Composition for forming resist underlayer film containing polycyclic aromatic polymer

A resist underlayer film with polycyclic aromatic hydrocarbon and maleimide structures addresses LER and LWR issues in semiconductor patterning, improving pattern quality and uniformity in EUV or EB lithography.

JP7559975B2Active Publication Date: 2024-10-02NISSAN CHEM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023564039
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-09
Filing Date
2022-12-08
Publication Date
2024-10-02
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

The formation of fine patterns in semiconductor devices is hindered by line edge roughness (LER) and line width roughness (LWR) in resist patterns, which adversely affect device performance, and existing methods to suppress these issues have not been satisfactory.

Method used

A resist underlayer film is developed using a polymer composition containing polycyclic aromatic hydrocarbon and maleimide structures, with a film thickness of less than 10 nm, which improves adhesion and reduces LWR when used in electron beam (EB) or extreme ultraviolet (EUV) lithography.

Benefits of technology

The resist underlayer film effectively reduces LWR, enhancing the quality of resist patterns and improving the uniformity of pattern formation, particularly in EUV or EB lithography, by maintaining film flatness and preventing pattern peeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559975000001
    Figure 0007559975000001
  • Figure 0007559975000002
    Figure 0007559975000002
  • Figure 0007559975000003
    Figure 0007559975000003
Patent Text Reader

Abstract

A resist underlayer film which is a burned coating film from a composition for resist underlayer film formation, wherein the composition for resist underlayer film formation includes a polymer having a unit structure (A) having a polycyclic aromatic hydrocarbon structure and / or a unit structure (B) derived from a maleimide structure. The resist underlayer film has a film thickness less than 10 nm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resist underlayer film, a composition for forming a resist underlayer film for EB or EUV lithography, a substrate for semiconductor processing, a method for producing a semiconductor element, a pattern forming method, and a method for improving the LWR of a resist pattern. [Background technology]

[0002] 2. Description of the Related Art In semiconductor devices such as LSIs (semiconductor integrated circuits), the formation of fine patterns is required as the integration density increases, and in recent years the minimum pattern size has reached 100 nm or less. The formation of such fine patterns in semiconductor devices has been made possible by shortening the wavelength of the light source in exposure equipment and improving resist materials. Currently, the immersion exposure method uses deep ultraviolet light of 193 nm wavelength ArF (argon fluoride) excimer laser light as a light source, and exposure is performed through water. Regarding resist materials, various ArF-compatible resist materials based on acrylic resins have been developed.

[0003] Furthermore, as next-generation exposure technologies, research is underway on electron beam (EB) exposure methods and extreme ultraviolet (EUV) exposure methods that use soft X-rays with a wavelength of 13.5 nm as a light source, and pattern sizes are expected to become even finer, reaching 30 nm or less. However, as pattern sizes become finer, the line edge roughness (LER) of the resist pattern sidewall and the line width roughness (LWR) of the resist pattern become larger, raising concerns that they may adversely affect device performance. Although studies have been conducted to suppress these issues by optimizing exposure equipment, resist materials, and process conditions, satisfactory results have not been obtained. Note that LWR and LER are related, and improving LWR will also improve LER.

[0004] As a method for solving the above problems, a method has been disclosed in which the resist pattern is treated with an aqueous solution containing a specific ionic surfactant in a rinsing step after the development process, thereby suppressing defects (such as residue generation and pattern collapse) caused by the development process and dissolving unevenness in the resist pattern, thereby improving the LWR and LER (see Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-213013 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a resist underlayer film capable of improving the LWR of a resist pattern, a composition for forming a resist underlayer film for EB or EUV lithography, a resist underlayer film for EB or EUV lithography, a substrate for semiconductor processing, a method for producing a semiconductor element, a pattern forming method, and a method for improving the LWR of a resist pattern. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved, and have completed the present invention having the following gist. That is, the present invention includes the following. [1] A resist underlayer film which is a fired product of a coating film of a composition for forming a resist underlayer film, The composition for forming a resist underlayer film contains a polymer having at least one unit structure selected from the group consisting of a unit structure (A) having a polycyclic aromatic hydrocarbon structure and a unit structure (B) having a maleimide structure, The resist underlayer film has a thickness of less than 10 nm. [2] The resist underlayer film according to [1], wherein the polycyclic aromatic hydrocarbon structure in the unit structure (A) includes at least one structure selected from the group consisting of naphthalene, anthracene, phenanthrene, carbazole, pyrene, triphenylene, chrysene, naphthacene, biphenylene, and fluorene. [3] The resist underlayer film according to [1] or [2], wherein the unit structure (B) is represented by the following formula (4): [ka] (In formula (4), R 2 represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted with a hydroxyl group, or an aryl group having 6 to 10 carbon atoms which may be substituted with a halogen atom. [4] The resist underlayer film according to any one of [1] to [3], wherein the polymer further comprises a unit structure (C) having a crosslinking group. [5] The resist underlayer film according to [4], wherein the crosslinking group in the unit structure (C) includes at least one group selected from the group consisting of a hydroxy group, an epoxy group, a protected hydroxy group, and a protected carboxy group. [6] The resist underlayer film according to any one of [1] to [5], wherein the composition for forming a resist underlayer film further contains a crosslinking agent. [7] The resist underlayer film according to any one of [1] to [6], wherein the composition for forming a resist underlayer film further contains a curing catalyst. [8] The resist underlayer film according to any one of [1] to [7], which is a resist underlayer film for EB or EUV lithography. [9] A composition for forming a resist underlayer film for EB or EUV lithography, comprising a polymer having at least one unit structure selected from the group consisting of a unit structure (A) having a polycyclic aromatic hydrocarbon structure and a unit structure (B) having a maleimide structure.

[10] The composition for forming a resist underlayer film for EB or EUV lithography according to [9], wherein the polycyclic aromatic hydrocarbon structure in the unit structure (A) includes at least one structure selected from the group consisting of naphthalene, anthracene, phenanthrene, carbazole, pyrene, triphenylene, chrysene, naphthacene, biphenylene, and fluorene.

[11] The composition for forming a resist underlayer film for EB or EUV lithography according to [9] or

[10] , wherein the unit structure (B) is represented by the following formula (4): [ka] (In formula (4), R 2 represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted with a hydroxyl group, or an aryl group having 6 to 10 carbon atoms which may be substituted with a halogen atom.

[12] The composition for forming a resist underlayer film for EB or EUV lithography according to any one of [9] to

[11] , wherein the polymer further has a unit structure (C) having a crosslinking group.

[13] The composition for forming a resist underlayer film for EB or EUV lithography according to

[12] , wherein the crosslinking group in the unit structure (C) includes at least one group selected from the group consisting of a hydroxy group, an epoxy group, a protected hydroxy group, and a protected carboxy group.

[14] The composition for forming a resist underlayer film for EB or EUV lithography according to any one of [9] to

[13] , further comprising a crosslinking agent.

[15] The composition for forming a resist underlayer film for EB or EUV lithography according to any one of [9] to

[14] , further comprising a curing catalyst.

[16] A composition for forming a resist underlayer film for EB or EUV lithography according to any one of claims 9 to 15, which is used in forming a resist underlayer film according to any one of [1] to [8].

[17] A resist underlayer film for EB or EUV lithography, which is a fired product of a coating film of a composition for forming a resist underlayer film for EB or EUV lithography according to any one of [9] to

[16] .

[18] A semiconductor substrate; [1] to [8] or the resist underlayer film for EB or EUV lithography according to

[17] ; A semiconductor processing substrate comprising:

[19] A step of forming a resist underlayer film having a thickness of less than 10 nm on a semiconductor substrate using a composition for forming a resist underlayer film for EB or EUV lithography according to any one of [9] to

[16] ; forming a resist film on the resist underlayer film using a resist for EB or EUV lithography; A method for manufacturing a semiconductor device, comprising:

[20] A step of forming a resist underlayer film having a thickness of less than 10 nm on a semiconductor substrate using a composition for forming a resist underlayer film for EB or EUV lithography according to any one of [9] to

[16] ; forming a resist film on the resist underlayer film using a resist for EB or EUV lithography; irradiating the resist film with EB or EUV, and then developing the resist film to obtain a resist pattern; Etching the resist underlayer film using the resist pattern as a mask; A pattern forming method comprising the steps of:

[21] A step of forming a resist underlayer film having a thickness of less than 10 nm on a semiconductor substrate using a composition for forming a resist underlayer film for EB or EUV lithography according to any one of [9] to

[16] ; forming a resist film on the resist underlayer film using a resist for EB or EUV lithography; irradiating the resist film with EB or EUV, and then developing the resist film to obtain a resist pattern; The present invention relates to a method for improving LWR of a resist pattern, Effect of the Invention

[0008] According to the present invention, it is possible to provide a resist underlayer film capable of improving the LWR of a resist pattern, a composition for forming a resist underlayer film for EB or EUV lithography, a resist underlayer film for EB or EUV lithography, a substrate for semiconductor processing, a method for producing a semiconductor element, a pattern forming method, and a method for improving the LWR of a resist pattern. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The resist underlayer film of the present invention is a product obtained by baking a coating film of a composition for forming a resist underlayer film. Therefore, after explaining the composition for forming a resist underlayer film, the resist underlayer film of the present invention will be explained.

[0010] (Composition for forming resist underlayer film) The composition for forming a resist underlayer film of the present embodiment contains a polymer having at least one unit structure of a unit structure (A) having a polycyclic aromatic hydrocarbon structure and a unit structure (B) derived from a maleimide structure. In addition to the polymer, the composition for forming a resist underlayer film of the present embodiment may further contain a solvent, a crosslinking agent, and a curing catalyst. In addition, other additives may be contained as long as they do not impair the effects of the present invention.

[0011] <Polymer> As described above, the polymer has at least one unit structure selected from the unit structure (A) having a polycyclic aromatic hydrocarbon structure and the unit structure (B) derived from a maleimide structure. Since the polymer has at least one of the unit structures (A) and (B) derived from a maleimide structure, when the polymer is used as a resist underlayer film, the adhesion between the resist and the resist underlayer film interface during resist pattern formation tends to be improved. Therefore, it is presumed that the peeling of the resist pattern does not occur and the deterioration of the LWR during resist pattern formation can be suppressed. In particular, a remarkable effect is exhibited when EUV (wavelength 13.5 nm) or EB (electron beam) is used.

[0012] In the present specification, the term "polycyclic aromatic hydrocarbon structure" refers to an aromatic structure having a polycyclic aromatic hydrocarbon. In addition, in the present specification, the term "unit structure derived from a maleimide structure" refers to a repeating unit in a polymer, which is obtained by reacting a carbon-carbon double bond of maleimide or a maleimide derivative. The maleimide derivative refers to a compound obtained by substituting a hydrogen atom of an NH group of maleimide.

[0013] <<Unit structure (A)>> As described above, the unit structure (A) is a unit structure having a polycyclic aromatic hydrocarbon structure. In this specification, the polycyclic aromatic hydrocarbon structure refers to an aromatic structure having a hydrocarbon composed of two or more aromatic rings exhibiting aromaticity, and includes a condensed polycyclic aromatic hydrocarbon structure having a condensed ring, and a hydrocarbon ring assembly structure in which a plurality of aromatic rings are directly bonded to each other via single bonds. In this specification, the polycyclic aromatic hydrocarbon structure also includes a heterocyclic structure in which some carbon atoms in an aromatic ring are substituted with nitrogen.

[0014] The condensed polycyclic aromatic hydrocarbon structure is not particularly limited, but examples thereof include a naphthalene structure, anthracene structure, phenanthrene structure, pyrene structure, triphenylene structure, chrysene structure, naphthacene structure, biphenylene structure, and fluorene structure.

[0015] The hydrocarbon ring assembly structure is not particularly limited, but examples thereof include a carbazole structure, a biphenyl structure, a terphenyl structure, a quaterphenyl structure, a binaphthalene structure, a phenylnaphthalene structure, a phenylfluorene structure, and a diphenylfluorene structure.

[0016] The polycyclic aromatic hydrocarbon structure may be substituted with a substituent. The optionally substituted substituent is not particularly limited, and examples thereof include an alkyl group, a hydroxyl group, a carboxyl group, and a halogen group (e.g., a fluorine group, a chlorine group, a bromine group, and an iodine group). Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, an n-hexyl group, a 1-methyl-n-pentyl group, a 2-methyl-n-pentyl group, a 3-methyl-n-pentyl group, a 2 ... Examples of such aryl groups include ethyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, and 1-ethyl-2-methyl-n-propyl groups.Furthermore, a cyclic alkyl group can also be used as the alkyl group. For example, examples of the cyclic alkyl group having 1 to 10 carbon atoms include a cyclopropyl group, a cyclobutyl group, a 1-methylcyclopropyl group, a 2-methylcyclopropyl group, a cyclopentyl group, a 1-methylcyclobutyl group, a 2-methylcyclobutyl group, a 3-methylcyclobutyl group, a 1,2-dimethylcyclopropyl group, a 2,3-dimethylcyclopropyl group, a 1-ethylcyclopropyl group, a 2-ethylcyclopropyl group, a cyclohexyl group, a 1-methylcyclopentyl group, a 2-methylcyclopentyl group, a 3-methylcyclopentyl group, a 1-ethylcyclobutyl group, a 2-ethylcyclobutyl group, a 3-ethylcyclobutyl group, a 1,2-dimethyl ... Examples of such groups include 1-n-propyl-cyclopropyl group, 2-n-propyl-cyclopropyl group, 1-i-propyl-cyclopropyl group, 2-i-propyl-cyclopropyl group, 1,2,2-trimethyl-cyclopropyl group, 1,2,3-trimethyl-cyclopropyl group, 2,2,3-trimethyl-cyclopropyl group, 1-ethyl-2-methyl-cyclopropyl group, 2-ethyl-1-methyl-cyclopropyl group, 2-ethyl-2-methyl-cyclopropyl group, and 2-ethyl-3-methyl-cyclopropyl group.

[0017] From the viewpoint of suitably obtaining the effects of the present invention, the polycyclic aromatic hydrocarbon structure is preferably a naphthalene structure, an anthracene structure, a phenanthrene structure, a pyrene structure, a triphenylene structure, a chrysene structure, a naphthacene structure, a biphenylene structure, a fluorene structure, or a carbazole structure, more preferably a naphthalene structure, an anthracene structure, a phenanthrene structure, a pyrene structure, or a carbazole structure, and even more preferably a naphthalene structure or a carbazole structure. The polycyclic aromatic hydrocarbon structure may be of one type or two or more types, but is preferably of one or two types.

[0018] The unit structure (A) is not particularly limited, but a unit structure represented by the following formula (1) can be suitably used. [ka] (In formula (1), R 1 represents a hydrogen atom or a methyl group. X represents an ester group or an amide group. Y represents an alkylene group having 1 to 6 carbon atoms. p and q each independently represent 0 or 1. Ar represents a monovalent group obtained by removing a hydrogen atom from naphthalene, anthracene, phenanthrene, pyrene, triphenylene, chrysene, naphthacene, biphenylene, fluorene, or carbazole, which may be substituted.

[0019] Furthermore, the unit structure (A) is not particularly limited, but a unit structure represented by the following formula (2) can be suitably used. [ka] (In formula (2), R 1 represents a hydrogen atom or a methyl group, Z represents a halogen atom, a hydroxyl group, an alkyl group, an alkoxy group, a thiol group, a cyano group, a carboxyl group, an amino group, an amido group, an alkoxycarbonyl group, or a thioalkyl group substituted on a naphthalene ring, and n represents an integer of 0 to 7. When n is 2 or more, two or more Z's may be the same or different.

[0020] In Z, the halogen atom may be a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom. The alkyl group may be, for example, a linear or branched alkyl group having 1 to 6 carbon atoms, which may be substituted with a halogen atom or the like. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butoxy group, a t-butoxy group, an n-hexyl group, and a chloromethyl group. Examples of the alkoxy group include an alkoxy group having 1 to 6 carbon atoms, such as a methoxy group, an ethoxy group, and an isopropoxy group. Examples of the amide group include an amide group having 1 to 12 carbon atoms, such as a formamide group, an acetamide group, a propionamide group, an isobutylamide group, a benzamide group, a naphthylamide group, and an acrylamide group. Examples of the alkoxycarbonyl group include an alkoxycarbonyl group having 1 to 12 carbon atoms, such as a methoxycarbonyl group, an ethoxycarbonyl group, and a benzyloxycarbonyl group. The thioalkyl group is, for example, a thioalkyl group having 1 to 6 carbon atoms, such as a methylthio group, an ethylthio group, a butylthio group, and a hexylthio group.

[0021] Specific examples of the unit structure (A) represented by formula (2) are as follows: [ka] [ka]

[0022] Furthermore, as the unit structure (A), although there is no particular limitation, a unit structure represented by the following formula (3) can be suitably used. [ka] (In formula (3), Ar 1 and Ar 2 each independently represents an aromatic ring having 6 to 40 carbon atoms which may be substituted, and Ar 1 and Ar 2At least one of is naphthalene, anthracene, phenanthrene, or pyrene, and Q represents a single bond or a divalent linking group.

[0023] Examples of aromatic rings having 6 to 40 carbon atoms include benzene, naphthalene, anthracene, acenaphthene, fluorene, triphenylene, phenalene, phenanthrene, indene, indane, indacene, pyrene, chrysene, perylene, naphthacene, pentacene, coronene, heptacene, benzo[a]anthracene, dibenzophenanthrene, and dibenzo[a,j]anthracene.

[0024] Examples of the divalent linking group for Q include an ether group, an ester group, and an imino group, and the imino group is preferable.

[0025] The unit structure (A) may be of one or more types, preferably one or two types.

[0026] When the polymer contains the unit structure (A), the molar ratio of the unit structure (A) is preferably 10 to 90 mol %, more preferably 30 to 85 mol %, and even more preferably 40 to 80 mol %, based on all unit structures of the polymer, from the viewpoint of suitably obtaining the effects of the present invention.

[0027] <<Unit structure (B)>> The unit structure (B) is the above-mentioned unit structure derived from a maleimide structure.

[0028] The unit structure (B) is preferably a unit structure represented by the following formula (4). [ka] (In formula (4), R 2 represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted with a hydroxyl group, or an aryl group having 6 to 10 carbon atoms which may be substituted with a halogen atom.

[0029] The alkyl group having 1 to 10 carbon atoms may be linear, branched, or cyclic. Examples of the alkylene group having 1 to 10 carbon atoms include a methylene group, an ethylene group, an n-propylene group, an isopropylene group, a cyclopropylene group, an n-butylene group, an isobutylene group, an s-butylene group, a t-butylene group, a cyclobutylene group, a 1-methyl-cyclopropylene group, a 2-methyl-cyclopropylene group, an n-pentylene group, a 1-methyl-n-butylene group, a 2-methyl-n-butylene group, a 3-methyl-n-butylene group, a 1,1-dimethyl-n-propylene group, a 1,2-dimethyl-n-propylene group, a 2 ... propylene, 1-ethyl-n-propylene, cyclopentylene, 1-methyl-cyclobutylene, 2-methyl-cyclobutylene, 3-methyl-cyclobutylene, 1,2-dimethyl-cyclopropylene, 2,3-dimethyl-cyclopropylene, 1-ethyl-cyclopropylene, 2-ethyl-cyclopropylene, n-hexylene, 1-methyl-n-pentylene, 2-methyl-n-pentylene, 3-methyl-n-pentylene, 4-methyl-n-pentylene, 1,1-dimethyl-n-butylene, 1,2-dimethyl- n-butylene group, 1,3-dimethyl-n-butylene group, 2,2-dimethyl-n-butylene group, 2,3-dimethyl-n-butylene group, 3,3-dimethyl-n-butylene group, 1-ethyl-n-butylene group, 2-ethyl-n-butylene group, 1,1,2-trimethyl-n-propylene group, 1,2,2-trimethyl-n-propylene group, 1-ethyl-1-methyl-n-propylene group, 1-ethyl-2-methyl-n-propylene group, cyclohexylene group, 1-methyl-cyclopentylene group, 2-methyl-cyclopentylene group, 3-methyl-cyclo Pentylene group, 1-ethyl-cyclobutylene group, 2-ethyl-cyclobutylene group, 3-ethyl-cyclobutylene group, 1,2-dimethyl-cyclobutylene group, 1,3-dimethyl-cyclobutylene group, 2,2-dimethyl-cyclobutylene group, 2,3-dimethyl-cyclobutylene group, 2,4-dimethyl-cyclobutylene group, 3,3-dimethyl-cyclobutylene group, 1-n-propyl-cyclopropylene group, 2-n-propyl-cyclopropylene group, 1-isopropyl-cyclopropylene group, 2-isopropyl-cyclopropylene group, 1,2,Examples of the cyclopropylene group include a 2-trimethylcyclopropylene group, a 1,2,3-trimethylcyclopropylene group, a 2,2,3-trimethylcyclopropylene group, a 1-ethyl-2-methylcyclopropylene group, a 2-ethyl-1-methylcyclopropylene group, a 2-ethyl-2-methylcyclopropylene group, a 2-ethyl-3-methylcyclopropylene group, an n-heptylene group, an n-octylene group, an n-nonylene group, and an n-decanylene group. Any hydrogen atom in these alkyl groups having 1 to 10 carbon atoms may be substituted with a hydroxy group.

[0030] The halogen atom is as described above. Examples of the aryl group having 6 to 10 carbon atoms include a phenyl group, a benzyl group, and a naphthyl group.

[0031] Specific examples of the unit structure (B) represented by formula (4) include the following unit structures. [ka]

[0032] The unit structure (B) may be of one or more types, preferably one or two types.

[0033] When the polymer contains the unit structure (B), the molar ratio of the unit structure (B) is preferably 10 to 90 mol %, more preferably 10 to 75 mol %, and even more preferably 10 to 50 mol %, based on all unit structures of the polymer, from the viewpoint of suitably obtaining the effects of the present invention.

[0034] When the polymer contains the unit structure (A) and the unit structure (B), the total molar ratio of the unit structures (A) and (B) is preferably 20 mol % or more, more preferably 40 mol % or more, and even more preferably 50 mol % or more, based on all the unit structures of the polymer, from the viewpoint of suitably obtaining the effects of the present invention.

[0035] <<Unit structure (C)>> The polymer of the present embodiment may optionally further contain a unit structure (C) having a crosslinking group in addition to the unit structure (A) and / or the unit structure (B). The crosslinking group can undergo a crosslinking reaction with a crosslinking agent component optionally introduced into the composition for forming a resist underlayer film of the present invention upon heating and baking. The resist underlayer film formed by such a crosslinking reaction has the effect of preventing intermixing with the resist film coated thereon.

[0036] The crosslinking group is not particularly limited as long as it is a group that forms a chemical bond between molecules, and may be, for example, a hydroxy group, an epoxy group, a protected hydroxy group, or a protected carboxyl group. There may be any number of crosslinking groups in one molecule.

[0037] Examples of the hydroxy group include hydroxy groups derived from hydroxyalkyl (meth)acrylates, vinyl alcohol, etc., and phenolic hydroxy groups derived from hydroxystyrene, etc. Examples of the alkyl group include the above-mentioned alkyl groups, such as methyl, ethyl, propyl, isopropyl, and butyl groups. In this specification, (meth)acrylate means both methacrylate and acrylate.

[0038] Examples of the epoxy group include epoxy groups derived from epoxy (meth)acrylate, glycidyl (meth)acrylate, and the like.

[0039] Examples of the protected hydroxyl group include a group in which the hydroxyl group of hydroxystyrene is protected with a tertiary butoxy group.Other examples include a hydroxyl group protected by reacting a phenolic hydroxyl group such as hydroxystyrene with a vinyl ether compound, and a hydroxyl group protected by reacting an alcoholic hydroxyl group such as hydroxyethyl methacrylate with a vinyl ether compound.Examples of the vinyl ether compound include aliphatic vinyl ether compounds having an alkyl chain with 1 to 10 carbon atoms and a vinyl ether group, such as methyl vinyl ether, ethyl vinyl ether, isopropyl vinyl ether, normal butyl vinyl ether, 2-ethylhexyl vinyl ether, tert-butyl vinyl ether, and cyclohexyl vinyl ether, and cyclic vinyl ether compounds such as 2,3-dihydrofuran, 4-methyl-2,3-dihydrofuran, and 2,3-dihydro-4H-pyran.

[0040] Examples of the protected carboxyl group include a carboxyl group protected by reacting a vinyl ether compound with a carboxyl group of (meth)acrylic acid or vinylbenzoic acid. Examples of the vinyl ether compound used here include the above-mentioned vinyl ether compounds.

[0041] Examples of the crosslinking group include an amino group, an isocyanate group, a protected amino group, and a protected isocyanate group. The amino group must have at least one active hydrogen, but an amino group in which one active hydrogen of the amino group is substituted with an alkyl group or the like can also be used. The alkyl group can be the above-mentioned alkyl group.

[0042] A protected amino group is one in which at least one hydrogen atom of an amino group is protected with an alkoxycarbonyl group such as a t-butoxycarbonyl group or a 9-fluorenylmethoxycarbonyl group.

[0043] The protected isocyanate group is obtained by reacting an isocyanate group with a protecting agent. The protecting agent is an active hydrogen-containing compound capable of reacting with isocyanate, such as alcohol, phenol, polycyclic phenol, amide, imide, imine, thiol, oxime, lactam, active hydrogen-containing heterocycle, and active methylene-containing compound.

[0044] Examples of the alcohol as the protecting agent include alcohols having 1 to 40 carbon atoms, such as methanol, ethanol, propanol, isopropanol, butanol, pentanol, hexanol, octanol, ethylene chlorohydrin, 1,3-dichloro-2-propanol, t-butanol, t-pentanol, 2-ethylhexanol, cyclohexanol, lauryl alcohol, ethylene glycol, butylene glycol, trimethylolpropane, glycerin, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and benzyl alcohol.

[0045] The phenol as the protecting agent may be, for example, a phenol having 6 to 20 carbon atoms, such as phenol, chlorophenol, and nitrophenol. Examples of the phenol derivative as the protecting agent include phenol derivatives having 6 to 20 carbon atoms, such as para-t-butylphenol, cresol, xylenol, and resorcinol. The polycyclic phenol as the protecting agent may be, for example, a polycyclic phenol having 10 to 20 carbon atoms, which is an aromatic condensed ring having a phenolic hydroxy group, and examples thereof include hydroxynaphthalene and hydroxyanthracene.

[0046] The amide as the protecting agent may be, for example, an amide having 1 to 20 carbon atoms, such as acetanilide, hexanamide, octanediamide, succinamide, benzenesulfonamide, or ethanediamide. The imide as the protecting agent may be, for example, an imide having 6 to 20 carbon atoms, such as cyclohexanedicarboximide, cyclohexaenedicarboximide, benzenedicarboximide, cyclobutanedicarboximide, carbodiimide, or the like. The imine as the protecting agent may be, for example, an imine having 1 to 20 carbon atoms, such as hexane-1-imine, 2-propaneimine, or ethane-1,2-imine.

[0047] The thiol as the protecting agent may be, for example, a thiol having 1 to 20 carbon atoms, such as ethanethiol, butanethiol, thiophenol, and 2,3-butanedithiol. The oxime as the protecting agent is, for example, an oxime having 1 to 20 carbon atoms, and examples thereof include acetoxime, methyl ethyl ketoxime, cyclohexanone oxime, dimethyl ketoxime, methyl isobutyl ketoxime, methyl amyl ketoxime, formamide oxime, acetaldoxime, diacetyl monoxime, benzophenone oxime, and cyclohexane oxime. The lactam as the protecting agent is, for example, a lactam having 4 to 20 carbon atoms, and examples thereof include ε-caprolactam, δ-valerolactam, γ-butyrolactam, β-propyllactam, γ-pyrrolidone, and lauryllactam.

[0048] The active hydrogen-containing heterocyclic compound as the protecting agent is, for example, an active hydrogen-containing heterocyclic compound having 3 to 30 carbon atoms, and examples thereof include pyrrole, imidazole, pyrazole, piperidine, piperazine, morpholine, pyridine, indole, indazole, purine, and carbazole. The active methylene-containing compound as the protecting agent is, for example, an active methylene-containing compound having 3 to 20 carbon atoms, and examples thereof include dimethyl malonate, diethyl malonate, methyl acetoacetate, ethyl acetoacetate, and acetylacetone.

[0049] The crosslinking group is not particularly limited, but a hydroxy group can be preferably used. As the unit structure (C) having such a crosslinking group, the unit structure derived from the above hydroxyalkyl (meth)acrylate is preferable, and in particular, the unit structure derived from hydroxyethyl (meth)acrylate is more preferable. The term "unit structure derived from a hydroxyalkyl (meth)acrylate" refers to a repeating unit in a polymer, which is obtained by reaction of the carbon-carbon double bond of a hydroxyalkyl (meth)acrylate.

[0050] When the polymer contains the unit structure (C), the molar ratio of the unit structure (C) is preferably 5 to 90 mol %, more preferably 10 to 80 mol %, and even more preferably 15 to 75 mol %, based on all unit structures of the polymer, from the viewpoint of suitably obtaining the effects of the present invention.

[0051] <<Polymer characteristics>> The distribution of the unit structures represented by unit structures (A), (B) and (C) in the polymer is not particularly limited. The polymer may be a homopolymer of unit structure (A) or a homopolymer of unit structure (B), but preferably has at least unit structure (A). When the polymer is a copolymer of unit structure (A) and unit structure (B), unit structure (A) and unit structure (B) may be alternately copolymerized or randomly copolymerized. In addition, when unit structure (C) coexists, the unit structures in the polymer may each constitute a block or may be randomly bonded.

[0052] The molecular weight of the polymer is not particularly limited, but the weight average molecular weight determined by gel permeation chromatography (hereinafter sometimes abbreviated as GPC) is preferably 1,500 to 100,000, and more preferably 2,000 to 50,000.

[0053] <<Polymer manufacturing method>> The method for producing the polymer is not particularly limited, but for example, the polymer of the present embodiment can be obtained by reacting a carbon-carbon double bond in a monomer of unit structure (A), a carbon-carbon double bond in a monomer of unit structure (B), and a carbon-carbon double bond in an arbitrary monomer of unit structure (C).

[0054] As a method for polymerizing the polymer, known polymerization methods such as radical polymerization, anionic polymerization, cationic polymerization, etc. Various known techniques such as solution polymerization, suspension polymerization, emulsion polymerization, bulk polymerization, etc. can be used.

[0055] The polymerization initiator used in the polymerization is not particularly limited, and examples thereof include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2 ,2'-Azobis(isobutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 1-[(1-cyano-1-methylethyl)azo]formamide, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], and 2,2'-azobis(2-methylpropionamidine)dihydrochloride, etc. are used.

[0056] The solvent used during polymerization is not particularly limited, but examples thereof include dioxane, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, etc. These may be used alone or in combination.

[0057] The reaction temperature is not particularly limited, but may be, for example, 20°C to 160°C. The reaction time is not particularly limited, but may be, for example, 1 hour to 72 hours.

[0058] The obtained solution containing the polymer can be used as it is for preparing a composition for forming a resist underlayer film, or the polymer can be recovered by precipitation and isolation in a poor solvent such as methanol, ethanol, isopropanol, water, or a mixed solvent thereof and then used.

[0059] The content of the polymer in the composition for forming a resist underlayer film is not particularly limited, but from the viewpoint of solubility, it is preferably 0.1% by mass to 50% by mass, and more preferably 0.1% by mass to 10% by mass, based on the entire composition for forming a resist underlayer film.

[0060] <Crosslinking agent> The crosslinking agent contained as an optional component in the composition for forming a resist underlayer film may be a nitrogen-containing compound having 2 to 6 substituents bonded to nitrogen atoms and represented by the following formula (1d) in one molecule, as described in WO 2017 / 187969.

[0061] [ka] (In formula (1d), R1 represents a methyl group or an ethyl group. * represents a bond bonded to the nitrogen atom.)

[0062] The nitrogen-containing compound having 2 to 6 substituents represented by the above formula (1d) in one molecule may be a glycoluril derivative represented by the following formula (1E).

[0063] [ka] (In formula (1E), the four R1s each independently represent a methyl group or an ethyl group, and R2 and R3 each independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group.)

[0064] Examples of the glycoluril derivative represented by the above formula (1E) include compounds represented by the following formulae (1E-1) to (1E-6).

[0065] [ka]

[0066] The nitrogen-containing compound having 2 to 6 substituents represented by the above formula (1d) in one molecule can be obtained by reacting a nitrogen-containing compound having 2 to 6 substituents bonded to a nitrogen atom in one molecule represented by the following formula (2d) with at least one compound represented by the following formula (3d).

[0067] [ka] (In formula (2d) and formula (3d), R1 represents a methyl group or an ethyl group, and R4 represents an alkyl group having 1 to 4 carbon atoms. * represents a bond bonded to a nitrogen atom.)

[0068] The glycoluril derivative represented by the above formula (1E) can be obtained by reacting a glycoluril derivative represented by the following formula (2E) with at least one compound represented by the above formula (3d).

[0069] The nitrogen-containing compound having 2 to 6 substituents represented by the above formula (2d) in one molecule is, for example, a glycoluril derivative represented by the following formula (2E).

[0070] [ka] (In formula (2E), R2 and R3 each independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group, and R4 each independently represent an alkyl group having 1 to 4 carbon atoms.)

[0071] Examples of the glycoluril derivative represented by the above formula (2E) include the compounds represented by the following formulae (2E-1) to (2E-4). Furthermore, examples of the compound represented by the above formula (3d) include the compounds represented by the following formulae (3d-1) and (3d-2).

[0072] [ka] [ka]

[0073] The entire disclosure of WO2017 / 187969 is incorporated herein by reference with respect to the content of the nitrogen-containing compound having 2 to 6 substituents represented by formula (1d) bonded to the nitrogen atom in one molecule.

[0074] The crosslinking agent may also be a compound represented by the following formula (21): [ka] (In formula (21), R 1 each independently represents an alkylene group having 1 to 6 carbon atoms; R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxyalkyl group having a total of 2 to 10 carbon atoms; R 3 Each independently represents an alkyl group having 1 to 6 carbon atoms. Each of m1 and m2 independently represents an integer of 1 to 2. When m1 and m2 are 1, Q 1 represents a single bond, an oxygen atom, or a divalent organic group having 1 to 20 carbon atoms, and in other cases, Q 1 represents an organic group having 1 to 20 carbon atoms and a valence of (m1+m2).

[0075] Q 1 In the above formula, examples of the organic group having 1 to 20 carbon atoms and a valence of (m1+m2) include groups represented by any of the following formulas (21-1) to (21-5).

[0076] [ka] (In formula (21-1), Ra and Rb each independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a -CF3 group. In formula (21-3), X represents a trivalent group having 1 to 30 carbon atoms. In formula (21-4), Ar represents a divalent aromatic hydrocarbon group. * represents a bond.)

[0077] Ar represents, for example, a divalent residue of a compound selected from benzene, biphenyl, naphthalene, and anthracene.

[0078] The group represented by formula (21-1) is a divalent group. The group represented by formula (21-2) is a tetravalent group. The group represented by formula (21-3) is a trivalent group. The group represented by formula (21-4) is a divalent group. The group represented by formula (21-5) is a trivalent group.

[0079] When the above-mentioned crosslinking agent is used, the content of the crosslinking agent is, for example, 1% by mass to 50% by mass, and preferably 5% by mass to 30% by mass, based on the polymer having at least one of the unit structures (A) and (B).

[0080] <<Curing catalyst>> The curing catalyst contained as an optional component in the composition for forming a resist underlayer film may be either a thermal acid generator or a photoacid generator, but it is preferable to use a thermal acid generator.

[0081] Examples of the thermal acid generator include sulfonic acid compounds and carboxylic acid compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate (pyridinium p-toluenesulfonic acid), pyridinium phenolsulfonic acid, pyridinium p-hydroxybenzenesulfonic acid (pyridinium p-phenolsulfonate salt), pyridinium trifluoromethanesulfonic acid, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-hydroxybenzenesulfonic acid, benzenedisulfonic acid, 1-naphthalenesulfonic acid, citric acid, benzoic acid, and hydroxybenzoic acid.

[0082] Examples of the photoacid generator include an onium salt compound, a sulfonimide compound, and a disulfonyldiazomethane compound.

[0083] Examples of the onium salt compound include iodonium salt compounds such as diphenyliodonium hexafluorophosphate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium nonafluoronormal butanesulfonate, diphenyliodonium perfluoronormal octanesulfonate, diphenyliodonium camphorsulfonate, bis(4-tert-butylphenyl)iodonium camphorsulfonate, and bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate; and sulfonium salt compounds such as triphenylsulfonium hexafluoroantimonate, triphenylsulfonium nonafluoronormal butanesulfonate, triphenylsulfonium camphorsulfonate, and triphenylsulfonium trifluoromethanesulfonate.

[0084] Examples of the sulfonimide compound include N-(trifluoromethanesulfonyloxy)succinimide, N-(nonafluoronormalbutanesulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, and N-(trifluoromethanesulfonyloxy)naphthalimide.

[0085] Examples of the disulfonyldiazomethane compound include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane, bis(2,4-dimethylbenzenesulfonyl)diazomethane, and methylsulfonyl-p-toluenesulfonyldiazomethane.

[0086] The curing catalyst may be used alone or in combination of two or more.

[0087] When a curing catalyst is used, the content of the curing catalyst is, for example, 0.1% by mass to 50% by mass, and preferably 1% by mass to 30% by mass, relative to the crosslinking agent.

[0088] <<Other ingredients>> A surfactant may be further added to the composition for forming a resist underlayer film in order to prevent pinholes, striations, and the like, and to further improve the coatability against surface unevenness.

[0089] Examples of the surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkyl allyl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether; polyoxyethylene-polyoxypropylene block copolymers; sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate; polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters, such as polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate; fluorosurfactants such as F-TOP EF301, EF303, and EF352 (trade names, manufactured by Tochem Products Co., Ltd.), Megafac F171, F173, and R-30 (trade names, manufactured by DIC Corporation), Fluorad FC430 and FC431 (trade names, manufactured by Sumitomo 3M Limited), Asahiguard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (trade names, manufactured by Asahi Glass Co., Ltd.); and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). The amount of these surfactants to be added is not particularly limited, but is usually 2.0% by mass or less, and preferably 1.0% by mass or less, based on the composition for forming a resist underlayer film. These surfactants may be added alone or in combination of two or more kinds.

[0090] <Solvent> The solvent is preferably an organic solvent generally used in chemicals for semiconductor lithography processes, specifically, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, cyclohexane ... Examples of the solvent include heptanone, 4-methyl-2-pentanol, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, ethyl ethoxyacetate, 2-hydroxyethyl acetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, methoxycyclopentane, anisole, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. These solvents can be used alone or in combination of two or more.

[0091] Among these solvents, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, butyl lactate, and cyclohexanone are preferred, and propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate are particularly preferred.

[0092] The composition for forming a resist underlayer film is preferably used as a composition for forming a resist underlayer film for EB or EUV lithography. The composition for forming a resist underlayer film for EB or EUV lithography is preferably used to form a resist underlayer film for EB or EUV lithography having a film thickness of less than 10 nm.

[0093] (Resist underlayer film) The resist underlayer film of the present invention is a fired product of a coating film of the above-mentioned composition for forming a resist underlayer film.

[0094] The thickness of the resist underlayer film of the present invention is less than 10 nm. Usually, when the thickness of the resist underlayer film is thin, it is difficult to obtain a film with a flat surface. If the surface is not flat, the thickness variation of the resist layer formed on the underlayer film becomes large, resulting in a large LWR. The resist underlayer film of the present invention contains the above-mentioned polymer, and thus tends to have excellent adhesion to the substrate and excellent film forming properties. Therefore, even if the resist underlayer film has a thickness of less than 10 nm, it is presumed that the film can have a flat surface and can improve the LWR of the resist pattern. This effect is particularly remarkable when EUV or EB is used.

[0095] In addition, when using EUV or EB and using a resist underlayer film with a thickness of 20 nm or more, in the dry etching process after resist pattern formation, the resist film is thin, so that the resist pattern is damaged in the process of etching the underlayer film, causing shape defects such as a reduction in resist film thickness and a top-rounding shape, making it difficult to form a pattern with the desired line width during actual substrate processing.

[0096] The resist underlayer film of the present invention can be produced by applying a composition for forming a resist underlayer film onto a semiconductor substrate and baking the composition.

[0097] Examples of semiconductor substrates to which the composition for forming a resist underlayer film of the present invention can be applied include silicon wafers, germanium wafers, and wafers of compound semiconductors such as gallium arsenide, indium phosphide, gallium nitride, indium nitride, and aluminum nitride.

[0098] When using a semiconductor substrate having an inorganic film formed on its surface, the inorganic film is formed by, for example, ALD (atomic layer deposition), CVD (chemical vapor deposition), reactive sputtering, ion plating, vacuum deposition, or spin-coating (spin-on glass: SOG). Examples of the inorganic film include polysilicon film, silicon oxide film, silicon nitride film, BPSG (Boro-Phospho Silicate Glass) film, titanium nitride film, titanium nitride oxide film, tungsten film, gallium nitride film, and gallium arsenide film.

[0099] The composition for forming a resist underlayer film of the present invention is applied onto such a semiconductor substrate by a suitable application method such as a spinner or coater. Then, the composition is baked using a heating means such as a hot plate to form a resist underlayer film. The baking conditions are appropriately selected from a baking temperature of 100°C to 400°C and a baking time of 0.3 minutes to 60 minutes. Preferably, the baking temperature is 120°C to 350°C, the baking time is 0.5 minutes to 30 minutes, and more preferably, the baking temperature is 150°C to 300°C, and the baking time is 0.8 minutes to 10 minutes.

[0100] The thickness of the resist underlayer film is less than 10 nm, preferably 9 nm or less, more preferably 8 nm or less, and even more preferably 7 nm or less. The thickness of the resist underlayer film may be 1 nm or more, 2 nm or more, or 3 nm or more.

[0101] In this specification, the method for measuring the film thickness of the resist underlayer film is as follows. Measurement device name: Ellipsometric film thickness measurement device RE-3100 (SCREEN Co., Ltd.) ·SWE (Single Wavelength Ellipsometer) mode - Arithmetic average of 8 points (for example, 8 points are measured at 1 cm intervals in the X direction of the wafer)

[0102] The resist underlayer film is preferably used as a resist underlayer film for EB or EUV lithography.

[0103] (Substrates for semiconductor processing) The substrate for semiconductor processing of the present invention comprises a semiconductor substrate and the resist underlayer film or the resist underlayer film for EB or EUV lithography of the present invention. The semiconductor substrate may be, for example, the semiconductor substrate described above. The resist underlayer film or the resist underlayer film for EB or EUV lithography is disposed, for example, over a semiconductor substrate.

[0104] (Semiconductor device manufacturing method, pattern formation method, and method for improving LWR of resist pattern) The method for manufacturing a semiconductor device of the present invention includes at least the following steps. forming a resist underlayer film having a thickness of less than 10 nm on a semiconductor substrate using the composition for forming a resist underlayer film for EB or EUV lithography of the present invention; and A process of forming a resist film on the resist underlayer film using a resist for EB or EUV lithography.

[0105] The pattern forming method of the present invention includes at least the following steps. forming a resist underlayer film having a thickness of less than 10 nm on a semiconductor substrate using the composition for forming a resist underlayer film for EB or EUV lithography of the present invention; A process of forming a resist film on the resist underlayer film using a resist for EB or EUV lithography. A step of irradiating the resist film with EB or EUV and then developing the resist film to obtain a resist pattern; and A process of etching the resist underlayer film using the resist pattern as a mask.

[0106] The method for improving LWR of a resist pattern of the present invention includes at least the following steps. forming a resist underlayer film having a thickness of less than 10 nm on a semiconductor substrate using the composition for forming a resist underlayer film for EB or EUV lithography of the present invention; forming a resist film on the resist underlayer film using a resist for EB or EUV lithography; and A step of irradiating the resist film with EB or EUV and then developing the resist film to obtain a resist pattern; In the method for improving the LWR of a resist pattern, the resist underlayer film obtained from the composition for forming a resist underlayer film for EB or EUV lithography of the present invention is used under a resist film, thereby making it possible to improve the non-uniformity of the resist pattern width (LWR: Line width roughness) in EB or EUV lithography.

[0107] Usually, a resist film is formed on the resist underlayer film. The thickness of the resist film is not particularly limited, but is preferably 200 nm or less, more preferably 150 nm or less, even more preferably 100 nm or less, and particularly preferably 80 nm or less. The thickness of the resist film is preferably 10 nm or more, more preferably 20 nm or more, and even more preferably 30 nm or more.

[0108] The resist formed by coating and baking on the resist underlayer film by a known method is not particularly limited as long as it responds to the EB or EUV used for irradiation. Either a negative photoresist or a positive photoresist can be used. In this specification, resists that respond to EB are also referred to as photoresists. Examples of photoresists include positive photoresists made of novolac resin and 1,2-naphthoquinone diazide sulfonic acid ester, chemically amplified photoresists made of a binder having a group that decomposes with acid to increase the alkaline dissolution rate and a photoacid generator, chemically amplified photoresists made of a low molecular compound that decomposes with acid to increase the alkaline dissolution rate of the photoresist, an alkali-soluble binder, and a photoacid generator, chemically amplified photoresists made of a binder having a group that decomposes with acid to increase the alkaline dissolution rate of the photoresist, a low molecular compound that decomposes with acid to increase the alkaline dissolution rate of the photoresist, and a photoacid generator, resists containing metal elements, etc. Examples of such resists include V146G (trade name) manufactured by JSR Corporation, APEX-E (trade name) manufactured by Shipley, PAR710 (trade name) manufactured by Sumitomo Chemical Co., Ltd., and AR2772 and SEPR430 (trade names) manufactured by Shin-Etsu Chemical Co., Ltd. Further, there can be mentioned fluorine-containing polymer photoresists as described in, for example, Proc. SPIE, Vol. 3999, 330-334 (2000), Proc. SPIE, Vol. 3999, 357-364 (2000), and Proc. SPIE, Vol. 3999, 365-374 (2000).

[0109] In addition, WO2019 / 188595, WO2019 / 187881, WO2019 / 187803, WO2019 / 167737, WO2019 / 167725, WO2019 / 187445, WO2019 / 167419, WO2019 / 123842, WO2019 / 054282, WO2019 / 058945, WO2019 / 058890, WO2019 / 039290, WO2019 / 044259, WO2019 / 044231, WO2019 / 026549, WO2018 / 193954, WO201 9 / 172054, WO2019 / 021975, WO2018 / 230334, WO2018 / 194123, JP 2018-180525, WO2018 / 190088, JP 2018-070596, JP 2018-028090, JP 2016-153409, JP 2016-130240, JP 2016-108325, JP 2016-047920, JP 2016-035570, JP 2016-035567, JP 2016-035565, JP 2019-101417, JP 2019-117373, JP 2019-052294, JP 2019-008280, JP 2019-008279, JP 2019-003176, JP 2019-003175, JP 2018-197853, JP 2019-191298, JP 2019-061217, JP 2018-045152, JP 2018-022039, JP 2016-090441, JP 2015-10878, JP 2012-168279, JP 2012-022261, JP 2012-022258, JP 2011-043749, JP 2010-18 1857, JP 2010-128369, WO2018 / 031896, JP 2019-113855, WO2017 / 156388, WO2017 / 066319, JP 2018-41099, WO2016 / 065120, WO2015 / 026482, JP 2016-29498, JP 2011-253185, etc., resist compositions, radiation-sensitive resin compositions, high-resolution patterning compositions based on organometallic solutions, and metal-containing resist compositions can be used, but are not limited to these.

[0110] Examples of the resist composition include the following compositions.

[0111] An actinic ray-sensitive or radiation-sensitive resin composition comprising: resin A having a repeating unit having an acid-decomposable group in which a polar group is protected with a protecting group that is eliminated by the action of an acid; and a compound represented by the following general formula (21):

[0112] [ka] In the general formula (21), m represents an integer of 1 to 6. R1 and R2 each independently represent a fluorine atom or a perfluoroalkyl group. L1 represents -O-, -S-, -COO-, -SO2- or -SO3-. L2 represents an alkylene group which may have a substituent or a single bond. W1 represents a cyclic organic group which may have a substituent. M + represents a cation.

[0113] A metal-containing film-forming composition for extreme ultraviolet or electron beam lithography, comprising a compound having a metal-oxygen covalent bond and a solvent, the metal element constituting the compound belonging to Period 3 to Period 7 of Groups 3 to 15 of the periodic table.

[0114] A radiation-sensitive resin composition comprising: a polymer having a first structural unit represented by the following formula (31) and a second structural unit represented by the following formula (32) containing an acid-dissociable group; and an acid generator.

[0115] [ka] In formula (31), Ar is a group in which (n+1) hydrogen atoms have been removed from an arene having 6 to 20 carbon atoms. 1 is a hydroxy group, a sulfanyl group, or a monovalent organic group having 1 to 20 carbon atoms. n is an integer of 0 to 11. When n is 2 or more, multiple R 1 are the same or different. R 2is a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group. 3 R is a monovalent group having 1 to 20 carbon atoms containing the above acid dissociable group. Z is a single bond, an oxygen atom, or a sulfur atom. 4 is a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group.

[0116] A resist composition comprising: a resin (A1) that includes a structural unit having a cyclic carbonate structure, a structural unit represented by the following formula, and a structural unit having an acid labile group; and an acid generator.

[0117] [ka] [In the formula, R 2 represents an alkyl group having 1 to 6 carbon atoms which may have a halogen atom, a hydrogen atom or a halogen atom; X 1 is a single bond, -CO-O-* or -CO-NR 4 -*, * represents a bond to -Ar, R 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and Ar represents an aromatic hydrocarbon group having 6 to 20 carbon atoms which may have one or more groups selected from the group consisting of a hydroxyl group and a carboxyl group.]

[0118] Examples of the resist film include the following.

[0119] A resist film comprising a base resin containing a repeating unit represented by the following formula (a1) and / or a repeating unit represented by the following formula (a2), and a repeating unit that generates an acid bonded to a polymer main chain upon exposure:

[0120] [ka] (In formula (a1) and formula (a2), R A R is each independently a hydrogen atom or a methyl group. 1 and R 2R are each independently a tertiary alkyl group having 4 to 6 carbon atoms. 3 are each independently a fluorine atom or a methyl group, and m is an integer of 0 to 4. 1 X is a single bond, a phenylene group, a naphthylene group, or an ester bond, a lactone ring, a phenylene group, or a naphthylene group, and is a linking group having 1 to 12 carbon atoms and containing at least one type selected from the group consisting of a phenylene group and a naphthylene group. 2 is a single bond, an ester bond, or an amide bond.

[0121] Examples of resist materials include the following:

[0122] A resist material comprising a polymer having a repeating unit represented by the following formula (b1) or formula (b2):

[0123] [ka] (In formula (b1) and formula (b2), R A is a hydrogen atom or a methyl group. 1 is a single bond or an ester group. 2 is a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms or an arylene group having 6 to 10 carbon atoms, a part of the methylene groups constituting the alkylene group may be substituted with an ether group, an ester group or a lactone ring-containing group, and X 2 At least one hydrogen atom in X is replaced with a bromine atom. 3 Rf is a single bond, an ether group, an ester group, or a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms, and a part of the methylene groups constituting the alkylene group may be substituted with an ether group or an ester group. 1 ~Rf 4 are each independently a hydrogen atom, a fluorine atom, or a trifluoromethyl group, but at least one is a fluorine atom or a trifluoromethyl group. 1 and Rf 2 may combine to form a carbonyl group. 1 ~R 5are each independently a linear, branched or cyclic alkyl group having 1 to 12 carbon atoms, a linear, branched or cyclic alkenyl group having 2 to 12 carbon atoms, an alkynyl group having 2 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or an aryloxyalkyl group having 7 to 12 carbon atoms, some or all of the hydrogen atoms in these groups may be substituted with a hydroxy group, a carboxy group, a halogen atom, an oxo group, a cyano group, an amide group, a nitro group, a sultone group, a sulfone group or a sulfonium salt-containing group, and some of the methylene groups constituting these groups may be substituted with an ether group, an ester group, a carbonyl group, a carbonate group or a sulfonate ester group. 1 and R 2 may combine to form a ring together with the sulfur atom to which they are attached.

[0124] A resist material comprising a base resin that includes a polymer containing a repeating unit represented by the following formula (a):

[0125] [ka] (In formula (a), R A R is a hydrogen atom or a methyl group. 1 R is a hydrogen atom or an acid labile group. 2 is a linear, branched or cyclic alkyl group having 1 to 6 carbon atoms, or a halogen atom other than bromine. 1 X is a single bond, a phenylene group, or a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms which may contain an ester group or a lactone ring. 2 is -O-, -O-CH2- or -NH-. m is an integer of 1 to 4. u is an integer of 0 to 3, with the proviso that m+u is an integer of 1 to 4.

[0126] A resist composition which generates an acid upon exposure and changes its solubility in a developer by the action of the acid, The composition contains a base component (A) whose solubility in a developer changes under the action of an acid, and a fluorine additive component (F) that is decomposable in an alkaline developer, The fluorine additive component (F) is a resist composition containing a fluorine resin component (F1) having a structural unit (f1) containing a base dissociable group and a structural unit (f2) containing a group represented by the following general formula (f2-r-1):

[0127] [ka] [In formula (f2-r-1), Rf 21 are each independently a hydrogen atom, an alkyl group, an alkoxy group, a hydroxyl group, a hydroxyalkyl group, or a cyano group. n" is an integer of 0 to 2. * is a bond.

[0128] The above structural unit (f1) includes a structural unit represented by the following general formula (f1-1) or a structural unit represented by the following general formula (f1-2).

[0129] [ka] In formulae (f1-1) and (f1-2), R is each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. X is a divalent linking group having no acid dissociable site. aryl X is a divalent aromatic cyclic group which may have a substituent. 01 R is a single bond or a divalent linking group. 2 each independently represents an organic group having a fluorine atom.

[0130] Coatings, coating solutions, and coating compositions include, for example:

[0131] A coating comprising a metal oxo-hydroxo network having organic ligands via metal carbon bonds and / or metal carboxylate bonds.

[0132] Inorganic oxo / hydroxy-based composition.

[0133] A coating solution comprising an organic solvent; a first organometallic composition represented by the formula R z SnO (2-(z / 2)-(x / 2)) (OH) x (where 0 < z ≦ 2 and 0 < (z + x) ≦ 4), the formula R’ n SnX 4-n (where n = 1 or 2), or a mixture thereof, where R and R’ are independently hydrocarbyl groups having 1 to 31 carbon atoms, and X is a ligand having a hydrolyzable bond to Sn or a combination thereof; and a hydrolyzable metal compound represented by the formula MX’ v (where M is a metal selected from Groups 2 to 16 of the Periodic Table of the Elements, v is a number from 2 to 6, and X’ is a ligand having a hydrolyzable M-X bond or a combination thereof), a coating solution containing a hydrolyzable metal compound.

[0134] A coating solution comprising an organic solvent and a first organometallic compound represented by the formula RSnO (3 / 2-x / 2) (OH) x (where 0 < x < 3), wherein the solution contains about 0.0025M to about 1.5M of tin, and R is an alkyl group or cycloalkyl group having 3 to 31 carbon atoms, and the alkyl group or cycloalkyl group is bonded to tin at a secondary or tertiary carbon atom.

[0135] An inorganic pattern-forming precursor aqueous solution comprising a mixture of water, metal oxide cations, polyatomic inorganic anions, and a radiation-sensitive ligand containing peroxide groups.

[0136] Irradiation with EB or EUV is performed, for example, through a mask (reticle) for forming a predetermined pattern. The resist underlayer film of the present invention is applied for EB (electron beam) or EUV (extreme ultraviolet: 13.5 nm) irradiation, and is preferably applied for EUV (extreme ultraviolet) exposure. The EB irradiation energy and the EUV exposure dose are not particularly limited.

[0137] After the irradiation with EB or EUV and before the development, baking (PEB: Post Exposure Bake) may be performed. The baking temperature is not particularly limited, but is preferably from 60°C to 150°C, more preferably from 70°C to 120°C, and particularly preferably from 75°C to 110°C. The baking time is not particularly limited, but is preferably from 1 second to 10 minutes, more preferably from 10 seconds to 5 minutes, and particularly preferably from 30 seconds to 3 minutes.

[0138] For development, for example, an alkaline developer is used. The development temperature is, for example, 5°C to 50°C. The development time is, for example, from 10 seconds to 300 seconds. As the alkaline developer, for example, aqueous solutions of alkalis such as inorganic alkalis such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, and ammonia water, primary amines such as ethylamine and n-propylamine, secondary amines such as diethylamine and di-n-butylamine, tertiary amines such as triethylamine and methyldiethylamine, alcohol amines such as dimethylethanolamine and triethanolamine, quaternary ammonium salts such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline, and cyclic amines such as pyrrole and piperidine can be used. Furthermore, an appropriate amount of alcohols such as isopropyl alcohol and a nonionic surfactant can be added to the aqueous solution of the above-mentioned alkalis. Among these, preferred developers are aqueous solutions of quaternary ammonium salts, more preferably aqueous solutions of tetramethylammonium hydroxide and aqueous solutions of choline. Furthermore, surfactants can be added to these developers. Instead of the alkaline developer, a method can be used in which development is performed with an organic solvent such as butyl acetate to develop the parts of the photoresist where the alkaline dissolution rate is not improved.

[0139] Next, the resist underlayer film is etched using the formed resist pattern as a mask. The etching may be dry etching or wet etching, but is preferably dry etching. When the inorganic film is formed on the surface of the semiconductor substrate used, the surface of the inorganic film is exposed, and when the inorganic film is not formed on the surface of the semiconductor substrate used, the surface of the semiconductor substrate is exposed. The semiconductor substrate is then processed by a known method (such as dry etching) to manufacture a semiconductor device. EXAMPLES

[0140] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these.

[0141] The weight average molecular weights of the polymers shown in the following Synthesis Examples 1 to 8 and Comparative Synthesis Example 1 in this specification are the results of measurement by gel permeation chromatography (hereinafter abbreviated as GPC). For the measurement, a GPC device manufactured by Tosoh Corporation was used, and the measurement conditions etc. are as follows. GPC column: TSKgel Super-MultiporeHZ-N (2 columns) Column temperature: 40℃ Solvent: Tetrahydrofuran (THF) Flow rate: 0.35ml / min Standard sample: Polystyrene (manufactured by Tosoh Corporation)

[0142] <Synthesis Example 1> 5.68 g of 2-vinylnaphthalene (75% molar ratio to the entire polymer 1), 1.60 g of 2-hydroxyethyl methacrylate (25% molar ratio to the entire polymer 1), and 0.73 g of 2,2'-azobisisobutyronitrile were dissolved in 32.00 g of propylene glycol monomethyl ether acetate. After replacing the atmosphere in the reaction vessel with nitrogen, the solution was heated and stirred at 140°C for about 4 hours. The reaction solution was dropped into isopropyl alcohol, and the precipitate was collected by suction filtration, and then dried under reduced pressure at 60°C to collect polymer 1. The weight average molecular weight Mw measured in terms of polystyrene by GPC was 8500. The structure present in polymer 1 is shown in the following formula.

[0143] [ka]

[0144] <Synthesis Example 2> 4.75 g of 2-vinylnaphthalene (55% by mole relative to the entire polymer 2), 2.96 g of benzyl methacrylate (30% by mole relative to the entire polymer 2), 1.21 g of 2-hydroxypropyl methacrylate (15% by mole relative to the entire polymer 2), and 1.07 g of 2,2'-azobisisobutyronitrile were dissolved in 40.00 g of propylene glycol monomethyl ether acetate. After replacing the reaction vessel with nitrogen, the solution was heated and stirred at 140°C for about 4 hours. The reaction solution was dropped into isopropyl alcohol, and the precipitate was collected by suction filtration, and then dried under reduced pressure at 60°C to collect polymer 2. The weight average molecular weight Mw measured in terms of polystyrene by GPC was 5900. The structure present in polymer 2 is shown in the following formula.

[0145] [ka]

[0146] <Synthesis Example 3> 10.00 g of 2-vinylnaphthalene (molar ratio 40% relative to the entire polymer 3) and 23.00 g of 3-hydroxy-2-adamantyl methacrylate (molar ratio 60% relative to the entire polymer 3) were dissolved in 97 g of cyclohexanone in a flask, and the flask was replaced with nitrogen and heated to 60°C. After heating, a solution in which 1.60 g of 2,2'-azobisisobutyronitrile was dissolved in 41.00 g of cyclohexanone was dropped and stirred for about 24 hours. This reaction solution was dropped into methanol, and the precipitate was collected by suction filtration, and then dried under reduced pressure at 60°C to collect polymer 3. The weight average molecular weight Mw measured in terms of polystyrene by GPC was 16,000. The structure present in polymer 3 is shown in the following formula.

[0147] [ka]

[0148] <Synthesis Example 4> 10.00g of 2-vinylnaphthalene (molar ratio 40% relative to the entire polymer 4), 17.90g of 9-anthracenemethyl methacrylate (molar ratio 40% relative to the entire polymer 4), and 4.67g of 2-hydroxyethyl methacrylate (molar ratio 20% relative to the entire polymer 4) were dissolved in 95g of cyclohexanone in a flask, and the flask was replaced with nitrogen and heated to 60°C. After heating, a solution in which 1.60g of 2,2'-azobisisobutyronitrile was dissolved in 41.00g of cyclohexanone was dropped and stirred for about 24 hours. This reaction solution was dropped into methanol, and the precipitate was collected by suction filtration, and then dried under reduced pressure at 60°C to collect polymer 4. The weight average molecular weight Mw measured in terms of polystyrene by GPC was 8000. The structure present in polymer 4 is shown in the following formula.

[0149] [ka]

[0150] <Synthesis Example 5> 2.94 g of 2-vinylnaphthalene (50% by mole relative to the entire polymer 5), 1.24 g of hydroxyethyl methacrylate (25% by mole relative to the entire polymer 5), 1.71 g of N-cyclohexylmaleimide (25% by mole relative to the entire polymer 5), and 0.12 g of 2,2'-azobisisobutyronitrile were dissolved in 24.00 g of propylene glycol monomethyl ether acetate. After replacing the reaction vessel with nitrogen, the solution was heated and stirred at 140°C for about 4 hours. The reaction solution was dropped into isopropyl alcohol, and the precipitate was collected by suction filtration, and then dried under reduced pressure at 60°C to collect polymer 5. The weight average molecular weight Mw measured by GPC in terms of polystyrene was 16300. The structure present in polymer 5 is shown in the following formula.

[0151] [ka]

[0152] <Synthesis Example 6> 2.86 g of 2-vinylnaphthalene (50% by mole relative to the entire polymer 6), 1.68 g of N-cyclohexylmaleimide (25% by mole relative to the entire polymer 6), 1.32 g of N-hydroxyethylmaleimide (25% by mole relative to the entire polymer 6), and 0.12 g of 2,2'-azobisisobutyronitrile were dissolved in 24.00 g of propylene glycol monomethyl ether acetate. After replacing the atmosphere in the reaction vessel with nitrogen, the solution was heated and stirred at 140°C for about 4 hours. The reaction solution was dropped into isopropyl alcohol, and the precipitate was collected by suction filtration, and then dried under reduced pressure at 60°C to collect polymer 6. The weight average molecular weight Mw measured in terms of polystyrene by GPC was 11900. The structure present in polymer 6 is shown in the following formula.

[0153] [ka]

[0154] <Synthesis Example 7> 167.27 g of propylene glycol monomethyl ether acetate was added to a flask with 50.00 g of N-phenyl-1-naphthylamine (67% molar ratio relative to the total of polymer 7), 20.43 g of N-cyclohexylmaleimide (33% molar ratio relative to the total of polymer 7), 21.91 g of methanesulfonic acid, and 1.26 g of hydroquinone, and the mixture was stirred at 140° C. for 24 hours. This reaction solution was dropped into methanol, and the precipitate was collected by suction filtration, and then dried under reduced pressure at 60° C. to collect polymer 7. The weight average molecular weight Mw measured in terms of polystyrene by GPC was 2000. The structure present in polymer 7 is shown in the following formula.

[0155] [ka]

[0156] <Synthesis Example 8> 15.00g of carbazole (67% molar ratio to the total of polymer 8), 8.04g of N-cyclohexylmaleimide (33% molar ratio to the total of polymer 8), 8.62g of methanesulfonic acid, and 0.49g of hydroquinone were added to 54.91g of propylene glycol monomethyl ether in a flask, and the mixture was stirred at 140°C for 23 hours. This reaction solution was dropped into methanol, and the precipitate was collected by suction filtration, and then dried under reduced pressure at 60°C to collect polymer 8. The weight average molecular weight Mw measured by GPC in terms of polystyrene was 6000. The structure present in polymer 8 is shown in the following formula.

[0157] [ka]

[0158] <Comparative Synthesis Example 1> 100.00 g of monoallyl diglycidyl isocyanuric acid (manufactured by Shikoku Chemical Industry Co., Ltd.), 66.4 g of 5,5-diethylbarbituric acid (manufactured by Tateyama Chemical Industry Co., Ltd.), and 4.1 g of benzyl triethylammonium chloride were added to 682.00 g of propylene glycol monomethyl ether in a reaction vessel and dissolved. After replacing the atmosphere in the reaction vessel with nitrogen, the reaction was carried out at 130°C for 24 hours to obtain a solution containing comparative polymer 1. When GPC analysis was performed, the comparative polymer 1 obtained had a weight average molecular weight of 6,800 and a dispersity of 4.8 in terms of standard polystyrene. The structure present in comparative polymer 1 is shown in the following formula.

[0159] [ka]

[0160] (Preparation of composition for forming resist underlayer film) The components were mixed in the ratios shown in Table 1, and filtered using a polyethylene microfilter having a pore size of 0.05 μm to prepare compositions for forming resist underlayer films of Preparation Examples 1 to 8 and a composition for forming resist underlayer films of Comparative Preparation Example 1.

[0161] The abbreviations in Table 1 are as follows. PyPSA: Pyridinium-p-hydroxybenzenesulfonic acid PGMEA: Propylene glycol monomethyl ether acetate PGME: Propylene glycol monomethyl ether

[0162] PGME-PL:Imidazo[4,5-d]imidazole-2,5(1H,3H)-dione,tetrahydro-1,3,4,6-tetrakis[(2-methoxy-1-methylethoxy)methyl]-(Structural formula below) [ka]

[0163] TMOM-BP: 3,3',5,5'-tetrakis(methoxymethyl)-[1,1'-biphenyl]-4,4'-diol (trade name: TMOM-BP, manufactured by Honshu Chemical Industry Co., Ltd., sub-structural formula) [ka]

[0164] [Table 1]

[0165] (Preparation of resist underlayer film) <Examples 1 to 8 and Comparative Example 1> Each of the resist underlayer film-forming compositions of Preparation Examples 1 to 8 and Comparative Preparation Example 1 was applied onto a silicon wafer using a spinner. The silicon wafer was baked on a hot plate at 205 to 250° C. for 60 seconds to obtain resist underlayer films of Examples 1 to 8 and Comparative Example 1 with a film thickness of 5 nm. The film thickness was measured using an ellipsometric film thickness measurement device RE-3100 (SCREEN Co., Ltd.). The resist underlayer film of Example 1 was obtained using the composition for forming the resist underlayer film of Preparation Example 1. The composition for forming a resist underlayer film of Preparation Example 2 was used to obtain a resist underlayer film of Example 2. The composition for forming a resist underlayer film of Preparation Example 3 was used to obtain a resist underlayer film of Example 3. The resist underlayer film of Example 4 was obtained using the composition for forming the resist underlayer film of Preparation Example 4. The composition for forming a resist underlayer film of Preparation Example 5 was used to obtain a resist underlayer film of Example 5. The composition for forming a resist underlayer film of Preparation Example 6 was used to obtain a resist underlayer film of Example 6. The resist underlayer film of Example 7 was obtained using the composition for forming the resist underlayer film of Preparation Example 7. The resist underlayer film of Example 8 was obtained using the composition for forming the resist underlayer film of Preparation Example 8. The resist underlayer film-forming composition of Comparative Preparation Example 1 was used to obtain a resist underlayer film of Comparative Example 1.

[0166] (Resist patterning evaluation) <Resist pattern formation test using electron beam lithography equipment> On each resist underlayer film of Examples 1 to 8 and Comparative Example 1 formed on a silicon wafer, an EUV positive resist solution was spin-coated and heated at 130°C for 60 seconds to form an EUV resist film with a film thickness of 35 nm. The resist film was exposed under predetermined conditions using an electron beam lithography device (ELS-G130). After exposure, the resist film was baked (PEB) at 90°C for 60 seconds, cooled to room temperature on a cooling plate, and paddle development was performed for 30 seconds using a 2.38% tetramethylammonium hydroxide aqueous solution (manufactured by Tokyo Ohka Kogyo Co., Ltd., product name NMD-3) as a photoresist developer. A resist pattern with a line size of 16 nm to 28 nm was formed. A scanning electron microscope (manufactured by Hitachi High-Technologies Corporation, CG4100) was used to measure the length of the resist pattern.

[0167] The photoresist pattern thus obtained was observed from above the pattern, and the charge amount forming 22 nm lines / 44 nm pitch (line and space (L / S=1 / 1)) was defined as the optimal irradiation energy. The irradiation energy at that time (μC / cm 2 ), and LWR, which is a value indicating the roughness of the pattern shape, were checked. LWR is expressed as three times the standard deviation (σ) (3σ) (unit: nm) calculated from the measurement results of measuring 400 line positions in the longitudinal direction of the line using a scanning electron microscope (CG4100, manufactured by Hitachi High-Technologies Corporation). The smaller the LWR value, the better the pattern that can be formed. The results are shown in Table 2.

[0168] As Comparative Example 2, a similar test was performed using a silicon substrate that was not formed with a resist underlayer film and was subjected to HMDS (hexamethyldisilazane) treatment. The results are shown in Table 2.

[0169] [Table 2]

[0170] In Examples 1 to 8, an improvement in LWR was confirmed compared to Comparative Examples 1 and 2. When a resist underlayer film having a thickness of 20 nm or more is used, the resist film thickness is thin in the dry etching process after the formation of the resist pattern, so that the resist pattern is damaged in the process of etching the underlayer film, resulting in shape defects such as a reduction in the resist film thickness and a top rounding shape, which makes it difficult to form a pattern with a desired line width during actual substrate processing.

Claims

1. A resist underlayer film which is a fired product of a coating film of a composition for forming a resist underlayer film, The composition for forming a resist underlayer film contains a polymer having a unit structure (A) having a polycyclic aromatic hydrocarbon structure and a unit structure (B) derived from a maleimide structure, and a crosslinking agent; the unit structure (A) is a unit structure represented by the following formula (1), the following formula (2), or the following formula (3), or the polycyclic aromatic hydrocarbon structure is a unit structure having a heterocyclic structure, The unit structure (B) is a unit structure represented by the following formula (4): The resist underlayer film has a thickness of less than 10 nm. 【Chemistry 1】 (In formula (1), R 1 represents a hydrogen atom or a methyl group. X represents an ester group or an amide group. Y represents an alkylene group having 1 to 6 carbon atoms. p represents 1. q represents 0 or 1. Ar represents a monovalent group obtained by removing a hydrogen atom from naphthalene, anthracene, phenanthrene, pyrene, triphenylene, chrysene, naphthacene, biphenylene, fluorene, or carbazole, which may be substituted. 【Chemistry 2】 (In formula (2), R 1 represents a hydrogen atom or a methyl group, Z represents a halogen atom, an alkyl group, an alkoxy group, a thiol group, a cyano group, a carboxyl group, an amino group, an amido group, an alkoxycarbonyl group, or a thioalkyl group substituted on a naphthalene ring, and n represents an integer of 0 to 7. When n is 2 or more, two or more Z's may be the same or different. 【Chemistry 3】 (In formula (3), Ar 1 and Ar 2 each independently represents an aromatic ring having 6 to 40 carbon atoms which may be substituted, and Ar 1 and Ar 2 At least one of is naphthalene, anthracene, phenanthrene, or pyrene, and Q represents a single bond, an ether group, an ester group, or an imino group. 【Chemistry 4】 (In formula (4), R 2 represents an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 10 carbon atoms which may be substituted with a halogen atom.

2. The resist underlayer film according to claim 1 , wherein the polymer further comprises a unit structure (C) having a crosslinking group.

3. The resist underlayer film according to claim 2, wherein the crosslinking group in the unit structure (C) comprises at least one group selected from the group consisting of a hydroxy group, an epoxy group, a protected hydroxy group, and a protected carboxy group.

4. The resist underlayer film according to claim 1 , wherein the composition for forming a resist underlayer film further comprises a curing catalyst.

5. The resist underlayer film according to claim 1 , which is a resist underlayer film for EB or EUV lithography.

6. A semiconductor substrate; The resist underlayer film according to any one of claims 1 to 5, A semiconductor processing substrate comprising:

7. forming a resist underlayer film according to any one of claims 1 to 5 on a semiconductor substrate; forming a resist film on the resist underlayer film; A method for manufacturing a semiconductor device, comprising:

8. forming a resist underlayer film according to any one of claims 1 to 5 on a semiconductor substrate; forming a resist film on the resist underlayer film using a resist for EB or EUV lithography; irradiating the resist film with EB or EUV, and then developing the resist film to obtain a resist pattern; Etching the resist underlayer film using the resist pattern as a mask; A pattern forming method comprising:

9. forming a resist underlayer film according to any one of claims 1 to 5 on a semiconductor substrate; forming a resist film on the resist underlayer film using a resist for EB or EUV lithography; irradiating the resist film with EB or EUV, and then developing the resist film to obtain a resist pattern; A method for improving LWR of a resist pattern, comprising:

Citation Information

Patent Citations

  • Composition for forming antireflection film for lithography

    JP2002323771A

  • Detergent for lithography and method for forming resist pattern with the same

    JP2007213013A

  • Antireflective coating composition, antireflective coating, and patterning process using the same

    JP2009098639A

  • Wet developable bottom antireflective coating composition and method of use

    JP2009534710A

  • Composition for resist underlay film formation, pattern formation method and polymer

    JP2013073125A