Oil-impregnated sintered bearing and fluid dynamic bearing device equipped with said bearing

The sintered oil-impregnated bearing with specific dimensions and density ratios addresses the challenge of achieving thinner, high-accuracy bearings by ensuring stable dynamic pressure generation and rigidity, enabling cost-effective assembly in cooling fan motors.

JP7560389B2Active Publication Date: 2024-10-02NTN CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021040488
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-12
Publication Date
2024-10-02
Estimated Expiration
2041-03-12

AI Technical Summary

Technical Problem

The challenge is to achieve thinner wall thickness and higher rotation accuracy in fluid dynamic bearing devices without increasing assembly costs, particularly for bearings used in thinner cooling fan motors, where reduced axial dimensions compromise radial dynamic pressure generation and bearing rigidity.

Method used

A sintered oil-impregnated bearing with specific dimensions and density ratios, including an axial dimension of 4.8 mm or less, a thickness of 0.5 to 1.5 mm, and a ratio of axial to outer diameter of 0.24 to 0.6, ensures stable formation of dynamic pressure grooves and provides sufficient thrust bearing area, allowing for accurate assembly without extra jigs or increased costs.

Benefits of technology

This configuration enables thinner bearings with high rotational accuracy and reduced assembly costs by ensuring stable dynamic pressure generation and bearing rigidity, facilitating easy assembly by simply inserting the shaft into the bearing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560389000001
    Figure 0007560389000001
  • Figure 0007560389000002
    Figure 0007560389000002
  • Figure 0007560389000003
    Figure 0007560389000003
Patent Text Reader

Abstract

To achieve both of reduction of thickness and improvement of rotational accuracy of a fluid dynamic pressure bearing device without increasing assembling cost.SOLUTION: An axial dimension L of an oil-impregnated sintered bearing 8 is 4.8 mm or less, a thickness dimension t is 0.5 mm or more and 1.5 mm or less, and a ratio L / D2 of the axial dimension L to an outer diameter dimension D2 is 0.24 or more and 0.6 or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sintered oil-impregnated bearing and a fluid dynamic bearing device equipped with the bearing, and more particularly to a sintered oil-impregnated bearing having a radial dynamic pressure generating portion and a fluid dynamic bearing device equipped with the bearing. [Background technology]

[0002] A sintered oil-impregnated bearing is a bearing in which the internal pores of a porous body made of sintered metal are impregnated with a lubricating oil, and as the shaft inserted into the inner circumference rotates relative to the shaft, the lubricating oil impregnated in the internal pores seeps out to the sliding part with the shaft to form an oil film, which supports the rotation of the shaft. Due to their excellent rotational accuracy and quietness, such bearings are suitably used as bearing devices for motors mounted on various electrical devices including information devices, more specifically, for spindle motors in disk drives for HDDs, CDs, DVDs, and Blu-ray disks, for fan motors mounted in these disk drives and PCs, and for polygon scanner motors mounted in laser beam printers (LBPs).

[0003] In addition, dynamic pressure generating parts such as dynamic pressure grooves may be formed on at least one of the inner peripheral surface and the axial end surface of the sintered oil-impregnated bearing in order to further improve noise reduction and extend the life of the bearing. Here, a method of forming dynamic pressure grooves is known as dynamic pressure groove sizing. In this sizing, for example, a sintered body to be a bearing is compressed in the axial direction by an upper punch and a lower punch, and the sintered body is pressed into the inner circumference of a die, so that the sintered body is bitten into a forming die on the outer circumference of a sizing pin that has been inserted into the inner circumference of the sintered body in advance. As a result, the shape of the forming die, i.e., the shape corresponding to the dynamic pressure grooves, is transferred to the inner circumference of the sintered body, and dynamic pressure grooves are formed as radial dynamic pressure generating parts (see, for example, Patent Document 1).

[0004] Recently, as information devices have become smaller and thinner, there is a demand for miniaturization of various motors mounted on the information devices. For example, cooling fan motors used in notebook computers and the like are becoming thinner, and the bearing devices used in these motors are also required to be thinner. At the same time, the same or higher level of cooling performance is required as before. Since the thinner bearing device leads to a reduction in the bearing area, there is a high risk of a decrease in bearing rigidity due to the reduction in bearing area, not only when the size of the impeller (fan) is increased, but also when the size of the impeller is maintained.

[0005] Here, Patent Document 2 describes a sintered oil-impregnated bearing with a hydrodynamic groove arrangement region on its inner peripheral surface, in which the axial dimension is 6 mm or less and the density ratio of the entire bearing is 80% or more and 95% or less. It also describes that, according to the bearing having the above configuration, the density ratio of the entire bearing is more uniform than in the past, so that sufficient bearing rigidity can be expected even if the axial dimension is reduced by eliminating the lubricating fluid reservoir (recess) that existed in the past between the hydrodynamic groove arrangement regions. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 3607492 [Patent Document 2] JP 2015-64019 A Summary of the Invention [Problem to be solved by the invention]

[0007] Recently, cooling fan motors used in notebook computers and the like have become thinner, and there is a demand for further reduction in the axial dimension of the bearings used in the motors. On the other hand, as the axial dimension of the bearing becomes smaller, the area in which the radial dynamic pressure generating portion can be formed decreases accordingly, and the dynamic pressure that can be generated in the radial bearing gap also becomes smaller. This makes it difficult to support the shaft portion (rotating body such as an impeller) with high precision, which may lead to a decrease in rotational precision (NRRO). For example, as described in Patent Document 2, it is possible to improve the bearing rigidity and therefore the rotational precision by providing thrust dynamic pressure grooves on both end faces of the bearing. However, in this case, the assembly of the fluid dynamic bearing device cannot be completed by simply inserting the shaft portion of the rotating body into the inner circumference of the bearing, and additional jigs and processes are required, which may lead to an increase in assembly costs.

[0008] In view of the above circumstances, the technical problem to be solved by the present invention is to make it possible to achieve a thinner fluid dynamic bearing device and higher rotational accuracy without incurring a rise in assembly costs. [Means for solving the problem]

[0009] The above-mentioned problems are solved by the sintered oil-impregnated bearing of the present invention. That is, this bearing is a sintered metal bearing obtained by compressing metal powder into a cylindrical shape to form a green compact and sintering the green compact, and the sintered oil-impregnated bearing has internal pores impregnated with a lubricating fluid and has a radial dynamic pressure generating portion formed on its inner circumferential surface, and is characterized in that the axial dimension L is 4.8 mm or less, the thickness dimension t is 0.5 mm or more and 1.5 mm or less, and the ratio L / D2 of the axial dimension L to the outer diameter dimension D2 is 0.24 or more and 0.6 or less.

[0010] The inventors have found that, in the above-mentioned hydrodynamic groove sizing, even when the axial dimension L of the sintered metal bearing is made smaller than conventionally (4.8 mm or less), by setting the thickness dimension t of the bearing and the ratio L / D2 of the axial dimension L to the outside diameter dimension D2 within respective predetermined numerical ranges, the press-fit force on the cylindrical sintered body can be sufficiently transmitted to the surface layer of the bearing's inner peripheral surface as a radial compression force. The present invention has been made in view of the above findings, and when the axial dimension L of a sintered oil-impregnated bearing is made smaller than conventionally (4.8 mm or less), the thickness dimension t is set in the range of 0.5 to 1.5 mm, and the bearing is made significantly flatter than conventionally (i.e., the ratio L / D2 of the axial dimension L to the outside diameter dimension D2 is set to a value significantly smaller than 1: 0.24 to 0.6). By making the bearing into such a shape and size, for example, during the above-mentioned dynamic pressure groove sizing, the radial pressure force generated by pressing into the die can be sufficiently transmitted to the inner peripheral surface layer of the sintered body that will become the bearing, regardless of the size of the axial dimension L. Therefore, even if the axial dimension L is set smaller than before, the radial dynamic pressure generating part (represented by a groove shape) can be accurately and stably molded, and the required radial bearing performance can be stably exhibited. In addition, by setting the thickness dimension t to 0.5 mm or more, the required thrust bearing area can be secured on the end face on one axial side of the bearing. As a result, even if the thrust bearing part is provided only on one axial side of the bearing, excellent rotational accuracy can be exhibited, so that, for example, by simply inserting the shaft part of the rotor into the inner circumference of the sintered oil-impregnated bearing, it becomes possible to assemble a fluid dynamic bearing device equipped with the bearing at low cost.

[0011] Furthermore, the sintered oil-impregnated bearing according to the present invention may have a density ratio of 86% or more and 92% or less. Note that the "density ratio" here means the value (percentage) obtained by dividing the density of the porous body constituting the sintered oil-impregnated bearing by the density when it is assumed that the porous body has no pores.

[0012] In this way, by making the density ratio of the sintered oil-impregnated bearing 86% or more, the press-in force on the die is sufficiently transmitted to the surface layer of the inner circumferential surface of the bearing as a radial pressure force, especially during dynamic pressure groove sizing. Therefore, it is possible to transfer and form dynamic pressure grooves of sufficient depth to the inner circumferential surface of the bearing. In addition, by suppressing the density ratio to 92% or less, excessive load on the sizing die can be suppressed, so that good dynamic pressure groove sizing can be stably and continuously performed. In particular, by making the bearing have the above-mentioned axial dimension L and flat shape and setting the density ratio within the above-mentioned range, the variation in density ratio inside the sintered body that becomes the bearing can be further reduced (to 1% or less), so that high rotation performance can be stably demonstrated. Specifically, the density ratio of the surface layer can be set to a degree that can appropriately and evenly exude lubricating oil, etc. into the bearing gap while preventing the escape of dynamic pressure from the bearing surface. In addition, it is possible to set the density ratio of the region other than the surface layer (the region inside the surface layer) so that the amount of impregnation of lubricating oil, etc. by the inner region is appropriate and uniform.

[0013] In the sintered oil-impregnated bearing according to the present invention, the ratio D2 / D1 of the outer diameter D2 to the inner diameter D1 may be 1.5 or more and 3.0 or less.

[0014] In this way, by setting the ratio D2 / D1 of the outer diameter D2 to the inner diameter D1 to be 1.5 or more and 3.0 or less, it is possible to ensure the bite of the sizing pin into the inner peripheral surface, and in turn the formability of the dynamic pressure grooves, etc. Also, by determining the ratio D2 / D1 of the inner diameter D1 to the outer diameter D2 in conjunction with the above-mentioned preferable numerical range of the thickness dimension t, it becomes possible to more effectively apply the radial compression force caused by the die press-fitting to the inner peripheral surface layer portion of the sintered body.

[0015] In the sintered oil-impregnated bearing according to the present invention, the inner diameter D1 may be 1.5 mm or more and 2.0 mm or less.

[0016] In this way, even by making the inner diameter dimension D1 1.5 mm or more, it is possible to ensure the bite of the sizing pin to the inner peripheral surface, and thus the formability of the dynamic pressure grooves, etc. In addition, by determining the preferable numerical range of the inner diameter dimension D1 together with the preferable numerical range of the thickness dimension t described above, it is possible to generate a sufficient amount of springback in the sintered body (porous body). As a result, it is possible to reliably form dynamic pressure grooves on the inner peripheral surface, even if the depth of the dynamic pressure grooves is, for example, appropriate (about 1 to 4 mm). In addition, by keeping the inner diameter dimension D1 at 2.0 mm or less, it is possible to avoid a situation in which the outer diameter dimension D2 and thus the thickness dimension t increase more than necessary, and it is possible to reliably transmit the radial compression force generated by pressing into the die to the surface layer of the inner peripheral surface.

[0017] In the sintered oil-impregnated bearing according to the present invention, the thrust dynamic pressure generating portion may be formed on one axial end face, and the other axial end face may be flat.

[0018] As described above, the sintered oil-impregnated bearing of the present invention can achieve both a thinner fluid dynamic bearing device and higher rotational accuracy, so that even when the thrust dynamic pressure generating portion is formed on only one axial end face, as described above, sufficient bearing rigidity can be exhibited. Therefore, for example, by simply inserting the shaft of the rotating body into the inner periphery of the bearing, assembly of the shaft (rotating body) to the bearing can be completed, making it possible to assemble the fluid dynamic bearing device at low cost.

[0019] Furthermore, the sintered oil-impregnated bearing described above can be suitably provided as a fluid dynamic bearing device comprising, for example, the sintered oil-impregnated bearing, a housing to whose inner circumference the sintered oil-impregnated bearing is fixed, a rotating body having a shaft portion inserted into the inner circumference of the sintered oil-impregnated bearing, and a radial bearing portion that supports the shaft portion in a non-contact manner in the radial direction by a film of lubricating fluid that is formed in the radial bearing gap between the inner surface of the sintered oil-impregnated bearing and the outer surface of the shaft portion by the dynamic pressure action of the radial dynamic pressure generating portion.

[0020] In addition, the fluid dynamic bearing device according to the present invention may further comprise a first thrust bearing portion which supports the shaft portion in a non-contact manner in the thrust direction by a film of lubricating fluid formed in a thrust bearing gap between the other axial end face of the rotating body facing each other in the thrust direction and one axial end face of the sintered oil-impregnated bearing.

[0021] In this case, the fluid dynamic bearing device according to the present invention may be provided with a thrust dynamic pressure generating portion on one axial end face of the sintered oil-impregnated bearing that faces in the thrust direction the disk portion of the hub portion as the rotating body.

[0022] Furthermore, the fluid dynamic bearing device according to the present invention may further comprise a second thrust bearing portion that supports the other axial end of the shaft portion in contact with one axial end face of the housing in the thrust direction.

[0023] In this way, by providing a first thrust bearing portion between the rotor and the sintered oil-impregnated bearing, which face each other in the thrust direction, and by providing a second thrust bearing portion between the shaft and the housing, which also face each other in the thrust direction, for contact support of the shaft, it is possible to provide sufficient bearing rigidity in the thrust direction while keeping the shape of the sintered oil-impregnated bearing as simple as possible. In addition, by providing a thrust dynamic pressure generating portion on one axial end face of the sintered oil-impregnated bearing, which faces the disk portion of the hub portion as the rotor, in the thrust direction, the thrust dynamic pressure generating portion can be molded with high precision. This makes it possible to provide extremely excellent thrust bearing performance.

[0024] As described above, the fluid dynamic bearing device according to the above description makes it possible to reduce the thickness of the fluid dynamic bearing device and achieve high rotational accuracy without incurring an increase in assembly costs, and can therefore be suitably used, for example, as a motor equipped with this fluid dynamic bearing device. Effect of the Invention

[0025] As described above, according to the present invention, it is possible to achieve a thinner fluid dynamic bearing device and higher rotational accuracy without incurring a rise in assembly costs. [Brief description of the drawings]

[0026] [Figure 1] 1 is a cross-sectional view of a fan motor according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view of the fluid dynamic bearing device shown in FIG. [Diagram 3] FIG. 3 is a cross-sectional view of the sintered oil-impregnated bearing shown in FIG. [Figure 4] FIG. 3 is a plan view of the sintered oil-impregnated bearing shown in FIG. 2. [Diagram 5] FIG. 3 is a bottom view of the sintered oil-impregnated bearing shown in FIG. 2. [Figure 6] FIG. 4 is a cross-sectional view of a fluid dynamic bearing device according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] An embodiment of the present invention will be described below with reference to the drawings. In the following description, the disk side of the hub part will be treated as the "upper side" and the bottom side of the housing as the "lower side" when viewed from the sintered oil-impregnated bearing. Of course, this up-down direction does not limit the actual installation or usage of the product.

[0028] 1 conceptually shows an example of the configuration of a fan motor 1 according to this embodiment. This fan motor 1 comprises a fluid dynamic bearing device 2, a plurality of fans 4 provided on a rotor 3 of the fluid dynamic bearing device 2, and a drive unit 5 for rotating these fans 4 integrally with the rotor 3. The drive unit 5 is made up of, for example, a coil 5a and a magnet 5b opposed to each other with a radial gap in between, and in this embodiment, the coil 5a is fixed to a base part 6 which is the fixed side of the fan motor 1, and the magnet 5b is fixed to the rotor 3 which is the rotating side of the fan motor 1.

[0029] In the fan motor 1 configured as above, when current is applied to the coil 5a, the magnet 5b rotates due to the excitation force between the coil 5a and the magnet 5b, and this rotation causes the multiple fans 4 erected on the outer periphery of the rotor 3 to rotate integrally with the rotor 3. This rotation causes each fan 4 to generate an airflow in a direction according to its shape (here, for example, an airflow toward the outside in the radial direction), and a secondary airflow is generated that is drawn into this airflow and flows from the upper side to the lower side in the axial direction of the fan motor 1. By generating an airflow around the fan motor 1 in this way, it is possible to cool an information device (not shown) to which the fan motor 1 is attached (not shown).

[0030] Furthermore, when an airflow occurs in the axial direction of the fan motor 1 as described above, a force (reaction force) in the opposite direction to the airflow is generated on the rotor 3 of the fluid dynamic bearing device 2. A magnetic force (repulsive force) in a direction that cancels out the reaction force is applied between the coil 5a and the magnet 5b, and a thrust load generated by the difference in magnitude between the reaction force and the magnetic force acts on the thrust bearing parts T1 and T2 (see FIG. 2 described later) of the fluid dynamic bearing device 2. The magnetic force in the direction that cancels out the reaction force can be generated, for example, by displacing the coil 5a and the magnet 5b in the axial direction (detailed illustration is omitted). Furthermore, when the rotor 3 rotates, a radial load acts on the shaft part 10 of the fluid dynamic bearing device 2 described later. This radial load acts on the radial bearing parts R1 and R2 of the fluid dynamic bearing device 2.

[0031] 2 shows a cross-sectional view of a fluid dynamic bearing device 2 incorporated in a fan motor 1. This fluid dynamic bearing device 2 comprises a housing 7, a sintered oil-impregnated bearing 8 fixed to the inner periphery of the housing 7, and a rotor 3 that rotates relative to the sintered oil-impregnated bearing 8.

[0032] The rotating body 3 has a hub portion 9 arranged on the upper end opening side of the housing 7 , and a shaft portion 10 inserted into the inner periphery of the sintered oil-impregnated bearing 8 .

[0033] As shown in Fig. 1 and Fig. 2, the hub portion 9 is composed of a disk portion 9a covering the upper end opening side of the housing 7, a first cylindrical portion 9b extending axially downward from the disk portion 9a, a second cylindrical portion 9c located radially outward from the first cylindrical portion 9b and extending axially downward from the disk portion 9a, and a flange portion 9d extending radially outward from the axial lower end of the second cylindrical portion 9c. The disk portion 9a faces one end face (upper end face 8b) of the sintered oil-impregnated bearing 8 fixed to the inner circumference of the housing 7. The fans 4 are provided integrally with the hub portion 9 in a manner that they stand from the outer circumferential edge of the flange portion 9d.

[0034] In this embodiment, the shaft portion 10 is formed separately from the hub portion 9, and its upper end is fixed to a mounting hole 9e provided in the hub portion 9. Here, the shaft portion 10 has an outer peripheral surface 10a with a constant outer diameter dimension, and a lower end portion 10b, for example, in a partially spherical shape, which is continuous with the lower end of the outer peripheral surface 10a. In other words, the shaft portion 10 has a shape that allows it to be inserted into the inner circumference of the sintered oil-impregnated bearing 8 from one axial side. Of course, the shaft portion 10 and the hub portion 9 may be integrally formed from the same material. Alternatively, the shaft portion 10 and the hub portion 9, which are formed from different materials, may be formed as an insert part with the other being formed by injection molding of metal or resin.

[0035] The housing 7 has an open upper end and a closed lower end. A sintered oil-impregnated bearing 8 is fixed to an inner peripheral surface 7a of the housing 7, and an outer peripheral surface 7b of the housing 7 is fixed to the base portion 6 (see FIG. 1). The axial distance between the upper end surface 7c of the housing 7 and the lower end surface 9a1 of the disk portion 9a of the hub portion 9 is larger than the distance between the upper end surface 8b of the sintered oil-impregnated bearing 8 and the lower end surface 9a1 of the disk portion 9a, and is set to a size that is deemed to have no substantial effect on the increase in loss torque during rotational driving.

[0036] A tapered seal surface 7d is formed on the upper outer periphery of the housing 7, the outer diameter of which increases as it goes upward. This tapered seal surface 7d forms an annular seal space S between the inner periphery 9b1 of the first cylindrical portion 9b, in which the radial distance between the tapered seal surface 7d and the inner periphery 9b1 of the first cylindrical portion 9b is gradually reduced from the closed side (lower side) of the housing 7 to the open side (upper side). This seal space S communicates with the outer diameter side of the thrust bearing gap of the first thrust bearing portion T1 described later when the shaft portion 10 and the hub portion 9 rotate, and allows the flow of lubricating oil between the seal space S and the bearing internal space including each bearing gap. In addition, when the lubricating oil is filled in the internal holes and the bearing internal space of the sintered oil-impregnated bearing 8, the amount of lubricating oil filled is adjusted so that the oil level (gas-liquid interface) of the lubricating oil is always maintained within the seal space S (see FIG. 2).

[0037] Furthermore, when the housing 7 has the above-mentioned seal structure, the coil 5a is positioned radially outward of the first cylindrical portion 9b of the hub portion 9, and is disposed so that the first cylindrical portion 9b and the coil 5a partially overlap in the axial direction. This makes it possible to reduce the thickness of the housing 7 and, ultimately, the fluid dynamic bearing device 2 (reduce the axial dimension).

[0038] In this embodiment, a thrust receiving portion 11 that receives the lower end portion 10b of the spherical shaft portion 10 is provided on the bottom portion 7e of the housing 7. That is, when the fluid dynamic bearing device 2 is in a completed state, this thrust receiving portion 11 is always in contact with the lower end portion 10b of the shaft portion 10, and is capable of supporting the rotation of the shaft portion 10. The vertical position of the thrust receiving portion 11 relative to the bearing abutment surface 7f of the housing 7 should preferably be set so that the abutment position between the shaft portion 10 and the thrust receiving portion 11 is within the vertical region of the inner chamfered portion 8e of the sintered oil-impregnated bearing 8, for example.

[0039] In principle, the material and composition of the housing 7 are arbitrary, and known materials such as resins and metals can be appropriately adopted depending on the fixing means for the sintered oil-impregnated bearing 8 to the housing 7, which will be described later.

[0040] The sintered oil-impregnated bearing 8 is a porous sintered metal body formed by compressing and sintering a predetermined raw material powder, and has a cylindrical shape. In this embodiment, it has a cylindrical shape as shown in FIG. 4 and the like. An area in which a plurality of dynamic pressure grooves 8a1 are arranged is formed as a radial dynamic pressure generating part on the entire surface or part of the inner peripheral surface 8a of the sintered oil-impregnated bearing 8. In this embodiment, as shown in FIG. 3, the dynamic pressure groove 8a1 arrangement area is formed by arranging a plurality of dynamic pressure grooves 8a1 inclined at a predetermined angle with respect to the circumferential direction, an inclined hill portion 8a2 that divides the dynamic pressure grooves 8a1 in the circumferential direction, and a band portion 8a3 that extends in the circumferential direction and divides each dynamic pressure groove 8a1 in the axial direction in a herringbone shape (both the inclined hill portion 8a2 and the band portion 8a3 are cross-hatched parts in FIG. 3), and is formed in two consecutive places in the axial direction. In this case, the upper dynamic pressure groove arrangement region A1 and the lower dynamic pressure groove arrangement region A2 are both formed axially symmetrically with respect to the axial centerline (an imaginary line connecting the axial centers of the band portion 8a3 in the circumferential direction), and their axial dimensions are equal to each other.

[0041] An area in which a plurality of dynamic pressure grooves 8b1 are arranged as a thrust dynamic pressure generating portion is formed on the entire surface or a part of the upper end surface 8b of the sintered oil-impregnated bearing 8. In this embodiment, for example as shown in Fig. 4, an area in which a plurality of dynamic pressure grooves 8b1 extending in a spiral shape are arranged side by side in the circumferential direction is formed. In this case, the spiral direction of the dynamic pressure grooves 8b1 is set to a direction corresponding to the rotation direction of the rotor 3. When the fluid dynamic bearing device 2 shown in Fig. 2 is rotated, the dynamic pressure groove 8b1 arrangement area configured as described above forms a thrust bearing gap of a first thrust bearing portion T1 described later between the lower end surface 9a1 of the disk portion 9a of the hub portion 9 facing the dynamic pressure groove 8b1 arrangement area.

[0042] No thrust dynamic pressure generating portion is formed on the lower end surface 8c of the sintered oil-impregnated bearing 8. That is, in this embodiment, the lower end surface 8c has a flat shape as shown in Fig. 5. The lower end surface 8c abuts on the housing 7 on the radially outer side of the housing 7 relative to the thrust receiving portion 11. In this case, the vertical position of the bearing abutment surface 7f of the housing 7 is appropriately set within a range in which the space between the upper end surface 8b of the sintered oil-impregnated bearing 8 and the lower end surface 9a1 of the hub portion 9 can function as a thrust bearing gap.

[0043] One or more (five in this embodiment) axial grooves 8d1 are formed in the outer peripheral surface 8d of the sintered oil-impregnated bearing 8 (see FIG. 4, for example). When the sintered oil-impregnated bearing 8 is fixed to the housing 7, the axial grooves 8d1 form a flow path for lubricating oil between the inner peripheral surface 7a of the housing 7 (see FIG. 2).

[0044] Next, various dimensions of the sintered oil-impregnated bearing 8 will be described with reference to Fig. 3. The axial dimension L of the sintered oil-impregnated bearing 8 (the axial distance between both end faces 8b, 8c) is set to 4.8 mm or less, preferably 3.0 mm or less, and more preferably 1.8 mm or less, from the viewpoint of reducing the thickness of the fluid dynamic bearing device 2 and therefore the fan motor 1. On the other hand, from the viewpoint of ensuring the required radial bearing rigidity, the axial dimension L is set to 0.8 mm or more, and preferably 1.1 mm or more.

[0045] The inner diameter dimension D1 of the sintered oil-impregnated bearing 8 (more precisely, the inner diameter dimension of the band portion 8a3 which, together with the inclined hill portion 8a2, forms the smallest diameter portion of the inner circumferential surface 8a) is arbitrary as long as the thickness dimension t of the sintered oil-impregnated bearing 8 is set within the range described below, but from the viewpoint of ensuring the bite of the sizing pin into the inner circumferential surface 8a during dynamic pressure groove sizing, it is preferable that it is 1.2 mm or more, and more preferable that it is 1.5 mm or more. On the other hand, from the viewpoint of avoiding a situation in which it becomes difficult to reliably transmit the press-fitting force to the surface portion of the inner circumferential surface 8a during dynamic pressure groove sizing due to an unnecessary increase in the thickness dimension t, the inner diameter dimension D1 is preferably 2.5 mm or less, and more preferably 2.0 mm or less.

[0046] The outer diameter D2 of the sintered oil-impregnated bearing 8 is arbitrary as long as the thickness t of the sintered oil-impregnated bearing 8 and the ratio L / D2 of the axial dimension L to the outer diameter D2 are set within the range described below, but considering the necessary inner diameter D1 and thickness t, it is preferable that the outer diameter D2 is 2.5 mm or more, and more preferably 3.0 mm or more. From the same viewpoint, the outer diameter D2 is preferably 5.0 mm or less, and more preferably 4.5 mm or less.

[0047] The ratio D2 / D1 of the outer diameter D2 to the inner diameter D1 is preferably set to 1.5 or more and 3.0 or less from the viewpoint of ensuring the bite of the sizing pin to the inner peripheral surface 8a and thus the formability of the dynamic pressure grooves 8a1.

[0048] The thickness dimension t {= (D2-D1) / 2} of the sintered oil-impregnated bearing 8 is preferably set to 0.5 mm or more from the viewpoint of ensuring the necessary thrust bearing area for the upper end face 8b. On the other hand, from the viewpoint of being able to transmit a sufficient compressive force from the die to the inner peripheral surface layer portion of the sintered compact during dynamic pressure groove sizing, the thickness dimension t is preferably set to 1.5 mm or less.

[0049] In addition, the ratio L / D2 of the axial dimension L to the outer diameter dimension D2 is set to 0.24 or more and 0.6 or less from the viewpoint of the efficiency of transmitting the radial compression force to the inner surface layer portion of the sintered compact during dynamic pressure groove sizing.

[0050] Next, the composition of the sintered oil-impregnated bearing 8 will be described. The sintered oil-impregnated bearing 8 is obtained by compression molding and sintering raw powder containing the most of either copper-based powder or iron-based powder and the second most of the other. In other words, the porous body of the sintered oil-impregnated bearing 8 is substantially composed of either copper or iron as the main component and the other as the second component (the second most abundant component). The copper-based powder referred to here includes not only pure copper powder but also copper alloy powder. Furthermore, pure copper includes not only 100% pure copper but also 99.99% or more copper that is industrially recognized as pure copper. Similarly, the iron-based powder referred to here includes not only pure iron powder but also iron alloy powder such as stainless steel. Furthermore, pure iron referred to here includes not only 100% pure iron but also 99.99% or more iron that is industrially recognized as pure iron. As long as the above composition (powder blending ratio) is established, the type and blending ratio of the powder that is the third or subsequent component are arbitrary.

[0051] The composition of the raw powder (powder blend ratio) that can be applied is, for example, [copper-based powder: 50-70% by weight, iron-based powder: 30-48% by weight, tin powder: 0-5%], and a specific example can be [pure iron powder of 140 mesh or less: 38-42% by weight, tin powder of 330 mesh or less: 1-3%, pure copper powder of 200 mesh or less: balance].

[0052] Next, the density ratio of the sintered oil-impregnated bearing 8 will be described. The density ratio of the entire sintered oil-impregnated bearing 8 is set to 80% or more and 95% or less, and preferably 86% or more and 92% or less. The density ratio can be set, for example, by adjusting the material, particle size (distribution), and compounding ratio of the raw metal powder. The variation in density ratio at this time can be evaluated using the porosity, which has a certain correlation with the density ratio. Here, the porosity is expressed as the volume ratio (percentage) of pores per unit volume of the bearing, and empirically, it shows an almost negative correlation with the density ratio (correlation coefficient of -1).

[0053] The surface porosity of the inner circumferential surface 8a, particularly the inner circumferential surfaces of the inclined hill portion 8a2 and band portion 8a3 which form the radial bearing surface, is adjusted to, for example, 2% or more and 15% or less. The surface porosity can be adjusted, for example, by rotational sizing, which will be described later.

[0054] The sintered oil-impregnated bearing 8 having the above configuration is manufactured, for example, through a powder compaction step S1, a sintering step S2, a dynamic pressure groove sizing step S3, and an oil impregnation step S4. Below, the details of each step will be explained using as an example a case in which a dimension sizing step S21 and a rotation sizing step S22 are provided after the sintering step S2 and before the dynamic pressure groove sizing step S3.

[0055] (S1) Powder compaction process First, raw powder that will be the material for the sintered oil-impregnated bearing 8 that will be the final product is prepared, and this is compression molded into a predetermined shape by die press molding. Specifically, although not shown in the figure, the raw powder is compression molded using a molding die that is composed of a die, a core pin inserted and arranged in a hole in the die, a lower punch arranged between the die and the core pin and configured to be able to move up and down with respect to the die, and an upper punch configured to be able to move (up and down) relative to both the die and the lower punch. In this case, the raw powder is filled into a space defined by the inner peripheral surface of the die, the outer peripheral surface of the core pin, and the upper end surface of the lower punch, and the upper punch is lowered with the lower punch fixed, and the filled raw powder is compressed in the axial direction. Then, the upper punch is lowered to a predetermined position while applying pressure, and the raw powder is compressed to a predetermined axial dimension, thereby forming a green compact. In this case, the axial dimension of the green compact can be set within an appropriate range by controlling the distance between the lower end face of the upper punch and the upper end face of the lower punch; more specifically, the bottom dead center of the upper punch; in accordance with the target axial dimension (more precisely, this is set taking into account the dimensional changes due to the subsequent sintering process and various sizing processes).

[0056] (S2) Sintering process After the green compact is obtained as described above, the green compact is sintered at a temperature according to the type of raw material powder (the melting point of the main component metal) to obtain a sintered body.

[0057] (S21) Dimensional sizing process, and (S22) Rotational sizing process The sintered body is then subjected to dimensional sizing to correct the outer diameter, inner diameter, and axial dimensions of the sintered body to dimensions conforming to those of the final product, and the surface porosity of the inner peripheral surface 8a is adjusted to a suitable ratio for a dynamic pressure bearing (for example, the above-mentioned numerical range: 2 to 15%). At this stage, the predetermined dynamic pressure groove 8a1 arrangement regions A1, A2 have not yet been formed on the inner peripheral surface 8a of the sintered body. Similarly, although not shown in the figure, the predetermined dynamic pressure groove 8b1 arrangement region has not yet been formed on the upper end surface 8b of the sintered body.

[0058] (S3) Dynamic groove sizing process The sintered body obtained through the above series of steps is subjected to a predetermined dynamic pressure groove sizing to form the dynamic pressure groove 8a1 arrangement areas A1, A2 on the inner peripheral surface 8a of the sintered body. The molding device used here, although not shown, includes a die having a press-fit hole for the sintered body, a sizing pin arranged so as to be inserted into the press-fit hole of the die, a lower punch arranged between the die and the sizing pin and configured so as to be able to move up and down relative to the die, and an upper punch configured so as to be able to move up and down relative to both the die and the lower punch. In this case, the inner diameter dimension of the press-fit hole of the die is appropriately set according to the press-fit allowance of the sintered body to be sized. In addition, a molding die having a shape corresponding to the dynamic pressure groove arrangement areas A1, A2 (FIG. 3) of the inner peripheral surface 8a to be molded is provided on the outer peripheral surface of the sizing pin, and a molding die having a shape corresponding to the dynamic pressure groove 8b1 arrangement area (FIG. 4) of the upper end surface 8b to be molded is provided on the lower end surface of the upper punch.

[0059] Next, an example of dynamic pressure groove sizing using the above molding device will be described. First, with the sintered body placed on the upper end surface of the die, the upper punch and the sizing pin are lowered from above. As a result, the sizing pin is inserted into the inner periphery of the sintered body, and the molding die provided on the outer periphery of the sizing pin is made to face the inner periphery of the sintered body in the radial direction. Then, after this molding die reaches a predetermined axial position on the inner periphery, only the upper punch is lowered to press the upper end surface of the sintered body. As a result, the sintered body is pressed into the press-fit hole of the die, the outer periphery of the sintered body is compressed, and the inner periphery of the sintered body bites into the molding die of the sizing pin that was previously inserted into the inner periphery. From this state, the upper punch is further lowered to hold the sintered body between the upper punch and the lower punch, and the sintered body in a state in which deformation in the outer diameter direction is restrained by the die is compressed in the axial direction, so that the inner periphery further bites into the molding die. In this way, the shape of the molding die is transferred to the inner periphery of the sintered body, and the dynamic pressure groove 8a1 arrangement areas A1 and A2 are formed on this inner periphery. At this time, the forming die provided on the lower end surface of the upper punch bites into the upper end surface of the sintered body, so that the shape of the forming die of the upper punch is transferred to the upper end surface, forming a corresponding arrangement area of ​​the dynamic pressure grooves 8b1.

[0060] After forming the predetermined dynamic pressure grooves 8a1, 8b1 arrangement regions on the inner peripheral surface and upper end surface of the sintered body in this way, the die is lowered relative to the lower punch to release the restraint state of the sintered body by the die. As a result, the sintered body springs back in the outer diameter direction, making it possible to remove the sintered body from the sizing pin. At this time, the required amount of springback is a size that does not cause the molding die provided on the sizing pin to get caught in the axial direction with the sintered body inner peripheral surface after sizing (especially the dynamic pressure grooves 8a1 arrangement regions A1, A2), so the thickness dimension t of the sintered body is set in consideration of the groove depth (several μm) of the dynamic pressure grooves 8a1 to be formed. In this embodiment, by setting the thickness dimension t to 0.5 mm or more and 1.5 mm or less as described above, the dynamic pressure grooves 8a1 of the required depth can be formed, while the sizing pin used for forming can be pulled out of the sintered body after sizing without getting caught.

[0061] (S4) Oil impregnation process The internal pores of the sintered body obtained as described above are impregnated with lubricating oil as a lubricating fluid, thereby completing the oil-impregnated sintered bearing 8.

[0062] Here, various types of lubricating oils can be used, and for example, ester-based lubricating oils, which have a small evaporation rate and a small decrease in viscosity at low temperatures, and fluorine-based lubricating oils, which have better resistance than ester-based lubricating oils, are preferably used. From the viewpoint of kinetic viscosity, for example, lubricating oils having a kinetic viscosity of 20 cSt or more and 170 cSt or less at 40°C and a kinetic viscosity of 2 cSt or more and 50 cSt or less at 100°C are preferably used.

[0063] The sintered oil-impregnated bearing 8 is fixed to the inner periphery of the housing 7 by known means such as press-fitting, press-fitting with adhesion, adhesion, welding, etc. Thereafter, the shaft portion 10 of the rotating body 3 is inserted into the inner periphery of the sintered oil-impregnated bearing 8 to complete the fluid dynamic bearing device 2. In this case, the interface of the lubricating oil is held in the seal space S (see FIG. 2).

[0064] The above-mentioned oil-impregnating step S4 may be carried out after the sintered body that will become the oil-impregnated sintered bearing 8 is fixed to the inner periphery of the housing 7, for example.

[0065] In the fluid dynamic bearing device 2 configured as above, when the shaft portion 10 (rotor 3) rotates, the regions (two upper and lower dynamic pressure groove 8a1 arrangement regions A1, A2) of the inner peripheral surface 8a of the sintered oil-impregnated bearing 8 that form the radial bearing surface face the outer peripheral surface 10a of the shaft portion 10 via a radial bearing gap. As the shaft portion 10 rotates, the lubricating oil in the radial bearing gap is pushed toward the axial center of each of the dynamic pressure groove 8a1 arrangement regions A1, A2, and the pressure of the lubricating oil rises in the region on the axial center side (here, the band portion 8a3). Due to the dynamic pressure action of the dynamic pressure grooves 8a1, a first radial bearing portion R1 and a second radial bearing portion R2 that support the shaft portion 10 in a non-contact manner so as to be rotatable in the radial direction are configured to be separated in the axial direction.

[0066] Furthermore, in the thrust bearing gap between the upper end surface 8b (area where the dynamic pressure grooves 8b1 are arranged) of the sintered oil-impregnated bearing 8 and the lower end surface 9a1 of the hub portion 9 facing it, an oil film of lubricating oil is formed by the dynamic pressure action of the dynamic pressure grooves 8b1. Then, the pressure of this oil film forms a first thrust bearing portion T1 that supports the rotor 3 in the thrust direction without contact. Furthermore, the lower end portion 10b of the shaft portion 10 is rotatably contact-supported by a thrust receiving portion 11 provided on the bottom 7e of the housing 7, thereby forming a second thrust bearing portion T2 that supports the rotor 3 in the thrust direction by contact.

[0067] As described above, in the sintered oil-impregnated bearing 8 according to this embodiment, when the axial dimension L is reduced (set to 4.8 mm or less) compared to the conventional one, the thickness dimension t is set to 0.5 mm or more and 1.5 mm or less, and the sintered oil-impregnated bearing 8 has a shape that is significantly flatter than the conventional one. That is, the ratio L / D2 of the axial dimension L to the outer diameter dimension D2 of the sintered oil-impregnated bearing 8 is set to a value that is significantly smaller than 1: 0.24 or more and 0.6 or less. By making the sintered oil-impregnated bearing 8 of this shape and size, for example, during the above-mentioned dynamic pressure groove sizing, the radial compression force of the press-in force generated by pressing into the die can be sufficiently transmitted to the inner peripheral surface layer part of the sintered body that becomes the sintered oil-impregnated bearing 8, regardless of the size of the axial dimension L. Therefore, even if the axial dimension L is set to be smaller than the conventional one, the dynamic pressure groove 8a1 arrangement areas A1 and A2 as the radial dynamic pressure generating part can be accurately and stably molded, and the required radial bearing performance can be stably exhibited. Furthermore, by setting the thickness dimension t to 0.5 mm or more, it is possible to ensure the necessary thrust bearing area on the upper end surface 8b of the sintered oil-impregnated bearing 8. As a result, even if a thrust bearing portion (first thrust bearing portion T1) is provided only on the upper end surface 8b side of the sintered oil-impregnated bearing 8, excellent rotation accuracy can be exhibited, so that, for example, simply by inserting the shaft portion 10 of the rotating body 3 into the inner periphery of the sintered oil-impregnated bearing 8, the fluid dynamic bearing device 2 equipped with the sintered oil-impregnated bearing 8 can be assembled at low cost.

[0068] In addition, as in this embodiment, by setting the density ratio of the porous body constituting the sintered oil-impregnated bearing 8 to 86% or more, the press-in force on the die is sufficiently transmitted to the surface layer of the inner peripheral surface of the porous body (sintered body) as a radial pressure force, particularly during dynamic pressure groove sizing. Therefore, it is possible to transfer and form a dynamic pressure groove 8a1 of sufficient depth to the inner peripheral surface of the sintered body. In addition, by suppressing the density ratio to 92% or less, it is possible to suppress excessive load on the sizing die, so that it is possible to stably and continuously perform good dynamic pressure groove sizing. In particular, by setting the axial dimension L of the sintered oil-impregnated bearing 8 to 4.8 mm or less, the thickness dimension t to 0.5 mm or more and 1.5 mm or less, the ratio L / D2 of the axial dimension L to the outer diameter dimension D2 to 0.24 or more and 0.6 or less, and the density ratio to 86% or more and 92% or less, it is possible to further reduce the variation in the density ratio of the porous body constituting the sintered oil-impregnated bearing 8 (to 1% or less). Therefore, it is possible to stably exhibit high rotation performance. Specifically, it will be possible to achieve rotational accuracy (NRRO) of 50 nm or less when using bearings.

[0069] While one embodiment of the present invention has been described above, the sintered oil-impregnated bearing and the fluid dynamic bearing device equipped with this bearing according to the present invention are not limited to the above-described exemplary embodiment and may take any form within the scope of the present invention.

[0070] FIG. 6 shows a cross-sectional view of a fluid dynamic bearing device 12 according to another embodiment of the present invention. As shown in FIG. 6, the fluid dynamic bearing device 12 according to this embodiment differs from the fluid dynamic bearing device 2 shown in FIG. 2 in that it has only a first thrust bearing portion T1. More specifically, in the fluid dynamic bearing device 2 according to this embodiment, a predetermined thrust direction gap always exists between the lower end surface 10c of the shaft portion 10 and the upper end surface 7e1 of the bottom portion 7e of the housing 7. Here, the size of the facing distance (thrust direction gap) between the upper end surface 7e1 of the bottom portion 7e and the lower end surface 10c of the shaft portion 10 is larger than the facing distance between the upper end surface 8b of the sintered oil-impregnated bearing 8 and the lower end surface 9a1 of the disk portion 9a, and is set to a size that is considered to have no substantial effect on the increase in loss torque during rotational driving. Other configurations are the same as those of the fluid dynamic bearing device 2 shown in FIG. 2 and the like, so detailed explanations will be omitted.

[0071] In the fluid dynamic bearing device 12 according to this embodiment, when the axial dimension L is 4.8 mm or less, the thickness dimension t is set to 0.5 mm or more and 1.5 mm or less, and the ratio L / D2 of the axial dimension L to the outer diameter dimension D2 is set to a value significantly smaller than 1: 0.24 or more and 0.6 or less. Therefore, the dynamic pressure groove 8a1 arrangement areas A1 and A2 as the radial dynamic pressure generating parts can be accurately and stably molded, and the required radial bearing performance can be stably exhibited. In addition, since the required thrust bearing area can be secured on the upper end surface 8b of the sintered oil-impregnated bearing 8, even if the thrust bearing part (first thrust bearing part T1) is provided only on the upper end surface 8b side of the sintered oil-impregnated bearing 8, excellent rotation accuracy can be exhibited. Therefore, as shown in FIG. 6, sufficient thrust bearing performance can be exhibited even if the lower end surface 10c of the shaft part 10 is not supported in the thrust direction, and the cost can be reduced by the amount of omission of the thrust receiving part 11 and the simplification of the lower end shape of the shaft part 10.

[0072] Of course, for either or both of the radial dynamic pressure generating portions (dynamic pressure groove 8a1 arrangement areas A1, A2 in Figure 3) formed between the radial bearing portions R1, R2 and the outer peripheral surface 10a of the shaft portion 10, it is possible to adopt known radial dynamic pressure generating portions having shapes other than dynamic pressure grooves, such as so-called multiple arc shapes, step shapes, and wave shapes.

[0073] In the above explanation, the housing 7 of the fluid dynamic bearing device 2 is fixed to the inner periphery of the base 6 of the fan motor 1, but the housing 7 may also be attached directly to, for example, the base (not shown) of an information device to which the fan motor 1 is attached. Alternatively, the parts equivalent to these base parts may be provided integrally with the housing 7.

[0074] In the above description, the magnet 5b and the coil 5a are arranged offset in the axial direction to apply an external force to the shaft portion 10 (rotating body 3) to press the shaft portion 10 against the bottom portion 7e of the housing 7, but the means for applying such an external force to the shaft portion 10 is not limited to the above. Although not shown in the drawings, for example, the magnetic force can be applied to the rotating body 3 by arranging a magnetic member capable of attracting the magnet 5b opposite the magnet 5b in the axial direction. In addition, if the thrust as a reaction force of the air blowing action is sufficiently large and the shaft portion 10 can be pressed downward by this thrust alone, the magnetic force (magnetic attraction force) as an external force for pressing the shaft portion 10 downward may be omitted.

[0075] Furthermore, in the above explanation, the present invention has been described as being applied to a fluid dynamic bearing device 2 in which a rotor 3 with a fan 4 is fixed to the shaft section 10, but the present invention can also be preferably applied to fluid dynamic bearing devices 2 in which a disk hub having a disk mounting surface, or a polygon mirror, is fixed to the shaft section 10 as the rotor 3. That is, the present invention can be preferably applied not only to a fan motor 1 as shown in Fig. 1, but also to fluid dynamic bearing devices 2 incorporated in other electrical equipment, such as spindle motors for disk devices and polygon scanner motors for laser beam printers (LBPs). [Explanation of symbols]

[0076] 1 Fan motor 2,12 Fluid dynamic bearing device 3 Rotating body 4 Fans 5 Drive unit 5a coil 5b Magnet 6 Base 7. Housing 7c Top surface 7d Sealing surface 8 Sintered oil-impregnated bearing 8a Inner surface 8a1 Dynamic pressure groove 8a2 Slope section 8a3 Belt 8b Top surface 8b1 Dynamic pressure groove 8c Lower end surface 8d Outer surface 8d1 Axial groove 9 Hub section 9a Disc Section 9a1 Lower end surface 9b, 9c Cylindrical part 9d Tsubabe 9e Mounting hole 10 Shaft 10a Outer surface 10b Bottom end 10c Lower end surface 11 Thrust receiving part A1, A2 dynamic pressure groove arrangement area D1 Inner diameter D2 Outer diameter L Axial dimension R1, R2 radial bearing section S Sealing space t Thickness dimension T1, T2 Thrust bearing section

Claims

1. A bearing made of sintered metal obtained by compressing metal powder into a cylindrical shape to form a green compact, and sintering the green compact, In a sintered oil-impregnated bearing, the internal pores are impregnated with a lubricating fluid and a radial dynamic pressure generating portion is formed on the inner circumferential surface, The axial dimension L is 4.8 mm or less, The thickness dimension t is 0.5 mm or more and 1.5 mm or less, The ratio L / D2 of the axial dimension L to the outer diameter dimension D2 is 0.24 or more and 0.6 or less, 1. A sintered oil-impregnated bearing, comprising: a thrust dynamic pressure generating portion formed on one axial end face; and a flat end face on the other axial end face.

2. 2. The sintered oil-impregnated bearing according to claim 1, wherein the density ratio is 86% or more and 92% or less.

3. 3. The sintered oil-impregnated bearing according to claim 1, wherein a ratio D2 / D1 of the outer diameter D2 to the inner diameter D1 is 1.5 or more and 3.0 or less.

4. 4. The sintered oil-impregnated bearing according to claim 1, wherein the inner diameter dimension D1 is 1.5 mm or more and 2.0 mm or less.

5. A sintered oil-impregnated bearing made of sintered metal obtained by compressing metal powder into a cylindrical shape to form a green compact and sintering the green compact, wherein the internal pores are impregnated with a lubricating fluid and a radial dynamic pressure generating portion is formed on the inner peripheral surface, the sintered oil-impregnated bearing having an axial dimension L of 4.8 mm or less, a thickness dimension t of 0.5 mm or more and 1.5 mm or less, and a ratio L / D2 of the axial dimension L to the outer diameter dimension D2 of 0.24 or more and 0.6 or less; a housing having the sintered oil-impregnated bearing fixed to its inner periphery; a rotor having a shaft portion that is inserted into the inner periphery of the sintered oil-impregnated bearing; a radial bearing portion that supports the shaft portion in a radial direction in a non-contact manner by a film of the lubricating fluid that is formed in a radial bearing gap between an inner peripheral surface of the sintered oil-impregnated bearing and an outer peripheral surface of the shaft portion due to a dynamic pressure action of the radial dynamic pressure generating portion; a first thrust bearing portion that supports the shaft portion in a non-contact manner in the thrust direction by a film of the lubricating fluid formed in a thrust bearing gap between an end face on the other axial side of the rotor and an end face on one axial side of the sintered oil-impregnated bearing that face each other in the thrust direction; A fluid dynamic bearing device comprising:

6. 6. A fluid dynamic bearing device according to claim 5, wherein a thrust dynamic pressure generating portion is provided on one axial end face of said sintered oil-impregnated bearing which faces in the thrust direction the disk portion of the hub portion as said rotating body.

7. 6. A fluid dynamic bearing device according to claim 5, further comprising a second thrust bearing portion that supports an end portion on the other axial side of said shaft portion in a thrust direction in contact with an end face on one axial side of said housing.

8. A motor comprising the fluid dynamic bearing device according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Dynamic pressure type oil-impregnated sintered bearing and manufacture thereof

    JP1998306827A

  • Dynamic pressure bearing manufacturing method

    JP2006125461A

  • Dynamic pressure bearing device and motor

    JP2007024089A

  • Sintered metal bearing and fluid dynamic pressure bearing device including the same

    JP2015064019A

  • Hydrodynamic porous oil-impregnated bearing and manufacturing method thereof

    JP3607492B2