A preparation method of pps diaphragm for hydrophilic water electrolysis
By melt-spinning zirconia and polyphenylene sulfide materials and combining them with an aramid core film, combined with the spunlace process, the pps separator is prepared, which solves the deficiencies of the existing separators in terms of ion permeability, mechanical strength and air tightness. Efficient electrolysis and gas purity improvement are achieved.
Patent Information
- Application Number
- CN202410087625.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-22
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-01-22
AI Technical Summary
The existing alkaline water electrolyzer diaphragm has deficiencies in ion permeability, mechanical strength, air tightness and electrical insulation, which affects electrolysis efficiency and gas purity.
Zirconium oxide and polyphenylene sulfide materials are mixed and melt-spun, and the surface is modified after spinning and weaving. The aramid core film is clamped for hot calendering, and combined with the spunlace process to prepare the pps separator for hydrophilic electrolysis of water.
The mechanical strength, hydrophilicity and mechanical properties of the separator are improved, the ion conduction efficiency and gas barrier properties are enhanced, and the life of the separator is extended.
Smart Images

Figure BDA0004675552980000091
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials, and in particular relates to a method for preparing a pps diaphragm for hydrophilic water electrolysis. Background Art
[0002] Alkaline water electrolyzer hydrogen production is the most mature water electrolysis hydrogen production technology so far. Its advantages of simple operation and high efficiency make it widely used in industry. The diaphragm used for alkaline water electrolysis should have good ion permeability, mechanical strength, air tightness, electrical insulation and suitable electrolyte permeability. Among them, ion permeability directly affects the electrolysis efficiency of the alkaline water electrolyzer of the diaphragm used. Improving the ion permeability of the diaphragm can reduce the surface resistance of the diaphragm, thereby improving the electrolysis efficiency of the alkaline water electrolyzer. Mechanical strength requires the diaphragm to have good mechanical strength so that it can withstand the friction between the electrodes and the diaphragm of the electrolyzer. Air tightness requires the diaphragm to have the performance of blocking gas, and the gas generated by electrolysis cannot pass through the diaphragm, that is, the diaphragm only allows ions to pass through. Electrical insulation means that the diaphragm cannot conduct electricity and needs to be in an insulating state.
[0003] Polyphenylene sulfide (PPS) is a new type of membrane material, which is a thermoplastic resin with excellent high temperature resistance, solvent resistance, acid and alkali corrosion resistance, radiation resistance, flame retardancy, and good mechanical and electrical properties. It can be used in acidic, alkaline and organic solvents for a long time at high temperature, so PPS fiber can directly handle organic solvents as a membrane material. PPS fiber diaphragm must have good and stable airtightness to be able to operate stably for a long time, so as to prevent the passage of gas molecules and bubbles, thereby effectively preventing the mutual mixing of anode side gas and cathode side gas, thereby ensuring gas purity. The present invention provides a preparation method of a pps diaphragm for hydrophilic electrolysis of water. Summary of the invention
[0004] The invention discloses a preparation method of a pps diaphragm for hydrophilic water electrolysis, which comprises the steps of: mixing zirconium oxide and polyphenylene sulfide materials and then melt-spinning them, then spinning and weaving them to obtain a diaphragm, surface-modifying the diaphragm to obtain a surface film, then mixing polyphenylene sulfide and aramid materials and melt-spinning them, then spinning and weaving them to obtain a core film, hot-calendering the surface diaphragm and the core film to obtain a composite diaphragm, and then performing a spunlace process to obtain the pps diaphragm for hydrophilic water electrolysis. The diaphragm obtained by the invention has high mechanical strength and good hydrophilicity.
[0005] The specific plan is as follows:
[0006] The present invention provides a method for preparing a hydrophilic pps diaphragm for water electrolysis, characterized in that it comprises:
[0007] 1) Mixing polyphenylene sulfide and zirconium oxide nanoparticles uniformly, melt blending and extruding granulation, and melt spinning to obtain modified pps fibers with an average diameter of 8-12 μm; weaving the fibers into yarns, and weaving them into fabrics through a loom;
[0008] 2) Mixing polyphenylene sulfide and aramid material and then melt spinning to obtain fibers with an average diameter of 8-12 μm; spinning the fibers into yarns, and weaving them into fabrics through a loom;
[0009] 3) dissolving imidazole-2-carboxaldehyde in deionized water containing polyvinyl pyrrolidone to prepare an imidazole-2-carboxaldehyde solution; adding the imidazole-2-carboxaldehyde solution to a tert-butanol solution containing zinc nitrate, wherein the mass ratio of imidazole-2-carboxaldehyde to zinc nitrate is 1:2, to obtain a MOFs modified solution;
[0010] 4) immersing the membrane obtained in step 1 into the modified solution of step 3, drying to obtain a modified membrane, and then hot-pressing the membrane obtained in step 2 between two layers of modified membranes and placing them in deionized water for rapid cooling;
[0011] 5) The membrane obtained in step 4 is subjected to a hydroentanglement process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis membrane.
[0012] Furthermore, in step 1), polyphenylene sulfide and zirconium oxide nanoparticles with an average particle size of 40-60 nm are mixed in a mass ratio of 100:2-5.
[0013] Furthermore, in step 2), polyphenylene sulfide and aramid material are mixed in a mass ratio of 100:3-10.
[0014] Furthermore, the melt spinning parameters of step 1 and step 2 are: melt temperature of 280-300°C, stretching temperature of 100-120°C, spinning speed of 800-1000 m / s
[0015] Furthermore, in step 1 and step 20, the linear density of the yarn is 100-150 tex; the gram weight of the fabric is 200-600 g / m 2
[0016] Furthermore, in step 3), imidazole-2-carboxaldehyde is dissolved in deionized water containing 2-4wt% polyvinyl pyrrolidone to prepare an imidazole-2-carboxaldehyde solution with a concentration of 1-1.5wt%; the imidazole-2-carboxaldehyde solution is added to an equal volume of a tert-butanol solution containing 2-3wt% zinc nitrate, wherein the mass ratio of imidazole-2-carboxaldehyde to zinc nitrate is 1:2, to obtain a MOFs modified solution.
[0017] Furthermore, in step 4), the membrane immersion time is 30-60 min, the deionized water temperature is 0° C., wherein the hot pressing temperature is 80-100° C., the pressure is 3-5 MPa, and the hot pressing time is 30-60 s.
[0018] Furthermore, the water jet pressure is 60-120 bar.
[0019] A pps diaphragm for hydrophilic water electrolysis, wherein the diaphragm is prepared by adopting the preparation method.
[0020] The present invention has the following beneficial effects:
[0021] Compared with the prior art, the beneficial effects of the present invention are:
[0022] 1) Zirconia-modified polyphenylene sulfide fibers have good hydrophilicity, so they can be better combined with MOFs-modified solutions. The combined materials can achieve better bonding strength with the core membrane during the hot pressing process.
[0023] 2) The core layer diaphragm is made of polyphenylene sulfide and aramid materials, which provide higher strength for the diaphragm material. At the same time, the rapid condensation process after hot pressing can reduce the degree of crystallization in the diaphragm and improve the mechanical properties of the diaphragm;
[0024] 3) After the membrane is hot-pressed, the pore structure of the fiber is changed, and the subsequent water entanglement causes the fibers in the yarn to shift and re-optimize the pore structure.
[0025] 4) The polyphenylene sulfide fiber fabric type alkaline water electrolysis diaphragm prepared by the preparation method of the present invention has excellent mechanical properties, good hydrophilicity, long service life and high ion conduction efficiency. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with specific embodiments. However, the protection scope of the present invention is not limited to the following embodiments, and any non-essential adjustments and modifications made to the present invention based on the above invention content still fall within the protection scope of the present invention.
[0027] Example 1
[0028] 1) polyphenylene sulfide and zirconium oxide nanoparticles with an average particle size of 40 nm are mixed uniformly in a mass ratio of 100:2, melt blended and extruded into granules, and melt spun, and the melt spinning parameters are: melting temperature of 280°C, stretching temperature of 100°C, spinning speed of 800m / s, to obtain modified pps fibers with an average diameter of 10μm; the fibers are spun into yarns, and woven into fabrics by a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0029] 2) melt spinning polyphenylene sulfide and aramid material at a mass ratio of 100:3, melt spinning parameters are: melting temperature of 300°C, stretching temperature of 120°C, spinning speed of 800m / s, to obtain fibers with an average diameter of 10μm; weaving the fibers into yarns, weaving them into fabrics through a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0030] 3) dissolving imidazole-2-carboxaldehyde in deionized water containing 2 wt % polyvinyl pyrrolidone to prepare a 1 wt % imidazole-2-carboxaldehyde solution; adding the imidazole-2-carboxaldehyde solution to an equal volume of a tert-butanol solution containing 2 wt % zinc nitrate to obtain a MOFs modified solution;
[0031] 4) immersing the membrane obtained in step 1 in the modified solution of step 3 for 45 minutes, and then vacuum drying to obtain a modified membrane, and then hot-pressing the two modified membranes to clamp the membrane obtained in step 2 and cool it in deionized water at 0° C., wherein the hot-pressing temperature is 100° C., the pressure is 4 MPa, and the hot-pressing time is 40 seconds;
[0032] 5) The membrane obtained in step 4 is subjected to a hydroentanglement process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis membrane, wherein the hydroentanglement pressure is 100 bar.
[0033] Example 2
[0034] 1) polyphenylene sulfide and zirconium oxide nanoparticles with an average particle size of 60 nm are mixed uniformly in a mass ratio of 100:5, melt blended and extruded into granules, and melt spun, and the melt spinning parameters are: melting temperature of 280°C, stretching temperature of 100°C, spinning speed of 800m / s, to obtain modified pps fibers with an average diameter of 10μm; the fibers are spun into yarns, and woven into fabrics by a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0035] 2) melt spinning polyphenylene sulfide and aramid material at a mass ratio of 100:10, the melt spinning parameters are: melting temperature of 300°C, stretching temperature of 120°C, spinning speed of 800m / s, to obtain fibers with an average diameter of 10μm; spinning the fibers into yarns, and weaving them into fabrics through a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0036] 3) dissolving imidazole-2-carboxaldehyde in deionized water containing 4 wt% polyvinyl pyrrolidone to prepare an imidazole-2-carboxaldehyde solution with a concentration of 1.5 wt%; adding the imidazole-2-carboxaldehyde solution to an equal volume of a tert-butanol solution containing 3 wt% zinc nitrate to obtain a MOFs modified solution;
[0037] 4) immersing the membrane obtained in step 1 in the modified solution of step 3 for 45 minutes, and then vacuum drying to obtain a modified membrane, and then hot-pressing the two modified membranes to clamp the membrane obtained in step 2 and cool it in deionized water at 0° C., wherein the hot-pressing temperature is 100° C., the pressure is 4 MPa, and the hot-pressing time is 40 seconds;
[0038] 5) The membrane obtained in step 4 is subjected to a hydroentanglement process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis membrane, wherein the hydroentanglement pressure is 100 bar.
[0039] Example 3
[0040] 1) polyphenylene sulfide and zirconium oxide nanoparticles with an average particle size of 50 nm are mixed uniformly in a mass ratio of 100:3, melt blended and extruded into granules, and melt spun, and the melt spinning parameters are: melting temperature of 280°C, stretching temperature of 100°C, spinning speed of 800m / s, to obtain modified pps fibers with an average diameter of 10μm; the fibers are spun into yarns, and woven into fabrics by a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0041] 2) melt spinning polyphenylene sulfide and aramid material at a mass ratio of 100:5, melt spinning parameters are: melting temperature of 300°C, stretching temperature of 120°C, spinning speed of 800m / s, to obtain fibers with an average diameter of 10μm; spinning the fibers into yarns, weaving them into fabrics through a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0042] 3) dissolving imidazole-2-carboxaldehyde in deionized water containing 3 wt% polyvinyl pyrrolidone to prepare an imidazole-2-carboxaldehyde solution with a concentration of 1.2 wt%; adding the imidazole-2-carboxaldehyde solution to an equal volume of a tert-butanol solution containing 2.4 wt% zinc nitrate to obtain a MOFs modified solution;
[0043] 4) immersing the membrane obtained in step 1 in the modified solution of step 3 for 45 minutes, and then vacuum drying to obtain a modified membrane, and then hot-pressing the two modified membranes to clamp the membrane obtained in step 2 and cool it in deionized water at 0° C., wherein the hot-pressing temperature is 100° C., the pressure is 4 MPa, and the hot-pressing time is 40 seconds;
[0044] 5) The membrane obtained in step 4 is subjected to a hydroentanglement process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis membrane, wherein the hydroentanglement pressure is 100 bar.
[0045] Example 4
[0046] 1) polyphenylene sulfide and zirconium oxide nanoparticles with an average particle size of 50 nm are mixed uniformly in a mass ratio of 100:4, melt blended and extruded into granules, and melt spun, and the melt spinning parameters are: melting temperature of 280°C, stretching temperature of 100°C, spinning speed of 800m / s, to obtain modified pps fibers with an average diameter of 10μm; the fibers are spun into yarns, and woven into fabrics by a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0047] 2) melt spinning polyphenylene sulfide and aramid material at a mass ratio of 100:8, melt spinning parameters are: melting temperature of 300°C, stretching temperature of 120°C, spinning speed of 800m / s, to obtain fibers with an average diameter of 10μm; weaving the fibers into yarns, weaving them into fabrics through a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0048] 3) dissolving imidazole-2-carboxaldehyde in deionized water containing 3 wt% polyvinyl pyrrolidone to prepare an imidazole-2-carboxaldehyde solution with a concentration of 1.4 wt%; adding the imidazole-2-carboxaldehyde solution to an equal volume of a tert-butanol solution containing 2.8 wt% zinc nitrate to obtain a MOFs modified solution;
[0049] 4) immersing the membrane obtained in step 1 in the modified solution of step 3 for 45 minutes, and then vacuum drying to obtain a modified membrane, and then hot-pressing the two modified membranes to clamp the membrane obtained in step 2 and cool it in deionized water at 0° C., wherein the hot-pressing temperature is 100° C., the pressure is 4 MPa, and the hot-pressing time is 40 seconds;
[0050] 5) The membrane obtained in step 4 is subjected to a hydroentanglement process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis membrane, wherein the hydroentanglement pressure is 100 bar.
[0051] Comparative Example 1
[0052] 1) melt spinning polyphenylene sulfide, melt spinning parameters are: melting temperature of 280 ° C, stretching temperature of 100 ° C, spinning speed of 800 m / s, to obtain modified pps fiber with an average diameter of 10 μm; spinning the fiber into yarn, and weaving it into fabric through a loom, the yarn has a linear density of 120 tex; the fabric has a gram weight of 300 g / m 2 ;
[0053] 2) melt spinning polyphenylene sulfide and aramid material at a mass ratio of 100:8, melt spinning parameters are: melting temperature of 300°C, stretching temperature of 120°C, spinning speed of 800m / s, to obtain fibers with an average diameter of 10μm; weaving the fibers into yarns, weaving them into fabrics through a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0054] 3) The two layers of the diaphragm obtained in step 1 are clamped with the diaphragm obtained in step 2, and then hot-pressed and placed in deionized water at 0° C. for cooling, wherein the hot-pressing temperature is 100° C., the pressure is 4 MPa, and the hot-pressing time is 40 s;
[0055] 4) The membrane obtained in step 3 is subjected to a hydroentanglement process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis membrane, wherein the hydroentanglement pressure is 100 bar.
[0056] Comparative Example 2
[0057] 1) melt spinning polyphenylene sulfide, melt spinning parameters are: melting temperature of 280 ° C, stretching temperature of 100 ° C, spinning speed of 800 m / s, to obtain modified pps fiber with an average diameter of 10 μm; spinning the fiber into yarn, and weaving it into fabric through a loom, the yarn has a linear density of 120 tex; the fabric has a gram weight of 300 g / m 2 ;
[0058] 2) melt spinning polyphenylene sulfide and aramid material at a mass ratio of 100:8, melt spinning parameters are: melting temperature of 300°C, stretching temperature of 120°C, spinning speed of 800m / s, to obtain fibers with an average diameter of 10μm; weaving the fibers into yarns, weaving them into fabrics through a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0059] 3) dissolving imidazole-2-carboxaldehyde in deionized water containing 3 wt% polyvinyl pyrrolidone to prepare an imidazole-2-carboxaldehyde solution with a concentration of 1.4 wt%; adding the imidazole-2-carboxaldehyde solution to an equal volume of a tert-butanol solution containing 2.8 wt% zinc nitrate to obtain a MOFs modified solution;
[0060] 4) immersing the membrane obtained in step 1 in the modified solution of step 3 for 45 minutes, and then vacuum drying to obtain a modified membrane, and then hot-pressing the two modified membranes to clamp the membrane obtained in step 2 and cool it in deionized water at 0° C., wherein the hot-pressing temperature is 100° C., the pressure is 4 MPa, and the hot-pressing time is 40 seconds;
[0061] 5) The membrane obtained in step 4 is subjected to a hydroentanglement process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis membrane, wherein the hydroentanglement pressure is 100 bar.
[0062] Comparative Example 3
[0063] 1) polyphenylene sulfide and zirconium oxide nanoparticles with an average particle size of 50 nm are mixed uniformly in a mass ratio of 100:4, melt blended and extruded into granules, and melt spun, and the melt spinning parameters are: melting temperature of 280°C, stretching temperature of 100°C, spinning speed of 800m / s, to obtain modified pps fibers with an average diameter of 10μm; the fibers are spun into yarns, and woven into fabrics by a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0064] 2) melt spinning polyphenylene sulfide and aramid material at a mass ratio of 100:8, melt spinning parameters are: melting temperature of 300°C, stretching temperature of 120°C, spinning speed of 800m / s, to obtain fibers with an average diameter of 10μm; weaving the fibers into yarns, weaving them into fabrics through a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0065] 3) The two layers of the diaphragm obtained in step 1 are clamped with the diaphragm obtained in step 2, and then hot-pressed and placed in deionized water at 0° C. for cooling, wherein the hot-pressing temperature is 100° C., the pressure is 4 MPa, and the hot-pressing time is 40 s;
[0066] 4) The membrane obtained in step 3 is subjected to a hydroentanglement process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis membrane, wherein the hydroentanglement pressure is 100 bar.
[0067] Comparative Example 4
[0068] 1) polyphenylene sulfide and zirconium oxide nanoparticles with an average particle size of 50 nm are mixed uniformly in a mass ratio of 100:4, melt blended and extruded into granules, and melt spun, and the melt spinning parameters are: melting temperature of 280°C, stretching temperature of 100°C, spinning speed of 800m / s, to obtain modified pps fibers with an average diameter of 10μm; the fibers are spun into yarns, and woven into fabrics by a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0069] 2) melt spinning polyphenylene sulfide and aramid material at a mass ratio of 100:8, melt spinning parameters are: melting temperature of 300°C, stretching temperature of 120°C, spinning speed of 800m / s, to obtain fibers with an average diameter of 10μm; weaving the fibers into yarns, weaving them into fabrics through a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0070] 3) dissolving imidazole-2-carboxaldehyde in deionized water containing 3 wt% polyvinyl pyrrolidone to prepare an imidazole-2-carboxaldehyde solution with a concentration of 1.4 wt%; adding the imidazole-2-carboxaldehyde solution to an equal volume of a tert-butanol solution containing 2.8 wt% zinc nitrate to obtain a MOFs modified solution;
[0071] 4) immersing the membrane obtained in step 1 in the modified solution of step 3 for 45 minutes, and then vacuum drying to obtain a modified membrane, and then hot pressing the membrane obtained in step 2 with two layers of modified membranes and cooling naturally, wherein the hot pressing temperature is 100° C., the pressure is 4 MPa, and the hot pressing time is 40 seconds;
[0072] 5) The membrane obtained in step 4 is subjected to a hydroentanglement process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis membrane, wherein the hydroentanglement pressure is 100 bar.
[0073] Comparative Example 5
[0074] 1) polyphenylene sulfide and zirconium oxide nanoparticles with an average particle size of 50 nm are mixed uniformly in a mass ratio of 100:4, melt blended and extruded into granules, and melt spun, and the melt spinning parameters are: melting temperature of 280°C, stretching temperature of 100°C, spinning speed of 800m / s, to obtain modified pps fibers with an average diameter of 10μm; the fibers are spun into yarns, and woven into fabrics by a loom, wherein the yarn has a linear density of 120tex; the fabric has a gram weight of 300g / m 2 ;
[0075] 2) melt spinning polyphenylene sulfide, melt spinning parameters are: melting temperature of 300 ° C, stretching temperature of 120 ° C, spinning speed of 800 m / s, to obtain fibers with an average diameter of 10 μm; spinning the fibers into yarns, and weaving them into fabrics through a loom, wherein the yarn has a linear density of 120 tex; the fabric has a gram weight of 300 g / m 2 ;
[0076] 3) dissolving imidazole-2-carboxaldehyde in deionized water containing 3 wt% polyvinyl pyrrolidone to prepare an imidazole-2-carboxaldehyde solution with a concentration of 1.4 wt%; adding the imidazole-2-carboxaldehyde solution to an equal volume of a tert-butanol solution containing 2.8 wt% zinc nitrate to obtain a MOFs modified solution;
[0077] 4) immersing the membrane obtained in step 1 in the modified solution of step 3 for 45 minutes, and then vacuum drying to obtain a modified membrane, and then hot-pressing the two modified membranes to clamp the membrane obtained in step 2 and cool it in deionized water at 0° C., wherein the hot-pressing temperature is 100° C., the pressure is 4 MPa, and the hot-pressing time is 40 seconds;
[0078] 5) The membrane obtained in step 4 is subjected to a hydroentanglement process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis membrane, wherein the hydroentanglement pressure is 100 bar.
[0079] Tests and Results
[0080] 1. Contact angle measurement: The JYSP-180 dynamic contact angle measuring device is used to characterize the hydrophilicity of the diaphragm, and the electrolyte contact angle of the diaphragm is measured in combination with the software.
[0081] 2. Liquid absorption rate is measured according to the provisions of national standard GB / T21655.1-2008.
[0082] 3. The surface resistance and breaking strength shall comply with the national electronic industry standard SJ-T 10171.
[0083] 4. Bubble point test method: Cut the diaphragm into small pieces, soak it with high-purity water, and put it into the bubble pressure membrane pore size analyzer (BSD-PB) for testing. Apply gas pressure on one side of the membrane. When a gas flow of 1 mL / min is detected on the other side of the membrane, the pressure is regarded as the bubble point of the diaphragm.
[0084] Table 1
[0085]
[0086] Tests and Results
[0087] Zirconium oxide-modified polyphenylene sulfide fibers have good hydrophilicity, which enables them to better combine with the MOFs modified solution. The combined material can achieve better bonding strength with the core layer diaphragm during the hot pressing process, thereby improving the mechanical properties and gas barrier properties of the diaphragm. Aramid provides higher strength for the diaphragm material, and the extremely rapid condensation process after hot pressing can improve the mechanical properties of the diaphragm.
[0088] Although the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention.
Claims
1. A method for preparing a pps diaphragm for hydrophilic water electrolysis, characterized in that: include: 1) polyphenylene sulfide and zirconium oxide nanoparticles with an average particle size of 40-60 nm are mixed in a mass ratio of 100:2-5, melt blended and extruded into granules, and melt spun to obtain modified pps fibers with an average diameter of 8-12 μm; the fibers are spun into yarns, and the yarns are woven into fabrics by a loom; 2) Mixing polyphenylene sulfide and aramid material in a mass ratio of 100:3-10 and melt spinning to obtain fibers with an average diameter of 8-12 μm; spinning the fibers into yarns, and weaving them into fabrics through a loom; 3) dissolving imidazole-2-carboxaldehyde in deionized water containing 2-4 wt% polyvinyl pyrrolidone to prepare an imidazole-2-carboxaldehyde solution with a concentration of 1-1.5 wt%; adding the imidazole-2-carboxaldehyde solution to an equal volume of a tert-butanol solution containing 2-3 wt% zinc nitrate, wherein the mass ratio of imidazole-2-carboxaldehyde to zinc nitrate is 1:2, to obtain a MOFs modified solution; 4) immersing the membrane obtained in step 1 into the modified solution of step 3 for 30-60 min, drying to obtain a modified membrane, and then hot-pressing the membrane obtained in step 2 with two layers of modified membranes, wherein the hot-pressing temperature is 80-100° C., the pressure is 3-5 MPa, and the hot-pressing time is 30-60 s, and then placed in deionized water at 0° C. for rapid cooling; 5) The membrane obtained in step 4 is subjected to a hydroentanglement process to obtain a polyphenylene sulfide fiber fabric type alkaline water electrolysis membrane.
2. A preparation method as claimed in claim 1, characterized in that The melt spinning parameters of step 1 and step 2 are: melting temperature of 280-300°C, stretching temperature of 100-120°C, and spinning speed of 800-1000m / s.
3. A preparation method as claimed in claim 1, characterized in that In step 1 and step 2, the linear density of the yarn is 100-150 tex; the gram weight of the fabric is 200-600 g / m 2 .
4. The preparation method according to claim 1, characterized in that : In step 5), the water jet pressure is 60-120 bar.
5. A pps diaphragm for hydrophilic water electrolysis, characterized in that: The diaphragm is prepared by the preparation method according to any one of claims 1 to 4.
Citation Information
Cited By
Hydrophilic modified polyphenylene sulfide fabric diaphragm and preparation method thereof
CN119843491A
A hydrophilic modified polyphenylene sulfide fabric diaphragm and preparation method thereof
CN119843491B
Modified preparation method of polyphenylene sulfide composite diaphragm and application of polyphenylene sulfide composite diaphragm in alkaline electrolytic cell
CN122382657A