Composition for forming underlayer film, pattern forming method, copolymer and monomer for composition for forming underlayer film

The use of a copolymer-based underlayer film composition with sugar derivatives and antireflection units addresses solvent and etching resistance issues, enhancing pattern precision and processability in semiconductor manufacturing.

JP7559861B2Active Publication Date: 2024-10-02OJI HLDG CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023062006
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-07-19
Filing Date
2023-04-06
Publication Date
2024-10-02
Estimated Expiration
2039-02-25

AI Technical Summary

Technical Problem

Conventional underlayer films for semiconductor patterns face issues with low survival rates in organic solvents, high ultraviolet reflectance, and insufficient etching resistance, leading to challenges in maintaining pattern shape and processability during lithography processes.

Method used

A composition for forming an underlayer film containing a copolymer with units derived from sugar derivatives, compounds with antireflection functions, and units capable of cross-coupling, which enhances solvent resistance, reduces ultraviolet reflectance, and improves etching resistance.

Benefits of technology

The composition allows for the formation of underlayer films with high solvent resistance, low ultraviolet reflectance, and excellent etching resistance, enabling precise pattern formation and improved processability on semiconductor substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559861000045
    Figure 0007559861000045
  • Figure 0007559861000001
    Figure 0007559861000001
  • Figure 0007559861000002
    Figure 0007559861000002
Patent Text Reader

Abstract

To provide an underlayer film-forming composition capable of forming an underlayer film, wherein the underlayer film resists being dissolved in an organic solvent, achieving a high remaining ratio, and the underlayer film also has low UV reflectivity and excellent etching resistance.SOLUTION: An underlayer film-forming composition contains a copolymer and an organic solvent and is used for patterning, wherein the copolymer contains: (a) a unit derived from a sugar derivative; (b) a unit derived from a compound having a light antireflection function; and (c) a unit derived from a compound capable of cross-coupling the copolymer, the unit derived from a sugar derivative (a) is at least one selected from a unit derived from a pentose derivative and a unit derived from a hexose derivative, and the underlayer film-forming composition is used for metal introduction.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for forming an underlayer film, a pattern forming method, a copolymer, and a monomer for the composition for forming an underlayer film. [Background technology]

[0002] Electronic devices such as semiconductors are required to be highly integrated by miniaturization, and miniaturization and diversification of shapes of semiconductor device patterns are being considered. As a method for forming such a pattern, a lithography method using a photoresist and a pattern formation method by self-organization using a directed self-assembly material (Directed Self Assembly) are known. For example, the lithography method using a photoresist is a processing method in which a thin film of photoresist is formed on a semiconductor substrate such as a silicon wafer, and the substrate is etched using the photoresist pattern obtained by irradiating the substrate with active light such as ultraviolet light through a mask pattern on which a semiconductor device pattern is drawn, and developing the photoresist pattern as a protective film, thereby forming fine projections and recesses corresponding to the pattern on the substrate.

[0003] In order to form a fine pattern, a method of forming a pattern after forming an underlayer film on a substrate such as a silicon wafer has also been considered. For example, Patent Document 1 describes a composition for forming a resist underlayer film, which contains [A] polysiloxane and [B] solvent, and the solvent [B] contains (B1) tertiary alcohol. Patent Document 2 describes a method for forming a resist underlayer film, which includes a coating step of coating a substrate with the composition for forming a resist underlayer film, and a heating step of heating the resulting coating film at a temperature of more than 450° C. and not more than 800° C. in an atmosphere with an oxygen concentration of less than 1% by volume, and the composition for forming a resist underlayer film contains a compound having an aromatic ring.

[0004] Patent Document 3 describes a composition for forming an underlayer film, which contains a dextrin ester compound in which 50% or more of dextrin is esterified, a crosslinkable compound, and an organic solvent. Patent Document 4 describes a composition for forming an underlayer film for lithography, which contains cyclodextrin containing an inclusion molecule. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-170338 A [Patent Document 2] JP 2016-206676 A [Patent Document 3] International Publication No. 2005 / 043248 [Patent Document 4] JP 2007-256773 A Summary of the Invention [Problem to be solved by the invention]

[0006] After the coating film formed from the composition for forming an underlayer film is heat-treated to become an underlayer film, it is necessary that it is less likely to dissolve in an organic solvent contained in the resist-forming composition, etc. (i.e., the underlayer film survival rate of the material used in the composition for forming an underlayer film is high.) However, it is difficult to say that the underlayer film survival rate of an underlayer film formed using a conventional composition for forming an underlayer film is sufficiently high.

[0007] After forming a pattern on the underlayer film, an etching process may be performed to process the pattern shape on a silicon wafer substrate using the pattern as a protective film, but the protective film formed using a conventional composition for forming an underlayer film does not have sufficient etching resistance, and there remains a problem with the pattern processability on the substrate. In addition, when forming a pattern on the underlayer film, a pattern may be formed using a resist, but the underlayer film formed using a conventional composition for forming an underlayer film may have a high ultraviolet reflectance, and there remains a problem with maintaining the pattern shape when forming a resist pattern by exposure.

[0008] Therefore, in order to solve such problems of the conventional technology, the inventors have conducted research with the aim of providing a composition for forming an underlayer film that can form an underlayer film that has a high residual rate in organic solvents, a low ultraviolet reflectance, and excellent etching resistance. [Means for solving the problem]

[0009] As a result of intensive research to solve the above problems, the inventors have found that by using a copolymer containing (a) units derived from a sugar derivative, (b) units derived from a compound having anti-reflection function, and (c) units derived from a compound capable of cross-coupling the copolymer as a material for a composition for forming an underlayer film, it is possible to form an underlayer film that has a high residual rate in organic solvents, a low ultraviolet reflectance, and excellent etching resistance, and have thus completed the present invention. Specifically, the present invention has the following configuration.

[0010] [1] A composition for forming an underlayer film used in pattern formation, comprising a copolymer and an organic solvent, The copolymer is (a) a unit derived from a sugar derivative; (b) a unit derived from a compound having an antireflection function; (c) units derived from compounds capable of cross-coupling the copolymer, (a) the unit derived from a sugar derivative is at least one selected from a unit derived from a pentose derivative and a unit derived from a hexose derivative; The composition for forming an underlayer film is for introducing a metal. [2] The composition for forming an underlayer film according to [1], wherein (b) the unit derived from a compound having an antireflection function is a unit derived from an aromatic ring-containing compound, and (c) the unit derived from a compound capable of cross-coupling a copolymer is a unit derived from a (meth)acrylate. [3] The composition for forming an undercoat film according to [1] or [2], wherein (a) the unit derived from a sugar derivative is at least one selected from the group consisting of a unit derived from a cellulose derivative, a unit derived from a hemicellulose derivative, and a unit derived from a xylooligosaccharide derivative. [4] The composition for forming an underlayer film according to [2] or [3], wherein the unit derived from an aromatic ring-containing compound is at least one selected from the group consisting of a unit derived from a benzene ring-containing compound and a unit derived from a naphthalene ring-containing compound. [5] The composition for forming an underlayer film according to any one of [2] to [4], wherein the unit derived from (meth)acrylate has at least one selected from an alkyl group which may have a substituent and an aryl group which may have a substituent. [6] The composition for forming an underlayer film according to any one of [2] to [5], wherein the unit derived from (meth)acrylate has an alkyl group which may have a substituent, and the alkyl group has 1 to 8 carbon atoms. [7] A pattern forming method comprising a step of forming an underlayer film using the composition for forming an underlayer film according to any one of [1] to [6]. [8] The pattern forming method according to [7], further comprising the step of introducing a metal into the underlayer film. [9] (a) a unit derived from a sugar derivative; (b) a unit derived from a compound having an antireflection function; (c) units derived from compounds capable of cross-coupling the copolymer, (a) A copolymer in which the unit derived from a sugar derivative is at least one selected from the group consisting of a unit derived from a pentose derivative and a unit derived from a hexose derivative.

[10] The copolymer according to [9], wherein (b) the unit derived from a compound having an antireflection function is a unit derived from an aromatic ring-containing compound, and (c) the unit derived from a compound capable of cross-coupling the copolymer is a unit derived from a (meth)acrylate.

[11] A monomer for a composition for forming an underlayer film, represented by the following general formula (1') or the following general formula (2'): [ka] In general formula (1'), R 1 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group; 1 may be the same or different; R' is a hydrogen atom, -OR 11 or -NR 12 Represents 2; R" is a hydrogen atom, -OR 11 , -COOR 13 or -CH2OR 13 where R 11 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group; R 12 represents a hydrogen atom, an alkyl group, a carboxyl group, or an acyl group, and there are multiple R 12 may be the same or different, R 13 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group; R 5 represents a hydrogen atom or an alkyl group; Y 1 each independently represents a single bond or a linking group; [ka] In general formula (2'), R 201each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group; 201 may be the same or different; R' is a hydrogen atom, -OR 11 or -NR 12 Represents 2; R" is a hydrogen atom, -OR 11 , -COOR 13 or -CH2OR 13 where R 11 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group; R 12 represents a hydrogen atom, an alkyl group, a carboxyl group, or an acyl group, and there are multiple R 12 may be the same or different, R 13 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group. Effect of the Invention

[0011] According to the present invention, it is possible to form an underlayer film that has a high residual rate in organic solvents, a low ultraviolet reflectance, and excellent etching resistance. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the structure of a substrate and an underlying film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "~" means a range including the numerical values ​​before and after "~" as the lower and upper limits.

[0014] In this specification, the term "(meth)acrylate" means that the group may have any substituent unless otherwise specified as substituted or unsubstituted. In addition, in this specification, the term "(meth)acrylate" means that the group includes both "acrylate" and "methacrylate".

[0015] (Composition for forming lower layer film) The present invention relates to a composition for forming an underlayer film, which comprises a copolymer and an organic solvent and is used for pattern formation. The copolymer comprises (a) a unit derived from a sugar derivative, (b) a unit derived from a compound having an antireflection function, and (c) a unit derived from a compound capable of cross-coupling the copolymer. (a) The unit derived from the sugar derivative is at least one selected from a unit derived from a pentose derivative and a unit derived from a hexose derivative, and the composition for forming an underlayer film is for introducing a metal.

[0016] The composition for forming an underlayer film of the present invention is an underlayer film having a high residual rate in an organic solvent, and can form an underlayer film having low ultraviolet reflectance and excellent etching resistance. The underlayer film formed from the composition for forming an underlayer film of the present invention has low ultraviolet reflectance, so that when a resist film is formed on the underlayer film and exposed to form a pattern, a pattern can be formed with high accuracy, and the pattern shape is easily maintained. In addition, the underlayer film formed from the composition for forming an underlayer film of the present invention has excellent etching resistance, so that the etching processability of a substrate or the like can be improved. Furthermore, since the copolymer contained in the composition for forming an underlayer film of the present invention contains the above-mentioned multiple structural units, it is highly soluble in an organic solvent, while it is also characterized in that after it is cured to become an underlayer film, it remains without being dissolved in the organic solvent contained in the resist forming composition or the like.

[0017] The units derived from the sugar derivative contained in the copolymer (hereinafter also referred to as units (a)) contain many crosslinking reaction sites, and therefore tend to be easily accelerated in crosslinking by heating (regardless of whether a crosslinking agent is added or not). This makes it possible to increase the survival rate of the underlayer film after the coating film is heat-treated to form an underlayer film. In other words, after the coating film formed from the composition for forming an underlayer film is heat-treated to form an underlayer film, the solubility of the copolymer in organic solvents can be reduced. Furthermore, the copolymer having units (a) can also improve etching processability.

[0018] The underlayer film residual rate is preferably 90% or more, more preferably 93% or more, and even more preferably 95% or more. Here, the underlayer film residual rate is a value calculated by the following formula from the thickness of the underlayer film before and after coating the underlayer film with a 50:50 (mass ratio) mixed solution of propylene glycol monomethyl ether acetate and propylene glycol monomethyl ether, which is a solvent used in photoresists (before and after cleaning). Underlayer film remaining rate (%) = underlayer film thickness after cleaning (μm) / underlayer film thickness before cleaning (μm) × 100

[0019] The etching processability can be evaluated by the following method. First, the composition for forming an underlayer film is applied to a silicon substrate to form an underlayer film, and the underlayer film is then patterned into a line-and-space shape, and the silicon substrate is etched. The patterned surface of the silicon substrate is then observed with a scanning electron microscope to confirm the state of the etching processability. If the pattern shape of the silicon substrate is in a state where there is no line collapse in one visual field of the scanning electron microscope, the etching processability can be determined to be good.

[0020] In addition, the composition for forming an underlayer film of the present invention can introduce a large amount of metal into the underlayer film by the copolymer having the unit (a). Therefore, it can be said that the composition for forming an underlayer film of the present invention is a material for introducing metal. The copolymer contained in the composition for forming an underlayer film can form an underlayer film containing a metal by reacting (bonding) with a metal. Such an underlayer film becomes harder than an underlayer film not containing a metal, and can thereby exhibit excellent etching processability. Here, the copolymer contained in the composition for forming an underlayer film is preferably one that reacts (bonds) with a metal at multiple sites in one copolymer molecule, and the more reaction (bonding) sites with the metal, the higher the metal introduction rate. In the present invention, the metal introduction rate is increased by reacting (bonding) the oxygen atom and the metal atom contained in the copolymer, and such a high metal introduction rate is achieved by the copolymer having the unit (a). The bond between the oxygen atom and the metal atom contained in the copolymer is not particularly limited, but for example, it is preferable that the oxygen atom and the metal atom contained in the copolymer are coordinately bonded or ionically bonded.

[0021] The metal introduction rate in the underlayer film is preferably 5 at% (atomic percent) or more, more preferably 8 at% or more, even more preferably 10 at% or more, and even more preferably 15 at% or more. The metal introduction rate can be calculated, for example, by the following method. First, the underlayer film formed from the composition for forming the underlayer film is placed in an ALD (atomic layer deposition apparatus), and Al(CH3)3 gas is introduced therein at 95°C, and then water vapor is introduced. This operation is repeated three times to introduce Al into the underlayer film. The underlayer film after the introduction of Al is subjected to EDX analysis (energy dispersive X-ray analysis) using an electron microscope JSM7800F (manufactured by JEOL Ltd.), and the ratio of the Al component (Al content) is calculated, which is the metal introduction rate.

[0022] The unit derived from the compound having the light antireflection function possessed by the copolymer (hereinafter also referred to as unit (b)) has the property of absorbing light. Regarding the light antireflection function of unit (b), a coating film having a thickness of 0.1 μm is formed from a coating solution consisting of a monomer of unit (b) and a solvent, and the coating film is irradiated with ultraviolet light (for example, ultraviolet light having a wavelength of 193 nm). If the reflectance is 30% or less, it can be evaluated that unit (b) has a light antireflection function. The reflectance of the coating film can be evaluated by measuring it with a spectrophotometer. As the spectrophotometer, for example, V770EX manufactured by JASCO Corporation can be used, and it is preferable to perform the measurement with an integrating sphere installed on the spectrophotometer. If the coating film cannot be formed from the monomer of unit (b), the coating film may be formed from a coating solution containing a polymer composed of unit (b).

[0023] The copolymer has the unit (b), so that the underlayer film formed from the composition for forming the underlayer film can exhibit an antireflection function. Therefore, when a resist film is formed on the underlayer film and exposed to form a pattern, a pattern shape can be formed with high accuracy. The antireflection function of the underlayer film can be evaluated by irradiating the underlayer film with ultraviolet light (for example, ultraviolet light with a wavelength of 193 nm) and measuring the reflectance with a spectrophotometer. As the spectrophotometer, for example, V770EX manufactured by JASCO Corporation can be used, and it is preferable to perform the measurement with an integrating sphere installed in the spectrophotometer. The ultraviolet light reflectance (light reflectance) of the underlayer film is preferably 50% or less, more preferably 30% or less, and even more preferably 20% or less.

[0024] Furthermore, the copolymer has a unit (hereinafter also referred to as unit (c)) derived from a compound capable of cross-coupling the copolymer, which can promote the cross-coupling reaction of the copolymer. Cross-coupling refers to the bonding of the copolymer in the composition for forming the underlayer film by heating or photoreaction, or the bonding of functional groups in the copolymer. This can increase the residual rate of the underlayer film in organic solvents, and can further increase the etching processability. In addition, the copolymer has unit (c), which can form an underlayer film that is less likely to crack when heated in air at a relatively low temperature. For example, even when the underlayer film is placed under harsh conditions such as high temperature conditions, the occurrence of cracks is suppressed.

[0025] The presence or absence of the unit (c) in the copolymer can be determined by detecting the change in the peak of the functional group before and after the underlayer film-forming composition is cured by FT-IR. For example, if the compound capable of cross-coupling the copolymer is glycidyl methacrylate, the copolymer is cross-coupled by curing the underlayer film-forming composition, and the peak of the functional group changes by FT-IR. -1 The peak at 1106 cm disappears. -1 Peaks derived from ether groups in the vicinity and 3160 to 3600 cm -1 A peak derived from a hydroxyl group in the vicinity of the cross-coupling reaction site is detected. This allows the occurrence of cross-coupling of the copolymer. Specifically, the peak height of a functional group that does not change, such as a methyl group, is used as the reference functional group, and the cross-coupling reaction rate is calculated from the ratio of the peak height that disappears due to cross-coupling. When the cross-coupling reaction rate is 95% or less, it can be determined that cross-coupling of the copolymer has occurred, that is, that the copolymer contains unit (c). Cross-coupling reaction rate (%) = (peak height of functional group derived from cross-coupling group after curing / peak height of reference functional group) / (peak height of functional group derived from cross-coupling group before curing / peak height of reference functional group) x 100

[0026] The underlayer film formed from the underlayer film forming composition of the present invention is, for example, a film (protective film) provided on a substrate such as a silicon wafer in order to form a pattern on the substrate. The underlayer film may be a film provided so as to be in direct contact with the substrate, or may be a film laminated on the substrate via another layer. The underlayer film is processed into a pattern shape to be formed on the substrate, and the part remaining as the pattern shape becomes a protective film in the subsequent etching process. After the pattern is formed on the substrate, the underlayer film (protective film) is generally removed from the substrate. In this way, the underlayer film is used in the process of forming a pattern on the substrate.

[0027] The underlayer film formed from the composition for forming an underlayer film of the present invention exhibits excellent etching resistance when processing a pattern shape on a substrate, and the etching resistance of such an underlayer film can be evaluated, for example, by the etching selectivity ratio calculated by the following formula. Etching selectivity = maximum depth of etched portion of substrate / (average thickness of underlayer film before etching - average thickness of underlayer film after etching) The depth of the etched portion of the substrate and the thickness of the underlayer film before and after the etching process can be measured, for example, by observing the cross section of the substrate with a scanning electron microscope (SEM). The depth of the etched portion of the substrate is the maximum depth of the portion removed by the etching process, and the thickness of the underlayer film before and after the etching process is the maximum thickness of the remaining portion of the underlayer film. The etching selectivity calculated as above is preferably greater than 1.5, more preferably 2 or more, even more preferably 3 or more, and even more preferably 4 or more. The upper limit of the etching selectivity is not particularly limited, but can be, for example, 200.

[0028] The composition for forming an underlayer film of the present invention may be used as a material for forming a photomask for forming a pattern. A photomask is formed by forming a predetermined pattern on a photomask substrate and then performing processes such as etching and resist stripping.

[0029] <Copolymer> The composition for forming an underlayer film of the present invention contains a copolymer. The copolymer contains units (a), (b) and (c). Here, the units (a) are units derived from a sugar derivative, the units (b) are units derived from a compound having an antireflection function, and the units (c) are units derived from a compound capable of cross-coupling the copolymer. Here, the units (a) are at least one selected from units derived from a pentose derivative and units derived from a hexose derivative. The present invention may also relate to a copolymer containing units (a), (b) and (c).

[0030] The copolymer may be a block copolymer or a random copolymer. The copolymer may have a structure in which a part is a random copolymer and a part is a block copolymer. From the viewpoint of increasing solubility in organic solvents, the copolymer is preferably a block copolymer, and from the viewpoint of promoting crosslinking and increasing strength, the copolymer is preferably a random copolymer. Therefore, an appropriate structure can be selected depending on the application and required physical properties.

[0031] When the copolymer is a block copolymer, it is preferably an ABC-type diblock copolymer containing a polymerized portion a consisting of a unit (a), a polymerized portion b consisting of a unit (b), and a polymerized portion c consisting of a unit (c), but it may also be a block copolymer (e.g., ABCABC type) containing a plurality of each of the polymerized portions a, b, and c.

[0032] The content of the copolymer is preferably 0.1% by mass or more, more preferably 1% by mass or more, based on the total mass of the composition for forming an underlayer film, and is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less, based on the total mass of the composition for forming an underlayer film.

[0033] The copolymer is preferably made of an organic material, which is preferable from the viewpoint of improving adhesion to organic resist materials and the like, compared with a case in which the copolymer contains an organic-inorganic hybrid material such as polysiloxane.

[0034] (Unit (a)) The unit (a) is a unit derived from a sugar derivative, and the unit derived from the sugar derivative is at least one selected from a unit derived from a pentose derivative and a unit derived from a hexose derivative. In this way, by introducing a unit derived from a sugar derivative having many oxygen atoms as the unit (a) of the copolymer, a structure that is easy to coordinate with a metal can be obtained, and a metal can be introduced into any of the copolymer, the composition for forming an underlayer film, and the underlayer film formed from the composition for forming an underlayer film by a simple method such as a sequential penetration synthesis method, thereby improving the etching processability. The underlayer film into which the metal has been introduced in this way can become a mask with higher performance in the lithography process.

[0035] The sugar derivative may be a sugar derivative derived from a monosaccharide, or may have a structure in which multiple sugar derivatives derived from monosaccharides are bonded. When the copolymer is a block copolymer, the polymerized part a consisting of the unit (a) has a structure in which multiple sugar derivatives derived from monosaccharides are bonded.

[0036] The unit derived from a sugar derivative is at least one selected from a unit derived from a pentose derivative and a unit derived from a hexose derivative. The pentose derivative is not particularly limited as long as it has a structure derived from a pentose in which the hydroxyl group of the pentose of a known monosaccharide or polysaccharide is modified with at least a substituent. The pentose derivative is preferably at least one selected from a hemicellulose derivative, a xylose derivative, and a xylooligosaccharide derivative, and more preferably at least one selected from a hemicellulose derivative and a xylooligosaccharide derivative. The hexose derivative is not particularly limited as long as it has a structure derived from a known monosaccharide or polysaccharide hexose in which the hydroxyl group is modified with at least a substituent. The hexose derivative is preferably at least one selected from glucose derivatives and cellulose derivatives, and more preferably a cellulose derivative. In particular, the unit (unit (a)) derived from a sugar derivative is preferably at least one selected from the group consisting of a unit derived from a cellulose derivative, a unit derived from a hemicellulose derivative, and a unit derived from a xylooligosaccharide derivative. Of these, it is more preferred that the polymer contains a unit derived from a xylooligosaccharide derivative, since the unit has a high intramolecular oxygen atom content and many metal-binding sites.

[0037] The unit derived from the sugar derivative may be a structural unit having a sugar derivative-derived structure in the side chain, or may be a structural unit having a sugar derivative-derived structure in the main chain. When the unit derived from the sugar derivative is a structural unit having a sugar derivative-derived structure in the side chain, the unit derived from the sugar derivative is preferably a structure represented by general formula (1) described later. When the unit derived from the sugar derivative is a structural unit having a sugar derivative-derived structure in the main chain, the unit derived from the sugar derivative is preferably a structure represented by general formula (2) described later. Among them, from the viewpoint of preventing the main chain from becoming too long and easily increasing the solubility of the copolymer in an organic solvent, the unit derived from the sugar derivative is preferably a structure represented by general formula (1). In addition, in general formulas (1) and (2), the structure of the sugar derivative is described as a cyclic structure, but the structure of the sugar derivative may be not only a cyclic structure but also an open-ring structure (chain structure) called an aldose or ketose.

[0038] The structure represented by general formula (1) will be described below.

[0039] [ka]

[0040] In general formula (1), R 1each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group, the alkyl group including a sugar derivative group, 1 may be the same or different. R' is a hydrogen atom, -OR 11 or -NR 12 Represents 2. R" is a hydrogen atom, -OR 11 , -COOR 13 or -CH2OR 13 Here, R 11 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group; R 12 represents a hydrogen atom, an alkyl group, a carboxyl group, or an acyl group, and there are multiple R 12 may be the same or different, R 13 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group. R 5 represents a hydrogen atom or an alkyl group. X 1 and Y 1 each independently represents a single bond or a linking group.

[0041] In general formula (1), R 1 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group, the alkyl group including a sugar derivative group, 1 may be the same or different. Among them, R 1 are preferably each independently a hydrogen atom or an acyl group having 1 to 3 carbon atoms. When the above alkyl group is an alkyl group having a substituent, such an alkyl group contains a sugar derivative group, and therefore the sugar chain portion may further have a unit derived from a linear or branched sugar derivative. The unit derived from a linear or branched sugar derivative is preferably a sugar derivative having the same structure as the sugar derivative to which it is bound. That is, R″ in the structure represented by the general formula (1) is a hydrogen atom, —OR 11 , carboxyl group, -COOR 13 When the sugar chain portion (sugar derivative) further has a unit derived from a linear or branched sugar derivative, the unit preferably has a unit derived from a pentose derivative. 13 When the sugar chain portion (sugar derivative) further comprises a unit derived from a linear or branched sugar derivative, it preferably comprises a unit derived from a hexose derivative. The further substituent that the hydroxyl group of the unit derived from a linear or branched sugar derivative may have is R 1 The range is similar to that of

[0042] In general formula (1), R 1 or more preferably further has a sugar derivative group as at least one alkyl group, i.e., forms a structure in which a plurality of units derived from sugar derivatives derived from monosaccharides are bonded, from the viewpoint of reducing the solubility of the copolymer in organic solvents. In this case, the average degree of polymerization of the sugar derivative (meaning the number of bonds of sugar derivatives derived from monosaccharides) is preferably 1 or more and 20 or less, more preferably 15 or less, and even more preferably 12 or less.

[0043] R 1 When is an alkyl group or an acyl group, the number of carbon atoms can be appropriately selected depending on the purpose. For example, the number of carbon atoms is preferably 1 or more, and is preferably 200 or less, more preferably 100 or less, even more preferably 20 or less, and particularly preferably 4 or less.

[0044] R 1Specific examples of the alkyl group include acyl groups such as acetyl, propanoyl, butyryl, isobutyryl, valeryl, isovaleryl, pivaloyl, hexanoyl, octanoyl, chloroacetyl, trifluoroacetyl, cyclopentanecarbonyl, cyclohexanecarbonyl, benzoyl, methoxybenzoyl, and chlorobenzoyl; alkyl groups such as methyl, ethyl, n-propyl, n-butyl, i-butyl, and t-butyl; and trimethylsilyl. Among these, methyl, ethyl, acetyl, propanoyl, n-butyryl, isobutyryl, benzoyl, and trimethylsilyl groups are preferred, and acetyl and propanoyl groups are particularly preferred.

[0045] In the general formula (1), R' is a hydrogen atom, -OR 11 or -NR 12 Represents 2. R 11 R represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group. 11 When R is an alkyl group or an acyl group, the number of carbon atoms can be appropriately selected depending on the purpose. For example, the number of carbon atoms is preferably 1 or more, and is preferably 200 or less, more preferably 100 or less, even more preferably 20 or less, and particularly preferably 4 or less. 11 R is preferably a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, an acyl group having 1 to 3 carbon atoms, or a trimethylsilyl group. 11Specific examples of the alkyl group include acyl groups such as acetyl, propanoyl, butyryl, isobutyryl, valeryl, isovaleryl, pivaloyl, hexanoyl, octanoyl, chloroacetyl, trifluoroacetyl, cyclopentanecarbonyl, cyclohexanecarbonyl, benzoyl, methoxybenzoyl, and chlorobenzoyl; alkyl groups such as methyl, ethyl, n-propyl, n-butyl, i-butyl, and t-butyl; and trimethylsilyl. Among these, methyl, ethyl, acetyl, propanoyl, n-butyryl, isobutyryl, benzoyl, and trimethylsilyl groups are preferred, and methyl, acetyl, and propanoyl groups are particularly preferred. R 12 represents a hydrogen atom, an alkyl group, a carboxyl group, or an acyl group. 12 may be the same or different. Among them, R 12 is preferably a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, a carboxyl group, or -COCH3. Preferred structures for R' are -H, -OH, -OAc, -OCOC2H5, -OCOC6H5, -NH2, -NHCOOH, -NHCOCH3, more preferred structures for R' are -H, -OH, -OAc, -OCOC2H5, -NH2, and particularly preferred structures for R' are -OH, -OAc, -OCOC2H5.

[0046] In the general formula (1), R″ is a hydrogen atom, —OR 11 , carboxyl group, -COOR 13 or -CH2OR 13 Represents R 13 R represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group. 13 When R is an alkyl group or an acyl group, the number of carbon atoms can be appropriately selected depending on the purpose. For example, the number of carbon atoms is preferably 1 or more, and is preferably 200 or less, more preferably 100 or less, even more preferably 20 or less, and particularly preferably 4 or less. 13is preferably a hydrogen atom, an alkyl acyl group having 1 to 3 carbon atoms, or a trimethylsilyl group. R 11 Specific examples of the alkyl group include acetyl, propanoyl, butyryl, isobutyryl, valeryl, isovaleryl, pivaloyl, hexanoyl, octanoyl, chloroacetyl, trifluoroacetyl, cyclopentanecarbonyl, cyclohexanecarbonyl, benzoyl, methoxybenzoyl, and chlorobenzoyl acyl groups; alkyl groups such as methyl, ethyl, n-propyl, n-butyl, i-butyl, and t-butyl; and trimethylsilyl groups. Among these, methyl, ethyl, acetyl, propanoyl, n-butyryl, isobutyryl, benzoyl, and trimethylsilyl groups are preferred, with acetyl and propanoyl being particularly preferred. Preferred structures for R" are -H, -OAc, -OCOC2H5, -COOH, -COOCH3, -COOC2H5, -CH2OH, -CH2OAc, -CH2OCOC2H5; more preferred structures for R" are -H, -OAc, -OCOC2H5, -COOH, -CH2OH, -CH2OAc, -CH2OCOC2H5; and particularly preferred structures for R" are -H, -CH2OH, -CH2OAc.

[0047] In general formula (1), R 5 represents a hydrogen atom or an alkyl group. 5 is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and particularly preferably a hydrogen atom or a methyl group.

[0048] In general formula (1), X 1 and Y 1 each independently represents a single bond or a linking group. X 1 When is a linking group, X 1 Examples of the X include an alkylene group, -O-, -NH2-, and a carbonyl group. 1is preferably a single bond or an alkylene group having 1 to 6 carbon atoms, and more preferably an alkylene group having 1 to 3 carbon atoms. Y 1 When is a linking group, Y 1 Examples of Y include groups containing an alkylene group, a phenylene group, -O-, -C(=O)O-, etc. 1 may be a linking group combining these groups. 1 is preferably a linking group represented by the following structural formula: [ka]

[0049] In the above structural formula, the * symbol indicates the bonding site with the main chain, and the * symbol indicates the bonding site with the sugar unit of the side chain.

[0050] The structure represented by general formula (2) will be described below.

[0051] [ka]

[0052] In general formula (2), R 201 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group; 201 may be the same or different. R' is a hydrogen atom, -OR 11 or -NR 12 Represents 2. R" is a hydrogen atom, -OR 11 , -COOR 13 or -CH2OR 13 Here, R 11 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group; R 12 represents a hydrogen atom, an alkyl group, a carboxyl group, or an acyl group, and there are multiple R 12may be the same or different, R 13 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group. * indicates R 201 Instead of R 201 represents the bonding site with any one of the oxygen atoms to which it is bonded.

[0053] In general formula (2), R 201 The preferred range of R, R′, and R″ is 1 The preferred ranges of R, R′, and R″ are the same as those of R′, R″.

[0054] In addition, the polymer after polymerization is 1 , R', R" are reduced back to hydrogen atoms, and R 1 , R 11 can be hydrogen, provided that R 1 and R 11 does not all need to be reduced.

[0055] (Unit (b)) The unit (b) is a unit derived from a compound having an antireflection function. In the present invention, the compound having an antireflection function is preferably a compound having a property of strongly absorbing ultraviolet rays, such as an aromatic ring-containing compound.

[0056] When the compound having the light antireflection function is an aromatic ring-containing compound, the unit (b) is a unit that exhibits hydrophobicity compared with the unit (a), and therefore serves to increase the solubility of the copolymer, which is a material of the composition for forming the underlayer film, in an organic solvent. That is, the copolymer is prevented from remaining undissolved in the composition for forming the underlayer film. In addition, it is preferable that the unit (b) is a unit derived from an aromatic ring-containing compound from the viewpoint of increasing the underlayer film residual rate when the underlayer film is formed without unnecessarily affecting the crosslinking property. In this way, when the compound having the light antireflection function is an aromatic ring-containing compound, the copolymer contained in the composition for forming the underlayer film can exhibit the characteristic that it has high solubility in organic solvents before film formation, but is difficult to dissolve in organic solvents after film formation.

[0057] Among them, the unit (b) is preferably at least one selected from a unit derived from a benzene ring-containing compound and a unit derived from a naphthalene ring-containing compound, and among them, the unit (b) is particularly preferably a unit derived from a benzene ring-containing compound.

[0058] The unit (b) is preferably a unit having a structure represented by the following general formula (3) or (4). [ka] [ka]

[0059] In the general formulas (3) and (4), R 5 represents a hydrogen atom or an alkyl group. X 1 represents a single bond or a linking group. R 50 represents an organic group or a hydroxyl group. In general formula (3), n represents an integer of 0 to 5, and in general formula (4), n represents an integer of 0 to 7.

[0060] In the general formulas (3) and (4), R 5 and X 1 The preferred range of R in general formula (1) is 5 and X 1 The preferred range is the same as that of the above.

[0061] In the general formulas (3) and (4), R 50 When R is an organic group, 50 is preferably a hydrocarbon group which may have a substituent, and is preferably an alkyl group which may have a substituent. Examples of the hydrocarbon group which may have a substituent include a hydrocarbon group in which any of the carbon atoms constituting the hydrocarbon group is substituted with an oxygen atom, a silicon atom, a nitrogen atom, a sulfur atom, a halogen atom, or the like. For example, R 50may be a trimethylsilyl group, a pentamethyldisilyl group, a trifluoromethyl group, or a pentafluoroethyl group.

[0062] In general formula (3), n represents an integer of 0 to 5, preferably an integer of 0 to 3, and particularly preferably 0. In general formula (4), n represents an integer of 0 to 7, preferably an integer of 0 to 5, more preferably an integer of 0 to 3, and particularly preferably 0.

[0063] (Unit (c)) The unit (c) is a unit derived from a compound capable of cross-coupling the copolymer. In the present invention, the unit derived from a compound capable of cross-coupling the copolymer is preferably a unit derived from a (meth)acrylate.

[0064] The unit derived from a (meth)acrylate is preferably, for example, a unit represented by the following general formula (5). [ka]

[0065] In general formula (5), R 5 represents a hydrogen atom or an alkyl group, R 60 represents an alkyl group which may have a substituent or an aryl group which may have a substituent.

[0066] In general formula (5), R 5 is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and particularly preferably a hydrogen atom or a methyl group.

[0067] The unit (c) preferably has at least one selected from an alkyl group which may have a substituent and an aryl group which may have a substituent. That is, in the general formula (5), R 60 represents an alkyl group which may have a substituent or an aryl group which may have a substituent. 60 may be a combination of the above groups.

[0068] Among them, the unit (c) preferably contains an alkyl group which may have a substituent. That is, R 60 is preferably an alkyl group which may have a substituent. The number of carbon atoms in the alkyl group is preferably 1 to 8, more preferably 1 to 5, and even more preferably 1 to 3. 60 is also preferably an alkyl group having no substituent, and the above carbon number is the number of carbon atoms excluding the number of carbon atoms of the substituent.

[0069] Examples of the substituent that the substituted alkyl group may have include an isocyanate group, an epoxy group, a (meth)acryloyl group, a hydroxymethylamino group, and an alkoxymethylamino group. Such a substituent may be a cross-coupling group, and may form a cross-coupling structure by self-condensation of the copolymer alone by heating or by cross-linking in the presence of a catalyst or the like. For example, in an alkyl group having an epoxy group as a substituent, a ring-opening reaction of the epoxy group occurs in the presence of an acid catalyst, which causes a cross-linking reaction. In this case, the above-mentioned unit (c) can strengthen the formed underlayer film by a cross-linking reaction. Examples of the alkyl group having a substituent include, for example, -CH2-OH, -CH2-O-methyl, -CH2-O-ethyl, -CH2-On-propyl, -CH2-O-isopropyl, -CH2-On-butyl, -CH2-O-isobutyl, -CH2-Ot-butyl, -CH2-O-(C=O)-methyl, -CH2-O-(C=O)-ethyl, -CH2-O-(C=O)-propyl, -CH2-O-(C=O)-isopropyl, -CH2-O-(C=O)-n-butyl, -CH2-O-(C=O)-isobutyl, -CH2-O-(C=O)-t-butyl, -CH2-ethylene oxide, -C2H4-OH, -C2H4-O-methyl, -C2H4-O-ethyl, -C2H4-On-propyl, - C2H4-O-isopropyl, -C2H4-O―n-butyl, -C2H4-O-isobutyl, -C2H4-Ot-butyl, -C2H4-O-(C=O)-methyl, -C2H4-O-(C=O)-ethyl, -C2H4-O-(C=O)-n-propyl, -C2H4-O-(C=O)-isopropyl, -C2H4-O-(C=O)-n-butyl, -C2H4-O-(C=O)-isobutyl, -C2H4-O-(C=O)-t-butyl, -C2H4-O-(C=O)-CH2-(C=O)-methyl, -C2H4-ethylene oxide, -C3H6-ethylene oxide, -C2H4-O-ethylene oxide, -C3H6-O-ethylene oxide, -C4H8-O-ethylene oxide, -C5H 10 Examples include -O-ethylene oxide, -CH2-CH=CH2, -CH2-O-CH=CH2, etc. Furthermore, the alkyl group having a substituent may be a cycloalkyl group or a bridged cyclic cycloalkyl group.

[0070] (Content rate) The content of units (a) in the copolymer (content of sugar derivative units) is preferably from 1% by mass to 95% by mass, more preferably from 5% by mass to 90% by mass, even more preferably from 10% by mass to 85% by mass, and particularly preferably from 20% by mass to 80% by mass, based on the total mass of the copolymer.

[0071] Here, the content of the sugar derivative unit in the copolymer is, for example, 1 It can be determined from H-NMR and the weight average molecular weight of the copolymer. Specifically, it can be calculated using the following formula. Content of unit (a) (mass%) = mass of unit (a) × number of unit (a) (number of monomers) / weight average molecular weight of copolymer

[0072] The content of units (b) in the copolymer is preferably from 1 to 95% by mass, more preferably from 5 to 90% by mass, and even more preferably from 10 to 85% by mass, based on the total mass of the copolymer. The content of units (c) in the copolymer is preferably from 1 to 95% by mass, more preferably from 5 to 90% by mass, and even more preferably from 10 to 85% by mass, based on the total mass of the copolymer. The content of each unit can be calculated in the same manner as the content of unit (a). Cut.

[0073] (Other building blocks) The copolymer may have other structural units in addition to the above structural units, such as a lactic acid-derived unit, a siloxane bond-containing unit, an amide bond-containing unit, or a urea bond-containing unit.

[0074] (Block copolymer structure) When the copolymer is a block copolymer, the block copolymer is preferably an ABC type block copolymer containing a polymerized portion a consisting of a unit (a), a polymerized portion b consisting of a unit (b), and a polymerized portion c consisting of a unit (c), but may also be a block copolymer (e.g., an ABCABC type) containing a plurality of each of the polymerized portions a, b, and C.

[0075] In the block copolymer, each polymerized portion may be linked by a linking group. Examples of such a linking group include -O-, an alkylene group, a disulfide group, and a group represented by the following structural formula. When the linking group is an alkylene group, a carbon atom in the alkylene group may be substituted with a heteroatom, and examples of the heteroatom include a nitrogen atom, an oxygen atom, a sulfur atom, and a silicon atom. In addition, the length of the linking group is preferably shorter than the length of each polymerized portion. [ka]

[0076] In the above structural formula, the marks * and ※ represent bonding sites with each polymerized portion.

[0077] The end group of the main chain of the block copolymer may be, for example, a hydrogen atom or a substituent. The end groups of the main chain may be the same or different. Examples of the substituent include acyl groups such as fluorine atom, chlorine atom, bromine atom, iodine atom, hydroxyl group, amino group, acetyl group, propanoyl group, butyryl group, isobutyryl group, valeryl group, isovaleryl group, pivaloyl group, hexanoyl group, octanoyl group, chloroacetyl group, trifluoroacetyl group, cyclopentanecarbonyl group, cyclohexanecarbonyl group, benzoyl group, methoxybenzoyl group, and chlorobenzoyl group; alkyl groups such as methyl group, ethyl group, propyl group, n-butyl group, sec-butyl group, tert-butyl group, 2-methylbutyronitrile, cyanovalerinoyl group, cyclohexyl-1-carbonitrile group, methylpropanoyl group, and N-butyl-methylpropionamide group; and substituents represented by the structural formula below. The terminal groups of the main chain of the block copolymer are each independently preferably a hydrogen atom, a hydroxyl group, an acetyl group, a propanoyl group, a butyryl group, an isobutyryl group, an n-butyl group, a sec-butyl group, a tert-butyl group, a 2-methylbutyronitrile group, a cyanovalerinoyl group, a cyclohexyl-1-carbonitrile group, a methylpropanoyl group, or a substituent group shown below, and more preferably a hydrogen atom, a hydroxyl group, a butyl group, or a substituent group shown below. [ka] [ka]

[0078] In the above structural formula, the * symbol indicates a bonding site with the block copolymer main chain.

[0079] (Weight average molecular weight of copolymer) The weight average molecular weight (Mw) of the copolymer is preferably 500 or more, more preferably 1000 or more, and even more preferably 1500 or more. The weight average molecular weight (Mw) of the copolymer is preferably 1 million or less, more preferably 500,000 or less, even more preferably 300,000 or less, and even more preferably 250,000 or less. It is preferable that the weight average molecular weight (Mw) of the copolymer is within the above range from the viewpoint of the underlayer film remaining after coating. The weight average molecular weight (Mw) of the copolymer is a value measured in terms of polystyrene by GPC.

[0080] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the copolymer is preferably at least 1. Moreover, Mw / Mn is preferably at most 52, more preferably at most 10, even more preferably at most 8, even more preferably at most 4, and particularly preferably at most 3. It is preferable to set Mw / Mn within the above range from the viewpoint of the underlayer film remaining after coating.

[0081] (Copolymer solubility) The solubility of the copolymer in at least one selected from PGMEA, PGME, THF, butyl acetate, anisole, cyclohexanone, ethyl lactate, N-methylpyrrolidone, γ-butyrolactone and DMF is preferably 1% by mass or more, more preferably 2% by mass or more, particularly preferably 3% by mass or more, and more particularly preferably 4% by mass or more. The upper limit of the solubility of the copolymer in the organic solvent is not particularly limited, but can be, for example, 40% by mass. The solubility is the solubility in at least one selected from PGMEA, PGME, THF, butyl acetate, anisole, cyclohexanone, ethyl lactate, N-methylpyrrolidone, γ-butyrolactone and DMF, and the copolymer used in the present invention preferably has a solubility in any of the organic solvents above a certain value.

[0082] The solubility of the copolymer is measured by gradually adding PGMEA, PGME, THF, butyl acetate, anisole, cyclohexanone, ethyl lactate, N-methylpyrrolidone, γ-butyrolactone or DMF to a given amount of copolymer while stirring, and recording the amount of organic solvent added when the copolymer is dissolved. A magnetic stirrer or the like may be used for stirring. The solubility is then calculated from the following formula. Solubility (mass%) = mass of copolymer / amount of organic solvent when dissolved x 100

[0083] In order to set the solubility of the copolymer in at least one of PGMEA, PGME, THF, butyl acetate, anisole, cyclohexanone, ethyl lactate, N-methylpyrrolidone, γ-butyrolactone and DMF within the above range, for example, it is considered that the unit (b) is a unit derived from an aromatic ring-containing compound. In addition, in order to set the solubility within the above range, it is considered that the content of the unit derived from a sugar derivative is controlled. Specifically, by setting the unit (b) to a unit derived from an aromatic ring-containing compound and setting the content of the unit derived from a sugar derivative (unit (a)) in the copolymer to a certain value or less, the solubility in an organic solvent can be more effectively increased.

[0084] <Method of synthesizing copolymer> The copolymer can be synthesized by known polymerization methods such as living radical polymerization, living anionic polymerization, and atom transfer radical polymerization. For example, in the case of living radical polymerization, a polymerization initiator such as AIBN (α,α'-azobisisobutyronitrile) is used and reacted with a monomer to obtain a copolymer. In the case of living anionic polymerization, a copolymer can be obtained by reacting butyllithium with a monomer in the presence of lithium chloride. Note that, although examples of synthesis using living anionic polymerization or living radical polymerization are shown in this embodiment, the present invention is not limited thereto, and the copolymer can be appropriately synthesized by the above-mentioned synthesis methods or known synthesis methods.

[0085] The copolymer or its raw material may be a commercially available product. For example, homopolymers, random polymers, or block copolymers such as P9128D-SMMAran, P9128C-SMMAran, Poly(methyl methacrylate), P9130C-SMMAran, P7040-SMMAran, and P2405-SMMA manufactured by Polymer Source Corp. may be used. Also, these polymers may be appropriately synthesized by known synthesis methods.

[0086] The polymer part a as described above may be obtained by synthesis, or may be obtained by combining a step of extraction from lignocellulose derived from woody plants or herbaceous plants, etc. When a method of extraction from lignocellulose derived from woody plants or herbaceous plants is adopted to obtain the sugar derivative part of the polymer part a, the extraction method described in JP 2012-100546 A or the like can be used.

[0087] Xylan can be extracted, for example, by the method disclosed in JP-A-2012-180424. Cellulose can be extracted, for example, by the method disclosed in JP 2014-148629 A.

[0088] The polymerized part a is preferably used after modifying the OH group of the sugar part extracted by the above-mentioned method by acetylation, halogenation, etc. For example, when an acetyl group is introduced, an acetylated sugar derivative part can be obtained by reacting with acetic anhydride.

[0089] Polymerization portion b and polymerization portion c may be formed by synthesis, or a commercially available product may be used. When polymerizing polymerization portion b or polymerization portion c, a known synthesis method may be adopted. When using a commercially available product, for example, Amino-terminated PS (Mw=12300 Da, Mw / Mn=1.02, manufactured by Polymer Source Co., Ltd.) may be used.

[0090] The copolymer can be synthesized with reference to Macromolecules Vol.36, No.6, 2003. Specifically, a compound containing polymerized part a and a compound containing polymerized part b are placed in a solvent containing DMF, water, acetonitrile, etc., and a reducing agent is added. Examples of the reducing agent include NaCNBH3. The mixture is then stirred at 30°C to 100°C for 1 day to 20 days, and the reducing agent is appropriately added as necessary. A precipitate is obtained by adding water, and the solid content is vacuum dried to obtain the copolymer.

[0091] In addition to the above-mentioned methods, examples of the copolymer synthesis method include synthesis methods using radical polymerization, RAFT polymerization, ATRP polymerization, click reaction, and NMP polymerization. Radical polymerization is a polymerization reaction that occurs by adding an initiator and generating two free radicals through a thermal or photoreaction. By heating a monomer (e.g., a styrene monomer and a sugar methacrylate compound in which methacrylic acid is added to the β-1 position at the terminal of a xylooligosaccharide) and an initiator (e.g., an azo compound such as azobisbutyronitrile (AIBN)) at 150°C, a polystyrene-polysaccharide methacrylate random copolymer can be synthesized. RAFT polymerization is a radical-initiated polymerization reaction that involves an exchange chain reaction using thiocarbonylthio groups. For example, the OH group at the terminal 1 position of xylooligosaccharides can be converted to a thiocarbonylthio group, and then styrene monomer can be reacted at 30°C to 100°C to synthesize a copolymer (Material Matters vol.5, No.1, Latest Polymer Synthesis, Sigma-Aldrich Japan Co., Ltd.). In ATRP polymerization, the terminal OH group of a sugar is halogenated, and then reacted with a metal complex [(CuCl, CuCl2, CuBr, CuBr2, CuI, etc.) + TPMA (tris(2-pyridylmethyl)amine)], MeTREN (tris[2-(dimethylamino)ethyl]amine), etc.), a monomer (e.g., styrene monomer), and a polymerization initiator (2,2,5-trimethyl-3-(1-phenylethoxy)-4-phenyl-3-azahexane) to synthesize a sugar copolymer (e.g., a sugar-styrene block copolymer). In NMP polymerization, an alkoxyamine derivative is used as an initiator and heated to couple with monomer molecules and produce nitroxides. The polymerization reaction then proceeds as radicals are generated by thermal dissociation. This type of NMP polymerization is a type of living radical polymerization reaction. By mixing monomers (for example, styrene monomers and sugar methacrylate compounds in which methacrylic acid is added to the β-1 position at the end of xylooligosaccharides), using 2,2,6,6-tetramethylpiperidine 1-oxyl (TEMPO) as an initiator, and heating at 140°C, a polystyrene-polysaccharide methacrylate random copolymer can be synthesized. The click reaction is a 1,3-dipolar azide / alkyne cycloaddition reaction using a sugar having a propargyl group and a Cu catalyst. In this case, the polymerized parts may have a linking group having the following structure between them. [ka]

[0092] <Organic solvent> The composition for forming an underlayer film of the present invention contains an organic solvent. However, the composition for forming an underlayer film may further contain an aqueous solvent such as water or various aqueous solutions in addition to the organic solvent. Examples of the organic solvent include alcohol-based solvents, ether-based solvents, ketone-based solvents, sulfur-containing solvents, amide-based solvents, ester-based solvents, and hydrocarbon-based solvents. These solvents may be used alone or in combination of two or more.

[0093] Examples of alcohol-based solvents include methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, sec-butanol, tert-butanol, n-pentanol, i-pentanol, 2-methylbutanol, sec-pentanol, tert-pentanol, 3-methoxybutanol, n-hexanol, 2-methylpentanol, sec-hexanol, 2-ethylbutanol, sec-heptanol, 3-heptanol, n-octanol, 2-ethylhexanol, sec-octanol, n-nonyl alcohol, 2,6-dimethyl-4-heptanol, n-decanol, sec-undecyl alcohol, trimethylnonyl alcohol, sec-tetradecyl alcohol, sec- Examples of the alcohol include heptadecyl alcohol, furfuryl alcohol, phenol, cyclohexanol, methylcyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, and diacetone alcohol; ethylene glycol, 1,2-propylene glycol, 1,3-butylene glycol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 2,4-heptanediol, 2-ethyl-1,3-hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, 1H,1H-trifluoroethanol, 1H,1H-pentafluoropropanol, and 6-(perfluoroethyl)hexanol.

[0094] Examples of polyhydric alcohol partial ether solvents include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, ethylene glycol monophenyl ether, ethylene glycol mono-2-ethylbutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol monohexyl ether, diethylene glycol dimethyl ether, diethylene glycol ethyl methyl ether, propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, and dipropylene glycol monopropyl ether.

[0095] Examples of ether solvents include diethyl ether, dipropyl ether, dibutyl ether, diphenyl ether, and tetrahydrofuran (THF).

[0096] Examples of ketone solvents include acetone, methyl ethyl ketone, methyl-n-propyl ketone, methyl-n-butyl ketone, diethyl ketone, methyl-i-butyl ketone, methyl-n-pentyl ketone, ethyl-n-butyl ketone, methyl-n-hexyl ketone, di-i-butyl ketone, trimethylnonanone, cyclopentanone, cyclohexanone, cycloheptanone, cyclooctanone, methylcyclohexanone, 2,4-pentanedione, acetonylacetone, acetophenone, and furfural.

[0097] An example of the sulfur-containing solvent is dimethyl sulfoxide.

[0098] Examples of amide solvents include N,N'-dimethylimidazolidinone, N-methylformamide, N,N-dimethylformamide, N,N-diethylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpropionamide, and N-methylpyrrolidone.

[0099] Examples of ester-based solvents include diethyl carbonate, propylene carbonate, methyl acetate, ethyl acetate, γ-butyrolactone, γ-valerolactone, n-propyl acetate, i-propyl acetate, n-butyl acetate, i-butyl acetate, sec-butyl acetate, n-pentyl acetate, sec-pentyl acetate, 3-methoxybutyl acetate, methylpentyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, benzyl acetate, cyclohexyl acetate, methylcyclohexyl acetate, n-nonyl acetate, methyl acetoacetate, ethyl acetoacetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, Examples of the monomer include diethylene glycol mono-n-butyl ether acetate, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monobutyl ether acetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol monoethyl ether acetate, glycol diacetate, methoxytriglycol acetate, ethyl propionate, n-butyl propionate, i-amyl propionate, methyl 3-methoxypropionate, diethyl oxalate, di-n-butyl oxalate, methyl lactate, ethyl lactate, n-butyl lactate, n-amyl lactate, diethyl malonate, dimethyl phthalate, and diethyl phthalate.

[0100] Examples of the hydrocarbon solvent include aliphatic hydrocarbon solvents such as n-pentane, i-pentane, n-hexane, i-hexane, n-heptane, i-heptane, 2,2,4-trimethylpentane, n-octane, i-octane, cyclohexane, and methylcyclohexane; and aromatic hydrocarbon solvents such as benzene, toluene, xylene, mesitylene, ethylbenzene, trimethylbenzene, methylethylbenzene, n-propylbenzene, i-propylbenzene, diethylbenzene, i-butylbenzene, triethylbenzene, di-i-propylbenzene, n-amylnaphthalene, and anisole.

[0101] Among these, propylene glycol monomethyl ether acetate (PGMEA), N,N-dimethylformamide (DMF), propylene glycol monomethyl ether (PGME), anisole, ethanol, methanol, acetone, methyl ethyl ketone, hexane, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), 1H,1H-trifluoroethanol, 1H,1H-pentafluoropropanol, 6-(perfluoroethyl)hexanol, ethyl acetate, propyl acetate, butyl acetate, cyclohexanone, furfural, N-methylpyrrolidone, and γ-butyrolactone are more preferred, PGMEA, PGME, THF, butyl acetate, anisole, cyclohexanone, N-methylpyrrolidone, γ-butyrolactone, or DMF are even more preferred, and PGMEA is even more preferred. These solvents may be used alone or in combination of two or more.

[0102] The content of the organic solvent is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on the total mass of the composition for forming an underlayer film. The content of the organic solvent is preferably 99.9% by mass or less, and more preferably 99% by mass or less. By setting the content of the organic solvent within the above range, the coatability of the composition for forming an underlayer film can be improved.

[0103] <Optional ingredients> The composition for forming an underlayer film of the present invention may contain optional components as described below.

[0104] <<Sugar derivative>> The underlayer film-forming composition of the present invention may further contain a sugar derivative in addition to the copolymer. Examples of the sugar derivative include xylose derivatives, xylooligosaccharide derivatives, glucose derivatives, cellulose derivatives, hemicellulose derivatives, etc., and among them, at least one selected from xylooligosaccharide derivatives and glucose derivatives is more preferred.

[0105] The underlayer film-forming composition of the present invention may further contain a monomer containing a structure derived from a sugar derivative in addition to the copolymer. The monomer containing a structure derived from a sugar derivative is preferably represented by general formula (1') or general formula (2') described below. In general formulas (1') and (2'), the structure of the sugar derivative is described as a cyclic structure, but the structure of the sugar derivative may be not only a cyclic structure but also an open-ring structure (chain structure) called an aldose or ketose.

[0106] The structure represented by formula (1') will be described below.

[0107] [ka]

[0108] In general formula (1'), R 1 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group, the alkyl group including a sugar derivative group, 1 may be the same or different. R' is a hydrogen atom, -OR 11 or -NR 12 Represents 2. R" is a hydrogen atom, -OR 11 , -COOR 13 or -CH2OR 13 Here, R11 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group; R 12 represents a hydrogen atom, an alkyl group, a carboxyl group, or an acyl group, 12 may be the same or different, R 13 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group. R 5 represents a hydrogen atom or an alkyl group. Y 1 each independently represents a single bond or a linking group.

[0109] In general formula (1'), R 1 , R', R", R 5 and Y 1 Specific and preferred embodiments of the formula (1) are 1 , R', R", R 5 and Y 1 In order to carry out polymerization effectively, R 1 At least one of these is preferably an acyl group, an aryl group, or a trimethylsilyl group, and more preferably an acyl group, among which -COCH3 and -COC2H5.

[0110] The structure represented by formula (2') will be described below.

[0111] [ka]

[0112] In general formula (2'), R 201 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group; 201 may be the same or different. R' is a hydrogen atom, -OR 11 or -NR 12 Represents 2. R" is a hydrogen atom, -OR 11, -COOR 13 or -CH2OR 13 Here, R 11 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group; R 12 represents a hydrogen atom, an alkyl group, a carboxyl group, or an acyl group, and there are multiple R 12 may be the same or different, R 13 represents a hydrogen atom, an alkyl group, an acyl group, an aryl group, a trimethylsilyl group, or a phosphoryl group.

[0113] In general formula (2), R 201 The preferred range of R, R′, and R″ is 1 The preferred ranges of R, R′, and R″ are the same as those of R′ and R″. 201 At least one of these is preferably an acyl group, an aryl group, or a trimethylsilyl group, and more preferably an acyl group, among which -COCH3 and -COC2H5.

[0114] The present invention may also relate to a monomer for a composition for forming an underlayer film. Specifically, the present invention may relate to a monomer containing a structure derived from a sugar derivative used as a composition for forming an underlayer film, or may relate to a monomer for a composition for forming an underlayer film having a structure represented by general formula (1') or general formula (2').

[0115] <<Crosslinkable compound>> The composition for forming an underlayer film of the present invention may further contain a crosslinking compound. This crosslinking reaction strengthens the formed underlayer film, and can more effectively improve the etching processability.

[0116] The crosslinkable compound is not particularly limited, but a crosslinkable compound having at least two crosslink-forming substituents is preferably used. A compound having two or more, for example, 2 to 6, of at least one type of crosslink-forming substituent selected from an isocyanate group, an epoxy group, a (meth)acryloyl group, a hydroxymethylamino group, and an alkoxymethylamino group can be used as the crosslinkable compound.

[0117] The crosslinkable compound may be a nitrogen-containing compound substituted with a hydroxymethyl group, an alkoxymethyl group, an epoxy group, or a (meth)acryloyl group, and having two or more nitrogen atoms, for example, 2 to 6. Among them, the crosslinkable compound is preferably a nitrogen-containing compound having a nitrogen atom substituted with a group such as a hydroxymethyl group, a methoxymethyl group, an ethoxymethyl group, a butoxymethyl group, or a hexyloxymethyl group. Specific examples of nitrogen-containing compounds include hexamethoxymethylmelamine, tetramethoxymethylbenzoguanamine, 1,3,4,6-tetrakis(butoxymethyl)glycoluril, 1,3,4,6-tetrakis(hydroxymethyl)glycoluril, 1,3-bis(hydroxymethyl)urea, 1,1,3,3-tetrakis(butoxymethyl)urea, 1,1,3,3-tetrakis(methoxymethyl)urea, 1,3-bis(hydroxymethyl)-4,5-dihydroxy-2-imidazolinone, and 1,3-bis(methoxymethyl)-4,5-dimethoxy-2-imidazolinone, dicyclohexylcarbodiimide, diisopropylcarbodiimide, di-tert-butylcarbodiimide, and piperazine.

[0118] Examples of crosslinkable compounds include methoxymethyl type melamine compounds (product names: Cymel 300, Cymel 301, Cymel 303, Cymel 350), butoxymethyl type melamine compounds (product names: Mycoat 506, Mycoat 508), glycoluril compounds (product names: Cymel 1170, Powder Link 1174), methylated urea resins (product names: UFR65), and butylated urea resins (product names: UFR300, U-VAN10), all manufactured by Mitsui Cytec Co., Ltd. Commercially available compounds such as urea / formaldehyde resins (product names: Beckamin J-300S, Beckamin P-955, Beckamin N) manufactured by Dainippon Ink and Chemicals, Inc., (meth)acrylate monomers (product names: SR209, SR272) manufactured by ARKEMA, epoxy acrylate oligomer (CN110NS), and neopentyl glycol diglycidyl ether manufactured by Tokyo Chemical Industry Co., Ltd. can be used. In addition, as the crosslinkable compound, a polymer produced using an acrylamide compound or methacrylamide compound substituted with a hydroxymethyl group or an alkoxymethyl group, such as N-hydroxymethylacrylamide, N-methoxymethylmethacrylamide, N-ethoxymethylacrylamide, or N-butoxymethylmethacrylamide, can be used. The crosslinking compound may be used alone or in combination of two or more kinds.

[0119] These crosslinking compounds can undergo a crosslinking reaction by self-condensation, or can undergo a crosslinking reaction with a structural unit contained in a polymer.

[0120] <<Catalyst>> The underlayer film-forming composition may contain an acid compound such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium-p-toluenesulfonic acid, salicylic acid, sulfosalicylic acid, citric acid, benzoic acid, ammonium dodecylbenzenesulfonate, or hydroxybenzoic acid as a catalyst for promoting the crosslinking reaction. Examples of the acid compound include aromatic sulfonic acid compounds such as p-toluenesulfonic acid, pyridinium-p-toluenesulfonic acid, sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-hydroxybenzenesulfonic acid, benzenedisulfonic acid, 1-naphthalenesulfonic acid, or pyridinium-1-naphthalenesulfonic acid. In addition, an acid generator such as 2,4,4,6-tetrabromocyclohexadienone, benzoin tosylate, 2-nitrobenzyl tosylate, bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate, triphenylsulfonium trifluoromethanesulfonate, phenyl-bis(trichloromethyl)-s-triazine, benzoin tosylate, N-hydroxysuccinimide trifluoromethanesulfonate, bis-(t-butylsulfonyl)diazomethane, or cyclohexylsulfonyldiazomethane can be added.

[0121] <<Anti-reflection agent>> The composition for forming the underlayer film of the present invention may further include a light-reflection preventing agent. Examples of light-reflection preventing agents include compounds having light-absorbing properties. Examples of compounds having light-absorbing properties include those having high absorption ability for light in the photosensitive characteristic wavelength region of the photosensitive component in the photoresist provided on the underlayer film, such as benzophenone compounds, benzotriazole compounds, azo compounds, naphthalene compounds, anthracene compounds, anthraquinone compounds, and triazine compounds. Examples of polymers include polyesters, polyimides, polystyrenes, novolac resins, polyacetals, and acrylic polymers. Examples of polymers having light-absorbing groups linked by chemical bonds include polymers having light-absorbing aromatic ring structures such as anthracene rings, naphthalene rings, benzene rings, quinoline rings, quinoxaline rings, and thiazole rings.

[0122] <<Other Ingredients>> The underlayer film-forming composition may further contain an ionic liquid, a surfactant, etc. By including an ionic liquid in the underlayer film-forming composition, the compatibility between the copolymer and the organic solvent can be increased. By adding a surfactant to the underlayer film forming composition, the coating property of the underlayer film forming composition on the substrate can be improved. In addition, when forming a pattern using the underlayer film forming composition, the coating property of the resist composition that is applied after the underlayer film forming composition can be improved. Preferable surfactants include nonionic surfactants, fluorine-based surfactants and silicone-based surfactants. In addition, any other materials, such as known rheology modifiers and adhesion promoters, may be included in the underlayer film-forming composition.

[0123] The content of the optional components as described above is preferably 10% by mass or less, and more preferably 5% by mass or less, based on the total mass of the composition for forming an underlayer film.

[0124] (lower layer membrane) The present invention may relate to an underlayer film formed from the above-mentioned composition for forming an underlayer film. The underlayer film is a layer provided on a substrate such as a silicon wafer. In this specification, the underlayer film processed into a pattern shape is also called a protective film, and such a protective film is also included in the underlayer film. In other words, the underlayer film includes a layered film before forming a pattern and an intermittent film after forming a pattern.

[0125] FIG. 1(a) shows a laminate in which an underlayer film 20 is formed on a substrate 10. Although not shown, the underlayer film is preferably a layer provided under a resist film, for example. That is, the underlayer film is preferably a layer provided between the substrate and the resist film. The underlayer film can also function as a layer for preventing interaction between the substrate and the resist film, a layer for preventing adverse effects on the substrate of materials used in the resist film or substances generated during exposure of the resist film, a layer for preventing diffusion of substances generated from the substrate during heating and baking into the resist film, and a barrier layer for reducing the poisoning effect of the resist film due to the semiconductor substrate dielectric layer. The underlayer film also functions as a planarizing material for planarizing the substrate surface.

[0126] As shown in FIG. 1(b), at least a part of the underlayer film 20 is removed so as to form a pattern shape to be formed on the substrate 10. For example, a resist film is laminated on the underlayer film 20, and exposure and development processes are performed to form a pattern shape as shown in FIG. 1(b). Thereafter, reactive ion etching such as inductively coupled plasma is performed on the exposed substrate 10 using chlorine gas, boron trichloride, tetrafluoromethane gas, trifluoromethane gas, hexafluoroethane gas, octafluoropropane gas, sulfur hexafluoride gas, argon gas, oxygen gas, helium gas, or the like to form a pattern on the substrate 10 as shown in FIG. 1(c).

[0127] It is also possible to form a self-assembled film or a resist film from the composition for forming an underlayer film of the present invention. When the composition for forming an underlayer film contains a block copolymer, the block copolymer is applied onto a substrate, and annealing or the like is performed to form a film (self-assembled film) having a phase separation structure due to self-organization, and a pattern can be formed by removing a portion of the phase in this self-assembled film. When a resist film is formed from the composition for forming an underlayer film, a resist film formed from the composition for forming an underlayer film is irradiated with far ultraviolet light having a short wavelength through a mask on which a circuit pattern is drawn, and the resist film in the portion exposed to the light is altered to transfer the pattern (exposure). Thereafter, a pattern can be formed by dissolving the exposed portion in a developer.

[0128] The thickness of the underlayer film can be adjusted appropriately depending on the application, but for example, it is preferably from 1 nm to 20,000 nm, more preferably from 1 nm to 10,000 nm, even more preferably from 1 nm to 5,000 nm, and particularly preferably from 1 nm to 3,000 nm.

[0129] The underlayer film is preferably a film into which a metal has been introduced, and thus preferably contains a metal. The metal content of the underlayer film is preferably 5 at% or more, more preferably 8 at% or more, even more preferably 10 at% or more, and even more preferably 15 at% or more. The metal content can be calculated, for example, by the following method. First, the underlayer film is placed in an ALD (atomic layer deposition) apparatus, and Al(CH3)3 gas is introduced therein at 95°C, and then water vapor is introduced. This operation is repeated three times to introduce Al into the underlayer film. The underlayer film after the introduction of Al is subjected to EDX (energy dispersive X-ray analysis) using an electron microscope JSM7800F (manufactured by JEOL Ltd.), and the ratio of the Al component (Al content) is calculated, which is the metal content.

[0130] (Pattern formation method) The present invention also relates to a method for forming a pattern using the above-mentioned composition for forming an underlayer film. The method for forming a pattern of the present invention includes a step of forming an underlayer film using the above-mentioned composition for forming an underlayer film.

[0131] The pattern forming method preferably includes a step of introducing a metal into the underlayer film-forming composition and / or the underlayer film, and more preferably includes a step of introducing a metal into the underlayer film.

[0132] The pattern forming method preferably includes a lithography process before the step of introducing the metal. The lithography process preferably includes a step of forming a resist film on the underlayer film, and a step of removing a part of the resist film and the underlayer film to form a pattern.

[0133] In addition, the method may further include a step of forming a guide pattern on a substrate between the step of forming an underlayer film and the step of forming a resist film. The step of forming a guide pattern on a substrate may be provided before the step of applying the composition for forming an underlayer film. The step of forming a guide pattern is a step of forming a prepattern on the underlayer film formed in the step of applying the composition for forming an underlayer film.

[0134] The pattern forming method preferably includes a step of processing a semiconductor substrate using the above-mentioned pattern as a protective film. Such a step is called an etching step.

[0135] <Process for forming underlayer film> The pattern forming method of the present invention preferably includes a step of forming an underlayer film. The step of forming an underlayer film is a step of applying an underlayer film-forming composition onto a substrate to form an underlayer film.

[0136] Examples of the substrate include glass, silicon, SiO2, SiN, GaN, AlN, etc. Substrates made of organic materials such as PET, PE, PEO, PS, cycloolefin polymer, polylactic acid, and cellulose nanofibers may also be used.

[0137] The substrate and the underlayer film are preferably laminated in this order so that adjacent layers are in direct contact with each other, but other layers may be provided between each layer. For example, an anchor layer may be provided between the substrate and the underlayer film. The anchor layer is a layer that controls the wettability of the substrate and enhances the adhesion between the substrate and the underlayer film. In addition, multiple layers made of different materials may be sandwiched between the substrate and the underlayer film. These materials are not particularly specified, but may include inorganic materials such as SiO2, SiN, Al2O3, AlN, GaN, GaAs, W, SOC, SOG, Cr, Mo, MoSi, Ta, Ni, Ru, TaBN, and Ag, and organic materials such as commercially available adhesives.

[0138] The method of applying the composition for forming an underlayer film is not particularly limited, but for example, the composition for forming an underlayer film can be applied to a substrate by a known method such as spin coating. After applying the composition for forming an underlayer film, the composition for forming an underlayer film may be cured by exposure and / or heating to form an underlayer film. Examples of radiation used for this exposure include visible light, ultraviolet light, far ultraviolet light, X-rays, electron beams, gamma rays, molecular beams, and ion beams. The temperature for heating the coating film is not particularly limited, but is preferably 90°C or higher and 550°C or lower.

[0139] Before applying the composition for forming an underlayer film to the substrate, it is preferable to provide a step of washing the substrate. Washing the substrate surface improves the applicability of the composition for forming an underlayer film. As a washing treatment method, a conventionally known method can be used, for example, oxygen plasma treatment, ozone oxidation treatment, acid-alkali treatment, chemical modification treatment, etc.

[0140] After forming the underlayer film, a heat treatment (baking) is preferably performed to form a layer of the underlayer film from the composition for forming the underlayer film. In the present invention, the heat treatment is preferably performed in the atmosphere at a relatively low temperature. The heat treatment conditions are preferably appropriately selected from a heat treatment temperature of 60° C. to 350° C. and a heat treatment time of 0.3 to 60 minutes. In particular, the heat treatment temperature is more preferably 130° C. to 250° C., and the heat treatment time is more preferably 0.5 to 30 minutes, and even more preferably 0.5 to 5 minutes.

[0141] After the underlayer film is formed, the underlayer film may be rinsed with a rinsing liquid such as a solvent, if necessary. The rinsing process removes uncrosslinked portions and the like in the underlayer film, thereby improving the film formability of a film such as a resist to be formed on the underlayer film. The rinse liquid may be any liquid capable of dissolving the uncrosslinked portions, and solvents such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), ethyl lactate (EL), cyclohexanone, or commercially available thinners may be used. After cleaning, post-baking may be performed to volatilize the rinse liquid. The temperature conditions for this post-baking are preferably 80° C. or higher and 300° C. or lower, and the baking time is preferably 30 seconds or higher and 600 seconds or lower.

[0142] The underlayer film formed from the composition for forming an underlayer film of the present invention has a property of absorbing ultraviolet rays, and therefore can also function as an antireflection film. As will be described later, an antireflection film may be formed separately from the underlayer film. When the underlayer film is used as an antireflection film in a lithography process using a KrF excimer laser (wavelength 248 nm), the composition for forming the underlayer film preferably contains a component having an anthracene ring or a naphthalene ring. When the underlayer film is used as an antireflection film in a lithography process using an ArF excimer laser (wavelength 193 nm), the composition for forming the underlayer film preferably contains a compound having a benzene ring. When the underlayer film is used as an antireflection film in a lithography process using an F2 excimer laser (wavelength 157 nm), the composition for forming the underlayer film preferably contains a compound having a bromine atom or an iodine atom.

[0143] Furthermore, the underlayer film can also function as a layer for preventing interaction between the substrate and the photoresist, a layer for preventing adverse effects on the substrate of materials used in the photoresist or substances generated during exposure of the photoresist, a layer for preventing diffusion of substances generated from the substrate during heating and baking into the upper photoresist, and a barrier layer for reducing the poisoning effect of the photoresist layer due to the dielectric layer of the semiconductor substrate, etc. The underlayer film formed from the composition for forming the underlayer film also functions as a planarizing material for planarizing the substrate surface.

[0144] <Process for forming anti-reflection film> When the pattern formation method is used in a semiconductor manufacturing method, a step of forming an organic or inorganic light antireflection film may be provided before or after the formation of an underlayer film on a substrate. In this case, a light antireflection film may be provided separately from the underlayer film.

[0145] The composition for the antireflection film used to form the antireflection film is not particularly limited, and can be arbitrarily selected from those commonly used in lithography processes. The antireflection film can be formed by a commonly used method, such as coating with a spinner or coater and baking. Examples of the composition for the antireflection film include a composition mainly composed of a light-absorbing compound and a polymer, a composition mainly composed of a polymer having a light-absorbing group linked by a chemical bond and a crosslinking agent, a composition mainly composed of a light-absorbing compound and a crosslinking agent, and a composition mainly composed of a polymeric crosslinking agent having light absorption. These compositions for the antireflection film can also contain an acid component, an acid generator component, a rheology adjuster, and the like, as necessary. The light-absorbing compound can be any compound that has a high absorption ability for light in the photosensitive characteristic wavelength region of the photosensitive component in the photoresist provided on the antireflection film, and examples thereof include benzophenone compounds, benzotriazole compounds, azo compounds, naphthalene compounds, anthracene compounds, anthraquinone compounds, and triazine compounds. Examples of the polymer include polyester, polyimide, polystyrene, novolac resin, polyacetal, acrylic polymer, etc. Examples of the polymer having a light-absorbing group linked by a chemical bond include polymers having a light-absorbing aromatic ring structure such as an anthracene ring, a naphthalene ring, a benzene ring, a quinoline ring, a quinoxaline ring, or a thiazole ring.

[0146] In addition, the substrate to which the underlayer film-forming composition of the present invention is applied may have an inorganic anti-reflection film formed on its surface by a CVD method or the like, and the underlayer film can be formed on top of that.

[0147] <Step of forming resist film> The step of forming the resist film is preferably a step of forming a photoresist layer. The formation of the photoresist layer is not particularly limited, and a well-known method can be adopted. For example, the photoresist layer can be formed by applying a photoresist composition solution onto an underlayer film and baking it.

[0148] The photoresist to be applied and formed on the underlayer film is not particularly limited as long as it is sensitive to the light used for exposure. In addition, both negative photoresists and positive photoresists can be used. There are positive photoresists made of novolac resin and 1,2-naphthoquinone diazide sulfonic acid ester, chemically amplified photoresists made of a binder having a group that decomposes with acid to increase the alkaline dissolution rate and a photoacid generator, chemically amplified photoresists made of a low molecular compound that decomposes with acid to increase the alkaline dissolution rate of the photoresist, an alkali-soluble binder, and a photoacid generator, and chemically amplified photoresists made of a binder having a group that decomposes with acid to increase the alkaline dissolution rate, a low molecular compound that decomposes with acid to increase the alkaline dissolution rate of the photoresist, and a photoacid generator. For example, there are APEX-E (trade name) manufactured by Shipley Co., Ltd., PAR710 (trade name) manufactured by Sumitomo Chemical Co., Ltd., and SEPR430 (trade name) manufactured by Shin-Etsu Chemical Co., Ltd. The composition for forming the underlayer film of the present invention can also be used as a composition for forming a resist film.

[0149] The step of forming the resist film preferably includes a step of exposing through a predetermined mask. For the exposure, a KrF excimer laser (wavelength 248 nm), an ArF excimer laser (wavelength 193 nm), an F2 excimer laser (wavelength 157 nm), EUV (extreme ultraviolet light) (13 nm), or the like can be used. After the exposure, a post exposure bake can be performed as necessary. The post exposure bake is preferably performed under conditions of a heating temperature of 70°C to 150°C and a heating time of 0.3 to 10 minutes.

[0150] The step of forming a resist film preferably includes a step of developing with a developer. As a result, when a positive photoresist is used, for example, the photoresist in the exposed portion is removed to form a photoresist pattern. Examples of the developer include an aqueous alkaline solution such as an aqueous solution of an alkali metal hydroxide such as potassium hydroxide or sodium hydroxide, an aqueous solution of a quaternary ammonium hydroxide such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, or choline, or an aqueous solution of an amine such as ethanolamine, propylamine, or ethylenediamine. Furthermore, a surfactant or the like can be added to these developers. The development conditions are appropriately selected from a temperature of 5 to 50° C. and a time of 10 to 300 seconds.

[0151] The resist film can also be formed by using nanoimprint lithography other than the above photolithography. In the case of nanoimprint lithography, the resist can be formed by applying a photocurable nanoimprint resist, pressing a mold on which a pattern has been formed in advance against the resist, and irradiating the resist with light such as UV light. The resist film may also be a self-assembled film.

[0152] <Patterning process of the underlayer film> In the pattern forming method, it is preferable that a part of the underlayer film is removed using the resist film pattern formed in the above-mentioned resist film forming step as a protective film. Such a step is called a pattern forming step of the underlayer film.

[0153] Examples of methods for removing a portion of the underlayer film include known methods such as reactive ion etching (RIE) such as chemical dry etching and chemical wet etching (wet development), sputter etching, physical etching such as ion beam etching, etc. The removal of the underlayer film is preferably performed by dry etching using a gas such as tetrafluoromethane, perfluorocyclobutane (C4F8), perfluoropropane (C3F8), perfluoroethane (C2F6), boron trichloride, trifluoromethane, trifluoromethane, carbon monoxide, argon, oxygen, nitrogen, chlorine, helium, sulfur hexafluoride, difluoromethane, nitrogen trifluoride, and chlorine trifluoride.

[0154] Also, a chemical wet etching process can be adopted as a process for removing a part of the underlayer film. Examples of the wet etching method include a process of treating the underlayer film by reacting it with acetic acid, a process of treating the underlayer film by reacting it with a mixed solution of water and alcohol such as ethanol or i-propanol, and a process of treating the underlayer film with acetic acid or alcohol after irradiating the underlayer film with UV light or EB light.

[0155] <Metal introduction process> The pattern formation method preferably further includes a step of introducing a metal into the underlayer film, such as the SIS method (Sequential Infiltration Synthesis). Examples of the metal to be introduced include Li, Be, B, Na, Mg, Al, Si, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Rb, Sr, Y, Zr, Nb, Mo, Ru, Pd, Ag, Cd, In, Sn, Sb, Te, Cs, Ba, La, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Tl, Pb, Bi, Po, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. Such a process can be carried out, for example, by the method described in Journal of Photopolymer Science and Technology Volume 29, Number 5 (2016) 653-657. In addition, in the step of introducing a metal, a method using a metal complex gas, a method of applying a solution containing a metal, or a method using ion implantation can be adopted.

[0156] The step of introducing metal is preferably provided after forming the underlayer film. For example, after forming the underlayer film, the steps of forming a resist film, forming a pattern of the underlayer film, introducing metal, and etching are preferably provided in this order. However, the step of introducing metal may be provided before the step of forming the underlayer film. That is, the object to introduce metal is not limited to the underlayer film, and may be the composition for forming the underlayer film.

[0157] <Etching process> In the pattern forming method, it is preferable that the semiconductor substrate is processed using the resist film pattern formed in the above-mentioned resist film forming step as a protective film. Such a step is called an etching step.

[0158] Examples of methods for processing the semiconductor substrate in the etching step include known methods such as reactive ion etching (RIE) such as chemical dry etching and chemical wet etching (wet development), sputter etching, physical etching such as ion beam etching, etc. The processing of the semiconductor substrate is preferably performed by dry etching using a gas such as tetrafluoromethane, perfluorocyclobutane (C4F8), perfluoropropane (C3F8), trifluoromethane, carbon monoxide, argon, helium, oxygen, nitrogen, chlorine, sulfur hexafluoride, difluoromethane, nitrogen trifluoride, and chlorine trifluoride.

[0159] In addition, the etching process may be a chemical wet etching process. Examples of the wet etching method include a method of treating the substrate by reaction with acetic acid, a method of treating the substrate by reaction with a mixed solution of water and alcohol such as ethanol or i-propanol, and a method of treating the substrate with acetic acid or alcohol after irradiation with UV light or EB light.

[0160] <Pattern Usage> The pattern thus formed is preferably used as a guide for pattern formation using a self-organizing pattern forming material (DSA (Directed Self Assembly lithography)). It is also preferably used as a mold for nanoimprint lithography.

[0161] The pattern formation method can be applied to various manufacturing methods. For example, the pattern formation method may be used in a semiconductor manufacturing process. An example of a semiconductor manufacturing process preferably includes a step of forming a pattern on a semiconductor substrate by the pattern formation method. EXAMPLES

[0162] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. In the copolymer examples, l, m, n, and r indicate the number of structural units contained in the copolymer.

[0163] [Sugar preparation] Xylooligosaccharides and xylose were obtained by extraction from wood pulp with reference to JP 2012-100546 A. D-(+) glucose was manufactured by Wako Pure Chemical Industries, Ltd.

[0164] [Synthesis of random copolymers] <Synthesis of copolymer 1> (Synthesis of acetyl sugar methacrylate 1) 10 g of xylooligosaccharide (average degree of polymerization 3) was added to a mixed solution of 120 g of acetic anhydride and 160 g of acetic acid, and stirred at 30°C for 2 hours. Approximately 5 times the amount of cold water as the solution was slowly added while stirring, and after stirring for 2 hours, the solution was left to stand overnight. 10 g of precipitated crystals were added to a solution of 200 mL of THF, 0.6 g of ethylenediamine and 0.7 g of acetic acid, and the temperature was adjusted to 0°C in a flask, and the solution was stirred for 4 hours. This was poured into 500 mL of cold water and extracted twice with dichloromethane. 10 g of this extract, 150 mL of dichloromethane, and 2.4 g of triethylamine were placed in a flask and cooled to -30°C. 1.4 g of methacryloyl chloride was added and stirred for 2 hours. This was poured into 150 mL of cold water, extracted twice with dichloromethane, and the solvent was concentrated to obtain 8.1 g of acetyl sugar methacrylate 1. The structure of the obtained acetyl sugar methacrylate 1 is as follows. [ka]

[0165] (Synthesis of Styrene-Methyl Methacrylate-Acetyl Sugar Methacrylate Random Copolymer) 500 mL of tetrahydrofuran and 92 g of a 2.6% by mass solution of lithium chloride in THF (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to the flask, and the mixture was cooled to -78°C under an argon atmosphere. 13 g of a 15.4% by mass solution of n-butyllithium in hexane (manufactured by Tokyo Chemical Industry Co., Ltd.) was added, and the mixture was stirred for 5 minutes, after which it was dehydrated and degassed. Next, a mixture of acetyl sugar methacrylate 1 (30 g), 20 g of styrene (manufactured by Tokyo Chemical Industry Co., Ltd.), and 20 g of methyl methacrylate was added and stirred for 30 minutes. Then, 10 g of methanol was added to stop the reaction, and copolymer 1 was synthesized. The structures of the copolymer structural units a, b, and c contained in copolymer 1 are as follows. [ka]

[0166] <Synthesis of copolymer 2> (Synthesis of Styrene-Butyl Acetyl Methacrylate Random Copolymer) Copolymer 2 was synthesized in the same manner as in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that methyl methacrylate was used instead of butyl acrylate in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a, b, and c contained in copolymer 2 are as follows. [ka]

[0167] <Synthesis of copolymer 3> (Synthesis of styrene-methyl acrylate-acetylglucosyl methacrylate 1 random copolymer) Copolymer 3 was synthesized in the same manner as in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that methyl methacrylate was used instead of methyl acrylate in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a, b, and c contained in copolymer 3 are as follows. [ka]

[0168] <Synthesis of copolymer 4> (Synthesis of naphthalene-methyl acrylate-acetyl sugar methacrylate 1 random copolymer) Copolymer 4 was synthesized in the same manner as in the synthesis of styrene-methyl acrylate-acetyl sugar methacrylate 1 random copolymer, except that styrene was replaced with 1-vinylnaphthalene (Tokyo Chemical Industry Co., Ltd.). The structures of the copolymer structural units a, b, and c contained in copolymer 4 are as follows. [ka]

[0169] <Synthesis of copolymer 5> (Synthesis of Styrene-Hydroxyethyl Methacrylate-Acetyl Sugar Methacrylate 1 Random Copolymer) Copolymer 5 was synthesized in the same manner as in the synthesis of styrene-methyl acrylate-acetyl sugar methacrylate 1 random copolymer, except that methyl acrylate was replaced with hydroxyethyl methacrylate (Tokyo Chemical Industry Co., Ltd.). The structures of the copolymer structural units a, b, and c contained in copolymer 5 are as follows: [ka]

[0170] <Synthesis of copolymer 6> (Synthesis of styrene-acrylic acid-acetylglucosyl methacrylate random copolymer) Copolymer 6 was synthesized in the same manner as in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that methyl methacrylate was used instead of acrylic acid (Tokyo Chemical Industry Co., Ltd.) in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a, b, and c contained in copolymer 6 are as follows. [ka]

[0171] <Synthesis of copolymer 7> (Synthesis of acetyl sugar methacrylate 2) Acetyl sugar methacrylate 2 was synthesized in the same manner as in the synthesis of acetyl sugar methacrylate 1, except that xylose was used instead of the xylooligosaccharide having an average degree of polymerization of 3 in the synthesis of acetyl sugar methacrylate 1. The structure of the obtained acetyl sugar methacrylate 2 is as follows. [ka]

[0172] (Synthesis of styrene-methacrylate-acetylglucosyl methacrylate 2 random copolymer) Copolymer 7 was synthesized in the same manner as in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that acetyl sugar methacrylate 1 was used instead of acetyl sugar methacrylate 2 in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a, b, and c contained in copolymer 7 are as follows. [ka]

[0173] <Synthesis of copolymer 8> (Synthesis of acetyl sugar acrylate) In the synthesis of acetyl sugar methacrylate 2, 10.0 g of acetyl sugar acrylate was synthesized in the same manner as in the synthesis of acetyl sugar methacrylate 2, except that 1.4 g of methacryloyl chloride was replaced with 1.3 g of acryloyl chloride (manufactured by Tokyo Chemical Industry Co., Ltd.). The structure of the obtained acetyl sugar acrylate is as follows. [ka]

[0174] (Synthesis of styrene-methyl methacrylate-acetyl sugar acrylate random copolymer) Copolymer 8 was synthesized in the same manner as for the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that acetyl sugar methacrylate 1 was used instead of acetyl sugar acrylate in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a, b, and c contained in copolymer 8 are as follows. [ka]

[0175] <Synthesis of copolymer 9> (Synthesis of sugar methacrylate) 33 g of xylooligosaccharide (average degree of polymerization 4) was dissolved in 150 mL of water, and 28.5 g of ammonium hydrogen carbonate (manufactured by Wako Pure Chemical Industries, Ltd.) was added 4 times every 24 hours, and the mixture was stirred at 37°C for 96 hours. Then, 200 mL of distilled water was added, and water was distilled off until the volume was 20 mL, after which 150 mL of water was added and the mixture was concentrated until the volume was 10 mL. This process was repeated until the ammonia odor disappeared, and after freeze-drying, a white solid was obtained. This substance was dissolved in 1x10 -3The resulting mixture was dissolved in 50 mL of KOH solution of 10.4 g of 2-isocyanate ethyl methacrylate (manufactured by Wako Pure Chemical Industries, Ltd.) and vigorously stirred for 12 hours while maintaining the temperature at 3°C. After removing the precipitated white solid, the filtrate was washed four times with 50 mL of diethyl ether and freeze-dried. The resulting white solid was then dissolved in a mixed solution of 2 mL of water and 10 mL of methanol, dropped into a mixed solution of 200 mL of acetone, and cooled. The mixture was then filtered and dried under reduced pressure to obtain sugar methacrylate. The structure of the resulting sugar methacrylate is as follows: [ka]

[0176] (Synthesis of styrene-methyl methacrylate-sugar methacrylate random copolymer) Copolymer 9 was synthesized in the same manner as in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that acetyl sugar methacrylate 1 was used instead of sugar methacrylate in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a, b, and c contained in copolymer 9 are as follows. [ka]

[0177] <Synthesis of copolymer 10> (Synthesis of acetyl sugar methacrylate 3) 10 g of sugar methacrylate was reacted with 120 g of acetic anhydride for 2 hours. After that, the reaction was stopped with a 33% magnesium acetate solution, and the product was precipitated by adding pure water to obtain acetyl sugar methacrylate 3. The structure of the obtained acetyl sugar methacrylate 3 is as follows. [ka]

[0178] (Synthesis of styrene-methyl methacrylate-acetylglucosyl methacrylate 3-random copolymer) Copolymer 10 was synthesized in the same manner as in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that acetyl sugar methacrylate 1 was used instead of acetyl sugar methacrylate 3 in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a, b, and c contained in copolymer 10 are as follows. [ka]

[0179] <Synthesis of copolymer 11> (Synthesis of acetylated sugar ethyl methacrylate) In the synthesis of acetyl sugar methacrylate 1, 1.4 g of methacryloyl chloride was replaced with 1.8 g of 1-chloroethyl methacrylate (manufactured by Alfa Aeser), and 1.1 g of acetyl sugar ethyl methacrylate was synthesized in the same manner as in the synthesis of acetyl sugar methacrylate 1. The structure of the obtained acetyl sugar ethyl methacrylate is as follows. [ka]

[0180] (Synthesis of styrene-methyl methacrylate-acetylglucoethyl methacrylate random copolymer) Copolymer 11 was synthesized in the same manner as in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that acetyl sugar methacrylate 1 was used instead of acetyl sugar ethyl methacrylate in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a, b, and c contained in copolymer 11 are as follows. [ka]

[0181] <Synthesis of copolymer 12> (Synthesis of acetyl sugar methacrylate 4) Acetyl sugar methacrylate 4 was synthesized in the same manner as in the synthesis of acetyl sugar methacrylate 1, except that glucose was used instead of the xylooligosaccharide with an average degree of polymerization of 3 in the synthesis of acetyl sugar methacrylate 1. The structure of the obtained acetyl sugar methacrylate 4 is as follows. [ka]

[0182] (Synthesis of Styrene-Methyl Methacrylate-Acetyl Sugar Methacrylate 4 Random Copolymer) Copolymer 12 was synthesized in the same manner as in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that acetyl sugar methacrylate 1 was used instead of acetyl sugar methacrylate 4 in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a, b, and c contained in copolymer 12 are as follows. [ka]

[0183] <Synthesis of copolymer 13> (Synthesis of acetylated sugar styrene) Acetyl sugar was synthesized in the same manner as in the synthesis of acetyl sugar methacrylate 1. Then, 10.8 g (90 mmol) of 4-vinylphenol, 32.2 g (32 mmol) of acetyl sugar, and 0.5 g of zinc chloride were heated in a silicon oil bath at 160°C for 30 minutes while stirring. The molten mixture was cooled to about 60°C and dissolved in 200 mL of benzene. This solution was washed twice with water and then with 1 M sodium hydroxide until the aqueous phase was almost colorless, and then washed twice with water, dried, and concentrated under reduced pressure to obtain 26.5 g of acetyl sugar styrene. The structure of the obtained acetyl sugar styrene is as follows: [ka]

[0184] (Synthesis of Styrene-Methyl Methacrylate-Acetyl Sugar Styrene Random Copolymer) Copolymer 13 was synthesized in the same manner as in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that acetyl sugar methacrylate 1 was used instead of acetyl sugar styrene in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a, b, and c contained in copolymer 13 are as follows. [ka]

[0185] <Synthesis of copolymer 14> (Synthesis of styrene-glycidyl methacrylate-cetyl sugar methacrylate 1 random copolymer) Copolymer 14 was synthesized in the same manner as in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that methyl methacrylate was used instead of glycidyl methacrylate (Tokyo Chemical Industry Co., Ltd.) in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a, b, and c contained in copolymer 14 are as follows. [ka]

[0186] <Synthesis of copolymer 15> (Synthesis of Styrene-Acetyl Sugar Methacrylate Random Copolymer) Copolymer 15 was synthesized in the same manner as for the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that methyl methacrylate was not used in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the structural units a and b of the copolymer contained in copolymer 15 are as follows. [ka]

[0187] <Synthesis of copolymer 16> (Synthesis of methyl methacrylate-acetylglucosyl methacrylate random copolymer) Copolymer 16 was synthesized in the same manner as for the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that styrene was not used in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units a and c contained in copolymer 16 are as follows. [ka]

[0188] <Synthesis of copolymer 17> (Synthesis of styrene-methyl methacrylate random copolymer) Copolymer 17 was synthesized in the same manner as in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer, except that acetyl sugar methacrylate 1 was not used in the synthesis of styrene-methyl methacrylate-acetyl sugar methacrylate 1 random copolymer. The structures of the copolymer structural units b and c contained in copolymer 17 are as follows. [ka]

[0189] [Analysis of copolymers] <Weight average molecular weight> The weight average molecular weight of the copolymer was measured by gel permeation chromatography (GPC). GPC column: Shodex K-806M / K-802 connected column (Showa Denko) Column temperature: 40℃ Mobile phase: Chloroform Detector: RI After the polymerization was completed, the degree of polymerization was confirmed by GPC method, and it was confirmed that the random copolymers with the targeted degree of polymerization and average molecular weight were produced. The molecular weight of each copolymer was 50,000 in weight average molecular weight Mw.

[0190] <Ratio of unit (a):unit (b):unit (c)> 1 The ratio (mass ratio) of units (a) to units (b) to units (c) in the copolymer was determined by H-NMR and calculated.

[0191] <Content of units derived from sugar derivatives> The content of units derived from sugar derivatives was calculated by the following formula. Content of units derived from sugar derivatives (mass%) = mass of units derived from sugar derivatives × number of units (monomers) derived from sugar derivatives × / weight average molecular weight of copolymer The number of units (monomers) containing the sugar derivative was calculated from the weight average molecular weight of the copolymer, the unit ratio of each structure calculated from NMR, and the molecular weight of each unit.

[0192] [Table 1]

[0193] [Evaluation of copolymers] <Calculation of copolymer solubility> 0.1 g of the weighed copolymer was placed in a sample bottle, and PGMEA was gradually added as an organic solvent (up to a maximum of 19.9 g of organic solvent) while stirring. The liquid temperature of the organic solvent was 25°C, and the copolymer was deemed dissolved when the solution became transparent to the naked eye. The copolymer solubility was calculated from the mass of the organic solvent added. Copolymer solubility (mass%) = mass of copolymer / mass of organic solvent when dissolved × 100 The results are shown in Table 3. The copolymer solubility was evaluated as good when it was 2% or more.

[0194] [Examples 1 to 19, Comparative Examples 1 to 3] <Preparation of Underlayer Film Composition Sample> 50 mg of the copolymer was dissolved in 1 mL of PGMEA to obtain a composition sample for forming an underlayer film in each of the Examples and Comparative Examples. When a catalyst was added, the catalyst was added so that the solid content of the catalyst was 3 mass% relative to the total mass of the copolymer. The types of catalyst added were as follows: Catalyst 1: Bis(t-butylsulfonyl)diazomethane (Wako Pure Chemical Industries, Ltd.) Catalyst 2: p-toluenesulfonic acid (Tokyo Chemical Industry Co., Ltd.) Catalyst 3: Bis(cyclohexylsulfonyl)diazomethanep (Wako Pure Chemical Industries, Ltd.)

[0195] <Evaluation of Metal Incorporation Rate in Underlayer Film-Forming Composition> The obtained composition for forming an underlayer film was spin-coated on a 2-inch silicon wafer substrate. After coating to a film thickness of 200 nm, the composition was baked on a hot plate at 230° C. for 5 minutes to form an underlayer film sample. The underlayer film sample thus formed was placed in an ALD (atomic layer deposition apparatus: PICUSAN SUNALE R-100B), and Al(CH3)3 gas was introduced therein at 95°C, followed by water vapor. This operation was repeated three times to introduce Al into the underlayer film. The underlayer film sample after introducing Al was subjected to EDX analysis (energy dispersive X-ray analysis) using an electron microscope JSM7800F (manufactured by JEOL Ltd.) to calculate the ratio of Al components (Al content). An Al content of 5 at% or more was evaluated as good.

[0196] <Calculation of the residual rate of the underlayer film> The obtained composition for forming an underlayer film was spin-coated onto a 2-inch silicon wafer substrate. After coating to a film thickness of 200 nm, the composition was baked on a hot plate at 210° C. for 2 minutes to form an underlayer film sample. The underlayer film sample before cleaning was cleaned by applying 1 ml of a 50:50 (mass ratio) mixture of propylene glycol monomethyl ether acetate and propylene glycol monomethyl ether, a solvent used in photoresists, for 30 seconds at 1000 rpm using a spin coater.Then, the sample was baked in air at 180°C for 2 minutes on a hot plate to obtain a cleaned underlayer film. The thickness of the underlayer film before and after cleaning was measured with a step gauge, and the remaining rate of the underlayer film was calculated as follows. Underlayer film remaining rate (%) = underlayer film thickness after cleaning (μm) / underlayer film thickness before cleaning (μm) × 100 The residual rate of the underlayer film was evaluated as good if it was 90% or more.

[0197] <UV reflectance> The obtained composition for forming an underlayer film was spin-coated onto a 2-inch silicon wafer substrate. After coating to a film thickness of 200 nm, the composition was baked on a hot plate at 210° C. for 2 minutes to form an underlayer film sample. The obtained underlayer film sample was set in a spectrophotometer (V770EX: manufactured by JASCO Corporation) equipped with an integrating sphere, and the reflectance at a wavelength of 193 nm was measured as the ultraviolet reflectance. An ultraviolet reflectance of 50% or less was evaluated as good.

[0198] <Evaluation of etching processability> The obtained composition for forming an underlayer film was spin-coated onto a 2-inch silicon wafer substrate. After coating to a film thickness of 200 nm, the composition was baked on a hot plate at 210° C. for 2 minutes to form an underlayer film sample. After applying and heating the ArF resist, the substrate was masked and exposed to light using an ArF excimer laser exposure machine to form a line-and-space (line width 50 nm, space width 50 nm) shape. After that, the substrate was baked on a hot plate at 60°C for 1 minute, and then immersed in a developer to produce a line-and-space pattern. The substrate was subjected to oxygen plasma treatment (100sccm, 4Pa, 100W, 300 seconds) using an ICP plasma etching device (Tokyo Electron Co., Ltd.), whereby the photoresist was removed and a line-and-space pattern was formed in the underlayer film. Then, metal was introduced into the underlayer film sample in the same manner as in the evaluation of the metal introduction rate of the underlayer film forming composition. Using this pattern as a mask, etching was performed on a silicon substrate using hexafluoroethane gas. The patterned surface of the trifluoromethane-treated substrate was observed with a scanning electron microscope (SEM) JSM7800F (manufactured by JEOL Ltd.) at an acceleration voltage of 1.5 kV, an emission current of 37.0 μA, and a magnification of 100,000 times to confirm the state of etching processability. The state of etching processability was evaluated according to the following evaluation criteria. ◯: The pattern has no line collapse in one field of view of the SEM. ×: The pattern has a state in which even a part of the lines is collapsed or has a distorted structure.

[0199] [Table 2]

[0200] As shown in Table 2, in the underlayer film-forming composition of each Example, the copolymer had high solubility in organic solvents. In addition, the underlayer film-forming composition of each Example was able to form an underlayer film that had extremely low UV reflectance used in exposure for photoresists and had a high underlayer film survival rate in the atmosphere at a relatively low temperature. In addition, in all Examples, a high metal introduction rate was achieved, and etching processability was good. On the other hand, in Comparative Example 1, the solubility of the copolymer in organic solvents was low, and the underlayer film residual rate was low. In Comparative Example 2, the underlayer film residual rate was low, and the etching processability was also poor. In Comparative Example 3, the metal introduction rate was extremely small, and the etching processability was not good. Furthermore, the underlayer films obtained in Comparative Examples 1 to 3 had high ultraviolet reflection. [Explanation of symbols]

[0201] 10 Substrate 20 Lower layer membrane

Claims

1. (a) a unit derived from a sugar derivative; (b) a unit derived from a compound having an antireflection function; and (c) units derived from compounds capable of cross-coupling the copolymer, the (a) unit derived from a sugar derivative is at least one selected from a unit derived from a pentose derivative and a unit derived from a hexose derivative, The (b) unit derived from a compound having a light reflection preventing function is a unit represented by the following general formula (3) or (4): The (c) random copolymer, wherein the unit derived from a compound capable of cross-coupling the copolymer is a unit represented by the following general formula (5): 【Chemistry 1】 【Chemistry 2】 (In the general formulas (3) and (4), R 5 represents a hydrogen atom or an alkyl group. X 1 represents a single bond or a linking group. R 50 represents an organic group or a hydroxyl group. In the general formula (3), n represents an integer of 0 to 5, and in the general formula (4), n represents an integer of 0 to 7. 【Chemistry 3】 (In general formula (5), R 5 represents a hydrogen atom or an alkyl group; R 60 represents an alkyl group which may have a substituent or an aryl group which may have a substituent.

2. The random copolymer according to claim 1, wherein the unit (a) derived from a sugar derivative is at least one selected from the group consisting of a unit derived from a cellulose derivative, a unit derived from a hemicellulose derivative, and a unit derived from a xylooligosaccharide derivative.

3. In the general formula (5), R 60 The random copolymer according to claim 1 or 2, wherein: is an alkyl group which may have a substituent, and the alkyl group has 1 to 8 carbon atoms.

Citation Information

Patent Citations

  • Base-layer film forming composition for lithography containing cyclodextrin containing clathrate molecule

    JP2007256773A

  • Oligosaccharide / silicon-containing block copolymer for use in lithography

    JP2014527089A

  • Composition for forming resist underlay film, and patterning method using the composition

    JP2016170338A

  • Method for forming resist underlay film and pattern forming method

    JP2016206676A

  • Pattern-forming material, pattern-forming method, and monomer for pattern-forming material

    JP2023107809A