Manufacturing method of porous alumina plate
The method efficiently produces porous alumina plates with regularly arranged pores by using a mask body forming step and anodization, addressing inefficiencies and costs in existing methods.
Patent Information
- Application Number
- JP2020161290
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-25
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-09-25
AI Technical Summary
Existing methods for producing porous alumina with regularly arranged pores are inefficient, costly, and difficult to scale due to the need for high pressure texturing and long anodization times, especially for thin aluminum materials.
A manufacturing method involving a mask body forming step followed by anodization to create a porous alumina layer with regularly arranged pores, eliminating the need for high-pressure texturing and allowing for large-area production.
Enables efficient and cost-effective production of porous alumina plates with regularly arranged pores over a large area, reducing the need for high-pressure texturing and long anodization times.
Smart Images

Figure 0007560097000001 
Figure 0007560097000002 
Figure 0007560097000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a porous alumina having a plurality of pores. Board It relates to a manufacturing method. [Background technology]
[0002] Anodized porous alumina, obtained by anodizing aluminum in an acidic solution, has a hole array structure in which uniformly sized pores are arranged, and is therefore a functional material that is expected to have a wide range of applications, including as filters, catalyst supports, template materials, etc. One of the characteristics of this anodized porous alumina is that when anodization is performed under appropriate conditions, the pores self-organize to form a regular arrangement (self-organization process).
[0003] The periodicity of the pores in anodized porous alumina changes depending on the voltage during anodization, so it has become clear that it is possible to produce anodized porous alumina with regularly arranged pores by optimizing various conditions such as the type, concentration, and temperature of the electrolyte and the anodization time under each voltage condition.
[0004] For example, if an aluminum material is anodized for a long time under optimized conditions, and then the oxide film (porous alumina) that is formed is selectively dissolved and removed, an aluminum material with a regular pattern of pits can be obtained. Since such pits function as starting points for the generation of pores during anodization, by anodizing again using an aluminum material from which the oxide film has been dissolved and removed as described above, it is possible to obtain porous alumina with a regular arrangement of pores extending from the surface in the thickness direction (for example, Non-Patent Document 1).
[0005] However, in order to obtain porous alumina with regularly-arranged pores from the surface in the above-mentioned two-stage anodization process, the first stage of anodization must be performed for a long time, resulting in low throughput. It is also difficult to obtain porous alumina with pores arranged in an ideal shape, such as a triangular lattice or square lattice. Furthermore, with thin aluminum materials such as sputtered thin films formed on substrates such as Si, the first stage of anodization cannot be performed for a long time due to the thinness of the aluminum material, which means that the thickness of the aluminum material is limited.
[0006] On the other hand, it is also possible to prepare porous alumina in which pores are regularly arranged by previously texturing the surface of the aluminum material used for anodization to form depressions that function as starting points for pore generation (for example, Non-Patent Document 2). According to such a preparation method, it is not necessary to perform anodization for a long period of time under appropriate conditions, as in the above-mentioned self-organization process, and therefore highly regular porous alumina can be obtained efficiently.
[0007] Furthermore, by creating a mold to be used for texturing using artificial techniques such as electron beam lithography, it is believed possible to produce porous alumina in which the pores are arranged in ideal shapes, such as equilateral triangular or quadrangular lattices, which are difficult to form by self-organization processes. [Prior art documents] [Non-patent literature]
[0008] [Non-Patent Document 1] H. Masuda and M. Satoh, Jpn. J. Appl. Phys., 35, L126 (1996) [Non-Patent Document 2] H. Masuda, H. Yamada, M. Satoh, H. Asoh, M. Nakao, T. Tamamura, Appl. Phys. Lett., 71, 2770 (1997) Summary of the Invention [Problem to be solved by the invention]
[0009] However, the method for producing porous alumina disclosed in Non-Patent Document 2 had the problem that texturing to form depressions on the surface of the aluminum material required high pressure to mechanically press a mold against the surface of the aluminum material. For example, a triangular lattice pattern of 500 nm is placed 1 cm on the surface of an aluminum material. 2 To form a porous alumina of this size, it is necessary to apply a high pressure of about 2 tons to the mold using a hydraulic press. This makes it difficult to produce porous alumina with regularly-arranged pores over a large area, and the mold is also subject to wear and tear, making it difficult to produce the material efficiently and at low cost.
[0010] The present invention has been made in consideration of the above circumstances, and provides a porous alumina plate capable of efficiently producing a porous alumina plate having regularly arranged pores at low cost. Board The object is to provide a manufacturing method. [Means for solving the problem]
[0016] The method for producing a porous alumina plate of the present invention comprises the steps of: A porous alumina plate having an aluminum substrate and a porous alumina layer formed by anodizing one surface of the aluminum substrate, the porous alumina layer having a plurality of pores regularly arranged and extending in the thickness direction. The manufacturing method of the present invention is characterized by comprising a mask body forming process for forming a mask body modeled on one side of the aluminum substrate, the mask body being patterned after the pore formation pattern, and a pore forming process for anodizing the aluminum substrate to form the porous alumina layer having a plurality of pores regularly arranged and extending in the thickness direction.
[0017] In addition, in the present invention, the mask body forming process may be a process of forming a mask body made of resist resin on one side of the aluminum substrate, and then etching the one side of the aluminum substrate to form a recess on the one side of the aluminum substrate.
[0018] In addition, in the present invention, the mask body forming process may be a process of forming a porous alumina intermediate layer by anodization on one side of the aluminum substrate, forming the mask body made of a resist resin on the porous alumina intermediate layer, and then etching the porous alumina intermediate layer to form a recess in the porous alumina intermediate layer.
[0019] In the present invention, the mask body forming step is performed after forming the recess. Nopo The method may include a step of dissolving and removing the glass alumina intermediate layer.
[0020] In the present invention, the mask body may be formed by transferring a stamp having a pattern in which the pores are to be formed onto the resist resin. Effect of the Invention
[0021] According to the present invention, a porous alumina plate having regularly arranged pores can be efficiently manufactured at low cost. Board A method of manufacture may be provided. [Brief description of the drawings]
[0022] [Figure 1] FIG. 2 is an enlarged cross-sectional view showing a main portion of a porous alumina plate according to one embodiment of the present invention. [Diagram 2] 1A is a micrograph showing the surface of a porous alumina layer of the present embodiment, and FIG. 1B is a micrograph showing a cross section of the porous alumina layer of the present embodiment along the thickness direction. [Diagram 3] 2A to 2C are enlarged schematic diagrams showing a main part in a stepwise manner of a method for producing the porous alumina plate according to the first embodiment. [Figure 4] 5A to 5C are enlarged schematic diagrams showing a main part in a stepwise manner of a method for producing a porous alumina plate according to a second embodiment. [Diagram 5] 11A to 11C are enlarged schematic views showing a main part in a stepwise manner of a method for producing a porous alumina plate according to a third embodiment. [Figure 6]10A to 10C are enlarged schematic diagrams showing a main part in a stepwise manner of a method for producing a porous alumina plate according to a fourth embodiment. [Figure 7] 13A to 13C are enlarged schematic diagrams showing a main part in a stepwise manner of a method for producing a porous alumina plate according to a fifth embodiment. [Figure 8] 1 is a microscope photograph of the surface of the porous alumina plate obtained in Example 1. [Figure 9] 2 is a surface microscope photograph of the porous alumina plate obtained in Example 2. [Figure 10] 1 is a microscope photograph of the surface of the porous alumina plate obtained in Example 3. [Figure 11] 1 is a surface microscope photograph of the porous alumina plate obtained in Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, a porous alumina plate according to one embodiment of the present invention and its manufacturing method will be described with reference to the drawings. Note that each embodiment shown below is specifically described to better understand the gist of the invention, and does not limit the present invention unless otherwise specified. In addition, the drawings used in the following description may show the main parts enlarged for convenience in order to easily understand the features of the present invention, and the dimensional ratios of each component may not necessarily be the same as the actual ones.
[0024] (Porous alumina plate) FIG. 1 is an enlarged cross-sectional view of a main part of a porous alumina plate according to one embodiment of the present invention. The porous alumina plate 10 has an aluminum substrate 11 and a porous alumina layer 12 formed on one surface 11a of the aluminum substrate 11. The porous alumina layer 12 has a plurality of pores 14 arranged regularly and extending in the thickness direction t of the porous alumina plate 10.
[0025] The aluminum substrate 11 is made of pure aluminum, for example, 4N aluminum. The aluminum substrate 11 may be made of an aluminum alloy containing a metal other than aluminum. The aluminum substrate 11 may be a thick plate having a thickness of 1 mm or more, or a bendable thin plate having a thickness of about 0.1 mm to 0.5 mm. The aluminum substrate 11 may also be an aluminum material formed into, for example, a cylindrical shape.
[0026] The porous alumina layer 12 is made of porous aluminum oxide (Al2O3) formed by anodizing the aluminum substrate 11. The porous alumina layer 12 can have various thicknesses depending on the conditions during anodization, but it is sufficient that the layer is formed to have a thickness of, for example, about 1 μm to 100 μm.
[0027] Fig. 2(a) is a micrograph showing the surface of the porous alumina layer of this embodiment, and Fig. 2(b) is a micrograph showing the cross section along the thickness direction of the porous alumina layer of this embodiment. The pores 14 formed in the porous alumina layer 12 are arranged with high regularity along the surface extension direction of the porous alumina layer 12. In this embodiment, the pores 14 are arranged in an equilateral triangular lattice shape (an ideal triangular lattice shape).
[0028] The arrangement interval between adjacent pores 14 may be set to be, for example, in the range of 100 nm or more and 3 μm or less. The area in which the pores 14 are formed is, for example, 1 cm 2 The porous alumina plate 10 of this embodiment has a formation area of 1 cm 2 Even with such a large area, the porous alumina layer 12 having the pores 14 can be easily formed.
[0029] The pores 14 are holes with a high aspect ratio, and are formed so that the diameter (opening diameter) is, for example, 0.01 μm or more and 2 μm or less, and the depth of the pores 14 along the thickness direction is, for example, 0.5 μm or more and 1000 μm or less.
[0030] In this embodiment, an example is shown in which the pores 14 are arranged in a regular triangular lattice shape (ideal triangular lattice shape), but the arrangement shape is not limited to this as long as the pores 14 are arranged regularly at a predetermined interval, such as a regular quadrangular lattice shape (ideal quadrangular lattice shape).
[0031] (Method of manufacturing porous alumina plate: First embodiment) FIG. 3 is an enlarged schematic diagram showing a main part of the method for producing the porous alumina plate according to the first embodiment in a stepwise manner. In this embodiment, first, an aluminum substrate 11 is prepared, and a mask body 21 modeled after a pattern of pores to be formed in a later step is directly formed on one surface 11a of the aluminum substrate 11 (mask body forming step).
[0032] The method of forming the mask body 21 involves applying a resist resin that constitutes the mask body 21 to a stamp S that has a pattern for forming pores, and then transferring this resist resin to one surface 11a of the aluminum substrate 11 and hardening it, thereby forming the mask body 21 having mask openings that expose one surface 11a of the aluminum substrate 11 only in the areas where the pores are to be formed (see Figure 3(a)).
[0033] In this embodiment, a 4N aluminum plate was used as the aluminum substrate 11. Moreover, an ultraviolet-curable resin was used as the resist resin constituting the mask body 21, and after being transferred to the aluminum substrate 11, it was cured by irradiation with ultraviolet light.
[0034] In addition to the ultraviolet curable resin, various organic materials such as a thermosetting resin and a chemical reaction curable resin can be used as the constituent material of the mask body 21. In addition to the above-mentioned organic materials, an inorganic material can also be used as the constituent material of the mask body 21.
[0035] In this embodiment, a silicone resin is used as the stamp S. Since the silicone resin is easily cured by heating (dehydration condensation reaction), it is possible to easily form a shape that resembles a pattern of pores of any size. Furthermore, since the silicone resin is flexible after curing, it is possible to transfer the resist resin by following various surface shapes, such as when the surface 11a of the aluminum substrate 11 is not only flat but also curved.
[0036] Next, the aluminum substrate 11 on which the mask body 21 has been formed is anodized to form a porous alumina layer 12 having pores 14 on one surface 11a of the aluminum substrate 11 (pore forming step). For the anodization of the aluminum substrate 11, for example, a mixed solution (electrolyte) of phosphoric acid and citric acid is used, and electrolysis is performed with the aluminum substrate 11 as the anode.
[0037] As a result, one surface 11a of the aluminum substrate 11 is anodized to form a porous alumina layer 12. At this time, the one surface 11a of the aluminum substrate 11 is exposed in the pore formation pattern portions (mask openings) that are not covered by the mask body 21, and therefore the generation of pores 14 is induced from this exposed portion of aluminum.
[0038] As the anodization progresses, a plurality of regularly arranged pores 14 extending in the thickness direction are formed in the porous alumina layer 12 (see FIG. 3(b)). Note that, as the electrolyte for the anodization, other than the mixed solution of phosphoric acid and citric acid, for example, a dilute sulfuric acid aqueous solution, a phosphoric acid aqueous solution, an oxalic acid aqueous solution, etc. can also be used.
[0039] According to the method for manufacturing a porous alumina plate of this embodiment as described above, a mask body 21 having a pore formation pattern is formed on one surface 11a of the aluminum substrate 11, and then the aluminum substrate 11 is simply anodized to obtain a porous alumina plate 10 having a porous alumina layer 12 having a plurality of regularly arranged pores 14.
[0040] In this embodiment, since there is no need for a process such as applying high pressure to an aluminum substrate to create a texture, as in the conventional method, it is possible to easily and at low cost manufacture a large-area porous alumina plate 10 having a porous alumina layer 12 having a plurality of regularly arranged pores 14.
[0041] Furthermore, when forming the mask body 21 bearing the pore formation pattern, the mask body 21 is formed by transfer using the stamp S. This makes it possible to easily form the porous alumina layer 12 having a plurality of regularly arranged pores 14 even on an aluminum substrate having a curved surface, which was difficult to achieve using conventional methods for manufacturing porous alumina plates having pores.
[0042] (Method of manufacturing porous alumina plate: Second embodiment) FIG. 4 is an enlarged schematic diagram showing a main part in a stepwise manner of the method for producing the porous alumina plate according to the second embodiment. In this embodiment, first, an aluminum substrate 11 is prepared, and a mask body 21 modeled on a pattern of pores to be formed in a later step is directly formed on one surface 11a of the aluminum substrate 11 (mask body forming step: see FIG. 4(a)). The mask body 21 may be formed by transfer using a stamp S.
[0043] Next, the aluminum substrate 11 is immersed in an etching solution using the mask body 21 as an etching mask to perform etching. The etching solution may be, for example, an acidic aqueous solution containing one or more acids such as phosphoric acid, hydrochloric acid, oxalic acid, nitric acid, and sulfuric acid. By this etching, a recess (dent) 22 is formed in the mask opening (a portion where one surface 11a of the aluminum substrate 11 is exposed) (see FIG. 4(b)).
[0044] Next, the aluminum substrate 11 in which the recesses 22 have been formed by etching is anodized to form the porous alumina layer 12 having the pores 14 on one surface 11a of the aluminum substrate 11 (pore forming step).
[0045] As a result, one surface 11a of the aluminum substrate 11 is anodized to form a porous alumina layer 12, and at this time, the generation of pores 14 is induced from the recesses 22 in the one surface 11a of the aluminum substrate 11 formed by etching. Then, as the anodization progresses, a plurality of regularly arranged pores 14 extending in the thickness direction are formed in the porous alumina layer 12 (see FIG. 4(c)).
[0046] In the second embodiment described above, the aluminum substrate 11 in which the recesses 22 have been formed by etching is anodized while leaving the mask body 21 on the aluminum substrate 11 to form a porous alumina layer 12 having a plurality of pores 14. However, as a modified example, the mask body 21 can be used as an etching mask to form recesses 22 on one surface 11a of the aluminum substrate 11, and then the mask body 21 can be dissolved and removed using, for example, an organic solvent, and then anodization can be performed to form a porous alumina layer 12 having a plurality of pores 14.
[0047] Even in such a modified example, the generation of pores 14 is induced from the recesses 22 formed in the aluminum substrate 11, so that as the anodization progresses, a porous alumina layer 12 having a plurality of regularly arranged pores 14 extending in the thickness direction can be formed.
[0048] (Method of manufacturing porous alumina plate: third embodiment) FIG. 5 is an enlarged schematic view showing a main part in a stepwise manner of the method for producing the porous alumina plate according to the third embodiment. In this embodiment, first, an aluminum substrate 11 is prepared, and a porous alumina intermediate layer 23 is formed on one surface 11a of the aluminum substrate 11 by anodization (see FIG. 5(a)). Then, a mask body 21 modeled on a pore formation pattern to be formed in a later step is formed on the porous alumina intermediate layer 23 by transfer using a stamp S (mask body formation step).
[0049] Next, the aluminum substrate 11 having the porous alumina intermediate layer 23 on which the mask body 21 is formed is anodized again to form the porous alumina layer 12 having the pores 14 on one surface 11a of the aluminum substrate 11 (pore forming step).
[0050] At this time, the generation of pores 14 is induced from the portion (mask opening) of the porous alumina intermediate layer 23 that is exposed from the mask body 21. Then, as the anodization progresses, a plurality of regularly arranged pores 14 extending in the thickness direction are formed in the porous alumina layer 12 (see FIG. 5(b)).
[0051] In this embodiment, a porous alumina intermediate layer 23 is formed in advance on one surface 11a of the aluminum substrate 11 by anodization, and the transfer accuracy of the mask body 21 can be improved by the anchor effect due to the uneven structure of the surface of the porous alumina intermediate layer 23.
[0052] In order to improve the accuracy of forming the pores 14 in a later process, the porous alumina intermediate layer 23 is preferably made of porous alumina having a period smaller than 100 nm and produced by applying a voltage of about 40 V during anodization. The thickness of the porous alumina intermediate layer 23 is preferably 1 μm or less.
[0053] (Method of manufacturing porous alumina plate: Fourth embodiment) FIG. 6 is an enlarged schematic diagram showing a main part in a stepwise manner of the method for producing the porous alumina plate according to the fourth embodiment. In this embodiment, first, an aluminum substrate 11 is prepared, and a porous alumina intermediate layer 23 is formed on one surface 11a of the aluminum substrate 11 by anodization (see FIG. 6(a)). Then, a mask body 21 modeled after a pore formation pattern to be formed in a later step is formed on the porous alumina intermediate layer 23 (mask body formation step). The mask body 21 may be formed by transfer using a stamp S.
[0054] Next, the aluminum substrate 11 having the porous alumina intermediate layer 23 on which the mask body 21 is formed is immersed in an alumina dissolving solution such as a chromic acid-phosphoric acid aqueous solution to selectively dissolve only those portions of the porous alumina intermediate layer 23 that are exposed by the mask openings of the mask body 21.
[0055] As a result, recesses 23a corresponding to the pore formation pattern are formed in the porous alumina intermediate layer 23, and only these portions of one surface 11a of the aluminum substrate 11 are exposed (see FIG. 6(b)). Such a porous alumina intermediate layer 23 functions as a mask body during anodization in the subsequent pore formation process.
[0056] Next, the aluminum substrate 11 having the porous alumina intermediate layer 23 on which the mask body 21 is formed is anodized again to form the porous alumina layer 12 having the pores 14 on one surface 11a of the aluminum substrate 11 (pore forming step).
[0057] At this time, the generation of pores 14 is induced from the aluminum substrate 11 in the portion exposed by the recesses 23a formed in the porous alumina intermediate layer 23. Then, as the anodization progresses, a plurality of regularly arranged pores 14 extending in the thickness direction are formed in the porous alumina layer 12 (see FIG. 6(c)).
[0058] As a modified example of the above-described fourth embodiment, after forming recesses 23a modeled on the pore formation pattern in the porous alumina intermediate layer 23 by alumina etching, recesses (dents) can be formed in the portions of the porous alumina intermediate layer 23 where the recesses 23a are to be formed (portions where one surface 11a of the aluminum substrate 11 is exposed) using an acidic aqueous solution containing one or more acids such as phosphoric acid, hydrochloric acid, oxalic acid, nitric acid, and sulfuric acid as an aluminum etching solution.
[0059] In this modified example, the generation of the pores 14 is induced from the recesses formed on the surface 11a of the aluminum substrate 11 in the pore forming step, so that the pores 14 can be formed with higher accuracy.
[0060] (Method of manufacturing porous alumina plate: Fifth embodiment) FIG. 7 is an enlarged schematic view showing a main part in a stepwise manner of the method for producing the porous alumina plate according to the fifth embodiment. In this embodiment, first, an aluminum substrate 11 is prepared, and a porous alumina intermediate layer 23 is formed on one surface 11a of the aluminum substrate 11 by anodization (see FIG. 7(a)). Then, a mask body 21 modeled after a pore formation pattern to be formed in a later step is formed on the porous alumina intermediate layer 23 (mask body formation step). The mask body 21 may be formed by transfer using a stamp S.
[0061] Next, the aluminum substrate 11 having the porous alumina intermediate layer 23 on which the mask body 21 is formed is immersed in an alumina dissolving solution such as a chromic acid-phosphoric acid aqueous solution to selectively dissolve only those portions of the porous alumina intermediate layer 23 that are exposed by the mask openings of the mask body 21.
[0062] As a result, recesses 23a corresponding to the pore formation pattern are formed in the porous alumina intermediate layer 23, and only in these portions is one surface 11a of the aluminum substrate 11 exposed (see FIG. 7(b)).
[0063] Next, the aluminum substrate 11 having the porous alumina intermediate layer 23 on which the mask body 21 is formed is anodized again to form a concave porous alumina intermediate layer 24 on the portion of one surface 11a of the aluminum substrate 11 exposed by the concave portion 23a of the porous alumina intermediate layer 23 (see Figure 7(c)).
[0064] Next, the mask body 21 is dissolved and removed using an organic solvent, and further, the porous alumina intermediate layer 23 and the porous alumina intermediate layer 24 are dissolved and removed using an alumina dissolving solution such as a chromic acid-phosphoric acid aqueous solution, thereby forming an aluminum substrate 11 having a recess (dent) 22 formed on one surface 11a (see FIG. 7(d)).
[0065] Next, the aluminum substrate 11 with the recesses 22 formed therein is anodized to form the porous alumina layer 12 having the pores 14 on one surface 11a of the aluminum substrate 11 (pore forming step).
[0066] As a result, one surface 11a of the aluminum substrate 11 is anodized to form a porous alumina layer 12, and at this time, the generation of pores 14 is induced from the recesses 22 in the one surface 11a of the aluminum substrate 11 formed by etching. Then, as the anodization progresses, a plurality of regularly arranged pores 14 extending in the thickness direction are formed in the porous alumina layer 12 (see FIG. 7(e)).
[0067] Although one embodiment of the present invention has been described above, this embodiment is presented as an example and is not intended to limit the scope of the invention. This embodiment can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. This embodiment and its modifications are included in the scope of the invention and its equivalents described in the claims, as well as in the scope and gist of the invention. EXAMPLES
[0068] Example 1 A polydimethylsiloxane stamp with a 1 μm-pitch pillar array pattern was created by dip-coating a neoprene thin film on the surface. This stamp was used to press against a 4N aluminum substrate that had been electropolished and then formed with a porous alumina film, transferring a neoprene mask with a pore pattern onto the surface of the porous alumina film.
[0069] The aluminum substrate was then immersed in 7M hydrochloric acid at 50°C for 1 second to dissolve the portions exposed from the mask openings, forming recesses (dents) modeled after the pore pattern to be formed on one side of the aluminum substrate. The aluminum substrate with the recesses formed was then anodized for 30 minutes in a mixed bath of 2mM phosphoric acid and 0.3M citric acid at an applied voltage of 400V and a bath temperature of 10°C, yielding a porous alumina plate with pores in an ideal triangular arrangement with a period of 1μm. A microscope photograph of the surface of the porous alumina plate obtained in Example 1 is shown in FIG.
[0070] Example 2 The electrolytically polished 4N aluminum substrate was anodized for 5 minutes in a 0.3M oxalic acid bath at an applied voltage of 40 V and a bath temperature of 17°C to form a porous alumina intermediate layer. A polydimethylsiloxane stamp with a pillar array pattern with a pitch of 1 μm, on whose surface a neoprene thin film was formed by dip coating, was pressed against the surface of the porous alumina intermediate layer to transfer the neoprene mask to the surface of the porous alumina intermediate layer.
[0071] The alumina portion of the mask opening was then selectively dissolved and removed by immersing the mask in an aqueous chromate-phosphoric acid solution for 2 minutes, partially exposing the aluminum substrate. Anodization was then performed for 30 minutes in a mixed bath of 2 mM phosphoric acid and 0.3 M citric acid at an applied voltage of 400 V and a bath temperature of 10°C. After anodization, all of the oxide layer (porous alumina intermediate layer) was dissolved and removed in chromate-phosphoric acid, and the aluminum substrate with the recesses was anodized again under the same conditions to obtain a porous alumina plate with pores in an ideal rectangular arrangement with a period of 1 μm. A microscope photograph of the surface of the porous alumina plate obtained in Example 2 is shown in FIG.
[0072] Example 3 The electrolytically polished 4N aluminum substrate was anodized for 5 minutes in a 0.3M oxalic acid bath at an applied voltage of 40 V and a bath temperature of 17°C to form a porous alumina intermediate layer. A polydimethylsiloxane stamp with a pillar array pattern with a pitch of 2 μm, on whose surface a neoprene thin film was formed by dip coating, was pressed against the surface of the porous alumina intermediate layer to transfer the neoprene mask to the surface of the porous alumina intermediate layer.
[0073] The alumina portion of the mask opening was then selectively dissolved and removed by immersing the mask in an aqueous chromate-phosphoric acid solution for 2 minutes, partially exposing the aluminum substrate. After this, anodization was performed for 1 hour at an applied voltage of 800 V and a bath temperature of 16°C in a mixed bath of organic solvent and water containing 0.2 mM phosphoric acid and 0.3 M citric acid, forming a porous alumina intermediate layer on the exposed aluminum substrate. After anodization, all of the oxide layer was dissolved and removed in chromate-phosphoric acid, and the aluminum substrate with the recesses formed at 2 μm intervals was anodized again under the same conditions to obtain a porous alumina plate with pores in an ideal triangular arrangement at 2 μm intervals. A microscope photograph of the surface of the porous alumina plate obtained in Example 3 is shown in FIG.
[0074] Example 4 The electrolytically polished 4N aluminum substrate was anodized for 5 minutes in a 0.3M oxalic acid bath at an applied voltage of 40 V and a bath temperature of 17°C to form a porous alumina intermediate layer. A polydimethylsiloxane stamp with a pillar array pattern with a pitch of 500 nm, on whose surface a neoprene thin film was formed by dip coating, was pressed against the surface of the porous alumina intermediate layer to transfer the neoprene mask onto the surface of the porous alumina intermediate layer.
[0075] The alumina portion of the mask opening was then selectively dissolved and removed by immersing the mask in a chromic acid-phosphoric acid solution for 2 minutes, partially exposing the aluminum substrate. After this, anodization was performed for 1 hour in a 0.1M phosphoric acid bath at an applied voltage of 200V and a bath temperature of 0°C, forming a porous alumina intermediate layer on the exposed aluminum substrate. After anodization, all of the oxide layer was dissolved and removed in chromic acid-phosphoric acid, and the aluminum substrate with the recesses formed at 500μm intervals was anodized again under the same conditions to obtain a porous alumina plate with pores in an ideal triangular arrangement at 500μm intervals. A microscope photograph of the surface of the porous alumina plate obtained in Example 4 is shown in FIG. [Explanation of symbols]
[0076] 10…Porous alumina plate 11...Aluminum substrate 12…Porous alumina layer 14...pore
Claims
1. A method for producing a porous alumina plate comprising: an aluminum substrate; and a porous alumina layer formed by anodizing one surface of the aluminum substrate, the porous alumina layer having a plurality of pores regularly arranged and extending in a thickness direction, the method comprising the steps of: a mask body forming step of forming a mask body on one surface of the aluminum substrate, the mask body being patterned after the pore formation pattern; and a pore forming step of anodizing the aluminum substrate to form the porous alumina layer having a plurality of pores regularly arranged and extending in the thickness direction.
2. The method for manufacturing a porous alumina plate according to claim 1, characterized in that the mask body forming process is a process of forming a mask body made of resist resin on one side of the aluminum substrate, and then etching the one side of the aluminum substrate to form a recess on the one side of the aluminum substrate.
3. The method for manufacturing a porous alumina plate as described in claim 1, characterized in that the mask body forming process is a process of forming a porous alumina intermediate layer by anodization on one side of the aluminum substrate, forming the mask body made of a resist resin on the porous alumina intermediate layer, and then etching the porous alumina intermediate layer to form a recess in the porous alumina intermediate layer.
4. 2. The method for producing a porous alumina plate according to claim 1, wherein the mask body forming step includes a step of dissolving and removing the porous alumina intermediate layer after the recesses are formed.
5. 4. The method for manufacturing a porous alumina plate according to claim 2, wherein the mask body is formed by transferring a stamp having a pattern of the pores to the resist resin.
Citation Information
Patent Citations
Porous anodic oxidation aluminum film and its production
JP1987185898A
Functional nanostructure and optical element using the same
JP2002353432A
Method of producing self-aligning nanochannel-array, and method of producing nanodot using self-aligning nanochannel array
JP2004323975A
Bright thin film body, bright pigment and method for producing bright thin film body
JP2006176827A
Structural body, its manufacturing method and magnetic recording medium
JP2007073127A