Seamless steel pipe and method for manufacturing steel pipe
A steel pipe with specific composition and a bending-unbending process enhances both tensile and compressive yield strengths, addressing the limitations of conventional cold rolling by improving fatigue properties under combined loads.
Patent Information
- Application Number
- JP2021159801
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-29
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2041-09-29
AI Technical Summary
Conventional cold rolling methods for steel pipes improve tensile yield strength in the axial direction but result in inferior compressive yield strength and fatigue properties when subjected to compressive loads, leading to inadequate performance in applications with combined tensile and compressive stresses.
A steel pipe composition with specific element ratios and a manufacturing process involving bending and unbending in the circumferential direction, followed by controlled heat treatment, to enhance both tensile and compressive yield strengths and fatigue properties.
The method achieves a high tensile yield strength of 400 MPa or more with a compressive yield strength ratio of 0.85 to 1.15, providing excellent fatigue properties under both tensile and compressive loads, suitable for applications with repeated bending and thermal stress.
Smart Images

Figure 0007559728000003 
Figure 0007559728000001 
Figure 0007559728000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel pipe having a high axial tensile yield strength, a small difference between the axial tensile yield strength and the axial compressive yield strength, and excellent fatigue properties, and a method for manufacturing the same. [Background technology]
[0002] Cold rolling of steel pipes includes cold drawing (cold drawing, punch rolling) and cold pilger rolling. In this cold rolling, strain is applied to the steel pipe by elongating it in the axial direction and reducing its wall thickness, which improves the axial yield strength of the steel pipe, which is one of its mechanical properties. Cold rolling is carried out in the manufacture of steel pipes used in applications where a high tensile load is applied in the pipe axial direction. For example, Patent Document 1 discloses a method for manufacturing a pipe having improved fatigue strength by cold drawing. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 4285053 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the technology described in Patent Document 1 has a problem with respect to fatigue characteristics when a load is applied by compressing the tube in the axial direction. In other words, cold rolling, such as cold drawing and cold pilger rolling, which stretches the tube in the axial direction, has the effect of improving the yield strength in the axial direction of the tube and also improving the fatigue strength in the axial direction of the tube. In contrast, the load generated by compression in the axial direction of the tube is significantly inferior to the yield strength characteristics in the tensile direction in the axial direction due to the Bauschinger effect. Fatigue strength is highly correlated with the tensile strength of the material. In other words, these methods of improving the strength of steel tubes using cold rolling have the problem that the yield strength when compressed in the axial direction of the tube (compressive yield strength in the axial direction of the tube) is lower than the yield strength due to tension (tensile yield strength in the axial direction of the tube), and the fatigue characteristics (compressive fatigue characteristics) when a load is generated by compression in the axial direction of the tube are also inferior.
[0005] Steel pipes in which the tensile yield strength in the axial direction has been increased using conventional cold rolling are effective in improving fatigue strength against repeated loads in the tensile direction only (tensile fatigue strength), but are weak against loads in the compressive direction, where the yield strength is relatively poor.
[0006] The load that affects the fatigue properties of steel pipes is rarely axial tension alone, but rather a combination of axial tension and axial compression. In other words, the conventional method of increasing the strength of steel pipes using cold drawing or cold pilger rolling is effective in improving the tensile yield strength in the axial direction of the pipe (tensile yield strength in the axial direction of the pipe) and the fatigue strength under tensile load only in the axial direction of the pipe (tensile fatigue strength). However, it is difficult to increase the yield strength when compressed in the axial direction of the pipe (compressive yield strength in the axial direction of the pipe) and the fatigue strength (compressive fatigue strength) compared to the tensile yield strength in the axial direction of the pipe and the fatigue strength obtained under tensile load in the axial direction of the pipe.
[0007] For the above reasons, the conventional method of increasing the strength of steel pipes by cold rolling cannot solve the problem that the mechanical properties (axial compressive yield strength and compressive fatigue strength) when compressed in the axial direction are inferior to the axial tensile yield strength and tensile fatigue strength. Excellent mechanical properties when compressed in the axial direction are required in applications where a compressive load is generated in the axial direction, such as in axles where the pipe is repeatedly subjected to bending loads in the axial direction (where a compressive load in the axial direction is generated on the inner diameter side of the bending curvature). Furthermore, when steel pipes are repeatedly connected with screws, a compressive load is applied to the threaded portion when the pipes are fastened, and a tensile load is applied when the pipes are used after fastening. Furthermore, when used as steel pipes for hot wells or oil well drilling, repeated compressive and tensile loads are generated in the axial direction of the pipe due to thermal expansion caused by high temperatures of geothermal energy and thermal contraction when the well cools down. In addition, when used as piping in chemical plants or for burying carbon dioxide underground for CCS (Carbon dioxide Capture and Storage) or CCUS (Carbon dioxide Capture, Utilization and Storage), temperature changes and internal and external pressure changes occur due to pressure fluctuations in the fluid inside the pipe, and thermal stress and pressure cause repeated tensile and compressive loads in the axial direction of the pipe. In these operating environments where repeated tension-compression fatigue loads are applied, sufficient fatigue strength cannot be obtained with steel pipes having low axial compressive yield strength obtained by conventional cold rolling.
[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide a steel pipe having a high axial tensile yield strength, a small difference between the axial tensile yield strength and the compressive yield strength, and excellent fatigue properties, and a manufacturing method thereof.
[0009] Here, a high axial tensile yield strength means that the axial tensile yield strength is 400 MPa or more, and a small difference between the axial tensile yield strength and the compressive yield strength means that the axial compressive yield strength / axial tensile yield strength is in the range of 0.85 to 1.15. "Excellent fatigue properties" means that the same steel pipe material has a higher fatigue strength than a steel pipe manufactured by cold drawing or cold pilgering. [Means for solving the problem]
[0010] As shown in Patent Document 1, cold drawing or cold pilger rolling has been conventionally used as a cold rolling method for improving axial strength, which is the most important mechanical property of a steel pipe. The present inventors have noticed that the direction in which plastic strain is imparted to the steel pipe by these cold working methods is the cause of the problem. In other words, in cold drawing and cold pilger rolling, plastic strain is applied to the steel pipe in the cold state, and the steel pipe is strengthened by dislocation strengthening. The plastic strain generated in cold drawing and cold pilger rolling causes diameter reduction or pipe expansion deformation on the outer periphery of the pipe. In addition, in the thickness direction of the pipe, a decrease or increase in thickness occurs due to plastic strain. On the other hand, in the axial direction of the tube, plastic strain is imparted only in the elongation direction. In metal materials, the Bauschinger effect generally occurs at the end of forming, which means that the material becomes weak against a load in the opposite direction to the direction in which plastic strain is applied. Therefore, in conventional cold rolling such as cold drawing and cold pilger rolling, the axial compressive strength of the tube inevitably decreases due to the Bauschinger effect.
[0011] Therefore, the inventors of the present invention have conducted extensive research focusing on the direction of plastic strain in the axial direction of a steel pipe, in contrast to the conventional cold rolling method for steel pipes, which only elongates the pipe in the axial direction. As a result, they have come up with a method for increasing the axial compressive yield strength and the associated fatigue strength of a steel pipe by cold working without relying on plastic strain caused by elongation in the axial direction.
[0012] The present invention has been made based on the above findings, and the gist of the present invention is as follows. [1] In mass percent, C: 0.01 to 1.15%, Si: 0.01 to 2.50%, Mn: 0.01 to 2.50%, N: 0.001 to 0.050%, with the balance being Fe and unavoidable impurities; The steel has a structure having a ferrite phase and a retained austenite phase of 10% or less in area ratio, The axial tensile yield strength is 400 MPa or more. A steel pipe in which the ratio of compressive yield strength in the pipe axis direction to tensile yield strength in the pipe axis direction is 0.85 to 1.15. [2] The component composition further comprises, in mass%, Cr: 2.00% or less, The steel pipe according to the above [1], containing one or two types selected from the following: Mo: 2.00% or less. [3] The component composition further comprises, in mass%, Ti: 0.50% or less, Al: 0.30% or less, V: 0.55% or less, The steel pipe according to the above [1] or [2], containing one or more selected from the following: Nb: 0.75% or less. [4] The component composition further comprises, in mass%, Ni: less than 2.5% W: less than 1.0%, Cu: less than 2.5% B: 0.010% or less, Zr: 0.10% or less, Ca: 0.010% or less, Ta: 0.01% or less, REM: 0.10% or less, Mg: 0.10% or less, Sn: 0.30% or less, Sb: 0.30% or less, The steel pipe according to any one of the above [1] to [3], containing one or more selected from the following: Ag: 0.30% or less. [5] A method for producing a steel pipe according to any one of the above [1] to [4], comprising bending and unbending a steel pipe material in a circumferential direction to obtain a steel pipe. [6] A method for manufacturing a steel pipe as described in [5] above, in which, after the bending and unbending in the circumferential direction of the pipe, a heat treatment is performed in which the holding temperature is 300°C or less and the holding time is 300 seconds or more and less than 3600 seconds, followed by air cooling. Effect of the Invention
[0013] According to the present invention, there are provided a steel pipe having a high axial tensile yield strength, a small difference between the axial tensile yield strength and the compressive yield strength, and excellent fatigue properties, and a method for producing the same. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic diagram showing a method of cold bending and unbending in the circumferential direction of a pipe. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described below.
[0016] The steel pipe of the present invention has a composition containing, by mass%, C: 0.01-1.15%, Si: 0.01-2.50%, Mn: 0.01-2.50%, N: 0.001-0.050%, with the balance being Fe and unavoidable impurities, has a ferrite phase and a microstructure in which the area fraction of the retained austenite phase is 10% or less, has an axial tensile yield strength of 400 MPa or more, and has an axial compressive yield strength / axial tensile yield strength of 0.85-1.15.
[0017] First, the reasons for limiting the composition of the steel pipe of the present invention will be explained. Unless otherwise specified, mass% will be simply abbreviated as % below.
[0018] C: 0.01 to 1.15% C is important for improving the strength and fatigue properties of steel, and must be contained at 0.01% or more. However, excessive C content forms an austenite phase and excess carbides, reducing strength, fatigue, and toughness properties. Therefore, the C content is set to 1.15% or less. From the viewpoint of obtaining high strength and fatigue properties while maintaining good toughness, the C content is preferably set to 0.05% or more. Moreover, the C content is preferably set to 0.55% or less.
[0019] Silicon: 0.01 to 2.50% Since Si has a deoxidizing effect on steel, it is effective to include an appropriate amount of Si in molten steel. In addition, since it is effective in improving the strength properties of steel, it is necessary to include Si. However, the cold workability and low-temperature toughness are impaired with the inclusion of a large amount of Si. Therefore, the Si content is set to 2.50% or less. On the other hand, since excessive reduction of Si after deoxidation leads to an increase in manufacturing costs, the Si content is set to 0.01% or more. In order to obtain a sufficient deoxidizing effect, the Si content is preferably set to 0.10% or more. From the viewpoint of suppressing the deterioration of cold workability and low-temperature toughness due to excess Si remaining in the steel, the Si content is preferably set to 0.80% or less.
[0020] Mn: 0.01 to 2.50% Mn must be present at 0.01% or more to improve the strength properties of steel. However, since Mn is a strong austenite phase forming element, excessive Mn content increases the amount of retained austenite phase and reduces strength. Therefore, the Mn content is set to 2.50% or less. In order to obtain a specified structure while improving the strength properties, the Mn content is preferably set to 0.10% or more. In addition, the Mn content is preferably set to 1.50% or less.
[0021] N: 0.001 to 0.050% In order to obtain a fine structure and strength properties, the N content must be 0.001% or more. However, if the N content is excessive, bubbles will form in the steel, so the N content is set to 0.050% or less. Reducing the N content to an extreme level requires time and costs for processing, and from the viewpoint of stably obtaining a fine structure without bubbles, the N content is preferably set to 0.005 to 0.050%.
[0022] The balance is Fe and unavoidable impurities. Examples of unavoidable impurities include P: 0.05% or less, S: 0.05% or less, and O (oxygen): 0.01% or less. P, S, and O are impurities that are inevitably mixed in during refining. If the remaining amounts of these elements as impurities are too high, various problems may occur, such as reduced hot workability, corrosion resistance, and low-temperature toughness. Therefore, it is preferable to control the amounts of P: 0.05% or less, S: 0.05% or less, and O: 0.01% or less, respectively.
[0023] In addition to the above-mentioned component composition, the present invention may contain the following elements as necessary.
[0024] Cr: 2.00% or less, Mo: 2.00% or less Selected from the following two types Cr: 2.00% or less (including 0%) Cr improves the strength properties of steel and is effective in improving corrosion resistance and wear resistance, so if Cr is contained, it is preferable to contain 0.05% or more. On the other hand, if an excessive amount of Cr is contained, the hardness increases and the cold workability decreases. Therefore, the Cr content is preferably 2.00% or less. From the viewpoint of obtaining a strength improvement effect and excellent cold workability, the Cr content is more preferably 0.5% or more. Also, the Cr content is more preferably 1.3% or less.
[0025] Mo: 2.00% or less (including 0%) Mo is effective in improving high-temperature strength, so if it is contained, it is preferable to contain 0.05% or more. On the other hand, if the Mo content is high, the hardness increases and the cold workability decreases. Therefore, the Mo content is preferably 2.00% or less. From the viewpoint of obtaining high-temperature strength and excellent cold workability, the Mo content is more preferably 0.1% or more. Also, the Mo content is more preferably 1.5% or less.
[0026] The present invention may further contain the following elements as necessary.
[0027] One or more selected from the following: Ti: 0.50% or less (including 0%), Al: 0.30% or less (including 0%), V: 0.55% or less (including 0%), Nb: 0.75% or less (including 0%) When contained in an appropriate amount, Ti, Al, V, and Nb form nitrides or carbides and are effective in refining the structure, and can be contained as necessary. When contained, the Ti content is preferably 0.001% or more. The Al content is preferably 0.001% or more. The V content is preferably 0.01% or more. The Nb content is preferably 0.01% or more. When contained, in order to prevent a decrease in toughness, it is preferable that Ti is contained at 0.50% or less, Al is contained at 0.30% or less, V is contained at 0.55% or less, and Nb is contained at 0.75% or less. In addition, from the viewpoint of suppressing alloy costs, the Ti content is preferably 0.05% or less, the Al content is preferably 0.10% or less, the V content is preferably 0.30% or less, and the Nb content is preferably 0.30% or less.
[0028] The present invention may further contain the following elements as necessary.
[0029] One or more selected from the following: Ni: less than 2.5% (including 0%), W: less than 1.0% (including 0%), Cu: less than 2.5% (including 0%) Ni: Less than 2.5% (including 0%) Ni is effective in improving the toughness of steel. When Ni is contained, it is preferable to contain 0.01% or more. On the other hand, if Ni is contained excessively, the tensile strength and fatigue strength decrease. Therefore, the Ni content is preferably less than 2.5%. From the viewpoint of obtaining toughness and excellent strength properties, the Ni content is more preferably 0.05% or more. Also, the Ni content is preferably 1.50% or less.
[0030] W: Less than 1.0% (including 0%), Cu: Less than 2.5% (including 0%) W and Cu improve the corrosion resistance of steel. When contained, the W content is preferably 0.01% or more and the Cu content is preferably 0.01% or more. If the content of each element is high, it may cause deterioration of the surface skin and defects during hot forming. Therefore, it is preferable that the W content is less than 1.0% and the Cu content is less than 2.5%. It is more preferable that the W content is 0.10% or less. It is more preferable that the Cu content is 1.50% or less.
[0031] The present invention may further contain the following elements as necessary.
[0032] One or more selected from the following: B: 0.010% or less (including 0%), Zr: 0.10% or less (including 0%), Ca: 0.010% or less (including 0%), Ta: 0.01% or less (including 0%), REM: 0.10% or less (including 0%), Mg: 0.10% or less (including 0%) When B, Zr, Ca, Ta, REM, and Mg are contained in very small amounts, they affect the workability and surface scale during hot forming, and are useful for suppressing surface defects. Therefore, when they are contained, the B content is preferably 0.001% or more. The Zr content is preferably 0.01% or more. The Ca content is preferably 0.001% or more. The Ta content is preferably 0.001% or more. The REM content is preferably 0.001% or more. The Mg content is preferably 0.001% or more. However, excessive content may worsen surface defects. It is preferable that B is contained at 0.010% or less, Zr is contained at 0.10% or less, Ca is contained at 0.010% or less, Ta is contained at 0.01% or less, REM is contained at 0.10% or less, and Mg is contained at 0.10% or less. It is more preferable that the B content is 0.005% or less. It is more preferable that the Zr content is 0.03% or less. The Ca content is more preferably 0.005% or less. The Ta content is more preferably 0.005% or less. The REM content is more preferably 0.005% or less. The Mg content is more preferably 0.005% or less.
[0033] The present invention may further contain the following elements as necessary.
[0034] One or more selected from the following: Sn: 0.30% or less (including 0%), Sb: 0.30% or less (including 0%), Ag: 0.30% or less (including 0%) Adding small amounts of Sn, Sb, and Ag improves corrosion resistance. There is no need to set a lower limit for the content, but if they are included, the corrosion resistance can be improved by making the Sn, Sb, and Ag content 0.0001% or more. On the other hand, if the content is too high, the hot workability decreases. Therefore, if they are included, the Sn, Sb, and Ag content should be 0.30% or less.
[0035] Next, the structure of the steel pipe according to the present invention will be described.
[0036] The microstructure of the present invention has a ferrite phase (including a bainite phase) and the area ratio of the retained austenite phase is 10% or less. The microstructure of the present invention may also contain a cementite phase (including pearlite). A steel pipe having such a microstructure does not have a high axial tensile yield strength when left to cool after hot rolling or when treated by annealing, but when cold working is performed, the strength is increased by dislocation strengthening due to plastic strain, and the pipe also exhibits excellent fatigue strength properties.
[0037] Since the Bauschinger effect operates in this structure, when cold drawing or cold pilger rolling is performed to increase the strength of a steel pipe by utilizing the elongation plastic strain in the axial direction, the compressive yield strength in the axial direction decreases, and as a result, the fatigue strength under a compressive load in the axial direction is inferior to the fatigue strength under a tensile load in the axial direction. Therefore, in order to obtain excellent fatigue strength in both the tensile and compressive directions in the axial direction, bending and unbending is required as cold working.
[0038] The area ratio of the ferrite phase is not particularly limited, but is preferably 50% or more because the workability during cold working is good. The upper limit of the area ratio of the ferrite phase is not particularly limited, but from the viewpoint of obtaining high strength characteristics while obtaining good workability, the area ratio of the ferrite phase is preferably 95% or less.
[0039] The area ratio of the cementite phase is not particularly limited, but is preferably 5% or more from the viewpoint of obtaining high strength and high hardness, and is preferably 50% or less from the viewpoint of obtaining excellent toughness and cold workability.
[0040] In addition, the area ratio of the retained austenite phase present in the ferrite phase or cementite phase exceeds 10%, which adversely affects cold workability and strength characteristics, but if it is 10% or less, this does not cause any problems. Therefore, in the structure of the present invention, the area ratio of the retained austenite phase is 10% or less.
[0041] The method for measuring the structure is as follows: After cold working, the steel pipe is mirror-polished and etched with an acid such as Nital or Virela's etching solution. An optical microscope can then be used to confirm that the structure contains ferrite phase, or ferrite phase and cementite phase (including pearlite); pearlite is colored black, making it possible to measure its fraction. The precision of the area fraction can be improved by using a magnification of 100 to 400 times and a field of view that allows observation of 50 or more ferrite grains, or a total of 50 or more ferrite grains and pearlite grains.
[0042] In addition, the ferrite phase, or the phases other than the ferrite phase and the cementite phase, can be observed with an electron microscope. The percentage of the retained austenite phase can be easily measured by separating the peaks of the body-centered cubic lattice of the ferrite phase and the face-centered cubic lattice of the austenite phase by X-ray diffraction on a mirror-polished test piece. The volume fraction of the retained austenite phase is measured by X-ray diffraction, and this is treated as the area fraction of the retained austenite phase.
[0043] Furthermore, in the steel pipe of the present invention, the same structure containing a ferrite phase or a ferrite phase and a cementite phase is obtained before and after cold working.
[0044] The structure of the steel pipe of the present invention can be controlled by adjusting the composition.
[0045] In the steel pipe of the present invention, the axial tensile yield strength is set to 400 MPa or more. Normally, since a structure containing a ferrite phase is soft, an axial tensile yield strength of 400 MPa or more cannot be obtained without cold working. Therefore, in the present invention, dislocation strengthening is performed by cold working in order to obtain a high axial tensile yield strength of 400 MPa or more. There is no upper limit to the axial tensile yield strength, but since delayed fracture may occur if the strength is too high, it is preferable that the axial tensile yield strength be 870 MPa or less.
[0046] In the present invention, the ratio of the tube axial compressive yield strength to the tube axial tensile yield strength, i.e., tube axial compressive yield strength / tube axial tensile yield strength, is set to 0.85 to 1.15. By setting the tube axial compressive yield strength / tube axial tensile yield strength to 0.85 to 1.15, excellent fatigue strength can be obtained even when a compressive load is included, compared to fatigue strength under tensile load in the tube axial direction. The ratio of the tube axial compressive yield strength to the tube axial tensile yield strength, i.e., tube axial compressive yield strength / tube axial tensile yield strength, is preferably closer to 1 because excellent fatigue properties can be obtained, and the tube axial compressive yield strength / tube axial tensile yield strength is preferably 0.95 or more. Also, the tube axial compressive yield strength / tube axial tensile yield strength is preferably 1.10 or less.
[0047] The tube axial compressive yield strength can be measured by a cylindrical compression test. The cylindrical test piece to be compressed is taken from the center of the tube wall thickness parallel to the tube axial direction. The outer diameter d [mm] of the cylinder and the height h [mm] should be h / d≦2.0. Specifically, a test piece with an outer diameter d = 3.0 mm and a height h = 5.0 mm is cut out from the center of the tube wall thickness. The compression test is performed at room temperature (25°C) by sandwiching the test piece between flat plates and applying a load, and the compressive yield strength is calculated using the stress-strain curve obtained during compression. The stress-strain curve is obtained by compressing 30% with a compression testing machine at a compression speed of 1.0 mm / min.
[0048] The axial tensile yield strength is measured according to JIS Z2241 (2011). First, a round bar tensile test piece with a parallel diameter of 3.0 mm is cut from the center of the wall thickness of the tube parallel to the axial direction. A tensile test is then performed at room temperature (25°C) with a crosshead speed of 1.0 mm / min until fracture. The tensile yield strength is calculated using the stress-strain curve obtained from this.
[0049] In the steel pipe of the present invention, the axial compressive yield strength / axial tensile yield strength can be controlled to 0.85 to 1.15 by subjecting the steel pipe material having the above-mentioned composition to bending and unbending processing described later.
[0050] The fatigue environment in which good fatigue strength can be obtained in the present invention will be explained. In conventional cold rolling, such as cold drawing and cold pilger rolling, the fatigue properties against stress in the tensile direction in the tube axis direction are good. In other words, it is good in a unilateral tensile stress environment in which the stress σ ratio R (=σmin / σmax) in the fatigue test is 0. On the other hand, most normal fatigue environments are alternating fatigue environments in which tension and compression are applied, R=-1, but conventional cold rolling, which has poor compressive yield strength, does not provide good fatigue strength in an alternating fatigue environment. Since the present invention is excellent in axial compressive yield strength / axial tensile yield strength, it exhibits good fatigue strength even in an alternating fatigue environment in which a stress in the compressive direction is loaded. Therefore, the steel pipe of the present invention is suitably used for axles, steel pipes with threaded joints, steel pipes for hot wells and oil wells, chemical plant piping, etc.
[0051] Next, a method for producing a steel pipe according to the present invention will be described.
[0052] First, a steel material with the above-mentioned composition is prepared. There are no limitations to the method of smelting steel, and various melting processes can be applied. For example, when producing steel by electrically melting scrap iron or lumps of each element, a vacuum melting furnace or an atmospheric melting furnace can be used. When using molten pig iron produced by the blast furnace method, an Ar-O2 mixed gas bottom blowing decarburization furnace or a vacuum decarburization furnace can be used. The molten material is solidified by static casting or continuous casting to form an ingot or slab, which is then hot-rolled into a plate-shaped steel material or forged or rolled into a round billet to produce the steel material.
[0053] Next, in the case of a plate-shaped steel material, it is formed into an approximately tubular shape, and the ends are welded to form a steel pipe. There is no particular limit to the steel pipe forming process, and forming techniques such as UOE forming and roll forming, welding using a molten material, and electric resistance welding using induction heating can be used. In addition, in the case of a round billet-shaped steel material, it is heated in a heating furnace and is turned into a steel pipe shape through various hot rolling processes. Then, hot forming (piercing process) is performed to make the round billet into a hollow pipe. As the hot forming, any method such as the Mannesmann method or the extrusion pipe making method can be used. In addition, if necessary, an elongator, an Assel mill, a mandrel mill, a plug mill, a sizer, a stretch reducer, etc., which are hot rolling processes for reducing the wall thickness and determining the outer diameter of the hollow pipe, may be used.
[0054] Next, it is preferable to perform annealing heat treatment on the steel pipe after forming before cold working in order to homogenize the structure and remove residual stress. Cooling after heat treatment is preferably performed by furnace cooling or natural cooling at a rate of 5°C / s or less in order to maintain the uniform state obtained by annealing with little residual stress.
[0055] In the present invention, the yield strength of a steel pipe is increased by bending and unbending the pipe in the circumferential direction.
[0056] In this cold working method, the strength of steel pipes is increased by utilizing dislocation strengthening caused by plastic strain caused by bending and unbending in the circumferential direction of the pipe. This working method will be described with reference to the drawings. Unlike cold drawing and cold pilger rolling, in which plastic strain caused by cold working occurs in the longitudinal direction of the pipe axis, this method is given by bending the pipe to flatten it (first flattening) and then bending it back to return it to a perfect circle (second flattening), as shown in Figure 1. In this method, the amount of strain is adjusted by using repeated bending and unbending and changes in the amount of bending, but the applied strain does not significantly change the shape before and after processing. Furthermore, since almost no strain occurs in the axial direction of the pipe and strength is increased by dislocation strengthening caused by strain applied in the circumferential direction and the wall thickness direction of the pipe, the occurrence of the Bauschinger effect in the axial direction of the pipe can be suppressed. In other words, there is no significant decrease in the axial compressive strength compared to the axial tensile strength, as occurs in cold drawing and cold pilger rolling, and therefore excellent axial compressive fatigue strength properties are obtained.
[0057] 1(a) and (b) are cross-sectional views when there are two tool contact areas, and FIG. 1(c) is a cross-sectional view when there are three tool contact areas. The thick arrow in FIG. 1 indicates the direction in which force is applied when flattening the steel pipe. As shown in FIG. 1, when performing the second flattening, the tool can be moved to rotate the steel pipe or the tool position can be shifted so that the tool comes into contact with areas that were not flattened in the first flattening (the shaded areas in FIG. 1 indicate the areas flattened in the first flattening).
[0058] As shown in Figure 1, by performing bending and unbending processing in the circumferential direction of the pipe to flatten it intermittently or continuously around the entire circumference of the pipe, bending strain is applied near the maximum value of the steel pipe's curvature, and unbending strain is applied toward the minimum value of the steel pipe's curvature. As a result, strain due to bending and unbending deformation necessary for improving the strength of the steel pipe (dislocation strengthening) accumulates. In addition, when using this processing method, unlike processing methods that compress the pipe's wall thickness and outer diameter, it is characterized by the fact that it does not require a large amount of power, and because the deformation is due to flattening, it is possible to process while minimizing the change in shape before and after processing.
[0059] In bending and unbending, in order to control the strength of the steel pipe in the axial direction, it is important to manage the flattening amount of the pipe. The more the pipe is flattened, the more distortion occurs, and the greater the improvement in the strength in the axial direction in one bending and unbending process. In order to obtain sufficient strength in the axial direction by bending and unbending, it is preferable to give a flattening amount of 5% or more (flattening to an outer diameter that is 95% or less of the initial outer diameter) to the outer diameter of the steel pipe before processing, although this depends on the material composition. In addition, a flattening amount of 10% or more can obtain stable strength in the axial direction. There is no particular upper limit to the flattening amount, but if the flattening amount is too large, the roundness after bending and unbending will deteriorate. In addition, there is a possibility that cracks will occur during processing. Therefore, it is preferable to perform bending and unbending with a flattening amount of 25% or less.
[0060] As shown in Fig. 1, rolls may be used as the tool shape used for flattening the steel pipe. If the steel pipe is flattened and rotated between two or more rolls arranged in the circumferential direction of the steel pipe, it is possible to easily give strain by repeated bending and unbending deformation. Even in this case, the strength in the pipe axis direction can be controlled by the amount of flattening, and it is preferable to set the roll interval to 95% or less of the initial outer diameter of the steel pipe so that the amount of flattening of the steel pipe relative to the initial outer diameter of the steel pipe is 5% or more, and stable strength characteristics in the pipe axis direction can be obtained by setting the roll interval to 90% or less of the initial outer diameter of the steel pipe and the amount of flattening to 10% or more. If the roll interval is set to give an amount of flattening of more than 25% of the initial outer diameter, cracks may occur, the roundness may deteriorate, and the bite into the rolls may decrease, so it is preferable to set the amount of flattening to 25% or less.
[0061] If the rotation axis of the roll is inclined within 90° with respect to the rotation axis of the tube, the steel tube advances in the direction of the tube rotation axis while undergoing flattening, so that continuous processing can be easily performed. In addition, continuous processing using this roll can easily change the curvature (flattening amount) of the steel tube in the first and second passes by, for example, changing the roll interval appropriately so as to change the flattening amount as the steel tube advances. Therefore, by changing the roll interval, the movement path of the neutral line can be changed, making it possible to homogenize the strain in the wall thickness direction. Similarly, the same effect can be obtained by changing the roll diameter instead of the roll interval to change the flattening amount. These methods may also be combined. Although the equipment becomes complicated, if the number of rolls is three or more, the touching of the tube during processing can be suppressed, and stable processing can be performed.
[0062] As described above, it is preferable that the flattening be performed by using tools such as rolls to pinch the outer periphery of the pipe with a gap that is 5 to 25% smaller than the outer diameter of the pipe and rotating the pipe.
[0063] Regarding the processing temperature in bending and unbending in the circumferential direction of the tube, if a desired strength in the axial direction of the tube can be obtained without significantly eliminating dislocations, heat generation caused by heating or increasing the processing speed will not be a problem. From these points of view, the processing temperature is preferably controlled at 300°C or less, and room temperature is preferable to prevent accumulated dislocations from disappearing.
[0064] Furthermore, even if processing heat occurs with an increase in processing speed, the processing time is not a problem as long as dislocations do not disappear significantly and a specified strength in the tube axis direction is obtained. It is preferable that the temperature of the steel pipe during processing does not exceed 300°C. When bending and unbending processing is performed using inclined rolls, it is preferable that the processing time is 10 seconds / m or more (bending and unbending 1 m of the steel pipe in the tube axis direction takes 10 seconds or more).
[0065] In the present invention, heat treatment may be performed within a range in which dislocations do not disappear significantly after cold working. By performing heat treatment, residual stress after cold working can be reduced, fatigue strength can be improved, and the ratio of compressive yield strength in the tube axis direction to tensile yield strength in the tube axis direction can be made closer to 1, so heat treatment is effective for obtaining a steel pipe with a smaller strength ratio. The upper limit of the heat treatment temperature (holding temperature) is 300°C or less, so there is no problem with strength reduction, and the heat treatment temperature is preferably 300°C or less. From the viewpoint of avoiding blue brittleness, this heat treatment temperature is preferably 100 to 250°C. From the viewpoint of maintaining strength after bending and unbending, the heat treatment time (holding time) is preferably 300 seconds or more and less than 3600 seconds. After the heat treatment (holding), air cooling is performed (average cooling rate (= (cooling start temperature (°C) - cooling end temperature (°C)) / cooling time (s)): 0.1 to 5.0°C / s). EXAMPLES
[0066] The present invention will be described below with reference to examples. Note that, although the present examples are directed to seamless steel pipes, the same effects can be obtained with steel pipes obtained by forming and welding steel material in the shape of a plate.
[0067] Materials having the composition of steel types A to N shown in Table 1 were melted in a vacuum melting furnace and then hot rolled into round billets with an outer diameter of φ60 mm.
[0068] [Table 1]
[0069] After hot rolling, the round billet was again inserted into the heating furnace and held at a high temperature of 1200°C or more, and then hot-formed into a seamless blank pipe with an outer diameter of φ70 mm and an inner diameter of 58 mm (wall thickness 6 mm) using a Mannesmann piercing mill. The blank pipes of each composition after hot forming were allowed to cool naturally. For steel types B, D, E, F, G, H, I, J, K, L, M, and N, they were allowed to cool naturally, then reheated to 850°C, and then slowly cooled, for annealing heat treatment. The blank pipes (steel pipe materials) after hot rolling or annealing heat treatment were cold worked to increase the strength in the tensile direction of the pipe axis. As shown in Table 2, the cold working method was either one of two methods, drawing rolling, which is one of the conventional cold working methods, or bending and bending back processing according to the present invention. In addition, the number of times of processing was increased to one, and a condition of performing processing twice for the purpose of further increasing the strength was added. The drawing rolling was performed under conditions of a wall thickness reduction of 10-25% and a 20% reduction in the outer periphery. The bending and unbending process was performed by preparing a rolling mill with three cylindrical rolls arranged at a 120° pitch around the outer periphery of the tube (see Figure 1(c)), clamping the outer periphery of the tube with the roll spacing set to 10-20% smaller than the outer diameter of the tube, and rotating the tube. The speed of the steel tube in the traveling direction during bending and unbending was 0.02 m / s, and it was confirmed that the temperature of the outer surface of the tube during processing was 150°C or less.
[0070] After the cold working during rolling, the steel was left as it was, and in some cases, heat treatment was performed at a heat treatment temperature (holding temperature) of 250° C. and a heating holding time of 20 minutes (1200 seconds).
[0071] [Textural observation] Test pieces were cut out from the centre of the wall thickness of the steel pipe after cold working or subsequent heat treatment (centre of the wall thickness in a cross section perpendicular to the axial direction of the pipe), mirror polished, and then subjected to nital etching. The structure was identified by observing it under an optical microscope at magnifications of 100 to 400 times to confirm whether it was a suitable structure containing a ferrite phase. The fraction of the retained austenite phase can be easily measured by separating the peaks of the body-centered cubic lattice of the ferrite phase and the face-centered cubic lattice of the austenite phase by X-ray diffraction on a mirror-polished test piece. The volume fraction of the retained austenite phase was measured by X-ray diffraction, and this was taken as the area fraction of the retained austenite phase. The measurement area was 5 mm 2 The range was set as follows.
[0072] The chemical composition and microstructural observation results for each steel type are shown in Table 1. As shown in Table 1, steel types J, K, and L had retained austenite phase exceeding 10% in the structure, or bubbles in the steel that were thought to be the result of N2 gas were confirmed. Additionally, steel types M and N (No. 27 and 28) had axial tensile yield strengths below 400 MPa after cold working. These steel types M and N (No. 27 and 28, respectively) did not have high mechanical properties even after cold working, so the evaluation of the axial compressive yield strength / axial tensile yield strength and axial fatigue strength described below was not carried out. In addition, steel types J, K, and L (No. 24, 25, and 26, respectively) had poor cold workability or contained defects such as voids in the steel, so cold working was not possible. Therefore, the evaluation of the axial compressive yield strength / axial tensile yield strength and axial fatigue strength, which will be described later, was not carried out for these steel types either.
[0073] [evaluation] The mechanical properties and fatigue properties in the axial direction of the obtained steel pipes were evaluated. The mechanical properties were evaluated by evaluating the tensile and compressive yield strength in the axial direction of the tube, and the fatigue strength (stress ratio R=-1) was measured by applying tensile and compressive stresses alternately. The tensile yield strength and compressive yield strength were evaluated by cutting round bar test pieces with a diameter of 3 mm from the center of the wall thickness parallel to the tube axis direction for the steel pipes after cold working, or for the steel pipes after heat treatment if heat treatment was performed after cold working. Tests were performed at a processing speed of 1.0 mm / min for both tension and compression, and the tensile yield strength and the ratio of compressive yield strength to tensile yield strength (compressive yield strength in the tube axis direction / tensile yield strength in the tube axis direction) were calculated.
[0074] Specifically, the tube axial compressive yield strength was measured by a cylindrical compression test. The cylindrical test piece to be compressed was taken from the center of the wall thickness parallel to the tube axial direction. In addition, the outer diameter d [mm] and the height h [mm] were set to h / d≦2.0. Specifically, a test piece was cut out from the center of the tube wall thickness with an outer diameter d = 3.0 mm and a height h = 5.0 mm. The compression test was performed at room temperature (25°C) by sandwiching the test piece between flat plates and applying a load, and the compressive yield strength was calculated using the stress-strain curve obtained during compression. The stress-strain curve was obtained by compressing the test piece by 30% at a compression speed of 1.0 mm / min using a compression tester.
[0075] The axial tensile yield strength was measured according to JIS Z2241 (2011). First, a round bar tensile test piece with a parallel diameter of 3.0 mm was cut out from the center of the wall thickness of the tube parallel to the axial direction. A tensile test was then performed at room temperature (25°C) at a crosshead speed of 1.0 mm / min until fracture. The tensile yield strength was calculated using the stress-strain curve obtained from this.
[0076] In addition, fatigue strength was investigated using test pieces of the same size. Various tensile and compressive stresses were applied to the evaluation part of a φ3 mm round bar in air at room temperature (25°C) with a stress ratio of R = -1 and a stress loading rate of 2 Hz. The number of times the stress was applied was 10. 7 The stress value obtained by applying the test for more than 1000 times was evaluated as the fatigue strength. The fatigue strength obtained was compared relative to the values obtained by drawing and rolling and bending and backbending for each steel type and cold working condition.
[0077] [Table 2]
[0078] From the results in Table 2, it can be seen that under the conditions in which the bending and unbending process of the present invention was carried out, the difference between the tensile yield strength and the compressive yield strength in the tube axial direction was small compared to the conventional cold rolling method of draw rolling, and the fatigue properties were excellent.
Claims
1. In mass percent, C: 0.01-1.15%, Si: 0.01-2.50%, Mn: 0.01 to 2.50%, N: 0.001 to 0.050%, with the balance being Fe and unavoidable impurities; The steel has a structure having a ferrite phase and a retained austenite phase of 10% or less in area ratio, The axial tensile yield strength is 400 MPa or more, A seamless steel pipe having a ratio of compressive yield strength in the pipe axis direction to tensile yield strength in the pipe axis direction of 0.85 to 1.
15.
2. The component composition further includes, in mass %, Cr: 2.00% or less, 2. The seamless steel pipe according to claim 1, further comprising one or two selected from the group consisting of Mo: 2.00% or less.
3. The component composition further includes, in mass %, Ti: 0.50% or less, Al: 0.30% or less, V: 0.55% or less, The seamless steel pipe according to claim 1 or 2, further comprising one or more selected from the group consisting of Nb: 0.75% or less.
4. The component composition further includes, in mass %, Ni: less than 2.5% W: less than 1.0% Cu: less than 2.5% B: 0.010% or less, Zr: 0.10% or less, Ca: 0.010% or less, Ta: 0.01% or less, REM: 0.10% or less, Mg: 0.10% or less, Sn: 0.30% or less, Sb: 0.30% or less, The seamless steel pipe according to any one of claims 1 to 3, further comprising one or more selected from the group consisting of Ag: 0.30% or less.
5. In mass %, C: 0.01-1.15%, Si: 0.01-2.50%, Mn: 0.01 to 2.50%, N: 0.001 to 0.050%; Or even more so: Cr: 2.00% or less, Mo: 2.00% or less, Ti: 0.50% or less, Al: 0.30% or less, V: 0.55% or less, Nb: 0.75% or less, Ni: less than 2.5% W: less than 1.0% Cu: less than 2.5% B: 0.010% or less, Zr: 0.10% or less, Ca: 0.010% or less, Ta: 0.01% or less, REM: 0.10% or less, Mg: 0.10% or less, Sn: 0.30% or less, Sb: 0.30% or less, Ag: 0.30% or less, The balance is Fe and unavoidable impurities, The steel has a structure having a ferrite phase and a retained austenite phase of 10% or less in area ratio, The axial tensile yield strength is 400 MPa or more, A method for producing a steel pipe having an axial compressive yield strength / axial tensile yield strength of 0.85 to 1.15, comprising bending and unbending a steel pipe material in the circumferential direction to obtain the steel pipe.
6. The method for producing a steel pipe according to claim 5, wherein after the bending and unbending in the pipe circumferential direction, a heat treatment is performed in which the pipe is held at a holding temperature of 300°C or less for 300 seconds or more and less than 3600 seconds, and then air-cooled.
Citation Information
Patent Citations
Weld steel pipe with excellent low-temperature toughness for high-strength thick-walled line pipe and process for producing the same
JP2008163455A
Steel pipe for line pipe with excellent collapse resisting performance
JP2012167329A
Welded steel pipe for sour linepipe and method for manufacturing the same
JP2020193374A
High dimensional precision tube and its manufacturing method
JP4285053B2