Electromagnetic wave shielding sheet, printed wiring board with electromagnetic wave shielding sheet, and electronic device
The electromagnetic shielding sheet with a protective, conductive, and adhesive layer structure addresses peeling, foaming, and gas release issues, enhancing the performance of printed wiring boards by maintaining structural integrity and shielding effectiveness.
Patent Information
- Application Number
- JP2023203175
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-11-30
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2043-11-30
AI Technical Summary
Electromagnetic shielding sheets used in printed wiring boards face issues such as peeling during punching, poor appearance due to foaming, and poor connection caused by volatile components generating interlayer formation during heat treatment, along with inadequate gas release properties.
An electromagnetic shielding sheet with a protective layer, conductive layer containing a metal filler and binder, and adhesive layer, designed to withstand heat treatment and maintain cohesive failure rates and peeling forces within specific ranges, ensuring strong bonding and effective gas release.
The shielding sheet maintains integrity during punching, provides excellent transmission characteristics and shielding properties, and effectively releases gases, improving the performance of printed wiring boards.
Smart Images

Figure 0007559913000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electromagnetic wave shielding sheet, a printed wiring board with an electromagnetic wave shielding sheet, and an electronic device. [Background technology]
[0002] Substrates such as printed wiring boards are built into various electronic devices, including mobile terminals, PCs, and servers. These substrates are provided with an electromagnetic shielding structure to prevent malfunctions caused by external magnetic fields and radio waves, and to reduce unnecessary radiation from electrical signals.
[0003] As transmission signals become faster, printed wiring boards with electromagnetic shielding sheets are required to have electromagnetic shielding properties (hereinafter referred to as high-frequency shielding properties) that can deal with high-frequency noise, and to reduce transmission loss in the high-frequency range (hereinafter sometimes referred to as transmission characteristics). Patent Document 1 discloses a shielding film that has a metal layer with a thickness of 0.5 to 12 μm and an anisotropic conductive adhesive layer in a laminated state. It is described that this configuration provides good shielding of electric field waves, magnetic field waves, and electromagnetic waves that travel from one side of the electromagnetic shielding sheet to the other side, and reduces transmission loss. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2013 / 077108 Summary of the Invention [Problem to be solved by the invention]
[0005] However, when an electromagnetic wave shielding printed wiring board in which an electromagnetic wave shielding sheet using a metal layer is attached to a printed wiring board is subjected to a heat treatment such as solder reflow, volatile components generated from inside the printed wiring board cause lifting between the layers, resulting in foaming and other problems that lead to poor appearance and poor connections. This is because outgassing, such as water vapor, generated from the printed wiring board is retained in the dense metal layer of the electromagnetic shielding sheet, and therefore the electromagnetic shielding sheet is required to have the permeability to outgassing (hereinafter referred to as gas release property).
[0006] On the other hand, when an electromagnetic shielding sheet is used, it may be punched out to the desired size and shape. In this case, there is a punching method in which the electromagnetic shielding sheet is laminated to a carrier tape, punched out, and then attached to a printed wiring board or the like, and the carrier tape is peeled off. In this method, when the carrier tape is peeled off, peeling may occur not at the adhesive interface between the carrier tape and the electromagnetic shielding sheet, but within the electromagnetic shielding sheet (hereinafter referred to as carrier punching suitability).
[0007] An object of the present invention is to provide an electromagnetic wave shielding sheet which does not peel off during punching and which has excellent transmission characteristics, shielding properties and gas escape properties, and a printed wiring board with the electromagnetic wave shielding sheet. [Means for solving the problem]
[0008] As a result of extensive investigations, the present inventors have found that the problems of the present invention can be solved in the following aspect, and have thus completed the present invention. [1]: An electromagnetic wave shielding sheet having a protective layer, a conductive layer, and an adhesive layer laminated in this order, the conductive layer containing a metal filler and a binder, and in a peel test conducted at a peel angle of 180° between the protective layer and the adhesive layer and a peel speed of 300 mm / min, the conductive layer has a peel force of 50 to 2500 [gf / 25 mm] when it undergoes cohesive failure, and the cohesive failure rate in the peel test is 10% or more. [2]: The conductivity of the conductive layer is 2.4 × 106 ~3.0×10 7 The electromagnetic wave shielding sheet according to [1], wherein the electromagnetic wave shielding sheet has a refractive index of [S / m]. [3]: the surface resistivity of the conductive layer is 4.0 × 10 -3 ~2.0×10 -1 The electromagnetic wave shielding sheet according to [1], wherein the inductive coupling coefficient is [Ω / □]. [4]: The electromagnetic wave shielding sheet according to [1], wherein, in a cut surface after the electromagnetic wave shielding sheet is heat-pressed under conditions of 170°C, 2 MPa, and 30 minutes, the area occupied by the metal filler is 23 to 95 when the cross-sectional area of the conductive layer is taken as 100. [5]: The electromagnetic shielding sheet according to [1], wherein the conductive layer has a thickness of 1 to 12 μm on a cut surface after the electromagnetic shielding sheet is heat-pressed under conditions of 170° C., 2 MPa, and 30 minutes. [6]: The electromagnetic wave shielding sheet according to [1], wherein the metal filler includes flake-shaped metal filler, and the average aspect ratio of the flake-shaped metal filler on the cut surface of the conductive layer after the electromagnetic wave shielding sheet is heated and pressed under conditions of 170°C, 2 MPa, and 30 minutes is 10 to 70. [7]: The electromagnetic shielding sheet according to [1], wherein the metal filler comprises silver-coated copper powder, and in a cut section of the conductive layer after the electromagnetic shielding sheet is heated and pressed under conditions of 170°C, 2 MPa, and 30 minutes, the mass ratio of silver element is 3% or more and 25% or less when the total mass of copper and silver element is taken as 100% as measured by energy dispersive X-ray analysis. [8]:[1]~[7] Either A printed wiring board comprising the electromagnetic shielding sheet according to claim 1. [9]: An electronic device comprising a printed wiring board with the electromagnetic shielding sheet according to [8]. Effect of the Invention
[0009] The present invention can provide an electromagnetic wave shielding sheet that does not peel off during punching and has excellent transmission characteristics, shielding properties and gas escape properties, and a printed wiring board with the electromagnetic wave shielding sheet. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a schematic plan view of a main surface side of the printed circuit board according to the embodiment. [Diagram 2] FIG. 2 is a schematic plan view of the rear surface side of the printed circuit board according to the embodiment. [Diagram 3] FIG. 2 is a schematic plan view of the rear surface side of a shielded wiring board according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Electromagnetic wave shielding sheet> The electromagnetic wave shielding sheet of the present invention has a protective layer, a conductive layer, and an adhesive layer in this order. The electromagnetic wave shielding sheet is attached to an adherend via the adhesive layer by hot pressing to form an electromagnetic wave shielding layer, and shields and reflects electromagnetic waves from the attached surface. The electromagnetic wave shielding sheet is characterized in that the peel strength (hereinafter sometimes referred to as peel strength) in a peel test at a peel angle of 180° between the protective layer and the adhesive layer and a peel speed of 300 mm / min is 50 to 2500 [gf / 25 mm]. The peel strength is preferably 100 to 2500 [gf / 25 mm], and more preferably 180 to 2500 [gf / 25 mm].
[0012] The electromagnetic wave shielding sheet of the present invention is also characterized in that it has a cohesive failure rate of 10% or more, which is defined as the ratio of the area of the cohesive failure portion of the conductive layer to the total area of the peel surface in the above-mentioned peel test for measuring the peel force. The cohesive failure rate is preferably 10% or more, more preferably 40% or more, and even more preferably 70% or more.
[0013] By setting the peel force and cohesive failure rate within the above ranges, strong adhesion can be achieved at the interfaces between the protective layer / conductive layer and the conductive layer / adhesive layer, and the cohesive force of the conductive layer can be maintained at a high level, thereby making it possible to achieve an appropriate level of suitability for carrier punching.
[0014] Examples of methods for adjusting the peel strength to a desired range include appropriately selecting the types of resins contained in the conductive layer, protective layer, and adhesive layer, and adjusting the amount of metal filler contained in the conductive layer. Details will be described later.
[0015] Methods for improving the cohesive failure rate include adjusting the type of binder in the conductive layer and the shape and content of the metal filler, and increasing the peel strength of the protective layer and adhesive layer. Each method will be described in detail later. <Conductive layer>
[0016] Next, the conductive layer used in the present invention will be described. The conductive layer used in the present invention contains a metal filler and a binder, and the binder preferably contains at least a resin. By containing the metal filler and the resin in the conductive layer, the gas escape property can be improved.
[0017] Suitable examples of the resin include thermoplastic resins and curable resins. The curable resin is preferably a thermosetting resin or a photocurable resin, and more preferably a thermosetting resin. The thermoplastic resin refers to a resin that becomes soft when heated to a glass transition temperature or melting point or higher, and the thermosetting resin refers to a resin that crosslinks when heated to form a polymer network structure, hardens, and cannot be restored to its original state. There are types of thermosetting resins that harden alone, and types that harden by using a thermosetting resin and a curing agent in combination.
[0018] When a thermoplastic resin is used as the binder resin, the included thermoplastic resin exists in a solid state, and melts when heat-pressed with an adherend such as an FPC, and then solidifies again after cooling, thereby obtaining the desired adhesive strength. When a thermosetting resin is used as the binder resin, the included thermosetting resin and curing agent exist in an uncured or semi-cured state (B stage), and can be cured by heat-pressing with an adherend such as an FPC (C stage) to obtain the desired adhesive strength. Among these, it is preferable to use a thermosetting resin and a curing agent as the binder component, and it is more preferable to use a thermosetting resin and a curing agent and then semi-cured. The method of semi-curing is not particularly limited, but examples include a method of applying heat to an extent that the curing agent does not completely react, a method of using multiple curing agents with different reaction temperatures, and a method of using multiple curing agents with different reaction times. Among these, a method of using multiple curing agents with different reaction temperatures is preferable. That is, in addition to a first curing agent whose curing reaction progresses during C-stage, it is preferable to include a second curing agent whose curing reaction progresses during B-stage. This strengthens the bond between the metal fillers, improves the peeling force, and improves the suitability for carrier punching.
[0019] Examples of thermoplastic resins include polyolefin resins, vinyl resins, styrene-acrylic resins, diene resins, terpene resins, petroleum resins, cellulose resins, polyamide resins, polyurethane resins, polyester resins, polycarbonate resins, polyimide resins, liquid crystal polymers, and fluororesins.
[0020] The thermosetting resin may be any resin having one or more functional groups per molecule that can be utilized in a crosslinking reaction upon heating, such as a hydroxyl group, a phenolic hydroxyl group, a methoxymethyl group, a carboxyl group, an amino group, an epoxy group, an oxetanyl group, an oxazoline group, an oxazine group, an aziridine group, a thiol group, an isocyanate group, a blocked isocyanate group, a blocked carboxyl group, or a silanol group, and preferably contains a carboxyl group or a phenolic hydroxyl group.
[0021] The total of the acid value and the phenolic hydroxyl value of the thermosetting resin is preferably 3 to 100 mgKOH / g, more preferably 3 to 70 mgKOH / g, and even more preferably 5 to 40 mgKOH / g. By setting the total of the acid value and the phenolic hydroxyl value of the thermosetting resin within this range, the bonds between the metal fillers are strengthened, the peeling force is improved, and the suitability for punching the carrier is improved.
[0022] Suitable examples of the thermosetting resin include acrylic resin, maleic acid resin, polybutadiene resin, polyester resin, polyurethane resin, epoxy resin, oxetane resin, phenoxy resin, polyimide resin, polyamide resin, phenolic resin, alkyd resin, amino resin, polylactic acid resin, oxazoline resin, benzoxazine resin, silicone resin, and fluororesin. Among these, polyurethane resin, polyurethane urea resin, addition type ester resin, epoxy compound, phenoxy resin, polyimide resin, polyamide resin, piperazine polyamide resin, and polyamideimide resin are preferred from the viewpoint of dispersion stability and adhesive strength of the metal filler. The thermosetting resin can be used alone or in combination of two or more kinds.
[0023] The weight-average molecular weight of the thermosetting resin is preferably 20,000 to 300,000, more preferably 50,000 to 300,000, and even more preferably 100,000 to 300,000. By setting the weight-average molecular weight of the thermosetting resin within this range, the bonds between the metal fillers are strengthened and the peeling force is improved, improving the suitability for punching the carrier.
[0024] In addition to the above-mentioned resin, the thermosetting resin in the present invention preferably contains, if necessary, a so-called "curing agent" such as a resin or a low molecular weight compound that reacts with the above-mentioned functional groups to form chemical crosslinks.
[0025] The curing agent is not particularly limited as long as it has two or more functional groups that can react with the functional groups of the thermosetting resin. Examples of the curing agent include epoxy compounds, acid anhydride group-containing compounds, isocyanate compounds, aziridine compounds, amine compounds, phenolic compounds, organometallic compounds (metal chelate compounds), polyol compounds, melamine compounds, silane compounds, carbodiimide compounds, phenolic compounds, benzoxazine compounds, maleimide compounds, and β-hydroxyalkylamide group-containing compounds. The curing agent can be used alone or in combination of two or more kinds. The curing agent may be a low molecular weight compound or a high molecular weight compound, but is a compound different from the above-mentioned thermosetting resin.
[0026] The photocurable resin may be any resin having one or more unsaturated bonds in one molecule that undergo a crosslinking reaction when exposed to light, and examples of such resins include acrylic resins, maleic acid resins, polybutadiene resins, polyester resins, polyurethane resins, epoxy resins, oxetane resins, phenoxy resins, polyimide resins, polyamide resins, phenolic resins, alkyd resins, amino resins, polylactic acid resins, oxazoline resins, benzoxazine resins, silicone resins, and fluororesins.
[0027] The surface resistivity of the conductive layer is 4.0×10 -3 ~2.0×10 -1 [Ω / □] is preferably 4.0×10 -3 ~1.0×10 -1 By setting the surface resistivity of the conductive layer in this range, good high frequency shielding properties can be obtained.
[0028] The surface resistivity of the conductive layer in the present invention is determined by multiplying the resistance value measured using a four-point probe, such as "Loresta GP" manufactured by Mitsubishi Chemical, in accordance with JIS K7194-1994, by a predetermined constant. Specifically, four conductive bumps arranged in a straight line at 5 mm intervals are inserted from the center of the adhesive layer of the electromagnetic shielding sheet of the present invention (a rectangular sample piece of 80 mm x 50 mm) until they reach the conductive layer. The positions of the four conductive bumps are parallel to the long side of the sample piece. A current is passed between the two outer points of the four conductive bumps, and the voltage between the two inner points is measured to determine the resistance value = voltage / current. The measured value is then multiplied by a constant "4.239" to obtain the "surface resistivity."
[0029] The conductivity of the conductive layer is 2.4 x 10 6 ~3.0×10 7 [S / m] is preferably 5.0×10 6 ~3.0×10 7 By setting the conductivity of the conductive layer in this range, transmission loss during high-speed transmission can be suppressed.
[0030] The electrical conductivity of the conductive layer in the present invention is determined from the thickness t (μm) of the conductive layer and the above-mentioned surface resistivity. Details will be described in the Examples.
[0031] As a method for adjusting the electrical conductivity to a desired range, for example, a method for forming a good conductive path by incorporating a suitable metal filler (described later) in a suitable amount (described later) can be mentioned. As a method for adjusting the surface resistivity to a desired range, in addition to the same method as for the electrical conductivity, a method for increasing the thickness of the conductive layer can be mentioned.
[0032] Examples of the metal filler include metal powders such as gold, silver, copper, and nickel, alloy powders such as solder, silver-coated copper powder (silver-coated copper powder), metal-plated glass fiber and carbon filler. Among them, silver powder and silver-coated copper powder, which have high electrical conductivity, are preferred. The amount of copper and silver elements in the conductive layer can be evaluated by observing the cut surface of the electromagnetic shielding sheet. In the cut surface, the mass ratio of silver element when the total mass of copper and silver elements is taken as 100% by energy dispersive X-ray analysis is preferably 3% to 25%, more preferably 6 to 15%. By setting it in this range, the effect of suppressing transmission loss during high-speed transmission and high-frequency shielding properties are improved, while the cost can be reduced by increasing the proportion of copper, which is cheaper than silver. As a method for controlling the amount of silver element to a desired range, for example, the amount of silver coating is controlled when preparing silver-coated copper powder.
[0033] The shape of the metal filler is not limited as long as the desired conductivity is obtained in the conductive layer, and two or more kinds of metal fillers of different shapes may be mixed. For example, spherical, flake-shaped (including leaf-shaped particles described later), dendritic, plate-shaped, needle-shaped, rod-shaped, and grape-shaped may be mentioned, and the flake-shaped is preferable from the viewpoint of improving the conductivity and increasing the cohesive failure rate. The flake-shaped particles also include leaf-shaped particles (for example, particles obtained by flattening dendritic particles) having multiple notches on the outer edge.
[0034] The average aspect ratio ([long diameter (μm)] / [thickness (μm)]) of the flaky metal filler in the cut surface of the conductive layer after the electromagnetic shielding sheet is heat-pressed under conditions of 170°C, 2 MPa, and 30 minutes is preferably in the range of 10 to 70, and more preferably in the range of 15 to 60. By setting the aspect ratio of the flaky particles within this range, it is possible to achieve a high level of both the effect of suppressing transmission loss during high-speed transmission, high-frequency shielding properties, and suitability for carrier punching.
[0035] The average particle size of the metal filler is preferably 1 to 100 μm, more preferably 3 to 50 μm, and even more preferably 5 to 20 μm. By setting it in this range, it is possible to improve the effect of suppressing transmission loss during high-speed transmission and the high-frequency shielding property, while also improving the flexibility of the printed wiring board with the electromagnetic shielding sheet.
[0036] The content of the metal filler is preferably 75% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, based on 100% by mass of the solid content of the conductive layer. Also, it is preferably 95% by mass or less. By making the content of the metal filler 75% by mass or more, the cohesive failure rate is improved, and by making it 95% by mass or less, the peel strength is improved.
[0037] When the area of the conductive layer in the cut surface of the conductive layer after the electromagnetic wave shielding sheet is heat-pressed under conditions of 170°C, 2 MPa, and 30 minutes is taken as 100%, the area occupied by the metal filler is preferably 23 to 95%, more preferably 30 to 95%, and even more preferably 45 to 95%. By keeping it within these ranges, it is possible to improve the effect of suppressing transmission loss during high-speed transmission and the high-frequency shielding property.
[0038] The thickness of the conductive layer on the cut surface after the electromagnetic wave shielding sheet is heat-pressed under conditions of 170°C, 2 MPa, and 30 minutes is preferably 1 to 12 μm, more preferably 1 to 8 μm. By making the thickness 1 μm or more, a conductive layer with high shielding properties can be obtained. In addition, by making the thickness 12 μm or less, the flexibility of the printed wiring board with the electromagnetic wave shielding sheet is improved. <Protective layer> The protective layer preferably contains at least a resin. The resin may be the same as that of the conductive layer, and it is preferable to use a thermosetting resin and a curing agent in combination. The protective layer may have a laminated structure of two or more layers. By making the total ratio of the resin and the hardener in the protective layer 50% or more, the peel strength and the cohesive failure rate of the protective layer are improved, and the suitability for punching the carrier is improved.
[0039] The thickness of the protective layer on the cut surface after the electromagnetic wave shielding sheet is heat-pressed under conditions of 170°C, 2 MPa, and 30 minutes can be appropriately designed depending on the application, but is preferably in the range of 0.5 μm to 25 μm, and more preferably 2 μm to 10 μm. By making the thickness of the protective layer 0.5 μm or more, sufficient protective properties are obtained. Furthermore, by making the thickness 25 μm or less, the flexibility of the printed wiring board with the electromagnetic wave shielding sheet is improved.
[0040] If necessary, the protective layer may contain a silane coupling agent, an antioxidant, a pigment, a dye, a tackifier resin, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling adjuster, a filler, a flame retardant, and the like. <Adhesive layer>
[0041] The adhesive layer is located on one side of the electromagnetic shielding sheet and serves to adhere to a printed wiring board described later. The adhesive layer preferably contains at least a resin. The resin may be the same as that of the conductive layer described above, and it is preferable to use a thermosetting resin and a hardener in combination. The resin and hardener are preferably materials with low dielectric constant and low dielectric tangent from the viewpoint of transmission loss, and materials with low dielectric constant from the viewpoint of characteristic impedance, for example, structures containing many fluorine atoms or hydrocarbons with small polarizability, and liquid crystal alignment or crystal alignment materials that fix dipoles are preferable. Similarly to the protective layer, by making the total ratio of the resin and hardener in the adhesive layer 50% or more, the peel strength and cohesive failure rate are improved, and the suitability for punching the carrier is improved.
[0042] The thickness of the adhesive layer on the cut surface after the electromagnetic shielding sheet is heat-pressed under conditions of 170°C, 2 MPa, and 30 minutes can be appropriately designed depending on the application, but is preferably in the range of 0.5 μm to 25 μm, and more preferably 2 μm to 10 μm. By making the thickness of the adhesive layer 0.5 μm or more, the adhesive strength to the printed wiring board can be increased. Also, by making the thickness 25 μm or less, the flexibility of the printed wiring board with the electromagnetic shielding sheet is improved.
[0043] The adhesive layer may be insulating or conductive. When the adhesive layer is to be conductive, the adhesive composition forming the adhesive layer may further contain the metal filler exemplified in the conductive layer. Also, fine particles of conductive polymers such as polyaniline and polyacetylene may be used. When the adhesive layer is to be conductive, it may be isotropically conductive or anisotropically conductive. Note that, the isotropic conductivity means that the adhesive layer has conductivity in both the thickness direction and the surface direction, and the anisotropic conductivity means that the adhesive layer has conductivity substantially only in the thickness direction. From the viewpoint of improving the transmission characteristics in the high frequency band and from the viewpoint of reducing costs, it is preferable to make the adhesive layer anisotropically conductive.
[0044] The anisotropic conductive adhesive layer contains a resin and a metal filler, and can be realized by setting the content and size of the metal filler within the ranges described below. The content of the metal filler can be appropriately designed, but is preferably 10 to 45 mass%, more preferably 15 to 40 mass%, and even more preferably 20 to 30 mass%, relative to 100 mass% of the adhesive layer. When the thickness of the adhesive layer to be formed is taken as the reference (100), the average particle diameter D50 of the metal filler is preferably about 100 to 300. By containing 10 to 45 mass% of conductive filler with the average particle diameter D50, it is possible to form an anisotropic conductive adhesive layer, rather than an isotropic one. The shape of the metal filler used is particularly preferably spherical or dendritic, which are likely to provide anisotropic conductivity.
[0045] If necessary, a silane coupling agent, an anti-rust agent, a reducing agent, an antioxidant, a pigment, a dye, a tackifier resin, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling adjuster, a filler, a flame retardant, etc. may be added to the adhesive layer. <Manufacturing method of electromagnetic wave shielding sheet>
[0046] An example of a method for producing the present sheet will be described below. However, the method of the present invention is not limited to the following method. The present sheet has a step of forming a conductive layer, a step of forming a protective layer, and a step of forming an adhesive layer.
[0047] <Conductive layer forming process> A metal filler-containing composition used to form a conductive layer is prepared. Specifically, a binder, a metal filler, and a solvent, if necessary, are mixed and stirred to obtain a metal filler-containing composition. A known stirring device such as a dispermat or homogenizer can be used for stirring. After preparing the metal filler-containing composition, the metal filler-containing composition can be coated on a release sheet and dried to form a conductive layer. Examples of the coating method include a gravure coating method, a kiss coating method, a die coating method, a lip coating method, a comma coating method, a blade method, a roll coating method, a knife coating method, a spray coating method, a bar coating method, a spin coating method, and a dip coating method. A known drying device such as a hot air dryer or an infrared heater can be used for the drying process. A sheet-shaped conductive layer may also be formed using an extrusion molding machine such as a T-die.
[0048] <Protective Layer Forming Process> The protective layer can be formed from a resin composition containing a resin by the same method as the conductive layer. Alternatively, the protective layer can be a film formed from an insulating resin such as polyester, polycarbonate, polyimide, polyamideimide, polyamide, polyphenylene sulfide, or polyether ether ketone.
[0049] <Adhesive layer forming process> The protective layer can be formed from a resin composition containing a resin and, if necessary, a conductive filler, by the same method as that for the conductive layer.
[0050] The layering order of this sheet is protective layer / conductive layer / adhesive layer. The layers can be formed by preparing a protective layer, conductive layer, and adhesive layer on a release sheet, and laminating them in the above-mentioned layering order. The lamination can be performed, for example, under conditions of a temperature of about 80 to 130°C, a pressure of about 0.2 to 5.0 MPa, and a lamination speed of about 0.5 to 20 m / min. By setting the lamination speed within these ranges, the adhesion between the layers is improved and the cohesive failure rate is improved. In addition, the peeling force is improved, and the suitability for punching the carrier is improved. It is preferable that a release sheet be laminated on the surface of the protective layer and the adhesive layer.
[0051] <Printed wiring board with electromagnetic shielding sheet> A printed wiring board with an electromagnetic wave shielding sheet comprises an electromagnetic wave shielding layer formed from the electromagnetic wave shielding sheet of the present invention, a cover coat layer, and a printed wiring board having a circuit pattern having signal wiring and ground wiring, and an insulating substrate. The printed wiring board can be produced by having a circuit pattern having signal wiring and ground wiring on the surface of an insulating base material, forming a cover coat layer on the printed wiring board that insulates and protects the signal wiring and ground wiring and has a via on at least a portion of the ground wiring, placing the adhesive layer surface of an electromagnetic wave shielding sheet on the cover coat layer, and then heat-pressing the electromagnetic wave shielding sheet to cause the adhesive layer to flow into the vias and adhere to the ground wiring.
[0052] The electromagnetic wave shielding layer includes an adhesive layer, a conductive layer, and a protective layer. The cover coat layer is an insulating material that covers the signal wiring of the printed wiring board and protects it from the external environment. The cover coat layer is preferably a polyimide film with a thermosetting adhesive, a thermosetting or ultraviolet-curing solder resist, or a photosensitive coverlay film, and a photosensitive coverlay film is more preferable for fine processing. In addition, the cover coat layer generally uses a known resin having heat resistance and flexibility, such as polyimide. The thickness of the cover coat layer is usually about 10 to 100 μm.
[0053] The circuit pattern includes ground wiring for earthing and signal wiring for sending electrical signals to electronic components. Both are generally formed by etching copper foil. The thickness of the circuit pattern is usually about 1 to 50 μm.
[0054] The insulating substrate is a support for the circuit pattern, and is preferably a flexible plastic such as polyester, polycarbonate, polyimide, polyphenylene sulfide, liquid crystal polymer, etc., and more preferably a liquid crystal polymer or polyimide. Among these, in consideration of the use of a printed wiring board that transmits high-frequency signals, a liquid crystal polymer having a low relative dielectric constant and a low dielectric loss tangent is even more preferable. When the printed wiring board is a rigid wiring board, the insulating base material is preferably made of glass epoxy. By providing such an insulating base material, the printed wiring board can have high heat resistance.
[0055] The heat pressing of the electromagnetic shielding sheet and the printed wiring board is generally performed under conditions of a temperature of about 150 to 190°C, a pressure of about 1 to 3 MPa, and a time of about 1 to 60 minutes. The heat pressing causes the adhesive layer to flow and fill the vias formed in the cover coat layer, thereby establishing electrical continuity with the ground wiring. In some cases, a post cure is performed at 150 to 190°C for 30 to 90 minutes after the heat pressing.
[0056] The opening area of the via is 0.8 mm 2 Less than 0.008mm is preferable. 2By setting the above range, the area of the ground wiring can be narrowed, and the printed wiring board can be made smaller. The shape of the via is not particularly limited, and any shape such as circle, square, rectangle, triangle, or irregular shape can be used depending on the application.
[0057] It is preferable to laminate the electromagnetic wave shielding layer on both sides of the printed wiring board, since this can more effectively suppress leakage of electromagnetic waves. In addition, the electromagnetic wave shielding layer in the printed wiring board with the electromagnetic wave shielding sheet of the present invention can be used as a ground circuit in addition to shielding electromagnetic waves, which allows a part of the ground circuit to be omitted, thereby reducing the area of the printed wiring board, thereby reducing costs and allowing it to be incorporated in a narrow area inside the housing.
[0058] In addition, the signal wiring is not particularly limited, and either a single-ended circuit consisting of one signal wiring or a differential circuit consisting of two signal wiring can be used, but a differential circuit is more preferable. On the other hand, when the circuit pattern area of the printed wiring board is limited and it is difficult to form a ground circuit in parallel, it is also possible to use an electromagnetic wave shielding layer as the ground circuit without providing a ground circuit next to the signal circuit, thereby forming a printed wiring board structure having a ground in the thickness direction.
[0059] The printed wiring board with the electromagnetic shielding sheet of the present invention is preferably provided (mounted) in electronic devices such as displays, touch panels, notebook PCs, mobile phones, smartphones, tablet terminals, and the like.
[0060] Furthermore, since the electromagnetic wave shielding sheet of the present invention has excellent shielding performance and high-speed transmission characteristics, it is preferably applied to applications requiring high-speed transmission, and specifically, it can be suitably used in electronic devices that transmit signals in the frequency range of 1 MHz to 20 GHz. EXAMPLES
[0061] The present invention will now be described in more detail with reference to examples, but the present invention is not limited thereto. In the examples and comparative examples, "parts" and "%" mean "parts by mass" and "% by mass", respectively. The acid value, phenolic hydroxyl value, and weight average molecular weight (Mw) of the resin and the average particle size of the metal filler were measured by the following methods.
[0062] <<Measurement of resin acid value>> The acid value was measured according to JIS K0070. Approximately 1 g of the sample was precisely placed in a stoppered Erlenmeyer flask. A small amount was weighed out and dissolved in 100 mL of a mixture of tetrahydrofuran and ethanol (volume ratio: tetrahydrofuran / ethanol = 2 / 1). Phenolphthalein test solution was added as an indicator, and titration was performed with 0.1N alcoholic potassium hydroxide solution. The end point was when the indicator retained a light pink color for 30 seconds. The acid value was calculated using the following formula (unit: mgKOH / g). Acid value (mgKOH / g)=(5.611×a×F) / S however, S: Amount of sample collected (g) a: Consumption of 0.1N alcoholic potassium hydroxide solution (mL) F: Potency of 0.1N alcoholic potassium hydroxide solution
[0063] <Measurement of phenolic hydroxyl value of resin> The phenolic hydroxyl value was measured according to JIS K0070. The phenolic hydroxyl value is expressed as the amount (mg) of potassium hydroxide required to neutralize the acetic acid bonded to the phenolic hydroxyl group when the phenolic hydroxyl group contained in 1 g of the phenolic hydroxyl group-containing resin is acetylated. The phenolic hydroxyl value of the phenolic hydroxyl group-containing resin was calculated taking into account the acid value as shown in the following formula. Specifically, about 1 g of the sample was precisely weighed and placed in a stoppered Erlenmeyer flask, and 100 mL of a tetrahydrofuran / ethanol (volume ratio: tetrahydrofuran / ethanol = 2 / 1) mixture was added and dissolved. Furthermore, exactly 5 mL of an acetylating agent (a solution in which 25 g of acetic anhydride was dissolved in pyridine to a volume of 100 mL) was added and stirred for about 1 hour. Phenolphthalein test solution was added as an indicator to this and held for 30 seconds. Then, the solution was titrated with 0.5 N alcoholic potassium hydroxide solution until it turned a pale pink color. The phenolic hydroxyl value was calculated according to the following formula. Phenolic hydroxyl value (mgKOH / g) = [{(ba) × F × 28.05} / S] + D however, S: Amount of sample collected (g) a: Consumption of 0.5N alcoholic potassium hydroxide solution (mL) b: Amount of 0.5N alcoholic potassium hydroxide solution consumed in the blank experiment (mL) F: Potency of 0.5N alcoholic potassium hydroxide solution D: Acid value (mgKOH / g)
[0064] <Measurement of the weight average molecular weight (Mw) of the resin of the binder component> The Mw was measured using a GPC (gel permeation chromatograph) "HPC-8020" ( GPC was performed using a gel electrophoresis system (manufactured by Tosoh Corporation). This is a liquid chromatograph that separates and quantifies substances based on the difference in their molecular size. Two "LF-604" (Showa Denko: GPC column for rapid analysis: 6 mm ID x 150 mm size) were connected in series to the column, and the flow rate was 0.6 mL / min and the column temperature was 40°C. The Mw was determined in terms of polystyrene.
[0065] <Measuring the average particle size of metal fillers> The average particle size was measured using a laser diffraction / scattering particle size distribution analyzer LS13320 (manufactured by Beckman Coulter). The D50 average particle size was obtained by measuring the filler using the Tornado dry powder sample module, and is the particle size at which the cumulative value in the cumulative particle size distribution is 50%. The refractive index was set to 1.6.
[0066] 《Raw materials》 The raw materials used in the examples and comparative examples are shown below. The binders in Tables 1 to 3 correspond to the following binders. The same applies to other hardeners and metal fillers. "binder" A-1: Polyimide resin with acid value 6 mgKOH / g, phenolic hydroxyl value 0 mgKOH / g, Mw 54,000 (manufactured by Toyochem Co., Ltd.) A-2: Polyurethane polyurea resin with an acid value of 0 mgKOH / g, a phenolic hydroxyl value of 10 mgKOH / g, and Mw of 120,000 (manufactured by Toyochem Co., Ltd.) A-3: Polyurethane polyurea resin with an acid value of 10 mgKOH / g, a phenolic hydroxyl value of 0 mgKOH / g, and Mw of 122,000 (manufactured by Toyochem Co., Ltd.) A-4: Polyurethane polyurea resin with acid value of 8 mgKOH / g, phenolic hydroxyl value of 0 mgKOH / g, and Mw of 54,000 (manufactured by Toyochem Co., Ltd.) Hardener B-1: Bisphenol A type epoxy resin "jER828" (manufactured by Mitsubishi Chemical Corporation) B-2: Multifunctional epoxy resin "TETRAD-X" (manufactured by Mitsubishi Gas Chemical Co., Ltd.) B-3: Aziridine compound "Chemithite PZ-33" (manufactured by Nippon Shokubai Co., Ltd.) B-4: Multifunctional epoxy resin "jER1031S" (manufactured by Mitsubishi Chemical Corporation) B-5: Bisphenol A type epoxy resin "jER1001" (manufactured by Mitsubishi Chemical Corporation) Metal filler C-1: Silver-coated copper powder with 10% by mass of silver coating on flake copper powder with an average particle size of 13 μm C-2: Silver-coated copper powder with 10% by mass of silver coating on flake copper powder with an average particle size of 11 μm C-3: Silver-coated copper powder with 10% by mass of silver coating on flake copper powder with an average particle size of 9 μm C-4: Silver-coated copper powder with 10% by mass of silver coating on flake copper powder with an average particle size of 16 μm C-5: Silver-coated copper powder with 10% by mass of silver coating on flake copper powder with an average particle size of 15 μm C-6: Silver-coated copper powder with 10% by mass of silver coating on flake copper powder with an average particle size of 10 μm C-7: Silver-coated copper powder with 1% by mass of silver coating on flake copper powder with an average particle size of 13 μm C-8: Silver-coated copper powder with 5% by mass of silver coating on flake copper powder with an average particle size of 13 μm C-9: Silver-coated copper powder with 8% by mass of silver coating on flake copper powder with an average particle size of 14 μm C-10: Silver-coated copper powder with 20% by mass of silver coating on flake copper powder with an average particle size of 13 μm C-11: Flake-shaped silver powder with an average particle size of 12 μm C-12: Silver-coated copper powder with 5% by mass of silver coating on dendritic copper powder with an average particle size of 8 μm
[0067] Example 1 <<Creation of protective layer>> 100 parts of binder A-1 and 15 parts of hardener B-1 were placed in a container in terms of solid content, and the mixture was stirred for 10 minutes with a disperser to obtain a resin composition. The obtained resin composition was applied onto a release sheet with a bar coater, and dried for 2 minutes in an electric oven at 100°C to produce a film (1) equipped with a protective layer (I). <<Preparation of Conductive Layer>> 100 parts of binder A-2, 20 parts of hardener B-2, 1 part of hardener B-3, and 363 parts of metal filler C-1 were charged in a container in terms of solid content, and stirred with a disperser for 10 minutes to obtain a metal filler-containing composition. The obtained metal filler-containing composition was applied to a release sheet with a bar coater and dried in an electric oven at 100°C for 2 minutes to produce a film (2) equipped with a conductive layer (II). <<Preparation of adhesive layer>> 100 parts of binder A-3, 40 parts of hardener B-4, 1.5 parts of hardener B-3, and 61 parts of metal filler C-12 were charged in a container in terms of solid content, and stirred with a disperser for 10 minutes to obtain a resin composition. The obtained resin composition was applied to a release sheet with a bar coater, and dried in an electric oven at 100°C for 2 minutes to produce a film (3) equipped with an adhesive layer (III) in the form of a release sheet. <<Making of electromagnetic wave shielding sheet>> The protective layer (I) surface of the film (1) thus prepared and the conductive layer (II) surface of the film (2) were bonded together using a laminator (100°C, pressure 2 MPa, lamination speed 1 m / min), and then the conductive layer (II) of the film (2) was peeled off from the release sheet to prepare a film (4) consisting of the conductive layer (II), protective layer (I), and release sheet. The conductive layer (II) side of the film (4) thus prepared and the adhesive layer (III) side of the film (3) were bonded together using a laminator (100°C, pressure 2 MPa, lamination speed 1 m / min) to obtain an electromagnetic wave shielding sheet with both sides covered with a release sheet.
[0068] (Examples 2 to 19, Comparative Examples 1 to 2) The same procedure as in Example 1 was carried out except that the raw materials used in Example 1 were changed to those shown in Tables 1 to 3, and an electromagnetic wave shielding sheet both sides of which were covered with a release sheet was obtained.
[0069] Comparative Example 4 An electromagnetic wave shielding sheet both sides of which were covered with a release sheet was obtained in the same manner as in Example 1, except that copper foil was used for the conductive layer.
[0070] Comparative Example 5 An electromagnetic wave shielding sheet, both sides of which were covered with a release sheet, was obtained in the same manner as in Example 1, except that a conductive layer was formed by vacuum copper deposition on the protective layer (I) side of the film (1).
[0071] Peel test An electromagnetic shielding sheet with a width of 60 mm and a length of 80 mm was prepared, the release sheet on the adhesive layer side was peeled off to expose the adhesive layer, and an adhesive tape with a width of 70 mm and a length of 140 mm (DF715 manufactured by Toyochem Co., Ltd.) was attached to the exposed surface. After the adhesive tape (DF715 manufactured by Toyochem Co., Ltd.) was attached to the release sheet laminated on the protective layer, the electromagnetic shielding sheet with the adhesive tape laminated on both sides was cut to a width of 25 mm to prepare two test pieces. The obtained test piece was pressed with a 2 kg roller for one round trip to bring the electromagnetic shielding sheet and the adhesive tape into close contact. The peel force was measured using a tensile tester conforming to JIS Z0237 under the conditions of a peel angle of 180° and a peel speed of 300 mm / min, and the average value of the two test pieces was taken as the peel force. Furthermore, the peeled surface after the peel test was visually observed, and the area of the conductive layer transferred to the protective layer and adhesive layer due to cohesive failure was measured. When the conductive layer peeled off together with the protective layer or adhesive layer without cohesive failure, the cohesive failure rate was recorded as 0%.
[0072] <Cross-section evaluation> The release sheet on the adhesive layer side of the electromagnetic shielding sheet was peeled off, and the exposed adhesive layer and polyimide film ("Kapton 200EN" manufactured by Toray DuPont Co., Ltd.) were bonded together, and the laminate was heat-pressed for 30 minutes under conditions of 2 MPa and 170°C. After cutting the laminate into a size of about 5 mm in width and 5 mm in length, 0.05 g of epoxy resin (Petropoxy 154, manufactured by Maruto Co., Ltd.) was dropped onto a slide glass and bonded to the electromagnetic shielding sheet, to obtain a laminate consisting of slide glass / electromagnetic shielding sheet / polyimide film. The obtained laminate was cut by ion beam irradiation from the polyimide film side using a cross-section polisher (manufactured by JEOL Ltd., SM-09010), and platinum was evaporated on the cross section to obtain a cross section of the electromagnetic shielding sheet after heat pressing (hereinafter referred to as "cross section of measurement sample").
[0073] <Thickness measurement> The cross section of the measurement sample was observed with a scanning electron microscope (JSM-6010Plus, manufactured by JEOL Ltd.) to measure the thickness of each layer. The magnification was 500 to 5000 times, and the average thickness of 10 points was taken as the thickness of each layer.
[0074] <Measuring the aspect ratio of metal filler> The cross section of the measurement sample was observed with a scanning electron microscope (JSM-6010Plus, manufactured by JEOL Ltd.) to measure the aspect ratio of the metal filler. The magnification was 3000 to 5000 times, and the average of 30 metal fillers was taken as the aspect ratio. The aspect ratio is [long diameter (μm)] / [thickness (μm)].
[0075] <<Measurement of the area occupied by metal filler>> The cross section of the measurement sample was observed at a magnification of 500 to 5000 times using a scanning electron microscope (JEOL, JSM-6010Plus), and the area of the filler in the conductive layer was measured. When observed with an electron microscope, the atomic number effect creates a contrast difference between the resin layer and the metal layer, making it possible to recognize the shape of the metal. Specifically, the metal is colored white, and the resin layer is colored gray to black, making it possible to distinguish between the resin and metal parts. The electron microscope images were binarized into black and white using the free image analysis software "GIMP2.6.11," and the number of black and white pixels was counted to calculate the area ratio of the metal filler in the conductive layer to the area of components other than the metal filler. The area of the filler (number of white pixels) was taken as the area occupied by the filler when the area of the conductive layer (number of black and white pixels) was taken as 100.
[0076] 《Measurement of the mass ratio of elemental silver》 A scanning electron microscope (JEOL, JSM-6010Plus) and an energy dispersive X-ray analyzer (JEOL, JED-2300) were used to obtain a qualitative analysis chart of each element in the cross section of the measurement sample at an acceleration voltage of 20 kV and a magnification of 3000 to 10000 times. For the conductive layer, the mass concentration of each element was calculated based on the qualitative analysis chart. The amount of silver is the relative mass (%) of silver when the "total mass of copper and silver elements" is taken as 100%, and when copper element is not detected or the amount of silver element is 98% or more, the amount of silver element is taken as 100%. In addition, energy dispersive X-ray analysis can detect elements located several μm deep from the surface, and cross-sectional analysis is difficult to perform from a completely vertical direction. Therefore, only 50% of the conductive layer in the thickness direction was analyzed to avoid being influenced by the protective layer and adhesive layer.
[0077] <<Measurement of the surface resistivity of the conductive layer>> A conductive paste consisting of epoxy resin and silver powder was used to screen print a pattern of four points spaced 5 mm apart in a straight line on the release-treated surface of a heat-resistant polyester film. After drying, the conductive paste was heated and cured in an oven at 180°C to form conductive bumps with a diameter of 500 μm and a height of 100 μm. The electromagnetic shielding sheet, both sides of which were covered with a release sheet, was cut into a long side of 80 mm and a short side of 50 mm, the release sheet on the adhesive layer (III) side was peeled off, and the exposed adhesive layer (III) was placed on the heat-resistant polyester film on which the conductive bumps were formed, and pressure-bonded under conditions of 170°C, 2 MPa, and 30 minutes. The four conductive bumps were pressure-bonded so as to be parallel to the long sides of the sample piece. The pressure-bonded conductive bumps with a height of 100 μm penetrated the adhesive layer (III) and reached the conductive layer (II). After the pressure bonding, the heat-resistant polyester film that had been subjected to a release treatment was removed to expose the adhesive layer (III) and the conductive bumps. The conductive bump was used as a measurement electrode, and the resistance was measured using a four-point probe, "Loresta GP" manufactured by Mitsubishi Chemical Corporation, in accordance with JIS K7194-1994. The surface resistivity was calculated by multiplying the measured value by the constant "4.239". In addition, since the adhesive layer (III) is an anisotropic conductive adhesive layer that exhibits electrical conductivity only in the thickness direction or an adhesive layer that has no electrical conductivity, the resistance value measured even if the conductive bump penetrates the adhesive layer (III) is the resistance value of the conductive layer (II).
[0078] How to determine the conductivity of a conductive layer The electrical conductivity σ (S / m) of the conductive layer was calculated from the thickness t (μm) and surface resistivity R (Ω / □) of the conductive layer measured above, according to the following formula. σ=10 6 / R / t
[0079] 《Career breakthrough aptitude assessment》 An electromagnetic shielding sheet with a width of 50 mm and a length of 250 mm was prepared, and a weak adhesive tape (LE951 manufactured by Toyochem Co., Ltd.) was attached to the release sheet on the protective layer side, and a 2 kg roller was used to pressurize the electromagnetic shielding sheet and the weak adhesive tape once. A total of 20 pieces of 10 mm x 30 mm were cut out using a die-cutting machine. The release sheet on the adhesive layer side of the die-cut electromagnetic shielding sheet was peeled off, and the exposed adhesive layer was bonded to a polyimide film ("Kapton 200EN" manufactured by Toray DuPont Co., Ltd.) and laminated (90°C, pressure 0.3 MPa, lamination speed 2 m / min). The weak adhesive tape was then peeled off, the peeling interface was observed, and the number of pieces corresponding to defective products was counted. The defective rate was calculated using the formula shown below to evaluate the punching processability. (Defective rate) = (Number of defective pieces) / (Total number of cut pieces) x 100 Here, a defective product refers to a product in which, when the weak adhesive tape is peeled off, the peeling interface is not the interface between the weak adhesive tape and the electromagnetic wave shield, but peeling occurs within the electromagnetic wave shielding sheet. The evaluation criteria were as follows: ++: The defect rate is 0%. Extremely good. +: The defect rate is 10% or less. Good. NG: The defect rate is greater than 10%. Not practical.
[0080] <Evaluation of transmission characteristics> The transmission characteristics were evaluated using a printed wiring board with an electromagnetic shielding sheet having a coplanar circuit. A schematic plan view of the main surface of a flexible printed wiring board 1 having a coplanar circuit (hereinafter, also referred to as a wiring circuit board having a coplanar circuit) used in the measurement is shown in FIG. 1, and a schematic plan view of the back surface is shown in FIG. 2. First, a double-sided CCL "R-F775" (manufactured by Panasonic Corporation) was prepared in which rolled copper foil having a thickness of 12 μm was laminated on both sides of a polyimide film 20 having a thickness of 50 μm. Then, six through holes 22 (diameter 0.1 mm) were provided near each of the four rectangular corners. Note that in the figure, only two through holes 22 are shown at each corner for convenience of illustration. Next, electroless plating was performed, and then electrolytic plating was performed to form a 10 μm copper plating film 21, and conduction between the main surface and the back surface was ensured through the copper plating film formed in the through holes 22. Then, as shown in FIG. 1, two signal wires 23, each 10 cm long, were formed on the main surface of the polyimide film 20, along with a ground wire 24 extending parallel to the signal wires 23 on the outside of the signal wires 23, and a ground pattern 25 was formed in an area including the through-holes 22 extending in the short direction of the polyimide film 20.
[0081] Thereafter, the copper foil formed on the back surface of the polyimide film 20 was etched to obtain a back surface ground pattern 26 as shown in FIG. 2 at a position corresponding to the ground pattern 25. The inspection specifications for the circuit appearance and tolerance were JPCA standard (JPCA-DG02). Next, a cover coat layer 3 "CISV1215 (manufactured by Nikkan Industries Co., Ltd.)" consisting of a polyimide film (thickness 12.5 μm) and an insulating adhesive layer (thickness 15 μm) was attached to the main surface side of the polyimide film 20. In addition, in FIG. 1, the cover coat layer 3 is shown in a perspective view so that the structure of the signal wiring 23 and the like can be seen. Thereafter, the copper foil pattern exposed from the cover coat layer 3 was nickel-plated (not shown) and then gold-plated (not shown).
[0082] Next, as shown in Fig. 3, an electromagnetic shielding sheet was prepared, and a release sheet (not shown) provided on the adhesive layer was peeled off. Then, the electromagnetic shielding sheet was pressure-bonded to the entire rear surface of the wiring circuit board 1 having a coplanar circuit with the adhesive layer of the electromagnetic shielding sheet facing inward under conditions of 170°C, 2.0 MPa, and 30 minutes, and the release sheet on the protective layer surface was peeled off to obtain a printed wiring board 5 with an electromagnetic shielding sheet having a coplanar circuit and the electromagnetic shielding sheet 4 of each of the Examples and Comparative Examples. In Fig. 3, the rear surface side ground pattern 26 is shown in a see-through view.
[0083] The L / S (line / space) of the signal wiring 23 was appropriately adjusted so that the characteristic impedance was within ±10 Ω. The width of the ground wiring 24 was 100 μm, and the distance between the ground wiring 24 and the signal wiring 23 was 1 mm.
[0084] A network analyzer E5071C (Keysight Technologies) was connected to the exposed signal wiring 23 of the printed wiring board 5 with an electromagnetic shielding sheet having a coplanar circuit, and a 15 GHz sine wave was input to measure the transmission loss to evaluate the transmission characteristics. The measured transmission characteristics were evaluated according to the following criteria. +++: Transmission loss at 15 GHz is less than 7.0 dB. Very good. ++: Transmission loss at 15 GHz is 7.0 dB or more and less than 8.0 dB. Good. +: Transmission loss at 15GHz is 8.0dB or more and less than 9.0dB. Practical use is possible. NG: Transmission loss at 15 GHz is 9.0 dB or more. Not practical.
[0085] <Shielding performance evaluation> The electromagnetic wave shielding sheet was sandwiched between release films and heat pressed at 170℃, 2MPa, and 30 minutes, and the release films were removed to obtain a measurement sample. The shielding effect was measured in accordance with ASTM D4935, and electromagnetic waves were irradiated at 300MHz to 20GHz using a coaxial tube type shielding effect measurement system manufactured by Keycom. The amount of attenuation of the electromagnetic waves by the electromagnetic wave shielding sheet was measured and evaluated according to the following criteria. The attenuation is measured in decibels (unit: dB). +++: Attenuation when exposed to 15GHz electromagnetic waves is less than -60dB. Extremely good. ++: Attenuation when exposed to 15GHz electromagnetic waves is -60dB or more and less than -55dB. Good. +: Attenuation when exposed to 15GHz electromagnetic waves is -55dB or more and less than -50dB. Practical use is possible. NG: Attenuation when exposed to 15GHz electromagnetic waves is -50dB or more. Not practical.
[0086] <Evaluation of gas release properties> Gas leakage was evaluated using a test sheet made of a copper-clad laminate simulating a printed circuit board and an electromagnetic shielding sheet. The test piece was brought into contact with molten solder, and the appearance of the sample was evaluated based on whether it changed or not. Electromagnetic shielding sheets with high gas release properties can release outgassing such as water vapor from printed circuit boards. The gas can be efficiently released outside the wiring circuit board, so the appearance does not change, but the gas release properties are With low-performance electromagnetic shielding sheets, outgassing does not escape efficiently, resulting in foaming and peeling. First, the release sheet on the adhesive layer side of an electromagnetic shielding sheet with a width of 25 mm and a length of 70 mm was peeled off, and the exposed adhesive layer was pressed against the gold-plated surface of a gold-plated copper-clad laminate (gold plating 0.3 μm / nickel plating 1 μm / copper foil 18 μm / adhesive 20 μm / polyimide film 25 μm) with a total thickness of 64 μm at 170°C, 2 MPa, and 30 minutes to obtain a thermoset laminate. The obtained laminate was cut into a size of 10 mm wide and 65 mm long to prepare a sample. The obtained sample was left in an atmosphere of 40°C and 90% RH for 72 hours. Then, the polyimide film side of the sample was placed down on molten solder at 250°C for 1 minute. The appearance of the removed sample was visually observed and evaluated according to the following criteria. ++: No visual change or defect in appearance is observed. Very good. +: The area of defective appearance is 10% or less of the protective layer area in the sample. Good. NG: The area of defective appearance is greater than 10% of the protective layer area in the sample.
[0087] [Table 1]
[0088] [Table 2]
[0089] [Table 3]
[0090] As shown in Tables 1 to 3, compared to Comparative Examples 1 to 4, the electromagnetic wave shielding sheets of Examples 1 to 19 of the present invention had high peel strength, low volume resistivity and surface resistivity, and were excellent in carrier punching suitability, shielding properties, and gas release properties. [Explanation of symbols]
[0091] 1: Wiring circuit board 20: Polyimide film 21: Copper plating film 22:Through hole 23: Signal wiring 24: Ground wiring 25: Ground Pattern 26: Ground pattern on the back side 3: Cover coat layer 4: Electromagnetic wave shielding sheet 5: Printed wiring board with electromagnetic shielding sheet
Claims
1. An electromagnetic wave shielding sheet in which a protective layer, a conductive layer, and an adhesive layer are laminated in this order, the conductive layer includes a metal filler and a binder; a peel test is performed at a peel angle of 180° between the protective layer and the adhesive layer and a peel rate of 300 mm / min, and the peel force at which the conductive layer experiences cohesive failure is 50 to 2500 [gf / 25 mm]; An electromagnetic wave shielding sheet in which the conductive layer has a cohesive failure rate of 10% or more in the peel test.
2. The conductivity of the conductive layer is 2.4×10 6 ~3.0 x 10 7 2. The electromagnetic wave shielding sheet according to claim 1, wherein the tensile strength is [S / m].
3. The surface resistivity of the conductive layer is 4.0×10 -3 ~2.0 x 10 -1 2. The electromagnetic wave shielding sheet according to claim 1, wherein the resistance is [Ω / □].
4. 2. The electromagnetic wave shielding sheet according to claim 1, wherein, in a cut surface of the electromagnetic wave shielding sheet after heat-pressure bonding under conditions of 170°C, 2 MPa, and 30 minutes, the area occupied by the metal filler is 23 to 95 when the cross-sectional area of the conductive layer is taken as 100.
5. 2. The electromagnetic wave shielding sheet according to claim 1, wherein the thickness of the conductive layer on the cut surface after the electromagnetic wave shielding sheet is heat-pressed under conditions of 170° C., 2 MPa, and 30 minutes is 1 to 12 μm.
6. The metal filler includes a flake metal filler, 2. The electromagnetic wave shielding sheet according to claim 1, wherein the flake metal filler has an average aspect ratio of 10 to 70 on a cut surface of the conductive layer after the electromagnetic wave shielding sheet is heat-pressurized under conditions of 170°C, 2 MPa, and 30 minutes.
7. 2. The electromagnetic wave shielding sheet according to claim 1, wherein the metal filler comprises silver-coated copper powder, and the proportion by mass of silver element is 3% or more and 25% or less when the total mass of copper and silver element is taken as 100%, as measured by energy dispersive X-ray analysis, on a cut surface of the conductive layer after the electromagnetic wave shielding sheet has been heat-pressed under conditions of 170°C, 2 MPa, and 30 minutes.
8. A printed wiring board provided with the electromagnetic wave shielding sheet according to any one of claims 1 to 7.
9. An electronic device comprising the printed wiring board with the electromagnetic wave shielding sheet according to claim 8.
Citation Information
Patent Citations
Protection film for temporarily laminating electromagnetic wave shielding sheet, its manufacturing method, and electromagnetic wave shielding sheet
JP2008031447A
Conductive adhesive tape and manufacturing method of conductive adhesive tape
JP2018053137A
Electromagnetic wave shielding film and method of producing the same, and printed wiring board with electromagnetic wave shielding film and method of manufacturing the same
JP2019016782A
JPP6544466B
Shield film, shielded printed wiring board, and method for manufacturing shield film
WO2013077108A1