtain a cured product or lens. The active energy ray refers to ionizing radiation such as ultraviolet rays, electron beams, α rays, β rays, and γ rays. When ultraviolet rays are irradiated as active energy rays, it is preferable to add a photopolymerization initiator (E) to the active energy ray curable composition of the present invention to improve the curability. On the other hand, when ionizing radiation such as electron beams, α rays, β rays, and γ rays is used, the composition is rapidly cured without using the photopolymerization initiator (E), so there is no need to add the photopolymerization initiator (E).

[0059] Examples of the photopolymerization initiator (E) include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone}, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, and 1-hydroxycyclohexyl phenyl ketone. , 2-methyl-2-morpholino(4-thiomethylphenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone and other acetophenone compounds; benzoin, benzoin methyl ether, benzoin isopropyl ether and other benzoin compounds; acylphosphine oxide compounds such as 2,4,6-trimethylbenzoin diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; benzyl compounds such as benzyl (dibenzoyl), methylphenylglyoxy ester, oxyphenylacetic acid 2-(2-hydroxyethoxy)ethyl ester, oxyphenylacetic acid 2-(2-oxo-2-phenylacetoxyethoxy)ethyl ester; benzophenone, o-benzoylbenzoic acid methyl-4-phenylbenzophenone, 4,4'-dichlorobenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, acrylated benzophenone, 3,3', Benzophenone compounds such as 4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 3,3'-dimethyl-4-methoxybenzophenone, 2,4,6-trimethylbenzophenone, and 4-methylbenzophenone; thioxanthone compounds such as 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone; aminobenzophenone compounds such as Michler's ketone and 4,4'-diethylaminobenzophenone;Examples of the photopolymerization initiator include 10-butyl-2-chloroacridone, 2-ethylanthraquinone, 9,10-phenanthrenequinone, camphorquinone, 1-[4-(4-benzoylphenylsulfanyl)phenyl]-2-methyl-2-(4-methylphenylsulfonyl)propan-1-one, etc. These photopolymerization initiators can be used alone or in combination of two or more kinds.

[0060] <h2 style=";text-align:left;direction:ltr">Omnirad 1173」、「Omnirad Omnirad 127」、「Omnirad 2959」、「Omnirad 369」、「Omnirad 379」、「Omnirad 907」、「Omnirad 4265」、「Omnirad 1000」、「Omnirad 651」、「Omnirad TPO」、「Omnirad TPO-L」、「Omnirad 819」、「Omnirad 2022」、「Omnirad 2100」、「Omnirad Omnirad 410」、「Omnirad OMBB」、「Omnirad BMS」、「Omnirad 500」、「Omnirad 81」、「Omnirad ITX」、「Omnirad DETX」、「Omnirad MBF」、「Omnirad EMK」、「Omnirad 784」、「Omnirad 1312」、「Omnirad BCIM」、「Omnirad BL 723」、「Omnirad BL 724」、「Omnirad BL 750」、「Omnirad BL751」、「Omnirad EDB」、「Omnirad EHA」、「Omnirad IADB」、「Esacure KIP 150」、「Esacure KIP 100F」、「Esacure KIP 75LT」、「Esacure KIP IT」、「Esacure TZT」、「Esacure KT55」、「Esacure TZM」、「Esacure ONE」、「Esacure 1001M」、「Esacure KIP 160」、「Esacure A 198」、「Esacure KTO 46」、「Esacure DP 250 Omnipol 910 Omnipol 9210 Omnipol BP Omnipol TX Omnipol 3TX Omnipol BL728 KAYACURE EPA」、「KAYACURE OA」、StoffaExamples of photopolymerization initiators include "Vicure 10" and "Vicure 55" manufactured by Akzo Nobel, "Trigonal P1" manufactured by Akzo Nobel, "SANDORAY 1000" manufactured by SANDOZ, "DEAP" manufactured by Upjohn Chemical, "Quantacure PDO", "Quantacure ITX", and "Quantacure EPD" manufactured by Ward Blenkinsop, and "Runtecure 1104" manufactured by Runtec. These photopolymerization initiators can be used alone or in combination of two or more kinds.

[0061] From the viewpoint of obtaining sufficient curability, the amount of the photopolymerization initiator (E) used is preferably in the range of 0.05 to 20 parts by mass, more preferably in the range of 0.1 to 10 parts by mass, and particularly preferably in the range of 0.5 to 5 parts by mass, relative to 100 parts by mass of the total mass of the component (A), the component (B), the component (C), and the component (D).

[0062] In addition, a heat stabilizer (F) may be added to the active energy ray-curable composition of the present invention for the purpose of further improving heat resistance.

[0063] Examples of the heat resistance stabilizer include ethanethiol, 2-methylpropane-2-thiol, n-dodecanethiol, 2,3,3,4,4,5-hexamethylhexane-2-thiol, 2-mercaptoethanol, 4-mercapto-1-butanol, methyl mercaptoacetate, methyl 3-mercaptopropionate, 2-ethylhexyl 3-mercaptopropionate, 3-methoxybutyl 3-mercaptopropionate, n-octyl 3-mercaptopropionate, stearyl 3-mercaptopropionate, 3-(trimethoxysilyl)propane-1-thiol, 3 -(Triethoxysilyl)propane-1-thiol, benzenethiol, benzylthiol, 3-methylbenzenethiol, 4-methylbenzenethiol, naphthalene-2-thiol, pyridine-2-thiol, benzimidazole-2-thiol, benzothiazole-2-thiol, 1,2-ethanedithiol, 1,2-propanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, 2,3-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,10-decanedithiol, 2,3-dihydroxy-1, 4-Butanedithiol, 3,6-dioxa-1,8-octanedithiol, 3,7-dithia-1,9-nonanedithiol, 1,4-bis(3-mercaptopropionyloxy)butane, 1,4-bis(3-mercaptobutyryloxy)butane, tetraethylene glycol bis(3-mercaptopropionate), 1,2-benzenedithiol, 1,3-benzenedithiol, 1,4-benzenedithiol, 2,3-diamino-1,4-benzenedithiol, 4,5-dimethyl-O-xylenedithiol, toluene-3,4-dithiol, 4,4'-biphenyl 1,5-Naphthalenedithiol, 6-(dibutylamino)-1,3,5-triazine-2,4-dithiol, 2-amino-1,3,5-triazine-4,6-dithiol, 6-anilino-1,3,5-triazine-2,4-dithiol, 6-(4'-anilinophenyl-isopropylamino)-1,3,5-triazine-2,4-dithiol, 6-(3',5'-tert-butyl-4'-hydroxyanilino)-1,3,5-triazine-2,4-dithiol, quinoxaline-2,3-dithiol, purine-2,6-dithiol, 1,3,4-Thiadiazole-2,5-dithiol, bis(2-mercaptoethyl)ether, trimethylolethane tris(3-mercaptopropionate), trimethylolethane tris(3-mercaptobutyrate), trimethylolpropane tris(3-mercaptopropionate), trimethylolpropane tris(3-mercaptobutyrate), 1,3,5-benzenetrithiol, 1,3,5-triazine-2,4,6-trithiol, tris[2-(3-mercaptoethyl)ether] Examples of the heat stabilizer include compounds having a mercapto group, such as tris[2-(3-mercaptopropionyloxy)ethyl]isocyanurate, tris[2-(3-mercaptobutyryloxy)ethyl]isocyanurate, pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), dipentaerythritol hexakis(3-mercaptopropionate), and dipentaerythritol hexakis(3-mercaptobutyrate). These heat stabilizers can be used alone or in combination of two or more.

[0064] Examples of commercially available heat stabilizers include "Chiokalcol 20" manufactured by Kao Corporation, "KarenzMT PE1", "KarenzMT BD1", "KarenzMT NR1", "TPMB", and "TEMB" manufactured by Showa Denko K.K., and "TMMP", "TEMPIC", "PEMP", "EGMP-4", "DPMP", "TMMP II-20P", and "PEMP II-20P" manufactured by SC Organic Chemical Co., Ltd.

[0065] From the viewpoint of obtaining sufficient heat resistance, the amount of the heat stabilizer (F) used is preferably in the range of 0.01 to 10 parts by mass, more preferably in the range of 0.1 to 5 parts by mass, and particularly preferably in the range of 0.5 to 3 parts by mass, relative to 100 parts by mass of the total mass of the components (A), (B), (C), and (D).

[0066] The active energy ray-curable composition of the present invention may further contain other additives in addition to the components (A) to (F) as necessary.

[0067] Examples of the other additives include additives such as polymerization inhibitors, photosensitizers, surface conditioners, antistatic agents, defoamers, viscosity modifiers, light resistance stabilizers, weather resistance stabilizers, ultraviolet absorbers, antioxidants, leveling agents, organic pigments, inorganic pigments, pigment dispersants, silica beads, and organic beads; and inorganic fillers such as silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, cerium oxide, and antimony oxide. These other additives can be used alone or in combination of two or more. Among these, antioxidants are preferred because they can improve heat resistance.

[0068] Examples of the antioxidant include phenol-based antioxidants, phosphite-based antioxidants, sulfur-based antioxidants, etc. These antioxidants can be used alone or in combination of two or more kinds.

[0069] Examples of the phenol-based antioxidant include styrenated phenol, 2,6-ditertiary butyl-p-cresol, 2,5-ditertiary butyl hydroquinone, 2,5-ditertiary amyl hydroquinone, 3-(3,5-ditertiary butyl-4-hydroxyphenyl)octadecyl propionate, 2,4-bis(octylthiomethyl)-6-methylphenol, 2,2-methylenebis(6-tertiary butyl-p-cresol), 2,2-methylenebis(6-tertiary butyl-4-ethylphenol), 4,4-butylidenebis(6-tert-butyl-m-cresol), 4,4-thiobis(6-tert-butyl-m-cresol), 2,2-thiodiethylbis[3-(3,5-ditert-butyl-4-hydroxyphenyl)propionate], 1,6-hexanediol bis[3-(3,5-ditert-butyl-4-hydroxyphenyl)propionate], bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate][ethylenebis(oxyethylene)], bis[3-[3 -(tert-butyl)-4-hydroxy-5-methylphenyl]propanoic acid]2,4,8,10-tetraoxaspiro[5.5]undecane-3,9-diylbis(2-methylpropane-2,1-diyl), N,N-bis[2-[2-(3,5-ditert-butyl-4-hydroxyphenyl)ethylcarbonyloxy]ethyl]oxamide, N,N-(hexane-1,6-diyl)bis[3-(3,5-ditert-butyl-4-hydroxyphenyl)propanamide], 2,4,6-tris(3,5-ditert-butyl) butyl-4-hydroxybenzyl)mesitylene, 1,3,5-tris(3,5-ditertiarybutyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1,1,3-tris(2-methyl-4-hydroxy-5-tertiarybutylphenyl)butane, pentaerythritol tetrakis[3-(3,5-ditertiarybutyl-4-hydroxyphenyl)propionate], diethyl(3,5-ditertiarybutyl-4-hydroxybenzyl)phosphonate, and the like.

[0070] Examples of commercially available phenol-based antioxidants include "IRGANOX 1010", "IRGANOX 1010FF", "IRGANOX 1035", "IRGANOX 1035FF(W&C)", "IRGANOX 1076", "IRGANOX 1076FD", "IRGANOX 1098", "IRGANOX 1135", "IRGANOX 1330", "IRGANOX 1520L", "IRGANOX 245", "IRGANOX 245FF", "IRGANOX 259", and "IRGANOX 3114" manufactured by BASF; "ANTAGE BHT", "ANTAGE DAH", "ANTAGE DBH", "ANTAGE W-300", "ANTAGE W-400", "ANTAGE W-500", "ANTAGE Crystal", "ANTAGE SP", "ANTAGE HP-200", and "ANTAGE Examples of such an agent include "ADK STAB HP-300" manufactured by ADEKA CORPORATION, "ADK STAB AO-20", "ADK STAB AO-30", "ADK STAB AO-40", "ADK STAB AO-50", "ADK STAB AO-50F", "ADK STAB AO-50T", "ADK STAB AO-60", "ADK STAB AO-60G", "ADK STAB AO-80", and "ADK STAB AO-330" manufactured by Sumitomo Chemical Co., Ltd., "SUMILIZER GA-80", "SUMILIZER GP", "SUMILIZER MDP-S", "SUMILIZER WX-R", and "SUMILIZER WX-RC" manufactured by Mitsubishi Chemical Corporation, "Yoshinox BB" manufactured by Johoku Chemical Industry Co., Ltd., and "JC-356" manufactured by Johoku Chemical Industry Co., Ltd.

[0071] Examples of the phosphite-based antioxidant include tris(2-ethylhexyl)phosphite, tridecyl phosphite, triisodecyl phosphite, trilauryl phosphite, tris(tridecyl)phosphite, tri(stearyl)phosphite, diphenyl mono(2-ethylhexyl)phosphite, diphenyl monodecyl phosphite, diphenyl isodecyl phosphite, diphenyl mono(tridecyl)phosphite, triphenyl phosphite, tricresyl phosphite, tris(2,4-ditertiary butylphenyl)phosphite, tris(nonylphenyl)phosphite, tetraphenyl dipropylene glycol diphosphite, 4,4-butylidene bis(3-methyl-6-tertiary butylphenyl ditridecyl phosphite), tetra(C12 to C1 5 alkyl)-4,4-isopropylidenediphenyl diphosphite, 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 3,9-bis(2,6-ditertiarybutyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 2,4,8,10-tetrakis(1,1-dimethylethyl)-6-[(2-ethylhexyl)oxy]-12H-dibenzo[d,g][1,3,2]dioxaphosphocin, bis(decyl)pentaerythritol diphosphite, bis(tridecyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, hydrogenated bisphenol A·pentaerythritol phosphite polymer, etc.

[0072] Commercially available products of the phosphite antioxidant include, for example, "IRGAFOS 168" and "IRGAFOS 168FF" manufactured by BASF, and "ADK STAB PEP-8", "ADK STAB PEP-36", "ADK STAB HP-10", "ADK STAB 2112", "ADK STAB 2112RG", "ADK STAB 1178", "ADK STAB 1500", "ADK STAB C", "ADK STAB 135A", "ADK STAB 3010", and "ADK STAB 2112R" manufactured by ADEKA CORPORATION. TPP" manufactured by Johoku Chemical Industry Co., Ltd., and "JP-360", "JP-351", "JP-3CP", "JP-308E", "JPE-308E", "JP-310", "JP-312L", "JP-333E", "JPM-308", "JPM-311", "JPM-313", "JPP-100", "JA-805", "JPH-1200", "JPP-88", "JPE-10", "JPE-13R", "JP-318E", "JPP-2000PT", "JP-650", and "JPH-3800" manufactured by Johoku Chemical Industry Co., Ltd.

[0073] Examples of the sulfur-based antioxidant include didodecyl 3,3-thiodipropionate, ditridecyl 3,3-thiobispropionate, dioctadecyl 3,3-thiodipropionate, and pentaerythritol tetrakis[3-(dodecylthio)propionate].

[0074] Examples of commercially available sulfur-based antioxidants include "IRGANOX PS800FL" and "IRGANOX PS802FL" manufactured by BASF, "ADK STAB AO-412S" and "ADK STAB AO-503" manufactured by ADEKA CORPORATION, "KEMINOX PLS" manufactured by Chemipro Chemical Co., Ltd., and "SUMILIZER TP-D" manufactured by Sumitomo Chemical Co., Ltd.

[0075] As the other additives, inorganic fillers are preferably used to adjust the refractive index and thermal expansion coefficient. Examples of the inorganic fillers include silica fine particles, zirconia fine particles, and other fine particles, and each of them can be used independently by one type or by combining two or more types. The particle size of the inorganic filler is preferably 1000 nm or less, more preferably 500 nm or less, and particularly preferably 100 nm or less.

[0076] Examples of commercially available products of the silica fine particles include "Methanol Silica Sol", "MA-ST-M", "MA-ST-L", "IPA-ST", "IPA-ST-L", "IPA-ST-ZL", "IPA-ST-UP", "EG-ST", "NPC-ST-30", "PGM-ST", "DMAC-ST", "MEK-ST-40", "MEK-ST-L", "MEK-ST-ZL", "MEK-ST-UP", "MIBK-ST", "MIBK-ST-L", "CHO-ST-M", "EAT-ST", "PMA-ST", "TOL-ST", "MEK-AC-2140Z", "MEK-AC-4130Y", "MEK-AC-5140Z", "MIBK-AC-2140Z", "MIBK-SD-L", "PGM-AC-2140Y", "PGM-AC-4140Y", and "MEK-EC-2130Y" manufactured by Nissan Chemical Co., Ltd.; KE-E10", "SeaHoster KE-E30", "SeaHoster KE-E150", "SeaHoster KE-W10", "SeaHoster KE-W30", "SeaHoster KE-W50", "SeaHoster KE-P10", "SeaHoster KE-P30", "SeaHoster KE-P50", "SeaHoster KE-P100", "SeaHoster KE-P150", "SeaHoster KE-P250", "SeaHoster KE-S10", "SeaHoster KE-S30", "SeaHoster KE-S50", "SeaHoster KE-S100", "SeaHoster KE-S150", "SeaHoster KE-S250", Shin-Etsu Chemical Co., Ltd.'s "QSG-10", "QSG-30", "QSG-100", "QSG-170", and Admatechs Co., Ltd.'s "Admanano" Examples of such fluoropolymers include "YA010C", "YA050C", and "YA100C", and "DLSB-001" and "DLSB-002" manufactured by Daiken Chemical Co., Ltd.

[0077] Examples of commercially available zirconia fine particles include "ZHR-101", "ZHR-103", and "ZHR-200" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Zircostar ZP-153" and "Zircostar HR-101" manufactured by Nippon Shokubai Co., Ltd., "SZR-W", "SZR-M", "SZR-CW", "SZR-CM", "SZR-KM", and "SZR-K" manufactured by Sakai Chemical Industry Co., Ltd., "DLZ-001", "DLZ-007", "DLZ-003U", "DLM-001", and "DLM-002" manufactured by Daiken Chemical Industry Co., Ltd., "ZSL-10A", "ZSL-10T", "ZSL-20N", and "ZSL-00014" manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd., "Zirconeo-Cw" and "Zirconeo-Ck" manufactured by ITEC Co., Ltd., and "TZP-103" manufactured by Taisei Kako Co., Ltd.

[0078] Examples of commercially available products of the other fine particles include titania fine particles such as "TTP-113" and "TTP-1132" manufactured by Taisei Chemical Industry Co., Ltd., barium titanate fine particles such as "DLB-001", "DLB-002", and "DLB-003" manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd., antimony tin oxide fine particles such as "DLAT-001" manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd., and indium tin oxide fine particles such as "DLIT-001" manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd.

[0079] Examples of a method for obtaining a cured product of the active energy ray-curable composition include a method in which the active energy ray-curable composition is applied onto a substrate and then irradiated with active energy rays.

[0080] Examples of the substrate include polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyolefin-based resins such as polypropylene, polyethylene, and polymethylpentene; cellulose-based resins such as cellulose acetate (diacetyl cellulose, triacetyl cellulose, and the like), cellulose acetate propionate, cellulose acetate butyrate, cellulose acetate propionate butyrate, cellulose acetate phthalate, and cellulose nitrate; acrylic resins such as polymethyl methacrylate; vinyl chloride-based resins such as polyvinyl chloride and polyvinylidene chloride; polyvinyl alcohol; ethylene-vinyl acetate copolymer; polystyrene; polyamide; polycarbonate. polyimide resins such as polyimide and polyetherimide; resin films such as norbornene resins (e.g., "ZEONOR" manufactured by Zeon Corporation), modified norbornene resins (e.g., "ARTON" manufactured by JSR Corporation), and cyclic olefin copolymers (e.g., "APEL" manufactured by Mitsui Chemicals, Inc.); semiconductor wafers such as silicon, silicon carbide, silicon nitride, sapphire, aluminum nitride, gallium nitride, gallium phosphide, gallium arsenide, and indium phosphide; and glasses such as quartz glass, borosilicate glass, soda-lime glass, silicate glass, and optical glass (crown glass, flint glass).

[0081] Examples of a method for applying the active energy ray-curable composition of the present invention to the substrate include die coating, microgravure coating, gravure coating, roll coating, comma coating, air knife coating, kiss coating, spray coating, dip coating, spinner coating, brush coating, solid coating by silk screen, wire bar coating, flow coating, dispenser, inkjet printing, screen printing, offset printing, and the like.

[0082] As described above, the active energy rays for curing the active energy ray-curable composition are ionizing radiation such as ultraviolet rays, electron beams, α rays, β rays, γ rays, etc. Here, when ultraviolet rays are used as the active energy rays, examples of devices for irradiating the ultraviolet rays include low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, electrodeless lamps (fusion lamps), chemical lamps, black light lamps, mercury-xenon lamps, short arc lamps, helium-cadmium lasers, argon lasers, sunlight, LED lamps, etc.

[0083] The irradiation dose (accumulated light amount) of the active energy rays is 100 to 10,000 mJ / cm 2 and preferably 300 to 8,000 mJ / cm 2 It is more preferable that the irradiation amount of the active energy ray is based on the value measured by a photometer suitable for the desired excitation wavelength, and for example, Iwasaki Electric Co., Ltd. Eye ultraviolet integrating illuminometer UVPF-A2 series, Hamamatsu Photonics ultraviolet actinometer C9536 / H9535 series, C9536 / H9958 series, C10427 / H10428 series, Ushio Electric Co., Ltd. ultraviolet integrating actinometer UIT-201, UIT-250, UIT-θ series, etc. can be used. In particular, in the present invention, the integrated light amount measured using Iwasaki Electric Co., Ltd. Eye ultraviolet integrating illuminometer UVPF-A2 (PD-365) is used as the standard.

[0084] The irradiation of the active energy rays may be carried out in one step or in two or more steps.

[0085] The film thickness of the cured product of the active energy ray-curable composition of the present invention is preferably in the range of 1 to 1000 μm, and more preferably in the range of 50 to 500 μm, in order to ensure sufficient hardness of the cured product.

[0086] The refractive index of the cured product (n d) is preferably in the range of 1.40 to 1.60, and more preferably in the range of 1.45 to 1.55. The refractive index of the cured product is a value measured in accordance with JIS test method K7142:2014, Method A.

[0087] The Abbe number of the cured product (ν d ) is preferably 53 or more, more preferably in the range of 53 to 60, even more preferably in the range of 55 to 59, and particularly preferably in the range of 56 to 58. The Abbe number of the cured product is a value calculated based on the refractive index measured in accordance with JIS test method K7142:2014, Method A.

[0088] The light transmittance of the cured product at a wavelength of 410 nm is preferably 85% or more, more preferably 88% or more, and particularly preferably 90% or more, from the viewpoint of suitable use in optical lenses. The method for measuring the light transmittance will be described in detail in the Examples.

[0089] The light transmittance of the cured product after the heat resistance test is preferably within ±5% of the initial light transmittance at a wavelength of 410 nm, more preferably within ±3%, and particularly preferably within ±1%, from the viewpoint of suitability for use in optical lenses having solder reflow resistance. The method for measuring the light transmittance after the heat resistance test will be described in detail in the Examples.

[0090] The water absorption of the cured product is preferably in the range of 0.1% to 4.0%, more preferably in the range of 0.3 to 3.5%, and particularly preferably in the range of 0.5 to 2.5%, in order to prevent defects from occurring inside the cured product under high temperature and humidity conditions. The water absorption of the cured product is a calculated value that takes into account the amount dissolved in water, using a measured value in accordance with JIS test method K7209:2000, Method C.

[0091] As for the wet heat resistance of the cured product, in order to prevent defects from occurring inside the cured product under a high temperature and high humidity environment, as a result of a wet heat test performed under conditions of a temperature of 85°C, humidity of 85% RH, and time of 1000 hours, it is preferable that there is no peeling from the substrate, it is more preferable that there is no defect at the interface between the cured product and the substrate, and it is particularly preferable that there is no defect inside the cured product. The method for evaluating the wet heat resistance of the cured product will be described in detail in the Examples.

[0092] The lens of the present invention has the cured product. If necessary, the lens may have an inorganic layer made of an inorganic compound on at least one surface of the cured product, and may further have a substrate.

[0093] The lens of the present invention can also be used as a wafer-level lens by imprint molding.

[0094] The method for producing the lens of the present invention is not particularly limited and may be any method, but for example, the active energy ray curable composition is applied onto a substrate such as a wafer or glass, and then shaped into a desired shape using a mold, and then the composition is temporarily cured by irradiating with active energy rays. After releasing the mold, the uncured active energy ray curable composition is washed with a solvent in a development process, and then irradiated with active energy rays again to perform full curing. Furthermore, if necessary, an inorganic layer made of an inorganic compound is formed on the surface of the cured product by physical vapor deposition or the like. Finally, a method of dividing the substrate into individual pieces is included.

[0095] Examples of the solvent include ketone-based solvents such as methyl ethyl ketone, acetone, isobutyl ketone, cyclopentanone, and cyclohexanone; cyclic ether-based solvents such as tetrahydrofuran, dioxolane, and dioxane; ester-based solvents such as methyl acetate, ethyl acetate, and butyl acetate; aromatic solvents such as toluene, xylene, and solvent naphtha; alicyclic hydrocarbon-based solvents such as cyclohexane and methylcyclohexane; alcohol-based solvents such as carbitol, cellosolve, methanol, isopropanol, butanol, and propylene glycol monomethyl ether; and glycol ether-based solvents such as alkylene glycol monoalkyl ether, dialkylene glycol monoalkyl ether, and dialkylene glycol monoalkyl ether acetate. These solvents can be used alone or in combination of two or more.

[0096] The inorganic layer means a layer made of an inorganic compound, and generally has functions such as anti-reflection and scratch resistance.

[0097] Examples of the inorganic compound include metal oxides, double oxides, metal nitrides, metal fluorides, double fluorides, silicon oxides, silicon nitrides, and mixtures thereof.

[0098] Examples of the metal include lithium, sodium, magnesium, aluminum, titanium, yttrium, indium, tin, zirconium, niobium, cerium, hafnium, and tantalum.

[0099] When the inorganic layer is used as an anti-reflection film layer, the anti-reflection film layer may be a single layer, or may have a low refractive index layer and a high refractive index layer.In addition, each of the low refractive index layer and the high refractive index layer may be one layer or multiple layers.In addition, the stacking order of the low refractive index layer and the high refractive index layer is not particularly limited.

[0100] Examples of the inorganic compound used in the high refractive index layer include lanthanum titanate, zirconium oxide, titanium oxide, tantalum oxide, niobium oxide, hafnium oxide, cerium oxide, yttrium oxide, and mixtures thereof.

[0101] Examples of the inorganic compound used in the low refractive index layer include silicon oxide, silicon nitride, magnesium fluoride, aluminum fluoride, and mixtures thereof.

[0102] The inorganic layer is obtained by forming a film on the surface of the resin layer. The method for forming the inorganic layer is not particularly limited, and any known film forming method can be used as appropriate, but it is preferable to form the film by physical vapor deposition (PVD) or chemical vapor deposition (CVD).

[0103] From the viewpoint of consistency and simplification of the film formation process, it is more preferable to use physical vapor deposition (PVD), and examples of the film formation method include vacuum deposition, ion plating, and sputtering.

[0104] The vacuum deposition can be carried out by, for example, a resistance heating method, a high-frequency induction heating method, an electron beam heating method, or the like.

[0105] The sputtering may be DC sputtering, RF sputtering, magnetron sputtering, or ion beam sputtering. In addition, it may be a parallel plate target system or a facing target system. In addition, examples of the gas introduced into the vacuum chamber include argon, krypton, oxygen, and nitrogen, and each of them may be used alone or in combination of two or more.

[0106] The thickness of the inorganic layer can be appropriately adjusted depending on the intended function. When the objective is anti-reflection function, the thickness is preferably in the range of 10 nm to 5,000 nm, and from the viewpoint of the film strength and productivity of the inorganic layer, the thickness is more preferably in the range of 100 nm to 2,000 nm, and particularly preferably in the range of 250 nm to 1,000 nm.

[0107] As described above, the cured product formed by the active energy ray-curable composition of the present invention has a high Abbe number and high light transmittance, is excellent in heat resistance and moist heat resistance, and can be easily cured by irradiation with active energy rays, and therefore can be suitably used for lens production by photoimprinting. EXAMPLES

[0108] The present invention will now be described more specifically with reference to examples.

[0109] In the present examples, the weight average molecular weight (Mw) is a value measured by gel permeation chromatography (GPC) under the following conditions.

[0110] Measuring device: Tosoh Corporation HLC-8220 Column: Guard column H manufactured by Tosoh Corporation XL -H + Tosoh Corporation TSKgel G5000HXL + Tosoh Corporation TSKgel G4000HXL + Tosoh Corporation TSKgel G3000HXL + Tosoh Corporation TSKgel G2000HXL Detector: RI (differential refractometer) Data processing: Tosoh Corporation SC-8010 Measurement conditions: Column temperature 40℃ Solvent Tetrahydrofuran Flow rate 1.0ml / min Standard: Polystyrene Sample: 100 μl of tetrahydrofuran solution containing 0.4% by mass of resin solids filtered through a microfilter

[0111] [Synthesis Example 1: Production of ethylene oxide (4 mol) modified hydrogenated bisphenol A diacrylate] In a pressure-resistant reactor equipped with a thermometer, a stirring rod, an alkylene oxide inlet tube, a nitrogen gas inlet tube, etc., 240 parts by mass (1 mol) of hydrogenated bisphenol A, 400 parts by mass of xylene, and 0.2 parts by mass (5 mmol) of sodium hydroxide were charged, and the pressure in the reactor was reduced and pressurized with nitrogen three times to replace the nitrogen in the reactor. Next, the reactor was heated to an internal temperature of 130°C while stirring, and held for 0.5 hours to form a homogeneous solution, after which water was distilled off from the reaction system. Next, while maintaining the internal temperature at 130°C, 185 parts by mass (4.2 mol) of ethylene oxide was fed into the reaction system under pressure over 6 hours, and the internal temperature was raised to 140°C and reacted for 2 hours. Thereafter, 10 parts by mass of activated clay was added to the reaction mixture obtained, and the mixture was stirred at 90°C under a nitrogen stream for 1 hour, after which the catalyst was removed by filtration, and unreacted ethylene oxide and xylene were distilled off under reduced pressure to obtain a hydrogenated bisphenol A ethylene oxide (4 mol) adduct (b-1). The average number of moles of ethylene oxide added to hydrogenated bisphenol A in the obtained hydrogenated bisphenol A ethylene oxide (4 mol) adduct (b-1) was 4, the weight average molecular weight was 450 g / mol, and the hydroxyl value was 180 mgKOH / g.

[0112] Next, 450 parts by mass (1 mol) of hydrogenated bisphenol A ethylene oxide (4 mol) adduct (b-1), 180 parts by mass (2.5 mol), 0.62 parts by mass (5 mmol) of methoquinone, 17 parts by mass (0.1 mol) of paratoluenesulfonic acid, and 500 parts by mass of toluene were charged into a reaction vessel equipped with a thermometer, a stirring rod, a Dean-Stark apparatus, an air inlet tube, etc., and air was blown into the reaction solution. Next, the reaction vessel was heated to an internal temperature of 110°C while stirring, and the water generated was removed from the system while maintaining the internal temperature, and the reaction was carried out for 5 hours. After cooling the reaction mixture, it was neutralized with a 20% by mass aqueous sodium hydroxide solution, and extracted and washed three times with saline. Next, unreacted acrylic acid and toluene were distilled off under reduced pressure to obtain ethylene oxide (4 mol) modified hydrogenated bisphenol A diacrylate (B-1). The weight average molecular weight of this compound (B-1) was 550 g / mol, and the ester value was 150 mgKOH / g.

[0113] [Synthesis Example 2: Production of ethylene oxide (6 mol) modified hydrogenated bisphenol A diacrylate] A hydrogenated bisphenol A ethylene oxide (6 mol) adduct (b-2) and an ethylene oxide (6 mol) modified hydrogenated bisphenol A diacrylate (B-2) were synthesized in the same manner as in Synthesis Example 1, except that the amount of ethylene oxide was changed to 273 parts by mass (6.2 mol). The average number of moles of ethylene oxide added to hydrogenated bisphenol A in the obtained hydrogenated bisphenol A ethylene oxide (6 mol) adduct (b-2) was 6, the weight average molecular weight was 550 g / mol, and the hydroxyl value was 150 mg KOH / g, and the weight average molecular weight of (B-2) was 650 g / mol, and the ester value was 120 mg KOH / g.

[0114] [Synthesis Example 3: Production of ethylene oxide (8 mol) modified hydrogenated bisphenol A diacrylate] A hydrogenated bisphenol A ethylene oxide (8 mol) adduct (b-3) and an ethylene oxide (8 mol) modified hydrogenated bisphenol A diacrylate (B-3) were synthesized in the same manner as in Synthesis Example 1, except that the amount of ethylene oxide was changed to 361 parts by mass (8.2 mol). The average number of moles of ethylene oxide added to hydrogenated bisphenol A in the obtained hydrogenated bisphenol A ethylene oxide (8 mol) adduct (b-3) was 8, the weight average molecular weight was 670 g / mol, and the hydroxyl value was 120 mg KOH / g, and the weight average molecular weight of (B-3) was 770 g / mol, and the ester value was 100 mg KOH / g.

[0115] [Synthesis Example 4: Production of ethylene oxide (6 mol) modified tricyclodecane dimethanol diacrylate] Tricyclodecane dimethanol ethylene oxide (6 mol) adduct (b-4) and ethylene oxide (6 mol) modified tricyclodecane dimethanol diacrylate (B-4) were synthesized in the same manner as in Synthesis Example 2, except that 240 parts by mass (1 mol) of hydrogenated bisphenol A was changed to 196 parts by mass (1 mol) of tricyclodecane dimethanol. The average number of moles of ethylene oxide added to tricyclodecane dimethanol in the obtained tricyclodecane dimethanol ethylene oxide (6 mol) adduct (b-4) was 6, the weight average molecular weight was 500 g / mol, and the hydroxyl value was 160 mg KOH / g, and the weight average molecular weight of (B-4) was 600 g / mol, and the ester value was 130 mg KOH / g.

[0116] [Synthesis Example 5: Production of Compound (C-1) Having Acryloyl Group and Multibranched Structure] In a reaction vessel equipped with a thermometer, a stirring rod, a Dean-Stark apparatus, and an air inlet tube, 134 parts by mass (1 mol) of pentaerythritol ethylene oxide (4 mol) adduct, 17 parts by mass (0.1 mol) of paratoluenesulfonic acid, and 200 parts by mass of toluene were charged, and the internal temperature of the reaction vessel was raised to 110 ° C. while stirring. Next, while maintaining the internal temperature at 110 ° C., 1,073 parts by mass (8 mol) of dimethylolpropionic acid was added to the reaction system in four portions every 2 hours, and the reaction was carried out for 10 hours while simultaneously removing the water generated from the system. Next, the reaction mixture was cooled, and 1081 parts by mass (15 mol) of acrylic acid, 1.24 parts by mass (10 mmol) of methoquinone, 34 parts by mass (0.2 mol) of paratoluenesulfonic acid, and 500 parts by mass of toluene were added to the reaction vessel. Next, air was blown into the reaction solution, and the internal temperature was raised to 110°C while stirring the reaction vessel, and the reaction was continued for 8 hours while removing the generated water from the system while maintaining the internal temperature. Next, the reaction solution was neutralized with a 20% by mass aqueous solution of sodium hydroxide, extracted and washed with saline three times, and the unreacted acrylic acid and toluene were distilled off under reduced pressure to obtain a compound (C-1) having an acryloyl group and a multi-branched structure. The weight average molecular weight of this compound (C-1) was 2200g / mol, and the ester value was 200mgKOH / g.

[0117] [Example 1] As the component (A), polycarbonate diol diacrylate ("UM-90(1 / 3)DA" manufactured by Ube Industries, Ltd.: R in the general formula (1) 1 is a hydrogen atom, and R 2 each independently has a linear hydrocarbon group having 6 carbon atoms and a cyclohexane structure arranged randomly, and n is 4 to 5.); 30 parts by mass of ethylene oxide (4 mol) modified hydrogenated bisphenol A diacrylate (B-1) as component (B); 40 parts by mass of ethylene oxide (4 mol) modified hydrogenated bisphenol A diacrylate (B-1) as component (B); 30 parts by mass of a compound (C-1) having an acryloyl group and a multi-branched structure as component (C); and 1 part by mass of 1-hydroxycyclohexyl phenyl ketone ("I-184" manufactured by BASF) as component (E) were mixed and heated to 50°C, and then stirred and mixed using a homodisper at a rotation speed of 1,000 rpm for 10 minutes to prepare an active energy ray curable composition.

[0118] [Examples 2 to 13, Comparative Examples 1 to 8] Active energy ray-curable compositions were prepared in the same manner as in Example 1, except that the types and / or amounts of (A), (B), (C), (D) and (F) were changed as shown in Tables 1 to 3.

[0119] [Refractive index measurement method] The active energy ray-curable compositions obtained in the Examples and Comparative Examples were poured into a triangular prism mold (thickness 5 mm, length of each side 10 mm) and exposed to 3,000 mJ / cm using a belt conveyor type ultraviolet irradiation device (120 W metal halide lamp) manufactured by iGraphics Co., Ltd. 2 The triangular prism was then irradiated with ultraviolet light of 1000 nm to produce a triangular prism. The refractive indexes of the resulting triangular prism at 25°C were measured using a Kalnew precision refractometer "KPR-3000" manufactured by Shimadzu Corporation, for the d-line, F-line, and C-line. The refractive index of the cured product (n d ) closest to the refractive index (n d ) was appropriately selected and used.

[0120] [How to calculate the Abbe number] Using the refractive indexes of the d line, F line, and C line measured in the above [Method of measuring refractive index], the Abbe number (ν d ) was calculated.

[0121]

number

[0122] [Transmittance measurement method] The active energy ray curable compositions obtained in the Examples and Comparative Examples were dropped onto a glass plate that had been subjected to a release treatment with octadecyltrichlorosilane, and 1 mm thick shim plates were placed on the left and right of the oil droplet as spacers, and then the oil droplet was sandwiched between two glass plates that had also been subjected to a release treatment with octadecyltrichlorosilane. The oil droplet of the active energy ray curable composition sandwiched between the two glass plates was exposed to irradiation intensity of 50 mW / cm using a UV-LED irradiation device "LHPUV365 / 2501" manufactured by a subsidiary of Iwasaki Electric Co., Ltd. 2 , cumulative light intensity 8000mJ / cm 2 The resulting coin-shaped cured product was heated in a fan oven at 100°C for 20 minutes, and the initial transmittance at a wavelength of 410 nm was measured using a JASCO V-770 UV-Vis-NIR spectrophotometer.

[0123] [Method for measuring transmittance after heat resistance test] The coin-shaped cured product measured by the transmittance measurement method was (1) heated at 175°C for 10 minutes in a fan oven, and then the transmittance at a wavelength of 410 nm was measured using a JASCO Corporation ultraviolet-visible-near infrared spectrophotometer "V-770" as transmittance after heat resistance test 1 and transmittance after heat resistance test 2. The heating temperature was set to 175°C in accordance with the reflow process of low-temperature molten solder and normal molten solder.

[0124] [Water absorption measurement method] Using a 0.2 mm thick shim plate and a glass rod, the active energy ray-curable compositions obtained in the Examples and Comparative Examples were applied to an acrylic plate, and then the applied compositions were irradiated with a belt conveyor-type ultraviolet ray irradiation device (120 W metal halide lamp) manufactured by I-Graphics Co., Ltd. at an integrated light dose of 3,000 mJ / cm. 2 A sheet-like cured product having a film thickness of 0.2 mm was obtained by irradiating the sheet-like cured product with ultraviolet rays of 1000 nm to obtain a test piece for measuring water absorption rate by cutting the obtained sheet-like cured product into a length of 5 cm × width of 5 cm using a dumbbell cutter. The test piece thus prepared was dried in a blower oven at 50°C for 24 hours, and the weight of the test piece was measured and defined as the initial weight m1. After the initial weight measurement, the test piece was immersed in 300 ml of pure water at 23°C for 24 hours. After the test piece was taken out of the pure water, the remaining moisture was wiped off with a nonwoven fabric "Bemcot" manufactured by Asahi Kasei Corporation, and the weight of the test piece was measured and defined as the weight after immersion m2. After the weight measurement after immersion, the test piece was dried in a blower oven at 50°C for 24 hours, and the weight of the test piece was measured and defined as the dry weight m3. Using the above m1 to m3, the water absorption rate was calculated according to the following formula.

[0125]

number

[0126] [Method for evaluating humidity and heat resistance] The active energy ray-curable compositions obtained in the examples and comparative examples were dropped onto a cover glass that had been subjected to an adhesion treatment using a silane coupling agent "KBM-5103" manufactured by Shin-Etsu Chemical Co., Ltd., and shaped by a lens replica. After that, the active energy ray-curable compositions were irradiated with a UV-LED irradiation device "LHPUV365 / 2501" manufactured by Iwasaki Electric Co., Ltd. at an irradiation intensity of 50 mW / cm. 2 , cumulative light intensity 450mJ / cm 2 After the lens replica was released from the mold, a development process was carried out with propylene glycol monomethyl ether to remove the uncured resin composition. 2After the main curing was performed by the above method, a wafer-level lens was obtained by post-baking at 100°C for 90 minutes using a fan oven. The obtained wafer-level lens was subjected to a moist heat resistance test at a temperature of 85°C and a relative humidity of 85% for 1000 hours using a small environmental tester "SH-222" manufactured by Espec Corporation. After the test, the lens was observed using a microscope "VHX900" manufactured by Keyence Corporation and a laser microscope "OLS5000" manufactured by Olympus Corporation, and evaluated according to the following criteria.

[0127] ⊚: No peeling, interface defects, or internal defects were observed. ○: No peeling or interface defects, but 1 to 10 internal defects. △: Medium degree of peeling, interface abnormalities, and internal defects. ×: Peeling, interface abnormalities, and internal defects are severe.

[0128] [Crack resistance evaluation method] A wafer-level lens was prepared in the same manner as in the lens preparation procedure described in the evaluation method for wet heat resistance, and sputtering was performed using a Shimadzu Corporation three-target magnetron sputtering device "HSR-522" under the conditions of target SiO2, introduction gas argon, gas flow rate 15sccm, room temperature 25°C, and sputtering time: 40min, to obtain a laminate in which a silicon oxide thin film having a thickness of 0.5μm was laminated on the surface of the cured product. The surface of the laminate was observed with a Keyence Corporation microscope "VHX900", and the initial appearance of the laminate was evaluated according to the following criteria. Next, after heat treatment at 175°C for 5 minutes using a blower oven, the surface of the laminate was observed with a Keyence Corporation microscope "VHX900", and the appearance of the laminate after heat resistance was evaluated according to the following criteria. ⊚: No cracks or wrinkles were observed in the sputtered film. ◯: Very slight cracks and wrinkles occurred in the sputtered film. △: Minor cracks and wrinkles occurred in the sputtered film. ×: Cracks and wrinkles occurred in the sputtered film.

[0129] [Table 1]

[0130] [Table 2]

[0131] [Table 3]

[0132] The abbreviations in Tables 1 to 3 stand for the following: "4-HBA"; 4-Hydroxybutyl acrylate (Mitsubishi Chemical Corporation) "CHDMMA"; Cyclohexanedimethanol monoacrylate (Mitsubishi Chemical Corporation) "PE-1"; Pentaerythritol tetrakis(3-mercaptobutyrate) (Showa Denko K.K.)

[0133] From the evaluation results in Tables 1 to 3, it was revealed that the cured products formed by the active energy ray curable compositions of the present invention in Examples 1 to 13 had high Abbe numbers, high heat resistance, water absorption controlled to 4% or less, and high moist heat resistance. Furthermore, the lens samples in Examples 1 to 13 had no warping after curing, no cracks or cracks, and had good appearances. Furthermore, it was revealed that the occurrence of cracks and wrinkles was suppressed in the laminates, both initially and after the heat resistance test.

[0134] On the other hand, Comparative Examples 1 to 4 are examples of active energy ray-curable compositions that do not contain the component (C), and it was confirmed that the laminate had slight wrinkles and cracks both in the initial appearance and in the appearance after the heat resistance test, and had insufficient crack resistance.

[0135] Comparative Examples 5 and 6 are examples of active energy ray-curable compositions which do not contain the component (C) defined in the present invention and which have different ratios of the component (A) and the component (B). It was confirmed that Comparative Example 5, in which the component (A) was used in an amount of 70 parts by mass, showed interface abnormalities and internal defects in the moist heat resistance test and had insufficient moist heat resistance, and Comparative Example 6, in which the component (B) was used in an amount of 70 parts by mass, showed wrinkles and cracks in the laminate both initially and after the heat resistance test, indicating that the crack resistance was significantly insufficient.

[0136] Comparative Example 7 is an example of an active energy ray-curable composition not containing the component (B). In the moist heat resistance test, interfacial abnormalities and internal defects occurred, and it was confirmed that the moist heat resistance was extremely insufficient, and that minor cracks occurred in the laminate after the heat resistance test, indicating that the crack resistance was insufficient.

[0137] Comparative Example 8 is an example of an active energy ray-curable composition that does not contain the component (A), and it was confirmed that the transmittance after the heat resistance test was significantly reduced and the heat resistance was insufficient.

Claims

1. A polycarbonate diol di(meth)acrylate (A) represented by the following general formula (1), a compound (B) other than the polycarbonate diol di(meth)acrylate (A) having one or two (meth)acryloyl groups, an alkylene glycol structure, and a cyclic structure in one molecule; and a compound (C) having six or more (meth)acryloyl groups and a multi-branched structure in one molecule, the cyclic structure is a cyclohexane structure and / or a tricyclodecane structure, The active energy ray-curable composition, wherein the multi-branched structure is at least one structure selected from the group consisting of a dendron structure, a dendritic structure, a hyperbranched structure, and a star structure. 【Chemistry 1】 (In the formula, R 1 each independently represents a hydrogen atom or a methyl group; R 2 each independently represents a hydrocarbon group having 1 to 10 carbon atoms; and n is an integer of 1 to 10.

2. R in the general formula (1) 2 The active energy ray-curable composition according to claim 1, wherein each of the groups independently has a linear hydrocarbon group having 5 to 6 carbon atoms or a cyclohexane structure.

3. 3. The active energy ray-curable composition according to claim 1, wherein the alkylene glycol structure is at least one selected from the group consisting of ethylene glycol, propylene glycol, and neopentyl glycol.

4. The active energy ray-curable composition according to any one of claims 1 to 3, wherein the number of repeating units of the alkylene glycol structure is an integer of 2 to 15.

5. The active energy ray curable composition according to any one of claims 1 to 4, further comprising a compound (D) having one or two (meth)acryloyl groups in one molecule and one or more hydroxyl groups in one molecule, other than the polycarbonate diol di(meth)acrylate (A), the compound (B), and the compound (C).

6. The active energy ray-curable composition according to claim 5, wherein the compound (D) is at least one selected from the group consisting of 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexanedimethanol mono(meth)acrylate, and sorbitol ethylene oxide-modified di(meth)acrylate.

7. A cured product of the active energy ray-curable composition according to any one of claims 1 to 6.

8. 8. The cured product according to claim 7, which has a water absorption rate in the range of 0.1 to 4.0% as measured by Method C of JIS test method (K7209:2000).

9. A lens comprising the cured product according to claim 7.

10. A wafer level lens comprising the cured product according to claim 7.

11. A lens comprising the cured product according to claim 7 and having an inorganic compound layer on at least one surface thereof.

12. The lens according to claim 11, wherein the inorganic compound layer is an anti-reflection layer.

13. A camera module comprising the lens according to any one of claims 7 to 12.

Citation Information

Patent Citations

  • Composition and article

    JP2006070145A

  • Film-like optical waveguide

    JP2009157125A

  • Imaging lens and imaging apparatus

    JP2009251368A

  • Curable resin composition, cured product thereof, and plastic lens

    JP2011157437A

  • Hard coat resin composition, cured product of the same, and method of manufacturing cured product

    JP2013204011A