Resin composition for three-dimensional optical modeling

A resin composition for three-dimensional stereolithography addresses the issues of hardness, heat resistance, and solubility in water-soluble materials by using a reactive monomer-free formulation, enabling easy dissolution in mild solvents and maintaining mold integrity.

JP7560400B2Active Publication Date: 2024-10-02NAGASE CHEMTEX CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021061047
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-31
Publication Date
2024-10-02
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

Conventional water-soluble UV-curable materials used in three-dimensional printers face issues with low hardness and heat resistance, and improving these properties often compromises water solubility, while existing sacrificial molds require strong alkalis for dissolution.

Method used

A resin composition for three-dimensional stereolithography is developed, containing a reactive monomer without bifunctional monomers, along with a water-soluble polymer and photopolymerization initiator, which allows for easy dissolution in mild solvents without strong alkalis, maintaining mold integrity and function.

Benefits of technology

The composition enables the production of a sacrificial mold that maintains form and function, easily dissolving in mild solvents, ensuring high heat resistance and strength without the need for powerful chemicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560400000003
    Figure 0007560400000003
  • Figure 0007560400000001
    Figure 0007560400000001
  • Figure 0007560400000002
    Figure 0007560400000002
Patent Text Reader

Abstract

To provide a resin composition for three-dimensional optical molding for use in a sacrificial mold for a curable resin that dissolve easily without use of strong alkalis or other deleterious chemicals.SOLUTION: In a resin composition for three-dimensional optical molding that contains a reactive monomer, a water-soluble polymer, and a photoinitiator and is used for sacrificial mold of curable resin, the reactive monomer contains substantially no bifunctional monomer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition for three-dimensional stereolithography used for a sacrificial mold of a curable resin, and a method for producing a curable resin molded article using the composition. [Background technology]

[0002] Three-dimensional printers, especially inkjet-type three-dimensional printers, often use water-soluble UV-curable materials as support materials. Such conventional water-soluble UV-curable materials often contain large amounts of water-soluble solvents to maintain water solubility, which poses the problem of low hardness and heat resistance. On the other hand, when trying to improve hardness and heat resistance, there is the problem of losing water solubility.

[0003] Patent Document 1 discloses a sacrificial mold made by a three-dimensional printer for use in injection molding of thermoplastic resin. The sacrificial mold is required to have high heat resistance and strength because it comes into contact with high-temperature and high-pressure thermoplastic resin during molding. For this reason, the sacrificial mold is made from a highly cross-linked composition, and after injection molding, the sacrificial mold needs to be dissolved for a long time in a heated high-concentration alkali. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2020-526413 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a resin composition for three-dimensional stereolithography to be used for a sacrificial mold of a curable resin that dissolves easily without using a poisonous substance such as a strong alkali. [Means for solving the problem]

[0006] The inventors have conducted extensive research into the components of resin compositions for 3D photopolymerization and have discovered that when a sacrificial mold is made from a composition that contains substantially no bifunctional monomers as reactive monomers, the sacrificial mold retains its shape and functions as a mold during the curing process of the curable resin, and that the sacrificial mold can then be easily dissolved and removed without the use of hazardous chemicals such as strong alkalis, thereby completing the present invention.

[0007] That is, the present invention provides A resin composition for three-dimensional stereolithography, comprising a reactive monomer, a water-soluble polymer, and a photopolymerization initiator, and used for a sacrificial mold of a curable resin, comprising: The present invention relates to a resin composition for three-dimensional stereolithography, in which the reactive monomer is substantially free of a bifunctional monomer.

[0008] It is also preferable that the composition contains a polymerization inhibitor.

[0009] It is preferred that the main peak temperature of tan δ of the cured product is 80° C. or higher, and that a 1 mm thick cured product has a remaining thickness of 0.7 mm or less after immersion in room temperature water for 5 hours.

[0010] The reactive monomer is preferably a reactive monomer that, when made into a homopolymer, has a glass transition temperature of 80° C. or higher.

[0011] The Shore D hardness after curing is preferably 60 or more.

[0012] The curable resin is preferably a urethane resin, an epoxy resin or a silicone resin.

[0013] The present invention also relates to a sacrificial mold for use with a curable resin comprising the cured product of the resin composition for three-dimensional stereolithography.

[0014] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: (α) forming a first liquid film made of the resin composition and curing the first liquid film to form a first pattern; (β) a step of forming a second liquid film made of the resin composition so as to be in contact with the first pattern, curing the second liquid film to laminate the second pattern, and producing a sacrificial mold of a curable resin. (γ) placing the sacrificial mold prepared in step (β) in a mold, filling it with a curable resin, and curing it; and (δ) A step of dissolving the sacrificial mold in a solvent The present invention relates to a method for producing a curable resin molded article comprising the steps of:

[0015] The solvent is preferably water having a pH of 5-9.

[0016] Furthermore, it is preferable to include a step of washing the sacrificial mold with a solvent having a Hansen solubility parameter of 25 MPa0.5 or less after step (β). Effect of the Invention

[0017] According to the resin composition for three-dimensional stereolithography of the present invention, a sacrificial mold of an easily soluble curable resin can be produced by a three-dimensional modeling method without using a poisonous substance such as a strong alkali. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is a schematic diagram for explaining a process of forming a sacrificial mold of a curable resin by stereolithography using a resin composition for three-dimensional modeling according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The resin composition for three-dimensional optical modeling of the present invention contains a reactive monomer, a water-soluble polymer, and a photopolymerization initiator, and is used as a sacrificial mold for a curable resin, and is characterized in that the reactive monomer is substantially free of a bifunctional monomer.

[0020] The reactive monomer is preferably a monomer that gives a homopolymer of the reactive monomer with a glass transition temperature of 80° C. or higher. The glass transition temperature is preferably 80° C. or higher, more preferably 100° C. or higher. If the glass transition temperature is lower than 80° C., the heat resistance will be poor. Here, the glass transition temperature may be measured by actually polymerizing a homopolymer, or may be calculated by the atomic group contribution method.

[0021] The reactive monomer is a photocurable monomer that can be cured or polymerized by the action of radicals or ions generated by light irradiation. The photocurable monomer is preferably a monomer having a polymerizable functional group. The number of polymerizable functional groups in the photocurable monomer is one. Examples of the polymerizable functional group include a group having a polymerizable carbon-carbon unsaturated bond such as a vinyl group or an allyl group, and an epoxy group.

[0022] More specifically, for example, radical polymerizable monomers such as (meth)acrylic monomers, cationic polymerizable monomers such as epoxy monomers, vinyl monomers, and diene monomers, etc. Among these, (meth)acrylic monomers and vinyl monomers are preferred in terms of reaction rate.

[0023] Examples of the (meth)acrylic monomer include monomers having a (meth)acryloyl group. For example, (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, neopentyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cetyl (meth)acrylate, ethyl carbitol (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, methoxyethyl (meth)acrylate, and methoxybutyl (meth)acrylate; N-methyl (meth)acrylate, ethyl ... Examples of (meth)acrylic acid amides include ethyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-propyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, Nt-butyl (meth)acrylamide, N-octyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, (meth)acryloyl morpholine, diacetone (meth)acrylamide, styrene, methyl itaconate, ethyl itaconate, vinyl acetate, vinyl propionate, N-vinylpyrrolidone, N-vinylcaprolactam, and 3-vinyl-5-methyl-2-oxazolidinone. Among these, (meth)acrylic acid amides are preferred in terms of reaction rate. Among (meth)acrylic acid amides, (meth)acryloyl morpholine, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, and dimethylaminopropyl acrylamide are preferred. In this specification, acrylic acid and methacrylic acid may be referred to as (meth)acrylic acid, and acrylic acid esters (or acrylates) and methacrylic acid esters (or methacrylates) may be referred to as (meth)acrylic acid esters (or (meth)acrylates).

[0024] Examples of vinyl monomers include vinyl ethers such as polyol poly(vinyl ether), aromatic vinyl monomers such as styrene, and vinylalkoxysilanes. Examples of polyols constituting polyol poly(vinyl ether) include polyols (butanediols) exemplified for acrylic monomers. Examples of diene monomers include isoprene and butadiene.

[0025] The epoxy monomer may be a compound having one epoxy group in the molecule, such as a compound containing an epoxycyclohexane ring or a 2,3-epoxypropyloxy group.

[0026] The content of the reactive monomer in the resin composition for three-dimensional optical molding of the present invention is not particularly limited, but is preferably 99.5 to 1 mass %, more preferably 90 to 60 mass %. If it is less than 1 mass %, the resin tends to have a high viscosity, and if it exceeds 99.5 mass %, the curing shrinkage tends to be large.

[0027] The photopolymerization initiator is activated by the action of light to initiate polymerization of the reactive monomer. Examples of the photopolymerization initiator include radical polymerization initiators that generate radicals by the action of light, as well as those that generate bases (or anions) or acids (or cations) by the action of light (specifically, anion generators and cation generators). The photopolymerization initiator can be selected depending on the type of photocurable monomer, for example, whether it is radically polymerizable or ionically polymerizable. Examples of the radical polymerization initiator (radical photopolymerization initiator) include alkylphenone-based photopolymerization initiators and acylphosphine oxide-based photopolymerization initiators.

[0028] Examples of alkylphenone polymerization initiators include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, and the like.

[0029] Examples of the acylphosphine oxide polymerization initiator include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and the like.

[0030] The amount of the photopolymerization initiator added is preferably 0.01 to 10 parts by weight, more preferably 0.1 to 5 parts by weight, based on 100 parts by weight of the reactive monomer. If the amount is less than 0.01 part by weight, curing tends to be insufficient, and if the amount is more than 10 parts by weight, storage stability tends to be poor and curing tends to be insufficient due to absorption.

[0031] Water-soluble polymers are polymers that swell or dissolve in water, and examples of such polymers include polyalkylene glycols, polyvinyl alcohols, modified polyvinyl alcohols (polyvinyl alcohol-polyacrylate block copolymers, grafted polyvinyl alcohols, etc.), polyesters, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinylpyrrolidone, vinylpyrrolidone-vinylimidazole copolymers, water-soluble alkyd resins, salts of copolymers containing (meth)acrylic acid (sodium salts, amine salts, etc.), and water-soluble polymers having ethylenic double bonds in the side chains.

[0032] The weight average molecular weight of the water-soluble polymer is not particularly limited, but is preferably 500 to 1,000,000, and more preferably 500 to 100,000. If it exceeds 1,000,000, the water solubility of the cured product tends to be impaired, or the solubility in monomers tends to be significantly reduced.

[0033] The mixing ratio of the reactive monomer to the water-soluble polymer is preferably 99.5 / 0.5 to 1 / 99 by weight, and more preferably 60 / 40 to 95 / 5. If the reactive monomer is more than 99.5, the cure shrinkage tends to increase, and if it is less than 1, the resin tends to have a high viscosity.

[0034] The content of the water-soluble polymer in the resin composition for three-dimensional optical molding of the present invention is not particularly limited, but is preferably 0.5 to 99% by mass, more preferably 5 to 40% by mass. If it is less than 0.5% by mass, the curing shrinkage tends to be large, and if it exceeds 99% by mass, the resin tends to have a high viscosity.

[0035] The resin composition may further contain other known curable resins, etc. In addition, the curable resin composition may contain known additives such as dyes, ultraviolet sensitizers, polymerization inhibitors, plasticizers, ultraviolet absorbers, pigments, and surfactants.

[0036] Examples of the polymerization inhibitor include hydroquinone, methylhydroquinone, tert-butyl-hydroquinone, hydroquinone monomethyl ether, 4-methylquinoline, phenothiazine, 2,6-diisobutylphenol, 2,6-di-tert-butyl-4-methylphenol, ammonium-N-nitrosophenylhydroxylamine, ammonium N-nitrosophenylhydroxylamine, etc. The amount of the polymerization inhibitor is preferably 0.001 to 1.0% by mass, more preferably 0.01 to 0.3% by mass, in the total reaction composition.

[0037] The reactive monomer does not substantially contain a bifunctional monomer means that the content of the bifunctional monomer is 10% by mass or less in the total reactive monomer, preferably 5% by mass or less, more preferably 2% by mass or less. If it exceeds 10% by mass, a crosslinking reaction occurs, the crosslinking density of the system increases, and the system becomes less soluble in water. It is also preferable that the reactive monomer does not substantially contain a trifunctional or higher monomer.

[0038] Examples of bifunctional monomers include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 2-n-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, methylene bisacrylamide, etc. Examples of trifunctional monomers include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, etc.

[0039] The resin composition is preferably liquid at room temperature. When the resin composition is liquid at room temperature, it can be easily photo-modeled using a 3D printer or the like. The viscosity of the curable resin composition at 25°C is preferably 5000 mPa·s or less, more preferably 2000 mPa·s or less. The viscosity of the resin composition can be measured at a rotation speed of 20 rpm using a cone-plate type E-type viscometer.

[0040] For the resin composition for three-dimensional stereolithography of the present invention, the main peak temperature of tan δ of the cured product is 80° C. or higher, preferably 100° C. or higher, and more preferably 120° C. or higher. If it is less than 80° C., the heat resistance is insufficient. Tan δ is Tg measured using a dynamic viscoelasticity measuring device (DMA). It can be measured while raising the temperature of the cured product from the low temperature side to the high temperature side (for example, from -100° C. to +200° C.). When multiple peaks exist, the peak temperature of the larger peak (main peak) is used.

[0041] Regarding the resin composition for three-dimensional stereolithography of the present invention, after immersing a 1 mm-thick cured product in water at room temperature for 5 hours, the remaining thickness is 0.7 mm or less, preferably 0.5 mm or less, and more preferably 0 mm or less (i.e., completely dissolved). If it exceeds 0.7 mm, the water solubility becomes insufficient.

[0042] The Shore D hardness of the cured product of the resin composition for three-dimensional stereolithography of the present invention is 60 or more, preferably 70 or more, and more preferably 80 or more. If it is less than 60, the strength tends to be insufficient. Here, the Shore D hardness is measured using a type D durometer in accordance with JIS K7215:1986.

[0043] Regarding the resin composition for three-dimensional stereolithography of the present invention, the elastic modulus Er of the cured product at 80°C is preferably 0.01 GPa or more, more preferably 0.1 GPa or more, and even more preferably 1 GPa or more. If it is less than 0.01 GPa, the strength is insufficient. Moreover, the elastic modulus Er at 25°C is preferably 0.1 GPa or more, more preferably 1 GPa or more. If the elastic modulus Er of the cured product at 25°C is less than 0.1 GPa, the strength is insufficient. Here, the elastic modulus Er can be measured by a viscoelasticity measuring device.

[0044] The resin composition for three-dimensional stereolithography of the present invention can form two-dimensional or three-dimensional objects (or patterns) by various modeling methods, and is particularly suitable for stereolithography. The resin composition for three-dimensional stereolithography is liquid at room temperature, so it may be used, for example, in vat-type stereolithography or ink-jet-type stereolithography.

[0045] The sacrificial mold of the present invention is formed from the cured product of the resin composition for three-dimensional stereolithography described above, and is characterized by being used for a curable resin. The sacrificial mold for a curable resin is one that is dissolved and removed after the curable resin is cured and molded. Examples of the curable resin include urethane resin, epoxy resin, silicone resin, phenolic resin, urea resin, melamine resin, unsaturated polyester resin, diallyl phthalate resin, acrylic resin, and alkyd resin. The curable resin may be either photocurable or thermosetting.

[0046] The method for producing a curable resin molded product of the present invention further comprises the steps of: (α) forming a first liquid film made of the resin composition and curing the first liquid film to form a first pattern; (β) a step of forming a second liquid film made of the resin composition so as to be in contact with the first pattern, curing the second liquid film to laminate the second pattern, and producing a sacrificial mold of a curable resin. (γ) placing the sacrificial mold prepared in step (β) in a mold, filling it with a curable resin, and curing it; and (δ) A step of dissolving the sacrificial mold in a solvent The present invention is characterized by comprising:

[0047] The procedure of the vat-type stereolithography will be described below with reference to Fig. 1. Fig. 1 shows an example of forming a three-dimensional object using a stereolithography device (patterning device) equipped with a resin vat (vat). In the illustrated example, a hanging-type modeling is shown, but there is no particular limitation as long as it is a method capable of three-dimensional stereolithography using a resin composition for three-dimensional modeling. There is also no particular limitation on the method of light irradiation (exposure), and it may be point exposure or surface exposure.

[0048] The patterning apparatus 1 includes a platform 2 having a pattern formation surface 2a, a resin tank 3 containing a resin composition 5 for three-dimensional modeling, and a projector 4 as a light source for a surface exposure method.

[0049] (α) A step of forming a first liquid film and curing it to form a first pattern In step (α), as shown in (a), first, the pattern-forming surface 2a of the platform 2 is immersed in the resin composition 5 for three-dimensional modeling contained in the resin tank 3 while facing the projector 4 (the bottom surface of the resin tank 3). At this time, the height of the pattern-forming surface 2a (or the platform 2) is adjusted so that a liquid film 7a (liquid film a) is formed between the pattern-forming surface 2a and the projector 4 (or the bottom surface of the resin tank 3). Next, as shown in (b), the liquid film 7a is photocured by irradiating light L from the projector 4 toward it (surface exposure), thereby forming a first pattern 8a (pattern a).

[0050] In the patterning apparatus 1, the resin tank 3 serves as a supply unit for the resin composition 5 for three-dimensional modeling. At least a portion of the resin tank between the liquid film and the projector 4 (the bottom surface in FIG. 1) is desirably transparent to the exposure wavelength so that the liquid film is irradiated with light from a light source. The shape, material, size, etc. of the platform 2 are not particularly limited.

[0051] After the liquid film a is formed, the liquid film a is photocured by irradiating light from a light source toward the liquid film a. The light irradiation can be performed by a known method. The exposure method is not particularly limited, and may be point exposure or surface exposure. As the light source, a known light source used for photocuring can be used. In the case of the point exposure method, for example, a plotter type, a galvano laser (or galvano scanner) type, an SLA (stereolithography) type, etc. are mentioned. In the case of the surface exposure method, a projector is preferable as the light source in terms of simplicity. As the projector, an LCD (transmissive liquid crystal) type, an LCoS (reflective liquid crystal) type, and a DLP (registered trademark, Digital Light Processing) type, etc. are mentioned. The exposure wavelength can be appropriately selected according to the components of the curable resin composition (particularly, the type of initiator).

[0052] (b) forming a second liquid film in contact with the first pattern, curing the second liquid film to laminate the second pattern, and producing a sacrificial mold of a curable resin; In step (β), a three-dimensional modeling resin composition 5 is supplied between the pattern a obtained in step (α) and a light source to form a liquid film (liquid film b). That is, the liquid film b is formed on the pattern a formed on the pattern formation surface. The supply of the three-dimensional modeling resin composition 5 is the same as in step (α).

[0053] 1(c), after the first pattern 8a (two-dimensional pattern a) is formed, the first pattern forming surface 2a may be raised together with the platform 2. Then, by supplying a curable resin composition 5 between the first pattern 8a and the bottom surface of the resin tank 3, a liquid film 7b (liquid film b) can be formed.

[0054] The formed liquid film b is exposed to light from a light source to photo-cure the liquid film b, and another pattern (pattern b obtained by photo-curing the liquid film b) is laminated on the first pattern a. By laminating the patterns in the thickness direction in this manner, a three-dimensional modeling pattern can be formed.

[0055] For example, as shown in (d) of FIG. 1, the liquid film 7b (liquid film b) formed between the first pattern 8a (pattern a) and the bottom surface of the resin tank 3 is exposed to light from the projector 4 to photo-cure the liquid film 7b. This photo-cure converts the liquid film 7b into the second pattern 8b (pattern b). In this way, the second pattern 8b can be laminated on the first pattern 8a. For the light source, exposure wavelength, etc., see the description of step (i).

[0056] Step (β) can be repeated multiple times. By repeating the process, multiple patterns b are stacked in the thickness direction, resulting in a more three-dimensional pattern. The number of repetitions can be appropriately determined depending on the shape and size of the desired three-dimensional object (three-dimensional pattern).

[0057] For example, as shown in (e) of FIG. 1, the platform 2 is raised in a state in which a first pattern 8a (pattern a) and a second pattern 8b (pattern b) are laminated on the pattern forming surface 2a. At this time, a liquid film 7b (liquid film b) is formed between the second pattern 8b and the bottom surface of the resin tank 3. Then, as shown in (f) of FIG. 1, the liquid film 7b is exposed to light from the projector 4, and the liquid film 7b is photocured. As a result, another pattern 8b (pattern b) is formed on the first pattern 8b. Then, by alternately repeating (e) and (f), a plurality of patterns 8b (two-dimensional patterns b) can be laminated.

[0058] The method for producing a curable resin molded product of the present invention preferably further includes a step of washing the first pattern and the second pattern with a solvent. Since the uncured curable resin composition adheres to the obtained three-dimensional molded pattern, this step is performed to remove the composition. The solvent has a Hansen solubility parameter of 25 MPa. 0.5 The following are preferred: Specific solvents include 3-methoxy-3-methyl-1-butanol, and the like.

[0059] The obtained three-dimensional pattern may be post-cured as necessary. The post-curing may be performed by irradiating the pattern with light. The light irradiation conditions may be appropriately adjusted depending on the type of resin composition and the degree of curing of the obtained pattern. The post-curing may be performed on a part of the pattern or on the entire pattern.

[0060] (γ) A process in which the sacrificial mold made in step (β) is placed in the mold, and curable resin is filled and cured. As the curable resin, not only photocurable resin but also thermosetting resin can be used. As the curable resin, the above-mentioned urethane resin, epoxy resin, condensation type silicone resin, deep silicone resin, phenol resin, urea resin, melamine resin, unsaturated polyester resin, diallyl phthalate resin, acrylic resin, alkyd resin, etc. can be mentioned. Among the silicone resins, condensation type silicone resin is preferable from the viewpoint of colorability and curing inhibition.

[0061] (δ) A step of dissolving the sacrificial mold in a solvent As a solvent for dissolving the sacrificial mold accompanying the curable resin molded article obtained in step (γ), water having a pH of 5 to 9 is preferred, and a pH of 6 to 8 is more preferred. EXAMPLES

[0062] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples. In the following, "parts" and "%" mean "parts by weight" and "% by weight", respectively, unless otherwise specified.

[0063] Various chemicals used in the examples and comparative examples will be collectively described below.

[0064] <<Monofunctional acrylate>> Acryloylmorpholine (ACMO): homopolymer Tg 144℃, manufactured by KJ Chemicals Co., Ltd. 3-vinyl-5-methyl-2-oxazoline (VMOX): homopolymer Tg 173°C, manufactured by BASF Dimethylacrylamide (DMAA): homopolymer Tg 119℃, manufactured by KJ Chemicals Co., Ltd. Diethylacrylamide (DEAA): homopolymer Tg 81℃, manufactured by KJ Chemicals Co., Ltd. Hydroxyethylacrylamide (HEAA): homopolymer Tg 98℃, manufactured by KJ Chemicals Co., Ltd. Dimethylaminopropylacrylamide (DMAPAA): homopolymer Tg 134℃, manufactured by KJ Chemicals Co., Ltd.

[0065] <<Bifunctional acrylate>> PEG#400 diacrylate (4EG-A): Tg 50°C, manufactured by Kyoeisha Chemical Co., Ltd. PEG#600 diacrylate (9EG-A): Tg-9°C, manufactured by Kyoeisha Chemical Co., Ltd.

[0066] <<Water-soluble polymer>> Polyethylene glycol (PEG600): Molecular weight 600, melting point 15 - 25°C Polyethylene glycol (PEG4000): Molecular weight 4000, manufactured by NOF Corporation Polyvinylpyrrolidone (PVP K-15): Tg 120°C, weight average molecular weight 6000 - 15000, manufactured by Ashland Japan Co., Ltd. Polyester (Plaskote Z-221): Manufactured by Gohsei Chemical Industry Co., Ltd.

[0067] <<Photoinitiator>> 2,4,6-Trimethylbenzoyl-diphenyl-phosphine oxide (Omnirad TPO-H): Manufactured by IGM resin Bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Omnirad 819): Manufactured by IGM resin

[0068] <<Polymerization inhibitor>> t-Butylhydroquinone (TBHQ): Manufactured by Tokyo Chemical Industry Co., Ltd.

[0069] <<Curable resin>> Urethane resin 1 (non-repellent, Clear Flex95 manufactured by smooth on) Silicone resin 1 (condensation type, KE-108 manufactured by Shin-Etsu Chemical Co., Ltd.) Silicone resin 2 (addition type, KE-1606 manufactured by Shin-Etsu Chemical Co., Ltd.) Silicone resin 3 (addition type, KE-1307 manufactured by Shin-Etsu Chemical Co., Ltd.)

[0070] Examples 1 - 9 and Comparative Examples 1 - 3 Acrylate, water-soluble polymer, photoinitiator, and polymerization inhibitor were mixed in the respective components and compounding amounts shown in Table 1. While stirring, heating was performed in an oven at 80°C to dissolve the solid components, thereby preparing a uniform liquid resin composition. The following evaluations were performed using the obtained resin composition. The evaluation results are shown in Table 1.

[0071] <tanδ peak temperature and elastic modulus Er> Approximately 1 g of the resin compositions prepared in the examples and comparative examples was sandwiched between glass plates, and using a UV irradiation device (manufactured by Aitech System Co., Ltd.), irradiation was performed every 60 seconds at 7 mW / cm 2 to produce a glass plate having a cured product formed on one side with a thickness of about 1 mm. For the obtained samples, using a DVA-2000 (manufactured by AIT Measurement & Control Co., Ltd.), the temperature was raised from -100 °C to +200 °C at a heating rate of 5 °C / min and a frequency of 1 Hz. Then, the elastic modulus Er at 25 °C and 80 °C was determined, and the temperature at which tanδ became the top peak was determined as the Tg of the cured product of the resin composition. When there were multiple peaks at which tanδ was maximum, the peak temperature of the larger peak (the Tg of the polymer serving as the matrix) was taken.

[0072] <Water solubility> Using the method described in <tanδ peak temperature and elastic modulus Er>, a glass plate having a cured product formed on one side with a thickness of about 1 mm was produced. After immersing in 100 g of water (pH 7) at room temperature for 5 hours, the film thickness was measured. Evaluation was performed according to the following evaluation criteria. 〇: Film thickness is 0.7 mm or less ×: Film thickness exceeds 0.7 mm

[0073] <Shore D hardness> Using an LCD type 3D printer (manufactured by Phrozen, Phrozen Shuffle XL), under the conditions of an irradiation time of 5 seconds per layer and a pitch of 50 μm in the z-axis (height direction), strip-shaped samples (length 35 mm × width 20 mm × thickness (height) 6 mm) were produced. Using a type D durometer, in accordance with JIS K7215:1986, the Shore D hardness was measured.

[0074]

Table 1

[0075] As shown in Table 1, the resin compositions of Examples 1 to 8 had high tan δ main peak temperatures, high elastic modulus at 80°C, and excellent water solubility. On the other hand, the resin composition of Comparative Example 1 had a low tan δ main peak temperature, and the elastic modulus at 80°C could not be measured. The resin compositions of Comparative Examples 2 and 3 had low tan δ main peak temperatures and high elastic modulus at 80°C, but gelled and did not have water solubility.

[0076] Examples 10 to 14 and Comparative Example 4 Using the resin compositions for three-dimensional photopolymerization prepared in Examples 2 and 3 and Comparative Example 2, a sacrificial mold was created using a 405 nm LCD type 3D printer for a hollow box-shaped object with the CAD of the desired structure.

[0077] A hollow box-shaped object was created using a resin composition for three-dimensional stereolithography, and a hardening resin was injected into the hole using a syringe. After sealing the hole, the box-shaped object was placed in an oven at 80°C for one hour to completely harden the hardening resin inside, and then removed from the oven.

[0078] The sacrificial mold with the cured resin inside was removed by immersing it in room temperature water in a container overnight. The curable resin was then dried. The Shore A hardness, the following dimensions, and the cleanliness of the hole were evaluated using the obtained cured product of the curable resin. The evaluation results are shown in Table 2.

[0079] <Dimensions> A sacrificial mold was created as a hollow block measuring 3 cm x 3 cm x 1 cm, and the dimensions after molding of the curable resin were measured and evaluated according to the following criteria, where a minus sign indicates that the object molded in the sacrificial mold became thicker, resulting in a smaller curable resin when transferred. ○: Within 3cm±0.05, ×: 3cm±0.1mm or more

[0080] <Cleaning the holes> The removal status of the sacrificial mold from holes of about 3 mm such as those in a honeycomb structure was visually observed and evaluated according to the following criteria. 〇: Completely removed △: A little bit remains, can be removed with time ×: Remains and is difficult to remove even after a long time

[0081] [Table 2]

[0082] As shown in Table 2, in the sacrificial mold made from the composition of Comparative Example 2 using a bifunctional monomer (Comparative Example 4), it was difficult to clean with water alone, and it was difficult to remove the fine holes. On the other hand, in the sacrificial mold made from the composition of Example 2 not using a bifunctional monomer and a polymerization inhibitor (Example 10), the sacrificial mold was thickened, the dimensional accuracy of the curable resin was somewhat poor, and it took a little time to remove the fine holes. However, it was usable as a sacrificial mold. In the sacrificial mold made from the composition of Example 2 or 3 using a polymerization inhibitor (Examples 11 to 14), there were no problems with the dimensions or the cleanliness of the hole parts, and they were excellent as sacrificial molds. [Explanation of symbols]

[0083] 1:Stereolithography device 2: Platform 2a: Patterned surface 3:Resin tank 4: Projector 5: Resin composition for three-dimensional modeling 6: Release agent layer 7a: Liquid film a 7b: Liquid film b 8a: First pattern a 8b: Second pattern b L:Light

Claims

1. A resin composition for three-dimensional stereolithography, comprising a reactive monomer, a water-soluble polymer, and a photopolymerization initiator, and used for a sacrificial mold of a curable resin, comprising: the water-soluble polymer is polyvinylpyrrolidone or a water-soluble polyester; A resin composition for three-dimensional optical molding, in which the reactive monomer is substantially free of a bifunctional monomer.

2. The resin composition for three-dimensional stereolithography according to claim 1, further comprising a polymerization inhibitor.

3. The main peak temperature of tan δ of the cured product is 80° C. or higher, 3. The resin composition for three-dimensional stereolithography according to claim 1, wherein a cured product having a thickness of 1 mm has a remaining thickness of 0.7 mm or less after immersion in water at room temperature for 5 hours.

4. The resin composition for three-dimensional optical molding according to any one of claims 1 to 3, wherein the reactive monomer is a reactive monomer having a glass transition temperature of 80°C or higher when made into a homopolymer.

5. The resin composition for three-dimensional optical molding according to any one of claims 1 to 4, which has a Shore D hardness of 60 or more after curing.

6. 6. The resin composition for three-dimensional optical molding according to claim 1, wherein the curable resin is a urethane resin, an epoxy resin or a silicone resin.

7. A sacrificial mold for use with a curable resin, which is formed from a cured product of the resin composition for three-dimensional stereolithography according to any one of claims 1 to 6.

8. (α) forming a first liquid film made of the resin composition according to any one of claims 1 to 6, and curing the first liquid film to form a first pattern; (β) A step of forming a second liquid film made of the resin composition according to any one of claims 1 to 6 so as to be in contact with the first pattern, curing the second liquid film to laminate the second pattern, and producing a sacrificial mold of a curable resin. (γ) placing the sacrificial mold produced in step (β) in a mold, filling it with a curable resin, and curing it; and (δ) Dissolving the sacrificial mold in a solvent A method for producing a curable resin molded article comprising the steps of:

9. The method for producing a curable resin molded article according to claim 8, wherein the solvent is water having a pH of 5 to 9.

10. Furthermore, after step (β), a step of washing the sacrificial mold with a solvent having a Hansen solubility parameter of 25 MPa or less. The method for producing a curable resin molded article according to claim 8 or 9, comprising:

Citation Information

Patent Citations

  • Active energy ray curable composition, cured article, composition accommodation container, image formation device and image formation method

    JP2017075296A

  • Support material composition

    JP2019206113A

  • Additive manufacturing device and system for producing a sacrificial mold for creating an object

    JP2019509192A

  • Additively manufactured sacrificial molds used in injection molding processes