Crimped body and manufacturing method thereof

The crimped body with fluororesin base materials and oriented polytetrafluoroethylene fibrils addresses mechanical strength and fiber integrity issues, ensuring robustness and shape retention through a carbon dioxide-based bonding process.

JP7560062B2Active Publication Date: 2024-10-02VALQUA LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021536929
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-01
Filing Date
2020-07-16
Publication Date
2024-10-02
Estimated Expiration
2040-07-16

AI Technical Summary

Technical Problem

Conventional fluororesin porous sheets, particularly crimped bodies made from nonwoven fabrics, porous membranes, and fibers, suffer from poor mechanical strength and fiber fraying or peeling issues, and high-temperature thermo-compression bonding eliminates voids, losing their structural integrity.

Method used

A crimped body configuration using fluororesin base materials with a high mass content of -CF2 groups and polytetrafluoroethylene fibrils oriented at 45 to 90 degrees, bonded via a process involving carbon dioxide to maintain voids and enhance mechanical strength.

Benefits of technology

The crimped body achieves excellent mechanical strength with reduced fiber fraying and peeling, maintaining desired shapes and voids without high-temperature fusion, suitable for various applications including medical and electrical equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560062000003
    Figure 0007560062000003
  • Figure 0007560062000004
    Figure 0007560062000004
  • Figure 0007560062000005
    Figure 0007560062000005
Patent Text Reader

Abstract

One embodiment of the present invention relates to a press-adhered body or a production method therefor. The press-adhered body is formed from at least one type of base material selected from the group consisting of non-woven fabric, stretched porous film, and fibers. The base material contains a fluorine resin (excluding polytetrafluoroethylene) having a -CF2- group content of 85% by mass or more. Polytetraethylene fibrils are used as bonds between the fibers constituting the base material. In addition, with respect to the entirety of the fibrils, the proportion of the number of fibrils that are oriented 45° to 90° relative to the direction of the fibers constituting the base material is 50% or greater.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] An embodiment of the present invention relates to a crimped body or a method for manufacturing the same. [Background technology]

[0002] Fluorine resins are functional polymers that have many excellent properties, such as excellent heat resistance, chemical resistance, weather resistance, and electrical properties, as well as a non-sticky surface and a low coefficient of friction.

[0003] Such substrates containing at least one selected from fluororesin nonwoven fabrics, porous membranes, and fibers have been attracting attention in the fields of medical use and precision electrical equipment, particularly due to their good chemical resistance, good electrical properties, etc. However, substrates made of fluororesin are poor in mechanical strength as a whole because the polymers constituting them are non-adhesive and have a small coefficient of friction, and there has been a high incidence of fiber and other components constituting the substrate falling off.

[0004] To address such problems, Patent Document 1 discloses a PFA porous sheet made of a group of PFA filaments containing a large number of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA) fine particles. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2011 / 105414 Summary of the Invention [Problem to be solved by the invention]

[0006] The present inventors have confirmed that conventional fluororesin porous sheets, particularly at least one type of pressure-bonded body selected from conventional nonwoven fabrics, porous membranes and fibers, have room for improvement in terms of mechanical strength. In addition, in order to improve mechanical strength and prevent the loss of fibers, etc., it is possible to heat-seal (thermocompress) the substrate at a high temperature above its melting point. In this case, however, the voids that were present in the substrate before fusion disappear and the substrate becomes a simple sheet, which makes it meaningless to use a substrate such as a nonwoven fabric, a porous membrane, or a fiber.

[0007] An embodiment of the present invention provides a pressure-bonded body having a desired shape, which has excellent mechanical strength and is less susceptible to fraying of fibers and peeling between substrates. [Means for solving the problem]

[0008] The inventors have found that the above problems can be solved by the following configuration examples, and have completed the present invention. A configuration example of the present invention is as follows.

[0009] [1] A pressure-bonded body of at least one substrate selected from the group consisting of a nonwoven fabric, an expanded porous membrane, and a fiber, the substrate is a substrate containing a fluororesin (excluding polytetrafluoroethylene) having a -CF2- group content of 85 mass% or more, The fibers constituting the base material are spaced apart by polytetrafluoroethylene. Fluoro Fibrils of ethylene are bonded, and the ratio of the number of fibrils oriented at 45 to 90° to the fiber direction constituting the base material to the total number of the fibrils is 50% or more. Crimp body.

[0010] [2] The pressure-bonded body according to [1], wherein the content of the polytetrafluoroethylene is 0.2 to 12 mass % relative to 100 mass % of the base material. [3] The bonded body according to [1] or [2], wherein the average fiber diameter of the fibrils is 10 nm to 1 μm.

[0011] [4] The pressure-bonded body according to any one of [1] to [3], wherein the base material contains at least one fluororesin selected from the group consisting of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether copolymer (EPE), fluoroethylene-vinyl ether copolymer (FEVE) and poly(chlorotrifluoroethylene) (PCTFE).

[0012] [5] At least one substrate selected from the group consisting of nonwoven fabrics, stretched porous membranes, and fibers, Polytetrafluoroethylene particles; Carbon dioxide in liquid, gas-liquid mixture or near-liquid state A method for producing a crimped body, comprising step 1 of crimping in the presence of

[0013] [6] The step 1 A step 1a of contacting at least one substrate selected from the group consisting of a nonwoven fabric, an expanded porous membrane, and a fiber, and a polytetrafluoroethylene dispersion with liquid or gaseous carbon dioxide and applying pressure; or A step 1b of contacting at least one member selected from the group consisting of nonwoven fabrics, stretched porous membranes, and fibers with a polytetrafluoroethylene dispersion, and then drying the resulting mixture, and contacting the resulting mixture with liquid or gaseous carbon dioxide and applying pressure. The method for producing a pressure-bonded body according to [5],

[0014] [7] The pressure-bonding body is a polytetrafluoroethylene substrate. Fluoro A method for producing a pressure-bonded body according to [5] or [6], which has a structure in which ethylene fibrils are bonded. [8] The method for producing a pressure-bonded body according to [7], wherein the ratio of the number of fibrils oriented at an angle of 0 to 45° to the pressure-bonding direction to the total number of fibrils is 50% or more.

[0015] [9] The method for producing a pressure-bonded body according to any one of [5] to [8], wherein the content of polytetrafluoroethylene in the pressure-bonded body is 0.2 to 12 mass % relative to 100 mass % of the base material in the pressure-bonded body.

[0016]

[10] The method for producing a pressure-bonded body according to [7] or [8], wherein the average fiber diameter of the fibrils is 10 nm to 1 μm.

[0017]

[11] The method for producing a pressure-bonded body according to any one of [5] to

[10] , wherein the base material contains at least one fluororesin selected from the group consisting of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether copolymer (EPE), fluoroethylene-vinyl ether copolymer (FEVE) and poly(chlorotrifluoroethylene) (PCTFE). Effect of the Invention

[0018] According to one embodiment of the present invention, it is possible to obtain a pressure-bonded body having a desired shape, which has excellent mechanical strength and is less susceptible to fraying of fibers and peeling between base materials. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is an SEM image of the space between PFA fibers in the crimped body of Example 2. [Diagram 2] FIG. 2 is an SEM image of the gap between PFA fibers in the bonded body of Comparative Example 2. [Diagram 3] FIG. 3 is an SEM image of the space between PFA fibers in the crimped body of Example 1. [Figure 4] FIG. 4 is an SEM image of the gap between PFA fibers in the pressure-bonded body of Comparative Example 1. [Diagram 5] FIG. 5 is an SEM image of a cross section of the compressed body of Comparative Example 5. [Figure 6] FIG. 6 is a photograph showing the appearance of the pressure-bonded body of Example 2. [Figure 7] FIG. 7 is a photograph showing the appearance of the pressure-bonded body of Comparative Example 2. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] <Crimping body> The pressure-bonded body according to one embodiment of the present invention (hereinafter also referred to as "this pressure-bonded body") is a pressure-bonded body of at least one substrate selected from the group consisting of a nonwoven fabric, an expanded porous membrane, and a fiber (hereinafter also referred to as "fiber A"). the substrate is a substrate containing a fluororesin (excluding polytetrafluoroethylene (PTFE)) having a -CF2- group content of 85 mass% or more, The fibers constituting the base material are spaced apart by polytetrafluoroethylene. Fluoro The base material is characterized in that ethylene fibrils are bonded, and the ratio of the number of fibrils oriented at 45 to 90° to the fiber direction constituting the base material to the total number of fibrils is 50% or more.

[0021] Examples of the present pressure-bonded body include, when a nonwoven fabric is used as the substrate, a pressure-bonded body of one sheet of nonwoven fabric, a pressure-bonded body in which two or more sheets of one or more types of nonwoven fabric are used and these nonwoven fabrics are pressure-bonded together, and a pressure-bonded body in which one or more types of nonwoven fabric are pressure-bonded to at least one type selected from the group consisting of an expanded porous membrane and fiber A. The above-mentioned pressed body of a single sheet of nonwoven fabric may have a reduced amount of voids in the nonwoven fabric. Even in this case, according to one embodiment of the present invention, particularly the method described below, it is possible to obtain a pressed body in which the voids in the nonwoven fabric are completely lost and the body does not simply become a film, but in which the volume is reduced while the voids remain. Examples of the bonded body when the expanded porous membrane or fiber A is used as the substrate are similar to those when the nonwoven fabric is used. When one type of fiber A is used as the substrate, a bonded body can be obtained by bonding between one bent fiber A with PTFE fibrils, but two or more fiber A are usually used.

[0022] Of these, the present compression body is preferably a compression body of two or more nonwoven fabrics, in terms of the effect of the present invention being more effectively exerted, etc. Conventionally, it has not been easy to compression-bond two or more nonwoven fabrics containing the above-mentioned fluororesin, or the nonwoven fabrics have been compression-bonded by eliminating the voids therein through fusion, but according to one embodiment of the present invention, particularly the method described below, two or more nonwoven fabrics can be compression-bonded while leaving the voids therein (fluffy state).

[0023] The phrase "PTFE fibrils bond between the fibers constituting the substrate" means that, for example, when a nonwoven fabric is used as the substrate, PTFE fibrils bond (bridge or connect) between the fibers constituting the nonwoven fabric, between the fibers constituting the nonwoven fabric and the fibers constituting the stretched porous membrane, and between the fibers constituting the nonwoven fabric and fiber A. In this case, PTFE fibrils usually bond between adjacent fibers among the fibers constituting the substrate. The same applies to the case where an expanded porous membrane or fiber A is used as the substrate.

[0024] Moreover, the phrase "the ratio of the number of fibrils oriented at 45 to 90 degrees to the fiber direction constituting the base material to the total number of fibrils is 50% or more" means that the ratio of the number of fibrils oriented in a direction approximately perpendicular to the fiber direction constituting the base material to the total number of fibrils constituting the compressed body is 50% or more. Note that the 45° angle is equivalent to 135° if the angle is measured in a different direction. In other words, 45 to 90° angle is equivalent to 90 to 135° angle. Since many of the PTFE fibrils in this bonded body are oriented approximately perpendicular to the direction of the fibers that make up the base material, the bonded body has excellent mechanical strength and is less susceptible to fraying of the fibers or peeling between the base materials, resulting in a bonded body having the desired shape.

[0025] The number of fibrils oriented at 45 to 90° to the fiber direction constituting the base material is preferably the number of fibrils oriented at 70 to 90° to the fiber direction constituting the base material, and more preferably the number of fibrils oriented at 80 to 90° to the fiber direction constituting the base material. The ratio of the number of fibrils oriented approximately perpendicular to the fiber direction constituting the base material to the total number of fibrils constituting the pressure-bonded body is preferably 75 to 100%, and more preferably 85 to 100%, in order to obtain a pressure-bonded body having excellent effects due to the above-mentioned effects. The orientation direction of the fibrils can be determined by checking the orientation direction of any 40 fibrils relative to the fiber direction constituting the substrate in an SEM image of the cross section of the pressure-bonded body, and the percentage is a value calculated from the number of fibrils that are oriented approximately perpendicular to the fiber direction constituting the substrate out of the 40 fibrils.

[0026] The shape and size of the pressure-bonded body are not particularly limited and may be appropriately selected depending on the desired application. The thickness of the laminate is not particularly limited and may be appropriately selected depending on the application, but in the case of a laminate of a nonwoven fabric or an expanded porous membrane, it is usually 10 μm or more, preferably 50 μm or more, and usually 30 mm or less, preferably 25 mm or less.

[0027] This pressure-bonded body can be suitably used in applications in which a nonwoven fabric, an expanded porous membrane, or fiber A containing a fluororesin has been used, and can be particularly suitably used in the medical field, the electrical equipment field, the semiconductor field, etc., and specifically, can be suitably used as a filter, various separators, clothing, etc.

[0028] The present pressure-bonded body may contain one or more functional materials required for a desired application, such as foodstuffs, drugs (medicinal, agricultural, industrial), dyes, adsorbents, deodorants, fragrances, insect repellents, electronic device materials, enzymes, and catalysts. When the present pressure-bonded body contains such a functional material, even if the functional material has poor heat resistance, it is possible to obtain a pressure-bonded body that makes the most of the functions and properties of the functional material. For example, when a drug or the like is contained, it is possible to obtain a compressed body in which the sustained release or the like of the drug or the like is controlled.

[0029] <Base material> The substrate is a substrate containing a fluororesin (excluding PTFE) having a -CF2- group content of 85 mass % or more, and a substrate made of such a fluororesin is preferable. The content of -CF2- groups in the fluororesin can be measured and calculated by solid-state nuclear magnetic resonance (NMR) or mass spectrometry (MS spectrometry), or the like.

[0030] The fluororesin is not particularly limited as long as it is a resin having a -CF2- group content of 85 mass% or more in the resin composition and is a resin other than PTFE, and specific examples include tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether copolymer (EPE), fluoroethylene-vinyl ether copolymer (FEVE) and poly(chlorotrifluoroethylene) (PCTFE). The substrate may contain two or more types of fluororesin, but typically contains one type.

[0031] Among these fluororesins, PFA and FEP are preferred because they have excellent mechanical strength, heat resistance, chemical resistance, weather resistance, and electrical insulation, and PFA is more preferred because it is easily plasticized with carbon dioxide in the method described below. Since PFA is non-adhesive and has a small coefficient of friction, it has not been possible to obtain a pressure-bonded body having excellent mechanical strength from at least one type selected from PFA nonwoven fabric, PFA expanded porous membrane, and PFA fiber A. However, according to one embodiment of the present invention, even a pressure-bonded body containing such PFA can easily be obtained which has excellent mechanical strength and has a desired shape that is less susceptible to fraying of fibers and peeling between substrates.

[0032] The nonwoven fabric, the stretched porous membrane, and the fiber A are not particularly limited, and any of the conventionally known nonwoven fabrics, stretched porous membranes, and fibers A can be used.

[0033] The average fiber diameter of the fibers constituting the nonwoven fabric and the fiber A is preferably 0.1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and is preferably 200 μm or less, more preferably 100 μm or less, even more preferably 80 μm or less. When the average fiber diameter is within the above range, the fiber surface area is increased, which allows more PTFE fibrils to be formed, and it is preferable in that a bonded body having a desired shape can be obtained that has excellent mechanical strength and is less susceptible to fraying of the fibers or peeling between the substrates.

[0034] The average fiber diameter is an average value calculated based on the measurement results by observing the fiber (group) to be measured with a scanning electron microscope (SEM), randomly selecting 20 fibers from the obtained SEM image, and measuring the fiber diameter (long diameter) of each of these fibers.

[0035] The fiber diameter variation coefficient of the fibers constituting the nonwoven fabric and the fiber A, calculated by the following formula, is preferably 0.7 or less, more preferably 0.01 or more, and more preferably 0.5 or less. When the fiber diameter variation coefficient is within the above range, the fiber diameter becomes uniform, and a pressure-bonded body having a desired shape and excellent mechanical strength, which is less susceptible to fraying of the fibers and peeling between the substrates, can be easily obtained. Coefficient of variation of fiber diameter = standard deviation / average fiber diameter (Note that the "standard deviation" refers to the standard deviation of the fiber diameters of the 20 fibers.)

[0036] The fiber length of the fibers constituting the nonwoven fabric and the fiber A is not particularly limited, but is preferably 0.5 mm or more, more preferably 1 mm or more, and is preferably 100 mm or less, more preferably 50 mm or less.

[0037] The stretched porous membrane is not particularly limited, and may be a uniaxially stretched porous membrane or a biaxially stretched porous membrane.

[0038] The porosity of the nonwoven fabric or stretched porous membrane is not particularly limited, but is, for example, 0.1 vol. % or more, preferably 1 vol. % or more, and is, for example, 70 vol. % or less, preferably 60 vol. % or less. The porosity can be calculated from the difference between the theoretical volume calculated assuming no voids based on the specific gravity of the resin constituting the nonwoven fabric or stretched porous membrane and the actual measured mass of the nonwoven fabric or stretched porous membrane, and the actual volume calculated by measuring the dimensions of the nonwoven fabric or stretched porous membrane, using the following formula. Porosity (volume%) = (1-(theoretical volume / measured volume)) x 100

[0039] The weight of the nonwoven fabric or the stretched porous membrane is preferably 100 g / m 2 More preferably, it is 1 g / m or less. 2 More preferably, 80 g / m 2 The following is the result.

[0040] The thickness of the nonwoven fabric or the stretched porous membrane is usually 10 μm or more, preferably 50 μm or more, and usually 1 mm or less, preferably 500 μm or less.

[0041] <PTFEのフィブリル> In this pressure-bonded body, the fibers constituting the base material are bonded with PTFE fibrils. The PTFE fibrils are preferably formed from PTFE particles (particles contained in a PTFE dispersion) and usually do not have nodes. In other words, the fibrils contained in this crimped body are different from fibrils formed by stretching.

[0042] The average fiber diameter of the fibrils is preferably 10 nm or more, more preferably 50 nm or more, and particularly preferably 80 nm or more, from the viewpoints of being able to firmly bond the substrates, being excellent in mechanical strength, and being able to easily obtain a bonded body having the desired shape that is less likely to fray the fibers or peel between the substrates, etc., and is preferably 1 μm or less, more preferably 800 nm or less, and particularly preferably 500 nm or less. The average fiber diameter of the fibrils can be calculated in the same manner as the average fiber diameter of the fibers.

[0043] The average fiber length of the fibrils is not particularly limited as long as it is long enough to bond the (adjacent) fibers that make up the substrate in the resulting bonded body, but is usually 1 μm or more, preferably 10 μm or more, and usually 100 μm or less, preferably 40 μm or less. The average fiber length is an average value calculated based on the measurement results by observing the fibril (group) to be measured with a scanning electron microscope (SEM), randomly selecting 20 fibrils from the obtained SEM image, measuring the fiber length of each of these fibrils, and calculating the average value based on the measurement results.

[0044] In this pressure-bonded body, the content of the fibrils (PTFE content) relative to 100% by mass of the substrate is preferably 0.2% by mass or more, more preferably 1% by mass or more, and particularly preferably 2% by mass or more, from the standpoint of being able to firmly bond the substrate, having excellent mechanical strength, and being able to easily obtain a pressure-bonded body having the desired shape that is less likely to fray fibers or peel between substrates, etc., and is preferably 12% by mass or less, more preferably 10% by mass or less, and particularly preferably 5% by mass or less.

[0045] <Method of manufacturing the pressure-bonded body> The method for producing a pressure-bonded body according to one embodiment of the present invention (hereinafter also referred to as "this method") comprises the steps of: PTFE particles, Carbon dioxide in liquid, gas-liquid mixture or near-liquid state The method includes the step of: The substrate is preferably a substrate containing a fluororesin (excluding polytetrafluoroethylene) having a -CF2- group content of 85 mass% or more. In this case, the present method can also be said to be a novel processing method for at least one material selected from a fluororesin nonwoven fabric, an expanded porous membrane, and fiber A, which are difficult to process.

[0046] According to this method, a pressure-bonded body can be produced at a low cost in a short time at a temperature of about 50°C or less without applying high heat that melts the resin constituting the substrate. In addition, since carbon dioxide does not remain in the obtained pressure-bonded body, it is easy to obtain a clean pressure-bonded body with excellent safety, controllability and productivity, and a pressure-bonded body having a desired shape with excellent mechanical strength and little fraying of fibers or peeling between substrates. In particular, a pressure-bonded body can be obtained while maintaining the characteristics of the substrate (e.g., voids and fiber shape of nonwoven fabric). Furthermore, according to this method, when manufacturing a pressure-bonded body containing a functional material to be used according to the desired application, even if the functional material has poor heat resistance, it is possible to obtain a pressure-bonded body that makes use of the functions, properties, etc. of the functional material.

[0047] The present pressure-bonded body is preferably a pressure-bonded body obtained by the present method, which can easily obtain a pressure-bonded body in which PTFE fibrils bond between the fibers constituting the base material. In this case, from the standpoint of being able to firmly bond the substrates, being able to easily obtain a bonded body having the desired shape that has excellent mechanical strength and is less prone to fraying of fibers or peeling between substrates, etc., it is preferable that the proportion of fibrils oriented at 0 to 45° to the bonding direction relative to the total number of fibrils in the bonded body obtained by this method is 50% or more. In the compressed body produced by this method, the fibers constituting the base material tend to be oriented in a direction approximately perpendicular to the bonding direction, and the PTFE fibrils tend to be oriented approximately in the bonding direction so as to connect the fibers. Therefore, "the ratio of the number of fibrils oriented at 0 to 45° to the bonding direction to the total number of fibrils is 50% or more" corresponds to "the ratio of the number of fibrils oriented at 45 to 90° to the fiber direction constituting the base material to the total number of fibrils is 50% or more" in this compressed body.

[0048] The phrase "the ratio of the number of fibrils oriented at 0 to 45° to the compression direction to the total number of fibrils is 50% or more" means that the ratio of the number of fibrils oriented in a direction approximately parallel to the compression direction (the direction in which pressure is applied) to the total number of fibrils constituting the compression body is 50% or more. As mentioned above, 45° is equivalent to 315° if the direction in which the angle is measured is changed. In other words, 0 to 45° is equivalent to 315 to 360°.

[0049] The number of fibrils oriented at an angle of 0 to 45° to the compression direction is preferably the number of fibrils oriented at an angle of 0 to 20° to the compression direction, and more preferably the number of fibrils oriented at an angle of 0 to 10° to the compression direction. The ratio of the number of fibrils oriented approximately parallel to the bonding direction to the total number of fibrils constituting the pressure-bonded body is preferably 75 to 100%, and more preferably 85 to 100%, from the viewpoint of easily obtaining a pressure-bonded body having the desired shape with superior mechanical strength and less susceptible to fraying of fibers and peeling between substrates. The orientation direction of the fibrils can be determined by checking the orientation direction of any 40 fibrils relative to the compression direction in an SEM image of the cross section of the compressed body, and the percentage is a value calculated from the number of fibrils that are oriented approximately parallel to the compression direction among the 40 fibrils.

[0050] Although it is not entirely clear why this method makes it possible to obtain a bonded body having the desired shape that has excellent mechanical strength and is less prone to fraying of fibers or peeling between substrates, it is thought that this is because applying pressure in the presence of carbon dioxide in a liquid, gas-liquid mixture, or near-liquid state plasticizes the surface of the substrate with the carbon dioxide, and applying pressure in this plasticized state makes it possible to fix the shape in an interlocking state and bond and join the substrates.

[0051] <Process 1> The step 1 is not particularly limited as long as it is a step of pressing the substrate in the presence of PTFE particles and carbon dioxide in a liquid, gas-liquid mixed state, or liquid-like state, and during this pressing, one or more functional materials required for the intended use may be included depending on the intended use. Examples of the functional materials include the same materials as those described in the section on the pressed body. Even if the functional material has poor heat resistance, the method of the present invention can provide a pressure-bonded body that makes the most of the functions and properties of the functional material.

[0052] There is no particular limitation on the PTFE particles used in step 1, and conventionally known PTFE particles can be used. Two or more types of PTFE particles having different average particle sizes, etc. may also be used. In step 1, it is preferable to use a PTFE dispersion, since a desired pressure-bonded body can be easily formed. In this case, it is sufficient that PTFE particles are present when the substrate is pressure-bonded, and pressure-bonding may be performed by contacting a contact body obtained by contacting the substrate with the PTFE dispersion with carbon dioxide, or pressure-bonding may be performed by contacting a dried body obtained by contacting the substrate with the PTFE dispersion in advance and then drying the resulting body with carbon dioxide.

[0053] The average particle size of the PTFE particles is preferably 0.15 to 0.35 μm, since it is possible to more firmly bond the substrate, have excellent mechanical strength, and easily obtain a bonded body having a desired shape that is less susceptible to fraying of fibers or peeling between substrates. The average particle size can be measured by a light scattering method.

[0054] The PTFE dispersion is not particularly limited, and any conventionally known dispersion can be used. However, it is preferable to use a dispersion having a PTFE particle concentration of 10 to 60 mass %, since the desired pressure-bonded body can be easily formed. The PTFE dispersion may contain conventionally known additives such as a stabilizer.

[0055] The amount of the PTFE particles used relative to 100% by mass of the substrate used in step 1 is preferably 0.2% by mass or more, more preferably 1% by mass or more, and particularly preferably 2% by mass or more, from the viewpoints of being able to firmly bond the substrate, being excellent in mechanical strength, and being able to easily obtain a bonded body having the desired shape that is less likely to cause fiber fraying or peeling between substrates, etc., and is preferably 12% by mass or less, more preferably 10% by mass or less, and particularly preferably 5% by mass or less.

[0056] In step 1, the substrate is compressed in the presence of carbon dioxide in a liquid state, a gas-liquid mixture state, or a state close to liquid. It is believed that contacting the substrate with carbon dioxide in a liquid state, a gas-liquid mixture state, or a state close to liquid causes the substrate to be impregnated with carbon dioxide, making it possible to plasticize the substrate, and thus making it possible to produce a compressed body without heating. In step 1, carbon dioxide in a subcritical or supercritical state may be used, but carbon dioxide in a liquid state or a gas-liquid mixed state is preferred from the viewpoints that the pressing force can be reduced and pressure bonding can be performed without using a device having a heating mechanism, etc. Also, since gaseous carbon dioxide is considered to hardly plasticize the base material or to require a considerable amount of time for plasticization, carbon dioxide in a liquid state or a gas-liquid mixed state is preferred from the viewpoints that the base material can be plasticized quickly, etc.

[0057] The above-mentioned "carbon dioxide in a state close to liquid" specifically refers to carbon dioxide in a state in which the density is 0.4 g / mL or more (about half the density of liquid carbon dioxide).

[0058] Specifically, the step 1 is preferably carried out by introducing liquid or gaseous carbon dioxide into the system. That is, specifically, the step 1 is preferably the following step 1a or 1b. Step 1a: A step of contacting at least one substrate selected from the group consisting of a nonwoven fabric, an expanded porous membrane, and fiber A, and a polytetrafluoroethylene dispersion with liquid or gaseous carbon dioxide, and applying pressure. Step 1b: A step of contacting at least one substrate selected from the group consisting of a nonwoven fabric, an expanded porous membrane, and fiber A with a polytetrafluoroethylene dispersion, and then contacting the resulting dried body with liquid or gaseous carbon dioxide and applying pressure.

[0059] When liquid or gaseous carbon dioxide is introduced into the system, the order in which the substrate, PTFE particles, and carbon dioxide are introduced into the system is not particularly limited. For example, the substrate and PTFE particles may be introduced into a system filled with carbon dioxide, but it is preferable to introduce carbon dioxide into the system into which the substrate and PTFE particles have been introduced. When introducing liquid carbon dioxide, the compression step for liquefaction can be omitted compared to when introducing gaseous carbon dioxide, and therefore the compressed body can be manufactured in a short time. On the other hand, when gaseous carbon dioxide is introduced, the process is easier than when liquid carbon dioxide is introduced, and a pressure pump may be unnecessary, allowing the device to be simplified. When gaseous carbon dioxide is introduced, the introduced carbon dioxide is usually pressurized to liquefy the carbon dioxide. In this case, it is not necessary to liquefy all of the introduced carbon dioxide, and it is sufficient to liquefy at least a portion of it.

[0060] The amount of carbon dioxide introduced is not particularly limited, but when gaseous carbon dioxide is introduced and compression is performed at a temperature of 31°C (the critical temperature of carbon dioxide) or higher, carbon dioxide is introduced so that the density of carbon dioxide during compression is 0.4 g / mL or higher (about half the density of liquid carbon dioxide).

[0061] The surface pressure during pressure bonding in step 1 may be appropriately selected depending on the type and amount of the base material used, the desired shape of the pressure-bonded body, etc., but is preferably 4 MPa or more, more preferably 5 MPa or more, and there is no particular upper limit, but it is, for example, 50 MPa or less. The surface pressure is the sum of the pressure of the carbon dioxide introduced into the system and the pressing pressure.

[0062] The pressing time during compression bonding in step 1 may be appropriately selected depending on the type and amount of the base material used, the surface pressure and temperature during compression bonding, etc., but is preferably 0.2 seconds or more, more preferably 1 second or more, and is preferably 15 minutes or less, more preferably 5 minutes or less.

[0063] The temperature during compression in step 1 may be appropriately selected depending on the type and amount of the base material used, the desired shape of the compression body, etc., but according to the present method, the desired compression body can be obtained without applying heat, so that this effect can be more effectively exhibited at a temperature that is usually 0°C or higher, more preferably 20°C or higher, and usually 40°C or lower, more preferably 30°C or lower.

[0064] Step 1 may be carried out in a sealed container capable of reducing the volume, or may be carried out using an open pressing device. The sealed container may, for example, be a container having an inlet for introducing liquid or gaseous carbon dioxide into the sealed space and an outlet for carbon dioxide, and having a member such as a piston that can reduce the volume of the sealed container to press the substrate.

[0065] An example of a method using an open press device is a method in which a contact body in which the base material is contacted with a PTFE dispersion or a dried body is placed between press members such as pistons, and pressing is performed while introducing liquid carbon dioxide therein. When an open pressing device is used, the object to be treated can be treated in a spot manner without using a large treatment container that covers the entire substrate to be treated. For example, the substrate can be sent out and pressed repeatedly in a different position, or a roller can be used instead of a piston to press the substrate, thereby continuously producing pressed bodies. EXAMPLES

[0066] Next, the present invention will be described in more detail by showing examples, but the present invention is not limited to these.

[0067] [Example 1] 0.5g of PFA short fibers with an average fiber diameter of 60μm and 0.03g of PTFE dispersion (manufactured by Daikin Industries, Ltd., Polyflon PTFE-D D-210C, aqueous dispersion with a solid content of 60% by mass, average particle size of PTFE particles: 0.22μm) (PTFE amount relative to PFA mass is 3.6% by mass) were added to a sealable container (diameter: φ20mm) having a piston, a carbon dioxide inlet, and a carbon dioxide outlet. Carbon dioxide equivalent to the vapor pressure of carbon dioxide (cylinder pressure: 6MPa) was introduced thereto at room temperature (25°C), the piston was lowered to reduce the volume in the container (while liquefying carbon dioxide), and a pressure of 100N (surface pressure: 6.3MPa) was applied for 10 seconds to bond the PFA fibers together. After that, the carbon dioxide was instantly discharged while maintaining the pressure, and then the pressure was released, and the bonded body (φ20mm) was taken out of the container.

[0068] [Example 2] A pressure-bonded body was produced in the same manner as in Example 1, except that the pressure during pressure-bonding was changed to a load of 3000 N (surface pressure: 18 MPa).

[0069] [Example 3] A pressure-bonded body was produced in the same manner as in Example 1, except that the pressure during pressure-bonding was changed to a load of 5000 N (surface pressure: 22 MPa).

[0070] [Comparative Example 1] A compressed body was produced in the same manner as in Example 1, except that carbon dioxide was not introduced.

[0071] [Comparative Example 2] A compressed body was produced in the same manner as in Example 2, except that carbon dioxide was not introduced.

[0072] [Comparative Example 3] A compressed body was produced in the same manner as in Example 3, except that carbon dioxide was not introduced.

[0073] [Comparative Example 4] 0.5 g of PFA short fibers with an average fiber diameter of 60 μm were pressed for 5 minutes using a hand press machine (Mini Test Press MP-WCH [manufactured by Toyo Seiki Seisakusho Co., Ltd.]) at a temperature of 260°C and a surface pressure of 12 MPa to produce a bonded body (thickness: 1.5 mm).

[0074] [Comparative Example 5] A pressure-bonded body (thickness: 1.0 mm) was produced in the same manner as in Comparative Example 4, except that the temperature was changed to 320°C.

[0075] The following evaluations were carried out using the pressure-bonded bodies obtained in the Examples and Comparative Examples.

[0076] 1.Structural Observation The structure between the PFA fibers was observed at a magnification of 500 or 1000 using an SEM (S-3400N, manufactured by Hitachi High-Technologies Corporation) to confirm the presence or absence of PTFE fibrils, the orientation of the fibrils, and the like. As representative examples of SEM images of the pressure-bonded bodies of Examples 1 to 3 and Comparative Examples 1 to 4, SEM images at a magnification of 500 times for the pressure-bonded bodies of Example 2 and Comparative Example 2 are shown in Figures 1 and 2, respectively, and SEM images at a magnification of 1000 times for the pressure-bonded bodies of Example 1 and Comparative Example 1 are shown in Figures 3 and 4, respectively.

[0077] The average fiber diameter of the PTFE fibrils was measured from the obtained SEM image. The average fiber diameter was calculated by randomly selecting 20 fibrils from the obtained SEM image, measuring the fiber diameter of each fibril, and averaging the results. The results are shown in Table 1. In addition, 40 fibrils were randomly selected from the obtained SEM image, the angle of each of these fibrils relative to the PFA fiber direction was measured, and the ratio of the number of fibrils oriented at 45 to 90 degrees relative to the PFA fiber direction (the ratio of fibrils oriented approximately perpendicular to the substrate fiber) to the number of these 40 fibrils was calculated. These results are shown in Table 1.

[0078] In the pressure-bonded bodies obtained in Examples 1 to 3, adjacent PFA fibers were bonded to each other by PTFE fibrils in a direction approximately perpendicular to the fiber direction, and the PFA fibers were integrated. Specifically, in the pressure-bonded body obtained in Example 1, PTFE fibrils of about several tens of nm (minimum fiber diameter: 40 nm, average fiber diameter: 80 nm) were bonded to connect the PFA fibers. In addition, in Examples 2 and 3, fibrils with a fiber diameter of about 0.2 to 0.3 μm were also generated. In addition, in the pressure-bonded bodies obtained in Examples 1 to 3, the number of fibrils oriented at 45 to 90° and the number of fibrils oriented at 80 to 90° to the PFA fiber direction were almost the same. On the other hand, in the pressed bodies obtained in Comparative Examples 1 to 4, the PTFE fibrils were not bonded to connect the PFA fibers, and as shown in Figure 4, it was confirmed that primary PTFE particles with an average particle size of about 0.2 μm derived from the PTFE dispersion were deposited on the PFA fibers and in the gaps between the fibers.

[0079] FIG. 5 shows an image of the cross-sectional structure of the pressure-bonded body obtained in Comparative Example 5 observed at a magnification of 500 times using the same SEM as above. In the compressed body obtained in Comparative Example 5, the fibers were heat-fused to eliminate voids and turn into a film, making the use of the fibers meaningless.

[0080] 2. Thickness measurement The thickness of the produced pressure-bonded body was measured using a micrometer (LITEMATIC VL-50, manufactured by Mitutoyo Corp.) The results are shown in Table 1.

[0081] 3. Measurement of maximum press-in resistance To examine the mechanical properties of the produced pressure-bonded body, a puncture test was performed using a universal tensile tester (EZ-test, manufactured by Shimadzu Corporation). Specifically, a φ20mm crimped body was attached to a dedicated piercing table with a φ12mm hole, and the crimped body was pierced at a speed of 1mm / s with a φ1mm piercing rod with a tip R of 0.5mm, and the maximum press-in resistance was calculated. The results are shown in Table 1.

[0082] [Table 1]

[0083] In the bonded body obtained in the examples, adjacent PFA fibers are integrated by the PTFE fibrils, so that the resistance value during thrusting is large. According to one embodiment of the present invention, a strong bonded body with excellent mechanical strength could be easily obtained.

[0084] 4. Measurement of thermal dimensional changes in the bonded body In order to confirm the degree of peeling between fibers due to heat in the produced laminate, the laminate was heated for 1 hour in an electric furnace set at 260°C, and the thickness of the laminate was measured before and after the heating in the same manner as in 2. The results are shown in Table 2.

[0085] [Table 2]

[0086] It is presumed that in the bonded body obtained in the examples, even when heated to 260°C, adjacent PFA fibers are integrated by the PTFE fibrils, thereby suppressing peeling of the PFA fibers due to thermal expansion. 6 and 7 show external appearance photographs of the pressure-bonded bodies of Example 2 and Comparative Example 2, respectively, as representative examples of the pressure-bonded bodies of Examples 1 to 3 and Comparative Examples 1 to 4. From these figures, it can be seen that in the examples, pressure-bonded bodies having desired shapes in which fraying of fibers and the like was suppressed were obtained.

Claims

1. A pressure-bonded body of at least one substrate selected from the group consisting of a nonwoven fabric, a stretched porous membrane, and a fiber, The substrate is made of a material other than polytetrafluoroethylene, such as -CF 2 A substrate containing a fluororesin having a - group content of 85% by mass or more, The fibers constituting the base material are bonded to each other by polytetrafluoroethylene fibrils, and the ratio of the number of fibrils oriented at 45 to 90° to the fiber direction constituting the base material to the total number of the fibrils is 50% or more. Crimp body.

2. The pressure-bonded body according to claim 1, wherein the content of the polytetrafluoroethylene is 0.2 to 12 mass% relative to 100 mass% of the base material.

3. The pressure-bonded body according to claim 1 or 2, wherein the average fiber diameter of the fibrils is 10 nm to 1 μm.

4. The substrate comprises at least one fluororesin selected from the group consisting of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether copolymer, fluoroethylene-vinyl ether copolymer and poly(chlorotrifluoroethylene). The pressure-bonded body according to any one of claims 1 to 3.

5. At least one substrate selected from the group consisting of a nonwoven fabric, a stretched porous membrane, and a fiber, Polytetrafluoroethylene particles; Carbon dioxide in liquid, gas-liquid mixture or near-liquid state A method for producing a pressure-bonded body, comprising the step of:

6. The step 1 comprises: A step 1a of contacting at least one substrate selected from the group consisting of a nonwoven fabric, an expanded porous membrane, and a fiber, and a polytetrafluoroethylene dispersion with liquid or gaseous carbon dioxide and applying pressure; or A step 1b of contacting at least one member selected from the group consisting of nonwoven fabric, stretched porous membrane, and fiber with a polytetrafluoroethylene dispersion, and then contacting the resulting dried body with liquid or gaseous carbon dioxide and applying pressure. The method for producing a pressure-bonded body according to claim 5,

7. The method for producing a pressure-bonded body according to claim 5 or 6, wherein the pressure-bonded body has a structure in which the base material is bonded with polytetrafluoroethylene fibrils.

8. The method for producing a pressure-bonded body according to claim 7, wherein the ratio of the number of fibrils oriented at an angle of 0 to 45° to the pressure-bonding direction to the total number of fibrils is 50% or more.

9. The method for producing a pressure-bonded body according to any one of claims 5 to 8, wherein the content of polytetrafluoroethylene in the pressure-bonded body is 0.2 to 12 mass% with respect to 100 mass% of the base material in the pressure-bonded body.

10. The method for producing a pressure-bonded body according to claim 7 or 8, wherein the average fiber diameter of the fibrils is 10 nm to 1 μm.

11. The method for producing a pressure-bonded body according to any one of claims 5 to 10, wherein the base material comprises at least one fluororesin selected from the group consisting of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether copolymer, fluoroethylene-vinyl ether copolymer and poly(chlorotrifluoroethylene).

Citation Information

Patent Citations

  • Packing contained composite material, sheet and circuit board containing same

    CN106928744A

  • surface treatment

    JP2002511907A

  • Nonwoven fabric and method for manufacturing nonwoven fabric

    JP2012188774A

  • Application and activation of durable water repellents using densifying fluids

    JP2016513191A

  • Porous PFA sheet

    WO2011105414A1