Aqueous dispersion, method for producing aqueous dispersion, method for producing laminate, and method for producing impregnated woven fabric

The use of a tetrafluoroethylene polymer with carbonyl or hydroxyl groups and anionic surfactants at a pH less than 7 stabilizes the dispersion, addressing instability issues and enhancing the production of high-quality molded articles.

JP7559646B2Active Publication Date: 2024-10-02AGC INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021054728
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-10-02
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Existing aqueous dispersions of tetrafluoroethylene polymers suffer from instability, foaming, settling, and poor uniformity when mixing with other components, leading to impaired physical properties in molded products.

Method used

Aqueous dispersion containing a heat-melting tetrafluoroethylene polymer with carbonyl or hydroxyl groups and an anionic surfactant, such as sulfosuccinates or phosphates, at a pH less than 7, with specific particle sizes and surfactant properties, enhancing dispersion stability and blendability.

Benefits of technology

The solution results in a stable dispersion with improved handling and long-term storage properties, enabling the production of molded articles with excellent physical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide an aqueous dispersion comprising particles of tetrafluoroethylene polymers, having excellent dispersion stability, handleability, blendability and long-term storageability, and a method for producing an aqueous dispersion, a method for producing a laminate, and a method for producing an impregnated woven fabric.SOLUTION: An aqueous dispersion comprises: powder of a hot-melt tetrafluoroethylene polymer having a carbonyl group-containing group or a hydroxy group-containing group; at least one anionic surfactant selected from the group consisting of sulfosuccinic acid ester, phosphoric acid ester and sulfuric acid ester; and water and has a pH of less than 7.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous dispersion containing a powder of a specific tetrafluoroethylene-based polymer, a method for producing the aqueous dispersion, a method for producing a laminate, and a method for producing an impregnated woven fabric. [Background technology]

[0002] Tetrafluoroethylene polymers such as polytetrafluoroethylene (PTFE) are excellent in physical properties such as electrical properties, water and oil repellency, chemical resistance, and heat resistance, and are used in various industrial applications. Dispersions containing tetrafluoroethylene polymer powders are used as coating agents used to impart the above physical properties to the surface of a substrate, and in recent years have also attracted attention as coating agents for forming insulating layers of printed circuit boards compatible with high-frequency band frequencies. On the other hand, tetrafluoroethylene-based polymers generally have low surface tension, and in order to improve the dispersibility of aqueous dispersions containing such powders, Patent Documents 1 and 2 each propose the use of a specific anionic surfactant. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2007 / 026822 [Patent Document 2] International Publication No. 2015 / 008649 Summary of the Invention [Problem to be solved by the invention]

[0004] However, even in the aqueous dispersions described in Patent Documents 1 and 2, the dispersion stability is still insufficient. In particular, the inventors have found that when such an aqueous dispersion itself is prepared, or when such an aqueous dispersion is mixed with other components (inorganic filler, resin varnish, etc.), the liquid properties are easily impaired.

[0005] Specifically, it has been found that when the powder is dispersed in water, foaming and powder settling may occur, resulting in poor handling. In addition, when other components are mixed, not only may it be difficult to mix uniformly, but other additives may also be required to maintain the liquid properties (uniformity, viscosity, thixotropy, etc.) of the resulting mixed liquid. In this case, not only is the preparation complicated, but the physical properties (electrical properties, surface smoothness, etc.) of the molded product formed from the mixed liquid may also be impaired.

[0006] The object of the present invention is to provide an aqueous dispersion containing a tetrafluoroethylene-based polymer powder, which has excellent dispersion stability, handleability, blendability, and long-term storage properties, a method for producing the aqueous dispersion, a method for producing a laminate, and a method for producing an impregnated woven fabric. Molded products based on the tetrafluoroethylene-based polymer and having excellent physical properties can be easily produced from such an aqueous dispersion. [Means for solving the problem]

[0007] The present invention has the following aspects. <1> An aqueous dispersion comprising a powder of a heat-fusible tetrafluoroethylene polymer having a carbonyl group-containing group or a hydroxyl group-containing group, at least one anionic surfactant selected from the group consisting of sulfosuccinate esters, phosphate esters and sulfate esters, and water, and having a pH of less than 7. <2> The tetrafluoroethylene polymer has a carbonyl group-containing group or a hydroxyl group-containing group in a main chain of 1×10 6 Each piece has 10 to 5,000 pieces. <1> An aqueous dispersion of. <3> The average particle size of the powder is 0.1 to 25 μm. <1> or <2> An aqueous dispersion of. <4> The surface tension of the anionic surfactant is 30 mN / m or less. <1> ~ <3> or an aqueous dispersion of any one of the above. <5> The anionic surfactant is a dialkyl sulfosuccinate salt, a polyoxyalkylene alkyl ether phosphate salt, or a polyoxyalkylene alkyl ether sulfate salt. <1> ~ <4> or an aqueous dispersion of any one of the above. <6> The content of the powder is 20% by mass or more. <1> ~ <5> or an aqueous dispersion of any one of the above. <7> 7. The aqueous dispersion according to claim 1, wherein the content of the anionic surfactant is 0.1 to 10% by mass. <8> Further, the composition contains a nonionic surfactant. <1> ~ <7> or an aqueous dispersion of any one of the above. <9> The nonionic surfactant is a polyoxyalkylene-modified polydimethylsiloxane or a glycol monoalkyl ether. <8> An aqueous dispersion of. <10> Further, the composition contains an inorganic filler or a polymer different from the tetrafluoroethylene-based polymer or a precursor thereof. <1> ~ <9> or an aqueous dispersion of any one of the above. <11> The different polymer is non-thermofusible polytetrafluoroethylene; <10> An aqueous dispersion of. <12> The pH is 4 to 6. <1> ~ <11> or an aqueous dispersion of any one of the above. <13> <1> ~ <12> 13. A method for producing any one of the aqueous dispersions described above, comprising mixing the powder with an aqueous solution containing the anionic surfactant. <14> <1> ~ <12> a method for producing a laminate, comprising: applying any one of the aqueous dispersions described above to a surface of a substrate, and heating the resulting mixture to form a polymer layer containing the tetrafluoroethylene-based polymer, thereby obtaining a laminate having a substrate layer constituted by the substrate and the polymer layer. <15> <1> ~ <12> and heating the aqueous dispersion of any one of the above to obtain an impregnated woven fabric comprising the tetrafluoroethylene-based polymer. Effect of the Invention

[0008] According to the present invention, an aqueous dispersion containing a tetrafluoroethylene-based polymer powder, which has excellent dispersion stability, handling properties, blendability, and long-term storage properties, and has a pH of less than 7, can be obtained. From the aqueous dispersion of the present invention, a molded product having excellent physical properties based on the tetrafluoroethylene-based polymer can be obtained. In addition, such an aqueous dispersion can be suitably used for coating a substrate having low base resistance and for impregnating a woven fabric having low base resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following terms have the following meanings. "Average particle size (D50)" is the cumulative 50% diameter on a volume basis of the target object (powders and fillers) determined by laser diffraction / scattering. In other words, the particle size distribution is measured by laser diffraction / scattering, the total volume of the target object group is set as 100%, and a cumulative curve is calculated. The average particle size (D50) is the particle size at the point on the cumulative curve where the cumulative volume is 50%. "Melting temperature" is the temperature corresponding to the maximum of the melting peak of a polymer as measured by differential scanning calorimetry (DSC). "Glass transition temperature (Tg)" is a value measured by analyzing a polymer, a cured product, or an elastomer using a dynamic mechanical analysis (DMA) method. The "viscosity of the aqueous dispersion" is the viscosity measured using a Brookfield viscometer at 25° C. and 60 rpm. The measurement is repeated three times, and the average value of the three measured values ​​is used. The "thixotropy ratio of an aqueous dispersion" is a value calculated by dividing the viscosity measured at a rotation speed of 30 rpm by the viscosity measured at a rotation speed of 60 rpm. Each viscosity measurement is repeated three times, and the average value of the three measured values ​​is used. The "specific surface area of ​​a powder" is a value calculated by measuring a powder using a gas adsorption (constant volume method) BET multipoint method, and is determined using a NOVA4200e (manufactured by Quantachrome Instruments). The term "unit" in a polymer means an atomic group based on the monomer formed by polymerization of the monomer. The unit may be a unit formed directly by a polymerization reaction, or may be a unit in which a part of the unit is converted into a different structure by treating the polymer. Hereinafter, a unit based on monomer a is also referred to simply as a "monomer a unit."

[0010] The aqueous dispersion of the present invention (hereinafter also referred to as "the present dispersion") contains a powder (hereinafter also referred to as "F powder") of a heat-fusible tetrafluoroethylene polymer (hereinafter also referred to as "F polymer") having a carbonyl group-containing group or a hydroxyl group-containing group, at least one anionic surfactant (hereinafter also referred to as "the present surfactant") selected from the group consisting of sulfosuccinate esters, phosphate esters, and sulfate esters, and water. The pH of the present dispersion is less than 7, and the F powder is dispersed in the form of particles in the present dispersion. This dispersion has excellent dispersion stability, handling properties, blendability, and long-term storage properties. From this dispersion, molded products based on tetrafluoroethylene polymers with excellent physical properties can be obtained. The reason for this is not entirely clear, but is thought to be as follows.

[0011] In the present invention, the F polymer has a carbonyl group-containing group or a hydroxyl group-containing group, which is a polar functional group, and the surfactant has a specific acid ester group, which is a polar functional group. The F polymer and the surfactant, both of which have specific polar functional groups, tend to have high interaction in liquid. In addition, a pH of less than 7 balances the degree of ionization of the surfactant and enhances the interaction between the surfactant and the F polymer. It is believed that these factors promote the adhesion of the surfactant to the surface of the F powder and the formation of stable micelles between the F powder and the surfactant. As a result, it is believed that an aqueous dispersion of a tetrafluoroethylene-based polymer with excellent handling properties, blendability, and long-term storage properties was obtained.

[0012] The F polymer in the present invention is a heat-fusible polymer containing units (TFE units) based on tetrafluoroethylene (TFE) having a carbonyl group-containing group or a hydroxyl group-containing group. The melting temperature of the F polymer is preferably 180° C. or higher, more preferably 200° C. or higher, and even more preferably 260° C. or higher. The melting temperature of the F polymer is preferably 325° C. or lower, and more preferably 320° C. or lower. The melting temperature of the F polymer is particularly preferably 260 to 320° C. The glass transition point of the F polymer is preferably 50° C. or higher, more preferably 75° C. or higher. The glass transition point of the F polymer is preferably 150° C. or lower, more preferably 125° C. or lower.

[0013] The surface tension of the F polymer is preferably 16 to 26 mN / m, more preferably 16 to 20 mN / m. The surface tension of the F polymer can be measured by placing a droplet of a wettability index reagent (manufactured by Wako Pure Chemical Industries, Ltd.) on a flat plate made of the F polymer. The fluorine content of the F polymer is preferably 70% by mass or more, more preferably 72 to 76% by mass. Although F polymers, which have low surface tension and high fluorine content, have excellent electrical properties and other physical properties, they have extremely low dispersion stability in water. However, in the present dispersion, the dispersion stability of such F polymers is easily improved due to the above-mentioned mechanism of action.

[0014] F polymer includes the low molecular weight polymer (low molecular weight PTFE) that consists of only TFE unit, the polymer that contains TFE unit and unit based on ethylene, the polymer that contains TFE unit and unit based on propylene, the polymer that contains TFE unit and unit based on perfluoro(alkyl vinyl ether) (PAVE) (PAVE unit) (PFA), the polymer that contains TFE unit and unit based on hexafluoropropylene (FEP), the polymer that contains TFE unit and unit based on fluoroalkylethylene, the polymer that contains TFE unit and unit based on chlorotrifluoroethylene, and PFA or FEP are preferred, and PFA is more preferred.The above-mentioned polymer may further contain unit based on other comonomer. As for PAVE, CF2 =CFOCF 3 , C.F. 2 =CFOCF 2 CF 3 or CF 2 =CFOCF 2 CF 2 CF 3 (hereinafter also referred to as "PPVE") is preferred, with PPVE being more preferred.

[0015] The number average molecular weight of the low molecular weight PTFE is preferably 10,000 to 200,000. In this case, the PTFE has thermal melting properties. The number average molecular weight of the low molecular weight PTFE is a value calculated based on the following formula (1). Mn = 2.1 × 10 10 ×ΔHc -5.16 ... (1) In formula (1), Mn represents the number average molecular weight of the low molecular weight PTFE, and ΔHc represents the heat of crystallization (cal / g) of the low molecular weight PTFE measured by differential scanning calorimetry. The low molecular weight PTFE may contain a small amount of units other than the TFE unit.

[0016] The F polymer has a carbonyl group-containing group or a hydroxyl group-containing group. In this case, due to the above-mentioned mechanism of action, the dispersion has excellent physical properties such as dispersion stability. The hydroxyl group-containing group is preferably a group containing an alcoholic hydroxyl group, and -CF 2 CH 2 OH or -C(CF 3 ) 2 OH is more preferred. The carbonyl-containing group is a group that contains a carbonyl group (>C(O)), and includes a carboxyl group, an alkoxycarbonyl group, an amide group, an isocyanate group, a carbamate group (-OC(O)NH 2 ), acid anhydride residue (-C(O)OC(O)-), imide residue (-C(O)NHC(O)-, etc.) or carbonate group (-OC(O)O-), and acid anhydride residue is more preferred. In this case, F powder and the present surfactant tend to interact with each other, and the present dispersion is likely to have excellent liquid physical properties such as dispersion stability.

[0017] The F polymer is preferably a polymer having a carbonyl group-containing group including TFE units and PAVE units, more preferably a polymer containing units based on a monomer having a TFE unit, a PAVE unit and a carbonyl group-containing group, and even more preferably a polymer containing these units in the order of 90 to 99 mol%, 0.5 to 9.97 mol%, and 0.01 to 3 mol% relative to the total units. The presence of a carbonyl group-containing group is preferable from the viewpoint of further improving affinity and adhesion. When the F polymer has a carbonyl group-containing group, the number of carbonyl group-containing groups in the F polymer is 1×10 6 The number of carbonyl-containing groups per unit is preferably 10 to 5000, more preferably 100 to 3000, and further preferably 800 to 1500. The number of carbonyl-containing groups in the F polymer can be quantified by the composition of the polymer or the method described in WO 2020 / 145133. In addition, the monomer having a carbonyl group-containing group is preferably itaconic anhydride, citraconic anhydride, or 5-norbornene-2,3-dicarboxylic anhydride (hereinafter also referred to as "NAH"). Specific examples of such polymers include the polymers described in WO 2018 / 16644.

[0018] The D50 of the F powder in the present invention is preferably 0.1 to 25 μm. The D50 of the F powder is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 8 μm or less. The D50 of the F powder is preferably 0.01 μm or more, more preferably 0.1 μm or more, and even more preferably 0.3 μm or more. With a D50 in this range, the fluidity and dispersion stability of the F powder tend to be good. From the viewpoint of dispersion stability, the specific surface area of ​​F powder is 1 to 25 m 2 / g is preferable, and 1 to 8m 2 / g is more preferable, and 1 to 3m 2 / g is more preferred. The F powder may be used alone or in combination of two or more kinds.

[0019] The F powder may contain a resin other than the F polymer or an inorganic filler, but preferably contains the F polymer as the main component. The content of the F polymer in the F powder is preferably 80% by mass or more, more preferably 100% by mass. Examples of resins other than the F polymer include heat-resistant resins such as aromatic polyester, polyamideimide, (thermoplastic) polyimide, polyphenylene ether, polyphenylene oxide, and maleimide. Examples of inorganic fillers include silicon oxide (silica), metal oxides (beryllium oxide, cerium oxide, alumina, soda alumina, magnesium oxide, zinc oxide, titanium oxide, etc.), boron nitride, and magnesium metasilicate (steatite). At least a part of the surface of the inorganic filler may be surface-treated.

[0020] The F powder containing a resin other than the F polymer or an inorganic filler may have a core-shell structure having an F polymer as the core and a resin other than the F polymer or an inorganic filler as the shell, or may have a core-shell structure having an F polymer as the shell and a resin other than the F polymer or an inorganic filler as the core. Such an F powder can be obtained, for example, by bonding (collision, aggregation, etc.) a powder of an F polymer and a powder of a resin other than the F polymer or an inorganic filler. The content of F powder in the present dispersion is preferably 20% by mass or more, more preferably 30% by mass or more, based on the total mass of the present dispersion. The content of F powder is preferably 80% by mass or less, more preferably 70% by mass or less, based on the total mass of the present dispersion.

[0021] The present surfactant is at least one anionic surfactant selected from the group consisting of sulfosuccinates, phosphates, and sulfates, and has a sulfo group, a phosphate group, or an anionic group thereof (sulfonate group, phosphonate group) as an anionic hydrophilic group, and a hydrophobic group. The molecular weight of the present surfactant is preferably at least 400, more preferably at least 600. The molecular weight of the present surfactant is preferably at most 5,000, more preferably at most 1,500. The surface tension of the present surfactant is preferably 30 mN / m or less, more preferably 15 mN / m or more, and even more preferably 20 mN / m or more. The surfactant may be partially or completely ionized in the dispersion.

[0022] When the surfactant has a pKa, the pKa in water is preferably 4 or less. When the surfactant undergoes multi-stage ionization, the lowest pKa value may be 4 or less. The pKa of the surfactant is preferably -3 or more. The counter cation of the anionic group in the surfactant is preferably an alkali metal ion, an alkaline earth metal ion, or an ammonium cation, more preferably a sodium ion.The surfactant is preferably an alkali metal salt, an alkaline earth metal salt, or an ammonium salt, more preferably a sodium salt. In these cases, the surfactant and the F powder tend to interact with each other, and the dispersion tends to have excellent liquid physical properties such as dispersion stability.

[0023] The hydrophobic group in the present surfactant is preferably an alkyl group, an aryl group or a polyoxyalkylene group. The hydrophobic group may include an alkyl group and a polyoxyalkylene group to form a polyoxyalkylene alkyl ether chain. The alkyl group may be linear, branched, or may have a cyclic structure, and is preferably branched. The number of carbon atoms in the alkyl group is preferably 1 to 30, more preferably 5 to 20, and further preferably 7 to 15. The aryl group is preferably an aryl group having an alkyl group having 6 to 12 carbon atoms as a substituent.

[0024] The oxyalkylene group in the polyoxyalkylene group includes an oxyethylene group and an oxypropylene group, and is preferably an oxyethylene group. The polyoxyalkylene group may be composed of only one type of oxyalkylene group, or may be composed of two or more types of oxyalkylene groups. In the latter case, the different types of oxyalkylene groups may be linked randomly or in a block shape. The degree of polymerization of the oxyalkylene group in the polyoxyalkylene group (the number of repeating units of the oxyalkylene group) is preferably at least 1, and more preferably at least 2. The degree of polymerization is preferably 100 or less, and more preferably 50 or less.

[0025] The hydrophobic group in the sulfosuccinate is preferably an alkyl group. In other words, the sulfosuccinate is preferably an alkyl sulfosuccinate, an alkyl diester sulfosuccinate, or a salt thereof, more preferably an alkyl diester sulfosuccinate salt. A preferred example of the sulfosuccinic acid alkyl diester salt is a compound represented by the formula: 11 OOC-CH 2 -CH(SO 3 - Na + )COOR 12 In the formula, R 11 , R 12 each independently represents an alkyl group. The alkyl group preferably has 1 to 30 carbon atoms, more preferably 5 to 20 carbon atoms, and further preferably 7 to 15 carbon atoms.

[0026] The hydrophobic group in the phosphate ester or sulfate ester preferably has a polyoxyalkylene alkyl ether chain. In other words, the phosphate ester or sulfate ester is preferably a polyoxyalkylene alkyl ether phosphate ester, a polyoxyalkylene alkyl ether sulfate ester, or a salt thereof, more preferably a polyoxyalkylene alkyl ether phosphate ester salt and a polyoxyalkylene alkyl ether sulfate ester salt. In these cases, the oxyalkylene group is preferably an oxyethylene group.

[0027] Suitable examples of the polyoxyalkylene alkyl ether phosphate ester salt and the polyoxyalkylene alkyl ether sulfate ester salt include those represented by the formula: 21 O(CH 2 CH 2 O) n -XNa + In the formula, R 21 represents a hydrogen atom or an alkyl group. The number of carbon atoms in such an alkyl group is preferably 3 to 20, and more preferably 5 to 15. In the formula, n is 0 to 100, preferably 1 to 50, and more preferably 2 to 30. In the formula, X represents a sulfonate group or a phosphonate group.

[0028] Specific examples of this surfactant include "Emulzogen SB10" (Clariant), "Polyrol TR / LNA" (Cesalpinia), "Sunmorin OT-70" (Sanyo Chemical Industries, Ltd.), "Newcol N-291-M", "Newcol 1305-SN", and "Anthox EHD-PNA" (all manufactured by Nippon Nyukazai Co., Ltd.), "Cosmacol AES-27-3-24NE" (Sasol), "Phosphanol RS-710", and "Phosphanol RS-610" (all manufactured by Toyo Chemical Industry Co., Ltd.).

[0029] The content of the present surfactant in the present dispersion is preferably 0.1% by mass or more, more preferably 1% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less. The water content in the present dispersion is preferably 40% by mass or more, more preferably 50% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less. Within this range, the liquid properties such as the dispersion stability of the present dispersion are more likely to be improved.

[0030] The dispersion may further contain a water-soluble dispersion medium other than water as a dispersion medium. As such a water-soluble dispersion medium, a water-soluble compound that is liquid at 25° C. and classified as polar under atmospheric pressure is preferable, and examples thereof include N,N-dimethylformamide, N,N-dimethylacetamide, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, and N-methyl-2-pyrrolidone.

[0031] The present dispersion may further contain a polymer different from the F polymer or a precursor thereof from the viewpoint of improving the adhesiveness, electrical properties and low linear expansion of a molded article formed from the present dispersion. The different polymer may be thermosetting or thermoplastic, or may be modified. The different polymer may be dissolved in the present dispersion, or may be dispersed without being dissolved.

[0032] Examples of the different polymers include acrylic resins, phenolic resins, liquid crystalline polyesters, liquid crystalline polyesteramides, polyolefin resins, modified polyphenylene ethers, polyfunctional cyanate ester resins, polyfunctional maleimide-cyanate ester resins, polyfunctional maleimides, aromatic elastomers such as styrene elastomers, vinyl ester resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, melamine-urea co-condensation resins, polycarbonates, polyarylates, polysulfones, polyarylsulfones, aromatic polyamides, aromatic polyether amides, polyphenylene sulfide, polyaryl ether ketones, polyphenylene ethers, epoxy resins, and fluoropolymers other than F polymers.

[0033] When the present dispersion further contains a different polymer, the content thereof is preferably 40% by mass or less based on the total mass of the present dispersion. Examples of fluoropolymers other than the F polymer include non-thermofusible fluoropolymers and thermoplastic tetrafluoroethylene polymers having no carbonyl group-containing groups and no hydroxyl group-containing groups. A specific example of the former is non-thermofusible PTFE, and a specific example of the latter is PFA and FEP which have no carbonyl-containing group or hydroxyl-containing group.

[0034] The present dispersion preferably further contains a non-thermofusible PTFE powder (hereinafter also referred to as "PTFE powder"). Because the present dispersion has excellent dispersion stability and blendability due to the above-mentioned mechanism of action, it is likely to have excellent liquid physical properties even when it further contains a PTFE powder with low surface tension and low dispersion stability. The PTFE powder preferably has a D50 of 0.1 to 1 μm. In this case, the melting temperature of the F polymer is preferably 200 to 320° C., and the F powder preferably has a D50 of 1 to 4 μm.

[0035] The proportion of F powder in the total of F powder and PTFE powder in the present dispersion is preferably 25% by mass or less, more preferably 15% by mass or less. The proportion of F powder is preferably 0.1% by mass or more, more preferably 1% by mass or more. Such a present dispersion is not only likely to have excellent dispersion stability, handling properties, and long-term storage stability, but also likely to form an adhesive molded product with excellent physical properties based on PTFE.

[0036] In addition, a preferred embodiment of the different polymer is an aromatic polymer. The aromatic polymer is preferably polyphenylene ether or an aromatic elastomer (styrene elastomer, etc.). In this case, not only is the adhesiveness and low linear expansion of the molded product formed from the present dispersion further improved, but the liquid properties (viscosity, thixotropy ratio, etc.) of the present dispersion are well balanced, and therefore the handling property is easily improved. Here, examples of the styrene elastomer include copolymers of styrene and conjugated dienes or (meth)acrylic esters (styrene-butadiene rubber, styrene-based core-shell type copolymers, styrene-based block copolymers, etc.), and preferred are styrene elastomers that have the properties of both rubber and plastic and become plasticized by heating to exhibit flexibility.

[0037] The present dispersion may further contain an inorganic filler. In this case, the molded product formed from the present dispersion is likely to have excellent electrical properties and low linear expansion. In addition, even if the present dispersion contains an inorganic filler, the above-mentioned mechanism of action makes it possible to obtain a molded product based on the F polymer and having excellent physical properties. Therefore, the present dispersion containing an inorganic filler is likely to produce a molded product having high physical properties of the F polymer and the inorganic filler.

[0038] The inorganic filler is preferably a nitride filler or an inorganic oxide filler, more preferably a boron nitride filler, a beryllia filler (a beryllium oxide filler), a silicate filler (a silica filler, a wollastonite filler, a talc filler), or a metal oxide (such as cerium oxide, aluminum oxide, magnesium oxide, zinc oxide, or titanium oxide) filler, and even more preferably a silica filler. It is preferable that at least a portion of the surface of the inorganic filler is surface-treated with a silane coupling agent (3-aminopropyltriethoxysilane, vinyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-isocyanatopropyltriethoxysilane, etc.).

[0039] The inorganic filler preferably has a D50 of 20 μm or less, more preferably 10 μm or less, and more preferably has a D50 of 0.01 μm or more, more preferably 0.1 μm or more. The shape of the inorganic filler may be any of granular, needle-like (fibrous) and plate-like. Specific shapes of the inorganic filler include spherical, scale-like, layered, leaf-like, apricot kernel-like, columnar, cockscomb-like, equiaxial, leaf-like, micaceous, block-like, flat, wedge-like, rosette-like, net-like and prismatic shapes. The inorganic filler may be used alone or in combination of two or more kinds. When the present dispersion further contains an inorganic filler, the amount thereof is preferably 1 to 50 mass %, more preferably 5 to 40 mass %, based on the total mass of the present dispersion.

[0040] Specific examples of suitable inorganic fillers include silica fillers (such as the "Admafine (registered trademark)" series manufactured by Admatechs Co., Ltd.), zinc oxide surface-treated with an ester such as propylene glycol dicaprylate (such as the "FINEX (registered trademark)" series manufactured by Sakai Chemical Industry Co., Ltd.), spherical fused silica (such as the "SFP (registered trademark)" series manufactured by Denka Co., Ltd.), titanium oxide coated with polyhydric alcohol and inorganic substances (such as the "Tipaque (registered trademark)" series manufactured by Ishihara Sangyo Kaisha, Ltd.), and rutile-type titanium oxide surface-treated with alkylsilane (such as the "Tipaque (registered trademark)" series manufactured by Teika Co., Ltd.). JMT (registered trademark) series, etc.), hollow silica filler (Taiheiyo Cement Corporation's E-SPHERES series, Nippon Steel Mining Co., Ltd.'s Silinax series, Emerson & Cumming Co., Ltd.'s Ecocosfyer series, etc.), talc filler (Nippon Talc Co., Ltd.'s SG series, etc.), steatite filler (Nippon Talc Co., Ltd.'s BST series, etc.), boron nitride filler (Showa Denko KK's UHP series, Denka Company, Ltd.'s Denka Boron Nitride series (GP, HGP grades, etc.), etc.).

[0041] The present dispersion preferably further contains a nonionic surfactant, which tends to further improve the dispersion stability during long-term storage of the present dispersion. When the present dispersion contains a nonionic surfactant, the content of the nonionic surfactant in the present dispersion is preferably 0.1 to 15 mass %, more preferably 1 to 10 mass %, and in this case, the ratio of the content of the present surfactant to the content of the other surfactant in the present dispersion is preferably 0.1 to 10.

[0042] As the nonionic surfactant, ether type surfactants, ester ether type surfactants and silicone surfactants are preferred, glycol monoalkyl ethers, glycol monoaryl ethers, glycol monoalkyl ether acetates, glycol monoaryl ether acetates and polyoxyalkylene-modified polydimethylsiloxanes are more preferred, and glycol monoalkyl ethers and polyoxyalkylene-modified polydimethylsiloxanes are even more preferred.

[0043] The glycol monoalkyl ether is preferably a polyoxyethylene glycol monoalkyl ether. The oxyethylene unit (-OCH 2 CH 2 The number of --) is preferably 1 to 10, and the monoalkyl ether group is preferably highly branched.

[0044] Specific examples of glycol monoalkyl ethers include polyethylene glycol decyl ether, polyethylene glycol undecyl ether, polyethylene glycol dodecyl ether, polyethylene glycol tridecyl ether, polyethylene glycol tetradecyl ether, triethylene glycol monomethyl ether, polyethylene glycol trimethylnonyl ether, ethylene glycol mono-2-ethylhexyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, dipropylene glycol monobutyl ether, triethylene glycol monomethyl ether, tripropylene glycol monobutyl ether, propylene glycol monophenyl ether, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate.

[0045] Specific preferred examples of glycol monoalkyl ethers include the "Tergitol" series (manufactured by The Dow Chemical Company, such as "Tergitol TMN-100X"), "Lutensol T08", "Lutensol XL70", "Lutensol XL80", "Lutensol XL90", "Lutensol XP80", and "Lutensol M5" (all manufactured by BASF), "Newcol 1308FA" and "Newcol 1310" (all manufactured by Nippon Nyukazai Co., Ltd.), "Leocol TDN-90-80", and "Leocol SC-90" (all manufactured by Lion Specialty Chemicals).

[0046] The polyoxyalkylene-modified polydimethylsiloxane is an organopolysiloxane having a polyoxyalkylene structure as a hydrophilic group and a polydimethylsiloxane structure as a hydrophobic group, and is preferably a linear polymer. The average molecular weight of the polyoxyalkylene-modified dimethylsiloxane is preferably 100-3,000, and more preferably 500-2,000. The polyoxyalkylene-modified polydimethylsiloxane is preferably a polyoxyalkylene-modified polydimethylsiloxane containing dimethylsiloxane units in the main chain and having oxyalkylene groups in the side chain, or a polyoxyalkylene-modified polydimethylsiloxane containing dimethylsiloxane units in the main chain and having oxyalkylene groups at the main chain terminals.

[0047] The former polyoxyalkylene-modified polydimethylsiloxane is represented by the formula: -(R 1 )(R 2 )SiO 2 / 2 It is preferred that the diorganosiloxane contains diorganosiloxane units represented by the formula: R in the formula 1 represents an alkyl group, preferably a methyl group. R in the formula 2 represents a group having a polyoxyalkylene group, and is represented by the formula: -X 2 -O-(Y 2 ) n -Z 2 (wherein, X 2 represents an alkylene group, Y 2 represents a polyoxyalkylene group, Z 2 represents a hydrogen atom, an alkyl group or an acyl group, and n represents an integer of 2 to 100. X 2 Examples of the alkyl group include an ethylene group, a propylene group, and a butylene group. Y 2 Examples of the oxyalkyl group include an oxyethylene group and an oxypropylene group. Z 2 The alkyl group or acyl group in the formula (I) includes a methyl group and an acetyl group.

[0048] The oxyalkylene group contained in the polyoxyalkylene-modified dimethylsiloxane may be composed of only one type of oxyalkylene group, or may be composed of two or more types of oxyalkylene groups. In the latter case, the different types of oxyalkylene groups may be linked randomly or in blocks. In the polyoxyalkylene-modified polydimethylsiloxane, the degree of polymerization of the oxyalkylene group (the number of repeating units of the oxyalkylene group) is preferably at least 2. The degree of polymerization is preferably 100 or less, more preferably 50 or less, and even more preferably 20 or less.

[0049] The degree of polymerization of dimethylsiloxane in the polyoxyalkylene-modified polydimethylsiloxane (the number of repeating dimethylsiloxane units) is preferably from 2 to 100, more preferably from 2 to 25. In this case, the dispersion tends to be excellent in dispersion stability, handleability, and long-term storage stability. Specific examples of polyoxyalkylene-modified polydimethylsiloxanes include "BYK-347", "BYK-349", "BYK-378", "BYK-3450", "BYK-3451", "BYK-3455", "BYK-3456" (manufactured by BYK Japan), "KF-6011", and "KF-6043".

[0050] The dispersion may further contain a pH adjuster to adjust the pH, such as an amine, ammonia, or citric acid. The dispersion may further contain a pH buffer to stabilize the pH, such as tris(hydroxymethyl)aminomethane, ethylenediaminetetraacetic acid, ammonium hydrogen carbonate, ammonium carbonate, or ammonium acetate. In addition to the above-mentioned components, the present dispersion may further contain other components such as a thixotropy imparting agent, a viscosity adjusting agent, an antifoaming agent, a silane coupling agent, a dehydrating agent, a plasticizer, a weathering agent, an antioxidant, a heat stabilizer, a lubricant, an antistatic agent, a brightening agent, a colorant, a conductive agent, a release agent, a surface treatment agent, a flame retardant, an antiseptic, an antifungal agent, and various fillers, provided that the effects of the present invention are not impaired.

[0051] The viscosity of the present dispersion is preferably 10 mPa·s or more, more preferably 30 mPa·s or more, and even more preferably 50 mPa·s or more. The viscosity of the present dispersion is preferably 10,000 mPa·s or less, more preferably 1,000 mPa·s or less, and even more preferably 800 mPa·s or less. In this case, the present dispersion is likely to have excellent liquid properties such as dispersion stability and excellent coatability. The thixotropy ratio of the present dispersion is preferably 1.0 or more. The thixotropy ratio of the present dispersion is preferably 3.0 or less, more preferably 2.0 or less. In this case, the present dispersion has excellent coatability and homogeneity, and is likely to form a denser molded product (polymer layer, etc.). The pH of the present dispersion is less than 7, and more preferably from 4 to 6. In this case, due to the above-mentioned mechanism of action, the present dispersion tends to have excellent liquid physical properties such as dispersion stability.

[0052] The dispersion layer ratio of the present dispersion is preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more. Since the present dispersion has excellent dispersion stability, the dispersion layer ratio is likely to be in the above range. Here, the dispersion layer ratio is a value calculated by the following formula from the height of the entire dispersion in the screw tube and the height of the sedimentation layer (dispersion layer) before and after standing when the present dispersion (18 mL) is placed in a screw tube (internal volume: 30 mL) and left to stand at 25° C. for 14 days. If no sedimentation layer is observed after standing and there is no change in the state, it is considered that there is no change in the height of the entire dispersion, and the dispersion layer ratio is 100%. Dispersion layer rate (%) = (height of sedimentation layer) / (total height of dispersion liquid) x 100

[0053] Due to the above-mentioned mechanism of action, the present dispersion has excellent dispersion stability, particularly long-term storage stability. In the present dispersion, the pH fluctuation range (absolute value) after storage at 25° C. for 30 days is preferably 1 or less, more preferably 0.5 or less. Furthermore, the viscosity of the present dispersion after storage for 30 days at 25° C. is preferably 500 mPa s or less, and more preferably 100 mPa s or less. If sedimentation is observed in the present dispersion after the storage, this viscosity refers to the viscosity measured after redispersion. In the present dispersion, the fluctuation range (absolute value) of the thixotropy ratio after storage at 25° C. for 30 days is preferably 3 or less, and more preferably less than 1.

[0054] The present dispersion can be produced by mixing F powder, the present surfactant, and water, and adjusting the pH as necessary. Examples of mixing methods include a method of adding F powder and the present surfactant to water all at once and mixing; a method of mixing F powder with an aqueous solution containing the present surfactant; a method of premixing F powder and water, and premixing the present surfactant and water, respectively, and further mixing the two mixtures obtained; and the like. The method of mixing F powder with an aqueous solution containing the present surfactant is preferred. In this case, the surface of the F powder is easily covered with the present surfactant, and the present dispersion is easily excellent in liquid physical properties such as dispersion stability.

[0055] The mixing method for preparing the present dispersion may be either a batch method or a continuous method. Examples of equipment used for mixing include stirring devices equipped with uniaxial or multiaxial blades (stirring impellers) such as propeller blades, turbine blades, paddle blades, and shell-shaped blades, as well as stirring using a Henschel mixer, pressure kneader, Banbury mixer, or planetary mixer; mixing using a disperser that uses media such as a ball mill, attritor, basket mill, sand mill, sand grinder, Dyno Mill (a bead mill using grinding media such as glass beads or zirconium oxide beads), Dispermat, SC mill, spike mill, or agitator mill; and mixing using a disperser that does not use media, such as high-pressure homogenizers such as a Microfluidizer, Nanomizer, or Ultimizer, ultrasonic homogenizer, Dissolver, Disper, or high-speed impeller disperser.

[0056] Among them, the device used for mixing is preferably a Henschel mixer, a pressure kneader, a Banbury mixer or a planetary mixer, and more preferably a planetary mixer. A planetary mixer has two agitating blades that rotate and revolve around each other, and is designed to agitate and mix the mixture in the mixing vessel. Therefore, there is little dead space in the mixing vessel where the agitating blades do not reach, reducing the load on the blades and allowing the contents to be mixed to a high degree. When the dispersion further contains optional additives such as inorganic fillers, different polymers, nonionic surfactants, other liquid components, etc., these can be mixed at any stage. The mixing method and mixing device can be the same as those described above.

[0057] This dispersion can be used for applications such as impregnating and drying an insulating layer for a printed wiring board, a thermal interface material, a substrate for a power module, or a coil used in a power device such as a motor to form a heat conductive heat resistant coating layer, bonding ceramic parts or metal parts together in an in-vehicle engine, imparting corrosion resistance to a heat exchanger or a fin or tube constituting the heat exchanger, and coating the inside and outside of a glass container. It is particularly suitable for coating to impart impact resistance. Examples of glass containers include vials, syringes, needle syringes, cartridge type syringes, and ampoules.

[0058] In addition, the present dispersion can be used as an electrode binder material, a separator coating material, and an electrode (positive electrode, negative electrode) coating material used in electrochemical devices equipped with electrodes, such as secondary batteries such as lithium ion batteries, primary batteries such as lithium batteries, radical batteries, solar cells (particularly dye-sensitized solar cells), fuel cells, lithium ion capacitors, hybrid capacitors, capacitors (electric double layer capacitors, etc.), various capacitors (aluminum electrolytic capacitors, tantalum electrolytic capacitors, etc.), electrochromic elements, electrochemical switching elements, and various electrochemical sensors.

[0059] The dispersions further containing conductive fillers can also be used in applications requiring electrical conductivity, such as in the field of printed electronics, for example in the manufacture of energized elements in printed circuit boards, sensor electrodes, displays, backplanes, RFID (radio frequency identification), photovoltaics, lighting, disposable electronics, automotive heaters, electromagnetic interference (EMI) shielding, membrane switches, etc.

[0060] In addition, the fired product obtained from the present dispersion can be used as an adhesive for bonding electronic components such as IC chips, resistors, and capacitors mounted on semiconductor elements, high-density substrates, and module components, bonding a circuit substrate to a heat sink, and bonding an LED chip to a substrate. Furthermore, the fired product can be used as a conductive bonding material (a substitute for solder bonding) between circuit wiring and electronic components in the mounting process of electronic components. It can also be used as an adhesive between ceramic parts and metal parts in an in-vehicle engine. The fired product can also be used for the applications described in paragraph number

[0149] of International Publication WO 2016 / 017801.

[0061] This dispersion has excellent dispersion stability and long-term storage stability, and can form molded products based on the F polymer with excellent physical properties. In addition, molded products that exhibit strong adhesion to substrates can be formed. The method for producing the laminate of the present invention is a method for obtaining a laminate having a substrate layer composed of a substrate and an F layer by applying the present dispersion to the surface of a substrate and heating the substrate to form a polymer layer containing an F polymer (hereinafter, also referred to as an "F layer"). This dispersion is applied to the surface of a substrate to form a liquid coating, which is then heated to remove the dispersion medium to form a dry coating, and the dry coating is further heated to bake the F polymer, thereby obtaining a laminate having an F layer on the surface of a substrate layer composed of a substrate.

[0062] The substrate may be a metal substrate (metal foil of copper, nickel, aluminum, titanium, or an alloy thereof), a heat-resistant resin film (polyimide, polyarylate, polysulfone, polyarylsulfone, polyamide, polyetheramide, polyphenylene sulfide, polyaryletherketone, polyamideimide, liquid crystalline polyester, liquid crystalline polyesteramide, etc.), Examples of the heat-resistant resin include a film containing one or more types of heat-resistant resin such as a tetrafluoroethylene-based polymer, and may be a single-layer film or a multi-layer film), a prepreg (a precursor of a fiber-reinforced resin substrate), and glass. The shape of the substrate may be flat, curved or uneven, and may further be any of foil, plate, film and fiber.

[0063] The present dispersion has a pH of less than 7 and can therefore be suitably used for coating substrates with poor base resistance. Substrates with poor base resistance include substrates that have been surface-treated with a surface treatment agent that is hydrolyzed in a base. The method for applying the present dispersion to the surface of the substrate may be any method that forms a stable liquid coating (wet film) of the present dispersion on the surface of the substrate, and includes coating, droplet ejection, and immersion methods, with the coating method being preferred. The coating method allows the liquid coating to be efficiently formed on the surface of the substrate with simple equipment. Examples of the coating method include spraying, roll coating, spin coating, gravure coating, microgravure coating, gravure offset, knife coating, kiss coating, bar coating, die coating, fountain-meyer bar, and slot die coating.

[0064] When drying the liquid coating, the liquid coating is heated to a temperature at which the dispersion medium (water) volatilizes, and a dry coating is formed on the surface of the substrate. The heating temperature in such drying is preferably 100° C. to 200° C. Air may be blown in the process of removing the dispersion medium. During drying, the dispersion medium does not necessarily have to be completely evaporated, but it is sufficient to evaporate it to an extent that the layer shape after holding is stable and a free-standing film can be maintained. When baking the F polymer, it is preferable to heat the dried coating to a temperature equal to or higher than the melting temperature of the F polymer, and the heating temperature is preferably 380° C. or lower, more preferably 350° C. or lower.

[0065] Examples of the heating method include a method using an oven, a method using a ventilated drying furnace, and a method using heat rays such as infrared rays. The heating may be carried out either under normal pressure or under reduced pressure. The heating atmosphere may be any of an oxidizing gas atmosphere (oxygen gas, etc.), a reducing gas atmosphere (hydrogen gas, etc.), and an inert gas atmosphere (helium gas, neon gas, argon gas, nitrogen gas, etc.). The heating time is preferably from 0.1 to 30 minutes, more preferably from 0.5 to 20 minutes. By carrying out heating under the above conditions, the F layer can be suitably formed while maintaining high productivity.

[0066] The thickness of the F layer is preferably 0.1 to 150 μm. Specifically, when the base layer is a metal foil, the thickness of the F layer is preferably 1 to 30 μm. When the base layer is a heat-resistant resin film, the thickness of the F layer is preferably 1 to 150 μm, and more preferably 10 to 50 μm. The peel strength between the F layer and the base layer is preferably 10 N / cm or more, more preferably 15 N / cm or more. The peel strength is preferably 100 N / cm or less. By using the present dispersion, the present laminate can be easily formed without impairing the physical properties of the F polymer in the F layer.

[0067] The dispersion may be applied to only one surface of the substrate, or may be applied to both surfaces of the substrate. In the former case, a laminate having a substrate layer made of the substrate and an F layer on one surface of the substrate layer is obtained, while in the latter case, a laminate having a substrate layer made of the substrate and an F layer on both surfaces of the substrate layer is obtained. The latter laminate is less likely to warp, and therefore has excellent handling properties during processing. Specific examples of such laminates include a metal-clad laminate having a metal foil and an F layer on at least one surface of the metal foil, and a multilayer film having a polyimide film and an F layer on both surfaces of the polyimide film. These laminates are suitable as printed circuit board materials, etc., because they have excellent physical properties such as electrical properties, and can be used in the manufacture of flexible printed circuit boards and rigid printed circuit boards.

[0068] Laminates of the F layer and substrate are useful as antenna parts, printed circuit boards, aircraft parts, automobile parts, sports equipment, food industry products, heat dissipation parts, paints, cosmetics, etc. In the case of printed circuit boards, they can also be used as a new printed circuit board material to replace conventional glass epoxy boards in order to prevent temperature rise in printed circuit boards where electronic components are densely mounted. Specifically, these include electric wire coating materials (aircraft electric wires, etc.), enamel wire coating materials used in motors for electric vehicles, etc., electrical insulating tape, insulating tape for oil drilling, materials for printed circuit boards, separation membranes (microfiltration membranes, ultrafiltration membranes, reverse osmosis membranes, ion exchange membranes, dialysis membranes, gas separation membranes, etc.), electrode binders (for lithium secondary batteries, for fuel cells, etc.), copy rolls, covers for furniture, automobile dashboards, home appliances, etc., sliding parts (load bearings, sliding shafts, valves, bearings, bushes, seals, thrust washers, wear rings, pistons, slide switches, gears, cams, belt conveyors, food transport belts, etc.), wear pads, wear strips, tube lamps, test sockets, wafer guides, wear parts for centrifugal pumps, hydrocarbon, chemical and water supply pumps, tools (shovels, files, saws, etc.), boilers, hoppers, pipes, ovens, baking molds, chutes, dies, toilets, container coating materials, power devices, transistors, thyristors, rectifiers, transformers, power MOS It is useful for FETs, CPUs, heat sink fins, metal heat sinks, and blades for wind turbines, wind power generation equipment, aircraft, etc. More specifically, they are useful as sealing materials for processing machines, vacuum ovens, plasma processing devices, and the like that perform heat treatment under low oxygen conditions, for example, housings for personal computers and displays, materials for electronic devices, and the interior and exterior of automobiles, as well as heat dissipation parts in processing units for sputtering and various dry etching devices.

[0069] The method for producing the impregnated woven fabric of the present invention involves impregnating a woven fabric with the present dispersion and heating it to obtain an impregnated woven fabric containing the F polymer (hereinafter also referred to as "the present woven fabric"). The dispersion is impregnated into a woven fabric, which is then dried by heating to obtain a woven fabric impregnated with the F polymer. This woven fabric can also be called a coated woven fabric, in which the woven fabric is coated with an F layer. The woven fabric is preferably a glass fiber woven fabric, a carbon fiber woven fabric, an aramid fiber woven fabric, or a metal fiber woven fabric, and more preferably a glass fiber woven fabric or a carbon fiber woven fabric. The woven fabric may be treated with a silane coupling agent from the viewpoint of increasing the adhesion to the F layer. The dispersion has a pH of less than 7 and can therefore be suitably used for impregnating woven fabrics with low base resistance. Examples of woven fabrics with low base resistance include woven fabrics that have been surface-treated with a surface treatment agent that is hydrolyzed in a base.

[0070] The total content of the F polymer in the present woven fabric is preferably 30 to 80% by mass. Methods for impregnating a woven fabric with the present dispersion include a method of immersing a woven fabric in the present dispersion and a method of coating a woven fabric with the present dispersion. When drying the woven fabric, the F polymer may be calcined. The F polymer may be calcined by passing the woven fabric through a forced-air drying oven in an atmosphere of 300 to 400°C. The drying of the woven fabric and the calcination of the F polymer may be carried out in one step. This woven fabric has excellent properties such as high adhesion (bonding) between the F layer and the woven fabric, high surface smoothness, little distortion, etc. By thermocompression bonding this woven fabric and metal foil, a metal clad laminate with high peel strength and resistance to warping is obtained, which can be suitably used as a printed circuit board material.

[0071] In addition, in the manufacture of the present woven fabric, a woven fabric impregnated with the present dispersion may be applied to the surface of a substrate, and then heated and dried to form an impregnated woven fabric layer containing the F polymer and the woven fabric, thereby producing a laminate in which the substrate and the impregnated woven fabric layer are laminated in this order. The mode of production is not particularly limited, and by applying a woven fabric impregnated with the present dispersion to a part or all of the inner wall surface of a member such as a tank, a pipe, a container, etc., and then heating the member while rotating, an impregnated woven fabric layer can be formed on a part or all of the inner wall surface of the member. This production method is also useful as a method for lining the inner wall surface of members such as a tank, a pipe, a container, etc.

[0072] As explained above, the present dispersion has excellent liquid physical properties such as dispersion stability, and can be highly impregnated into porous or fibrous materials. Such porous or fibrous materials include materials other than the above-mentioned woven fabrics, specifically, plate-like, columnar or fibrous materials. These materials may be pretreated with a curable resin, a silane coupling agent, or the like, and may further be filled with an inorganic filler, etc. These materials may also be twisted together to form a thread, cable, or wire. When twisting together, an intervening layer made of another polymer, such as polyethylene, may be disposed.

[0073] An embodiment in which such a material is impregnated with the present dispersion to produce a molded product includes an embodiment in which a fibrous material carrying a curable resin or a cured product thereof is impregnated with the present dispersion. Examples of fibrous materials include high strength, low elongation fibers such as carbon fibers, aramid fibers, and silicon carbide fibers. As the curable resin, a thermosetting resin such as an epoxy resin, an unsaturated polyester resin, or a polyurethane resin is preferable. A specific example of such an embodiment is a composite cable formed by impregnating a cable made of twisted carbon fibers carrying a thermosetting resin with the present dispersion, and then heating the cable to sinter the F polymer. Such a composite cable is useful as a cable for large structures, ground anchors, oil drilling, cranes, cableways, elevators, agriculture, forestry, fisheries, and slings. EXAMPLES

[0074] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. 1. Preparation of each ingredient [F Powder] F Powder 1: Contains 97.9 mol% TFE units, 0.1 mol% NAH units, and 2.0 mol% PPVE units, in that order, and has a carbonyl group-containing group with a main chain carbon number of 1 × 10 6 Powder (D50: 2.1 μm) made of F polymer 1 (melting temperature: 300°C) with 1000 particles per particle F Powder 2: Powder (D50: 1.8 μm) made of F Polymer 2 (melting temperature 305 ° C.) containing 97.5 mol % and 2.5 mol % of TFE units and PPVE units, in that order, and having no carbonyl group-containing group or hydroxyl group-containing group.

[0075] [Anionic surfactants] Anionic surfactant 1: Dialkyl sulfosuccinate salt (surface tension: 29 mN / m; Sanyo Chemical Industries, Ltd., "Sunmorin OT-70") [Nonionic surfactants] Nonionic surfactant 1: Polyoxyalkylene-modified polydimethylsiloxane having dimethylsiloxane units in the main chain and oxyethylene groups in the side chain Nonionic surfactant 2: Polyethylene glycol trimethylnonyl ether

[0076] 2. Example of production of aqueous dispersion (Example 1) Anionic surfactant 1, nonionic surfactant 1, and water were added to the pot, and zirconia balls were added. The pot was then rolled at 150 rpm for 1 hour to obtain a composition. The composition and F powder 1 were added to the pot, and zirconia balls were added. The pot was then rolled at 150 rpm for 1 hour to obtain an aqueous dispersion 1 containing F powder 1 (30 parts by mass), anionic surfactant 1 (4 parts by mass), nonionic surfactant 1 (4 parts by mass), and water (62 parts by mass). The viscosity of the obtained aqueous dispersion 1 was 50 mPa·s, and the pH of the aqueous dispersion 1 immediately after preparation was 5.5.

[0077] (Example 2) Aqueous dispersion 2 containing F powder 1 (30 parts by mass), anionic surfactant 1 (4 parts by mass), nonionic surfactant 2 (4 parts by mass), and water (62 parts by mass) was obtained in the same manner as in Example 1, except that nonionic surfactant 2 was used instead of nonionic surfactant 1. The viscosity of the obtained aqueous dispersion 2 was 70 mPa s, and the pH of aqueous dispersion 2 immediately after preparation was 5.7.

[0078] (Example 3) Except for using aqueous ammonia instead of water, aqueous dispersion 3 containing F powder 1 (30 parts by mass), anionic surfactant 1 (4 parts by mass), nonionic surfactant 1 (4 parts by mass), and aqueous ammonia (62 parts by mass) was obtained in the same manner as in Example 1. The viscosity of the obtained aqueous dispersion was 80 mPa s, and the pH of aqueous dispersion 3 immediately after preparation was 8.0.

[0079] (Example 4) Aqueous dispersion 4 containing F powder 2 (30 parts by mass), anionic surfactant 1 (4 parts by mass), nonionic surfactant 1 (4 parts by mass), and water (62 parts by mass) was obtained in the same manner as in Example 1, except that F powder 1 was changed to F powder 2. The viscosity of the obtained aqueous dispersion was 80 mPa s, and the pH of aqueous dispersion 4 immediately after preparation was 5.5.

[0080] 3. Evaluation example of aqueous dispersion After storing each aqueous dispersion in a container for a long period of time, the aqueous dispersion was filtered through a microfilter, and the residue was visually inspected to evaluate the dispersion stability according to the following criteria. As a result, the aqueous dispersions 1 to 4 were evaluated as "good", "good", "bad", and "bad", in that order. [Evaluation Criteria] ○: No filtered material is visible. ×: Filtered matter was visible and powder was partially agglomerated.

[0081] 4. Example of evaluation of mixing with aqueous dispersion of polytetrafluoroethylene (PTFE) The miscibility of each aqueous dispersion when it was mixed with a commercially available aqueous dispersion of PTFE was evaluated according to the following criteria. As a result, the aqueous dispersions 1 to 4 were evaluated as "good", "good", "good", and "poor", in that order. [Evaluation Criteria] ◯: A uniform dispersion was formed by shear stirring. ×: A dispersion was formed by shear stirring, but settling of aggregates was observed.

[0082] 5. Evaluation example of laminate Using each of the aqueous dispersions, a laminate was produced according to the following procedure. A wet film was formed by applying an aqueous dispersion onto the surface of a long copper foil (thickness: 18 μm) using a bar coater. The metal foil on which the wet film was formed was then passed through a drying oven at 120° C. for 5 minutes and dried by heating to obtain a dry film. The dry film was then heated at 380° C. for 3 minutes in a nitrogen oven. This produced a laminate having a metal foil and a polymer layer (thickness: 20 μm) as a molded product on its surface.

[0083] Each laminate was irradiated with light from the polymer layer side, and the polymer layer was visually observed from diagonally above to evaluate the surface smoothness according to the following criteria. As a result, the laminate obtained from aqueous dispersion 1, the laminate obtained from aqueous dispersion 2, the laminate obtained from aqueous dispersion 3, and the laminate obtained from aqueous dispersion 4 were evaluated as "good", "good", "poor", and "poor", in that order. [Evaluation Criteria] ◯: The entire surface of the polymer layer is smooth. ×: Bumpy patterns are observed in the polymer layer. [Industrial Applicability]

[0084] The aqueous dispersion of the present invention is excellent in dispersion stability, handling properties, blendability and long-term storage properties, and can be used to produce molded articles (laminates, impregnated woven fabrics, etc.) having physical properties based on the F polymer. The laminate and impregnated woven fabric of the present invention are useful as antenna parts, printed circuit boards, aircraft parts, automobile parts, sports equipment, food industry products, paints, cosmetics, etc., and specifically, are useful as electric wire covering materials (aircraft electric wires, etc.), electrical insulating tapes, insulating tapes for oil drilling, materials for printed circuit boards, separation membranes (microfiltration membranes, ultrafiltration membranes, reverse osmosis membranes, ion exchange membranes, dialysis membranes, gas separation membranes, etc.), electrode binders (for lithium secondary batteries, for fuel cells, etc.), copy rolls, furniture, automobile dashboards, covers for home appliances, etc., sliding members (load bearings, sliding shafts, valves, bearings, gears, cams, belt conveyors, food transport belts, etc.), tools (shovels, files, saws, saws, etc.), boilers, hoppers, pipes, ovens, baking molds, chutes, dies, toilets, and container covering materials.

Claims

1. The aqueous dispersion contains 20% by mass or more and 70% by mass or less of a powder of a heat-fusible tetrafluoroethylene-based polymer having 100 to 3,000 carbonyl group-containing groups per 1 x 10 carbon atoms in the main chain, 0.1 to 10% by mass of an anionic surfactant which is a dialkyl sulfosuccinate salt, a polyoxyalkylene alkyl ether phosphate salt or a polyoxyalkylene alkyl ether sulfate salt, and water, and has a pH of less than 7.

2. 2. The aqueous dispersion according to claim 1, wherein the powder has an average particle size of 0.1 to 25 μm.

3. 3. The aqueous dispersion according to claim 1, wherein the anionic surfactant has a surface tension of 30 mN / m or less.

4. The aqueous dispersion according to any one of claims 1 to 3, further comprising a nonionic surfactant.

5. 5. The aqueous dispersion according to claim 4, wherein the nonionic surfactant is a polyoxyalkylene-modified polydimethylsiloxane or a glycol monoalkyl ether.

6. The aqueous dispersion according to any one of claims 1 to 5, further comprising an inorganic filler or a polymer different from the tetrafluoroethylene-based polymer or a precursor thereof.

7. 7. The aqueous dispersion of claim 6, wherein the different polymer is non-thermofusible polytetrafluoroethylene.

8. The aqueous dispersion according to any one of claims 1 to 7, wherein the pH is from 4 to 6.

9. A method for producing the aqueous dispersion according to any one of claims 1 to 8, comprising mixing the powder with an aqueous solution containing the anionic surfactant.

10. A method for producing a laminate, comprising applying the aqueous dispersion according to any one of claims 1 to 8 to a surface of a substrate, heating the surface, and forming a polymer layer containing the tetrafluoroethylene-based polymer to obtain a laminate having a substrate layer constituted by the substrate and the polymer layer.

11. A method for producing an impregnated woven fabric, comprising impregnating a woven fabric with the aqueous dispersion according to any one of claims 1 to 8 and heating the same to obtain an impregnated woven fabric containing the tetrafluoroethylene-based polymer.

Citation Information

Patent Citations

  • Sulfonate compound, method for producing sulfonate compound

    JP2009029722A

  • Aqueous fluoropolymer dispersion

    WO2007026822A1

  • Method for producing aqueous dispersion of fluorine-containing polymer, aqueous dispersion of fluorine-containing polymer, and fluorine-containing polymer

    WO2015008649A1

  • Method for producing modified polytetrafluoroethylene, method for producing modified polytetrafluoroethylene powder, and method for producing stretched porous body

    WO2019065638A1