Accelerating admixtures for hydraulic compositions
A novel C-S-H seed-based admixture for cement accelerates hydration without corrosion or structural risks, addressing scalability and effectiveness issues of existing technologies, promoting rapid strength development and durability.
Patent Information
- Application Number
- JP2023043746
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-09-25
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2038-09-21
AI Technical Summary
Existing cement accelerators, such as chlorides and nitrates, accelerate corrosion of reinforcing steel and introduce alkali or nitrate ions that can cause cracking and structural deterioration in concrete, while organic compounds like triethanolamine reduce hydration rates at high doses, and current methods for producing C-S-H seeds are energy-intensive and difficult to scale.
A novel admixture based on C-S-H seeds is developed in an aqueous suspension, using carboxylic acids or their calcium salts, without grinding, to promote rapid strength development in cement mixtures, compatible with supplementary cementitious materials, and avoiding alkali or nitrate introduction.
The admixture effectively accelerates cement hydration without corrosion risks, maintains mechanical strength, and is scalable, allowing for rapid development of strength even with reduced Portland cement use, enhancing durability and processability.
Smart Images

Figure 0007560592000015 
Figure 0007560592000016 
Figure 0007560592000017
Abstract
Description
[Technical field]
[0001] The object of the present invention is to provide a water-based cementitious material based on Portland cement and other auxiliary cementitious materials. A novel admixture containing a hardening accelerator for hard compositions. [Background technology]
[0002] Accelerators are used in the construction industry to increase the mechanical strength of cement mixtures with short hardening times. Their use results in faster removal of steel and therefore the need for more rapid recovery and reuse of structural materials, or the fact that significant The need to allow work to proceed more quickly when under load The lower temperature slows down the cement hydration reaction, so that the structure does not have enough strength to support itself. The use of accelerating admixtures is most effective because long curing times are required to reach mechanical strength values. It is most prevalent in geographical areas and periods with cold climates. Accelerating admixtures are used to It accelerates the hydration reaction rate, so it increases mechanical strength in a short curing time, but it also increases mechanical strength over a long period of time. It does not affect the total amount of cement that reacts with water and therefore the final mechanical strength of the product. does not substantially change the
[0003] Contains chlorides, fluorides, carbonates, nitrites, nitrates, thiosulfates and thiocyanates. Many inorganic compounds, including fluorine, are known to have accelerating properties. Organic compounds include triethanolamine, diethanolamine, urea, and glyoxal. and formates.
[0004] Chlorides and nitrates, especially calcium chloride and calcium nitrate, are the most effective accelerators. However, it has the disadvantage of promoting corrosion of reinforcing bars, resulting in Their use in cement masses is precluded. Calcium formate does not present the above mentioned risks. When added in small weight percentages, it acts as a cure accelerator. The greatest limitation to its usefulness is its low solubility in water, which prevents its use in aqueous solutions. Therefore, it must be used in powder form, which is added directly to the concrete during mixing. No.
[0005] Other organic accelerators such as triethanolamine are used at low doses (0.025% by weight of cement). At high doses (0.06% by weight of cement), it acts as a cement hydration accelerator. ) slows down the hydration rate.
[0006] The action of the accelerator is mainly to increase the silicate phase of the cement, especially the main phase of Portland cement. It is performed on the key component tricalcium silicate, 3CaO·SiO2. Cement chemistry So the importance of tricalcium silicate, abbreviated as C3S (C=CaO, S=SiO2), is It is the most abundant component (50-70%) of cement, especially in cementitious pastes. This phase contributes to hardening. Due to the reaction of this phase with water, the cement hardens and hardens within a few hours. The material changes from a pourable plastic mass to a hardened aggregate capable of withstanding considerable mechanical stress. The hydration reaction of tricalcium silicate is as follows: C3S+(3-x+y)·H2O→(3-x)·Ca(OH)2+C x SH y The product formed by hydration of C3S with water, i.e. calcium silicate hydrate, is It is a compound of uncertain composition, and the ratio of the various components (C=CaO, S=SiO2, H=H2O) varies over time. For this reason, and because no definite crystal structure exists, Therefore, the compound is generally known by the name "calcium silicate hydrate gel" and CS- It is indicated by the notation H. CSH covers the cement granules and is characterized by a large surface area. A porous product, made of fibres with lengths up to a few microns and thicknesses of a few tenths of a micron The granules are present as agglomerates of granular particles, the connections of which contribute to determining the bonding properties of the cement.
[0007] Although the mechanism of action of the above-mentioned accelerators has not yet been fully elucidated, the compounds are believed to Adsorption processes, ion chelation, precipitation of insoluble salts, and modification of the microstructure of the hydrated phase It is believed that this accelerates the C3S hydration reaction. A comprehensive review of the literature can be found in Collepardi, M., "Scienzae Tecnologia del Calcestruzzo", Hoep li Editore, Milano, 1987, pp. 335-337, in Ramachandran, VS, "Concrete Admixtur es Handbook - Second edition", Noyes Publications, Park Ridge, NY, 1995, pp. 1 85-273 and pp. 1047-1049, and Cheung, J. et al., "Impact of Admixtures on the Hy dration Kinetics of Portland Cement", Cement and Concrete Research, 41, 2011, pp . It can be seen in 1289-1309.
[0008] It has been reported that CSH can act as a hydration promoter for C3S (Kondo, R., Da Immon, M., J. Am. Ceram. Soc. 52, 1969. These results were obtained using calcium nitrate and Recently confirmed using synthetic CSH obtained by precipitation from sodium silicate solution. (Thomas, JJ et al., J. Phys. Chem., 113, 2009, pp. 4327-4334). The addition of the precipitate to the cement paste increases the production of CSH by hydration of C3S in the cement. They act as crystallization seeds for the composition, both on the cement particles and in the capillary porosity of the admixture. , which promotes the nucleation and precipitation of the granules, resulting in enhanced mechanical strength of the hardened agglomerates. It has been demonstrated that this provides improved durability and performance.
[0009] International Publication No. 2010026155 describes CS- describes a process for producing H, in which calcium ions and silica Branched polymer superplasticizers for cement mixtures from aqueous liquids containing methylcellulose or silica ions ( Precipitating calcium silicate hydrate in the presence of 'comb polymers' .
[0010] Examples of such compounds are maleic acid, acrylic acid and vinyloxybutyl-polyethylene. Based on a terpolymer of glycol-5800, the molecular weight (Mw ), a polycarboxylate ether having a molecular weight (Mw) of about 73,000 g / mol Maleic acid, acrylic acid and vinyloxybutyl-polyethylene glycol 12000 terpolymer, and methacrylic acid and methoxypolyethylene methacrylate Based on copolymer of ethylene glycol-5,000, molecular weight of about 40,000 g / mol (Mw).
[0011] One drawback of the method described in WO 2010026155 is that high concentrations The presence of alkali and nitrate anions, which are the final products of the reaction. The alkali metals present are present in the amorphous silica particles present in some aggregates. to the point of reacting with the oxidizing agent to cause cracking and structural deterioration in the hardened concrete. This causes an expansion reaction (ASR - alkali silica reaction) that creates tension in the concrete. Nitrate anions are a potential cause of reinforcement deterioration. The use of the admixture in the production of rites is precluded.
[0012] A commercially available example of a product produced by the above process is Product Master X-Seed 100 (BAS F) and its data sheet indicates an alkali content of 5%.
[0013] U.S. Pat. No. 5,709,743 discloses a method for preparing a siliceous hydraulic binder in the form of an aqueous suspension. Use of hardening and hardening accelerators for siliceous binders obtained by hydration and grinding of suspensions The admixture, based on the promotion effect of CSH seeds, has a water ratio of 0.6 to 25. In the presence of water in an amount sufficient to form a binder weight ratio (W / B), at temperatures between 5°C and 90°C, Hydrate Rutland cement or other hydraulic binder rich in silicate phases and dissolve the resulting suspension. The liquid is subjected to a grinding process in a fine grinding mill until the desired particle size is obtained. Alternatively, the hydration and grinding steps can be simultaneous, and for example, corundum borate can be used. The final product has a solids content ranging from 5% to 55% by weight. It has a shape and a settling that reaches at least 60% of its initial height after 2 days.
[0014] The disadvantage of this method is that it requires wet grinding of the cement and water suspension, which is difficult to achieve on a large scale industrial scale. The disadvantage is that it requires a mill, which entails significant energy consumption and maintenance costs.
[0015] The accelerators developed to date that act primarily on the silicate phase of Portland cement are Portland cement may be partially or entirely substituted for other binders, particularly Portland cement. Fly ash or coal from coal-fired power plants used to reduce cement consumption originates from other types of production, such as ground granulated blast furnace slag obtained in the cast iron production process. It is not equally effective for hydraulic systems that are replaced by industrial by-products.
[0016] These supplementary cementitious materials have a longer hardening time (60 days after mixing) and therefore a higher mechanical strength. It only contributes to the development of , but not to the development of , at short curing times (less than 24 hours). As a result, no more than 15-20% of Portland cement is replaced with supplemental cementitious materials. Otherwise, excessive initial delays in the concrete hardening stage can occur, resulting in short The mechanical properties deteriorate over the curing time, making the construction process unacceptably slow. The steel mould is removed until the concrete inside has reached a mechanical strength sufficient to stand on its own. This means that construction work cannot proceed. Summary of the Invention
[0017] The present invention relates to a novel admixture based on CSH seeds in aqueous suspension, A hydraulic binder derived from cement or other silicate-based binders that improves the mechanical properties of cementitious mixtures. It is extremely effective in promoting rapid strength development and at the same time is the most effective promoter developed to date. It relates to an admixture that can produce an accelerated admixture that does not exhibit any of the disadvantages of the admixture.
[0018] The present invention relates to a method for obtaining said admixture, in particular the method according to the present invention is described in WO 02 / 04336. Unlike the method described in the brochure No. 2010026155, the final product No alkali or nitrate ions are introduced, so the product can be used in concrete. In the case of concrete, the risk of promoting alkali-aggregate reaction and corrosion of reinforcing bars is not increased. The method according to the present invention differs from that of U.S. Pat. No. 5,709,743 in that the maximum No milling step is required to ensure efficacy and stability of the resulting suspension.
[0019] The admixture according to the invention, either alone or in combination with sodium carbonate, is used in fly ash. It is particularly effective in activating auxiliary cementitious materials such as granulated blast furnace slag and ground granulated blast furnace slag. and their hardening even when little or no Portland cement is present. This property promotes the formation of viscoelasticity in hydraulic compositions without compromising mechanical strength in short curing times. This significantly increases the replacement rate of auxiliary cementitious materials.
[0020] An important aspect of the present invention is the use of Portland cement (or other hydraulic cement based on silicates). The hydration reaction of the mixture is carried out with carboxylic acid or its calcium salt, polyethanolamine or Surprisingly, the hydraulic The hydration of the binder is carried out in pure water as described in U.S. Pat. No. 5,709,743. Instead, the compounds mentioned above, in particular formic acid, acetic acid or their calcium salts, monoethanolamine, diethanolamine and triethanolamine, isopropanolamine or or mixtures thereof in aqueous solution, the acceleration properties of the final product are surprisingly improved. The aqueous suspension of the product thus obtained is completely stable and no longer subject to settling. It was found not to be subject to the process.
[0021] These results characterize the synthesis process leading to the formation of the product according to the invention. Under these conditions, calcium ions and organic substances (carboxylic acids or This is thought to be due to the formation of compounds between MOFs (Metal-Organic Compounds) and amino compounds. These compounds, called crystalline frameworks (C Frameworks), are essentially metal complexes coordinated with rigid organic binders. A crystalline material made of ions, with a very high degree of porosity, one-, two- or three-dimensional Generate the original structure. The empty space in the material can reach 90% of its volume, and 600 0m 2 1. It has a very large internal surface area that can exceed 1 / g (Zhou, H., Long, J. R. and Yaghi, OM, Chem. Rev, 2012, 112 (2), pp. 673-674). [Brief description of the drawings]
[0022] [Figure 1] 1 is an environmental electron microscope photograph of a sample of Example 4. [Diagram 2] 1 is an environmental control electron microscope photograph of a sample of Comparative Example 2. [Diagram 3]FIG. 1 shows XPRD spectra of the sample of Example 14 and the sample of Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The carboxylic acids or their calcium salts and polyethanolamines used according to the invention The amount of min is based on the weight of Portland cement or other primarily silicate-based hydraulic binder. A wide range of 2% to 40%, preferably 5% to 25%, and even more preferably 10% to 20% of the It varies within the range of Portland cement and standard UNI-EN197-1:2006 All of the other cement types mentioned may be advantageously used in the present invention.
[0024] Examples of cements are those based only on clinker and gypsum (type CEM I), limestone cement, (Type CEM II / AL, CEM II / BL, CEM II / A-LL, CEM II / B-LL), Blast furnace slag Cement (types CEM II / AS, CEM II / BS) and pozzolanic cement (types CEM IV CEM IV / A, CEM IV / B). The cements with the highest silicate phase content are the ones that undergo the most hydration. This is naturally preferred since it allows for the production of large amounts of CSH seeds.
[0025] The amount of water required to develop hydration of the binder in a method useful for the purposes of the present invention is W / B=1 to W / B=6, preferably W / B=1.5 to W / B=4, and even more preferably W / B=2 to W / B=3. The water / binder ratio varies within a wide range.
[0026] The hydration of the binder in the aqueous solution containing the compound according to the invention is preferably carried out in a stirred tank or The temperature in the reactor is atmospheric pressure and 10°C to 90°C, preferably 20°C to 80°C, and more preferably The treatment is preferably carried out at a temperature in the range of 40° C. to 60° C. for a time in the range of 2 hours to 300 hours.
[0027] The stirring can be continuous or discontinuous using anchor or rotor stirrers, which It must be effective to ensure homogenization of the mass during the reaction. The auxiliary ultradispersion system is It can be conveniently combined with conventional stirring systems.
[0028] From an operational point of view, the reactor or tank is a defined vessel in which the compound according to the invention is dissolved. The temperature is adjusted to the desired value for the reaction and the hydraulic binder is stirred. Add gradually while stirring.
[0029] The hydration reaction may be carried out in the presence of auxiliary ingredients such as dispersants, viscosity control agents or stabilizers, The dispersants that can be used to impart desired properties to the final product include, for example, For example, gluconic acid and its salts, polyether carboxylate polymers, lignin sulfate, etc. of naphthalene sulfonate, naphthalene sulfonate and melamine sulfonate with formaldehyde Condensates, polysaccharide derivatives and phosphonated polymers. The medications include sodium carbonate, methylcellulose, hydroxyethylcellulose (HEC), Hydroxypropyl cellulose (HPC), methylhydroxyethyl cellulose (MHE C) a polysaccharide derivative selected from the group including methylhydroxypropylcellulose (MHPC); Conductors, and / or non-ionic monomers of (meth)acrylamide and sulfonated monomers The average molecular weight is 500,000 g / mol. mol, preferably more than 1,000,000 g / mol (co)polymers or is a modified polyurea. Hydroxy carboxylic acids or their salts, such as citric acid, malic acid Alternatively, oxalic acid can be used as a stabilizer. It can be added at the end of the reaction.
[0030] Add sodium carbonate or sodium sulfate during or at the end of the hydration stage In addition, even in the absence of Portland cement, fly ash, ground granulated blast furnace slag and The hydraulic properties of auxiliary cementitious materials such as carbon and calcined clay are effectively promoted. In combination with sodium sulfate or sodium sulphate, the admixture according to the invention is No Portland cement is used, known as "mar" or alkali-activated binder. Hydraulic admixtures, i.e., sodium aluminosilicates whose structural units are derived from sodium carbonate It can be conveniently used to prepare a binder system that condenses with ammonium ions. The amount of sodium that can be used is 3% to 40% of the dry weight of the hydrated suspension, preferably 5% to 30%, and even more preferably in the range of 10% to 20%.
[0031] The accelerator according to the invention is optionally in combination with sodium carbonate or sodium sulfate. , as an activator for admixtures based on "geopolymer" binders, and for conventional plasticizing and superplasticizing It can be used in combination with plasticizing admixtures, this embodiment being alkaline silicates and Common "geopolymer" activators, such as those based on alkali hydroxides, act as plasticizers and and superplasticizers are known to be incompatible with the use of Please note that.
[0032] The accelerator of the present invention is added to the concrete production unit together with the mixing water and other admixtures. or optionally after drying in solid form, other components of the admixture, e.g. The cementitious material may be premixed with cement, fly ash or other auxiliary cementitious materials. The accelerator according to the invention can also be added during the clinker grinding stage. A typical dosage of the agent is 1% by weight of the cementitious materials used to prepare the cement mix. It may be in the range of 0.1 to 60%, preferably 2% to 45%, and even more preferably 5% to 35%. EXAMPLES
[0033] Particular features of the invention are described in the following examples.
[0034] Example 1 56 g of calcium formate was dissolved in 1400 g of water at 80°C, and the resulting solution was treated with calcium formate. Heat the solution in a 2000 ml glass beaker with a mechanical stirrer until the sodium is completely dissolved. Stirring was maintained. Portland according to the classification of standard UNI-EN197-1:2006 Add 560 g of Dosed Cement Type 52.5R to the liquid within 30 seconds at a temperature of 80°C. Ta. The properties of the 52.5R cement used are given in the table below.
[0035] [Table 1]
[0036] The hydration reaction was continued for 6 hours under stirring at a temperature of 80°C. During the reaction, the product was in the form of a fluid suspension. The gray color remained the same, but tended to become paler over time. At the end of the period, the product was cooled and transferred to a plastic container. Approximately 2000 g of product was obtained. The dry matter content was measured at 105°C to be 32% and constant weight.
[0037] Comparative Example 1 560 g of 52.5R cement from Table 1 was mixed for 80 minutes using the same procedure as described in Example 1. The hydration reaction was continued for 6 hours at a temperature of 80° C. under stirring. During this time, the product remains in the form of a fluid suspension, and its grey colour becomes more blue over time. It tended to turn white. At the end of the reaction, the product was cooled and transferred to a plastic container. About 1950 g of product was obtained, the dry matter content measured at 105° C. being 31.5%. The weight was constant.
[0038] Example 2 The products of Example 1 and Comparative Example 1 are specified in the standard UNI-EN197-1:2006. As shown in the figure, in the plastic mortar test, the hardening rate was 1.0% using standard sand and a sand / cement ratio of 3. The cement used to manufacture the plastic mortar was The cement was the same as in Example 1, CEMI 52.5R. To achieve the desired workability, poly Dynamon SP1 (Ma), a superplasticizing admixture based on ether carboxylate polymers All mixtures were prepared with a water / cement ratio of W / C = 0.42 and various In some cases, the water introduced with the mixture was measured as mixing water.
[0039] After spreading measurement, it has dimensions of 4 cm x 4 cm x 16 cm Prismatic specimens were prepared using mortar and stored under standard laboratory conditions (20°C and 95% R / H). Their compressive strengths were measured after 7 and 24 hours of curing. The composition and properties of the two other mixes (Mix 3 and Mix 4) are shown in Table 2 below. Mix 3 was prepared by adding the product of Comparative Example 1 to the product of Example 1. Add separately the same amount of calcium formate (2.5 g) as was introduced into the mix by Mix 4 was prepared by adding the same amount (2.5 g) of the mixture introduced in Example 1. The proportions of the admixtures in Example 1 and Comparative Example 1 are In this case, the dry matter content as a percentage of the weight of cement was 6.2%.
[0040] [Table 2]
[0041] As can be seen from the results in Table 2, Mix 1 containing the admixture of Example 1 of the present invention has a mechanical It develops mechanical strength most rapidly (14.5 MPa after 7 hours of curing). The product of Comparative Example 1 used in Mix 2 was synthesized without calcium formate and after 7 hours of curing It exhibits about half the mechanical strength of the product according to the invention (7.8 MPa after 7 hours of curing). The product of Comparative Example 1 was mixed with the product of Example 1 in the same amount of gypsum (2.5 g). The addition of calcium hydroxide did not substantially change the mechanical strength development, and the mechanical strength after 7 hours The pressure value increased from 7.8 MPa to 8.0 MPa. Calcium formate added directly to the mix The moderate contribution of calcium formate is also shown by the low intensity value of Mix 4, which contains only calcium formate. It was confirmed that after 7 hours, the mechanical strength was only 1.4 MPa. Afterwards, all specimens performed as expected since all mixes had the same water / cement ratio. Comparable mechanical strength values were reached.
[0042] The results of this example were obtained by using calcium formate solution (according to the present invention) instead of pure water (Comparative Example 1). Accelerated properties of the final product by carrying out the hydration reaction of the hydraulic binder in Example 1) The results were surprisingly improved, and this improvement was observed when the same amount of calcium formate and Portland The effect of simple combination with admixtures obtained by hydrating cement in water alone This proves to be significantly greater than that (Comparative Example 1).
[0043] Example 3 In this example, calcium formate (CaF) in the synthesis of Example 1 was used as shown in Table 3 below. As prescribed, other substances were substituted, specifically 100% calcium acetate (CaAC). (Recipe 3A), diethanolamine (DEA) 85% aqueous solution (Recipe 3B), and Triethanolamine (TEA) 85% aqueous solution (recipe 3C) was used. The type of compound was the same as that in Example 1, and the synthesis method was also the same. The calcium was mixed with an equal amount of 100% calcium nitrate ( The synthesis was carried out under the same conditions as in Example 1, with CaN (recipe 3COMP) replacing CaN.
[0044] [Table 3]
[0045] Table 4 below shows the characteristics of mortars produced using the products synthesized according to the recipes in Table 3. Indicates gender.
[0046] [Table 4]
[0047] As can be seen from the results in Table 4, calcium acetate, monoethanolamine and triethanolamine All mixtures made with admixtures made with Nolamine showed short setting times (7 It exhibits very high mechanical strength at 1000 rpm (300 rpm), which is the same as that of calcium acetate. 3COMP is made using calcium nitrate, one of the most powerful cement accelerators. , which is much the same as the product synthesized using only water (Comparative Example 1, Table 2, Mix 2). It exhibited low mechanical strength.
[0048] Example 4 56 g of calcium formate was dissolved in 1400 g of water at room temperature (22°C), and the resulting solution was Heat the mixture in a 2000 ml glass beaker with a mechanical stirrer until the calcium formate is completely dissolved. The mixture was maintained under stirring using 560 g of Portland Cereal with the properties reported in Table 1. Cement type 52.5R was added to the solution in 30 seconds. The hydration reaction was carried out at 22° C. under stirring. The reaction was continued at temperature for 288 hours. During the reaction, the product remained in the form of a fluid suspension and its gray color The reaction mixture tended to become paler over time. Approximately 2000 g of product was obtained, with a dry matter content of 0.01 g measured at 105° C. The concentration was 40% and constant weight. A 5 g aliquot of the product was centrifuged to separate the aqueous phase. The separated solid material was washed repeatedly with acetone to inhibit hydration and then stored at 60°C for 2 h. The mixture was then left in a oven for 15 minutes to dry, yielding a light grey dry powder.
[0049] Comparative Example 2 560 g of 52.5R cement from Table 1 was mixed with 22 ml of 10 ... The hydration reaction was continued with stirring for 288 hours at a temperature of 22°C. During the reaction, the product remains in the form of a fluid suspension, and its gray color fades over time. At the end of the reaction, the product was transferred to a plastic container. 1950 g of product was obtained, the dry matter content measured at 105° C. was 37% and the product was then cooled to constant weight. A 5 g aliquot of the product was centrifuged to separate the aqueous phase. The separated solid material The hydration reaction was suppressed by repeatedly washing with acetone and then leaving it in a stove at 60°C for 15 minutes. The mixture was then dried to give a light grey dry powder.
[0050] Example 5 The samples of Example 4 and Comparative Example 2 were centrifuged, washed with acetone, dried, and then analyzed by ESEM ( The samples were analyzed for microstructural analysis using an environmental electron microscope (EMS), and the results are shown in the figures below. FIG. 1 shows an image of the product of Example 4 synthesized in the presence of 10% calcium formate per cement. 1 shows an image of the product of Comparative Example 2, which was synthesized without calcium formate, whereas FIG.
[0051] Comparison of the images in Figures 1 and 2 reveals significant differences in the microstructure of the two products. In fact, the product of Comparative Example 2 (FIG. 2), which was synthesized without calcium formate, was several microns in size. It takes the form of a set of particles having dimensions of 10% calcium formate, but is synthesized in the presence of 10% calcium formate. The product of Example 4 (Figure 1) shows a large number of submicron particles associated with larger particles. This result indicates that the cement was not oxidized during the synthesis of the product according to the invention. This paper demonstrates the surprising effectiveness of calcium formate in modifying the microstructure of the hydrated products.
[0052] The specific surface area was measured using a Beckman-Coulter SA3100 instrument to measure the microstructure of Example 4 and Comparative Example 2. The same samples used for the microstructural analysis were measured by the BET technique. The result was 154 m for the sample of Example 3. 2 The specific surface area value of the sample in Comparative Example 2 was About pull 27m 2 / g, and compared with those synthesized in pure water, 10% formic acid We demonstrate a significant increase in the specific surface area of the synthesis products in the presence of calcium. These differences are The two products evaluated in the plastic mortar test using the products of Example 4 and Comparative Example 2 were The test was carried out in the same manner as reported in Example 2. The results are shown in Table 5 below.
[0053] [Table 5]
[0054] As can be seen, the admixture of Example 4 according to the invention, synthesized with 10% calcium formate, Mix 10 containing the admixture was prepared using the admixture of Comparative Example 2 synthesized in pure water. It exhibits mechanical strength approximately 10 times greater than that of 11 after 6 and 7 hours of cure. Ta.
[0055] Example 6 112 g of calcium formate was dissolved in 1400 g of water at room temperature (22°C) and the resulting solution in a 2000 ml glass beaker with mechanical stirring until the calcium formate is completely dissolved. The mixture was maintained under stirring using a mixing machine. 560 g of Portland® with the properties reported in Table 1 Dosed cement type 52.5R was added to the solution in 30 seconds. The hydration reaction was continued for 22 minutes under stirring. The reaction was continued for 60 hours at a temperature of 100° C. During the reaction, the product remained in the form of a fluid suspension and the ash was The color tends to become paler over time. At the end of the reaction, the product is added to the Approximately 2000 g of product was obtained, with a dry matter content of 0.01 g measured at 105° C. was 40% and was constant weight.
[0056] Comparative Example 3 100 g of 52.5R Portland cement having the properties shown in Table 1 was heated at 22°C for 10 4 kg of alumina balls with diameters of 20 mm to 40 mm are dispersed in 00 ml of water. Hydration was carried out for 60 hours in a charged alumina jar with a volume of 8 liters. Rotation of the jar The velocity is 70 rp, as reported in Example A1 of U.S. Pat. No. 5,709,743. The hydrated cement had a dry matter content of 13%, measured to constant weight at 105°C. About 1100 g of a suspension of cement was obtained.
[0057] Comparative Example 4 560 g of 52.5 Portland cement having the properties reported in Table 1 was heated to 140 The mixture was dispersed in 0.0 ml of water and 4 kg of alumina balls with diameters of 20 mm to 40 mm were placed in the container. The mixture was hydrated for 60 hours in an 8-liter alumina jar filled with water. The rotational speed is 70 rpm, as reported in Example A1 of U.S. Pat. No. 5,709,743. The hydrated cement had a dry matter content of 39%, measured to a constant weight at 105°C. About 1550 g of a suspension of 1,2-dichloro-1,2-diphenyl-2,4-tetramethylphenylacetate was obtained.
[0058] Example 7 The products of Example 6 and Comparative Examples 3 and 4 were subjected to the same 52.5R polystyrene copolymer having the properties shown in Table 1. Trand cement was used in the plastic mortar test.
[0059] The dosage of different admixtures is the same amount of admixture on dry basis i.e. 5% of the weight of cement. was adjusted to ensure that was added in all cases.
[0060] The superplasticizing admixture Dynamon SP1 (Mapei) was used to achieve the desired processability. All admixtures were made with a water / cement ratio of 0.42 and used as admixtures in various cases as mixing water. The water introduced at the same time was measured. After the spread measurement, the size of the tube was 4 cm x 4 cm x 16 cm. Prismatic specimens were then placed in mortar and stored under standard laboratory conditions (20°C and 95% R / H). The compressive strength was measured after 6 and 7 hours of curing and the results are shown in Table 6 below. show.
[0061] [Table 6]
[0062] The results shown in Table 6 indicate that the product of Example 6 follows the teachings of U.S. Pat. No. 5,709,743. The products synthesized in Comparative Examples 3 and 4 had shorter curing times (6 and 7 hours). Greatly accelerates mechanical strength development, which is achieved by means of the wet grinding process during the cement hydration stage. Thus, it is demonstrated that the inclusion of increasing the fineness of the product is essential.
[0063] Example 8 112 g of calcium formate was dissolved in 1400 g of water at 60°C, and the resulting solution was treated with calcium formate. In a 2000 ml glass beaker, stir with a mechanical stirrer until the calcium is completely dissolved. The mixture was stirred at 40° C. for 24 hours and maintained at 4° C. for 24 hours. 560 g of Portland cement having the properties shown in Table 1 was added. Type 52.5R was added to this solution at a temperature of 60°C for 30 seconds. The hydration reaction was allowed to proceed without stirring. The reaction was continued for 8 hours. Throughout the reaction, the product remained in the form of a liquid suspension and its gray color remained. The color tended to fade over time. At the end of the reaction, the product was cooled and Approximately 2050 g of a fluid aqueous dispersion was obtained, with a dry mass measured at 105° C. The dry matter content was 39% and constant weight.
[0064] Example 9 The product of Example 8 was used to make a cement mixture, where the cement was It was gradually replaced by fly ash from thermal combustion plants. The by-product is cement Calcium silicate hydrate derived from calcium silicate hydrates, which form cement products very similar to CSH. It is a co-cementing ingredient and is used to replace part of the cement in cement mixtures. The advantage of using fly ash in cementitious mixtures is the lower use of cement. Lower environmental impact due to the amount of by-products and the effect on the durability of the cementitious mass. However, the reaction of fly ash in cementitious mixtures is slower. As a result, for long curing times (>90 days) the mixtures based only on cement It produces mechanical strengths very similar to those of fresh cellulose, but the short-term strength is much lower. The concrete-containing formwork cannot be removed quickly and therefore the progress of work is delayed. Delay. Therefore, while it is desirable to incorporate large amounts of fly ash into cementitious mixtures, A proportion of 15-20% of the weight of the component should not be exceeded for the reasons mentioned above. The cement used to manufacture the plastic mortar was the same 52.5R cement as in Table 1. On the other hand, the fly ash used, which can be classified as F type according to the standard ASTM C618, The composition is shown in Table 7 below.
[0065] [Table 7]
[0066] The superplasticizing admixture Dynamon SP1 (Mapei) was used to achieve the desired processability. All admixtures were made with a water / binder ratio of W / B = 0.42, where the "binder" is the cement and the filler. The mixing water is the sum of the product of Example 8 having a dry weight of 39%. The calculation was done by including the water introduced into the admixture. After the spread measurement, Prismatic specimens with dimensions of 16 cm x 16 cm were prepared and measured under standard laboratory conditions (20°C). and 95% R / H). Their compressive strength was measured at 7 hours, 24 hours and 90 days. The results are shown in Table 8 below.
[0067] [Table 8]
[0068] The results of the plastic mortar test shown in Table 8 show that the admixture according to the present invention is effective in reducing the fly ash Even in admixtures containing large amounts of EDTA, their ultimate long-term strength (90 days) is not affected. It has been shown to promote mechanical strength development at short cure times (7 hours) without compromising the hardness of the material. In the presence of the accelerator of Example 8, the admixture was different from that made with Portland cement alone. and the short hardening time caused by the introduction of fly ash into the cementitious mixture. It is possible not only to eliminate the delay between the In fact, by replacing 32% of the cement with fly ash, the strength after 7 hours was increased from 1.2MPa (Mix 15) to 7.3MPa (Mix 16), 44% The replacement rate of 67% ( Mix 18) showed that the compressive strength after 7 hours of hardening was higher than that of the mix containing only Portland cement. The compressive strength of the mixture is the same as that of the reference mix (Mix 15). In the absence of the agent, it was still too soft (Mix 19) after 7 hours. is not possible.
[0069] Example 10 The product of Example 8 was used to make a cement mixture, in which the cement was ground granular. It was gradually replaced by granulated blast furnace slag (GGBFS). It is a co-polymer that forms a cement product very similar to the calcium silicate hydrate (CSH) that is produced. It is a cement ingredient and is used to replace part of the cement in cement mixes. do. As in the case of fly ash, the advantage of using GGBFS in cementitious mixtures is that Lower environmental impact resulting from lower dosage of cement and the fact that said by-products are cementitious concrete. The resulting improvement in the durability of the glomerates. The slag reaction proceeds more slowly, resulting in a longer cure time (>90 days) for the cement. It produces mechanical strengths very similar to those of mixtures based solely on cement, but with a short-term The strength is much lower and therefore it is not possible to quickly remove the formwork containing fresh concrete. Therefore, large amounts of GGBFS are mixed with cementitious materials. It is desirable to incorporate it into the mixture, but for the above reasons, the ratio of 15 to 20% by weight of cement is The cement used to manufacture plastic mortar should not exceed The cement used was 52.5R, the same as in Table 1, but the composition of the slag used is shown in Table 9 below. .
[0070] [Table 9]
[0071] The superplasticizing admixture Dynamon SP1 (Mapei) was used to achieve the desired processability. All mixtures were made with a water / binder ratio W / B = 0.42, where the "binder" was the cement and slurry. The blend water is the sum of the mixture with the product of Example 7 having a dry weight of 39%. The calculation was done by including the water introduced into the 4cm x 4cm x 1 Prismatic specimens with dimensions of 6 cm were prepared and were then stored under standard laboratory conditions (20°C and 9 The compressive strengths of the specimens were measured after 7 hours, 24 hours and 90 days of curing. The results are shown in Table 10 below.
[0072] [Table 10]
[0073] The results of the mortar test shown in Table 10 show that the mixture of Example 8 of the present invention contains a large amount of slag. Even in mixtures that do not undergo any short-term aging without compromising their ultimate long-term strength (90 days), It shows that the mechanical strength development during the curing time (7 hours) is accelerated. In fact, the acceleration of Example 8 In the presence of the agent, the short-term adhesion caused by the introduction of slag into the cementitious mixture Not only does it eliminate any delay in hardening time, but it also provides a It is possible to increase the mechanical strength value at a short curing time (7 hours). When 32% of the cement was replaced with slag, the strength after 7 hours was 1.2 MPa (mil). Mix 15) to 9.8MPa (Mix 20), and 44% was replaced. 5.5MPa (Mix 21). For 67% replacement value (Mix 22) The compressive strength after 7 hours of hardening was compared with that of the reference mixture (Mix) using only Portland cement. 15) is still greater than the compressive strength of Example 8 according to the present invention in the absence of the accelerator. In this case, after 7 hours the sample was still too soft (mixture 23) and demolding was not possible. It is.
[0074] Example 11 112 g of calcium formate was dissolved in 1700 g of water at 60°C, and the resulting solution was In a 2000 ml glass beaker, stir with a mechanical stirrer until the calcium carbonate is completely dissolved. The mixture was maintained under stirring using 560 g of Portland malt having the properties reported in Table 1. Cement type 52.5R was added to this solution at a temperature of 60°C for 30 seconds. The reaction was continued for 8 hours with stirring. Throughout the reaction, the product was present in the form of a fluid suspension. The grey colour of the product tended to become paler over time. It was cooled and transferred to a plastic container. Approximately 2370 g of a fluid aqueous dispersion was obtained, which was then dried. The material content is 34% measured to constant weight at 105°C and the viscosity is 2.0% measured at 20°C. 000cP.
[0075] The product obtained from the synthesis was divided into three aliquots of 750 g each. One was kept untreated while different aliquots of powdered sodium carbonate, Na2CO3, were added to the other The addition was carried out under stirring, and the powdered carbonate was added to the aqueous suspension of the mixture in 10 minutes. The addition of sodium carbonate resulted in an increase in the viscosity of the aqueous suspension. Stirring was continued for 30 minutes.The samples shown in Table 11 below were prepared.
[0076] [Table 11]
[0077] Example 12 The sample of Example 11 was used to make a cement mixture in which fossil fuel thermal combustion It originates from the plant and can be classified as type F according to standard ASTM C618 and is shown in Table 7. The cement was completely replaced by fly ash having the composition of superplasticizing admixture Dy. The desired workability was achieved using a namon SP1 (Mapei). After spread measurements, 4c A prism-shaped specimen with dimensions of 100 mm × 4 cm × 16 cm was prepared and subjected to standard laboratory conditions ( The compressive strength of the specimens was measured after 7 and 28 days of curing at 20°C and 95% R / H. Measurements were taken after curing and the results are shown in Table 12 below.
[0078] [Table 12]
[0079] The results of the plastic mortar test in Table 12 show that the admixture of Example 11 and sodium carbonate This paper demonstrates the positive effect on mechanical strength development produced by the combination of Fly ash alone does not exhibit hydraulic properties. In fact, Mix 24, which is based solely on fly ash, does not develop mechanical strength even after 28 days of curing. The addition of the admixture of Example 11 resulted in moderate activation of the fly ash (2.5 MPa, 28 After hardening for 25 days, the mix was mixed with sodium carbonate and the admixture according to the invention. The compressive strength of the specimens improved progressively (Mixes 26 and 27), and this result was greater for Mix 2. Sodium carbonate alone, added at the same dosage as in 7, was used to measure the mechanical properties of fly ash (Mix 28). This is clearly surprising, bearing in mind that the effect of the
[0080] Example 13 A cement mixture was prepared using the sample of Example 11, and the cement had the composition shown in Table 9. It has been completely replaced by ground granulated blast furnace slag (GGBFS) with the superplasticizing admixture Dynamon SP1 (Mapei) was used to achieve the desired workability. After spread measurement, a 4cm x 4 Prismatic specimens with dimensions of 16 cm x 16 cm were prepared and measured under standard laboratory conditions (20°C). and 95% R / H). Their compressive strength was measured after 24 hours, 7 days, and 28 days of hardening. The results are shown in Table 13 below.
[0081] [Table 13]
[0082] The results of the plastic mortar test in Table 13 show that the admixture according to the present invention and sodium carbonate have demonstrated the favorable effect on mechanical strength development produced by the combination of As in the case of fly ash, blast furnace slag alone does not exhibit hydraulic properties, and in fact, Mix 29 based solely on GBFS does not develop mechanical strength even after 28 days of curing The combination of sodium carbonate and the admixture according to the invention was found to reduce the strength of the test specimens after 24 hours of hardening. Progressively improves compressive strength (Mix 31 and 32). Add at the same dosage as Mix 31. The mechanical strength of GGBFS after 24 hours (Mix 33) was This result is clearly surprising, bearing in mind that the compound does not promote the development of
[0083] Example 14 112 g of calcium formate was dissolved in 1653 g of water at 60°C, and the resulting solution was treated with calcium formate. In a 2000 ml glass beaker, stir with a mechanical stirrer until the calcium is completely dissolved. The mixture was then stirred at 37°C for 10 min. for 20 min. The mixture was then cooled to room temperature and maintained under stirring. Based on a copolymer of methacrylic acid and a polyoxyethylene ester of methacrylic acid 75 g of a 37% aqueous solution of the polymer dispersant was added. Weight average molecular weight Mw = 80,000 Daltons, measured by LA-2000; The ratio of acid groups to alkyl groups, A / E, is 7, and the polyoxyethylene chain length is 5,000 daltons. The 560 g Portland cement type with the properties reported in Table 1 was used. The hydration reaction was stirred for 30 seconds at a temperature of 60°C. The reaction was continued for 8 hours with stirring. Throughout the reaction, the product was present in the form of a fluid suspension, and the ash was The color tended to become paler over time. At the end of the reaction, the product was cooled. Approximately 2400 g of a fluid aqueous dispersion was obtained and stirred at 105° C. for 1 hour. The dry matter content measured to constant weight was 33% and the viscosity measured at 20°C was 400 cP. As can be seen, the presence of dispersed polymer was observed even though the polymer was synthesized under the same conditions. The viscosity of the final product was significantly lower, as can be seen by comparison with the product of Example 11, which does not contain any polymer. It decreased by .
[0084] Comparative Example 5 Methacrylic acid and methacrylic acid, commonly used as superplasticizers for cementitious mixtures A 37% aqueous solution of a polymeric dispersant based on a copolymer of 1 and polyoxyethylene ester 50 g of the polymer was added to 1607 g of water. The polymer was analyzed by gel permeation chromatography. The weight average molecular weight Mw of 80,000 Daltons measured by ester group Characterized by a ratio of acid groups to ethylene of A / E=7 and a polyoxyethylene chain length of 5,000 daltons. 560 g Portland cement type 52 having the properties reported in Table 1. 0.5R was added to the resulting clear solution in 30 seconds at a temperature of 60°C. The hydration reaction was stirred. The reaction was continued for 8 hours. Throughout the reaction, the product was present in the form of a fluid suspension, the grey color of which was It tended to become paler over time. At the end of the reaction, the product was cooled and Approximately 2300 g of a fluid aqueous dispersion was obtained, the dry matter content of which was It was measured to a constant weight of 32% at 105°C and had a viscosity of 400 cP at 20°C.
[0085] Example 15 The products of Example 14 and Comparative Example 5 were mixed in the same 52.5R Portland oil having the properties of Table 1. The plastic mortar test was carried out using cement. A reference mix was prepared based solely on the superplasticizing admixture Dynamon SP1 (Mapei). All mixtures were made with a water / cement ratio of 0.42. In various cases, the water introduced with the mixture was measured as the mixed water. After the spread measurement, Prismatic specimens with dimensions of 4 cm x 16 cm x 4 cm were prepared in mortar and standard Cured under laboratory conditions (20°C and 95% R / H). Curing times were 6, 8, 10 and 24 hours. After curing, the compressive strength was measured and the results are shown in Table 14 below.
[0086] [Table 14]
[0087] The results shown in Table 14 show that the accelerating effect of the admixture according to the present invention is due to the polyether carboxylate This shows that the addition of a base dispersant does not substantially affect the mixing ratio of the mixture of Example 15. Mix 34, which contains the antibacterial agent, showed a significant stimulatory effect compared to the reference (Mix 36). Conversely, the mix containing the product of Comparative Example 5 based only on superplasticizer (Mix 35) The dispersion polymer alone does not exert any acceleration effect, but in fact, compared to the reference mix It has been demonstrated that it causes an initial delay in hydration.
[0088] Example 16 Samples of Example 14 and Comparative Example 5 were analyzed using a PANalytical X' equipped with an X'Celerator detector. The samples were analyzed by XRPD technique using a Pert Pro MPD diffractometer. and Co-K produced by Co anode with a current of 40 mA α1.2 Irradiation powder The diffraction spectrum is shown in FIG. 3 and corresponds to Example 14. The spectrum of the corresponding sample is represented by a black line at the top, and the spectrum related to Comparative Example 5 is represented by a black line at the bottom. As can be seen, the results are shown in gray lines in the experiments synthesized in the presence of calcium formate. The spectrum corresponding to the product of Example 14 shows some defects not present in the spectrum of the sample of Comparative Example 5. The cations in the cations of calcium formate are shown in Fig. 1. No calcium was added during the synthesis. However, the peak was due to crystalline calcium formate. Not corresponding to the peak, but 380-390 (angstroms) 3 Or 790(Angst ROHM) 3 Consistently indexed in tetragonal or orthorhombic cells with a volume of 0.01, Ca The cations coordinate with the formic acid binder to produce three-dimensional crystal structures typical of MOFs (metal-organic frameworks). The various polymorphic structures of the product according to the invention compared to that synthesized in pure water are shown. The high porosity of these structures is confirmed by a significant increase in the specific surface area of The BET data (see Table 5) show the improved stimulatory and safety effects of the products according to the invention. This is thought to be the fundamental reason for the qualitative difference.
Claims
1. A method for preparing an accelerating admixture for hydraulic compositions based on C-S-H seeds, comprising hydrating in an aqueous suspension of Portland cement based hydraulic binder or other hydraulic binders mainly based on silicates in the presence of a carboxylic acid, its calcium salt, polyethanolamine, or mixtures thereof, at a water / binder ratio (W / B) ranging from 1 to 6, at a temperature ranging from 20°C to 90°C, for 2 hours to 300 hours, without a grinding step, said hydration comprising adding said hydraulic binder to said carboxylic acid, its calcium salt, polyethanolamine, or mixtures thereof.
2. 2. The method for preparing the accelerating admixture according to claim 1, wherein the carboxylic acid is formic acid or acetic acid or a calcium salt thereof.
3. 3. The method for preparing the accelerating admixture according to claim 1 or 2, wherein the hydration is carried out in the presence of calcium formate.
4. 2. The method of preparing the accelerating admixture of claim 1, wherein the polyethanolamine is selected from monoethanolamine, diethanolamine, triethanolamine, triisopropanolamine and diethanolisopropanolamine.
5. 5. The method for preparing the accelerating admixture according to any one of claims 1 to 4, wherein the carboxylic acid or its calcium salt and polyethanolamine are present in an amount ranging from 2% to 40% by weight of Portland cement or other hydraulic binder mainly based on silicates.
6. The method for preparing the accelerating admixture according to any one of claims 1 to 5, wherein a dispersant, viscosity control agent or stabilizer is added during hydration or at the end of the hydration reaction.
7. 7. The method for preparing the accelerating admixture according to claim 6, wherein the dispersing agent is selected from the group consisting of gluconic acid and its salts, polyether carboxylate based polymers, lignin sulfonates, naphthalene sulfonates and melamine sulfonates condensates with formaldehyde, and derivatives of polysaccharides and phosphonated polymers.
8. 7. The method for preparing the accelerating admixture according to claim 6, wherein the viscosity control agent is a polysaccharide derivative selected from methyl cellulose, hydroxyethyl cellulose (HEC), hydroxypropyl cellulose (HPC), methyl hydroxyethyl cellulose (MHEC), methyl hydroxypropyl cellulose (MHPC), and / or a (co)polymer containing structural units derived from non-ionic monomers of (meth)acrylamide and sulfonated monomers, or a modified polyurea, with an average molecular weight of more than 500,000 g / mol.
9. 7. The method for preparing the accelerating admixture according to claim 6, wherein the stabilizing agent is oxalic acid or a hydroxycarboxylic acid selected from citric acid and malic acid, or a salt thereof.
10. A method for preparing an accelerating admixture for hydraulic compositions based on C-S-H seeds, which comprises the hydration in an aqueous suspension of a Portland cement based hydraulic binder or other hydraulic binders, mainly based on silicates, in the presence of a carboxylic acid, its calcium salt, polyethanolamine or mixtures thereof, without a grinding step, said hydration comprising adding said hydraulic binder to said carboxylic acid, its calcium salt, polyethanolamine or mixtures thereof, and the hydration reaction is carried out at a temperature ranging from 20°C to 90°C.
11. The method of claim 10, wherein the hydration reaction is carried out in a stirred tank or reactor at a temperature in the range of 20°C to 80°C and atmospheric pressure.
12. 12. The method according to claim 11, wherein the stirring is continuous or discontinuous, with an anchor or rotor agitator, optionally in combination with an ultradispersion system.
13. A method according to any one of claims 10 to 12, wherein sodium carbonate is added to the suspension obtained from hydration in an amount ranging from 3% to 40% of the dry weight of the suspension.
14. Use of the accelerating admixture prepared by the preparation method according to any one of claims 1 to 9 for the preparation of a composition based on a hydraulic binder based on Portland cement and an auxiliary cementitious material selected from ground granulated blast furnace slag, fly ash, calcined clay or mixtures thereof.
Citation Information
Patent Citations
Mixed cementitious material for GRC manufacture
JP1983181752A
Mixing material for accelerating aggregation of hydraulic cement combined with amino acid derivative
JP1994040756A
Coagulation and hardening accelerator for silica-based hydraulic binders
JP1997500605A
Cement hardening promoter and method for promoting cement hardening
JP2001158650A
Cement composition, grouting material using the same and use thereof
JP2008169055A