Secondary battery cell having solid polymer electrolyte

The semi-IPN SPE addresses the limitations of conventional liquid electrolytes by offering a mechanically stable and highly conductive solid electrolyte, enhancing battery safety and performance for high-voltage applications.

JP7560579B2Active Publication Date: 2024-10-02CMC MATERIALS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022575333
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-08
Filing Date
2021-06-07
Publication Date
2024-10-02
Estimated Expiration
2041-06-07

AI Technical Summary

Technical Problem

Conventional liquid electrolytes in secondary batteries are toxic, flammable, and lack mechanical stability and high ionic conductivity, posing safety and performance issues.

Method used

Development of a semi-interpenetrating polymer network (semi-IPN) solid polymer electrolyte (SPE) using a cellulose polymer matrix with dispersed ceramic particles and plasticizers, enhancing mechanical strength and ionic conductivity.

Benefits of technology

The semi-IPN SPE provides high thermal stability, improved safety, and increased energy density, enabling thinner battery designs suitable for high-voltage applications and reduced production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560579000005
    Figure 0007560579000005
  • Figure 0007560579000006
    Figure 0007560579000006
  • Figure 0007560579000007
    Figure 0007560579000007
Patent Text Reader

Abstract

The secondary battery cell includes a cathode of a first electrode material, an anode of a second electrode material, and a solid polymer electrolyte layer disposed between the cathode and the anode. The solid polymer electrolyte includes a first surface in contact with the cathode and a second surface in contact with the anode. The solid polymer electrolyte layer includes a cellulose polymer matrix. The cellulose polymer matrix includes a cellulose polymer network. Lithium ions are dispersed in the cellulose polymer matrix. Ceramic particles are dispersed in the cellulose polymer matrix. The ceramic particles include a metal oxide. One or more plasticizers are dispersed in the cellulose polymer matrix. The one or more polymer networks are in contact with the cellulose polymer matrix. The one or more polymer networks include an acrylate-containing polymer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates generally to electrodes, and more specifically to secondary battery cells having solid polymer electrolytes. [Background technology]

[0002] Secondary energy cells, such as those used in rechargeable batteries, facilitate repeated depletion and recharging of electrical energy. In a secondary battery or cell, the chemical reactions that facilitate energy storage in the positive and negative electrodes are reversible. The electrodes of a secondary battery or cell can be regenerated (i.e., recharged) multiple times by applying an electrical charge thereto. Summary of the Invention [Means for solving the problem]

[0003] In one embodiment, a solid polymer electrolyte precursor composition comprises: (i) one or more organic solvents; (ii) one or more cellulose polymers dissolved in the one or more organic solvents; (iii) one or more polymerizable components dissolved or dispersed in the one or more organic solvents; and (iv) one or more photoinitiators dissolved or dispersed in the one or more organic solvents, wherein at least one of the one or more photoinitiators promotes polymerization of at least one of the one or more polymerizable components following irradiation with light. (v) one or more photoinitiators that promote the formation of a lithium ion source, each lithium ion source comprising a lithium ion salt or a lithium ion complex, (vi) one or more plasticizers dissolved or dispersed in said one or more organic solvents, and (vii) one or more ceramic particles dissolved or dispersed in said one or more organic solvents, the ceramic particles comprising a metal oxide.

[0004] In another embodiment, a method for preparing a solid polymer electrolyte precursor composition includes dissolving one or more cellulose polymers in one or more organic solvents, thereby preparing a polymer solution in the solvent. Combining one or more polymerizable components with the polymer solution in the solvent. Combining one or more photoinitiators with the polymer solution in the solvent, at least one of the one or more photoinitiators promoting polymerization of at least one of the one or more polymerizable components following irradiation with light, and combining one or more sources of lithium ions with the polymer solution in the solvent. Each source of lithium ions comprises a lithium ion salt or a lithium ion complex. Combining one or more plasticizers with the polymer solution in the solvent. Combining one or more ceramic particles with the polymer solution in the solvent. The ceramic particles comprise a metal oxide.

[0005] In yet another embodiment, a secondary battery cell includes a cathode of a first electrode material, an anode of a second electrode material, and a solid polymer electrolyte layer disposed between the cathode and the anode. The solid polymer electrolyte includes a first surface in contact with the cathode and a second surface in contact with the anode. The solid polymer electrolyte layer includes a cellulose polymer matrix. The cellulose polymer matrix includes a cellulose polymer network. Lithium ions are dispersed in the cellulose polymer matrix. Ceramic particles are dispersed in the cellulose polymer matrix. The ceramic particles include a metal oxide. One or more plasticizers are dispersed in the cellulose polymer matrix. The one or more polymer networks are in contact with the cellulose polymer matrix (e.g., extend at least partially into the cellulose polymer matrix network). The one or more polymer networks include an acrylate-containing polymer.

[0006] In yet another embodiment, a method of making a semi-interpenetrating polymer network solid polymer electrolyte includes making a precursor. The precursor is made by combining one or more cellulose polymers with one or more organic solvents. One or more polymerizable components are combined with one or more organic solvents. One or more photoinitiators are combined with one or more organic solvents. At least one of the one or more photoinitiators promotes polymerization of at least one of the one or more polymerizable components following irradiation with light. One or more lithium ion sources are combined with one or more organic solvents. Each lithium ion source comprises a lithium ion salt or lithium ion complex. One or more plasticizers are combined with one or more organic solvents. One or more ceramic particles are combined with one or more organic solvents. The ceramic particles comprise a metal oxide. At least a portion of the precursor is deposited on a surface of a substrate. The deposited precursor is exposed to light (eg, irradiated with light). Effect of the Invention

[0007] Most secondary batteries employ liquid electrolytes to facilitate charge transfer between the anode and the cathode. However, such electrolytes have some drawbacks. For example, liquid electrolytes may be toxic and / or flammable, so electrolyte leakage may cause significant harm. Several alternative electrolytes have been developed. However, these electrolyte materials are generally not suitable for many applications due to poor mechanical stability and / or low ionic conductivity at room temperature. Adding ceramic particles is insufficient to increase conductivity.

[0008] The present disclosure recognizes that materials used as both the separator between electrodes and the electrolyte in an electrochemical cell should include the following properties: (1) chemical compatibility with the electrode materials used in the cell, (2) sufficient mechanical strength to withstand the rigors of manufacture and use, (3) the ability to be prepared in reasonable thicknesses (i.e., thin materials may be desirable to minimize ion transport distances and maximize ion transport rates), and (4) high ionic conductivity at room temperature. The unique semi-interpenetrating polymer network solid polymer electrolytes (semi-IPN SPEs), and related precursor compositions described in this disclosure, overcome the problems of the prior art and provide the desired properties identified above.

[0009] The semi-IPN SPE described in this disclosure has a molecular weight of 10 per centimeter at room temperature. -3 The semi-IPN SPEs provide a siemens (S / cm) or approaching this value, and thus can be used in place of conventional liquid electrolytes. The semi-IPN SPEs have high thermal stability. The high thermal stability facilitates the production of secondary cells with simplified casing modules and cooling systems, thereby reducing the weight and volume of batteries containing such cells and increasing the energy density of such batteries. Multiple cells prepared as described in this disclosure can be combined (e.g., stacked) into a single unit to facilitate the preparation of batteries having large capacities and / or providing high voltages. The preparation processes described in this disclosure are compatible with high throughput approaches, such as roll-to-roll fabrication. These preparation processes can also proceed at relatively low temperatures, resulting in reduced costs and improved safety compared to conventional electrolyte preparation strategies. The semi-IPN SPEs have high electrochemical stability, making them suitable for high voltage applications (e.g., portable power tools, electric vehicles, etc.). For example, the semi-IPN SPEs described in this disclosure can provide a wide electrochemical window (e.g., up to 5V or more), which facilitates the use of high voltage electrode materials.

[0010] Certain embodiments may include none, some, or all of the above technical advantages, and one or more other technical advantages will be readily apparent to one of ordinary skill in the art from the drawings, specification, and claims contained herein.

[0011] For an aid in understanding the present disclosure, reference is now made to the following descriptions taken in conjunction with the accompanying drawings, in which: [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a diagram showing precursor compositions for preparing semi-interpenetrating network solid polymer electrolyte films according to an exemplary embodiment of the present disclosure. [Diagram 2] FIG. 2 is a diagram illustrating an example cell prepared using the solid polymer electrolyte film of FIG. [Diagram 3] FIG. 3 is a flow chart illustrating an example method for preparing the precursor and solid polymer electrolyte film of FIG. [Figure 4] FIG. 4 is a Bode plot showing impedance versus frequency response for cells having semi-interpenetrating network solid polymer electrolyte films prepared using different precursor compositions. [Diagram 5] FIG. 5 is a plot showing dynamic mechanical analysis for an example solid polymer electrolyte film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] It should be understood at the outset that although examples of embodiments of the disclosure are set forth below, the disclosure may be practiced using any number of techniques, whether currently known or not. The disclosure should in no way be limited to the examples, drawings, and techniques set forth below. Additionally, the drawings are not necessarily drawn to scale.

[0014] As discussed above, recent advances in portable electronic devices have been accompanied by an increasing demand for rechargeable batteries with improved characteristics (e.g., lower cost, increased energy density, improved safety, etc.). Lithium metal and lithium ion secondary cells typically have increased electrical energy storage capacity, or energy density, compared to that of other cell types (e.g., nickel-metal hydride). For convenience, the terms "lithium secondary cell" and "lithium cell" are used herein to refer to both lithium metal and lithium ion types of batteries and secondary cells.

[0015] A conventional lithium secondary cell may include a porous dielectric separator or diaphragm interposed between the electrodes of the cell and a liquid electrolyte. The liquid electrolyte provides ionic conductivity such that charge can be transferred between the electrodes. The liquid electrolytes widely employed in lithium cells generally provide acceptable ionic conductivity for adequate cell performance. However, the use of liquid electrolytes entails several drawbacks. For example, liquid electrolytes are prone to leaking from the cell in which they are sealed. These electrolytes may contain harmful materials. Thus, leakage may not only result in reduced cell performance (i.e., due to loss of ionic conductivity), but may also harm people and / or the environment. Cells employing liquid electrolytes also tend to have stricter size constraints, so cells with liquid electrolytes tend to be larger than may be desired or of impractical shapes for a given purpose. Other conventional electrolytes generally lack the appropriate combination of electrical and mechanical properties required for many battery applications (e.g., portable electronic devices, portable power tools, satellite technology, electric vehicles, etc.). For example, conventional alternatives to liquid electrolytes generally lack sufficiently high ionic conductivity and / or sufficient mechanical strength for reliable performance in most applications.

[0016] The non-conventional semi-interpenetrating polymer network solid polymer electrolytes (semi-IPN SPEs) described in the present disclosure provide a solution to the technical problems of conventional electrolytes, including those mentioned above, by providing electrolytes that are safer than liquid electrolytes and have sufficient mechanical strength and ionic conductivity for modern applications. The exemplary advantages of the compositions and methods described in the present disclosure may be derived, at least in part, from the unexpected synergistic effects of the components contained in the semi-IPN SPE precursors. The cellulose polymers used to form the polymer matrix in the semi-IPN SPEs effectively solubilize lithium ions due to the large amount of oxygen atoms present in each saccharide unit of the cellulose polymer. However, the mechanical properties (strength and stability) of films prepared from such cellulose matrices may be reduced by the addition of lithium ions. In an exemplary embodiment, the mechanical strength and stability of solid polymer electrolytes prepared from these materials can be increased by appropriately incorporating another polymer network with the cellulose polymer matrix described herein to obtain the desired mechanical properties. In another exemplary embodiment, the addition of ceramic particles not only improves the mechanical properties of the semi-IPN SPE, but also enhances the ionic conductivity of the semi-IPN SPE. The ionic conductivity can be improved using the process described in this disclosure. The ceramic particles are maintained in a well-dispersed state before the preparation of the semi-IPN SPE film. For example, a stable cellulose slurry can be prepared. In the cellulose slurry, the ceramic particles remain well-dispersed (e.g., homogeneously) before the formation of the semi-IPN SPE.

[0017] Semi-IPN solid polymer electrolyte FIG. 1 shows an example of a semi-IPN solid polymer electrolyte 100. The electrolyte 100 is generally prepared from a precursor 102. The precursor includes (a) one or more polymers 104 (e.g., one or more cellulose polymers), (b) one or more photochemically or thermally polymerizable components 106, (c) one or more lithium ion sources 108 (e.g., one or more lithium salts and / or lithium complexes), (d) one or more organic solvents 110, (e) one or more plasticizers 112, (f) one or more photoinitiators 114, and (g) one or more metal oxide nanoparticles 116. In some embodiments, the precursor 102 may further include a low molecular weight vinyl backbone polymer 118. Examples of the various components 104, 106, 108, 110, 112, 114, 116, 118 of the precursor 102 are described in detail below. Illustrative examples are described below with respect to the various components 104, 106, 108, 110, 112, 114, 116, 118, although it will be appreciated that other possible such components 104, 106, 108, 110, 112, 114, 116, 118 will be readily apparent to one of ordinary skill in the art in light of this disclosure.

[0018] As described in more detail below in connection with FIG. 3, a subset 103 of components of precursor 102 (i.e., subset 103 includes one or more of components 104, 106, 110, 112, 114, 116, and / or 118) may be first combined (e.g., via mixing under appropriate conditions). For example, the components of subset 103 may be mixed under predetermined conditions (e.g., room temperature) so that a thermochemical reaction (e.g., thermal reduction) does not proceed prematurely to a significant extent. In some embodiments, subset 103 includes all of precursor 102 except for lithium ion source 108. The subset 103 of components may be prepared as a “premixed” solution, and the lithium ion source 108 (e.g., lithium salt and / or complex) may then be added to the premixed solution at room temperature or in a controlled manner under appropriate heating. 1, the resulting precursor 102 can be applied to a substrate and heated and / or exposed to light 120 to produce a semi-IPN SPE 100 film (e.g., a thin film). An example method for preparing a semi-IPN SPE 100 film is described in more detail below in conjunction with FIG.

[0019] Table 1 below shows an example composition of precursor 102. Precursor 102 includes components 104, 106, 108, 112, 114, 116, and optionally 118 dissolved and / or dispersed in liquid solvent 110. Exemplary ranges for the amounts of each component 104, 106, 108, 110, 112, 114, 116, and 118 that may be included in the precursor are shown in Table 1. In an exemplary embodiment, the precursor 102 comprises 41% cellulose acetate propionate (CAP) (i.e., polymer 104), 11% polyethylene glycol (200) diacrylate (SR 259) and 6% alkoxylated pentaerythritol tetraacrylate (SR 494) (i.e., acrylic monomers 106 as polymerizable components 106), 19% lithium iodide (i.e., lithium ion source 108), 6% polycaprolactone triol (i.e., plasticizer 112), and 17% titanium dioxide particles (i.e., ceramic particles 116), dissolved and / or dispersed in one or more solvents 110. [Table 1]

[0020] As discussed above and in more detail below in connection with FIG. 3, the semi-IPN SPE 100 may be prepared as a thin film (e.g., from a few micrometers to tens of micrometers in thickness) on a substrate. The relative amounts of components in the precursor 102 may be selected to facilitate improved mechanical and electrical properties of the resulting semi-IPN SPE 100 as well as to enable reliable and efficient thin film processing. For example, the solid polymer electrolyte precursor 102 may include at least 5% solids (e.g., all components except the solvent 110) and no more than 90% solids. In some embodiments, the precursor 102 includes at least 15% solids and no more than 50% solids. In some embodiments, the total amount of solids and organic solvent 110 may be selected to adjust the viscosity of the precursor 102 for a particular deposition method (e.g., for preparing a thin film of the precursor 102). For example, the precursor 102 may be a mixture having a viscosity of at least 1 centipoise (cP) and no more than 5,000 cP. In some embodiments, the viscosity of the precursor 102 is at least 3 cP and no greater than 50 cP. All of the above example viscosity values ​​are measured at about 25°C.

[0021] The semi-IPN SPE 100 generally comprises one or more cellulosic polymer networks (i.e., networks of polymers 104) as shown in Figure 1. The semi-IPN SPE 100 also comprises one or more linear or branched polymers 106a (i.e., polymers produced via polymerization of polymerizable components 106, which polymerization can be facilitated by a photoinitiator 114 after exposure to light). The polymers at least partially "penetrate" or extend into one of the polymer networks on a molecular scale. In some embodiments, the semi-IPN SPE 100 film comprises 25-60% by weight of one or more polymers 104, 10-25% by weight of polymerizable component 106 (and / or polymer 106a derived therefrom), 20-35% by weight of lithium source 108, 1-10% by weight of plasticizer 112, 0.1-5% by weight of photoinitiator 114 (and / or by-products derived therefrom), and 10-25% by weight of ceramic particles 116. The weight percentages are based on the total weight of components 104, 106, 108, 112, 114, and 116 in the semi-IPN SPE 100. The semi-IPN SPE 100 can be a thin film (e.g., less than 500 micrometers thick). In some embodiments, the semi-IPN SPE 100 has a thickness of less than 150 micrometers. In some embodiments, the thickness of the semi-IPN SPE 100 is less than 100 micrometers. In some embodiments, the thickness of the semi-IPN SPE 100 is between about 10 micrometers and less than 100 micrometers. The ionic conductivity of the semi-IPN SPE 100 is 1x10 -4 In some embodiments, the ionic conductivity is 5×10 S / cm or more. -4 In some embodiments, the ionic conductivity is 1x10 S / cm or more. -3 S / cm or more.

[0022] FIG. 2 illustrates an example of a lithium cell 200 (e.g., a secondary cell or battery) prepared using the semi-IPN SPE 100 of FIG. 1. The cell 200 includes a first electrode 202 and a second electrode 204 separated by the SPE 100. The first and second electrodes 202, 204 may be any suitable electrode material for use in a secondary cell or battery. For example, the first electrode 202 may be formed to act as a cathode (i.e., positive electrode) and may be any suitable cathode material, such as lithium, lithium cobalt oxide, lithium iron phosphate, lithium manganate, or the like. The second electrode 204 may be formed to act as an anode (i.e., negative electrode) and may be any suitable anode material, such as lithium, graphite, graphite-containing materials, silicon-containing materials, or the like. The thickness 206 of the semi-IPN may be less than 200 micrometers. In some embodiments, the thickness 206 of the semi-IPN SPE 100 is less than 150 micrometers. In some embodiments, the thickness 206 of the semi-IPN SPE 100 can be less than 100 micrometers. In some embodiments, the thickness 206 of the semi-IPN SPE 100 is between about 10 micrometers and less than 100 micrometers.

[0023] Polymer 104 Example In some embodiments, the one or more polymers 104 of the electrolyte precursor 102 include one or more cellulose polymers. For example, the polymer 104 may include one or more cellulose ester polymers. The polymer 104 may be an organic polymer. A single polymer 104 may be employed in the precursor 102. However, in some embodiments, a mixture of polymers 104 is used. When the precursor 102 includes multiple different polymers 104, two or more different polymers 104 may be present in the same or different amounts. In some embodiments, the polymer 104 includes one or both of one or more cellulose esters and one or more cellulose acetate polymers. In some embodiments, the polymer 104 includes a modified cellulose ester. The modified cellulose ester is formed by modifying an initial cellulose ester with at least one plasticizer 112.

[0024] Examples of polymer 104 include cellulose acetate, cellulose acetate phthalate, cellulose acetate butyrate, cellulose acetate propionate, cellulose propionate, cellulose butyrate, cellulose acetate trimellitate, hydroxypropyl methylcellulose phthalate, methylcellulose, ethylcellulose, hydroxyethylcellulose, hydroxypropyl methylcellulose, carboxymethylcellulose, and mixtures of two or more thereof. In some embodiments, polymer 104 is limited to one or more of carboxymethylcellulose, cellulose acetate butyrate, cellulose acetate propionate, cellulose propionate, and cellulose acetate.

[0025] In some embodiments, polymer 104 comprises a cellulosic polymer, such as a cellulose ester having free hydroxy groups attached directly to the polymer backbone, thereby providing a free hydroxyl content in an amount of at least 1%, or at least 2%, and no more than 5%, based on the total hydroxy groups present in polymer 104. The remaining hydroxyl groups in polymer 104 can be esterified to provide a relatively low free hydroxyl content.

[0026] In the composition of precursor 102, polymer 104 may be present in precursor 102 in an amount of at least 1% and no more than 50% by weight (weight % based on the total weight of components 104, 106, 108, 110, 112, 114, 116, 118 of precursor 102). In some embodiments, polymer 104 may be present in precursor 102 in an amount of at least 2% and no more than 15% by weight. In some embodiments, polymer 104 may be present in precursor 102 in an amount of at least 3% and no more than 10% by weight.

[0027] Examples of polymerizable components 106 The polymerizable component 106 generally includes one or more relatively small molecules (e.g., monomers, oligomers, or the like). These molecules can combine to form larger molecules (macromolecules or polymers). The polymerizable component 106 may include one or more photochemically polymerizable materials. The term "photochemically polymerizable" component is used herein to mean molecules that can combine via covalent bonds after exposure to light (e.g., of a particular wavelength range and / or intensity), for example, to form a larger molecule. For example, the "photochemically polymerizable" component 106 may be an acrylate material or an epoxy that polymerizes when irradiated with light (ultraviolet (UV), visible, or infrared) having suitable properties in the presence of one or more suitable photoinitiators 114. As described further below, the photoinitiators 114 can facilitate polymerization of the polymerizable component after exposure to light.

[0028] The polymerizable components 106 can coalesce to form linear and / or three-dimensional macromolecules (e.g., cross-linked polymers). The polymerizable components 106 can coalesce (e.g., polymerize, cure, etc.) via free radical polymerization, acid-catalyzed (cationic) polymerization, or a combination of both.

[0029] The polymerizable component 106 may include any material capable of participating in a photopolymerization reaction, such as a photopolymerizable monomer, oligomer, or polymer, or a photoinitiator or co-initiator. Such polymerizable component 106 may be configured to participate in a free radical photocure, in which free radicals are generated upon exposure to light, or to participate in an acid catalyzed photocure, in which an acid is generated upon exposure to light for reaction and curing of the epoxy, or both.

[0030] The polymerizable component 106 may include one or more free radical polymerizable compounds. Examples of such polymerizable components 106 include ethylenically unsaturated polymerizable monomers and / or oligomers and polymers, such as mono- or polyfunctional acrylates (e.g., methacrylates). Such free radical polymerizable compounds include at least one ethylenically unsaturated polymerizable bond and may include two or more such unsaturated moieties. These materials include at least one ethylenically unsaturated polymerizable bond and are generally capable of undergoing addition (e.g., or free radical) polymerization. Examples of polymerizable components 106 that react via free radical polymerization include mono-, di-, and poly-acrylates and methacrylates. Examples of mono-, di-, and poly-acrylates and methacrylates include, but are not limited to, methyl acrylate, methyl methacrylate, ethyl acrylate, isopropyl methacrylate, n-hexyl acrylate, stearyl acrylate, allyl acrylate, glycerol diacrylate, glycerol triacrylate, ethylene glycol diacrylate, diethylene glycol diacrylate, triethylene glycol dimethacrylate, 1,3-propanediol diacrylate, 1,3-propanediol dimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, neopentyl glycol diacrylate, and neopentyl glycol diacrylate. Examples of suitable bis-acrylates include ethyl glycol dimethacrylate, trimethylolpropane triacrylate, 1,2,4-butanetriol trimethacrylate, 1,4-cyclohexanediol diacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol tetramethacrylate, dipentaerythritol hexaacrylate, sorbitol hexaacrylate, bis[1-(2-acryloxy)]-p-ethoxyphenyl-dimethylmethane, bis[1-(3-acryloxy-2-hydroxy)]-p-propoxyphenyl-dimethylmethane, and tris-hydroxyethyl-isocyanurate trimethacrylate. The molecular weight of the bis-acrylate and bis-methacrylate of polyethylene glycol used as the polymerizable component 106 is generally 200 to about 500.Other examples of polymerizable components 106 that react via free radical polymerization include copolymerizable mixtures of acrylate monomers and acrylate oligomers. Other examples of polymerizable components 106 include vinyl compounds such as styrene and styrene derivatives, diallyl phthalate, divinyl succinate, divinyl adipate, and divinyl phthalate. In general, polymerizable component 106 may include a mixture of any two or more of the above free radical polymerizable materials.

[0031] One or more of the polymerizable components 106 may be acid-catalyzed polymerizable compounds. Examples of polymerizable components 106 that may participate in an acid-catalyzed reaction include photopolymerizable epoxy materials (e.g., organic compounds having at least one oxirane ring that can be polymerized via a ring-opening reaction). Such epoxy materials, also referred to as "epoxides," may include monomeric epoxy compounds and polymeric epoxides. Epoxides used as the polymerizable components 106 may be aliphatic, cycloaliphatic, aromatic, or heterocyclic. Such materials generally contain, on average, at least one polymerizable epoxy group per molecule. In some embodiments, such materials contain about 1.5 to about 2 polymerizable epoxy groups per molecule. The "average" number of epoxy groups per molecule is determined by dividing the total number of epoxy groups in the epoxy material by the total number of epoxy-containing molecules present. Polymeric epoxy materials that can be used as the polymerizable component 106 include linear polymers with terminal epoxy groups (e.g., diglycidyl ethers of polyoxyalkylene glycols), polymers with backbone (main chain) oxirane units (e.g., polybutadiene polyepoxides), and polymers with pendant epoxy groups (e.g., glycidyl methacrylate polymers or copolymers).

[0032] The epoxy materials used as the polymerizable component 106 may vary from low molecular weight monomeric materials to high molecular weight polymers. These epoxy materials may have a wide variety of backbone structures and substituted (or pendant) groups. For example, the backbone of such epoxy materials may be of any type, and the substituents on the backbone may be any groups that do not significantly interfere with cationic photocuring at room temperature. Illustrative examples of possible substituents include halogen, ester, ether, sulfonic acid, siloxane, nitro, and phosphate groups. The molecular weight of the epoxy materials used as the polymerizable component 106 may be at least 58 to about 100,000 (grams / mole). In some embodiments, the molecular weight is greater than 100,000.

[0033] Exemplary epoxy materials for use as the polymerizable component 106 include glycidyl ethers (e.g., bisphenol-A-diglycidyl ether (DGEBA)), glycidyl ethers of bisphenol S and bisphenol F, butanediol glycidyl ether, bisphenol-A-extended glycidyl ether, phenol-formaldehyde glycidyl ethers (e.g., epoxy novolacs), cresol-formaldehyde glycidyl ethers (e.g., epoxy cresol novolacs), epoxy glycidyl ethers (e.g., epoxy glycidyl ether ... Alkenes, 1,2-epoxyoctane, 1,2,13,14-tetradecane diepoxide, 1,2,7,8-octane diepoxide, octadecylene oxide, epichlorohydrin, styrene oxide, vinylcyclohexeneoxycyclohexene oxide, glycidol, glycidyl methacrylate, glycidyl ether of bisphenol A, vinylcyclohexane dioxide, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexene carboxylate, 3,4-epoxy-6-methyl Bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, Bis(2,3-epoxy-cyclopentyl)ether, Aliphatic epoxies modified with polypropylene glycol, Dipentene dioxide, Epoxidized polybutadiene, Silicone resins with epoxy functionality, Flame retardant epoxy resins, 1,4-butanediol diglycidyl ether of phenol formaldehyde novolac, Resorcinol diglycidyl ether Glycidyl ethers, 2-(3,4-epoxycyclohexyl-5,5-spiro-3,4-epoxy)cyclohexane-meta-dioxane, 2-(3,4-epoxycyclohexyl-5,5-spiro-3,4-epoxy)cyclohexane-meta-dioxane, vinylcyclohexene monoxide, 1,2-epoxyhexadecane, alkyl glycidyl ethers, butyl glycidyl ether, cresyl glycidyl ether, p-tert butylphenyl glycidyl ether, polyfunctional glycidyl ethers, e.g. 1,Diglycidyl ether of 4-butanediol, diglycidyl ether of neopentyl glycol, diglycidyl ether of cyclohexanedimethanol, trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, polyglycidyl ethers of aliphatic polyols, polyglycol diepoxides, bisphenol F epoxide, and 9,9-bis-4-(2,3-epoxypropoxy)-phenylfluorenone.

[0034] Although the amount of polymerizable components 106 is not particularly limited, these components 106 may be present in the precursor 102 in an amount of at least 1% and no more than 75% by weight (weight % is based on the total weight of components 104, 106, 108, 110, 112, 114, 116, 118 of the precursor 102). In some embodiments, the polymerizable components 106 are present in an amount of at least 5% and no more than 50% by weight. In some embodiments, the polymerizable components 106 are present in an amount of at least 5% and no more than 10% by weight. The amount of polymerizable components 106 can generally be adjusted based on the desired properties of the precursor 102 (e.g., the solubility of the components in the precursor 102) and / or the resulting mechanical properties of the semi-IPN SPE 100 (e.g., mechanical strength).

[0035] Example of Lithium Ion Source 108 The lithium ion source 108 may include any one or more lithium salts and / or lithium ion complexes (e.g., inorganic and / or inorganic salts and / or complexes). Representative examples of inorganic salts suitable for use as the lithium ion source 108 are the alkali metal salts. The inorganic salts may include lithium cations and anions that are weak bases. Such anions may have a relatively large anionic radius. Examples of such anions include I - , Br - , SCN - , CIO 4 - , B.F. 4 - , P.F. 6 - , AsF 6 - , C.F. 3COO - , C.F. 3 SO 3 - , N(SO 2 CF 3 ) 2 - Further examples of suitable inorganic lithium salts are LiSCN, (CF 3 SO 2 ) 2 NLi, (CF 3 SO 2 ) 3 CLi, and the like. Examples of lithium salts and complexes for use as the lithium ion source 108 include lithium nitrate (LiNO 3 ), lithium iodide (LiI), lithium sulfide (Li 2 S), lithium perchlorate (LiClO 4 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), lithium hexafluoroarsenate(V) (LiAsF 6 ), lithium hexafluorophosphate (LiPF 6 ), and lithium tetrafluoroborate (LiBF 4 In some embodiments, the lithium salt used as the lithium ion source 108 includes LiAsF 6 , LiCF 3 SO 3 , LiPF 6 , LiBF 4 , or a mixture of one or more of these salts. The lithium ion source may be present in the precursor 102 at a concentration of about 1% to about 80% by weight (weight % based on the total weight of the components 104, 106, 10-8, 110, 112, 114, 116, 118 of the precursor 102). In some embodiments, the lithium ion source 108 is present in the precursor 102 at a concentration of about 5% to about 40% by weight. The weight % of the lithium ion source 108 may be adjusted based on the structure and molecular weight of a given salt.

[0036] Solvent 110 Example The solvent 110 of the precursor 102 can generally be any solvent (e.g., an organic solvent) capable of dissolving and / or dispersing the components 104, 106, 108, 112, 114, 116, and 118. In most embodiments, at least the polymer 104 is soluble (i.e., soluble) in the solvent 110. In some embodiments, the boiling point of each of the one or more solvents 110 used in the precursor composition 102 is 90° C. or higher. In some embodiments, the boiling point of each of the one or more solvents 110 used in the precursor composition 102 is at least 100° C. In some embodiments, the boiling point of each of the one or more solvents 110 used in the precursor composition 102 is at least 150° C. In some embodiments, the boiling point of each of the one or more solvents 110 used in the precursor composition 102 is greater than about 200° C. Generally, the boiling point of the solvent 110 is less than 500° C. When solvent 110 comprises two or more different organic solvents, the difference in boiling point between any two of the organic solvents may be greater than 10°C.

[0037] Examples of solvents 110 include one or more hydroxyl organic solvents (e.g., alcohols) or non-hydroxyl solvents. While solvent 110 may generally include primary and / or secondary alcohols and monohydric and / or polyhydric alcohols, in some embodiments, the alcohols used as solvent 110 do not include olefinic unsaturation. In other words, in some embodiments, alcohol solvent 110 does not include carbon-carbon double bonds. Examples of hydroxyl solvents 110 include straight-chain or branched-chain alcohols that have none, either, or both of alicyclic and aromatic carbon-carbon moieties. Representative examples of suitable straight-chain primary alcohol solvents include ethanol, 2-propanol, 2-butanol, 1-pentanol, 1-hexanol, 1-octanol, 2-ethyl-1-hexanol, 1-decanol, ethylene glycol, propylene glycol, and benzyl alcohol. Representative examples of branched-chain alcohol solvents 110 include isobutyl alcohol, isoamyl alcohol, and sec-butyl carbinol. Representative examples of secondary alcohol solvents 110 include isopropyl alcohol, secondary butyl alcohol, secondary amyl alcohol, diethyl carbinol, methyl isobutyl carbinol, methyl-3-heptanol, diisobutyl carbinol, dodecanol-Z, methyl allyl carbinol, cyclohexanol, methyl cyclohexyl carbinol, phenyl methyl carbinol, and similar materials. Any combination of these alcohol solvents 110 may be used.

[0038] In some embodiments, the solvent 110 includes a glycol ether, which has both ether and alcohol functional groups in the same molecule. Representative examples of such glycol ether solvents 110 include 2-methoxyethanol, 2-ethoxyethanol, diethylene glycol monoethyl ether (carbitol), and methoxyisopropanol. The solvent 110 may include mixtures of these or similar materials. Further examples of solvents 110 include dimethylformamide (DMF), dimethylsulfoxide (DMSO), ketone solvents, ester solvents, carbonate solvents, and the like.

[0039] Any suitable amount of one or more solvents 110 may be included in the precursor 102. The solvent 110 may be present in the precursor 102 in an amount of at least 50% and no more than 95% by weight (weight % based on the total weight of the components 104, 106, 108, 110, 112, 114, 116, 118 of the precursor 102). In some embodiments, the solvent 110 is present in the precursor 102 in an amount of at least 70% and no more than 90% by weight. In some embodiments, the solvent 110 is present in the precursor 102 in an amount of at least 75% and no more than 90% by weight.

[0040] In some embodiments, the solvent 110 may be selected based on the relative solubility of one or more of the components 104, 106, 108, 110, 112, 114, 116, 118 in the solvent 110. In some embodiments, the solvent may be selected based at least in part on the expected solubility of the polymer 104 in the solvent 110. For example, solubility parameters (total Hansen parameters) may be determined for the polymer 104 and the solvent. The solvent 110 may be selected such that these parameters indicate that the polymer 104 should be soluble in the solvent 110. For example, the solubility parameters of the one or more polymers 104 and the one or more solvents 110 may be within a predetermined range. In some embodiments, the total solubility parameter of the solvent 110 is equal to or greater than the total solubility parameter of the one or more polymers 104. In such an embodiment, when a mixture of solvents 110 is used, the total solubility parameter of the mixture is equal to or exceeds the total solubility parameter of the polymer 104. The solvent 110 may further be selected to maintain a predetermined total solubility parameter having a certain range, even if the solvent profile changes during deposition of the precursor 102 (e.g., when the solvent evaporates during preparation of the precursor 102 film, as described below with respect to step 318 of FIG. 3).

[0041] Solubility parameters for various molecules can be roughly determined from manufacturer information (if available), estimated from studies of similar materials, and / or determined via solubility studies. For example, the total Hansen parameter of an organic solvent mixture can be calculated using the sum of the volume fractions of the individual organic solvent components in the solution. The total Hansen parameter is an example of a solubility parameter, which provides information about whether one material is expected to dissolve in another. Each molecule is given three Hansen parameters. Each of the Hansen parameters is roughly expressed in MPa. 0.5 It is measured by (1)δ D The parameter represents the energy from dispersion bonds between molecules, (2) δ P The parameters represent the energy from polar bonds between molecules, and (3) δ H The parameter represents the energy from hydrogen bonds between molecules. The total Hansen solubility parameter (δ) is δ = δ D 2 +δ P 2 +δ PH 2 The three Hansen parameters (δ D , δ P , δ H ) can be treated as coordinates corresponding to points in three dimensions, also known as "Hansen space." The closer two molecules are in this three-dimensional space, the greater the probability that these molecules will dissolve (i.e., be soluble) in one another. As an example, to determine whether the overall Hansen parameters of the solvent 110 and the polymer 104 indicate that the polymer 104 dissolves in the solvent 110, the δ D , δ P and δ H Based on the value of D , δ P , δ H ) can be determined.

[0042] Examples of Plasticizers 112 An optional plasticizer 112 can be used in the precursor 102. The one or more plasticizers 112 are generally selected to reduce the melt temperature and / or melt viscosity of the polymer 104. The plasticizer 112 can be monomeric or polymeric. In some embodiments, the plasticizer 112 includes at least one phosphate plasticizer, benzoate plasticizer, adipate plasticizer, phthalate plasticizer, glycolate plasticizer, citrate plasticizer, and / or hydroxyl-functionalized plasticizer. In some embodiments, the plasticizer 112 includes one or more of triphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, octyl diphenyl phosphate, diphenyl biphenyl phosphate, trioctyl phosphate, tributyl phosphate, diethyl phthalate, dimethoxyethyl phthalate, dimethyl phthalate, dioctyl phthalate, dibutyl phthalate, di-2-ethylhexyl phthalate, butyl benzyl phthalate, dibenzyl phthalate, butyl phthalyl butyl glycolate, ethyl phthalyl ethyl glycolate, methyl phthalyl ethyl glycolate, triethyl citrate, tri-n-butyl citrate, acetyl triethyl citrate, acetyl-tri-n-butyl citrate, and acetyl-tri-n-(2-ethylhexyl) citrate.

[0043] In some embodiments, the plasticizer 112 comprises (1) at least one acid residue comprising a residue of phthalic acid, adipic acid, trimellitic acid, succinic acid, benzoic acid, azelaic acid, terephthalic acid, isophthalic acid, butyric acid, glutaric acid, citric acid, and / or phosphoric acid, and (2) an alcohol residue having one or more residues of an aliphatic, alicyclic, or aromatic alcohol having up to about 20 carbon atoms. In some embodiments, the plasticizer 112 comprises an alcohol residue, such as stearyl alcohol, lauryl alcohol, phenol, benzyl alcohol, hydroquinone, catechol, resorcinol, ethylene glycol, neopentyl glycol, 1,4-cyclohexanedimethanol, and diethylene glycol. In some embodiments, the plasticizer 112 comprises at least one of a benzoate, a phthalate, a phosphate, an arylene-bis(diarylphosphate), and an isophthalate. In some embodiments, the plasticizer comprises diethylene glycol dibenzoate (DEGDB).

[0044] In some embodiments, the plasticizer 112 comprises (1) an aliphatic polyester containing C2-10 diacid residues, such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid, and (2) a C2-10 diol residue. In some embodiments, the plasticizer 112 comprises a diol residue, such as at least one of the residues of a C2-C10 diol (e.g., ethylene glycol, diethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, neopentyl glycol, 1,5-pentanediol, 1,6 hexanediol, 1,5-pentylene glycol, triethylene glycol, and tetraethylene glycol).

[0045] In some embodiments, the plasticizer 112 includes polyglycols, such as polyethylene glycols, polypropylene glycols, and polybutylene glycols. These polyglycols may include molecules from low molecular weight dimers and trimers and / or high molecular weight oligomers and polymers. In some embodiments, the molecular weight of the polyglycols included in the plasticizer 112 may range from about 200 to about 2,000.

[0046] In some embodiments, the plasticizer 112 comprises at least one of Resoflex® R296 plasticizer, Resoflex® 804 plasticizer, sorbitol hexapropionate (SHP), xylitol pentapropionate (XPP), xylitol pentaacetate (XPA), glucose pentaacetate (GPP), glucose pentapropionate (GPA), and arabitol pentapropionate (APP). In some embodiments, the plasticizer 112 comprises (1) about 5 to about 95% by weight of a C2-C12 carbohydrate organic ester, the carbohydrate comprising about 1 to about 3 monosaccharide units, and (2) about 5 to about 95% by weight of a C2-C12 polyol ester, the polyol being derived from a C5 or C6 carbohydrate. In some embodiments, the polyol ester of the plasticizer 112 does not comprise or does not contain a polyol acetate.

[0047] In some embodiments, the plasticizer 112 comprises at least one carbohydrate ester, and the carbohydrate portion of the carbohydrate ester is derived from one or more of glucose, galactose, mannose, xylose, arabinose, lactose, fructose, sorbose, sucrose, cellobiose, cellotriose, and raffinose. In some embodiments, the polymer 104 (e.g., a cellulose ester) is modified using one or more of the plasticizers 112. The plasticizer 112 may be present in the precursor 102 in an amount of about 1% to 10% by weight (weight % based on the total weight of the components 104, 106, 108, 110, 112, 114, 116, 118 of the precursor 102). In some embodiments, the plasticizer 112 is about 5% or less by weight of the precursor 102.

[0048] Photoinitiator 114 Examples The photoinitiator 114 of the precursor 102 may include one or more photoinitiators for free radical polymerization. The photoinitiator generates free radicals in the presence of at least one of the polymerizable components 106. Such free radical photoinitiators 114 include any compound capable of generating free radicals upon exposure to photopolymerizing radiation, such as ultraviolet or visible radiation. Examples of free radical photoinitiators 114 may be triazine compounds, thioxanthone compounds, benzoin compounds, carbazole compounds, diketone compounds, sulfonium borate compounds, diazo compounds, biimidazole compounds, and any of these compounds. The photoinitiator 114 may be a benzophenone compound, such as benzophenone, benzoyl benzoate, methyl benzoyl benzoate, 4-phenyl benzophenone, hydroxyl benzophenone, acrylated benzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, anthraquinone compounds, and acetophenone compounds (e.g., 2,2'-diethoxyacetophenone, 2,2'-dibutoxyacetophenone, 2-hydroxy-2-methylpropiophenone, para-t -butyltrichloroacetophenone, para-t-butyldichloroacetophenone, benzophenone, 4-chloro-acetophenone, 4,4'-dimethylaminobenzophenone, 4,4'-dichlorobenzophenone, 3,3'-dimethyl-2-methoxybenzophenone, 2,2'-dichloro-4-phenoxyacetophenone, 2-methyl-1-(4-(methylthio)phenyl)-2-morpholinopropan-1-one, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one). Additional compounds that may be used as the photoinitiator 144 include triazine compounds, benzophenone compounds, acetophenone compounds, thioxanthone compounds, benzoin compounds, carbazole compounds, diketone compounds, sulfonium borate compounds, diazo compounds, and biimidazole compounds.

[0049] The photoinitiator 114 of the precursor 102 may include one or more photoinitiators for acid polymerization. A variety of compounds may be used to generate an acid suitable for participating in the polymerization of the polymerizable component 106 (e.g., specifically the epoxy polymerizable component 106 described above). Such "photoacid generators" may be acidic, while others may be nonionic. Examples of acid generators include onium hydrochloride acid generators, such as diazonium salts (e.g., polyaryldiazonium), phosphonium salts, iodonium salts, and / or sulfonium salts. Examples of iodonium and sulfonium salts include diaryliodonium salts and triarylsulfonium salts. Counter anions in such salts include complex metal halides, such as tetrafluoroborates, hexafluoroantimonates, trifluoromethanesulfonates, hexafluoroarsenates, hexafluorophosphates, and arenesulfonates. The onium salts may be oligomeric or polymeric compounds having one or more onium salt moieties.

[0050] The photoinitiators 114 may be dispersed in the precursor 102, individually or in combination, in an amount of about 0.1% to about 10% by weight (weight % based on the total weight of the components 104, 106, 108, 110, 112, 114, 116, 118 of the precursor 102).

[0051] In some embodiments, ceramic particles 116 (below) can function as photoinitiators 114. For example, TiO 2 And / or the ZnO particles may function to initiate the photopolymerization reaction.

[0052] Examples of ceramic particles 116 As discussed above, the ceramic particles 116 provide improved mechanical strength and ionic conductivity to the semi-IPN SPE 100. Specifically, it has been found (Test Examples below) that the ceramic particles 116 unexpectedly and significantly increase both the ionic conductivity and the mechanical strength of the semi-IPN SPE 100. The ceramic particles 116 are metal oxide particles, such as TiO 2 , Al2 O3, SiO 2 , ZrO2, SnO 2 , WO 3 , Ta 2 O 3 or a combination thereof.

[0053] The ceramic particles 116 may have any shape. For example, the ceramic particles 116 may have a spherical, ellipsoidal, tetrahedral, pyramidal, cuboctahedral, cylindrical, polyhedral, multiarmed, and / or cubic shape. The ceramic particles 116 may be nanoparticles having a characteristic size (e.g., diameter) of about 1 nm to about 100 nm. In some embodiments, the ceramic particles 116 have a diameter of about 0.5 nm to about 100 nm. In some embodiments, the ceramic particles 116 have a diameter of about 1 nm to about 5 nm. The above particle size range examples may be average particle sizes from a group of measured particle sizes for the ceramic particles 116. In some cases, the average particle size refers to the number average diameter. The "average diameter" may be the D50 particle size (i.e., half of the particles measured have a larger diameter and half have a smaller diameter).

[0054] Generally, the ceramic particles 116 are dispersed in the precursor 102 in an amount of about 1% to about 25% by weight (weight % being based on the total weight of the components 104, 106, 108, 110, 112, 114, 116, and 118 of the precursor 102). In some embodiments, the ceramic particles 116 are included in the precursor 102 in an amount of about 2% to about 7% by weight. In some embodiments, the ceramic particles 116 are included in the precursor 102 in an amount of about 3% to about 5% by weight.

[0055] Examples of vinyl backbone polymers 118 As noted above, in some embodiments, the precursor includes one or more polymers 118 having a vinyl backbone and a molecular weight of less than about 100,000. In some embodiments, the molecular weight of the polymer 118 is less than 50,000. In some embodiments, the molecular weight of the polymer 118 is less than 25,000. Examples of such polymers 118 include poly(alkyl methacrylates), poly(alkyl acrylates), poly(vinyl acetates), poly(alpha olefins), poly(styrene sulfonates), polystyrene, poly(acrylic acid) (and salts thereof), poly(methacrylic acid) (and salts thereof), and the like. These optional vinyl backbone polymers 118 may be present in the precursor 102 in an amount of about 1% to about 10% by weight (weight percent is based on the total weight of the components 104, 106, 108, 110, 112, 114, 116, 118 of the precursor 102).

[0056] Example of a method for preparing semi-IPN SPE and an electrode containing the same FIG. 3 illustrates an example of a process 300 for preparing the semi-IPN SPE 100 of FIG. 1. The method 300 may begin at step 302. One or more polymers 104 are combined with a solvent 110. For example, a predetermined amount of the polymer 104 (e.g., cellulose acetate) may be added to a predetermined volume of the solvent 110. As described above, the solvent 110 may be selected such that the polymer 104 is soluble in the solvent 110. The resulting solution including the polymer 104 dissolved in the solvent 110 may have a concentration of the polymer 104 between 0.1% and 30% by weight (weight % is based on the weight of the polymer 104 per total weight of the polymer solution in the solvent).

[0057] In step 304, the ceramic particles 116 are prepared. The ceramic particles 116 may be prepared using any suitable method. For example, the ceramic particles 116 may be prepared by ball milling a ceramic material powder. In some embodiments, the ceramic particles 116 are obtained in a pre-prepared form such that step 304 is not required.

[0058] In step 306, a slurry of ceramic particles 116 is prepared. For example, ceramic particles 116 may be combined with a volume of the solvent 110 used to dissolve the polymer 104 in step 302 and / or other solvents 110. The ceramic particles 116 and the solvent 110 may be combined via a ball milling process to disperse the ceramic particles 116 in the solvent 110. This initial slurry of ceramic particles 116 may then be combined with all or a portion of the polymer-in-solvent solution prepared in step 302. For example, the polymer-in-solvent solution of step 302 may be combined with the initial slurry. In some embodiments, a first portion of the polymer-in-solvent solution of step 302 may be combined with the initial slurry near the end of milling the ceramic particles 116 to prepare the slurry of ceramic particles 116. After the milling process is completed, a second portion of the polymer-in-solvent solution may be combined with the mixture. The ratio of the mass of polymer 104 to the mass of ceramic particles 116 can be from about 1 to about 600. In some embodiments, the ratio of the mass of polymer 104 to the mass of ceramic particles 116 can be from about 1 to about 400.

[0059] In step 308, the plasticizer 112 is combined with the mixture of step 306. For example, the plasticizer 112 may be combined with the mixture via mixing with a mechanical agitator / mixer and / or a ball milling process. Generally, sufficient mixing is provided such that the plasticizer 112 is dispersed or dissolved in the mixture. The weight ratio of the plasticizer 112 to the polymer 104 is generally from about 0.001 to about 32.

[0060] In step 310, polymerizable component 106 is combined with the mixture of step 308. For example, polymerizable component 106 may be combined with the mixture via mixing (e.g., using a mechanical mixer and / or a ball mill). The weight ratio of polymer 104 to polymerizable component 106 is generally from about 0.1 to about 20.

[0061] In step 312, the lithium ion source 108 is combined with the mixture of step 310. For example, the lithium ion source 108 may be combined with the mixture via mixing (e.g., using a mechanical mixer and / or a ball mill). In some embodiments, the lithium ion source 108 is first dissolved in one or more of the solvents 110, and the resulting lithium-in-solvent solution is combined with the mixture of step 310. The weight ratio of the lithium ion source 108 to the polymer 104 is about 0.01-100. As described with respect to FIG. 1 above, in some embodiments, the addition of the lithium ion source 108 in step 312 is delayed until a later time when it is desired to prepare the semi-IPN SPE 100. For example, a premixed portion 103 of the precursor 103 (see FIG. 1) can be first prepared (e.g., by performing steps 302, 304, 306, 308, 310, 314, and / or 316). This premixed precursor portion 103 may be stored under suitable storage conditions (e.g., in the absence of light that may induce reaction of the polymerizable component 106 and / or the photoinitiator 114) and used when desired.

[0062] In step 314, a photoinitiator 112 is combined with the mixture of step 312. For example, the photoinitiator 112 may be combined with the mixture via mixing (e.g., using a mechanical mixer and / or a ball mill). The weight ratio of the photoinitiator 112 to the polymerizable component 106 is generally from about 0.001 to about 10. In some embodiments, the addition of the photoinitiator 112 in step 314 may be delayed until a later time when it is desired to prepare the SPE 100. For example, a portion of the precursor 102 without the photoinitiator 112 (or a premixed precursor portion 103) can be stored before it is desired to prepare the semi-IPN SPE 100 without risking that photochemical reactions will occur to any significant extent.

[0063] In step 316, a vinyl backbone polymer 118 may optionally be combined with the mixture of step 314. For example, the vinyl backbone polymer 118 may be combined with the mixture via mixing (e.g., using a mechanical mixer and / or a ball mill). The mass ratio of polymer 104 to vinyl backbone polymer 118 is about 1% to about 10% by weight.

[0064] In step 318, one or more layers of the precursor 102 from the previous step are applied to a substrate. The substrate may be any suitable material (e.g., aluminum). The precursor 102 may be applied to the substrate using any suitable method. Examples of such methods include air knife coating, gravure coating, hopper coating, roller coating, spray coating, electrochemical coating, inkjet printing, and flexographic printing. In some embodiments, a layer of the precursor 102 may be contact printed in a desired pattern (e.g., to prepare a thin film of the semi-IPN SPE 100 in a desired pattern and / or to prepare cells 200 of suitable size, shape, pattern, etc.). Such a contact printing approach may be easily scaled up for mass production of the semi-IPN SPE 100 at a relatively low cost. For example, the contact printing approach may involve a layer of the precursor 102 being applied to a donor member and transferred to a receiver member via application of heat and / or pressure. An adhesive layer may be present between the layer of precursor 102 and the receiving member. In general, the deposited precursor 102 may be dried at an elevated temperature (e.g., about 100° C.) for a predetermined period of time before proceeding to step 320.

[0065] In step 320, the precursor 102 deposited in step 318 is cured. For example, the precursor 102 may be exposed to heat and / or light. For example, the layer of precursor 102 in step 318 may be irradiated with light (e.g., UV light) for a predetermined time (e.g., about 1 second to 10 minutes or more). Generally speaking, the curing process may continue as long as required to prepare a tack-free semi-IPN SPE 100. Following polymerization, the semi-IPN SPE 100 may be further dried and annealed by heating for a predetermined time (e.g., 100° C. to 150° C. for 1 hour or 2 hours or more). The resulting semi-IPN SPE 100 may be a thin film (e.g., less than 200 micrometers thick). In some embodiments, the semi-IPN SPE 100 is less than 150 micrometers thick. In some embodiments, the semi-IPN SPE 100 is less than 100 micrometers thick. In some embodiments, the thickness of the semi-IPN SPE 100 is less than about 10 micrometers to 100 micrometers.

[0066] In step 322, the semi-IPN SPE 100 of step 320 is used to prepare a cell, such as the lithium cell 200 shown in FIG. 2. For example, a cell the same or similar to the cell 200 shown in FIG. 2 can be obtained by placing (sandwiching) the SPE film 100 between two electrodes 202, 204. In some embodiments, a battery of a desired voltage can be prepared by preparing multiple cells 200 and appropriately combining (e.g., stacking in series). Appropriate electrical contacts can be provided to consume and charge the cells 200.

[0067] The cell 200 prepared in step 322 may have any suitable configuration. For example, the cell 200 may be configured based on the type of electrodes used. For example, one or both of the electrodes 202, 204 of the cell 200 may be a blocking electrode that does not allow lithium ions to pass through. Examples of blocking electrodes include aluminum foil or stainless steel foil. Such foils may have a thickness of about 5 micrometers to about 50 micrometers. The cell 200 having the blocking electrodes as the electrodes 202, 204 may be used for ionic conductivity measurements. In some cases, one or both of the electrodes 202, 204 may be a lithium metal foil. The lithium metal foil may have a thickness of about 25 to about 100 micrometers. The cell 200 having the lithium foil electrodes 202, 204 may be used, for example, to determine the electrochemical stability window of the semi-IPN SPE 100, to determine the lithium plating and / or stripping behavior associated with the presence of the semi-IPN SPE 100, and for similar purposes. In some embodiments, cathode 202 can be any other suitable cathode material (e.g., lithium nickel manganese cobalt oxide having a thickness of about 20-200 micrometers) and anode 204 can be any suitable anode material (e.g., graphite, as described above, having a thickness of about 20-200 micrometers, or lithium metal).

[0068] As an example, the cell 200 may be prepared by coating the precursor 102 on a metal foil (e.g., aluminum foil, stainless steel foil, or the like) or other surface (e.g., glass). The film of precursor 102 may then be irradiated with light (e.g., UV light) of appropriate power and wavelength for a predetermined time (e.g., to activate the photoinitiator 114). The film is then cured (e.g., at a temperature of 50-100° C.) and dried to produce a thin film semi-IPN SPE 100 having a thickness of about 5 micrometers to about 500 micrometers. The film semi-IPN SPE 100 may be removed (e.g., via peeling) from the metal foil or other surface. The film semi-IPN SPE 100 is then sandwiched between an anode 204 and a cathode 202.

[0069] As described above, the cathode 202 may include any cathode active material and / or component. For example, the cathode active material may be lithium cobalt oxide (LiCoO 2 ), lithium iron phosphate (LiFePO 4 ), lithium nickel manganese cobalt oxide (LiNi x Mn y Co z O 2 ), lithium nickel cobalt aluminum oxide (LiNi x Co y Al z O 2 ), or mixtures thereof. Other cathode components may include conductive carbon, polymer binders, other additives, and any combination thereof. Polymer binders may include, for example, poly(vinylidene fluoride), poly(tetrafluoroethylene), carboxymethyl cellulose, poly(acrylic acid), styrene-butadiene rubber, or mixtures of any one or more of the foregoing. Cathode 202 may be a film having any suitable thickness. In some embodiments, cathode 202 has a thickness of about 20 to about 500 micrometers.

[0070] Also as described above, the anode 204 may be comprised of any anode active material and / or other anode components, such as, for example, graphite, graphene, carbon nanotubes, carbon black, silicon, doped silicon, silicon oxide (SiO x ), tin, tin oxide, lithium titanate (Li 4 Ti 5 O 12 ), or mixtures thereof. Other cathode components may include any of conductive carbon, polymer binders, and / or other additives. The polymer binder may include, for example, poly(vinylidene fluoride), poly(tetrafluoroethylene), carboxymethyl cellulose, poly(acrylic acid), styrene-butadiene rubber, or mixtures thereof. Anode 204 may be a film having any suitable thickness. In some embodiments, anode 204 has a thickness of about 20 to about 500 micrometers.

[0071] After the film of semi-IPN SPE 100 is sandwiched between the cathode 202 and anode 204, pressure is applied to laminate the semi-IPN SPE 100 between the cathode and anode to form the completed cell 200. This lamination process can create suitable interfaces to form between the semi-IPN SPE 100 and the cathode and anode. The applied pressure can be about 1-10 per square meter. 8 In some embodiments, the applied pressure is about 10 3 ~10 5 N / m 2 While pressure is being applied, heat can be applied. Heat may be provided, for example, via electrical heating and / or infrared heating. The temperature achieved via this heating may be from about 25 to about 250° C. In some embodiments, the temperature during application of pressure to the semi-IPN 100 sandwiched between the cathode 202 and the anode 204 may be from about 40 to about 80° C.

[0072] The laminated film can be cut into appropriately shaped pieces to produce cells 200 of the desired shape. For example, the cells 200 may have a square shape (e.g., for use as a pouch cell), or a cylindrical or circular disk shape (e.g., for use as a coin cell). For example, for a pouch cell, aluminum / copper tabs can be welded to the cathode 202 and anode 204 of the cell 200. The resulting cells 200 can be stacked and placed into a pouch. The pouch is vacuum sealed. For cylindrical cells, the cells are rolled to form a cylinder and placed into cylindrical cans, which are then sealed. For coin cells, the circular disks of the cells 200 are placed into coin cell casings. The casings are crimped to result in coin cells. Any of these types of cells can be connected to a standard fill-discharge circuit to perform a fill-discharge operation, or to a potentiostat or dielectric spectrometer for impedance spectroscopy measurements.

[0073] In some embodiments, the semi-IPN SPE 100 may be prepared directly on the cathode 202. For example, the cell 200 may be prepared by coating the cathode 202 (as described above) with the precursor 102. The precursor-coated cathode 202 may be irradiated with light (e.g., UV light and microwave irradiation) having an appropriate power and wavelength for a predetermined time (e.g., to activate the photoinitiator 114). The film is then cured (e.g., at a temperature of 50-100° C.) and dried to produce a thin film semi-IPN SPE 100 having a thickness of about 5 micrometers to about 500 micrometers. In some embodiments, the thickness of the semi-IPN SPE 100 film is about 50-150 micrometers. The resulting structure (i.e., the cathode 202 coated with the semi-IPN SPE 100 film) may be laminated with the anode 204 by applying pressure and / or heat as described above. The resulting cell 200 can be cut and assembled into any of the cell types described above.

[0074] In some embodiments, the semi-IPN SPE 100 may be prepared directly on the anode 204. For example, the cell 200 may be prepared by coating the anode 204 (as described above) with the precursor 102. The precursor-coated anode 204 may be irradiated with light (e.g., UV light and microwave irradiation) having an appropriate power and wavelength for a predetermined time (e.g., to activate the photoinitiator 114). The film is then cured (e.g., at a temperature of 50-100° C.) and dried to produce a thin film semi-IPN SPE 100 having a thickness of about 5 micrometers to about 500 micrometers. In some embodiments, the thickness of the semi-IPN SPE 100 film is about 50-150 micrometers. The resulting structure (i.e., the anode 204 coated with the semi-IPN SPE 100 film) may be laminated with the cathode 202 by applying pressure and / or heat as described above. The resulting cell 200 can be cut and assembled into any of the cell types described above.

[0075] In some embodiments, the semi-IPN SPE 100 can be prepared as a stand-alone film and laminated between the cathode 202 and anode 204 as described above. For example, the semi-IPN SPE 100 can be pre-coated on a suitable current collector, such as a metal sheet or foil. In some cases, the precursor mixture can be combined with the cathode and anode films and cured in situ.

[0076] Test Example The preparation of an example of semi-IPN SPE 100 is described in the Examples below. In these Examples, the fumed silica particles have a primary particle size of 10-20 nm. The fumed alumina particles have a primary particle size of 80 nm. The fumed titania (i.e. titanium dioxide) particles have a primary particle size of 21 nm. The fumed titania particles are 80-90% anatase with a smaller portion being rutile.

[0077] Example 1: Preparation of Semi-IPN Solid Polymer Electrolyte Precursor Containing Cellulose Acetate (CA) and Polymerizable Oligomer A cellulose ester solution was prepared by dissolving cellulose acetate (0.72 g) in 2-methoxyethanol (7.73 g) with stirring. After complete dissolution, the cellulose ester solution (8.45 g) was diluted with poly(ethylene glycol) 200 diacrylate (SR 259, 0.20 g), ethoxylated (15) trimethylolpropane triacrylate (SR 9035, 0.04 g), LiClO 4 (0.24 g) and a 9 wt % solution of the photoinitiator 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone in acetone (0.09 g). The resulting solution was homogenized via stirring.

[0078] The weight percentages of the components in this precursor composition are 8.0% CA, 2.6% LiClO 4 , 2.2% SR 259, 0.4% SR 9035, and 0.1% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone. In dry-down form, the components in this precursor composition were 59.7% CA, 19.8% LiClO 4 , 16.6% SR 259, 3.3% SR 9035, and 0.7% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone.

[0079] Example 2: Preparation of Semi-IPN Solid Polymer Electrolyte Precursor Containing Cellulose Acetate Propionate (CAP) and Polymerizable Oligomer A cellulose ester solution was prepared by dissolving cellulose acetate propionate (0.68 g) in 1-methoxy-2-propanol (6.13 g) with stirring. After complete dissolution, the cellulose ester solution (6.8 g) was diluted with poly(ethylene glycol) 200 diacrylate (SR 259, 0.20 g), ethoxylated (15) trimethylolpropane triacrylate (SR 9035, 0.05 g), LiClO 4(0.24 g) and a 9 wt % solution of 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone in acetone (0.10 g). The solution was homogenized via stirring.

[0080] The weight percentages of the components in this example precursor composition are: 9.1% CAP, 3.3% LiClO 4 , 2.2% SR 259, 0.6% SR 9035, and 0.1% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone. In dry down form, the weight percentages of the components in this example precursor composition were 57.4% CAP, 20.5% LiClO 4 , 17.0% SR 259, 4.3% SR 9035, and 0.8% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone.

[0081] Example 3: Preparation of Semi-IPN Solid Polymer Electrolyte Precursor Containing Cellulose Acetate Propionate (CAP), Polymerizable Oligomer, and Polycaprolactone Triol Plasticizer A cellulose ester solution was prepared by dissolving cellulose acetate propionate (16.30 g) in dimethylformamide (83.7 g) with stirring. After complete dissolution, the first cellulose ester solution (16.3%, 6.24 g) was combined with poly(ethylene glycol) 200 diacrylate (SR 259, 0.29 g), alkoxylated pentaerythritol tetraacrylate (SR 494, 0.145 g), polycaprolactone triol (Mw=300 0.076 g), lithium iodide (0.48 g), 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone (0.01 g), and 1-methoxy-2-propanol (2.83 g). The solution was homogenized via stirring.

[0082] The weight percentages of the components in this example precursor composition were 10.1% CAP, 4.8% LiI, 2.9% SR 259, 1.4% SR 494, 0.8% poly(caprolactone triol), 0.1% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, 28.1% 1-methoxy-2-propanol, and 51.8% dimethylformamide. In dry down form, the weight percentages of the components in this example precursor composition were 50.2% CAP, 23.9% LiI, 14.3% SR 259, 7.2% SR 494, 3.1% polycaprolactone triol, and 0.8% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone.

[0083] Example 4: Semi-IPN solid polymer electrolyte precursor 102 containing cellulose acetate propionate (CAP), polymerizable oligomer, and silica A cellulose ester solution was prepared by dissolving cellulose acetate propionate (CAP, 16.30 g) in dimethylformamide (83.7 g) with stirring. After complete dissolution, a second solution was prepared by combining the first cellulose ester solution (16.3%, 31.18 g) with poly(ethylene glycol) 200 diacrylate (SR 259, 1.45 g), alkoxylated pentaerythritol tetraacrylate (SR 494, 0.73 g), polycaprolactone triol (Mw=300, 0.72 g), and 1-methoxy-2-propanol (11.25 g). The solution was homogenized via stirring. Separately, lithium iodide (0.24 g) was combined with fumed silica (0.22 g) and the solid mixture was homogenized to disperse the silica particles. The solid mixture (0.46 g) was combined with 4.54 g of the second solution and homogenized via stirring.

[0084] The weight percentages of the components in this example precursor composition were 10.2% CAP, 4.8% LiI, 2.9% SR 259, 1.5% SR 494, 1.4% poly(caprolactone triol), 0.1% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, 22.5% 1-methoxy-2-propanol, 52.2% dimethylformamide, and 4.4% silica. In dry down form, the weight percentages of the components in this example precursor composition were 40.2% CAP, 19.1% LiI, 11.5% SR 259, 5.7% SR 494, 5.7% polycaprolactone triol, 0.5% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, and 17.2% silica.

[0085] Example 5: Semi-IPN nanocomposite solid polymer electrolyte precursor composition containing cellulose acetate propionate (CAP), polymerizable oligomer, and alumina A cellulose ester solution was prepared by dissolving cellulose acetate propionate (CAP, 16.30 g) in dimethylformamide (83.7 g) with stirring. Separately, lithium iodide (1.10 g) was combined with alumina (1.00 g) and the resulting solid mixture was homogenized to disperse the alumina particles. The cellulose ester solution (16.3%, 3.12 g) was combined with poly(ethylene glycol) 200 diacrylate (SR 259, 0.14 g), alkoxylated pentaerythritol tetraacrylate (SR 494, 0.07 g), polycaprolactone triol (Mw=300 0.04 g), 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone (0.06 g), the solid mixture of lithium iodide and alumina, and 1-methoxy-2-propanol (1.19 g). The slurry was homogenized via stirring.

[0086] The weight percentages of the components in this example precursor composition were 10.1% CAP, 4.8% LiI, 2.9% SR 259, 1.4% SR 494, 0.8% poly(caprolactone triol), 0.1% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, 23.7% 1-methoxy-2-propanol, 51.8% dimethylformamide, and 4.4% silica. In the dry down form, the weight percentages are as follows: 41.2% CAP, 19.6% LiI, 11.8% SR 259, 5.9% SR 494, 3.1% polycaprolactone triol, 0.5% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, and 17.9% alumina.

[0087] Example 6: Semi-IPN nanocomposite solid polymer electrolyte precursor composition containing cellulose acetate propionate, polymerizable oligomer, titania, and alumina A cellulose ester solution was prepared by dissolving cellulose acetate propionate (CAP, 16.30 g) in dimethylformamide (83.7 g) with stirring. After complete dissolution, a second solution was prepared by combining the first cellulose ester solution (16.3%, 31.18 g) with poly(ethylene glycol) 200 diacrylate (SR 259, 1.45 g), alkoxylated pentaerythritol tetraacrylate (SR 494, 0.73 g), polycaprolactone triol (Mw=300, 0.72 g), 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone (0.06 g), and 1-methoxy-2-propanol (11.25 g). The solution was homogenized via stirring. Separately, lithium iodide (0.24 g) was combined with alumina (0.11 g) and titania (0.11 g). The resulting solid mixture was homogenized to disperse the particles. The second solution (4.54 g) was added to the lithium iodide, alumina, and titania solid mixture (0.46 g). The resulting slurry was homogenized via stirring.

[0088] The weight percentages of the components in this example precursor composition were 10.2% CAP, 4.8% LiI, 2.9% SR 259, 1.5% SR 494, 1.4% poly(caprolactone triol), 0.1% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyro-phenone, 22.5% 1-methoxy-2-propanol, 52.2% dimethylformamide, and 2.2% silica and 2.2% titania. In dry-down form, the weight percentages of the components in this example precursor composition were 40.2% CAP, 19.1% LiI, 11.5% SR 259, 5.7% SR 494, 5.7% polycaprolactone triol, 0.5% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, 8.6% alumina, and 8.6% titania.

[0089] Example 7: Semi-IPN nanocomposite solid polymer electrolyte precursor composition containing cellulose acetate propionate, polymerizable oligomer, and titania A cellulose ester solution was prepared by dissolving cellulose acetate propionate (16.30 g) in dimethylformamide (83.7 g) with stirring. After complete dissolution, a second solution was prepared by combining the first cellulose ester solution (16.3%, 31.18 g) with poly(ethylene glycol) diacrylate (SR 259, 1.45 g), alkoxylated pentaerythritol tetraacrylate (SR 494, 0.73 g), polycaprolactone triol (Mw=300, 0.72 g), 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone (0.06 g), and 1-methoxy-2-propanol (11.25 g). The solution was homogenized via stirring. Separately, lithium iodide (0.24 g) was combined with titania (0.22 g) and the resulting solid mixture was homogenized to disperse the particles. The second solution (4.54 g) was added to the lithium iodide and titania solid mixture (0.46 g). The slurry was homogenized via stirring.

[0090] The weight percentages of the components in this example precursor composition were 10.2% CAP, 4.8% LiI, 2.9% SR 259, 1% SR 494, 1.4% poly(caprolactone triol), 0.1% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyro-phenone, 22.5% 1-methoxy-2-propanol, 52.2% dimethylformamide, and 4.4% titania. In dry-down form, the weight percentages of the components in this example precursor composition were 40.2% CAP, 19.1% LiI, 11.5% SR 259, 5.7% SR 494, 5.7% polycaprolactone triol, 0.5% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, and 17.2% titania.

[0091] Example 8: Semi-IPN nanocomposite solid polymer electrolyte precursor composition containing cellulose acetate propionate, polymerizable oligomer, titania, and bis(2-ethylhexyl adipate) as a plasticizer A cellulose ester solution was prepared by dissolving cellulose acetate propionate (12.23 g) in 1-methoxy-2-propanol (87 g) with stirring. After complete dissolution, bis(2-ethylhexyl) adipate (0.80 g) was added to the solution, and the solution was homogenized via stirring. A second solution was prepared by combining the first cellulose ester solution (12.2%, 32.60 g) with poly(ethylene glycol) 200 diacrylate (SR 259, 1.20 g), alkoxylated pentaerythritol tetraacrylate (SR 494, 0.6 g), and diethylene glycol monoethyl ether acetate (4.80 g). The solution was homogenized via stirring. Separately, a third cellulose ester solution was prepared by dissolving cellulose acetate propionate (3.10 g) in 1-methoxy-2-propanol (96.90 g) with stirring. After complete dissolution, titania (3.00 g) was combined with the third cellulose ester solution (9.68 g) and 1-methoxy-2-propanol (4.00 g). The resulting slurry was homogenized via stirring to disperse the particles. Lithium iodide (0.24 g) was combined with titania (0.22 g) and the resulting solid mixture was homogenized to disperse the particles. Separately, the titania slurry (0.57 g), the second solution (2.00), lithium iodide (0.21 g), and a 5% solution of 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone in acetone (0.06 g) were combined. The resulting slurry was homogenized via stirring.

[0092] The weight percentages of the components in this precursor composition were 7.2% CAP, 0.5% bis(2-ethylhexyl)adipate, 7.3% LiI, 2.2% SR 259, 1.1% SR 494, 0.1% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, 3.6% titania, 67.5% 1-methoxy-2-propanol, 8.7% diethylene glycol monoethyl ether acetate, and 1.9% acetone. In dry down form, the weight percentages of the components in this example were 32.7% CAP, 2.1% bis(2-ethylhexyl)adipate, 33.2% LiI, 10.0% SR 259, 5.0% SR 494, 0.4% 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone, and 16.6% titania.

[0093] Example 9: Preparation of semi-IPN solid polymer electrolyte and ionic conductivity test The precursor compositions of the above examples were coated onto aluminum substrates to obtain the corresponding semi-IPN solid polymer electrolyte films. Prior to coating the films, the substrates were immersed in 5 wt% KOH aqueous solution for 30 seconds, rinsed three times with water, rinsed with isopropanol, and dried. The precursor compositions were blade coated onto the surface of cleaned aluminum foil at different wet coverages to yield dry film thicknesses of about 75 μm to 150 μm. Each coating was dried at 100° C. for 5 minutes before being exposed to UV light using Xe-Hg 1000W for 15 seconds under nitrogen or argon flow to photopolymerize the polymerizable components (e.g., acrylates). The samples were then dried and annealed at temperatures of 100° C. to 150° C. for 1 to 2 hours to obtain dried semi-IPN solid polymer electrolyte films.

[0094] Typically, the dried semi-IPN solid polymer electrolyte film contained 25-60 wt. % of the polymer component 104 of FIG. 1, 2-7 wt. % of the plasticizer 112 of FIG. 1, 20-35 wt. % of the lithium salt and / or complex 108 of FIG. 1, 10-25 wt. % of the polymerizable component 106 (or by-products thereof), 10-25 wt. % of the ceramic particles 116 of FIG. 1, and 1-5 wt. % of the photoinitiator 114 of FIG. 1 (or by-products thereof).

[0095] The ionic conductivity of the exemplary semi-IPN solid polymer electrolyte films was tested by placing the films (e.g., sandwiching) between two aluminum electrodes and recording electrochemical impedance spectra at an alternating current (AC) voltage of 10 mV and a frequency sweep from 1 MHz to 1 mHz.

number

[0096] FIG. 4 shows Bode plots 400 of cells containing semi-IPN SPEs prepared using the different precursor compositions of Examples 3-8 above.

[0097] Table 2 shows the ionic conductivity determined for the different solid polymer electrolyte film examples above. The information in Table 2 shows that improved ionic conductivity was obtained by including ceramic particles in the electrolyte precursor. Each of the solid polymer electrolyte films prepared from the precursors of Examples 4-7 having ceramic particles had enhanced ionic conductivity compared to that of the solid polymer electrolyte film prepared from the precursor of Example 3 lacking ceramic particles. [Table 2]

[0098] Table 3 below shows the ionic conductivity determined for the above example solid polymer electrolyte films having different types of plasticizers. The information in Table 3 shows that the inclusion of bis(2-ethylhexyl)adipate as a plasticizer instead of polycaprolactone triol improves the ionic conductivity. [Table 3]

[0099] Example 10: Dynamic Mechanical Analysis of Semi-IPN Solid Polymer Electrolytes The mechanical and thermal properties of the semi-IPN solid polymer electrolyte film examples were tested by dynamic mechanical analysis (DMA) under tension with a temperature sweep of 2° C. / min, a frequency of 1 Hz (6.28 rad / s), a strain of 0.4%, and an applied force of 3.0 grams. FIG. 5 shows a plot 500 of the DMA data of the semi-IPN SPEs prepared using the precursor compositions of Examples 1-8. As shown in FIG. 5, the solid polymer electrolytes described in this disclosure have a high glass transition temperature of 135° C., which makes these semi-IPN SPEs suitable for high temperature applications. In addition, the semi-IPN SPEs exhibit a storage modulus of about 0.45 Gpa, which is useful for solid polymer electrolyte films.

[0100] Modifications, additions, or omissions may be made to the systems, devices, and methods described herein. System and device components may be integrated or separated. Furthermore, system and device operations may be performed by more, fewer, or other components. Methods may include more, fewer, or other steps. Additionally, steps may be performed in any suitable order. Additionally, system and device operations may be implemented using any suitable logic. As used herein, "each" means each member of a set, or each member of a subset of a set.

[0101] As used herein, "or" is inclusive and not exclusive, unless expressly indicated otherwise or the context indicates otherwise. Thus, as used herein, "A or B" means "A, B, or both," unless expressly indicated otherwise or the context indicates otherwise. Furthermore, "and" is jointly and severally, unless expressly indicated otherwise or the context indicates otherwise. Thus, as used herein, "A and B" means "A and B, jointly or severally."

[0102] The scope of the present disclosure includes all changes, substitutions, changes, modifications, and alterations to the embodiments described and illustrated herein that are apparent to one of ordinary skill in the art. The scope of the present disclosure is not limited to the embodiments described or illustrated herein. Furthermore, although the present disclosure describes and illustrates each embodiment herein as including specific components, elements, features, functions, operations, or steps, any of these embodiments may include any combination or substitution of any of the components, elements, features, functions, operations, or steps described or illustrated anywhere herein that is apparent to one of ordinary skill in the art. Furthermore, in the appended claims, references to an apparatus or system, or a component part of an apparatus or system, being configured, arranged, capable, formed, enabled, operable, or operates to perform a particular function include the apparatus, system, or component, so long as the apparatus, system, or component is so configured, arranged, capable, formed, enabled, operable, or operates, regardless of whether the apparatus, system, component, or its particular function is activated, turned on, or unlocked. In addition, although the present disclosure may describe or illustrate particular embodiments as providing certain advantages, a particular embodiment may provide none, some, or all of these advantages.

[0103] In the context of describing the present invention (particularly in the context of the claims below), the terms "a" and "an" and "the" and similar referents should be construed to cover both the singular and the plural unless otherwise indicated or clearly contradicted by context. The terms "comprising," "having," "including," and "containing" should be construed as open-ended terms (i.e., meaning "including, but not limited to") unless otherwise indicated. The recitation of ranges of values ​​herein is merely intended to serve as a shorthand method of referring individually to each separate value contained within the range, unless otherwise indicated. Each separate value is then incorporated herein as if it were individually set forth herein. The use of any and all examples or example language (e.g., "such as") provided herein is merely intended to better illustrate the disclosure and does not limit the scope of the claims. The present invention can be embodied in the following manner. (Appendix 1) 1. A secondary battery cell, comprising: a cathode comprising a first electrode material; an anode comprising a second electrode material; a solid polymer electrolyte layer disposed between the cathode and the anode, the solid polymer electrolyte including a first surface in contact with the cathode and a second surface in contact with the anode, the solid polymer electrolyte layer comprising: a cellulose polymer matrix, the cellulose polymer matrix comprising a network of cellulose polymers; lithium ions dispersed in the cellulose polymer matrix; ceramic particles dispersed in the cellulose polymer matrix, the ceramic particles comprising a metal oxide; and one or more plasticizers dispersed in the cellulose polymer matrix; one or more polymer networks in contact with the cellulose polymer matrix, the one or more polymer networks comprising a crosslinked acrylate-containing polymer; A solid polymer electrolyte layer further comprising: a secondary battery cell. (Appendix 2) 2. The secondary battery cell of claim 1, wherein the solid polymer electrolyte layer further comprises one or more vinyl backbone polymers dispersed in or in contact with the cellulose polymer matrix, the one or more vinyl backbone polymers comprising a vinyl backbone and a molecular weight of less than 100,000 grams per mole. (Appendix 3) 2. The secondary battery cell of claim 1, wherein the solid polymer electrolyte layer comprises 25% to 60% by weight of the cellulose polymer matrix, 10% to 25% by weight of the acrylate-containing polymer, 20% to 35% by weight of the lithium ion source, 2% to 7% by weight of the one or more plasticizers, and 10% to 25% by weight of the ceramic particles. (Appendix 4) The solid polymer electrolyte layer has an ionic conductivity of at least 1×10 per centimeter -4 2. The secondary battery cell of claim 1, wherein the secondary battery cell is a Siemens. (Appendix 5) 2. The secondary battery cell of claim 1, wherein the ceramic particles include nanoparticles of one or more of titanium oxide, aluminum oxide, silicon oxide, zirconium oxide, tin oxide, tungsten oxide, and tantalum oxide. (Appendix 6) 2. The secondary battery cell of claim 1, wherein the cellulose polymer of the cellulose polymer matrix comprises one or more of a cellulose ester, cellulose acetate, and cellulose acetate propionate. (Appendix 7) The solid polymer electrolyte layer is made of lithium nitrate (LiNO 3 ), lithium iodide (LiI), lithium sulfide (Li 2 S), lithium perchlorate (LiClO 4 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), lithium hexafluoroarsenate(V) (LiAsF 6 ), lithium hexafluorophosphate (LiPF 6 ), and lithium tetrafluoroborate (LiBF 4 2. The secondary battery cell of claim 1, further comprising one or more lithium ion sources selected from the group consisting of: (Appendix 8) A solid polymer electrolyte, a cellulose polymer matrix comprising a network of cellulose polymers; lithium ions dispersed in the cellulose polymer matrix; ceramic particles dispersed in said cellulose polymer matrix, said ceramic particles comprising a metal oxide; one or more plasticizers dispersed in the cellulose polymer matrix; one or more polymer networks in contact with the cellulose polymer matrix, the polymer networks comprising crosslinked acrylate-containing polymers; A solid polymer electrolyte comprising: (Appendix 9) 9. The solid polymer electrolyte of claim 8, further comprising one or more vinyl backbone polymers dispersed in or in contact with the cellulose polymer matrix, the one or more vinyl backbone polymers comprising a vinyl backbone and a molecular weight of less than 100,000 grams per mole. (Appendix 10) 9. The solid polymer electrolyte of claim 8, further comprising 25% to 60% by weight of the cellulose polymer matrix, 10% to 25% by weight of the acrylate-containing polymer, 20% to 35% by weight of the lithium ion source, 2% to 7% by weight of the one or more plasticizers, and 10% to 25% by weight of the ceramic particles. (Appendix 11) The solid polymer electrolyte has an ionic conductivity of at least 1x10 per centimeter -4 9. The solid polymer electrolyte of claim 8, wherein the solid polymer electrolyte is Siemens. (Appendix 12) 9. The solid polymer electrolyte of claim 8, wherein the ceramic particles comprise nanoparticles of one or more of titanium oxide, aluminum oxide, silicon oxide, zirconium oxide, tin oxide, tungsten oxide, and tantalum oxide. (Appendix 13) 9. The solid polymer electrolyte of claim 8, wherein the cellulose polymer of the cellulose polymer matrix comprises one or more of a cellulose ester, a cellulose acetate, and a cellulose acetate propionate. (Appendix 14) Lithium nitrate (LiNO 3 ), lithium iodide (LiI), lithium sulfide (Li 2 S), lithium perchlorate (LiClO 4 ), lithium trifluoromethanesulfonate (LiCF3 SO 3 ), lithium hexafluoroarsenate(V) (LiAsF 6 ), lithium hexafluorophosphate (LiPF 6 ), and lithium tetrafluoroborate (LiBF 4 9. The solid polymer electrolyte of claim 8, further comprising one or more lithium ion sources selected from the group consisting of: (Appendix 15) 1. A method for producing a semi-interpenetrating polymer network solid polymer electrolyte, the method comprising: combining one or more cellulose polymers with one or more organic solvents; combining one or more polymerizable components with said one or more organic solvents; combining one or more photoinitiators with the one or more organic solvents, at least one of the one or more photoinitiators promoting polymerization of at least one of the one or more polymerizable components following irradiation with light; combining one or more lithium ion sources with the one or more organic solvents, each lithium ion source comprising a lithium ion salt or a lithium ion complex; combining one or more plasticizers with said one or more organic solvents; combining one or more ceramic particles with said one or more organic solvents, said ceramic particles comprising a metal oxide; producing a precursor by depositing at least a portion of the precursor on a surface of a substrate; exposing the deposited precursor to light, thereby forming a semi-interpenetrating polymer network solid polymer electrolyte; A method for producing a semi-interpenetrating polymer network solid polymer electrolyte, comprising: (Appendix 16) 16. The method of claim 15, further comprising applying heat to the deposited precursor. (Appendix 17) Following exposure of the deposited precursor to light, removing the semi-interpenetrating polymer network solid polymer electrolyte; disposing said semi-interpenetrating polymer network solid polymer electrolyte between a cathode layer and an anode layer, thereby forming a cathode-electrolyte-anode sandwich structure; applying pressure to the cathode-electrolyte-anode sandwich; 16. The method of claim 15, further comprising: (Appendix 18) 18. The method of claim 17, further comprising applying heat to the cathode-electrolyte-anode sandwich structure while applying pressure to the cathode-electrolyte-anode sandwich structure. (Appendix 19) 16. The method of claim 15, wherein the substrate is an anode or cathode for use in a secondary battery cell. (Appendix 20) The semi-interpenetrating polymer network solid polymer electrolyte is a cellulose polymer matrix comprising a network of cellulose polymers; lithium ions dispersed in the cellulose polymer matrix; ceramic particles dispersed in the cellulose polymer matrix, the ceramic particles comprising a metal oxide; one or more plasticizers dispersed in the cellulose polymer matrix; one or more polymer networks in contact with the cellulose polymer matrix, the polymer networks comprising crosslinked acrylate-containing polymers; 16. The method of claim 15, comprising:

Claims

1. 1. A secondary battery cell, comprising: a cathode comprising a first electrode material; an anode comprising a second electrode material; a solid polymer electrolyte layer disposed between the cathode and the anode, the solid polymer electrolyte including a first surface in contact with the cathode and a second surface in contact with the anode, the solid polymer electrolyte layer comprising: a cellulose polymer matrix, the cellulose polymer matrix comprising a network of cellulose polymers; lithium ions dispersed in the cellulose polymer matrix; ceramic particles dispersed in the cellulose polymer matrix, the ceramic particles comprising a metal oxide; and one or more plasticizers dispersed in the cellulose polymer matrix; one or more polymer networks in contact with the cellulose polymer matrix, the one or more polymer networks comprising a crosslinked acrylate-containing polymer; A solid polymer electrolyte layer further comprising: a secondary battery cell.

2. 10. The secondary battery cell of claim 1, wherein the solid polymer electrolyte layer further comprises one or more vinyl backbone polymers dispersed in or in contact with the cellulose polymer matrix, the one or more vinyl backbone polymers comprising a vinyl backbone and a molecular weight of less than 100,000 grams per mole.

3. 2. The secondary battery cell of claim 1, wherein the solid polymer electrolyte layer comprises 25% to 60% by weight of the cellulose polymer matrix, 10% to 25% by weight of the crosslinked acrylate-containing polymer, 20% to 35% by weight of the source of lithium ions, 2% to 7% by weight of the one or more plasticizers, and 10% to 25% by weight of the ceramic particles.

4. The solid polymer electrolyte layer has an ionic conductivity of at least 1×10 per centimeter -4 10. The secondary battery cell of claim 1, wherein the secondary battery cell is Siemens.

5. 10. The secondary battery cell of claim 1, wherein the ceramic particles comprise nanoparticles of one or more of titanium oxide, aluminum oxide, silicon oxide, zirconium oxide, tin oxide, tungsten oxide, and tantalum oxide.

6. 10. The secondary battery cell of claim 1, wherein the cellulose polymer of the cellulose polymer matrix comprises one or more of a cellulose ester, cellulose acetate, and cellulose acetate propionate.

7. The source of lithium ions is lithium nitrate (LiNO 3 ), lithium iodide (LiI), lithium sulfide (Li 2 S), lithium perchlorate (LiClO 4 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), lithium hexafluoroarsenate(V) (LiAsF 6 ), lithium hexafluorophosphate (LiPF 6 ), and lithium tetrafluoroborate (LiBF 4 2. The secondary battery cell according to claim 1, wherein the second battery cell comprises one or more selected from the group consisting of:

8. A solid polymer electrolyte, a cellulose polymer matrix comprising a network of cellulose polymers; lithium ions dispersed in the cellulose polymer matrix; ceramic particles dispersed in said cellulose polymer matrix, said ceramic particles comprising a metal oxide; one or more plasticizers dispersed in the cellulose polymer matrix; one or more polymer networks in contact with the cellulose polymer matrix, the polymer networks comprising crosslinked acrylate-containing polymers; A solid polymer electrolyte comprising:

9. 9. The solid polymer electrolyte of claim 8, further comprising one or more vinyl backbone polymers dispersed in or in contact with said cellulose polymer matrix, said one or more vinyl backbone polymers comprising a vinyl backbone and a molecular weight of less than 100,000 grams per mole.

10. 9. The solid polymer electrolyte of claim 8 further comprising 25% to 60% by weight of said cellulose polymer matrix, 10% to 25% by weight of said crosslinked acrylate-containing polymer, 20% to 35% by weight of said source of lithium ions, 2% to 7% by weight of said one or more plasticizers, and 10% to 25% by weight of said ceramic particles.

11. The solid polymer electrolyte has an ionic conductivity of at least 1×10 per centimeter -4 9. The solid polymer electrolyte of claim 8 which is Siemens.

12. 9. The solid polymer electrolyte of claim 8, wherein the ceramic particles comprise nanoparticles of one or more of titanium oxide, aluminum oxide, silicon oxide, zirconium oxide, tin oxide, tungsten oxide, and tantalum oxide.

13. 9. The solid polymer electrolyte of claim 8, wherein the cellulose polymer of the cellulose polymer matrix comprises one or more of a cellulose ester, cellulose acetate, cellulose acetate propionate.

14. The source of lithium ions is lithium nitrate (LiNO 3 ), lithium iodide (LiI), lithium sulfide (Li 2 S), lithium perchlorate (LiClO 4 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), lithium hexafluoroarsenate(V) (LiAsF 6 ), lithium hexafluorophosphate (LiPF 6 ), and lithium tetrafluoroborate (LiBF 4 The solid polymer electrolyte according to claim 8, wherein the solid polymer electrolyte is one or more selected from the group consisting of:

15. 1. A method for producing a semi-interpenetrating polymer network solid polymer electrolyte, the method comprising: combining one or more cellulose polymers with one or more organic solvents; combining one or more polymerizable components with said one or more organic solvents; combining one or more photoinitiators with the one or more organic solvents, at least one of the one or more photoinitiators promoting polymerization of at least one of the one or more polymerizable components following irradiation with light; combining one or more lithium ion sources with the one or more organic solvents, each lithium ion source comprising a lithium ion salt or a lithium ion complex; combining one or more plasticizers with said one or more organic solvents; combining one or more ceramic particles with the one or more organic solvents, the ceramic particles comprising a metal oxide; producing a precursor by depositing at least a portion of the precursor on a surface of a substrate; exposing the deposited precursor to light, thereby forming a semi-interpenetrating polymer network solid polymer electrolyte; A method for producing a semi-interpenetrating polymer network solid polymer electrolyte, comprising:

16. The method of claim 15 further comprising applying heat to the deposited precursor.

17. Following exposure of the deposited precursor to light, removing the semi-interpenetrating polymer network solid polymer electrolyte; disposing said semi-interpenetrating polymer network solid polymer electrolyte between a cathode layer and an anode layer, thereby forming a cathode-electrolyte-anode sandwich structure; applying pressure to the cathode-electrolyte-anode sandwich; The method of claim 15 further comprising:

18. The method of claim 17 further comprising applying heat to the cathode-electrolyte-anode sandwich structure while applying pressure to the cathode-electrolyte-anode sandwich structure.

19. The method of claim 15 , wherein the substrate is an anode or cathode for use in a secondary battery cell.

20. The semi-interpenetrating polymer network solid polymer electrolyte is a cellulose polymer matrix comprising a network of cellulose polymers; lithium ions dispersed in the cellulose polymer matrix; ceramic particles dispersed in the cellulose polymer matrix, the ceramic particles comprising a metal oxide; one or more plasticizers dispersed in the cellulose polymer matrix; one or more polymer networks in contact with the cellulose polymer matrix, the polymer networks comprising crosslinked acrylate-containing polymers; 16. The method of claim 15, comprising:

Citation Information

Patent Citations

  • Polymer electrolyte for secondary battery and lithium secondary battery comprising same

    EP3605705A1

  • Ionically conductive high-molecular solid electrolyte, composition, and production

    JP1996225626A

  • Ion conductive polymer sold electrolyte battery

    JP1997050824A

  • Solid polymer electrolyte composition and method for producing said solid polymer electrolyte composition

    JP2023529418A

  • High-ionic conductivity electrolyte compositions comprising semi-interpenetrating polymer networks and their composites

    WO2014147648A1