Magnetic Recording Media
The tape-shaped magnetic recording medium with optimized magnetic powder dispersibility and orientation addresses the challenge of electromagnetic conversion characteristics, achieving improved data storage efficiency through enhanced C/N ratio and stability.
Patent Information
- Application Number
- JP2023080869
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-11-19
- Filing Date
- 2023-05-16
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-04-01
AI Technical Summary
Existing magnetic recording media face challenges in improving electromagnetic conversion characteristics, particularly in tape-shaped media, where the dispersibility and orientation of magnetic powder affect the efficiency of data storage.
A tape-shaped magnetic recording medium with a specific configuration, including a substrate, magnetic layer with hexagonal ferrite or ε iron oxide particles, and controlled thickness and aspect ratio, along with optimized coercive forces and Young's modulus, enhances the dispersibility and orientation of magnetic powder, thereby improving electromagnetic conversion characteristics.
The proposed configuration leads to enhanced electromagnetic conversion characteristics, such as improved C/N ratio, allowing for higher recording density and stability in data storage.
Smart Images

Figure 0007559870000004 
Figure 0007559870000005 
Figure 0007559870000006
Abstract
Description
[Technical field]
[0001] The present disclosure relates to magnetic recording media. [Background technology]
[0002] In recent years, tape-type magnetic recording media have been attracting attention as a data storage medium. Various improvements in the characteristics of these magnetic recording media have been studied, and one of these improvements is the improvement of electromagnetic conversion characteristics.
[0003] Patent Documents 1 to 3 propose techniques for improving the dispersibility of barium ferrite magnetic powder and improving electromagnetic conversion characteristics. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-298333 A [Patent Document 2] JP 2002-373413 A [Patent Document 3] JP 2009-99240 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present disclosure is to provide a magnetic recording medium capable of improving electromagnetic conversion characteristics. [Means for solving the problem]
[0006] In order to solve the above problems, the present disclosure provides: A tape-shaped magnetic recording medium, A substrate; a magnetic layer including magnetic powder provided on a substrate; Equipped with The magnetic powder includes hexagonal ferrite, ε iron oxide, or Co-containing spinel ferrite, The magnetic layer has five or more servo bands, The average thickness of the magnetic recording medium is 5.6 μm or less, The average thickness of the magnetic layer is 90 nm or less, When the average thickness of the substrate is TB and the average thickness of the magnetic recording medium is TL, the value of (TL-TB) / TB is 0.41 or less; The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, The coercive force Hc2 of the magnetic recording medium in the longitudinal direction of the magnetic recording medium is 1000 Oe or more, of the magnetic recording medium in the perpendicular direction the coercive force Hc1 and the coercive force Hc2 of the magnetic recording medium in the longitudinal direction of the magnetic recording medium satisfy the relationship Hc2 / Hc1≦0.8; The Young's modulus of the magnetic recording medium in the longitudinal direction is 8.3 GPa or less. Effect of the Invention
[0007] According to the present disclosure, it is possible to improve electromagnetic conversion characteristics. Note that the effects described herein are not necessarily limited to those described herein, and may be any of the effects described in the present disclosure or effects different from those effects. [Brief description of the drawings]
[0008] [Figure 1] 1 is a cross-sectional view of a magnetic recording medium according to a first embodiment of the present disclosure. [Diagram 2] Figure 2A is a schematic diagram of the layout of the data band and the servo band, and Figure 2B is an expanded view of the data band. [Diagram 3] FIG. 2 is a cross-sectional view of a magnetic particle. [Figure 4] 1 is a graph showing an example of an MH loop. [Diagram 5] 1 is a graph showing an example of an SFD curve. [Figure 6] FIG. 1 is a schematic diagram of a recording and reproducing device. [Figure 7] FIG. 11 is a cross-sectional view of a magnetic particle in a modified example. [Figure 8] FIG. 11 is a cross-sectional view of a magnetic recording medium according to a modified example. [Figure 9] Fig. 9A shows an MFM image when a data signal is recorded at a wavelength λ, and Fig. 9B shows an MFM image when a data signal is recorded at the shortest recording wavelength L'. [Figure 10] FIG. 4 is a diagram showing the relationship between the elongation rate in the longitudinal direction of a magnetic recording medium and the load in a tensile test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The embodiments of the present disclosure will be described in the following order. 1. First embodiment 1.1 Structure of magnetic recording media 1.2 Manufacturing method of magnetic recording media 1.3 Configuration of recording / playback device 1.4 Effects 1.5 Variations 2. Second embodiment
[0010] <1 First embodiment> [1.1 Structure of magnetic recording media] First, the configuration of a magnetic recording medium 10 according to the first embodiment will be described with reference to Fig. 1. The magnetic recording medium 10 comprises a long substrate 11, an underlayer 12 provided on one main surface of the substrate 11, a magnetic layer 13 provided on the underlayer 12, and a back layer 14 provided on the other main surface of the substrate 11. Note that the underlayer 12 and the back layer 14 are provided as necessary and may not be required.
[0011] The magnetic recording medium 10 has a long tape shape, and runs in the longitudinal direction during recording and reproduction. The surface of the magnetic layer 13 is the surface on which the magnetic head runs. The magnetic recording medium 10 is preferably used in a recording and reproduction device equipped with a ring-type head as a recording head. In this specification, the term "vertical direction" means the direction perpendicular to the surface of the magnetic recording medium 10 (thickness direction of the magnetic recording medium 10), and the term "longitudinal direction" means the longitudinal direction (running direction) of the magnetic recording medium 10.
[0012] (Base) The substrate 11 is a non-magnetic support that supports the underlayer 12 and the magnetic layer 13. The substrate 11 has a long film shape. The upper limit of the average thickness of the substrate 11 is preferably 4.2 μm or less, more preferably 3.8 μm or less, and even more preferably 3.4 μm or less. When the upper limit of the average thickness of the substrate 11 is 4.2 μm or less, the recording capacity that can be recorded in one data cartridge can be increased compared to that of a general magnetic recording medium. The lower limit of the average thickness of the substrate 11 is preferably 3 μm or more, more preferably 3.2 μm or more. When the lower limit of the average thickness of the substrate 11 is 3 μm or more, a decrease in the strength of the substrate 11 can be suppressed.
[0013] The average thickness of the substrate 11 is obtained as follows. First, a magnetic recording medium 10 having a width of 1 / 2 inch is prepared and cut into a length of 250 mm to prepare a sample. Next, layers other than the substrate 11 of the sample (i.e., the underlayer 12, the magnetic layer 13, and the back layer 14) are removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. Next, the thickness of the sample (substrate 11) is measured at five or more positions using a Mitsutoyo laser hologram as a measuring device, and the measured values are simply averaged (arithmetic average) to calculate the average thickness of the substrate 11. Note that the measurement positions are selected randomly from the sample.
[0014] The substrate 11 includes at least one of polyesters, polyolefins, cellulose derivatives, vinyl resins, and other polymer resins, for example. When the substrate 11 includes two or more of the above materials, the two or more materials may be mixed, copolymerized, or laminated.
[0015] The polyesters include, for example, at least one of PET (polyethylene terephthalate), PEN (polyethylene naphthalate), PBT (polybutylene terephthalate), PBN (polybutylene naphthalate), PCT (polycyclohexylene dimethylene terephthalate), PEB (polyethylene-p-oxybenzoate), and polyethylene bisphenoxycarboxylate.
[0016] The polyolefins include, for example, at least one of PE (polyethylene) and PP (polypropylene). The cellulose derivatives include, for example, at least one of cellulose diacetate, cellulose triacetate, CAB (cellulose acetate butyrate) and CAP (cellulose acetate propionate). The vinyl resins include, for example, at least one of PVC (polyvinyl chloride) and PVDC (polyvinylidene chloride).
[0017] Other polymer resins include, for example, at least one of PA (polyamide, nylon), aromatic PA (aromatic polyamide, aramid), PI (polyimide), aromatic PI (aromatic polyimide), PAI (polyamideimide), aromatic PAI (aromatic polyamideimide), PBO (polybenzoxazole, such as Zylon (registered trademark)), polyether, PEK (polyetherketone), polyetherester, PES (polyethersulfone), PEI (polyetherimide), PSF (polysulfone), PPS (polyphenylene sulfide), PC (polycarbonate), PAR (polyarylate), and PU (polyurethane).
[0018] (magnetic layer) The magnetic layer 13 is a recording layer for recording signals. The magnetic layer 13 contains, for example, a magnetic powder and a binder. If necessary, the magnetic layer 13 may further contain at least one additive selected from the group consisting of a lubricant, an antistatic agent, an abrasive, a hardener, an anti-rust agent, and non-magnetic reinforcing particles.
[0019] As shown in Fig. 2A, the magnetic layer 13 preferably has a plurality of servo bands SB and a plurality of data bands DB in advance. The plurality of servo bands SB are provided at equal intervals in the width direction of the magnetic recording medium 10. A data band DB is provided between adjacent servo bands SB. A servo signal for tracking control of the magnetic head is written in advance in the servo band SB. User data is recorded in the data band DB.
[0020] The total area S of the servo bands SB relative to the surface area S of the magnetic layer 13 SB The ratio of R S (=(S SB From the viewpoint of ensuring a high recording capacity, the upper limit of the ratio of the total area S of the plurality of servo bands SB to the area S of the surface of the magnetic layer 13 is preferably 4.0% or less, more preferably 3.0% or less, and even more preferably 2.0% or less. SB The ratio of R S The lower limit is preferably 0.8% or more, from the viewpoint of ensuring five or more servo tracks.
[0021] The total area S of the servo bands SB relative to the surface area S of the magnetic layer 13 SB The ratio of R S is obtained as follows. First, the surface of the magnetic layer 13 is observed using a magnetic force microscope (MFM) to obtain an MFM image. Next, the servo bandwidth W is calculated using the obtained MFM image. SB and the number of servo bands SB. Next, calculate the ratio R from the following formula: S Request. Ratio R S [%]=(((Servo bandwidth W SB )×(number of servo bands) / (width of magnetic recording medium 10)×100
[0022] The lower limit of the number of servo bands SB is preferably 5 or more, more preferably 5+4n or more (where n is a positive integer), and even more preferably 9+4n or more. If the number of servo bands SB is 5 or more, the effect of dimensional changes in the width direction of the magnetic recording medium 10 on the servo signal can be suppressed, and stable recording and reproducing characteristics with less off-track can be ensured. The upper limit of the number of servo bands SB is not particularly limited, but is, for example, 33 or less.
[0023] The number of servo bands SB can be confirmed as follows. First, the surface of the magnetic layer 13 is observed using a magnetic force microscope (MFM) to obtain an MFM image. Next, the number of servo bands SB is counted using the MFM image.
[0024] Servo Bandwidth W SB From the viewpoint of ensuring a high recording capacity, the upper limit of the servo band width W is preferably 95 μm or less, more preferably 60 μm or less, and even more preferably 30 μm or less. SB The lower limit of the servo bandwidth W is preferably 10 μm or more. SB It is difficult to manufacture a recording head capable of reading such servo signals.
[0025] Servo Bandwidth W SB The width of the servo band is obtained as follows. First, the surface of the magnetic layer 13 is observed using a magnetic force microscope (MFM) to obtain an MFM image. Next, the servo band width W SB Measure the width.
[0026] As shown in Fig. 2B, the magnetic layer 13 is configured so that a plurality of data tracks Tk can be formed on the data band DB. From the viewpoint of improving the track recording density and ensuring a high recording capacity, the upper limit of the data track width W is preferably 3.0 µm or less, more preferably 1.6 µm or less, even more preferably 0.95 µm or less, and particularly preferably 0.51 µm or less. Taking into account the magnetic grain size, the lower limit of the data track width W is preferably 0.02 µm or more.
[0027] The magnetic layer 13 is configured to be capable of recording data such that the minimum value L of the magnetic reversal distance and the data track width W are preferably W / L≦200, more preferably W / L≦60, even more preferably W / L≦45, and particularly preferably W / L≦30. If the minimum value L of the magnetic reversal distance is a constant value and the minimum value L of the magnetic reversal distance and the track width W are W / L>200 (i.e., if the track width W is large), the track recording density does not increase, and there is a risk that the recording capacity cannot be sufficiently secured. Also, if the track width W is a constant value and the minimum value L of the magnetic reversal distance and the track width W are W / L>200 (i.e., if the minimum value L of the magnetic reversal distance is small), the bit length becomes small and the linear recording density increases, but there is a risk that the SNR may be significantly deteriorated due to the effect of spacing loss. Therefore, in order to suppress the deterioration of the SNR while securing the recording capacity, it is preferable that W / L is in the range of W / L≦60 as described above. However, W / L is not limited to the above range, and may be W / L≦23 or W / L≦13. The lower limit of W / L is not particularly limited, but is, for example, 1≦W / L.
[0028] From the viewpoint of ensuring a high recording capacity, the magnetic layer 13 is configured to be capable of recording data such that the minimum value of the distance L between magnetization reversals is preferably 50 nm or less, more preferably 48 nm or less, even more preferably 44 nm or less, and particularly preferably 40 nm or less. Taking into account the magnetic grain size, the lower limit of the minimum value of the distance L between magnetization reversals is preferably 20 nm or more.
[0029] The upper limit of the average thickness of the magnetic layer 13 is preferably 90 nm or less, particularly preferably 80 nm or less, more preferably 70 nm or less, and even more preferably 50 nm or less. When the upper limit of the average thickness of the magnetic layer 13 is 90 nm or less, when a ring-type head is used as a recording head, magnetization can be recorded uniformly in the thickness direction of the magnetic layer 13, and therefore the electromagnetic conversion characteristics (e.g., C / N (Carrier to Noise Ratio)) can be improved.
[0030] The lower limit of the average thickness of the magnetic layer 13 is preferably 30 nm or more, and more preferably 35 nm or more. If the upper limit of the average thickness of the magnetic layer 13 is 30 nm or more, output can be ensured when an MR head is used as the reproducing head, and therefore the electromagnetic conversion characteristics (e.g., C / N) can be improved.
[0031] The average thickness of the magnetic layer 13 is determined as follows. First, the magnetic recording medium 10 is thinned perpendicularly to its main surface to prepare a sample piece, and the cross section of the test piece is observed with a transmission electron microscope (TEM). The apparatus and observation conditions are shown below. Equipment: TEM (Hitachi H9000NAR) Acceleration voltage: 300 kV Magnification: 100,000x Next, using the obtained TEM image, the thickness of magnetic layer 13 is measured at at least 10 positions in the longitudinal direction of magnetic recording medium 10, and then these measurements are simply averaged (arithmetic mean) to obtain the average thickness of magnetic layer 13. Note that the measurement positions are selected at random from the test piece.
[0032] (magnetic powder) The magnetic powder includes a powder of nanoparticles containing ε-iron oxide (hereinafter referred to as "ε-iron oxide particles"). The ε-iron oxide particles are hard magnetic particles that can obtain high coercive force even though they are fine particles. It is preferable that the ε-iron oxide contained in the ε-iron oxide particles has a crystal orientation preferentially in the vertical direction.
[0033] The ε-iron oxide particles are spherical or nearly spherical, or cubic or nearly cubic. Because the ε-iron oxide particles have the above-mentioned shapes, when the ε-iron oxide particles are used as the magnetic particles, the contact area between the particles in the thickness direction of the magnetic recording medium 10 can be reduced and the aggregation between the particles can be suppressed, compared to when hexagonal plate-shaped barium ferrite particles are used as the magnetic particles. This improves the dispersibility of the magnetic powder, and allows for better electromagnetic conversion characteristics (e.g., C / N).
[0034] The ε-iron oxide particles have a core-shell structure. Specifically, as shown in Fig. 3, the ε-iron oxide particles include a core portion 21 and a two-layered shell portion 22 provided around the core portion 21. The two-layered shell portion 22 includes a first shell portion 22a provided on the core portion 21 and a second shell portion 22b provided on the first shell portion 22a.
[0035] The core portion 21 contains ε-iron oxide. The ε-iron oxide contained in the core portion 21 preferably has ε-Fe2O3 crystals as a main phase, and more preferably is made of single-phase ε-Fe2O3.
[0036] The first shell portion 22a covers at least a part of the periphery of the core portion 21. Specifically, the first shell portion 22a may cover a part of the periphery of the core portion 21, or may cover the entire periphery of the core portion 21. From the viewpoint of ensuring sufficient exchange coupling between the core portion 21 and the first shell portion 22a and improving magnetic characteristics, it is preferable that the entire surface of the core portion 21 is covered.
[0037] The first shell portion 22a is a so-called soft magnetic layer, and includes a soft magnetic material such as α-Fe, a Ni-Fe alloy, an Fe-Si-Al alloy, etc. The α-Fe may be obtained by reducing ε-iron oxide included in the core portion 21.
[0038] The second shell portion 22b is an oxide coating serving as an anti-oxidation layer. The second shell portion 22b includes α-iron oxide, aluminum oxide, or silicon oxide. The α-iron oxide includes at least one type of iron oxide, for example, Fe3O4, Fe2O3, and FeO. When the first shell portion 22a includes α-Fe (soft magnetic material), the α-iron oxide may be obtained by oxidizing the α-Fe included in the first shell portion 22a.
[0039] By having the first shell portion 22a as described above, the coercivity Hc of the ε iron oxide particles (core-shell particles) as a whole can be adjusted to a coercivity Hc suitable for recording while maintaining the coercivity Hc of the core portion 21 alone at a large value to ensure thermal stability. Furthermore, by having the second shell portion 22b as described above, it is possible to prevent the ε iron oxide particles from being exposed to air during and before the manufacturing process of the magnetic recording medium 10, which would cause rust or the like on the particle surface, thereby preventing the properties of the ε iron oxide particles from deteriorating. Therefore, it is possible to prevent the properties of the magnetic recording medium 10 from deteriorating.
[0040] The average particle size (average maximum particle size) of the magnetic powder is preferably 22 nm or less, more preferably 8 nm to 22 nm, and even more preferably 12 nm to 22 nm. In the magnetic recording medium 10, the area with a size of 1 / 2 of the recording wavelength becomes the actual magnetization area. Therefore, by setting the average particle size of the magnetic powder to half the shortest recording wavelength or less, a good S / N ratio can be obtained. Therefore, when the average particle size of the magnetic powder is 22 nm or less, good electromagnetic conversion characteristics (e.g., C / N) can be obtained in a high recording density magnetic recording medium 10 (e.g., a magnetic recording medium 10 configured to be able to record signals at the shortest recording wavelength of 44 nm or less). On the other hand, when the average particle size of the magnetic powder is 8 nm or more, the dispersibility of the magnetic powder is further improved, and better electromagnetic conversion characteristics (e.g., C / N) can be obtained.
[0041] The average aspect ratio of the magnetic powder is preferably 1.0 or more and 3.0 or less, more preferably 1.0 or more and 2.5 or less, even more preferably 1.0 or more and 2.1 or less, and particularly preferably 1.0 or more and 1.8 or less. When the average aspect ratio of the magnetic powder is within the range of 1.0 or more and 3.0 or less, aggregation of the magnetic powder can be suppressed, and the resistance applied to the magnetic powder when the magnetic powder is vertically oriented in the process of forming the magnetic layer 13 can be suppressed. Therefore, the degree of vertical orientation of the magnetic powder can be increased. Therefore, the electromagnetic conversion characteristics (e.g., C / N) can be improved.
[0042] The average particle size and average aspect ratio of the magnetic powder are obtained as follows. First, the magnetic recording medium 10 to be measured is processed by a FIB (Focused Ion Beam) method or the like to prepare a thin piece, and the cross section of the thin piece is observed by a TEM. Next, 50 ε-iron oxide particles are randomly selected from the TEM photograph, and the long axis length DL and short axis length DS of each ε-iron oxide particle are measured. Here, the long axis length DL means the maximum distance between two parallel lines drawn from all angles so as to be tangent to the contour of the ε-iron oxide particle (so-called maximum Feret diameter). Meanwhile, the short axis length DS means the maximum length of the ε-iron oxide particle in the direction perpendicular to the long axis of the ε-iron oxide particle.
[0043] Next, the long axis lengths DL of the 50 measured ε iron oxide particles are simply averaged (arithmetic mean) to determine the average long axis length DLave. The average long axis length DLave thus determined is the average particle size of the magnetic powder. The short axis lengths DS of the 10 measured ε iron oxide particles are also simply averaged (arithmetic mean) to determine the average short axis length DSave. The average aspect ratio (DLave / DSave) of the ε iron oxide particles is then calculated from the average long axis length DLave and the average short axis length DSave.
[0044] The average particle volume of the magnetic powder is preferably 5600 nm 3 Less than or equal to 250 nm, preferably 3 Above 5600nm 3 Less than or equal to 900 nm, and even more preferably 3 Above 5600nm 3 The average particle volume of the magnetic powder is 5600 nm or less. 3 When the average particle size of the magnetic powder is 22 nm or less, the same effect as when the average particle volume of the magnetic powder is 250 nm or less can be obtained. 3 If the average particle size of the magnetic powder is 8 nm or more, the same effect as in the case where the average particle size of the magnetic powder is 8 nm or more can be obtained.
[0045] When the ε iron oxide particles are spherical or nearly spherical, the average particle volume of the magnetic powder is calculated as follows. First, the average major axis length DLave is calculated in the same manner as in the above-mentioned method for calculating the average particle size of the magnetic powder. Next, the average volume V of the magnetic powder is calculated using the following formula. V = (π / 6) × DLave 3
[0046] When the ε iron oxide particles are cubic or nearly cubic, the average volume of the magnetic powder is calculated as follows. First, the average major axis length DLave is calculated in the same manner as in the calculation method for the average particle size of the magnetic powder described above. Next, the average volume V of the magnetic powder is calculated using the following formula. V=DLave 3
[0047] (Binding agent) Examples of the binder include thermoplastic resins, thermosetting resins, and reactive resins. Examples of the thermoplastic resins include vinyl chloride, vinyl acetate, vinyl chloride-vinyl acetate copolymers, vinyl chloride-vinylidene chloride copolymers, vinyl chloride-acrylonitrile copolymers, acrylic acid ester-acrylonitrile copolymers, acrylic acid ester-vinyl chloride-vinylidene chloride copolymers, acrylic acid ester-acrylonitrile copolymers, acrylic acid ester-vinylidene chloride copolymers, methacrylic acid ester-vinylidene chloride copolymers, methacrylic acid ester-vinyl chloride copolymers, methacrylic acid ester-ethylene copolymers, polyvinyl fluoride, vinylidene chloride-acrylonitrile copolymers, acrylonitrile-butadiene copolymers, polyamide resins, polyvinyl butyral, cellulose derivatives (cellulose acetate butyrate, cellulose diacetate, cellulose triacetate, cellulose propionate, nitrocellulose), styrene-butadiene copolymers, polyurethane resins, polyester resins, amino resins, and synthetic rubbers.
[0048] Examples of the thermosetting resin include phenol resin, epoxy resin, polyurethane curing resin, urea resin, melamine resin, alkyd resin, silicone resin, polyamine resin, and urea formaldehyde resin.
[0049] All of the above binders contain -SO3M, -OSO3M, -COOM, P=O(OM)2 (where M represents a hydrogen atom or an alkali metal such as lithium, potassium, or sodium), -NR1R2, -NR1R2R3, etc., in order to improve the dispersibility of the magnetic powder. + X - Side chain amines with terminal groups represented by >NR1R2 + X - (wherein R1, R2, and R3 each represent a hydrogen atom or a hydrocarbon group; X - represents a halogen element ion such as fluorine, chlorine, bromine, or iodine, an inorganic ion, or an organic ion.) Polar functional groups such as -OH, -SH, -CN, and an epoxy group may be introduced. The amount of these polar functional groups introduced into the binder is 10 -1 ~10 -8 mol / g, preferably 10 -2 ~10 -6 More preferably, it is expressed in moles / g.
[0050] (Lubricant) Examples of lubricants include esters of monobasic fatty acids having 10 to 24 carbon atoms with any one of monohydric to hexahydric alcohols having 2 to 12 carbon atoms, mixed esters thereof, difatty acid esters, trifatty acid esters, etc. Specific examples of lubricants include lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, linoleic acid, linolenic acid, elaidic acid, butyl stearate, pentyl stearate, heptyl stearate, octyl stearate, isooctyl stearate, octyl myristate, etc.
[0051] (Antistatic agent) Examples of the antistatic agent include carbon black, natural surfactants, nonionic surfactants, and cationic surfactants.
[0052] (Abrasive) Examples of abrasives include acicular α-iron oxide obtained by dehydrating and annealing raw materials such as α-alumina with an α-conversion rate of 90% or more, β-alumina, γ-alumina, silicon carbide, chromium oxide, cerium oxide, α-iron oxide, corundum, silicon nitride, titanium carbide, titanium oxide, silicon dioxide, tin oxide, magnesium oxide, tungsten oxide, zirconium oxide, boron nitride, zinc oxide, calcium carbonate, calcium sulfate, barium sulfate, molybdenum disulfide, and magnetic iron oxide, and these may be surface-treated with aluminum and / or silica as necessary.
[0053] (hardening agent) Examples of the curing agent include polyisocyanates. Examples of the polyisocyanates include aromatic polyisocyanates such as an adduct of tolylene diisocyanate (TDI) and an active hydrogen compound, and aliphatic polyisocyanates such as an adduct of hexamethylene diisocyanate (HMDI) and an active hydrogen compound. The weight average molecular weight of these polyisocyanates is preferably in the range of 100 to 3000.
[0054] (rust inhibitor) Examples of the rust inhibitor include phenols, naphthols, quinones, heterocyclic compounds containing a nitrogen atom, heterocyclic compounds containing an oxygen atom, and heterocyclic compounds containing a sulfur atom.
[0055] (Non-magnetic reinforcing particles) Examples of non-magnetic reinforcing particles include aluminum oxide (α, β or γ alumina), chromium oxide, silicon oxide, diamond, garnet, emery, boron nitride, titanium carbide, silicon carbide, titanium carbide, titanium oxide (rutile or anatase type titanium oxide), and the like.
[0056] (base layer) The underlayer 12 is a non-magnetic layer containing a non-magnetic powder and a binder. If necessary, the underlayer 12 may further contain at least one additive selected from the group consisting of a lubricant, an antistatic agent, a hardener, and an anti-rust agent.
[0057] The average thickness of the underlayer 12 is preferably 0.6 μm or more and 2.0 μm or less, and more preferably 0.8 μm or more and 1.4 μm or less. The average thickness of the underlayer 12 is determined in the same manner as the average thickness of the magnetic layer 13. However, the magnification of the TEM image is appropriately adjusted depending on the thickness of the underlayer 12.
[0058] (Non-magnetic powder) The non-magnetic powder includes at least one of inorganic particle powder and organic particle powder. The non-magnetic powder may also include carbon powder such as carbon black. One type of non-magnetic powder may be used alone, or two or more types of non-magnetic powder may be used in combination. The inorganic particles include, for example, metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, or metal sulfides. The shape of the non-magnetic powder may be, for example, various shapes such as needle-like, spherical, cubic, and plate-like, but is not limited to these shapes.
[0059] (Binding agent) The binder is the same as that used in the magnetic layer 13 described above.
[0060] (Additives) The lubricant, antistatic agent, hardener and rust inhibitor are the same as those in the magnetic layer 13 described above.
[0061] (Back layer) The back layer 14 includes a binder and a non-magnetic powder. The back layer 14 may further include at least one additive selected from the group consisting of a lubricant, a hardener, and an antistatic agent, if necessary. The binder and the non-magnetic powder are the same as those of the underlayer 12 described above.
[0062] The average particle size of the non-magnetic powder is preferably 10 nm or more and 150 nm or less, more preferably 15 nm or more and 110 nm or less. The average particle size of the non-magnetic powder is determined in the same manner as the average particle size of the magnetic powder. The non-magnetic powder may contain non-magnetic powder having two or more particle size distributions.
[0063] The upper limit of the average thickness of the back layer 14 is preferably 0.6 μm or less. If the upper limit of the average thickness of the back layer 14 is 0.6 μm or less, the thickness of the underlayer 12 and the base 11 can be kept thick even when the average thickness of the magnetic recording medium 10 is 5.6 μm or less, so that the running stability of the magnetic recording medium 10 in a recording and reproducing device can be maintained. The lower limit of the average thickness of the back layer 14 is not particularly limited, but is, for example, 0.2 μm or more.
[0064] The average thickness of the back layer 14 is obtained as follows. First, a magnetic recording medium 10 having a width of 1 / 2 inch is prepared and cut into a length of 250 mm to prepare a sample. Next, the thickness of the sample is measured at five or more points using a Mitsutoyo laser hologram as a measuring device, and the measured values are simply averaged (arithmetic average) to obtain the average thickness t T [μm] is calculated. The measurement positions are selected randomly from the sample. Next, the back layer 14 of the sample is removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. After that, the thickness of the sample is measured again at five or more points using the above-mentioned laser hologram, and the measured values are simply averaged (arithmetic mean) to obtain the average thickness t B [μm] is calculated. The measurement positions are selected randomly from the sample. Then, the average thickness t of the back layer 14 is calculated from the following formula: b Calculate [μm]. t b [μm]=t T [μm]-t B [μm]
[0065] (Average thickness of magnetic recording medium) The upper limit of the average thickness (average total thickness) of the magnetic recording medium 10 is preferably 5.6 μm or less, more preferably 5.0 μm or less, particularly preferably 4.6 μm or less, and even more preferably 4.4 μm or less. When the average thickness of the magnetic recording medium 10 is 5.6 μm or less, the recording capacity that can be recorded in one data cartridge can be increased compared to that of a general magnetic recording medium. The lower limit of the average thickness of the magnetic recording medium 10 is not particularly limited, but is, for example, 3.5 μm or more.
[0066] The average thickness of the magnetic recording medium 10 is determined by the procedure explained above in determining the average thickness of the back layer 14 .
[0067] (Coercive force Hc1 in the perpendicular direction) The upper limit of the coercive force Hc1 in the perpendicular direction is 3000 Oe or less, more preferably 2900 Oe or less, and even more preferably 2850 Oe or less. A large coercive force Hc1 is preferable because it is less susceptible to the effects of thermal disturbance and demagnetizing fields, but if the coercive force Hc1 exceeds 3000 Oe, there is a risk that saturation recording with the recording head will become difficult, resulting in some areas that cannot be recorded and increased noise, which will result in a deterioration of the electromagnetic conversion characteristics (e.g., C / N).
[0068] The lower limit of the coercive force Hc1 in the perpendicular direction is preferably 2200 Oe or more, more preferably 2400 Oe or more, and even more preferably 2600 Oe or more. If the coercive force Hc1 is 2200 Oe or more, it is possible to suppress the deterioration of the electromagnetic conversion characteristics (e.g., C / N) in a high-temperature environment due to the influence of thermal disturbance and the influence of a demagnetizing field.
[0069] The coercive force Hc1 is obtained as follows. First, a measurement sample is cut out from the long magnetic recording medium 10, and the MH loop of the entire measurement sample is measured in the vertical direction (thickness direction) of the measurement sample using a vibrating sample magnetometer (VSM). Next, the coating film (underlayer 12, magnetic layer 13, back layer 14, etc.) is wiped off using acetone or ethanol, etc., leaving only the substrate 11 as a sample for background correction, and the MH loop of the substrate 11 is measured in the vertical direction (thickness direction) of the substrate 11 using a VSM. After that, the MH loop of the substrate 11 is subtracted from the MH loop of the entire measurement sample to obtain the MH loop after background correction. The coercive force Hc1 is obtained from the obtained MH loop. Note that all of the above MH loop measurements are performed at 25° C. Furthermore, no “demagnetization field correction” is performed when measuring the MH loop in the vertical direction of the magnetic recording medium 10.
[0070] (Coercive force Hc2 in the longitudinal direction) The upper limit of the coercive force Hc2 in the longitudinal direction is preferably 2000 Oe or less, more preferably 1900 Oe or less, and even more preferably 1800 Oe or less. When the coercive force Hc2 in the longitudinal direction is 2000 Oe or less, the magnetization reacts sensitively to the perpendicular magnetic field from the recording head, so that a good recording pattern can be formed.
[0071] The lower limit of the coercive force Hc2 in the longitudinal direction is preferably 1000 Oe or more. When the coercive force Hc2 in the longitudinal direction is 1000 Oe or more, demagnetization due to leakage flux from the recording head can be suppressed.
[0072] The above coercive force Hc2 is determined in the same manner as the coercive force Hc1 in the perpendicular direction, except that the MH loops of the entire measurement sample and the sample for background correction are measured in the direction corresponding to the longitudinal direction (running direction) of the magnetic recording medium 10.
[0073] (Hc2 / Hc1) The ratio Hc2 / Hc1 of the coercive force Hc1 in the perpendicular direction to the coercive force Hc2 in the longitudinal direction satisfies the relationship Hc2 / Hc1≦0.8, preferably Hc2 / Hc1≦0.75, more preferably Hc2 / Hc1≦0.7, even more preferably Hc2 / Hc1≦0.65, and particularly preferably Hc2 / Hc1≦0.6. When the coercive forces Hc1 and Hc2 satisfy the relationship Hc2 / Hc1≦0.8, the degree of perpendicular orientation of the magnetic powder can be increased. Therefore, the magnetization transition width can be reduced and a high-output signal can be obtained during signal reproduction, thereby improving the electromagnetic conversion characteristics (e.g., C / N). As described above, when Hc2 is small, the magnetization reacts sensitively to the magnetic field in the perpendicular direction from the recording head, so that a good recording pattern can be formed.
[0074] When the ratio Hc2 / Hc1 is Hc2 / Hc1≦0.8, it is particularly effective that the average thickness of the magnetic layer 13 is 90 nm or less. If the average thickness of the magnetic layer 13 exceeds 90 nm, when a ring-type head is used as a recording head, the lower region of the magnetic layer 13 (the region on the underlayer 12 side) is magnetized in the longitudinal direction, and the magnetic layer 13 may not be uniformly magnetized in the thickness direction. Therefore, even if the ratio Hc2 / Hc1 is Hc2 / Hc1≦0.8 (i.e., even if the degree of vertical orientation of the magnetic powder is increased), there is a risk that the electromagnetic conversion characteristics (e.g., C / N) cannot be improved.
[0075] The lower limit of Hc2 / Hc1 is not particularly limited, but is, for example, 0.5≦Hc2 / Hc1.
[0076] In addition, Hc2 / Hc1 represents the degree of vertical orientation of the magnetic powder, and the smaller Hc2 / Hc1, the higher the degree of vertical orientation of the magnetic powder. Below, the reason for using Hc2 / Hc1 as an index showing the degree of vertical orientation of the magnetic powder in this embodiment will be explained.
[0077] Conventionally, the squareness ratio SQ (=(Mr / Ms)×100, where Mr(emu): residual magnetization, Ms(emu): saturation magnetization) has generally been used as an index (parameter) indicating the degree of vertical orientation of magnetic powder. However, according to the findings of the present inventors, the squareness ratio SQ is not an appropriate index to indicate the degree of vertical orientation of magnetic powder for the following reasons. (1) The squareness ratio SQ varies depending on the value of the coercive force Hc of the magnetic powder. For example, as shown in Figure 5, when the coercive force Hc of the magnetic powder increases, the squareness ratio SQ also appears to increase. (2) The squareness ratio SQ is affected by the distortion of the MH loop due to overdispersion.
[0078] Therefore, in this embodiment, Hc2 / Hc1 is used as an index that more appropriately indicates the degree of orientation of the magnetic powder. Since the coercive forces Hc1 and Hc2 simply change depending on the orientation direction of the magnetic powder, Hc2 / Hc1 is a more appropriate index that more appropriately indicates the degree of orientation of the magnetic powder.
[0079] (SFD) In the SFD (Switching Field Distribution) curve of the magnetic recording medium 10, the peak ratio X / Y between the main peak height X and the sub-peak height Y near zero magnetic field is preferably 3.0 or more, more preferably 5.0 or more, even more preferably 7.0 or more, particularly preferably 10.0 or more, and most preferably 20.0 or more (see FIG. 5). When the peak ratio X / Y is 3.0 or more, it is possible to suppress the inclusion of a large amount of low coercive force components specific to ε-iron oxide (e.g., soft magnetic particles and superparamagnetic particles) in the magnetic powder in addition to the ε-iron oxide particles that contribute to actual recording. Therefore, it is possible to suppress the deterioration of the magnetization signal recorded on the adjacent track due to the leakage magnetic field from the recording head, and therefore it is possible to obtain better electromagnetic conversion characteristics (e.g., C / N). The upper limit of the peak ratio X / Y is not particularly limited, but is, for example, 100 or less.
[0080] The above peak ratio X / Y is obtained as follows. First, an MH loop after background correction is obtained in the same manner as in the above-mentioned method for measuring the coercive force Hc1. Next, an SFD curve is calculated from the obtained MH loop. The SFD curve may be calculated using a program provided with the measuring device or other programs. The peak ratio X / Y is calculated by taking the absolute value of the point where the calculated SFD curve crosses the Y axis (dM / dH) as "Y" and the height of the main peak observed in the vicinity of the coercive force Hc1 in the MH loop as "X."
[0081] (Activation volume V act ) Activation volume V act However, preferably 8000 nm 3 Less than 6000 nm, more preferably 3 Less than or equal to 5000 nm, and even more preferably less than 5000 nm 3 Below 4000 nm, particularly preferably 3 Below 3000 nm, most preferably 3 The activation volume V is act 8000nm 3 At or below this value, the magnetic powder is well dispersed, reducing the bit inversion area and preventing the magnetic signal recorded on the adjacent track from being deteriorated by the leakage magnetic field from the recording head, resulting in better electromagnetic conversion characteristics (e.g., C / N).
[0082] The activation volume V act is calculated by the following formula derived by Street & Woolley. V act (nm 3 )=k B ×T×Χ irr / (μ0×Ms×S) (However, k B : Boltzmann constant (1.38×10 -23 J / K), T: Temperature (K), Χ irr : irreversible magnetic susceptibility, μ0: vacuum permeability, S: magnetic viscosity coefficient, Ms: saturation magnetization (emu / cm 3 ))
[0083] The irreversible magnetic susceptibility Χ substituted into the above formula irr The saturation magnetization Ms and magnetic viscosity coefficient S are obtained using VSM as follows. The measurement direction using VSM is the vertical direction. The measurement using VSM is performed at 25° C. on a measurement sample cut out from a long magnetic recording medium 10. When measuring the MH loop in the vertical direction, no "demagnetization correction" is performed.
[0084] (irreversible magnetic susceptibility Χ irr ) Irreversible magnetic susceptibility Χ irr is defined as the slope of the remanent magnetization curve (DCD curve) near the remanent coercivity Hr. First, a magnetic field of -1193 kA / m (15 kOe) is applied to the entire magnetic recording medium 10, and the magnetic field is returned to zero to create a remanent magnetization state. After that, a magnetic field of approximately 15.9 kA / m (200 Oe) is applied in the opposite direction, and the magnetic field is returned to zero again to measure the amount of remanent magnetization. After that, a magnetic field 15.9 kA / m larger than the previous applied magnetic field is applied, and the measurement is repeated to return the magnetic field to zero, and the amount of remanent magnetization is plotted against the applied magnetic field to measure the DCD curve. From the obtained DCD curve, the point where the amount of magnetization is zero is taken as the remanent coercivity Hr, and the DCD curve is differentiated to determine the slope of the DCD curve for each magnetic field. In the slope of this DCD curve, the slope near the remanent coercivity Hr is Χ irr It becomes.
[0085] (Saturation magnetization Ms) First, a background-corrected MH loop is obtained in the same manner as in the measurement of the coercive force Hc1 described above. Next, the value of the saturation magnetization Ms(emu) of the obtained MH loop and the volume (cm 3 ) to Ms(emu / cm 3 ) is calculated. The volume of the magnetic layer 13 is found by multiplying the area of the measurement sample by the average thickness of the magnetic layer 13. The method for calculating the average thickness of the magnetic layer 13, which is necessary for calculating the volume of the magnetic layer 13, is as described above.
[0086] (Magnetic viscosity coefficient S) First, a magnetic field of -1193 kA / m (15 kOe) is applied to the entire magnetic recording medium 10 (measurement sample), and the magnetic field is returned to zero to create a state of residual magnetization. After that, a magnetic field equivalent to the value of the residual coercivity Hr obtained from the DCD curve is applied in the opposite direction. With the magnetic field applied, the amount of magnetization is continuously measured at regular time intervals for 1000 seconds. The magnetic viscosity coefficient S is calculated by referring to the relationship between time t and amount of magnetization M(t) obtained in this way according to the following formula. M(t) = M0 + S × ln(t) (where M(t) is the amount of magnetization at time t, M0 is the initial amount of magnetization, S is the magnetic viscosity coefficient, and ln(t) is the natural logarithm of time.)
[0087] [1.2 Manufacturing method of magnetic recording media] Next, a method for manufacturing the magnetic recording medium 10 having the above-mentioned configuration will be described. First, a paint for forming the undercoat layer is prepared by kneading and dispersing non-magnetic powder, binder, etc. in a solvent. Next, a paint for forming the magnetic layer is prepared by kneading and dispersing magnetic powder, binder, etc. in a solvent. The following solvents, dispersing devices, and kneading devices can be used to prepare the paint for forming the magnetic layer and the paint for forming the undercoat layer.
[0088] Examples of the solvent used in preparing the coating material include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, alcohol-based solvents such as methanol, ethanol, and propanol, ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, propyl acetate, ethyl lactate, and ethylene glycol acetate, ether-based solvents such as diethylene glycol dimethyl ether, 2-ethoxyethanol, tetrahydrofuran, and dioxane, aromatic hydrocarbon-based solvents such as benzene, toluene, and xylene, and halogenated hydrocarbon-based solvents such as methylene chloride, ethylene chloride, carbon tetrachloride, chloroform, and chlorobenzene. These may be used alone or in appropriate mixture.
[0089] Examples of the kneading device used in the preparation of the above-mentioned coating material include, but are not limited to, a continuous twin-screw kneader, a continuous twin-screw kneader capable of diluting in multiple stages, a kneader, a pressure kneader, a roll kneader, etc. Examples of the dispersing device used in the preparation of the above-mentioned coating material include, but are not limited to, a roll mill, a ball mill, a horizontal sand mill, a vertical sand mill, a spike mill, a pin mill, a tower mill, a pearl mill (for example, "DCP Mill" manufactured by Eirich Co., Ltd.), a homogenizer, an ultrasonic dispersing machine, etc.
[0090] Next, a coating material for forming a base layer is applied to one main surface of the substrate 11 and dried to form the base layer 12. Subsequently, a coating material for forming a magnetic layer is applied to the base layer 12 and dried to form the magnetic layer 13 on the base layer 12. During drying, the magnetic powder is magnetically oriented in the thickness direction of the substrate 11, for example, by a solenoid coil. Also, during drying, the magnetic powder may be magnetically oriented in the running direction (longitudinal direction) of the substrate 11, and then magnetically oriented in the thickness direction of the substrate 11, for example, by a solenoid coil. By carrying out such a magnetic field orientation process, the ratio Hc2 / Hc1 can be lowered. Therefore, the degree of vertical orientation of the magnetic powder can be improved. After the magnetic layer 13 is formed, a back layer 14 is formed on the other main surface of the substrate 11. This results in a magnetic recording medium 10.
[0091] The ratio Hc2 / Hc1 is set to a desired value by, for example, adjusting the strength of the magnetic field applied to the coating film of the magnetic layer forming paint, the concentration of the solid content in the magnetic layer forming paint, and the drying conditions (drying temperature and drying time) of the coating film of the magnetic layer forming paint. The strength of the magnetic field applied to the coating film is preferably two to three times the coercive force of the magnetic powder. In order to further increase the ratio Hc2 / Hc1, it is preferable to improve the dispersion state of the magnetic powder in the magnetic layer forming paint. In addition, in order to further increase the ratio Hc2 / Hc1, it is also effective to magnetize the magnetic powder before the magnetic layer forming paint enters an orientation device for magnetic field orientation of the magnetic powder. The above-mentioned methods for adjusting the ratio Hc2 / Hc1 may be used alone or in combination of two or more.
[0092] The magnetic recording medium 10 thus obtained is then rewound around a large diameter core and hardened. Finally, the magnetic recording medium 10 is calendered and then cut to a predetermined width (e.g., 1 / 2 inch width). In this manner, the desired elongated magnetic recording medium 10 is obtained.
[0093] [1.3 Configuration of recording / playback device] Next, with reference to FIG. 6, a description will be given of the configuration of a recording / reproducing device 30 that performs recording and reproducing on the magnetic recording medium 10 having the above-mentioned configuration.
[0094] The recording / reproducing device 30 has a configuration capable of being loaded with a magnetic recording medium cartridge 10A. For ease of explanation, the recording / reproducing device 30 will be described as having a configuration capable of being loaded with one magnetic recording medium cartridge 10A, but the recording / reproducing device 30 may have a configuration capable of being loaded with a plurality of magnetic recording medium cartridges 10A.
[0095] The recording / playback device 30 is connected to information processing devices such as a server 41 and a personal computer (hereinafter referred to as "PC") 42 via a network 43, and is configured to be able to record data supplied from these information processing devices onto the magnetic recording medium cartridge 10A.
[0096] As shown in FIG. 6, the recording / playback device 30 includes a spindle 31, a reel 32 on the recording / playback device 30 side, a spindle drive device 33, a reel drive device 34, a number of guide rollers 35, a head unit 36, a communication interface (hereinafter, I / F) 37, and a control device 38.
[0097] The spindle 31 is configured to be able to mount the magnetic recording medium cartridge 10A. The magnetic recording medium cartridge 10A is, for example, compliant with the LTO (Linear Tape Open) standard, and rotatably accommodates a single reel 10C around which the magnetic recording medium 10 is wound in a cartridge case 10B. A V-shaped servo pattern is recorded in advance as a servo signal on the magnetic recording medium 10. The reel 32 is configured to be able to fix the tip of the magnetic recording medium 10 pulled out from the magnetic recording medium cartridge 10A.
[0098] The spindle drive device 33 is a device that rotates the spindle 31. The reel drive device 34 is a device that rotates the reel 32. When recording or reproducing data on the magnetic recording medium 10, the spindle drive device 33 and the reel drive device 34 rotate the spindle 31 and the reel 32, thereby running the magnetic recording medium 10. The guide roller 35 is a roller for guiding the running of the magnetic recording medium 10.
[0099] The head unit 36 includes a plurality of recording heads for recording data signals on the magnetic recording medium 10, a plurality of reproducing heads for reproducing the data signals recorded on the magnetic recording medium 10, and a plurality of servo heads for reproducing the servo signals recorded on the magnetic recording medium 10. As the recording heads, for example, ring-type heads can be used, but the type of recording head is not limited to this.
[0100] The communication I / F 37 is for communicating with information processing devices such as a server 41 and a PC 42 , and is connected to a network 43 .
[0101] The control device 38 controls the entire recording / reproducing device 30. For example, in response to a request from the information processing device, such as the server 41 or the PC 42, the control device 38 records a data signal supplied from the information processing device on the magnetic recording medium 10 by the head unit 36. In addition, in response to a request from the information processing device, such as the server 41 or the PC 42, the control device 38 reproduces the data signal recorded on the magnetic recording medium 10 by the head unit 36, and supplies it to the information processing device.
[0102] [1.4 Effects] In the magnetic recording medium 10 according to the first embodiment, (1) the average thickness of the magnetic layer 13 is 90 nm or less, (2) the average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, (3) the coercive force Hc1 in the perpendicular direction is 3000 Oe or less, and (4) the coercive force Hc1 in the perpendicular direction and the coercive force Hc2 in the longitudinal direction satisfy the relationship Hc2 / Hc1≦0.8. This can improve the electromagnetic conversion characteristics (e.g., C / N).
[0103] [1.5 Modifications] (Variation 1) In the above-mentioned first embodiment, the ε-iron oxide particles have a shell portion 22 with a two-layer structure, but as shown in Fig. 7, the ε-iron oxide particles may have a shell portion 23 with a single layer structure. In this case, the shell portion 23 has a similar structure to the first shell portion 22a. However, from the viewpoint of suppressing deterioration of the properties of the ε-iron oxide particles, it is preferable that the ε-iron oxide particles have a shell portion 22 with a two-layer structure as in the above-mentioned first embodiment.
[0104] (Variation 2) In the above-mentioned first embodiment, the ε iron oxide particles have a core-shell structure, but the ε iron oxide particles may contain an additive instead of the core-shell structure, or may have a core-shell structure and contain an additive. In this case, a part of Fe in the ε iron oxide particles is substituted with the additive. By containing an additive in the ε iron oxide particles, the coercive force Hc of the ε iron oxide particles as a whole can be adjusted to a coercive force Hc suitable for recording, thereby improving ease of recording. The additive is a metal element other than iron, preferably a trivalent metal element, more preferably at least one of Al, Ga and In, and even more preferably at least one of Al and Ga.
[0105] Specifically, ε-iron oxide containing additives is ε-Fe 2-x M x O3 crystal (wherein M is a metal element other than iron, preferably a trivalent metal element, more preferably at least one of Al, Ga and In, and even more preferably at least one of Al and Ga. x is, for example, 0 <x<1である。)である。
[0106] (Variation 3) The magnetic powder may contain a powder of nanoparticles containing hexagonal ferrite (hereinafter referred to as "hexagonal ferrite particles") instead of a powder of ε iron oxide particles. The hexagonal ferrite particles have, for example, a hexagonal plate shape or a nearly hexagonal plate shape. The hexagonal ferrite preferably contains at least one of Ba, Sr, Pb and Ca, more preferably at least one of Ba and Sr. The hexagonal ferrite may specifically be, for example, barium ferrite or strontium ferrite. The barium ferrite may further contain at least one of Sr, Pb and Ca in addition to Ba. The strontium ferrite may further contain at least one of Ba, Pb and Ca in addition to Sr.
[0107] More specifically, hexagonal ferrite has the general formula MFe 12 O 19The average composition is represented by the formula: where M is, for example, at least one metal selected from Ba, Sr, Pb, and Ca, and preferably at least one metal selected from Ba and Sr. M may be a combination of Ba and at least one metal selected from the group consisting of Sr, Pb, and Ca. M may also be a combination of Sr and at least one metal selected from the group consisting of Ba, Pb, and Ca. In the above general formula, a part of Fe may be substituted with another metal element.
[0108] When the magnetic powder contains hexagonal ferrite particles, the average particle size of the magnetic powder is preferably 30 nm or less, more preferably 12 nm to 25 nm, and even more preferably 15 nm to 22 nm. When the average particle size of the magnetic powder is 30 nm or less, good electromagnetic conversion characteristics (e.g., C / N) can be obtained in a high recording density magnetic recording medium 10. On the other hand, when the average particle size of the magnetic powder is 12 nm or more, the dispersibility of the magnetic powder is further improved, and better electromagnetic conversion characteristics (e.g., C / N) can be obtained. When the magnetic powder contains hexagonal ferrite particles, the average aspect ratio of the magnetic powder is the same as that of the first embodiment described above.
[0109] The average particle size and average aspect ratio of the magnetic powder are obtained as follows. First, the magnetic recording medium 10 to be measured is processed by the FIB method or the like to produce a thin piece, and the cross section of the thin piece is observed by TEM. Next, 50 magnetic powder particles oriented at an angle of 75 degrees or more to the horizontal direction are randomly selected from the TEM photograph, and the maximum plate thickness DA of each magnetic powder is measured. Next, the maximum plate thicknesses DA of the 50 measured magnetic powder particles are simply averaged (arithmetic mean) to obtain the average maximum plate thickness DAave.
[0110] Next, the surface of the magnetic layer 13 of the magnetic recording medium 10 is observed by TEM. Next, 50 magnetic powder particles are randomly selected from the TEM photograph, and the maximum plate diameter DB of each magnetic powder particle is measured. Here, the maximum plate diameter DB means the maximum distance between two parallel lines drawn from all angles so as to be tangent to the outline of the magnetic powder particle (so-called maximum Feret diameter). Next, the maximum plate diameters DB of the 50 measured magnetic powder particles are simply averaged (arithmetic mean) to obtain the average maximum plate diameter DBave. The average maximum plate diameter DBave thus obtained is the average particle size of the magnetic powder particle. Next, the average aspect ratio (DBave / DAave) of the magnetic powder particle is obtained from the average maximum plate thickness DAave and the average maximum plate diameter DBave.
[0111] When the magnetic powder comprises a powder of hexagonal ferrite particles, the average particle volume of the magnetic powder is preferably 5900 nm 3 Less than or equal to 500 nm, preferably 3 More than 3400nm 3 Less than or equal to 1000 nm, and even more preferably less than 1000 nm 3 More than 2500nm 3 The average particle volume of the magnetic powder is 5900 nm or less. 3 If the average particle size of the magnetic powder is 30 nm or less, the same effect as when the average particle volume of the magnetic powder is 500 nm or less can be obtained. 3 If the average particle size of the magnetic powder is 12 nm or more, the same effect as in the case where the average particle size of the magnetic powder is 12 nm or more can be obtained.
[0112] The average particle volume of the magnetic powder is calculated as follows. First, the average maximum plate thickness DAave and the average maximum plate diameter DBave are calculated in the same manner as in the above-mentioned method for calculating the average particle size of the magnetic powder. Next, the average particle volume V of the magnetic powder is calculated using the following formula. V=3√3 / 8×DAave×DBave 2
[0113] (Variation 4) The magnetic powder may contain a powder of nanoparticles containing Co-containing spinel ferrite (hereinafter referred to as "cobalt ferrite particles") instead of the powder of ε iron oxide particles. The cobalt ferrite particles preferably have uniaxial anisotropy. The cobalt ferrite particles have, for example, a cubic or nearly cubic shape. The Co-containing spinel ferrite may further contain at least one of Ni, Mn, Al, Cu, and Zn in addition to Co.
[0114] The Co-containing spinel ferrite has, for example, an average composition represented by the following formula (1). Co x M y FeO Z (1) (In formula (1), M is, for example, at least one metal selected from the group consisting of Ni, Mn, Al, Cu, and Zn. x is a value within the range of 0.4≦x≦1.0. y is a value within the range of 0≦y≦0.3. However, x and y satisfy the relationship of (x+y)≦1.0. z is a value within the range of 3≦z≦4. A part of Fe may be substituted with another metal element.)
[0115] When the magnetic powder contains cobalt ferrite particles, the average particle size of the magnetic powder is preferably 25 nm or less, more preferably 8 nm or more and 23 nm or less. When the average particle size of the magnetic powder is 25 nm or less, good electromagnetic conversion characteristics (e.g., C / N) can be obtained in a high recording density magnetic recording medium 10. On the other hand, when the average particle size of the magnetic powder is 8 nm or more, the dispersibility of the magnetic powder is further improved, and better electromagnetic conversion characteristics (e.g., C / N) can be obtained. When the magnetic powder contains cobalt ferrite particles, the average aspect ratio of the magnetic powder is the same as that of the first embodiment described above. The average particle size and average aspect ratio of the magnetic powder can be calculated in the same manner as that of the first embodiment described above.
[0116] The average particle volume of the magnetic powder is preferably 15,000 nm 3 Less than or equal to 500 nm, preferably 3 More than 12000nm 3The average particle volume of the magnetic powder is 15,000 nm or less. 3 If the average particle size of the magnetic powder is 25 nm or less, the same effect as when the average particle volume of the magnetic powder is 500 nm or less can be obtained. 3 With this or more, the same effect as when the average particle size of the magnetic powder is 8 nm or more can be obtained. Note that the average particle volume of the magnetic powder is calculated in the same manner as in the first embodiment described above (the method for calculating the average particle volume when the ε iron oxide particles are cubic or nearly cubic).
[0117] (Variation 5) As shown in FIG. 8, the magnetic recording medium 10 may further include a barrier layer 15 provided on at least one surface of the substrate 11. The barrier layer 15 is a layer for suppressing dimensional changes of the substrate 11 according to the environment. For example, one example of a cause of the dimensional changes is the hygroscopicity of the substrate 11, and the provision of the barrier layer 15 can reduce the rate at which moisture penetrates into the substrate 11. The barrier layer 15 includes, for example, a metal or a metal oxide. As the metal, for example, at least one of Al, Cu, Co, Mg, Si, Ti, V, Cr, Mn, Fe, Ni, Zn, Ga, Ge, Y, Zr, Mo, Ru, Pd, Ag, Ba, Pt, Au, and Ta can be used. As the metal oxide, for example, a metal oxide including one or more of the above metals can be used. More specifically, for example, at least one of Al2O3, CuO, CoO, SiO2, Cr2O3, TiO2, Ta2O5, and ZrO2 can be used. The barrier layer 15 may also contain diamond-like carbon (DLC) or diamond.
[0118] The average thickness of the barrier layer 15 is preferably 20 nm or more and 1000 nm or less, more preferably 50 nm or more and 1000 nm or less. The average thickness of the barrier layer 15 is determined in the same manner as the average thickness of the magnetic layer 13. However, the magnification of the TEM image is appropriately adjusted according to the thickness of the barrier layer 15.
[0119] (Variation 6) The magnetic recording medium 10 according to the first embodiment may be used in a library device. In this case, the library device may include a plurality of recording / reproducing devices 30 according to the first embodiment.
[0120] <2. Second embodiment> (Stretchability and tension control of magnetic recording media) The elasticity of the magnetic recording medium 10 and tension control of the magnetic recording medium 10 by the recording and reproducing device 30 will be described below. In the LTO standard, the number of recording tracks is rapidly increasing due to the demand for high density data recording. In such a case, the recording track width becomes narrow, and even a slight variation in the width of the magnetic recording medium 10 may become a problem.
[0121] For example, suppose that predetermined data is stored in the magnetic recording medium 10 by the recording and reproducing device 30, and then (for example, after a certain period of storage), the data recorded on the magnetic recording medium 10 is reproduced by the recording and reproducing device 30. In such a case, if the width of the magnetic recording medium 10 during data reproduction varies even slightly compared to the width of the magnetic recording medium 10 during data recording, off-track (the data read head is positioned on the wrong recording track) may occur. As a result, the data recorded on the magnetic recording medium 10 may not be reproduced accurately, and an error may occur.
[0122] Causes of the width fluctuation of the magnetic recording medium 10 include, for example, temperature fluctuation, humidity fluctuation, etc. Generally, a method is used in which the magnetic recording medium 10 is designed so that the magnetic recording medium 10 does not expand or contract, thereby dealing with the width fluctuation of the magnetic recording medium 10. However, it is practically impossible to completely prevent the magnetic recording medium 10 from expanding or contracting.
[0123] Therefore, in this embodiment, rather than making the magnetic recording medium 10 difficult to expand and contract, a method is used in which the magnetic recording medium 10 is made somewhat easier to expand and contract, and the tension of the magnetic recording medium 10 (the conveying direction of the magnetic recording medium 10) is controlled (increased or decreased) on the recording and reproducing device 30 side. That is, in this embodiment, the magnetic recording medium 10 is configured so that the width of the magnetic recording medium 10 can be adjusted by increasing or decreasing the tension in the longitudinal direction.
[0124] Specifically, when reproducing a data signal, the recording and reproducing device 30 increases the tension in the longitudinal direction of the magnetic recording medium 10 as necessary (when the width of the magnetic recording medium 10 is widened), thereby reducing the width of the magnetic recording medium 10. Also, when reproducing a data signal, the recording and reproducing device 30 decreases the tension in the longitudinal direction of the magnetic recording medium 10 as necessary (when the width of the magnetic recording medium 10 is narrowed), thereby increasing the width of the magnetic recording medium 10. Note that the recording and reproducing device 30 may control the tension in the longitudinal direction of the magnetic recording medium 10 not only when reproducing a data signal, but also when recording a data signal.
[0125] According to this method, when the width of the magnetic recording medium 10 fluctuates due to temperature or the like, it is possible to adjust the width of the magnetic recording medium 10 as necessary to make the width of the magnetic recording medium 10 constant. Therefore, it is considered that off-track can be suppressed and data recorded on the magnetic recording medium 10 can be accurately reproduced.
[0126] (The load when the magnetic recording medium is stretched by 1% in the longitudinal direction) The load [N] when the magnetic recording medium 10 is elongated by 1% in the longitudinal direction (hereinafter simply referred to as "longitudinal 1% elongation load") is preferably 0.6 N or less, more preferably 0.58 N or less, even more preferably 0.55 N or less, particularly preferably 0.5 N or less, and most preferably 0.45 N or less. When the longitudinal 1% elongation load is 0.6 N or less, the magnetic recording medium 10 has high elasticity, so that the width of the magnetic recording medium 10 can be easily adjusted by tension control. Therefore, even if the width of the magnetic recording medium 10 fluctuates due to temperature or the like (for example, under an accelerated deterioration environment such as 45°C for one month), the width of the magnetic recording medium 10 can be made constant by adjusting the width of the magnetic recording medium 10. Therefore, off-track can be suppressed, and data recorded on the magnetic recording medium 10 can be accurately reproduced.
[0127] Furthermore, since it becomes possible to accommodate slight variations in the width of the magnetic recording medium 10, as a result, the number of recording tracks on the magnetic recording medium 10 can be increased, enabling higher density data recording to be achieved.
[0128] The longitudinal 1% elongation load is determined as follows. First, a magnetic recording medium 10 with a tape width of 12.65 mm is cut to a length (longitudinal direction) of 100 mm to prepare a sample of the magnetic recording medium 10 with a width of 12.65 mm and a length of 100 mm. The sample is then set in a measuring device, which stretches the sample in the longitudinal direction and measures the load at that time. An AUTO GRAPH AG-100D manufactured by Shimadzu Corporation is used as the measuring device. The measurement temperature is room temperature, and the pulling speed is 10 mm / min.
[0129] Fig. 10 is a diagram showing the relationship between longitudinal elongation [%] and load [N]. As shown in Fig. 10, the relationship between elongation and load is nonlinear when the sample is barely elongated (when the elongation is close to 0), and approaches linear when the sample is elongated to a certain extent. Therefore, the value of the longitudinal elongation load at 1% is not the value at the nonlinear point, but the value at the point close to linear.
[0130] Specifically, in a longitudinal tensile test of the magnetic recording medium 10, if the load when the elongation rate of the magnetic recording medium 10 is 0.5% is σ0.5 [N] and the load when the elongation rate of the magnetic recording medium 10 is 1.5% is σ1.5 [N], the longitudinal 1% elongation load is expressed by the following formula. Longitudinal 1% elongation load [N] = σ1.5-σ0.5
[0131] This 1% longitudinal elongation load is a value that indicates the difficulty of the magnetic recording medium 10 to expand and contract in the longitudinal direction due to an external force; the larger this value, the more difficult it is for the magnetic recording medium 10 to expand and contract in the longitudinal direction due to an external force, and the smaller this value, the more easily the magnetic recording medium 10 can expand and contract in the longitudinal direction due to an external force.
[0132] The 1% longitudinal elongation load is a value related to the longitudinal direction of the magnetic recording medium 10, but it also correlates with the difficulty of the magnetic recording medium 10 to expand and contract in the width direction. In other words, the larger the value of this 1% longitudinal elongation load, the more difficult it is for the magnetic recording medium 10 to expand and contract in the width direction due to an external force, and the smaller this value, the more easily the magnetic recording medium 10 expands and contracts in the width direction due to an external force.
[0133] Since it is easier to adjust the width of the magnetic recording medium 10 by tension control if the magnetic recording medium 10 is easily stretchable in the width direction, a smaller 1% elongation load in the longitudinal direction is advantageous.
[0134] (Shrinkage rate in the longitudinal direction of the magnetic recording medium 10) The longitudinal shrinkage rate of the magnetic recording medium 10 (hereinafter simply referred to as "longitudinal shrinkage rate") is preferably 0.1% or less, and more preferably 0.09% or less, 0.08% or less, 0.07% or less, 0.06% or less, or 0.05% or less. If the longitudinal shrinkage rate is 0.1% or less, the width of the magnetic recording medium 10 is less likely to vary due to temperature or the like (for example, even under a long-term accelerated deterioration environment such as 45°C for one month). Therefore, off-track can be suppressed, and data recorded on the magnetic recording medium 10 can be accurately reproduced.
[0135] In this embodiment, the magnetic recording medium 10 expands and contracts relatively easily when an external force is applied (tension control), but is configured so that the magnetic recording medium 10 does not expand and contract easily due to environmental changes such as temperature fluctuations.
[0136] The longitudinal shrinkage rate is determined as follows: First, the magnetic recording medium 10 is cut to a length (longitudinal direction) of 50 mm to prepare a sample of the magnetic recording medium 10. Then, two indentations are made with a needle on the surface of the magnetic layer 13 of this sample at positions 15 mm apart in the longitudinal direction.
[0137] Next, using a Topcon measuring microscope TMU-220ES and coordinate measuring machine CA-1B, the distance L1 between the two indentations is measured at room temperature. The sample is then stored (aged) for 72 hours in a thermostatic chamber at 60°C and 10% RH without tension applied to the sample. The sample is then removed from the thermostatic chamber and left at room temperature for one hour, and the distance L2 between the two indentations is measured using the same method as above.
[0138] Then, based on the distance L1 (before aging) and the distance L2 (after aging), the longitudinal shrinkage rate [%] is calculated by the following formula. Longitudinal shrinkage ratio = {(L1-L2) / L1} x 100
[0139] This longitudinal shrinkage rate is a value that indicates the ease with which the magnetic recording medium 10 expands and contracts in the longitudinal direction due to heat in a tension-free state; the larger this value, the more easily the magnetic recording medium 10 expands and contracts in the longitudinal direction due to heat, and the smaller this value, the less likely the magnetic recording medium 10 will expand and contract in the longitudinal direction due to heat.
[0140] The longitudinal shrinkage rate is a value related to the longitudinal direction of the magnetic recording medium 10, but it also correlates with the ease of expansion and contraction in the width direction of the magnetic recording medium 10. In other words, the larger the value of this longitudinal shrinkage rate, the more easily the magnetic recording medium 10 expands and contracts in the width direction due to heat, and the smaller this value, the less likely the magnetic recording medium 10 to expand and contract in the width direction due to heat.
[0141] As described above, from the viewpoint of tension control, it is advantageous for the magnetic recording medium 10 to expand and contract. On the other hand, it is not preferable for the magnetic recording medium 10 to expand and contract due to environmental changes such as temperature changes, as this will induce off-track. Therefore, it is advantageous for the longitudinal shrinkage rate to be small.
[0142] ((TL-TB) / TB) When the average thickness of the substrate 11 is TB and the average thickness of the magnetic recording medium 10 is TL, the value of (TL-TB) / TB is preferably 0.41 or less, more preferably 0.39 or less, even more preferably 0.37 or less, and particularly preferably 0.35 or less. When the value of (TL-TB) / TB is 0.41 or less, the elasticity of the magnetic recording medium 10 due to an external force is further increased, so that the width of the magnetic recording medium 10 can be further easily adjusted by tension control. Therefore, off-track can be further appropriately suppressed, and data recorded on the magnetic recording medium 10 can be reproduced more accurately.
[0143] The denominator of (TL-TB) / TB represents the average thickness TB of the substrate 11, and the numerator represents the average thickness (TL-TB) of the coating film (magnetic layer 13, underlayer 12, and back layer 14). The average thickness of the coating film is the average thickness TL of the magnetic recording medium 10 minus the average thickness TB of the substrate 11. In other words, (TL-TB) / TB means the ratio of the average thickness (TL-TB) of the coating film to the average thickness TB of the substrate 11. Here, the coating film is less likely to expand or contract due to external forces compared to the substrate 11. If the average thickness TB of the substrate 11 is fixed and the average thickness (TL-TB) of the coating film is increased, the value of (TL-TB) / TB will be large, but in this case, the magnetic recording medium 10 will be less likely to expand or contract.
[0144] The value of (TL-TB) / TB correlates with the difficulty of the magnetic recording medium 10 to expand and contract due to an external force, and the larger this value, the more difficult it is for the magnetic recording medium 10 to expand and contract due to an external force, and the smaller this value, the more easily the magnetic recording medium 10 will expand and contract due to an external force. Therefore, from the viewpoint of tension control, a smaller value of (TL-TB) / TB is advantageous.
[0145] (Young's modulus in the longitudinal direction of the magnetic recording medium) The Young's modulus in the longitudinal direction of the magnetic recording medium 10 is preferably 8.5 GPa or less, more preferably 8.3 GPa or less, even more preferably 7.9 GPa or less, particularly preferably 7.5 GPa or less, and most preferably 7.1 GPa or less. When the Young's modulus in the longitudinal direction of the magnetic recording medium 10 is 8.5 GPa or less, the magnetic recording medium 10 has a higher elasticity due to an external force, so that the width of the magnetic recording medium 10 can be adjusted more easily by tension control. Therefore, off-track can be more appropriately suppressed, and data recorded on the magnetic recording medium 10 can be reproduced more accurately.
[0146] The Young's modulus in the longitudinal direction of the magnetic recording medium 10 is a value that indicates the resistance of the magnetic recording medium 10 to expansion and contraction in the longitudinal direction due to an external force; the larger this value, the more difficult it is for the magnetic recording medium 10 to expand and contract in the longitudinal direction due to an external force, and the smaller this value, the more easily the magnetic recording medium 10 expands and contracts in the longitudinal direction due to an external force.
[0147] The Young's modulus in the longitudinal direction of the magnetic recording medium 10 is a value related to the longitudinal direction of the magnetic recording medium 10, but it also correlates with the difficulty of the magnetic recording medium 10 to expand and contract in the width direction. In other words, the larger this value, the more difficult it is for the magnetic recording medium 10 to expand and contract in the width direction due to an external force, and the smaller this value, the more easily the magnetic recording medium 10 expands and contracts in the width direction due to an external force. Therefore, from the viewpoint of tension control, it is advantageous for the magnetic recording medium 10 to have a smaller Young's modulus in the longitudinal direction.
[0148] The Young's modulus in the longitudinal direction of the magnetic recording medium 10 is measured using a tensile tester (AG-100D, manufactured by Shimadzu Corporation). A measurement sample is prepared by cutting the magnetic recording medium 10 to a length of 180 mm. A jig capable of fixing the width (1 / 2 inch) of the measurement sample is attached to the tensile tester, and the top and bottom of the measurement sample are fixed. The distance is set to 100 mm. After the measurement sample is chucked, stress is gradually applied in the direction in which the measurement sample is pulled. The pulling speed is set to 0.1 mm / min. The Young's modulus is calculated from the change in stress and the amount of elongation at this time using the following formula. E = (ΔN / S) / (Δx / L) × 10 -3 ΔN: Change in stress (N) S: Cross-sectional area of the test piece (mm 2 ) Δx: Elongation (mm) L: Distance between gripping jigs (mm) The stress range is set to 0.5N to 1.0N, and the change in stress (ΔN) and the amount of elongation (Δx) at this point are used in the calculation.
[0149] (Young's modulus in the longitudinal direction of the base 11) The Young's modulus in the longitudinal direction of the substrate 11 is preferably 8.0 GPa or less, more preferably 7.8 GPa or less, even more preferably 7.4 GPa or less, particularly preferably 7.0 GPa or less, and most preferably 6.4 GPa or less. When the Young's modulus in the longitudinal direction of the substrate 11 is 8.0 GPa or less, the elasticity of the magnetic recording medium 10 due to an external force is further increased, so that the width of the magnetic recording medium 10 can be further easily adjusted by tension control. Therefore, off-track can be further appropriately suppressed, and data recorded on the magnetic recording medium 10 can be reproduced more accurately.
[0150] The Young's modulus in the longitudinal direction of the substrate 11 is determined as follows. First, the underlayer 12, the magnetic layer 13, and the back layer 14 are removed from the magnetic recording medium 10 to obtain the substrate 11. Using this substrate 11, the Young's modulus in the longitudinal direction of the substrate 11 is determined in the same manner as for the Young's modulus in the longitudinal direction of the magnetic recording medium 10.
[0151] The thickness of the substrate 11 accounts for more than half of the total thickness of the magnetic recording medium 10. Therefore, the Young's modulus in the longitudinal direction of the substrate 11 correlates with the difficulty of the magnetic recording medium 10 to expand and contract due to an external force, and the larger this value is, the more difficult it is for the magnetic recording medium 10 to expand and contract in the width direction due to an external force, and the smaller this value is, the more easily the magnetic recording medium 10 will expand and contract in the width direction due to an external force.
[0152] The Young's modulus of the substrate 11 in the longitudinal direction is a value related to the magnetic recording medium 10 in the longitudinal direction, but it also correlates with the difficulty of the magnetic recording medium 10 to expand and contract in the width direction. In other words, the larger this value, the more difficult it is for the magnetic recording medium 10 to expand and contract in the width direction due to an external force, and the smaller this value, the more easily the magnetic recording medium 10 expands and contracts in the width direction due to an external force. Therefore, from the viewpoint of tension control, it is advantageous for the substrate 11 to have a smaller Young's modulus in the longitudinal direction.
[0153] (Average thickness of magnetic recording medium) The average thickness TL of the magnetic recording medium 10 is preferably 5.6 μm or less, more preferably 5.0 μm or less, even more preferably 4.6 μm or less, and particularly preferably 4.4 μm or less. When the average thickness TL of the magnetic recording medium 10 is 5.6 μm or less, the elasticity of the magnetic recording medium 10 due to an external force is further increased, so that the width of the magnetic recording medium 10 can be further easily adjusted by tension control. Therefore, off-track can be further appropriately suppressed, and data recorded on the magnetic recording medium 10 can be reproduced more accurately.
[0154] The average thickness of the magnetic recording medium 10 is determined in the same manner as the method for measuring the average thickness of the magnetic recording medium 10 described in the first embodiment.
[0155] The average thickness of the magnetic recording medium 10 correlates with the ease with which the magnetic recording medium 10 expands and contracts due to an external force, and the thinner the average thickness of the magnetic recording medium 10, the easier it is for the magnetic recording medium 10 to expand and contract due to an external force, and the thicker the average thickness, the less likely it is for the magnetic recording medium 10 to expand and contract due to an external force. Therefore, from the viewpoint of tension control, it is advantageous for the magnetic recording medium 10 to have a thinner average thickness.
[0156] (average thickness of substrate) The average thickness TB of the substrate 11 is preferably 4.2 μm or less, more preferably 3.8 μm or less, and even more preferably 3.4 μm or less. When the average thickness TB of the substrate 11 is 4.2 μm or less, the elasticity of the magnetic recording medium 10 due to an external force is further increased, so that the width of the magnetic recording medium 10 can be further easily adjusted by tension control. Therefore, off-track can be further appropriately suppressed, and data recorded on the magnetic recording medium 10 can be reproduced more accurately.
[0157] The average thickness of the substrate 11 can be determined in the same manner as the method for measuring the average thickness of the substrate 11 described in the first embodiment.
[0158] The thickness of the substrate 11 accounts for more than half of the total thickness of the magnetic recording medium 10. Therefore, the average thickness of the substrate 11 correlates with the ease with which the magnetic recording medium 10 expands and contracts due to an external force, and the thinner the average thickness of the substrate 11, the easier it is for the magnetic recording medium 10 to expand and contract due to an external force, and the thicker the average thickness of the substrate 11, the more difficult it is for the magnetic recording medium 10 to expand and contract due to an external force. Therefore, from the viewpoint of tension control, it is advantageous for the average thickness of the substrate 11 to be thinner.
[0159] (Recording and playback device) The control device 38 obtains a distance d1 between two adjacent servo bands SB (the distance in the width direction of the magnetic recording medium 10) from the reproduced waveforms of the servo signals read from the two adjacent servo bands SB when recording data on the magnetic recording medium 10. Then, the control device 38 stores the obtained distance in a storage unit included in the control device 38.
[0160] The control device 38 obtains the distance d2 between two adjacent servo bands SB (the distance in the width direction of the magnetic recording medium 10) from the reproduced waveform of the servo signal read from the two adjacent servo bands SB when reproducing data from the magnetic recording medium 10. At the same time, the control device 38 reads out the distance d1 between the two adjacent servo bands SB obtained when recording data on the magnetic recording medium 10 from the storage unit. The control device 38 controls the rotation of the spindle drive device 33 and the reel drive device 34 so that the difference Δd between the distance d1 between the servo bands SB obtained when recording data on the magnetic recording medium 10 and the distance d2 between the servo bands SB obtained when reproducing data from the magnetic recording medium 10 falls within a specified range, thereby adjusting the tension applied in the longitudinal direction of the magnetic recording medium 10. This tension adjustment is controlled by, for example, feedback control.
[0161] Instead of determining the distance d1 between the servo bands SB when recording data on the magnetic recording medium 10, the control device 38 may store in advance in a storage unit a known interval d3 between the servo bands SB that serves as a reference when adjusting the tension in the longitudinal direction of the magnetic recording medium 10. In this case, the control device 38 controls the rotation of the spindle drive device 33 and the reel drive device 34, and adjusts the tension applied in the longitudinal direction of the magnetic recording medium 10 so that the difference Δd between the distance d3 between the servo bands SB previously stored in the storage unit and the distance d2 between the servo bands SB determined when reproducing data from the magnetic recording medium 10 falls within a specified range. EXAMPLES
[0162] The present disclosure will be specifically described below using examples, but the present disclosure is not limited to these examples.
[0163] In this embodiment, the average thickness of the base film (substrate), the average thickness of the magnetic layer, the average thickness of the underlayer, the average thickness of the back layer, the average thickness of the magnetic tape (magnetic recording medium), the average aspect ratio of the magnetic powder, the average particle size of the magnetic powder, the average particle volume of the magnetic powder, the coercive force Hc1 of the magnetic tape in the perpendicular direction, the coercive force Hc2 of the magnetic tape in the longitudinal direction, and the servo band width W SB was determined by the measurement method described in the first embodiment above.
[0164] In this example, the 1% longitudinal elongation load of the magnetic tape, the longitudinal shrinkage rate of the magnetic tape, the average thickness TL of the magnetic tape, the average thickness TB of the base film, (TL-TB) / TB, the longitudinal Young's modulus of the magnetic tape, and the longitudinal Young's modulus of the base film were determined by the measurement method described in the second embodiment above.
[0165] [Examples 1 to 9, Comparative Examples 1 to 6] (Preparation process of paint for forming magnetic layer) The magnetic layer-forming paint was prepared as follows. First, the first composition having the following composition was kneaded with an extruder. Next, the kneaded first composition and the second composition having the following composition were added to a stirring tank equipped with a disperser and premixed. Then, further sand mill mixing was performed and filtering was performed to prepare the magnetic layer-forming paint.
[0166] (First composition) Magnetic powder: 100 parts by mass Vinyl chloride resin (cyclohexanone solution 30% by mass): 10 parts by mass (Degree of polymerization: 300, Mn=10,000, contains polar groups OSO3K=0.07mmol / g and secondary OH=0.3mmol / g.) Aluminum oxide powder: 5 parts by weight (α-Al2O3, average particle size 0.2μm) Carbon black: 2 parts by weight (Manufactured by Tokai Carbon Co., Ltd., product name: Seast TA) The magnetic powder used was as shown in Table 1.
[0167] (Second composition) Vinyl chloride resin: 1.1 parts by mass (Resin solution: resin 30% by mass, cyclohexanone 70% by mass) n-Butyl stearate: 2 parts by weight Methyl ethyl ketone: 121.3 parts by mass Toluene: 121.3 parts by mass Cyclohexanone: 60.7 parts by mass
[0168] Finally, 4 parts by mass of polyisocyanate (product name: Coronate L, manufactured by Nippon Polyurethane Industries, Ltd.) and 2 parts by mass of myristic acid were added as a curing agent to the magnetic layer-forming coating material prepared as described above.
[0169] (Preparation process of paint for forming base layer) The paint for forming the undercoat layer was prepared as follows. First, the third composition having the following composition was kneaded with an extruder. Next, the kneaded third composition and the fourth composition having the following composition were added to a stirring tank equipped with a disperser and premixed. Then, further mixing was performed with a sand mill and filtering was performed to prepare the paint for forming the undercoat layer.
[0170] (Third composition) Acicular iron oxide powder: 100 parts by weight (α-Fe2O3, average major axis length 0.15μm) Vinyl chloride resin: 55.6 parts by mass (Resin solution: resin 30% by mass, cyclohexanone 70% by mass) Carbon black: 10 parts by weight (Average particle size 20nm)
[0171] (4th composition) Polyurethane resin UR8200 (manufactured by Toyobo): 18.5 parts by weight n-Butyl stearate: 2 parts by weight Methyl ethyl ketone: 108.2 parts by mass Toluene: 108.2 parts by mass Cyclohexanone: 18.5 parts by mass
[0172] Finally, 4 parts by mass of polyisocyanate (product name: Coronate L, manufactured by Nippon Polyurethane Industries, Ltd.) as a curing agent and 2 parts by mass of myristic acid were added to the coating material for forming the undercoat layer prepared as described above.
[0173] (Preparation process of paint for forming back layer) The coating material for forming the back layer was prepared as follows: The following raw materials were mixed in a stirring tank equipped with a disperser, and the mixture was filtered to prepare the coating material for forming the back layer. Carbon black (manufactured by Asahi Corporation, product name: #80): 100 parts by weight Polyester polyurethane: 100 parts by weight (Manufactured by Nippon Polyurethane Co., Ltd., product name: N-2304) Methyl ethyl ketone: 500 parts by weight Toluene: 400 parts by mass Cyclohexanone: 100 parts by mass
[0174] (Film forming process) Using the paint prepared as described above, a magnetic tape of media configuration 1 was prepared as follows. First, a long PEN film (base film) having an average thickness of 4.0 μm was prepared as a support. Next, a paint for forming an undercoat layer was applied to one main surface of the PEN film and dried to form an undercoat layer having an average thickness of 1.0 to 1.1 μm on one main surface of the PEN film. Next, a paint for forming a magnetic layer was applied to the undercoat layer and dried to form a magnetic layer having an average thickness of 60 to 100 nm on the undercoat layer. During drying of the paint for forming a magnetic layer, the magnetic powder was magnetically oriented in the thickness direction of the PEN film by a solenoid coil. Specifically, the magnetic powder was magnetically oriented once in the running direction (longitudinal direction) of the PEN film by a solenoid coil, and then magnetically oriented in the thickness direction of the PEN film. Furthermore, the drying conditions (drying temperature and drying time) of the coating material for forming the magnetic layer were adjusted to set the coercive force Hc1 in the perpendicular direction to 2450 to 3100 Oe, the coercive force Hc2 in the longitudinal direction to 1820 to 2080 Oe, and Hc2 / Hc1 to 0.65 to 0.85.
[0175] Next, the paint for forming the back layer was applied to the other main surface of the PEN film on which the undercoat layer and the magnetic layer were formed, and dried to form a back layer with an average thickness of 0.4 μm. Then, the PEN film on which the undercoat layer, the magnetic layer, and the back layer were formed was subjected to a hardening treatment. After that, a calendar treatment was performed to smooth the surface of the magnetic layer.
[0176] (Cutting process) The magnetic tape obtained as described above was cut into a width of 1 / 2 inch (12.65 mm), thereby obtaining a long magnetic tape with an average thickness of 5.6 μm.
[0177] (writing servo and data signals) A servo signal and a data signal were written on the long magnetic tape obtained as described above as follows. First, a servo signal was written on the magnetic tape using a servo writer, so that a servo bandwidth W SB Five servo bands with a diameter of 96 μm were formed. By writing servo signals, a row of V-shaped magnetic patterns was formed on each servo band.
[0178] Next, a recording and reproducing device was used to write data signals in the data bands between the servo bands. At this time, the recording and reproducing device was controlled so that the recording track width W was 2.9 μm and the recording wavelength λ was a single recording wavelength of 0.208 μm. The recording wavelength λ [nm] of the data signal was four times the distance between magnetization reversals L [nm] (= 0.052 μm) when recorded with the shortest recording wavelength (i.e., the shortest recording wavelength L' = 2 × L, and the recording wavelength λ = (twice the length of L')). A ring head with a gap length of 0.2 μm was used as the recording head.
[0179] Here, the recording wavelength λ is twice the shortest recording wavelength L' for the following reason. That is, in a recording / reproducing system using a short wavelength, the output / noise ratio when recording / reproducing with a recording wavelength twice the shortest recording wavelength is generally used as the C / N. Also, the C / N at twice the recording wavelength has a higher correlation with the error rate than the C / N at the shortest recording wavelength. Furthermore, when measuring the C / N at the shortest recording wavelength, depending on the wavelength characteristics of the recording / reproducing system, the tape noise may be hidden by the system noise of the recording / reproducing system, and the noise characteristics of the media may not be reflected correctly. Especially in the case of high linear recording density recording, the noise characteristics of the media may not be reflected correctly in many cases.
[0180] The minimum value L of the distance between magnetization reversals and the data track width W were obtained as follows. First, the surface of the magnetic layer 13 was observed using a magnetic force microscope (MFM) to obtain an MFM image. An example of an MFM image is shown in FIG. 9A and FIG. 9B. Next, the dimensions of the magnetization pattern row in the width direction of the magnetic tape were measured from the obtained MFM image, and the track width W [nm] was obtained. In addition, the distance between the light parts or the dark parts in the longitudinal direction of the magnetic tape was determined as λ [nm]. After that, half the value of λ [nm] was determined as L' [nm], and further half of L' [nm] was determined as L [nm].
[0181] [Example 10] A magnetic tape of media configuration 2 was obtained in the same manner as in Example 1, except for the following points. That is, the recording and reproducing device was controlled so that the recording track width W was 1.5 μm and the recording wavelength λ was a single recording wavelength of 0.192 μm. The recording wavelength λ [nm] of the data signal was set to four times the distance between magnetization reversals L [nm] (=0.048 μm) when recorded with the shortest recording wavelength.
[0182] [Example 11] A magnetic tape of media configuration 3 was obtained in the same manner as in Example 2, except for the following points. That is, a PEN film with an average thickness of 3.6 μm was used as the support, and the average thickness of the magnetic tape was set to 5.2 μm. In addition, the recording and reproducing device was controlled so that the recording track width W was 0.95 μm and the recording wavelength λ was a single recording wavelength of 0.168 μm. The recording wavelength λ [nm] of the data signal was set to four times the distance between magnetization reversals L [nm] (=0.042 μm) when recorded with the shortest recording wavelength.
[0183] [Example 12] A magnetic tape of media configuration 4 was obtained in the same manner as in Example 8, except for the following points. That is, a PEN film with an average thickness of 3.6 μm was used as the support, and the average thickness of the magnetic tape was 5.2 μm. In addition, the servo band width W SB Nine servo bands with a width of 96 μm were formed. The recording and reproducing device was controlled so that the recording track width W was 0.51 μm and the recording wavelength λ was a single recording wavelength of 0.156 μm. The recording wavelength λ [nm] of the data signal was set to four times the distance between magnetization reversals L [nm] (=0.039 μm) when recorded with the shortest recording wavelength.
[0184] [Example 13] A magnetic tape of media configuration 5 was obtained in the same manner as in Example 8, except for the following points. That is, a PEN film with an average thickness of 3.1 μm was used as the support, and the average thickness of the magnetic tape was 4.5 μm. In addition, the servo band width W SB Nine servo bands with a width of 96 μm were formed. The recording and reproducing device was controlled so that the recording track width W was 0.83 μm and the recording wavelength λ was a single recording wavelength of 0.156 μm. The recording wavelength λ [nm] of the data signal was set to four times the distance between magnetization reversals L [nm] (=0.039 μm) when recorded with the shortest recording wavelength.
[0185] [Example 14] A magnetic tape having a media configuration 6 was obtained in the same manner as in Example 9, except for the following points. That is, a PEN film having an average thickness of 3.1 μm was used as the support, and the average thickness of the magnetic tape was 4.5 μm. In addition, the servo band width W SBNine servo bands with a width of 96 μm were formed. The recording and reproducing device was controlled so that the recording track width W was 0.63 μm and the recording wavelength λ was a single recording wavelength of 0.152 μm. The recording wavelength λ [nm] of the data signal was set to four times the distance between magnetization reversals L [nm] (=0.038 μm) when recorded with the shortest recording wavelength.
[0186] [Example 15] A magnetic tape of media configuration 1 was obtained in the same manner as in Example 1, except for the following points. That is, the coating thickness of the magnetic layer-forming paint was adjusted to form a magnetic layer with an average thickness of 90 nm on the underlayer. In addition, the dispersion conditions of the magnetic layer-forming paint and the drying conditions (drying temperature and drying time) of the magnetic layer-forming paint were adjusted to set the coercive force Hc1 in the perpendicular direction to 2990 Oe, the coercive force Hc2 in the longitudinal direction to 1500 Oe, and Hc2 / Hc1 to 0.50.
[0187] [Example 16] A magnetic tape of media configuration 1 was obtained in the same manner as in Example 1, except for the following points: The drying conditions (drying temperature and drying time) of the coating material for forming the magnetic layer were adjusted to set the coercive force Hc1 in the perpendicular direction to 2690 Oe, the coercive force Hc2 in the longitudinal direction to 2150 Oe, and Hc2 / Hc1 to 0.80.
[0188] [Example 17] A magnetic tape of media configuration 1 was obtained in the same manner as in Example 6, except for the following points. That is, the coating thickness of the magnetic layer-forming paint was adjusted to form a magnetic layer with an average thickness of 90 nm on the undercoat layer. In addition, the drying conditions (drying temperature and drying time) of the magnetic layer-forming paint were adjusted to set the coercive force Hc1 in the perpendicular direction to 2900 Oe, the coercive force Hc2 in the longitudinal direction to 1950 Oe, and Hc2 / Hc1 to 0.67.
[0189] [Example 18, Comparative Examples 7 to 9] A magnetic tape was obtained in the same manner as in Example 1, except that the parameters of the magnetic tape and the parameters of the PEN film (base film) were set as shown in Table 2.
[0190] (C / N) First, a loop tester (Microphysics) was used to obtain a playback signal from the magnetic tape. The conditions for obtaining the playback signal are as follows: head:GMR head speed:2m / s signal: single recording frequency (10MHz) Recording current: Optimum recording current
[0191] Next, the playback signal was captured by a spectrum analyzer, and the playback output value of 10 MHz and the average noise value of 10 MHz ± 1 MHz were measured, and the difference between them was taken as the C / N. The results are shown in Table 1 as relative values with the C / N of Comparative Example 1 set to 0 dB. Note that if the C / N is 1.5 dB or higher, a medium that can withstand short wavelengths and narrow track densities can be realized.
[0192] (Determining the amount of change in tape width) First, a cartridge sample incorporating a 1 / 2 inch wide magnetic tape was prepared. The cartridge sample contained the magnetic tape wound around a reel provided in a cartridge case. Two or more rows of V-shaped magnetic patterns were recorded in advance on the magnetic tape in parallel in the longitudinal direction at known intervals (hereinafter referred to as "known intervals of magnetic pattern rows when recorded in advance"). Next, the cartridge sample was run back and forth by a recording and reproducing device. During the back and forth run, two or more rows of the V-shaped magnetic pattern rows were simultaneously played back, and the intervals of the magnetic pattern rows during the run were continuously measured from the shapes of the played back waveforms of each row. During the run, the rotational drive of the spindle drive device and the reel drive device was controlled based on the measured interval information of the magnetic pattern rows, and the tension in the longitudinal direction of the magnetic tape was automatically adjusted so that the intervals of the magnetic pattern rows were a specified width or approximately a specified width. All measured values of the spacing between the magnetic pattern rows for one round trip were defined as the "measured spacing between the magnetic pattern rows," and the maximum difference between this and the "known spacing between the magnetic pattern rows during previous runs" was defined as the "change in tape width."
[0193] The reciprocating run by the recording / reproducing device was performed in a constant temperature and humidity chamber. The reciprocating run speed was 5 m / sec. The temperature and humidity during the reciprocating run were gradually and repeatedly changed in accordance with a pre-programmed environment change program (10°C 10% → 29°C 80% → 10°C 10% repeated twice, changing from 10°C 10% to 29°C 80% in 2 hours, and changing from 29°C 80% to 10°C 10% in 2 hours) in a temperature range of 10°C to 45°C and a relative humidity range of 10% to 80%, independent of the reciprocating run.
[0194] This evaluation was repeated until the "preprogrammed environmental change program" was completed. After the evaluation was completed, the average value (simple average) was calculated using all the absolute values of the "change in tape width" obtained during each round trip, and this value was taken as the "effective amount of change in tape width" for that tape. Each tape was judged according to the deviation of this "effective amount of change in tape width" from the ideal (the smaller the better), and each was given an 8-level rating. A rating of "8" indicated the most desirable result, and a rating of "1" indicated the least desirable result. For magnetic tapes that have any of the above 8-level ratings, the following conditions are observed during tape running. 8: No abnormality occurs 7: A slight increase in error rate is observed during driving. 6: A significant increase in error rate is observed during operation. 5: When driving, the servo signal cannot be read and a slight re-read (1-2 times) is required. 4: When driving, the servo signal cannot be read and a moderate re-read (up to 10 times) is required. 3: When driving, the servo signal cannot be read and heavy reloads (more than 10 times) are required. 2: The servo cannot be read and the system sometimes stops due to an error. 1: Servo cannot be read and system error occurs, causing immediate stop
[0195] Table 1 shows the magnetic properties and evaluation results of the magnetic tapes of Examples 1-18 and Comparative Examples 1-9. [Table 1]
[0196] Table 2 shows the evaluation results of the magnetic tapes of Examples 1-18 and Comparative Examples 1-9. [Table 2]
[0197] Table 3 shows the media configurations employed in the magnetic tapes of Examples 1-18 and Comparative Examples 1-9. [Table 3]
[0198] The following can be seen from Tables 1 and 3: In Examples 1 to 5, 15, and 16, (1) the average thickness of the magnetic layer is 90 nm or less, (2) the average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, (3) the coercive force Hc1 in the perpendicular direction is 3000 Oe or less, and (4) the coercive force Hc1 in the perpendicular direction and the coercive force Hc2 in the longitudinal direction satisfy the relationship Hc2 / Hc1≦0.8. This allows a good C / N ratio to be obtained. In Examples 6, 7, and 17, in which ε-iron oxide particles or Co-containing spinel ferrite particles were used as the magnetic powder, good C / N ratios could be obtained by satisfying the above configurations (1) to (4), similarly to Examples 1 to 5, in which hexagonal ferrite particles were used as the magnetic powder. Even in Examples 8 and 9, in which ultrafine particles are used as the magnetic powder, good C / N can be obtained by satisfying the above configurations (1) to (4). Even in Examples 10 to 14, which have a higher recording density than Examples 1 to 9 and 15 to 17, a good C / N ratio can be obtained by satisfying the above configurations (1) to (4).
[0199] In Comparative Example 1, the average aspect ratio of the magnetic powder exceeds 3.0, that is, the above configuration (2) is not satisfied, so that the magnetic powder stacks and a good C / N ratio cannot be obtained. In Comparative Example 2, the average thickness of the magnetic layer exceeds 90 nm, that is, the above configuration (1) is not satisfied, so that the short wavelength characteristics are deteriorated and a good C / N ratio cannot be obtained. In Comparative Example 3, Hc2 / Hc1 exceeds 0.8, that is, the above configuration (4) is not satisfied, so the degree of perpendicular orientation of the magnetic powder is low, and therefore a good C / N ratio cannot be obtained. In Comparative Example 4, the coercive force Hc1 in the perpendicular direction exceeds 3000 Oe, that is, the configuration of (3) above is not satisfied, so saturation recording with the write head becomes difficult, and a good C / N ratio cannot be obtained. In Comparative Examples 5 and 6, in which ε-iron oxide or Co-containing spinel ferrite was used as the magnetic powder, a good C / N ratio could not be obtained unless the above configurations (1) to (4) were satisfied, as in Comparative Examples 1 to 4, in which hexagonal ferrite was used as the magnetic powder.
[0200] From the evaluation results of Examples 1 and 11 and Comparative Examples 7 to 9, it can be seen that when (1) the average thickness of the magnetic layer is 90 nm or less, (2) the average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, (3) the coercive force Hc1 in the perpendicular direction is 3000 Oe or less, (4) the coercive force Hc1 in the perpendicular direction and the coercive force Hc2 in the longitudinal direction satisfy the relationship Hc2 / Hc1≦0.8, and (5) the longitudinal 1% elongation load of the magnetic tape is 0.6 N or less, deviation from the ideal in the “effective change in tape width” can be suppressed.
[0201] Although the embodiments of the present disclosure and their modified examples have been specifically described above, the present disclosure is not limited to the above-described embodiments and their modified examples, and various modifications based on the technical ideas of the present disclosure are possible.
[0202] For example, the configurations, methods, steps, shapes, materials, and values given in the above-mentioned embodiments and their modified examples are merely examples, and different configurations, methods, steps, shapes, materials, and values may be used as necessary. In addition, the chemical formulas of compounds, etc. are representative, and are not limited to the valences, etc. given as long as they are general names of the same compounds.
[0203] Furthermore, the configurations, methods, steps, shapes, materials, numerical values, and the like of the above-described embodiments and their modified examples can be combined with each other without departing from the spirit of this disclosure.
[0204] In addition, in this specification, a numerical range indicated using "~" indicates a range including the numerical values before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range of a certain stage may be replaced with the upper limit or lower limit of a numerical range of another stage. Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more types.
[0205] The present disclosure may also employ the following configuration. (1) A tape-shaped magnetic recording medium, A substrate; a magnetic layer provided on the substrate and containing magnetic powder; Equipped with The average thickness of the magnetic layer is 90 nm or less, The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, The coercive force Hc1 of the magnetic recording medium in the perpendicular direction is 3000 Oe or less, the coercive force Hc1 and the coercive force Hc2 of the magnetic recording medium in the longitudinal direction of the magnetic recording medium satisfy the relationship Hc2 / Hc1≦0.8, A magnetic recording medium in which, in a longitudinal tensile test of the magnetic recording medium, the load when the elongation rate of the magnetic recording medium is 0.5% is σ0.5, and the load when the elongation rate of the magnetic recording medium is 1.5% is σ1.5, and the value of σ1.5-σ0.5 is 0.6 N or less. (2) 2. The magnetic recording medium according to claim 1, wherein the magnetic recording medium has a shrinkage rate of 0.1% or less in the longitudinal direction when stored at 60° C. for 72 hours. (3) The magnetic recording medium according to (1) or (2), wherein the value of (TL-TB) / TB is 0.41 or less, where TB is the average thickness of the substrate and TL is the average thickness of the magnetic recording medium. (4) The magnetic recording medium according to any one of (1) to (3), wherein the Young's modulus in the longitudinal direction of the magnetic recording medium is 8.5 GPa or less. (5) The magnetic recording medium according to any one of (1) to (4), wherein the substrate has a Young's modulus in the longitudinal direction of 8.0 GPa or less. (6) The magnetic recording medium according to any one of (1) to (5), wherein the width of the magnetic recording medium is adjustable by increasing or decreasing the tension in the longitudinal direction of the magnetic recording medium. (7) the magnetic layer having a plurality of servo bands; 7. The magnetic recording medium according to any one of (1) to (6), wherein the ratio of the total area of the plurality of servo bands to the surface area of the magnetic layer is 4.0% or less. (8) The magnetic recording medium according to (7), wherein the number of the servo bands is 5 or more. (9) The magnetic recording medium according to (7) or (8), wherein the number of the servo bands is 5+4n or more (where n is a positive integer). (10) The magnetic recording medium according to any one of (7) to (9), wherein the width of the servo band is 95 μm or less. (11) the magnetic layer is configured to be capable of forming a plurality of data tracks; The magnetic recording medium according to any one of (1) to (10), wherein the width of the data track is 3.0 μm or less. (12) The magnetic recording medium according to any one of (1) to (11), wherein the magnetic layer is configured to be capable of recording data such that the ratio W / L of the minimum distance L between magnetization reversals and the width W of the data track satisfies the relationship W / L≦200. (13) The magnetic recording medium according to any one of (1) to (12), wherein the magnetic layer is configured to be capable of recording data such that the minimum distance L between magnetization reversals is 48 nm or less. (14) The magnetic recording medium according to any one of (1) to (13), wherein the coercive force Hc2 is 2000 Oe or less. (15) The magnetic recording medium according to any one of (1) to (14), wherein the average thickness of the magnetic recording medium is 5.6 μm or less. (16) The magnetic recording medium according to any one of (1) to (15), wherein the substrate has an average thickness of 4.2 μm or less. (17) The average thickness of the magnetic recording medium is 5.6 μm or less; the magnetic layer has a plurality of servo bands, the number of the servo bands being 5 or more; The magnetic recording medium according to any one of (1) to (16), wherein the magnetic layer is configured to be capable of forming a plurality of data tracks, the width of the data tracks is 1.6 μm or less, the minimum value L of the distance between magnetization reversals is 50 nm or less, and the ratio W / L of the minimum value L of the distance between magnetization reversals to the width W of the data tracks satisfies the relationship W / L≦30. (18) The magnetic recording medium according to any one of (1) to (17), wherein the magnetic powder contains hexagonal ferrite, ε iron oxide, or Co-containing spinel ferrite. (19) The hexagonal ferrite contains at least one of Ba and Sr, The magnetic recording medium according to (18), wherein the ε-iron oxide contains at least one of Al and Ga. (20) The magnetic recording medium according to any one of (1) to (19), wherein the average thickness of the magnetic layer is 80 nm or less. (twenty one) The magnetic recording medium according to any one of (1) to (20), wherein the average thickness of the magnetic layer is 70 nm or less. (twenty two) The magnetic recording medium according to any one of (1) to (21), wherein the coercive force Hc1 and the coercive force Hc2 satisfy the relationship Hc2 / Hc1≦0.7. (twenty three) The magnetic recording medium according to any one of (1) to (22), wherein the coercive force Hc1 is 2200 Oe or more. (twenty four) A tape-shaped magnetic recording medium, A substrate; a magnetic layer provided on the substrate and containing magnetic powder; Equipped with The average thickness of the magnetic layer is 90 nm or less, The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, The coercive force Hc1 of the magnetic recording medium in the perpendicular direction is 3000 Oe or less, the coercive force Hc1 and the coercive force Hc2 of the magnetic recording medium in the longitudinal direction of the magnetic recording medium satisfy the relationship Hc2 / Hc1≦0.8, The magnetic recording medium has a shrinkage rate of 0.1% or less in the longitudinal direction when stored at 60° C. for 72 hours. (twenty five) A tape-shaped magnetic recording medium, A substrate; a magnetic layer provided on the substrate and containing magnetic powder; Equipped with The average thickness of the magnetic layer is 90 nm or less, The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, The coercive force Hc1 of the magnetic recording medium in the perpendicular direction is 3000 Oe or less, the coercive force Hc1 and the coercive force Hc2 of the magnetic recording medium in the longitudinal direction of the magnetic recording medium satisfy the relationship Hc2 / Hc1≦0.8, A magnetic recording medium, in which the value of (TL-TB) / TB is 0.41 or less, where TB is the average thickness of the substrate and TL is the average thickness of the magnetic recording medium. (26) A tape-shaped magnetic recording medium, A substrate; a magnetic layer provided on the substrate and containing magnetic powder; Equipped with The average thickness of the magnetic layer is 90 nm or less, The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, The coercive force Hc1 of the magnetic recording medium in the perpendicular direction is 3000 Oe or less, the coercive force Hc1 and the coercive force Hc2 of the magnetic recording medium in the longitudinal direction of the magnetic recording medium satisfy the relationship Hc2 / Hc1≦0.8, The magnetic recording medium has a Young's modulus in the longitudinal direction of 8.5 GPa or less. (27) A tape-shaped magnetic recording medium, A substrate; a magnetic layer provided on the substrate and containing magnetic powder; Equipped with The average thickness of the magnetic layer is 90 nm or less, The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, The coercive force Hc1 of the magnetic recording medium in the perpendicular direction is 3000 Oe or less, the coercive force Hc1 and the coercive force Hc2 of the magnetic recording medium in the longitudinal direction of the magnetic recording medium satisfy the relationship Hc2 / Hc1≦0.8, A magnetic recording medium, wherein the substrate has a Young's modulus in the longitudinal direction of 8.0 GPa or less. (28) A tape-shaped magnetic recording medium, A substrate; a magnetic layer provided on the substrate and containing magnetic powder; Equipped with The average thickness of the magnetic layer is 90 nm or less, The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, The coercive force Hc1 of the magnetic recording medium in the perpendicular direction is 3000 Oe or less, the coercive force Hc1 and the coercive force Hc2 of the magnetic recording medium in the longitudinal direction of the magnetic recording medium satisfy the relationship Hc2 / Hc1≦0.8, The magnetic recording medium is configured so that the width of the magnetic recording medium can be adjusted by increasing or decreasing tension in the longitudinal direction of the magnetic recording medium. [Explanation of symbols]
[0206] 10 Magnetic recording media 10A Magnetic recording medium cartridge 10B Cartridge Case 10C Reel 11 Base 12 Base layer 13 Magnetic layer 14 Back layer 15 Barrier Layer 21 Core 22 Shell part 22a First shell part 22b Second shell part 30 Recording and playback equipment 31 Spindle 32 Reels 33 Spindle drive unit 34 Reel drive unit 35 Guide roller 36 Head Unit 37 Communication Interface 38 Control device 41 Server 42 Personal Computers 43 Network
Claims
1. A tape-shaped magnetic recording medium, A substrate; a magnetic layer provided on the substrate and containing magnetic powder; Equipped with The magnetic powder includes hexagonal ferrite, ε iron oxide, or Co-containing spinel ferrite, the magnetic layer has five or more servo bands; The average thickness of the magnetic recording medium is 5.6 μm or less; The average thickness of the magnetic layer is 90 nm or less, When the average thickness of the substrate is TB and the average thickness of the magnetic recording medium is TL, the value of (TL-TB) / TB is 0.41 or less; The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, the coercive force Hc2 of the magnetic recording medium in the longitudinal direction of the magnetic recording medium is 1000 Oe or more; a coercive force Hc1 of the magnetic recording medium in a perpendicular direction of the magnetic recording medium and a coercive force Hc2 of the magnetic recording medium in a longitudinal direction of the magnetic recording medium satisfy a relationship of Hc2 / Hc1≦0.8; The magnetic recording medium has a Young's modulus in the longitudinal direction of 8.3 GPa or less.
2. 2. The magnetic recording medium according to claim 1, wherein the value of (TL-TB) / TB is 0.39 or less, where TB is the average thickness of the substrate and TL is the average thickness of the magnetic recording medium.
3. 2. The magnetic recording medium according to claim 1, wherein the value of (TL-TB) / TB is 0.37 or less, where TB is the average thickness of the substrate and TL is the average thickness of the magnetic recording medium.
4. 2. The magnetic recording medium according to claim 1, wherein the value of (TL-TB) / TB is 0.35 or less, where TB is the average thickness of the substrate and TL is the average thickness of the magnetic recording medium.
5. 2. The magnetic recording medium according to claim 1, wherein the average thickness of the substrate is 4.2 [mu]m or less.
6. 2. The magnetic recording medium according to claim 1, wherein the width of the magnetic recording medium is adjustable by increasing or decreasing tension in the longitudinal direction of the magnetic recording medium.
7. 2. The magnetic recording medium according to claim 1, wherein the ratio of the total area of the plurality of servo bands to the surface area of the magnetic layer is 4.0% or less.
8. 2. The magnetic recording medium according to claim 1, wherein the number of said servo bands is 5+4n or more (n is a positive integer).
9. 2. The magnetic recording medium according to claim 1, wherein the width of the servo band is 95 [mu]m or less.
10. 2. The magnetic recording medium according to claim 1, wherein the coercive force Hc2 is 2000 Oe or less.
11. 2. The magnetic recording medium according to claim 1, wherein the average thickness of the substrate is 3.8 [mu]m or less.
12. 2. The magnetic recording medium according to claim 1, wherein the hexagonal ferrite contains at least one of Ba and Sr.
13. 2. The magnetic recording medium according to claim 1, wherein the average thickness of the magnetic layer is 70 nm or less.
14. 2. The magnetic recording medium according to claim 1, wherein the coercive force Hc1 and the coercive force Hc2 satisfy the relationship Hc2 / Hc1≦0.
7.
15. 2. The magnetic recording medium according to claim 1, wherein the average aspect ratio of the magnetic powder is 1.0 or more and 2.5 or less.
16. 2. The magnetic recording medium according to claim 1, wherein the average aspect ratio of the magnetic powder is 1.0 or more and 2.1 or less.
17. 2. The magnetic recording medium according to claim 1, wherein the average aspect ratio of the magnetic powder is 1.0 or more and 1.8 or less.
18. 2. The magnetic recording medium according to claim 1, further comprising an underlayer between the substrate and the magnetic layer.
Citation Information
Patent Citations
Magnetic recording medium
JP1997320031A
Method for manufacturing hexagonal ferrite and magnetic recording medium using the same
JP2002298333A
Metal thin film type magnetic recording medium
JP2002367150A
Magnetic recording medium
JP2002373413A
Method for manufacturing magnetic recording medium, and magnetic recording medium
JP2009099240A