Polyphenylene sulfide film, polyphenylene sulfide film roll and its manufacturing method

By controlling the fluorescence spectrum and manufacturing conditions, polyphenylene sulfide films with minimal modified polymers are produced, addressing defects and ensuring high-quality film production for electronic devices.

JP7559469B2Active Publication Date: 2024-10-02TORAY INDUSTRIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020161688
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-22
Filing Date
2020-09-28
Publication Date
2024-10-02
Estimated Expiration
2040-09-28

AI Technical Summary

Technical Problem

Polyphenylene sulfide films used in high-performance electronic devices are prone to defects due to the presence of modified polymers, which can cause shape changes and holes during the film-forming process, and there is no effective method to identify or suppress their production.

Method used

A polyphenylene sulfide film and roll are produced with minimal modified polymers by controlling the fluorescence spectrum, using infrared spectroscopy to measure peak intensities, and optimizing film thickness, orientation, and manufacturing conditions to minimize defects.

Benefits of technology

The solution results in a high-quality film with few defects, maintaining excellent mechanical properties and flatness, suitable for applications requiring precise film quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559469000001
    Figure 0007559469000001
  • Figure 0007559469000002
    Figure 0007559469000002
Patent Text Reader

Abstract

To provide a polyphenylene sulfide film containing very little polyphenylene sulfide modified polymer, and a film roll.SOLUTION: There is provided a polyphenylene sulfide film in which, in a film plane, a maximum wavelength of a fluorescence spectrum is not observed in a wavelength region of 450 nm or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyphenylene sulfide film having an extremely small amount of modified polymer, the main component of which is a resin material constituting the film, within the film plane, a roll made of the film, and a method for producing the same. [Background technology]

[0002] As electronic and information devices become more functional and precise, the quality requirements for the materials used are becoming stricter. For example, the quality requirements are strict for base films for capacitors, substrate films for high-frequency circuits, release films, etc. These materials often require processing such as laminating other materials to the base film or coating.

[0003] Therefore, in order not to impair the quality of the above-mentioned components, it is desirable for the base film to have few surface defects and internal defects, and at the same time, to improve workability during processing, it is required that the base film have good heat resistance, chemical resistance, dimensional stability, and mechanical properties.

[0004] As films and sheets conventionally used in the above fields, films of polyethylene, polypropylene, polyester, polyimide, fluororesin, etc. have been used, among which polyphenylene sulfide films are suitable for use due to their excellent heat resistance, chemical resistance, dimensional stability, and mechanical properties, and their range of use is expanding. As an example of a high-quality polyphenylene sulfide film, a polyphenylene sulfide film with few surface defects has been proposed (Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-34356 A Summary of the Invention [Problem to be solved by the invention]

[0006] Polyphenylene sulfide film has good heat resistance, chemical resistance, dimensional stability, and mechanical properties, making it suitable for high-performance electronic device components, but a chronic issue is that polyphenylene sulfide film may contain localized modified substances. Since modified polyphenylene sulfide has different resin properties from polyphenylene sulfide, it may induce shape changes or holes around the modified substances during the film production process, which may impair the quality of the film. However, since no analytical method has been found that can distinguish between modified polyphenylene sulfide and polyphenylene sulfide, the true nature and cause of the modified substances could not be identified, and no method has been established to suppress the generation of modified substances.

[0007] The present invention provides a polyphenylene sulfide film and a polyphenylene sulfide film roll, which are characterized by having very few defects due to modified polymers containing the resin raw material constituting the film as a main component and having good flatness, and a method for producing the same. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention has the following configuration. [1] A polyphenylene sulfide film, characterized in that no maximum wavelength of the fluorescence spectrum is observed in the wavelength region of 450 nm or more within the film plane. [2] The cross section of the film was measured at 4096 points using infrared spectroscopy (ATR method) at wavelengths of 1200 to 1250 cm -1 Peak intensity (IR-p) in the range of 1450-1500 cm -1 A polyphenylene sulfide film in which, when the ratio X [(IR-p) / (IR-s)] of peak intensities (IR-s) in the range is calculated, the proportion of ratios X that are 0.01 or less is 0.5 or more. [3] The polyphenylene sulfide film according to [1] or [2], characterized in that the thickness of the film is 1.0 μm or more and 500 μm or less. [4] A polyphenylene sulfide film roll obtained by winding up a polyphenylene sulfide film characterized in that no maximum wavelength of the fluorescence spectrum is observed in the wavelength region of 450 nm or more within the film plane. [5] The cross section of the film was measured at 4096 points using infrared spectroscopy (ATR method) at wavelengths of 1200 to 1250 cm -1 Peak intensity (IR-p) in the range of 1450-1500 cm -1 A polyphenylene sulfide film roll obtained by winding up a polyphenylene sulfide film in which, when the ratio X [(IR-p) / (IR-s)] of peak intensities (IR-s) in the range of 100 to 1500 nm is calculated, the ratio X being 0.01 or less is 0.5 or more. [6] The polyphenylene sulfide film roll according to [4] or [5], wherein the thickness of the film is 1.0 μm or more and 500 μm or less. [7] The polyphenylene sulfide film roll according to any one of [4] to [6], characterized in that the width of the film roll is 300 mm or more, and the length of the polyphenylene sulfide film wound around the roll is 500 m or more. [8] The polyphenylene sulfide film roll according to any one of [4] to [7], wherein the orientation angle of the film roll is 85 degrees or less with respect to the longitudinal direction of the film. [9] A method for producing a polyphenylene sulfide film according to either [1] or [3], comprising the steps of feeding a polyphenylene sulfide film resin composition into an extruder, melt-kneading the composition in the extruder, extruding the composition from a die and cooling and solidifying the composition, and then stretching the composition at least in the running direction of the film, wherein the oxygen concentration in the die from the extruder is 1.0 volume % or less.

[10] A method for producing a polyphenylene sulfide film according to [9], characterized in that the residence time of the resin after the polyphenylene sulfide resin composition is charged into an extruder and melt-kneaded in the extruder and before being extruded from a die is less than 120 minutes.

[11] A method for producing a polyphenylene sulfide film roll according to any one of [4] to [8], comprising the steps of feeding a polyphenylene sulfide film resin composition into an extruder, melt-kneading the composition in the extruder, extruding the composition from a die, cooling and solidifying the composition, and stretching the composition at least in the running direction of the film, wherein the oxygen concentration in the die from the extruder is 1.0 volume % or less.

[12] The method for producing a polyphenylene sulfide film roll according to

[11] , wherein the residence time of the polyphenylene sulfide resin composition after being charged into an extruder and melt-kneaded in the extruder until being extruded through a die is less than 120 minutes. Effect of the Invention

[0009] According to the present invention, it is possible to provide a polyphenylene sulfide film and a polyphenylene sulfide film roll which contain an extremely small amount of modified polymer that is mainly composed of the resin raw material constituting the film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The polyphenylene sulfide in the present invention refers to a polymer in which 85 mol % or more (preferably 90 mol % or more) of the repeating units are composed of structural units represented by the following structural formula: If the content of such components is less than 85 mol %, the crystallinity and softening point of the polymer may decrease, and the heat resistance, dimensional stability, mechanical properties, mold releasability, etc. may be impaired. chemical formula 1

[0011] [ka]

[0012] In the above polyphenylene sulfide, units containing copolymerizable sulfide bonds may be contained as repeating units, so long as the repeating units account for less than 15 mol %, preferably less than 10 mol %, of the total repeating units. The copolymerization method for the polymer may be random or block type.

[0013] In the present invention, the PPS film refers to a film in which 90% by weight or more of the resin constituting the film is PPS.

[0014] One embodiment of the present invention is a polyphenylene sulfide film in which the maximum wavelength of the fluorescence spectrum is not observed in the wavelength region of 450 nm or more in the film plane. By making such a polyphenylene sulfide film, it is possible to make a film in which the modified polymer mainly composed of the resin constituting the film is very small. Such modified polymers have a fluorescence intensity peak observed at 450 nm or more. This modified polymer is produced by modifying polyphenylene sulfide resin, and as a result of the inventors' intensive investigation, it was found that it is either a polyphenylene sulfide resin in which polyphenylene sulfide resins are oxygen-bridged with each other, or a polyphenylene sulfide resin having a sulfonyl group in which the sulfur atom of the polyphenylene sulfide resin is oxidized. In addition, since these modified sites have resin properties different from polyphenylene sulfide, deformation of the peripheral part during the film formation process, especially when the film is thin, is caused by thickness unevenness, and conversely, because it is a thin film, holes are induced, which may significantly impair the quality of the film. As a result of intensive research by the present inventors, it was found that modified polymers of polyphenylene sulfide resin are generated especially during the process of drying the resin before film formation or during melt extrusion during film formation. It is important to manage these modified polymers as modified sites in the film. For example, unlike unmelted polyphenylene sulfide resin due to insufficient melting or iron powder generated during the film formation process due to friction of the manufacturing machine, these foreign matters can be observed as having a fluorescence spectrum maximum wavelength of 450 nm or more and can be managed.

[0015] This modified portion does not contain inorganic substances such as SUS, and is composed only of resin.

[0016] In another embodiment of the present invention, the cross section of the film is measured at 4096 points by infrared spectroscopy (ATR method) in the measurement method described below, and the measurement results are shown in Table 1.-1 Peak intensity (IR-p) in the range of 1450-1500 cm -1 When the ratio X [(IR-p) / (IR-s)] of the peak intensity (IR-s) in the range is calculated, the ratio X of 0.01 or less is 0.5 or more. By producing such a polyphenylene sulfide film, the film can be made to have an extremely small amount of modified polymer. When the cross section of the film is measured by infrared spectroscopy (ATR method), the modified polymer is -1 On the other hand, unmodified polyphenylene sulfide resin has a wavelength of 1450 to 1500 cm -1 (peak due to aromatic ring C=C stretching) in the range of 1200 to 1250 cm -1 Peak intensity (IR-p) in the range of 1450-1500 cm -1 By having many portions where the ratio X [(IR-p) / (IR-s)] of peak intensities (IR-s) in the range is 0.01 or less, the film can have an extremely small amount of modified polymer. More preferably, the proportion where the ratio X is 0.01 or less is 0.6 or more.

[0017] The polyphenylene sulfide film of the present invention preferably has a thickness of 1.0 μm or more and 500 μm or less, more preferably 250 μm or less. If the film thickness is less than 1.0 μm, the film breaking strength and breaking elongation are significantly reduced, and the processability may deteriorate. If the film thickness is more than 500 μm, burrs may easily occur during processing of the film, making handling difficult. By setting the film thickness within the above range, the film can be made to have good film breaking strength and breaking elongation, and to suppress the generation of burrs during processing.

[0018] One embodiment of the present invention is a polyphenylene sulfide film roll obtained by winding up a polyphenylene sulfide film characterized in that no maximum wavelength of the fluorescence spectrum is observed in the wavelength region of 450 nm or more within the film plane.

[0019] The polyphenylene sulfide film roll of the present invention preferably has a width of 300 mm or more. It may be an intermediate product roll wound immediately after the film is produced, or may be a product roll obtained by slitting the intermediate product roll. The length of the polyphenylene sulfide film wound on the polyphenylene sulfide film roll is preferably 500 m or more, and more preferably 1000 m or more. Since the longer the film length, the easier it is for the molten resin to remain, when the film length is 1000 m or more in particular, the conventional polyphenylene sulfide film roll has a modified portion, but the polyphenylene sulfide film of the present invention has the effect of suppressing the modified portion, and is therefore less likely to have defects.

[0020] The polyphenylene sulfide film wound on the polyphenylene sulfide film roll of the present invention is particularly effective in suppressing modified sites when the orientation angle with respect to the longitudinal direction of the film is 85 degrees or less. As described above, when the residence time in the film production process is long, the molten resin is usually extruded from a rectangular die in the width direction perpendicular to the film production direction while filtering the molten resin with a cylindrical filter, but the molten resin is more likely to stagnate at the flow rate in the outer periphery of the filter than at the flow rate in the center of the filter, and the resin conveyed to the rectangular die has a larger amount of resin remaining at the end, so that modified sites are more likely to occur in the end direction with respect to the width direction of the film. Therefore, modified resin is more likely to occur in the part where the orientation angle with respect to the longitudinal direction of the film is 85 degrees or less.

[0021] The polyphenylene sulfide film of the present invention preferably contains particles for the purpose of increasing the lubricity of the film. As the type of particles, particles that do not affect the fluorescent spectrum of the polyphenylene sulfide film of the present invention can be used. One type of particle may be used alone, or two or more types may be used in combination. Among the particles, calcium carbonate particles are preferred because they have good dispersibility in the polyphenylene sulfide film.

[0022] The particles contained in the polyphenylene sulfide film of the present invention preferably have an average particle size of 0.1 μm or more and 10 μm or less, more preferably 5 μm or less, and even more preferably 2 μm or less. If the average particle size is larger than 10 μm, the film surface protrusions become large, and the film may not be suitable for use in release applications. If the average particle size is less than 0.1 μm, the film surface has poor slipperiness, and the film is likely to be scratched during transport or processing, and the quality of the film may be deteriorated.

[0023] The content of particles contained in the polyphenylene sulfide film of the present invention is preferably 0.1% by weight or more and 5% by weight or less, more preferably 3% by weight or less. If the particle content is more than 5% by weight, the film surface protrusions become large, and the film may not be suitable for use in release applications. If the particle content is less than 0.1% by weight, the film surface becomes less slippery, and the film may be easily scratched during transport or processing, resulting in a deterioration in film quality.

[0024] The polyphenylene sulfide film of the present invention may be blended with resins other than polyphenylene sulfide (heterogeneous polymers) as long as they do not adversely affect the fluorescence spectrum of the present invention, and additives such as antioxidants, heat stabilizers, lubricants, and ultraviolet absorbers may also be added.

[0025] The polyphenylene sulfide film of the present invention may be a single film or a composite film. Examples of composite films include laminated films of two or more layers. For example, the film may be a two-layer laminated film consisting of layer A / layer B having the polyphenylene sulfide film of the present invention as a surface layer (layer A), or a three-layer laminated film consisting of layer A / layer B / layer A. From the viewpoints of flatness and voltage resistance, it is preferable to apply the polyphenylene sulfide film of the present invention to all layers.

[0026] The surface of the polyphenylene sulfide film of the present invention may be coated or laminated with a resin or compound such as an antistatic agent, or may be subjected to a suitable surface treatment, such as a corona discharge treatment or plasma treatment, as long as it does not adversely affect the fluorescent spectrum of the present invention.

[0027] (Film manufacturing method) Regarding the method for producing the polyphenylene sulfide film of the present invention, it is preferable to produce it, for example, by the steps shown below.

[0028] First, the method for producing polyphenylene sulfide of the present invention will be described. Polyphenylene sulfide can be produced, for example, by polymerizing an alkali metal sulfide (alkali sulfide) and a dihalobenzene.

[0029] Examples of alkali metal sulfides include lithium sulfide, sodium sulfide, potassium sulfide, rubidium sulfide, and cesium sulfide, among which sodium sulfide is preferred. These alkali metal sulfides can be used as hydrates or aqueous mixtures, or in the form of anhydrides. In addition, alkali metal sulfides prepared in situ in the reaction system, and alkali metal sulfides prepared from alkali metal hydrates such as sulfide, lithium hydroxide, and sodium hydroxide and hydrogen sulfide, can also be used. The alkali metal sulfides may be used alone or in combination of two or more.

[0030] Examples of dihalobenzenes include p-dihalobenzenes such as p-dichlorobenzene and p-dibromobenzene, m-dihalobenzenes such as m-dichlorobenzene, and dihalobenzenes containing a substituent other than a halogen atom, such as 1-methoxy-2,5-dihalobenzene and 3,5-dichlorobenzoic acid. Among these, p-dihalobenzene is preferred, and p-dichlorobenzene is particularly preferred. Dihalobenzenes may be used alone or in combination of two or more.

[0031] The amount of dihalobenzene used (charged amount) is preferably in the range of 0.9 to 2.0 mol, more preferably 1.0 to 1.3 mol, per 1 mol of charged alkali metal sulfide, in order to obtain polyphenylene sulfide with a high molecular weight. If the amount of dihalobenzene used is less than 0.9 mol or more than 2.0 mol, it is difficult to obtain polyphenylene sulfide with a high viscosity (high degree of polymerization) suitable for processing, which is not preferable.

[0032] In the present invention, a monohalo compound (not necessarily an aromatic compound) can be used in combination with dihalobenzene in order to form terminals of the resulting polyphenylene sulfide or to adjust the polymerization reaction or molecular weight, etc. Also, in order to form a branched or crosslinked polymer, it is possible to use in combination a trihalo or higher polyhalo compound (not necessarily an aromatic compound) such as 1,2,4-trichlorobenzene or 1,3,5-trichlorobenzene, an active hydrogen-containing halogen aromatic compound, a halogen aromatic nitro compound, etc.

[0033] In the present invention, it is preferable to add a polymerization aid to carry out the reaction in order to adjust the degree of polymerization. As the polymerization aid, a known polymerization aid generally used as a polymerization aid for polyphenylene sulfide can be used, and examples thereof include alkali metal hydroxides (caustic alkali), alkali metal carboxylates, alkali metal carbonates, alkaline earth metal hydroxides, and alkaline earth metal carbonates. Among these, alkali metal hydroxides and alkali metal carboxylates are preferably used.

[0034] Examples of alkali metal hydroxides include sodium hydroxide, potassium hydroxide, and lithium hydroxide. Examples of alkali metal salts of carboxylic acids include lithium acetate, sodium acetate, potassium acetate, sodium propionate, lithium valerate, sodium benzoate, sodium phenylacetate, and potassium p-toluate. Among these, sodium acetate is preferably used because it is inexpensive and easily available. The alkali metal salts of carboxylic acids can be used as anhydrides, hydrates, or aqueous solutions. The alkali metal salts of carboxylic acids may be formed by adding and reacting an organic acid with one or more compounds selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, and alkali metal bicarbonates in an organic amide solvent in approximately equal chemical equivalent amounts.

[0035] The polymerization aid may be used alone or in combination of two or more. The amount of the polymerization aid used can be appropriately selected from a wide range depending on the type of the polymerization aid itself, and the types of the alkali metal sulfide and dihalobenzene, but is preferably in the range of 0.01 mol to 5 mol, more preferably 0.1 to 2 mol, per mol of the alkali metal sulfide charged.

[0036] As the solvent, it is preferable to use a polar solvent such as an organic amide solvent. Among organic amide solvents, N-alkylpyrrolidones such as N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone, caprolactams such as N-methyl-ε-caprolactam, and abrogative organic amide solvents such as 1,3-dialkyl-2-imidazolidinone, tetraalkylurea, and hexaalkylphosphoric acid triamide are preferably used because of their high reaction stability. Among these, N-methyl-2-pyrrolidone (hereinafter sometimes abbreviated as NMP) is particularly preferably used. The amount of the solvent used is preferably in the range of 0.2 to 10 moles per mole of the charged alkali metal sulfide, and more preferably in the range of 2 to 5 moles.

[0037] (1) The polyphenylene sulfide used in the polyphenylene sulfide film of the present invention can be produced by adding an appropriate amount of an alkali metal sulfide and a dihalobenzene, and if necessary, an appropriate amount of a halogenated compound other than dihalobenzene and a polymerization aid to a polar solvent such as an amide-based high-boiling point solvent, and reacting them under high temperature and high pressure. The pressure in the polymerization system is appropriately selected depending on the type and amount of the aid used, the desired degree of polymerization, etc. The temperature in the polymerization system and the polymerization time are also appropriately selected depending on the type and amount of the aid used, the desired degree of polymerization, etc., but are preferably 20 minutes to 50 hours at a temperature of 200 to 300 ° C, and more preferably 1 to 10 hours at a temperature of 230 to 280 ° C. As described above, a powdery or granular polyphenylene sulfide is obtained. Next, the obtained powdery or granular polyphenylene sulfide is washed with water and / or a solvent to separate by-product salts, polymerization aids, unreacted monomers, etc.

[0038] (2) When particles are added to the polyphenylene sulfide film of the present invention as described above, the particles are first mixed with the powdered or granular polyphenylene sulfide obtained in (1) above, and then uniformly mixed using a Henschel etc. When blending resins (heterogeneous polymers) other than polyphenylene sulfide, or when adding additives such as antioxidants, heat stabilizers, lubricants, and ultraviolet absorbers, they are mixed with polyphenylene sulfide in the same manner.

[0039] The resulting mixture is then fed to an extruder (preferably an extruder having one or more vent holes), melt-kneaded at a temperature of 290 to 360°C, and extruded through an appropriate die to obtain a polyphenylene sulfide resin composition. Alternatively, the mixture may be melt-molded into a gut shape and cut to a length of about 2 to 10 mm to obtain a pellet-shaped polyphenylene sulfide resin composition. The resulting polyphenylene sulfide resin composition is dried in a vacuum heating dryer at a temperature of 100 to 180°C for about 1 to 5 hours.

[0040] In the case where particles are not added, the polyphenylene sulfide obtained in (1) can be mixed with a resin other than polyphenylene sulfide (heterogeneous polymer) and additives such as an antioxidant, a heat stabilizer, a lubricant, and an ultraviolet absorber as necessary, and extrusion-molded or melt-molded in the same manner as in the case of a mixture containing particles, and used as a polyphenylene sulfide resin composition.

[0041] The polyphenylene sulfide resin composition thus produced may be used alone or in a mixture of two or more. For example, polyphenylene sulfide resin pellets to which particles have been added (hereinafter also referred to as particle pellets) and polyphenylene sulfide resin pellets to which particles have not been added (hereinafter also referred to as particle-free pellets) may be mixed and used.

[0042] (3) Next, the polyphenylene sulfide film of the present invention is produced using the polyphenylene sulfide resin pellets obtained in (2). The polyphenylene resin pellets obtained in (2) are stirred in a mixer while being heated to a temperature of 120 to 230°C (preferably 160°C to 200°C) under reduced pressure (preferably a vacuum degree of 0 to 50 mmHg), and dried for 3 hours or more (preferably 5 to 10 hours). The drying of the polyphenylene sulfide resin composition may be carried out in multiple stages, such as drying the polyphenylene sulfide resin composition as described above, gradually cooling it to room temperature, and drying it again. Here, if the drying temperature exceeds 230°C, there is a concern that the dried raw material will solidify and interfere with the film formation, and if the temperature is less than 120°C, impurities in the polyphenylene sulfide raw material, particularly high-boiling point compounds that volatilize when heated to about 250°C, may remain, causing defects in the film. If the pressure reduction is insufficient, the polyphenylene sulfide resin will react with oxygen, and a modified polymer will be easily produced.

[0043] Next, the polyphenylene sulfide film of the present invention is produced using the dried polyphenylene sulfide resin composition, and the film may be a single layer or a composite layer. When producing a composite film, the lamination method may be coating, laminating, coextrusion, or the like. Among them, lamination by coextrusion is preferred in terms of controlling the thickness of each layer constituting the polyphenylene sulfide film of the present invention. The polyphenylene sulfide film of the present invention is produced as follows. First, the polyphenylene sulfide resin composition is fed to a melt extrusion device and heated to a temperature equal to or higher than the melting point of the polyphenylene sulfide resin composition (preferably 290 to 360°C) to melt it. Next, the melt is extruded from a slit-shaped die outlet and rapidly cooled (cast) on a rotating metal drum called a casting roll to solidify it, or the like, to produce an unstretched film. At this time, it is preferable to install a gear pump, a static mixer, and a filtration device in the polymer flow path. If the melt extrusion time is long, the polyphenylene sulfide resin has more opportunities to react with remaining oxygen, so that there is a high possibility of oxygen crosslinking or sulfonation, i.e., the generation of a modified polymer. In the filtration device, the resin is more likely to remain near the outer wall on the inner surface of the casing, so that the polymer has more opportunities to be modified, and is more likely to be observed as a modified polymer in the final film.

[0044] The residence time during melting of the resin (the time from when the polyphenylene sulfide resin composition is fed into the extruder to when it is melt-kneaded in the extruder and then extruded from the die) is preferably less than 120 minutes, and more preferably less than 90 minutes. From the viewpoint of the object of the present invention, it is not necessary to set a lower limit for the residence time, but in order to prevent insufficient melting, it is practical to set the residence time to 10 minutes or more. In addition, the thinner the film thickness, the lower the amount of molten polymer discharged in the film forming process described below, so that the residence time in the extrusion system tends to be longer. As a method for shortening the residence time, there is a method of increasing the film forming speed, but there is a case where the amount of heat is insufficient in the film heat treatment process, and the dimensional stability is deteriorated in the post-processing in which heat is applied to the film. Therefore, in the present invention, a method of controlling the residence time and suppressing the generation of modified polymers can be mentioned as a preferred method.

[0045] In the polyphenylene sulfide film of the present invention, the oxygen concentration in the die from the extruder is preferably 1.0% by volume or less. If the oxygen concentration in the die from the extruder is greater than 1.0% by volume, the sulfur atoms of the polyphenylene sulfide resin may react with oxygen, promoting the sulfonation of polyphenylene sulfide, or polyphenylene sulfide may be crosslinked with oxygen, which may lead to the generation of modified polymers. The cause of the oxygen concentration being greater than 1.0% by volume may be that the air remaining in the gaps between the pellets is directly contained in the extruder. In order to make the oxygen concentration in the die from the extruder 1.0% by volume or less, a method of injecting an inert gas such as nitrogen gas, argon gas, or helium gas when equalizing the pressure in the system after drying the pellets under reduced pressure may be mentioned. Among inert gases, a gas with a high purity is more effective in suppressing the generation of modified polymers.

[0046] Examples of such methods include a sequential biaxial stretching method in which the obtained unstretched film is stretched in the film's longitudinal direction (sometimes called the machine direction or the running direction of the film) and then in the film's width direction (horizontal direction) using a group of rolls and a tenter, and a simultaneous biaxial stretching method in which stretching is simultaneously performed in the film's longitudinal direction and width direction. Of these, the sequential biaxial stretching method is preferred.

[0047] When the sequential biaxial stretching method is used, the stretching conditions can be appropriately selected from a wide range depending on various conditions such as the type of polyphenylene sulfide contained in the polyphenylene sulfide resin composition, and the presence and type of other resins and additives. However, it is preferable to stretch at a temperature of 60 to 150°C, preferably 70 to 130°C, and more preferably 80 to 110°C, at a stretching ratio of 2 to 7 times, preferably 2 to 5 times, and more preferably 3 to 5 times in the longitudinal direction (machine direction) and width direction (transverse direction), respectively.

[0048] The obtained stretched film is preferably further subjected to a heat treatment. The heat treatment conditions can be appropriately selected from a wide range depending on various conditions such as the type of polyphenylene sulfide contained in the polyphenylene sulfide resin composition, and the presence and type of other resins and additives. However, it is preferable to perform the heat treatment at a temperature of 180 to (melting point of polyphenylene sulfide composition)°C, preferably 200 to (melting point of polyphenylene sulfide resin composition-5)°C, for 1 to 60 seconds under a constant length or limited shrinkage of 15% or less, in terms of heat resistance, mechanical properties, and thermal dimensional stability. Furthermore, the film may be relaxed in one or two directions in order to improve the thermal dimensional stability.

[0049] The polyphenylene sulfide film thus obtained can be used for various industrial purposes, and since it also has the electrical insulation property that is a characteristic of polyphenylene sulfide resin, it can be particularly suitably used for capacitor applications and mold release applications. EXAMPLES

[0050] (Method of measuring physical properties) (1) Collection of evaluation target roles The intermediate product rolls obtained from each of the Examples and Comparative Examples were rewound, and slit 200 mm from the center of the intermediate product roll in the width direction, and 400 mm from the cross section to both ends to make a total of five film rolls. In the obtained film rolls, the first, third, and fifth rolls were measured from one end (left side) of the intermediate product roll to the other end (right side). Also, for convenience, the first measurement object is designated "-1", the third "-2", and the fifth "-3". In other words, in Example 1, the first object (left end) is Example 1-1, the third object (center) is Example 1-2, the fifth object (right end) is Example 1-3, etc., and similar notations are used for the other Examples and Comparative Examples.

[0051] (2) Number of denatured sites and fluorescence intensity limit wavelength Each film roll obtained in (1) was divided into three equal parts in the longitudinal direction, and within each of the three equal parts, a piece of 500 x 500 mm was cut out in the longitudinal direction from an arbitrary location, and these were designated as samples A, B, and C in the order of the unwinding direction. Among the samples A, B, and C, the defective parts that could be visually confirmed within the sample were identified, and the one with the most defects was designated as observed sample D, and if no defects were confirmed, sample A was designated as observed sample D. If multiple defects were confirmed within a 10 mm square centered on an arbitrary defective part of observed sample D, they were counted as one defect within the sample. The defects were examined using a fluorescent microscope "BX-51" (Olympus Medical Science Co., Ltd.) and a spectroscopic unit "TFCAM-7000 / F" (Lambda Vision Co., Ltd.), with the wavelength region on the X axis and the wavelength spectrum on the Y axis, and the wavelength spectrum at the maximum of all defects was obtained. Among the wavelength spectra obtained, the wavelength with the maximum wavelength spectrum at 450 nm or more was designated as the intensity limit wavelength, and the defects were designated as the denatured parts, and the number of denatured parts was counted.

[0052] (3) Infrared spectroscopy (ATR method) In the observation sample D in (2), a cross section of the defect measured by the fluorescence microscope was cut out, and a micro PL spectroscopic analyzer "HR-320" (manufactured by Horiba Jobin Yvon) was used to perform infrared spectroscopic analysis by the ATR method at 64 × 64 points (4096 points) within a 32 μm square area, and data was collected using a two-dimensional infrared detector. -1 The peak observed in the range of 1450 to 1500 cm was determined as the peak derived from modified PPS (oxygen crosslinking, sulfonic acid component), and its intensity was determined as IR-p. -1 The peak observed in the IR-p / IR-s spectrum was determined as the peak derived from PPS (aromatic ring C=C stretching), and its intensity was determined as IR-s. For the 4096 points of ratio X [(IR-p) / (IR-s)], the proportion where ratio X≦0.01 was determined as A, and the proportion where ratio X>0.01 was determined as B. In the case of a laminated film, ATR measurements were carried out for each layer. For IR-s, the peak position does not change even if a few weight percent of resin other than PPS is mixed. -1 The peak observed in the IR spectrum was designated as IR-s.

[0053] (4) Thickness (μm) The cross-section of the film sliced ​​from the observation sample D obtained in (2) was cut using an electric microtome ST-201 manufactured by Japan Microtome Laboratory, and the sliced ​​film was observed under a transmitted light microscope to measure the thickness (μm).

[0054] (5) Orientation angle From the observation sample D obtained in (2), a microwave transmission type molecular orientation meter MOA-6004 (manufactured by Oji Scientific Instruments Co., Ltd.) was used to cut out a 300 x 300 mm piece in the longitudinal direction from a position 20 mm from the end of the film roll toward the center, and the orientation angle from the longitudinal direction was measured.

[0055] (6) Film formation stability In the film formation, the film formation stability was evaluated as follows. Good: Film breaks less than once per 2 days Pass: If the film breaks more than once per 2 days but less than once per day Fail ×: Film tear occurs more than once per day.

[0056] (7) Flatness Any two points were selected from the areas of the observation sample D where no defects were found, and the cross-sectional heights were confirmed with SEM, and the average was taken to obtain the film thickness A. In addition, the cross-sectional heights of the areas identified as modified areas of the sample used in (1) (any three modified areas were measured, and if there were fewer than three modified areas, only the number present was measured) were also confirmed with SEM in the same manner, and the average was taken to obtain the thickness B of the film where the modified areas were present, and the absolute value of the difference in thickness, |thickness A - thickness B|, was calculated, and the flatness of the film was evaluated as follows.

[0057] Good: 1.0% ≧ |Thickness A - Thickness B| / Thickness A x 100 Pass: 1.5% ≧ |Thickness A - Thickness B| / Thickness A x 100>1.0% Fail ×: |Thickness A - Thickness B| / Thickness A × 100>1.5%.

[0058] (8) Overall rating The overall evaluation of the film was made based on the film formation stability and flatness, and was rated on the following three-level scale. ◎: Both film formation stability and flatness are good ◯: Both film formation stability and flatness are acceptable or good, and at least one of them is acceptable ×: Failed at least one of film formation stability and flatness.

[0059] [Film manufacturing] (Production method of polyphenylene sulfide powder) In a 70L autoclave equipped with a stirrer, 8.181 kg (70.00 mol) of 48% by weight sodium hydrosulfide aqueous solution, 2.943 kg (70.63 mol) of sodium hydroxide with a purity of 96%, 11.45 kg (115.5 mol) of N-methyl-2-pyrrolidone (NMP), 2.239 kg (27.30 mol) of anhydrous sodium acetate, and 4.900 kg (272.2 mol) of ion-exchanged water were charged, and the mixture was gradually heated to 240°C over about 3 hours while passing nitrogen at normal pressure, and 9.12 kg of water and 0.14 kg of NMP were distilled out, and the reaction vessel was cooled to 160°C. The stirring speed in this reaction was 240 revolutions per minute (240 rpm).

[0060] The amount of water remaining in the system per mole of the charged alkali metal sulfide was 72.0 moles, including the water consumed in the hydrolysis of NMP. Also, 0.020 moles of hydrogen sulfide was scattered outside the reaction system per mole of the charged alkali metal sulfide.

[0061] Next, 10.29 kg (69.97 mol) of p-dichlorobenzene (p-DCB) and 9.090 kg (91.70 mol) of NMP were added to the reaction system. After sealing the reaction vessel under nitrogen gas, the temperature was raised from 200°C to 227°C at a rate of 0.8°C / min while stirring at 400 rpm, then the temperature was raised from 227°C to 270°C at a rate of 0.6°C / min, and the temperature was maintained at 270°C for 140 minutes. After that, the reaction system was gradually cooled to 250°C while adding 2.346 kg (130.3 mol) of ion-exchanged water to the system over 15 minutes. Next, the reaction system was gradually cooled from 250°C to 200°C at a rate of 1.0°C / min, and then quenched to near room temperature.

[0062] The obtained polymer was washed with 15 kg of N-methyl-2-pyrrolidone solvent (bath ratio 15) per 1 kg of dried PPS at 90°C for 1.5 hours and filtered. The obtained cake was washed / filtered twice with ion-exchanged water (bath ratio 15) at 70°C for 1.5 hours, then washed / filtered with ion-exchanged water (bath ratio 15) containing 1 wt% calcium acetate at 70°C for 1.5 hours, and again washed / filtered twice with ion-exchanged water (bath ratio 15) at 70°C for 1.5 hours. The obtained polymer was dried at a temperature of 150°C under vacuum for 4 days to obtain polyphenylene sulfide powder.

[0063] (Creating particle pellets) A slurry was prepared by dispersing 50% by weight of calcium carbonate particles having an average particle size of 1.0 μm in ethylene glycol. After filtering the slurry, the polyphenylene sulfide powder polymer was mixed with the calcium carbonate to a content of 7.0% by weight using a Henschel mixer. The resulting mixture was fed to a vent extruder having a twin screw with a diameter of 30 mm and melted at a temperature of 320° C. The melt was filtered through a metal fiber filter with a 95% cut pore size of 10 μm, and then extruded from a die with a pore size of 2 mm to obtain a gut-like resin composition. The composition was then cut into pieces of approximately 3 mm length to obtain particle pellets with a particle content of 5.0% by weight. Hereinafter, this is referred to as PPS resin A. (Preparation of particle-free pellets) The polyphenylene sulfide powder polymer alone was melt-extruded in the same manner as for the particle pellets to obtain particle-free pellets, hereinafter referred to as PPS resin B.

[0064] Comparative Example 1 The PPS resin A and PPS resin B obtained as described above were mixed so that the calcium carbonate content was 1.0% by weight relative to the total amount of resin, and then dried at a temperature of 180°C under a reduced pressure of 3 mmHg for 4 hours using a rotary vacuum dryer. After drying, nitrogen with a purity of 99% by volume or more was introduced to equalize the pressure.

[0065] The dried pellets were fed to a single-screw extruder, melted at 310°C in an atmosphere with an oxygen concentration of 0.1% by volume, and extruded in the form of a sheet with a width of 940 mm and a lip gap of 3 mm over 130 minutes. The sheet was then wrapped around a casting drum with a surface temperature of 25°C using an electrostatic casting method, and cooled and solidified to produce an unstretched film.

[0066] Using a sequential biaxial stretching method, the obtained unstretched film was stretched 4.0 times in the longitudinal direction at a temperature of 100° C., and then passed through a tenter to further stretch in the width direction, where it was stretched 3.5 times in the width direction at a temperature of 100° C. In a heat treatment chamber subsequent to the tenter used for stretching in the width direction, the film was further heat-treated at a temperature of 260° C., and relaxed in the width direction under a limited shrinkage of 5%, and the film was wound around a core to obtain an intermediate product roll of polyphenylene sulfide film having a width of 2000 mm and a length of 6000 m.

[0067] Comparative Example 2 An intermediate product roll of polyphenylene sulfide film was obtained in the same manner as in Comparative Example 1, except that low-purity nitrogen (nitrogen purity less than 99% by volume) was introduced to equalize the pressure after drying the pellets under reduced pressure, and the film thickness, oxygen concentration in extrusion system A, and residence time are shown in Table 1.

[0068] Comparative Example 3 The particle pellets and non-particle pellets were mixed with PPS resin A and PPS resin B so that the calcium carbonate content was 1.0% by weight, and then dried for 4 hours at a temperature of 180°C under a reduced pressure of 3 mmHg using a rotary vacuum dryer. After drying, low-purity nitrogen (nitrogen purity less than 99% by volume) was introduced to equalize the pressure. The dried pellets for layer A were fed to single-screw extruder A and melted at 310°C. For layer B, PPS resin A and PPS resin B before drying were fed to another vented twin-screw kneading extruder B and melted at 310°C. After high-precision filtration, these two polymers were laminated in a three-layer merging block equipped with a rectangular lamination section, and extruded into a sheet shape from a die with a lip gap of 3 mm and a width of 940 mm, with layer A as the outermost layer and a layer A / layer B / layer A configuration. Next, this sheet was wrapped around a casting drum with a surface temperature of 25°C using an electrostatic casting method, cooled and solidified, and an unstretched film was produced. An intermediate product roll of polyphenylene sulfide film was obtained in the same manner as in Comparative Example 1, except for the above method and those described in the table.

[0069] Example 1 An intermediate product roll of polyphenylene sulfide film was obtained in the same manner as in Comparative Example 1, except that the residence time in extrusion system A was as shown in Table 1.

[0070] Example 2 An intermediate product roll of polyphenylene sulfide film was obtained in the same manner as in Comparative Example 1, except that the film thickness and residence time in extrusion system A were as shown in Table 1.

[0071] Example 3 An intermediate product roll of polyphenylene sulfide film was obtained in the same manner as in Comparative Example 3, except that after the pellets were dried under reduced pressure, nitrogen having a purity of 99% by volume or more was introduced to equalize the pressure, and the oxygen concentration in extrusion system A and the residence time in extrusion system B are shown in Table 1.

[0072] (Summary of Observations) In Comparative Example 1, the long residence time in the extrusion system caused the modification of polyphenylene sulfide, resulting in many defects with a maximum fluorescence intensity wavelength exceeding 450 nm, and a low-quality polyphenylene sulfide film roll with poor film formation stability and flatness was obtained. In addition, the thickness of this roll around the modified site was thin, so that the voltage resistance of the roll when made into a capacitor was low, and the roll could not be used suitably for capacitor applications.

[0073] In Example 1, since the residence time in the extrusion system was short, no modification of polyphenylene sulfide occurred, and a high-quality polyphenylene sulfide film roll was obtained without the defect of a maximum fluorescent intensity wavelength exceeding 450 nm. In Example 2, since the oxygen concentration in the extrusion system was low, the polyphenylene sulfide was not modified, and the defect of the maximum wavelength of the fluorescent intensity exceeding 450 nm was not observed, and a high-quality polyphenylene sulfide film roll was obtained.

[0074] In Comparative Example 2, the high oxygen concentration in the extrusion system caused the modification of polyphenylene sulfide, resulting in a film with many defects in which the fluorescence intensity maximum wavelength exceeded 450 nm and poor flatness. In addition, the thickness of this roll around the modified site was thin, so that the voltage resistance of the roll when made into a capacitor was low, and the roll could not be used suitably for capacitor applications.

[0075] In Comparative Example 3, since the residence time in the extrusion system B was long, the modification of the polyphenylene sulfide progressed, and a low-quality polyphenylene sulfide film roll was obtained with many defects in which the fluorescence intensity maximum wavelength exceeded 450 nm and the flatness was poor.

[0076] In Example 3, since the residence time in the extrusion system B was short, no modification of the polyphenylene sulfide occurred, and a high-quality polyphenylene sulfide film roll was obtained without the defect of a maximum fluorescence intensity wavelength exceeding 450 nm.

[0077] [Table 1]

Claims

1. A polyphenylene sulfide film, characterized in that no maximum wavelength of the fluorescence spectrum is observed in the wavelength region of 450 nm or more within the film plane.

2. The cross section of the film was measured at 4096 points by infrared spectroscopy (ATR method), and the wavelength was 1200 to 1250 cm -1 Peak intensity (IR-p) in the range of 1450 to 1500 cm -1 When the ratio X [(IR-p) / (IR-s)] of peak intensities (IR-s) in the range of 100 to 1500 nm is calculated, the proportion of the polyphenylene sulfide film in which the ratio X is 0.01 or less is 0.5 or more.

3. 3. The polyphenylene sulfide film according to claim 1, wherein the thickness of the film is from 1.0 μm to 500 μm.

4. A polyphenylene sulfide film roll obtained by winding up a polyphenylene sulfide film, which is characterized in that no maximum wavelength of the fluorescence spectrum is observed in the wavelength region of 450 nm or more within the film plane.

5. The cross section of the film was measured at 4096 points by infrared spectroscopy (ATR method), and the wavelength was 1200 to 1250 cm -1 Peak intensity (IR-p) in the range of 1450 to 1500 cm -1 The polyphenylene sulfide film roll is obtained by winding up a polyphenylene sulfide film in which, when the ratio X [(IR-p) / (IR-s)] of peak intensities (IR-s) in the respective ranges is calculated, the proportion of the ratio X being 0.01 or less is 0.5 or more.

6. 6. The polyphenylene sulfide film roll according to claim 4, wherein the thickness of the film is 1.0 μm or more and 500 μm or less.

7. The polyphenylene sulfide film roll according to any one of claims 4 to 6, characterized in that the width of the film roll is 300 mm or more, and the length of the polyphenylene sulfide film wound on the roll is 500 m or more.

8. 8. The polyphenylene sulfide film roll according to claim 4, wherein the orientation angle of the film is 85 degrees or less with respect to a longitudinal direction of the film.

9. The method for producing a polyphenylene sulfide film according to any one of claims 1 to 3, characterized in that it comprises a step of feeding a polyphenylene sulfide resin composition into an extruder, melt-kneading the composition in the extruder, extruding the composition from a die, cooling and solidifying the composition, and stretching the composition at least in the running direction of the film, and the oxygen concentration in the die from the extruder is 1.0 volume % or less.

10. 10. The method for producing a polyphenylene sulfide film according to claim 9, wherein the residence time of the polyphenylene sulfide resin composition from when it is charged into an extruder, when it is melt-kneaded in the extruder, until it is extruded from a die is less than 120 minutes.

11. The method for producing a polyphenylene sulfide film roll according to any one of claims 4 to 8, further comprising a step of feeding a polyphenylene sulfide film resin composition into an extruder, melting and kneading the composition in the extruder, extruding the composition from a die, cooling and solidifying the composition, and then stretching the composition at least in the running direction of the film, and a step of winding up the polyphenylene sulfide film produced by the method in which the oxygen concentration in the die is 1.0 volume % or less from the extruder.

12. 12. The method for producing a polyphenylene sulfide film roll according to claim 11, wherein the residence time of the polyphenylene sulfide resin composition from when it is charged into the extruder and when it is melt-kneaded in the extruder until it is extruded from a die is less than 120 minutes.

Citation Information

Patent Citations

  • Polyphenylene sulfide composition

    JP1994107795A

  • Biaxially oriented polyphenylene sulfide film for releasing and production thereof

    JP2000034356A

  • Polyphenylenesulfide film and film capacitor thereof

    JP2004090551A

  • Production method of optical film

    JP2014159082A

  • Method for producing polyarylene sulfide resin

    JP2018154731A