Multi-element alloy electrode catalyst for hydrogen production by alkaline electrolysis of water and preparation method of multi-element alloy electrode catalyst

By using multi-alloy materials such as nickel, chromium, molybdenum, cobalt, niobium and plasma spraying processes, an aluminum-encapsulated transition layer and ultrafine catalytic layer are formed, which solves the problems of short life of Rayney nickel catalyst and the potential rise, and the electrode potential is achieved Reduce and prolong the catalyst life.

CN118996472APending Publication Date: 2024-11-22BEIJING HUAYI HYDROGEN TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411111253.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing Rainey nickel catalyst has a short catalytic life and a sharp increase in the electrode potential during the electrolytic hydrogen production process, resulting in a decline in catalytic performance, and lacks an effective solution that can simultaneously reduce the electrode potential and extend the catalyst life.

Method used

Using multi-alloy materials such as nickel, chromium, molybdenum, cobalt, niobium, etc., spherical powder is prepared by aerosolization, and an aluminum-encapsulated transition layer and ultrafine catalytic layer are formed through plasma spraying to improve the bonding strength and corrosion resistance of the coating. , adapt to the electrolytic cell temperature and extend the catalyst life.

Benefits of technology

Effectively reduce the electrode potential, improve catalytic performance and corrosion resistance, extend the service life of the catalyst, and significantly improve the overall performance of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996472A_ABST
    Figure CN118996472A_ABST
Patent Text Reader

Abstract

The invention discloses a multi-element alloy electrode catalyst for hydrogen production by alkaline electrolysis of water and a preparation method of the multi-element alloy electrode catalyst, and relates to the technical field of electrode catalysts. The method comprises the following steps that firstly, multi-element alloy materials are prepared, and the multi-element alloy materials are smelted after being fully mixed; secondly, spherical multi-component alloy powder is prepared through gas atomization; thirdly, the powder material is treated; 4, spraying the electrode by adopting a plasma process; and 5, activating the sprayed electrode in a potassium hydroxide solution, cleaning the electrode after activation, and putting the electrode into an electrolytic cell for use. The multi-component alloy material contains nickel-chromium-molybdenum-cobalt-niobium, so that the electrode potential can be effectively reduced, the catalytic performance of an electrode can be effectively improved, the corrosion resistance of a catalyst is improved, and the service life of the catalyst is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrode catalysts, and in particular relates to a multi-element alloy electrode catalyst for producing hydrogen by alkaline water electrolysis and a preparation method thereof. Background Art

[0002] As a clean and efficient energy carrier, hydrogen energy has received extensive attention. However, the current production of hydrogen mainly relies on fossil fuels, which not only consumes a large amount of fossil resources but also aggravates environmental pollution. Therefore, it is of great significance to develop green and sustainable hydrogen production technology.

[0003] Hydrogen production from water electrolysis has become an important direction for future hydrogen production due to its clean and efficient advantages. The research and development of multi-element alloy electrode catalysts is the key to promoting the development of hydrogen production from water electrolysis technology.

[0004] At present, the electrode market mainly uses Raney nickel as an electrode catalyst. Although Raney nickel is cheap and easy to prepare, its catalytic performance is not optimal. Currently, many electrode manufacturers are trying to add other elements to Raney nickel to optimize its catalytic performance. Raney nickel and catalysts derived from Raney nickel have a huge shortcoming, that is, short catalytic life. Many electrolytic cells equipped with Raney nickel catalyst electrodes will have a sharp rise in potential after being put into use for a few months, and finally tend to the catalytic level of ordinary nickel mesh electrodes.

[0005] For example, the preparation method of the multi-catalyst and nickel wire mesh electrode for hydrogen production by alkaline water electrolysis with publication number CN117344334A adopts a multi-alloy method. In theory, the catalytic effect of the catalyst will be very good, but the spraying process of this scheme is poor and the coating bonding strength is poor. During the long-term operation of the electrode, the coating will peel off, thereby affecting the life of the catalyst and causing the potential to continue to rise.

[0006] Therefore, the current research and development direction of Raney nickel catalysts is to continue to reduce the electrode potential and to extend the catalytic life of the catalyst. Now there is an urgent need for a new type of Raney nickel catalyst electrode that can both reduce the electrode potential and extend the catalyst life. Based on this, a multi-element alloy electrode catalyst for hydrogen production by alkaline water electrolysis and a preparation method thereof are proposed. Summary of the invention

[0007] The object of the present invention is to provide a multi-element alloy electrode catalyst for hydrogen production by alkaline water electrolysis and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0008] In order to solve the above technical problems, the present invention is achieved through the following technical solutions:

[0009] The present invention is a method for preparing a multi-element alloy electrode catalyst for producing hydrogen by alkaline water electrolysis, comprising the following steps:

[0010] Step 1: prepare multi-element alloy materials, mix the multi-element alloy materials sufficiently and then smelt them;

[0011] Step 2: Produce spherical multi-element alloy powder by gas atomization;

[0012] Step 3: Process the powder material;

[0013] Step 4: Spray the electrode using plasma process;

[0014] Step 5: Place the sprayed electrode in potassium hydroxide solution for activation. After activation, clean it and put it into the electrolytic cell for use.

[0015] Furthermore, the multi-element alloy material in the first step is composed of the following raw materials:

[0016] Nickel, chromium, molybdenum, cobalt, niobium.

[0017] Furthermore, the mass percentage of each raw material in the multi-element alloy material is as follows:

[0018] Nickel 63%, chromium 15%, molybdenum 10%, cobalt 8%, niobium 4.

[0019] Furthermore, the processing of the powder material in the third step includes the following steps:

[0020] The spherical multi-element alloy powder with a size of 25-45 microns is coated with 5% aluminum to form a 5% aluminum-coated multi-element alloy powder, which is used as a transition layer and catalytic layer powder material of an electrode catalyst;

[0021] Spherical multi-element alloy powder with a particle size greater than 45 microns is crushed into ultrafine crushed multi-element alloy powder with a particle size less than 25 microns by ball milling, and mixed with ultrafine spherical multi-element alloy powder with a particle size less than 25 microns produced by atomization to form an ultrafine mixed multi-element alloy powder with a particle size less than 25 microns, which is then mixed with Raney nickel to serve as the catalytic layer multi-element alloy powder material of the electrode catalyst.

[0022] Furthermore, the fourth step of spraying the electrode with a plasma process includes the following steps:

[0023] A plasma spraying process is used to spray 5% aluminum-clad multi-element alloy powder onto the surface of the nickel mesh electrode pretreated by sandblasting to form a transition layer;

[0024] The mixed catalyst layer multi-element alloy powder material is sprayed onto the nickel mesh electrode containing the transition layer by a plasma spraying process to form an electrode catalyst layer.

[0025] The present invention has the following beneficial effects:

[0026] The multi-element alloy material of the present invention contains nickel, chromium, molybdenum, cobalt and niobium, which can effectively reduce the electrode potential, effectively improve the catalytic performance of the electrode, and improve the corrosion resistance of the catalyst, which is beneficial to prolonging the life of the catalyst; and through the combination of niobium, the coating can effectively adapt to the temperature of the electrolytic cell, and will not be affected by the temperature and cause the coating to peel off, further improving the life of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0028] Figure 1 is a preparation flow chart of the present invention;

[0029] Figure 2 It is a schematic diagram of the multi-element alloy powder material of the catalyst layer of the present invention;

[0030] Figure 3 It is a schematic diagram of the electrode of the present invention after being sprayed with aluminum-clad multi-element alloy powder;

[0031] Figure 4 It is a schematic diagram of the electrode of the present invention after the catalytic layer multi-element alloy powder material is sprayed;

[0032] Figure 5 It is a schematic diagram of the electrode after activation of the present invention;

[0033] Figure 6 This is a schematic diagram of the electrode of the present invention after running for a period of time. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Embodiment 1:

[0036] See also Figure 1-6 As shown, a method for preparing a multi-element alloy electrode catalyst for producing hydrogen by alkaline water electrolysis comprises the following steps:

[0037] Step 1: prepare multi-element alloy materials, which are composed of the following raw materials: nickel, chromium, molybdenum, cobalt, and niobium, and the mass percentage of each raw material is: nickel 63%, chromium 15%, molybdenum 10%, cobalt 8%, and niobium 4; then mix the multi-element alloy materials sufficiently and then smelt them;

[0038] Step 2: Produce spherical multi-element alloy powder by gas atomization;

[0039] Step 3: Processing the powder material, specifically, by encapsulating 25-45 micron spherical multi-element alloy powder with 5% aluminum to form 5% aluminum-encapsulated multi-element alloy powder as a transition layer and catalytic layer powder material of the electrode catalyst;

[0040] Spherical multi-element alloy powder with a particle size greater than 45 microns is crushed into ultrafine crushed multi-element alloy powder with a particle size less than 25 microns by ball milling, and mixed with ultrafine spherical multi-element alloy powder with a particle size less than 25 microns produced by gas atomization to form ultrafine mixed multi-element alloy powder with a particle size less than 25 microns, and then mixed with Raney nickel to serve as a catalyst layer multi-element alloy powder material for an electrode catalyst;

[0041] The multi-element alloy powder will form a coarse powder with a particle size greater than 45 microns during the powder making process. The coarse powder is ball-milled to form ultra-fine crushed multi-element alloy powder. The structure of the crushed powder is very complex, and there are a large number of nano-rough structures and a large number of catalytic points, which are very helpful in reducing the electrode potential. However, the fluidity of the crushed powder is very poor, so the amount mixed into the overall powder is small, adsorbed on Raney nickel, and the fluidity of Raney nickel is used to bring the crushed ultra-fine multi-element alloy powder into the plasma flame flow for spraying.

[0042] The powder is wrapped with aluminum as a transition layer powder. Conventional transition layer powder is 5% aluminum-coated nickel. The multi-element alloy powder of the present invention has an appropriate nickel content and still has a good transition effect when wrapped with aluminum. The bonding strength of the coating with a transition layer will be significantly improved, and the probability of peeling of the coating of the present invention will be greatly reduced. The Raney nickel coating will form a large number of pores after activation, further reducing the bonding strength of the coating. In an environment without a transition layer, the coating is very easy to peel off. After the coating peels off, it will also peel off in a large area with the peeling point as the center. With the protection of the transition layer, the Raney nickel catalytic layer will not be easy to peel off, and even after peeling off, it will not form a large area of ​​collapse.

[0043] In the absence of a transition layer, after the Raney nickel catalytic layer is peeled off, the catalytic performance of the exposed nickel mesh substrate will be very poor. The transition layer of the present invention adopts a multi-element alloy, and the coordination of multiple elements can effectively reduce the potential. Even if the Raney nickel coating is peeled off, the exposed multi-element alloy transition layer has very good catalytic performance. In addition, the multi-element alloy of the present invention has two elements, chromium and niobium, which can resist the corrosion of alkali solution and the temperature of the electrolytic cell, and can effectively extend the life of the transition layer. Even if the surface catalytic layer is completely peeled off like the catalytic layer of other electrodes, the transition layer can still continue to operate for many years, and the life of the transition layer is even 3 to 5 times that of the catalytic layer.

[0044] Step 4: After the powder is processed, a plasma spraying process is used to spray 5% aluminum-clad multi-element alloy powder onto the surface of the nickel mesh electrode pre-treated by sandblasting to form a transition layer. Since the nickel content in the multi-element alloy powder accounts for more than 60%, it will react with the aluminum coating layer during the spraying process. Just when the powder hits the nickel mesh electrode, a large amount of heat is generated, forming a local metallurgical bond with the nickel mesh electrode, which greatly improves the bonding strength of the coating and forms a transition layer connecting the nickel mesh electrode and the catalyst layer, ensuring the bonding strength of the catalyst layer;

[0045] The mixed catalyst layer multi-element alloy powder material is sprayed onto the nickel mesh electrode containing the transition layer by a plasma spraying process to form an electrode catalyst layer;

[0046] Step 5: Place the sprayed electrode in potassium hydroxide solution for activation. After activation, clean it and put it into the electrolytic cell for use.

[0047] See also Figure 2 As shown, the left side is a schematic diagram of aluminum-encapsulated multi-component alloy powder, and the right side is a schematic diagram of mixed multi-component alloy powder. In the aluminum-encapsulated multi-component alloy powder, aluminum is wrapped around the multi-component alloy powder, and the content is 5%.

[0048] See also Figure 3 As shown, a 5% aluminum-clad multi-element alloy powder is sprayed onto the surface of a nickel mesh electrode pretreated by sandblasting using plasma spraying technology to form a transition layer. Since the nickel content in the multi-element alloy powder is more than 60%, it will undergo an aluminothermic reaction with the aluminum coating during the spraying process. Just when the powder hits the nickel mesh electrode, a large amount of heat is generated, forming a local metallurgical bond with the nickel mesh electrode, greatly improving the bonding strength of the coating. Moreover, during the spraying process, aluminum and nickel at other locations undergo an aluminothermic reaction, forming an ablation surface on the surface of the multi-element alloy coating. The ablation surface is a nano-rough structure, which helps to improve the catalytic performance of the electrode and can effectively reduce the electrode potential.

[0049] The schematic diagram of the electrode after spraying the catalyst layer with multi-element alloy powder material is as follows Figure 4As shown, when the Raney nickel powder is directly applied on the substrate, the bonding strength will be poor. However, when it is applied on the transition layer, the bonding strength between the Raney nickel catalytic layer and the transition layer will be very good.

[0050] The schematic diagram of the electrode after activation is shown in Figure 5 As shown in the figure, during the activation process, aluminum will react violently with sodium hydroxide and be dissolved by sodium hydroxide. Other powder particles adhering to aluminum will be peeled off from the coating during this process. In the catalytic layer, the ablation surface formed by the reaction of aluminum and nickel will appear on the surface of the electrode, which is of great help in reducing the potential and improving the catalytic performance of the electrode. In the transition layer, pores will be formed after aluminum is dissolved.

[0051] The schematic diagram of the electrode after running for a period of time is as follows Figure 6 As shown in the figure, due to the large number of pores in the Raney nickel coating, the coating bonding strength is poor, and the local coating peels off due to the pores. After the local Raney nickel catalytic layer peels off, the transition layer under the catalytic layer will replace the catalyst to play a catalytic role. Since the transition layer is a multi-element alloy layer and the surface has a nano-ablation rough structure left after the thermite reaction, the transition layer still has a strong catalytic performance. If there is no transition layer, after the Raney nickel coating peels off, a large piece of the coating will peel off with the peeling point as the center. With the transition layer, even if the Raney nickel coating peels off locally, it will not cause a large piece of coating to peel off with the peeling point as the center.

[0052] Among them, nickel, molybdenum and cobalt are all commonly used materials for alkaline electrode catalysts, especially molybdenum. Adding a small amount of molybdenum can effectively improve the catalytic performance of the electrode. After adding chromium, the corrosion resistance of the catalyst will be further improved. Among the many factors that cause the failure of alkaline catalysts, one of them is that the catalyst is corroded by alkaline solution. After adding chromium to improve the corrosion resistance of the catalyst, it is beneficial to extend the life of the catalyst. Niobium is a rare metal that is widely used in aviation, aerospace, nuclear industry and other fields. Niobium can improve the comprehensive performance of the coating and has high temperature resistance. The temperature of the electrolytic cell is about 90 degrees, which is higher than normal temperature. At this temperature, the life of the coating will be affected and the bonding strength of the coating will be reduced. After adding niobium, the coating can effectively adapt to the temperature of the electrolytic cell and will not be affected by the temperature and cause the coating to peel off, which improves the life of the catalyst to a certain extent.

[0053] Embodiment 2:

[0054] See also Figure 1-6 As shown, a method for preparing a multi-element alloy electrode catalyst for producing hydrogen by alkaline water electrolysis, the specific steps are as follows:

[0055] Step 1: Accurately weigh the raw materials according to the mass percentage of nickel 63.5%, chromium 14.5%, molybdenum 10%, cobalt 7.5%, and niobium 4.5%, mix them evenly, and then perform vacuum melting under the protection of high-purity argon to ensure uniform alloy composition.

[0056] Step 2: The smelted alloy liquid is atomized by high-pressure gas to obtain spherical multi-element alloy powder with uniform particle size distribution.

[0057] Step 3: Select spherical multi-element alloy powder of 25-35 microns, and wrap it with 5% aluminum through chemical vapor deposition to form 5% aluminum-coated multi-element alloy powder.

[0058] The powder with a particle size greater than 45 microns is ball-milled to less than 25 microns, and mixed with the powder with a particle size less than 25 microns directly generated during the atomization process, and Raney nickel is added at a mass ratio of 1:1, and stirred evenly to form a catalytic layer powder.

[0059] Step 4: Pre-treat the nickel mesh electrode by sandblasting to enhance the surface roughness.

[0060] Using plasma spraying technology, 5% aluminum-clad multi-element alloy powder is first sprayed on the nickel mesh electrode to form a transition layer. The heat generated by the thermite reaction promotes the close bonding of the coating and the substrate.

[0061] Subsequently, the catalyst layer multi-element alloy powder is evenly sprayed onto the transition layer to form a dense catalyst layer.

[0062] Step 5: Place the sprayed electrode in a 30% potassium hydroxide solution, activate it at 80°C for 2 hours, and then rinse it thoroughly with deionized water to ensure no residue.

[0063] This significantly improves the bonding strength and catalytic efficiency of the electrode catalyst, prolongs the service life of the electrode, and is suitable for large-scale alkaline water electrolysis hydrogen production systems.

[0064] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0065] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the present invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a multi-element alloy electrode catalyst for producing hydrogen by alkaline water electrolysis, characterized in that: The following steps are involved: Step 1: prepare multi-element alloy materials, mix the multi-element alloy materials sufficiently and then smelt them; Step 2: Produce spherical multi-element alloy powder by gas atomization; Step 3: Process the powder material; Step 4: Spray the electrode using plasma process; Step 5: Place the sprayed electrode in potassium hydroxide solution for activation. After activation, clean it and put it into the electrolytic cell for use.

2. The method for preparing a multi-element alloy electrode catalyst for producing hydrogen by alkaline water electrolysis according to claim 1, characterized in that: In the first step, the multi-element alloy material is composed of the following raw materials: Nickel, chromium, molybdenum, cobalt, niobium.

3. The method for preparing a multi-element alloy electrode catalyst for producing hydrogen by alkaline water electrolysis according to claim 2, characterized in that: The mass percentages of the various raw materials in the multi-element alloy material are as follows: Nickel 63%, chromium 15%, molybdenum 10%, cobalt 8%, niobium 4.

4. The method for preparing a multi-element alloy electrode catalyst for producing hydrogen by alkaline water electrolysis according to claim 1, characterized in that: The third step of processing the powder material comprises the following steps: The spherical multi-element alloy powder with a size of 25-45 microns is coated with 5% aluminum to form a 5% aluminum-coated multi-element alloy powder, which is used as a transition layer and catalytic layer powder material of an electrode catalyst; Spherical multi-element alloy powder with a particle size greater than 45 microns is crushed into ultrafine crushed multi-element alloy powder with a particle size less than 25 microns by ball milling, and mixed with ultrafine spherical multi-element alloy powder with a particle size less than 25 microns produced by atomization to form an ultrafine mixed multi-element alloy powder with a particle size less than 25 microns, which is then mixed with Raney nickel to serve as the catalytic layer multi-element alloy powder material of the electrode catalyst.

5. The method for preparing a multi-element alloy electrode catalyst for producing hydrogen by alkaline water electrolysis according to claim 4, characterized in that: The fourth step of using a plasma process to spray the electrode comprises the following steps: A plasma spraying process is used to spray 5% aluminum-clad multi-element alloy powder onto the surface of the nickel mesh electrode pretreated by sandblasting to form a transition layer; The mixed catalyst layer multi-element alloy powder material is sprayed onto the nickel mesh electrode containing the transition layer by a plasma spraying process to form an electrode catalyst layer.

6. A multi-element alloy electrode catalyst for producing hydrogen by alkaline water electrolysis, characterized in that: The multi-element alloy electrode catalyst for producing hydrogen by alkaline water electrolysis is prepared by the preparation method according to any one of claims 1 to 5.

Citation Information

Cited By

  • Method for efficiently preparing high-performance and high-stability hydrogen production electrode

    CN121992334A

  • Electrode for alkaline water electrolysis and electrolysis cell comprising such an electrode

    DE102024135927A1

  • Electrode for alkaline water electrolysis, electrolysis cell comprising such an electrode and method for producing such an electrode

    WO2026119814A1