Seamless steel pipes used as materials for bearing parts
A seamless steel pipe with a specific chemical composition and microstructure enhances dimensional accuracy by controlling residual stress and spherical cementite distribution, addressing the need for precision bearings in machinery.
Patent Information
- Application Number
- JP2020145787
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-31
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2040-08-31
AI Technical Summary
Existing seamless steel pipes do not meet the high dimensional accuracy requirements for precision bearings, particularly in precision machinery, despite advancements in technologies like those described in International Publication No. 2005/075121.
A seamless steel pipe with a specific chemical composition (C: 0.60~1.40%, Si: 0.05~0.50%, Mn: 0.10~1.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.01~0.05%, N: 0.020% or less, and Cr: 0.50~2.00%) and microstructure consisting of ferrite and spherical cementite, with a number ratio of spherical cementites with an equivalent circle diameter of 0.50 to 1.50 μm being 50.0% or more, and residual stress less than 30 MPa, to enhance dimensional accuracy.
The proposed seamless steel pipe significantly improves the dimensional accuracy of bearing components by minimizing shape deformation during manufacturing processes, ensuring high precision in bearing parts.
Smart Images

Figure 0007560721000003 
Figure 0007560721000004 
Figure 0007560721000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a steel pipe, and more specifically, to a seamless steel pipe that is used as a material for bearing parts. [Background technology]
[0002] Among bearings typified by deep groove ball bearings, tapered roller bearings, thrust ball bearings, etc., bearing components such as raceways (inner and outer races) and raceways are manufactured from seamless steel pipes. An example of the manufacturing process for manufacturing bearing components from seamless steel pipes is as follows. First, the seamless steel pipe is cut to a predetermined length. The cut seamless steel pipe is turned to manufacture an intermediate product (cylindrical or annular steel material) of a predetermined shape. The intermediate product is hardened and tempered. The intermediate product after hardening and tempering is polished. Through the above steps, bearing components such as raceways and raceways are manufactured. These bearing components are combined with balls, rollers, cages, etc. to manufacture bearings.
[0003] Bearing parts such as raceways and bearing disks require high dimensional accuracy. If the dimensional accuracy of these bearing parts is high, the rotation runout accuracy of the bearings will also be significantly improved, and they can be used as precision bearings in precision machinery, etc. Therefore, there is a demand for seamless steel pipes that can improve the dimensional accuracy of bearing parts when they are manufactured into bearing parts.
[0004] International Publication No. 2005 / 075121 (Patent Document 1) proposes a seamless steel pipe that can improve the dimensional accuracy of bearing parts when manufactured into them. The seamless steel pipe disclosed in Patent Document 1 has a residual stress of 30 MPa or more and a residual stress variation of 30 MPa or less. The seamless steel pipe disclosed in Patent Document 1 further has an average grain size of spheroidized carbides of 0.35 to 0.70 μm. Patent Document 1 states that when bearing parts are manufactured using a seamless steel pipe having the above configuration as a material, the dimensional accuracy of the bearing parts is improved. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2005 / 075121 Summary of the Invention [Problem to be solved by the invention]
[0006] As described above, the seamless steel pipe disclosed in Patent Document 1 can suppress shape changes during the manufacturing process of bearing parts and can improve the dimensional accuracy of the bearing parts. However, recently, there has been a demand for further improvement in dimensional accuracy, particularly in bearings used in precision machinery and the like.
[0007] An object of the present disclosure is to provide a seamless steel pipe that, when manufactured into a bearing component, can improve the dimensional accuracy of the bearing component. [Means for solving the problem]
[0008] The seamless steel pipe according to the present disclosure has Chemical composition, in mass%, C: 0.60-1.40%, Si: 0.05 to 0.50%, Mn: 0.10-1.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.01 to 0.05%, N: 0.020% or less, and Cr: 0.50 to 2.00%, The balance is Fe and impurities. The microstructure consists of ferrite and spheroidal cementite, Among the spheroidal cementite, the number ratio of spheroidal cementite having an equivalent circle diameter of more than 0.50 to 1.50 μm is 50.0% or more, The residual stress is less than 30 MPa. Effect of the Invention
[0009] When the seamless steel pipe according to the present disclosure is manufactured into a bearing component, it can improve the dimensional accuracy of the bearing component. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a histogram diagram of the particle size distribution of spheroidal cementite in a seamless steel pipe having the chemical composition of this embodiment. [Diagram 2] FIG. 2 is a histogram diagram of the particle size distribution of spheroidized cementite in a seamless steel pipe having a chemical composition of this embodiment, which is different from that in FIG. [Diagram 3] FIG. 3 is a schematic diagram for explaining a method for measuring the residual stress of a seamless steel pipe by the Crampton method. [Figure 4] FIG. 4 is a schematic diagram illustrating the method for measuring the residual stress of a seamless steel pipe by the Crampton method, following FIG. [Diagram 5] FIG. 5 is a schematic diagram for explaining the manufacturing process of the seamless steel pipes of each test number in the examples. [Figure 6] FIG. 6 is a diagram showing a measuring device for the radial runout Kia of the inner ring of a bearing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the seamless steel pipe of this embodiment will be described in detail with reference to the drawings.
[0012] The present inventors have studied seamless steel pipes capable of improving the dimensional accuracy of bearing parts when manufactured into bearing parts. First, the present inventors have studied the chemical composition of seamless steel pipes suitable for bearing parts. As a result, they have considered that a seamless steel pipe as a material for bearing parts has a chemical composition containing, in mass%, C: 0.60 to 1.40%, Si: 0.05 to 0.50%, Mn: 0.10 to 1.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.01 to 0.05%, N: 0.020% or less, and Cr: 0.50 to 2.00%, with the balance being Fe and impurities.
[0013] Next, the inventors of the present invention have studied means for improving the dimensional accuracy of bearing parts when the seamless steel pipe having the above-mentioned chemical composition is manufactured into bearing parts. In the case of a steel material having a high C content and Cr content such as the above-mentioned chemical composition, the bearing parts are manufactured by the following manufacturing process. First, the seamless steel pipe is cut to a predetermined length. The cut seamless steel pipe is subjected to a turning process to manufacture an intermediate product having a predetermined shape. The intermediate product is quenched and tempered. The intermediate product after quenching and tempering is polished as necessary. Through the above manufacturing process, bearing parts such as raceways and races are manufactured using the seamless steel pipe as a material.
[0014] In the above-mentioned manufacturing process, the shape is easily deformed, particularly during turning and quenching. Therefore, the inventors have focused on the shape deformation during turning and quenching in seamless steel pipes having the above-mentioned chemical composition, and have studied means for suppressing the shape deformation during these manufacturing processes.
[0015] The present inventors have studied shape deformation during turning. As a result, it has been found that the residual stress of the seamless steel pipe mainly affects shape deformation during turning. Specifically, when the residual stress of the seamless steel pipe is large, shape deformation is likely to occur during turning. Therefore, the present inventors have studied the residual stress capable of suppressing shape deformation during turning in a seamless steel pipe having the above-mentioned chemical composition. As a result, it has been found that in the case of a seamless steel pipe having the above-mentioned chemical composition, if the residual stress is less than 30 MPa, shape deformation due to the turning process is sufficiently suppressed.
[0016] Next, the inventors of the present invention investigated the shape deformation during quenching. The inventors of the present invention considered that the average particle size of the spheroidal cementite mainly affects the shape deformation during quenching. Therefore, the inventors of the present invention focused on the average particle size of the spheroidal cementite and worked on suppressing the shape deformation during quenching. However, it was difficult to significantly improve the dimensional accuracy by only adjusting the average particle size of the spheroidal cementite.
[0017] Therefore, the inventors of the present invention have considered that the particle size distribution of the spheroidal cementite in the steel material has an effect on the shape deformation during quenching, rather than on the average particle size of the spheroidal cementite. Therefore, the inventors of the present invention have investigated and examined the relationship between the particle size distribution of the spheroidal cementite and the dimensional accuracy of the bearing parts.
[0018] First, the inventors of the present invention considered that the higher the percentage of spheroidal cementite particles with a small equivalent circle diameter, the easier it is for the spheroidal cementite particles to be solid-dissolved during quenching, and as a result, the easier it is to quench uniformly. For example, as shown in FIG. 1, in a seamless steel pipe having the above-mentioned chemical composition, the higher the percentage of spheroidal cementite particles with an equivalent circle diameter of 0.50 μm or less than the percentage of spheroidal cementite particles with an equivalent circle diameter of more than 0.50 μm, the easier it is to quench uniformly, and as a result, the dimensional accuracy of the bearing parts is improved. However, when the percentage of spheroidal cementite particles with a small particle diameter as shown in FIG. 1 is high, the dimensional accuracy of the bearing parts is low.
[0019] Therefore, the inventors of the present invention thought that a higher proportion of spherical cementite particles having a certain equivalent circle diameter would enable uniform quenching and, as a result, the dimensional accuracy of the bearing parts could be suppressed. As shown in Fig. 2, the proportion of spherical cementite particles having an equivalent circle diameter of more than 0.50 to 1.50 μm was increased in a seamless steel pipe having the above-mentioned chemical composition, and the dimensional accuracy of the bearing parts was investigated. As a result, it was found that the dimensional accuracy of the bearing parts was significantly improved.
[0020] Based on the above findings, the present inventors further investigated and examined the relationship between the particle size distribution of spheroidal cementite in a seamless steel pipe having the above-mentioned chemical composition and the dimensional accuracy of bearing parts. As a result, it was found that by setting the number ratio of spheroidal cementite having a circle equivalent diameter of more than 0.50 to 1.50 μm to 50.0% or more in a seamless steel pipe having the above-mentioned chemical composition, more uniform quenching can be achieved in the manufacturing process of bearing parts, and as a result, the dimensional accuracy of bearing parts can be significantly improved.
[0021] The seamless steel pipe of this embodiment has been completed based on the above technical concept. The seamless steel pipe of this embodiment has the following configuration.
[0022] [1] Chemical composition, in mass%, C: 0.60-1.40%, Si: 0.05 to 0.50%, Mn: 0.10-1.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.01 to 0.05%, N: 0.020% or less, and Cr: 0.50 to 2.00%, The balance is Fe and impurities. The microstructure consists of ferrite and spheroidal cementite, Among the spheroidal cementite, the number ratio of spheroidal cementite having an equivalent circle diameter of more than 0.50 to 1.50 μm is 50.0% or more, The residual stress is less than 30 MPa. Seamless steel pipe.
[0023] [2] A seamless steel pipe according to [1], The number ratio of the spherical cementite having a circle equivalent diameter of more than 0.50 to 1.50 μm is 52.0% or more. Seamless steel pipe.
[0024] The seamless steel pipe of this embodiment will be described in detail below.
[0025] [Seamless steel tubes as materials for bearing parts] The seamless steel pipe of this embodiment is suitable as a material for bearing parts. The bearing parts manufactured using the seamless steel pipe of this embodiment refer to rolling bearing parts. The bearing parts are, for example, races and races. The races may be inner or outer rings, and the races may be shaft races, housing races, central races, or aligning housing races. There are no particular limitations on the races and races as long as they are members having raceway surfaces.
[0026] The seamless steel pipe of this embodiment is used as a material for the above-mentioned bearing parts. Details of the seamless steel pipe of this embodiment are described below.
[0027] [Chemical composition of the seamless steel pipe of this embodiment] The chemical composition of the seamless steel pipe of this embodiment contains the following elements. Hereinafter, "%" regarding the element content means mass % unless otherwise specified.
[0028] C: 0.60-1.40% Carbon (C) improves the hardenability of steel and increases the strength of bearing parts. If the C content is less than 0.60%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the C content exceeds 1.40%, the melting start temperature of the steel is excessively reduced even if the contents of other elements are within the range of this embodiment. In this case, cracks and scratches are likely to occur in the manufacturing process of the steel (seamless steel pipe). Therefore, the C content is 0.60 to 1.40%. The preferred lower limit of the C content is 0.70%, more preferably 0.80%, and more preferably 0.90%. The preferred upper limit of the C content is 1.35%, more preferably 1.30%, and more preferably 1.25%.
[0029] Silicon: 0.05 to 0.50% Silicon (Si) improves the hardenability of steel. Si also improves the temper softening resistance of steel in the process of manufacturing bearing parts using steel as a raw material. Si also improves the fatigue strength of the bearing parts. If the Si content is less than 0.05%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Si content exceeds 0.50%, the fatigue strength of the bearing parts is saturated even if the contents of other elements are within the range of this embodiment. If the Si content exceeds 0.50%, the machinability of the steel material is further reduced. Therefore, the Si content is 0.05 to 0.50%. The preferred lower limit of the Si content is 0.10%, more preferably 0.15%, and even more preferably 0.18%. The preferred upper limit of the Si content is 0.48%, more preferably 0.45%, more preferably 0.40%, and even more preferably 0.38%.
[0030] Mn: 0.10-1.00% Manganese (Mn) improves the hardenability of steel material. This increases the strength of the bearing part. If the Mn content is less than 0.10%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Mn content exceeds 1.00%, the hardness of the steel material (seamless steel pipe) that is the material of the bearing part becomes too high even if the contents of other elements are within the range of this embodiment. In this case, the machinability of the steel material decreases. Therefore, the Mn content is 0.10 to 1.00%. The preferable lower limit of the Mn content is 0.15%, and more preferably 0.20%. The preferable upper limit of the Mn content is 0.90%, more preferably 0.80%, more preferably 0.70%, and more preferably 0.60%.
[0031] P:0.050% or less Phosphorus (P) is an impurity that is inevitably contained. That is, the P content is more than 0%. P segregates at grain boundaries and reduces grain boundary strength. If the P content exceeds 0.050%, even if the contents of other elements are within the range of this embodiment, P will excessively segregate at grain boundaries and reduce grain boundary strength. In this case, cracks and defects are likely to occur during hot working in the manufacturing process of the steel material (seamless steel pipe). Therefore, the P content is 0.050% or less. A preferable upper limit of the P content is 0.040%, more preferably 0.030%. The P content is preferably as low as possible. However, excessive reduction of the P content increases manufacturing costs. Therefore, in consideration of normal industrial production, a preferable lower limit of the P content is 0.001%, more preferably 0.002%.
[0032] S: 0.050% or less Sulfur (S) is an impurity that is inevitably contained. That is, the S content is more than 0%. S generates sulfide-based inclusions. Coarse sulfide-based inclusions are likely to become the starting point of cracks and defects during hot working in the manufacturing process of steel materials (seamless steel pipes). If the S content exceeds 0.050%, even if the contents of other elements are within the range of this embodiment, the sulfide-based inclusions become coarse, and cracks and defects are likely to occur during hot working in the manufacturing process of steel materials (seamless steel pipes). Therefore, the S content is 0.050% or less. The preferred upper limit of the S content is 0.040%, more preferably 0.030%. The S content is preferably as low as possible. However, excessive reduction of the S content increases the manufacturing cost. Therefore, in consideration of normal industrial production, the preferred lower limit of the S content is 0.001%, more preferably 0.002%.
[0033] Al: 0.01 to 0.05% Aluminum (Al) deoxidizes steel. If the Al content is less than 0.01%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Al content exceeds 0.05%, clustered coarse oxides are generated even if the contents of other elements are within the range of this embodiment. The clustered coarse oxides reduce the fatigue strength of the bearing part. Therefore, the Al content is 0.01 to 0.05%. The preferable lower limit of the Al content is 0.02%. The preferable upper limit of the Al content is 0.04%, and more preferably 0.03%. The Al content in this specification means the content of total Al.
[0034] N: 0.020% or less Nitrogen (N) is an unavoidably contained impurity. In other words, the N content is more than 0%. N dissolves in steel and reduces the hot workability of the steel. If the N content exceeds 0.020%, the hot workability of the steel decreases. Therefore, the N content is 0.020% or less. The preferred upper limit of the N content is 0.015%, and more preferably 0.010%. The N content is preferably as low as possible. However, excessive reduction of the N content increases the manufacturing cost. Therefore, in consideration of normal industrial production, the preferred lower limit of the N content is 0.001%, and more preferably 0.002%.
[0035] Cr: 0.50~2.00% Chromium (Cr) improves the hardenability of steel material. This increases the strength of the bearing part. If the Cr content is less than 0.50%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Cr content exceeds 2.00%, coarse Cr carbides are generated even if the contents of other elements are within the range of this embodiment. In this case, the fatigue strength of the bearing part decreases. Therefore, the Cr content is 0.50 to 2.00%. The preferred lower limit of the Cr content is 0.70%, more preferably 0.90%, and more preferably 1.00%. The preferred upper limit of the Cr content is 1.80%, more preferably 1.70%, and more preferably 1.65%.
[0036] The balance of the chemical composition of the seamless steel pipe according to the present embodiment is composed of Fe and impurities. Here, the impurities refer to substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of seamless steel pipes, and are permissible within a range that does not adversely affect the seamless steel pipe of the present embodiment.
[0037] [On the microstructure of seamless steel pipes] The microstructure of the seamless steel pipe of this embodiment is composed of ferrite and spheroidal cementite. In the microstructure of the seamless steel pipe, the regions other than ferrite and spheroidal cementite are, for example, precipitates and inclusions other than spheroidal cementite. The precipitates and inclusions other than spheroidal cementite are negligibly small compared to ferrite and spheroidal cementite.
[0038] [Method of identifying phases in microstructure] The microstructure of the seamless steel pipe of this embodiment can be observed by the following method. A sample is taken from the center position of the wall thickness of the seamless steel pipe. Of the surfaces of the taken sample, a cross section (surface) in a direction perpendicular to the longitudinal direction of the seamless steel pipe is used as the observation surface. The observation surface is mirror-polished and then etched using picric acid (picral etchant). The etched observation surface is observed using an optical microscope at 500x magnification to generate a photographic image of any one field of view. The size of the field of view is 100 μm×100 μm. In the field of view, each phase, such as ferrite, spheroidal cementite, and bainite, has a different contrast for each phase. Therefore, each phase can be identified based on the contrast.
[0039] As described above, the microstructure of the seamless steel pipe of this embodiment is composed of ferrite and spheroidal cementite.
[0040] [Regarding the specific spheroidal cementite number ratio Ra] Furthermore, in the seamless steel pipe of this embodiment, the percentage by number of spheroidal cementite having an equivalent circle diameter of more than 0.50 to 1.50 μm (specific spheroidal cementite number percentage Ra) is 50.0% or more.
[0041] As described above, in the seamless steel pipe of this embodiment, the specific spheroidal cementite number ratio Ra of the spheroidal cementite in the steel material is set to 50.0% or more. If the specific spheroidal cementite number ratio Ra is less than 50.0%, the number ratio of fine spheroidal cementite having a circle equivalent diameter of 0.50 μm or less is too high. In this case, the steel material is difficult to be quenched uniformly in the quenching process in the process of manufacturing bearing parts using the seamless steel pipe as a raw material, and the martensitic transformation start time of the steel material varies depending on the location. As a result, the steel material after quenching is deformed due to thermal strain.
[0042] When the specific spheroidal cementite number ratio Ra is 50.0% or more, there is a sufficiently large amount of spheroidal cementite having a circle equivalent diameter of more than 0.50 to 1.50 μm, and there is a sufficiently small amount of fine spheroidal cementite having a circle equivalent diameter of 0.50 μm or less. In this case, the solid solution timing of the spheroidal cementite is unlikely to vary in the quenching process in the process of manufacturing bearing parts using the seamless steel pipe as a raw material. Therefore, the steel material is easily quenched uniformly, and the martensitic transformation start timing of the steel material is unlikely to vary depending on the location. As a result, deformation due to thermal strain is suppressed in the steel material after quenching.
[0043] The preferred lower limit of the specific spheroidal cementite number ratio Ra is 52.0%, more preferably 53.0%, and even more preferably 54.0%. The upper limit of the specific spheroidal cementite number ratio Ra is not particularly limited, but is naturally 100.0% or less, and in normal production, the upper limit of the specific spheroidal cementite number ratio Ra is, for example, 95.0%.
[0044] [Method for measuring the specific spheroidal cementite number ratio Ra] The number proportion Ra of specific spheroidal cementite can be obtained by the following method. Spheroidal cementite is identified in the visual field (100 μm × 100 μm) observed in the above-mentioned microstructure observation. Spheroidal cementite can be identified by contrast. The circle-equivalent diameter of each identified spheroidal cementite is obtained. The circle-equivalent diameter can be obtained by well-known image processing. Based on the circle-equivalent diameter of each spheroidal cementite, the number N of spheroidal cementite having a circle-equivalent diameter of more than 0.50 to 1.50 μm is calculated. sp The total number of spheroidal cementite particles in the field of view, N total and the number N of spheroidal cementite with a circle equivalent diameter of more than 0.50 to 1.50 μm sp Based on this, the specific spheroidal cementite number ratio Ra (%) is calculated by the following formula. Specific spheroidal cementite number ratio Ra=N sp / N total ×100 In addition, it is extremely difficult to identify spheroidal cementite having an equivalent circle diameter of less than 0.05 μm in the field of view, and therefore, in this specification, the spheroidal cementite to be counted is spheroidal cementite having an equivalent circle diameter of 0.05 μm or more.
[0045] The upper limit of the equivalent circle diameter of the spheroidal cementite is not particularly limited. However, in a seamless steel pipe having the above-mentioned chemical composition, the equivalent circle diameter of the spheroidal cementite is unlikely to exceed 2.00 μm. Therefore, the upper limit of the equivalent circle diameter of the spheroidal cementite is, for example, 2.00 μm.
[0046] [Residual stress in seamless steel pipes] Furthermore, the seamless steel pipe of this embodiment has a residual stress of less than 30.0 MPa. If the residual stress is 30.0 MPa or more, distortion occurs during the turning process in the process of manufacturing bearing components using the seamless steel pipe as a material. In this case, the steel material (seamless steel pipe) is deformed due to distortion during the manufacturing process of the bearing components. This reduces the dimensional accuracy. On the other hand, if the residual stress is less than 30 MPa, the residual stress in the seamless steel pipe is kept sufficiently low. In this case, it is possible to suppress the occurrence of distortion during the turning process in the manufacturing process of the bearing components. As a result, it is possible to suppress the deformation of the steel material during the manufacturing process of the bearing components, and to improve the dimensional accuracy.
[0047] In this specification, the residual stress of a seamless steel pipe means the residual stress (MPa) measured by the Crampton method. Hereinafter, a method for measuring the residual stress by the Crampton method will be described.
[0048] [Method of measuring residual stress] The residual stress of a seamless steel pipe can be obtained by the Crampton method. Specifically, three cylindrical test pieces 1 with length L = 10 mm, outer diameter D0 mm, and wall thickness t mm are taken from any position of the seamless steel pipe, as shown in Figure 3. The cylindrical test pieces 1 are taken from positions 500 mm or more away from both ends of the seamless steel pipe. The outer diameter D0 and wall thickness t of each cylindrical test piece 1 are measured.
[0049] As shown in Fig. 4, the cylindrical test piece 1 is cut in the axial direction to form a slit 2. At this time, the outer diameter D0 of the cylindrical test piece 1 expands slightly to an outer diameter D1 due to the formation of the slit 2. Then, the outer diameter D1 (mm) is measured.
[0050] Based on the measured outer diameters D0 and D1 and wall thickness t, the residual stress F is calculated using formula (1). F = E × (1 / D0-1 / D1) × t / (1-ν 2 ) (1) Here, E in formula (1) is Young's modulus (MPa) of the steel constituting the seamless steel pipe, and ν is Poisson's ratio. Young's modulus and Poisson's ratio are values specific to the chemical composition of the seamless steel pipe, and it is well known to those skilled in the art that Young's modulus and Poisson's ratio can be specified once the chemical composition of the seamless steel pipe is determined.
[0051] The residual stress F is determined for each of the three cylindrical test pieces 1. The arithmetic mean value of the three residual stresses F is then defined as the residual stress (MPa) of the seamless steel pipe.
[0052] The upper limit of the residual stress is preferably 28.0 MPa, more preferably 25.0 MPa, and even more preferably 23.0 MPa.
[0053] As described above, the seamless steel pipe of this embodiment has a chemical composition in which the content of each element falls within the range of this embodiment, the microstructure is composed of ferrite and spheroidal cementite, the specific spheroidal cementite number ratio Ra is 50.0% or more, and the residual stress is less than 30 MPa. Therefore, when bearing parts are manufactured using the seamless steel pipe of this embodiment, deformation due to distortion is unlikely to occur during turning and quenching in the manufacturing process. As a result, bearing parts with excellent dimensional accuracy can be manufactured.
[0054] [Manufacturing method of seamless steel pipes] An example of a method for manufacturing a seamless steel pipe of this embodiment will be described. The method for manufacturing a seamless steel pipe described below is an example for manufacturing a seamless steel pipe of this embodiment. Therefore, a seamless steel pipe having the above-mentioned configuration may be manufactured by a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of a method for manufacturing a seamless steel pipe of this embodiment.
[0055] An example of a method for manufacturing a seamless steel pipe of this embodiment includes a process for manufacturing a blank pipe (pipe making process), a process for performing a first spheroidizing annealing (first spheroidizing annealing process), a process for performing a first cold drawing (first cold drawing process), a process for performing a second spheroidizing annealing (second spheroidizing annealing process), a process for performing a second cold drawing (second cold drawing process), a process for performing softening annealing (softening annealing process), a process for straightening bends (straightening process), and a process for performing stress relief annealing (stress relief annealing process). Each process will be described below.
[0056] [Pipe manufacturing process] In the pipe making process, a mother pipe is manufactured by a well-known method using a material having the above-mentioned chemical composition. The material may be, for example, a cast material or a round billet (steel material). The material is hot worked to manufacture a mother pipe. For example, piercing and rolling by the Mannesmann method is performed as the hot working. Specifically, the material is heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1100 to 1300°C. Piercing and rolling is performed on the material removed from the heating furnace to manufacture a mother pipe. Elongation rolling is performed on the billet after piercing and rolling using a mandrel mill. Furthermore, as necessary, sizing rolling is performed on the billet after elongation rolling using a reducer or a sizing mill. Through the above steps, a mother pipe is manufactured.
[0057] In the above description, the pipe-making process using the Mannesmann process has been described as an example of the pipe-making process. However, the pipe-making process may be performed using a pipe-making process other than the Mannesmann process. For example, the pipe-making process may be performed using the Eugène-Sejournet process or the Erhardt push bench process (i.e., hot extrusion).
[0058] [First spheroidizing annealing process] In the first spheroidizing annealing process, spheroidizing annealing is performed on the mother pipe produced in the pipe making process. The spheroidizing annealing is performed using a heat treatment furnace with the following heat pattern. First, the mother pipe is charged into the heat treatment furnace, and then the furnace temperature is increased to A. c1The steel sheet is heated to an annealing temperature higher than the transformation point. The annealing temperature is preferably set to 750 to 800°C. After holding the steel sheet at the annealing temperature for a predetermined time, A r1 The material is slowly cooled until it reaches a temperature below the transformation point. This heat pattern is repeated at least twice. This promotes the spheroidization of cementite in the raw tube.
[0059] [First cold drawing process] In the first cold drawing step, cold drawing is performed on the mother pipe after the first spheroidizing annealing step. In the first cold drawing step, strain is imparted to the mother pipe having a microstructure containing spheroidal cementite. In this case, strain accumulates around the spheroidal cementite. Therefore, in the next step, the second spheroidizing annealing step, the strain around the spheroidal cementite becomes the driving force for the growth (coarsening) of the spheroidal cementite.
[0060] The preferred area reduction rate in the first cold drawing step is 20% or more. If the area reduction rate in the first cold drawing step is 20% or more, sufficient strain can be imparted to the spheroidized cementite in the subsequent second spheroidizing annealing step. The upper limit of the area reduction rate is not particularly limited, but is, for example, 45%, taking into account the equipment capacity.
[0061] [Second spheroidizing annealing process] In the second spheroidizing annealing step, the mother pipe after the first cold drawing step is subjected to a second spheroidizing annealing. As described above, strain is accumulated around the spheroidized cementite in the mother pipe after the first cold drawing step. By subjecting the mother pipe in a state in which strain is accumulated around the spheroidized cementite to another spheroidizing annealing step, the existing spheroidized cementite grows (coarsens) using the surrounding strain as a driving force. As a result, the proportion of spheroidized cementite having a circle equivalent diameter of more than 0.50 to 1.50 μm in the seamless steel pipe can be made 50.0% or more.
[0062] The heat pattern in the second spheroidizing annealing step may be the same as that in the first spheroidizing annealing step. Specifically, after the blank pipe is charged into the heat treatment furnace, the furnace temperature is increased to A c1The steel sheet is heated to an annealing temperature higher than the transformation point. The annealing temperature is preferably set to 750 to 800°C. After holding the steel sheet at the annealing temperature for a predetermined time, A r1 The tube is slowly cooled until it reaches a temperature below the transformation point. This heat pattern is repeated at least twice. As a result, the spheroidized cementite grows and coarsens in the tube.
[0063] [Second cold drawing process] In the second cold drawing process, cold drawing is performed on the mother tube after the second spheroidizing annealing process. The mother tube after the second spheroidizing annealing process is curved due to heat treatment. Therefore, the second cold drawing process is performed to increase the straightness of the mother tube. Furthermore, the cold drawing process is performed twice to increase the cumulative area reduction rate of the cold drawing. This improves the dimensional accuracy of the seamless steel tube. As a result, the dimensional accuracy of bearing parts manufactured using the seamless steel tube as a material is also improved.
[0064] The preferred area reduction rate in the second cold drawing step is 20% or more, and the preferred cumulative area reduction rate in the first cold drawing step and the second cold drawing step is 40% or more. In this case, even if two spheroidizing annealing steps are performed, a seamless steel pipe with high straightness and dimensional accuracy can be obtained.
[0065] [Softening annealing process] In the softening annealing step, the mother pipe after the second cold drawing step is subjected to a well-known softening annealing. The softening annealing removes the strain introduced into the mother pipe by the second cold drawing step. The preferred annealing temperature for the softening annealing is A c1 Transformation point -5~A c1 The transformation point is −90° C. The preferred holding time at the annealing temperature is 5 to 60 minutes.
[0066] [Correcting process] In the straightening process, the mother pipe after the soft annealing process is straightened to increase the straightness of the mother pipe. The straightening may be performed using a two-roll straightener or a multi-roll straightener. The straightening process may be performed by a well-known method.
[0067] [Stress relief annealing process] In the stress relief annealing process, stress relief annealing is performed on the mother pipe after the straightening process. This makes it possible to remove the strain introduced into the mother pipe in the straightening process, and to make the residual stress of the seamless steel pipe less than 30 MPa. The preferred annealing temperature for stress relief annealing is 500 to 600°C, and the preferred holding time at the annealing temperature is 10 to 60 minutes. By appropriately adjusting the annealing temperature and holding time in stress relief annealing, the residual stress of the seamless steel pipe can be adjusted to less than 30 MPa. The more preferred lower limit of the annealing temperature for stress relief annealing is 530°C. The more preferred upper limit of the annealing temperature for stress relief annealing is 560°C.
[0068] By the above-mentioned manufacturing process, a seamless steel pipe having the above-mentioned configuration can be manufactured.
[0069] [Manufacturing method for bearing parts] An example of a method for manufacturing a bearing component using the seamless steel pipe of this embodiment is as follows. The manufacturing process for the bearing component includes a turning process and a quenching and tempering process. In the turning process, the seamless steel pipe is cut to a predetermined length, and then the cut seamless steel pipe is turned to manufacture an intermediate product of a predetermined shape. In the quenching and tempering process, the intermediate product manufactured in the turning process is quenched. The quenching temperature is A c3 The intermediate product is tempered at a temperature equal to or higher than the transformation point, and a known temperature is sufficient. The intermediate product after quenching is tempered. The tempering temperature is a known temperature. A polishing process may be performed on the intermediate product after the quenching and tempering processes. In the polishing process, the intermediate product after the quenching and tempering processes is ground or polished to form a predetermined product shape. The polishing process does not have to be performed.
[0070] The bearing component is manufactured by the above manufacturing process. In the seamless steel pipe of this embodiment, the chromium structure is composed of ferrite and spheroidal cementite, the specific spheroidal cementite number ratio Ra is 50.0% or more, and the residual stress is less than 30 MPa. Therefore, when a bearing component is manufactured using the seamless steel pipe of this embodiment as a material, shape deformation due to residual stress is unlikely to occur in the above-mentioned turning process. Furthermore, the variation in the occurrence time of martensitic transformation during quenching can be suppressed, and martensitic transformation is likely to occur uniformly. As a result, shape deformation due to quenching is also unlikely to occur. Therefore, when a bearing component is manufactured using the seamless steel pipe of this embodiment as a material, the dimensional accuracy of the bearing component can be improved. EXAMPLES
[0071] The effects of the seamless steel pipe of this embodiment will be described in more detail below with reference to examples. The conditions in the following examples are one example of conditions adopted to confirm the feasibility and effects of the seamless steel pipe of this embodiment. Therefore, the seamless steel pipe of this embodiment is not limited to this one example of conditions.
[0072] A blank tube having the chemical composition shown in Table 1 was prepared.
[0073] [Table 1]
[0074] The mother pipe of each test number was produced by the Mannesmann process by heating a round billet at 1100 to 1300°C. The mother pipe of each test number was subjected to the process shown in Fig. 5. Specifically, for test numbers A to J, seamless steel pipes were produced by subjecting the mother pipe to process 5 shown in Fig. 5.
[0075] In process 5, the first spheroidizing annealing process was carried out on the mother pipe produced in the pipe making process. In the first spheroidizing annealing process, the mother pipe was heated to 770 to 780°C and then slowly cooled. Spheroidizing annealing with this heat pattern was carried out twice in succession. After the first spheroidizing annealing process, the first cold drawing process was carried out. In the first cold drawing process, the mother pipe was cold drawn. The area reduction rate in the first cold drawing process was 26 to 35%. After the first cold drawing process, the second spheroidizing annealing process was carried out. In the second spheroidizing annealing process, spheroidizing annealing with the same heat pattern as the first spheroidizing annealing process was carried out twice in succession. After the second spheroidizing annealing process, the second cold drawing process was carried out. In the second cold drawing process, the mother pipe was cold drawn. The area reduction rate in the second cold drawing process was 21 to 33%. After the second cold drawing process, a softening annealing process was carried out. In the softening annealing process, softening annealing was carried out at an annealing temperature of 720°C, with a holding time at the annealing temperature of 30 minutes. After the softening annealing process, a straightening process was carried out. In the straightening process, bending straightening was carried out on the blank pipe using a multi-roll straightener. After the straightening process, a stress relief annealing process was carried out. In the stress relief annealing process, stress relief annealing was carried out at an annealing temperature of 550°C, with a holding time at the annealing temperature of 30 minutes. Through the above processes, seamless steel pipes of test numbers A to J having the outer diameters and wall thicknesses shown in Table 2 were produced.
[0076] [Table 2]
[0077] In the test number K, a seamless steel pipe was produced by carrying out the process 1 shown in FIG. 5 on the mother pipe. In the process 1, a spheroidizing annealing process was carried out on the mother pipe produced in the pipe making process. In the spheroidizing annealing process, spheroidizing annealing was carried out twice in succession with the same heat pattern as the first spheroidizing annealing process of the process 5. After the spheroidizing annealing, a cold drawing process was carried out. In the cold drawing process, the mother pipe was cold drawn. The reduction in area in the cold drawing process was 24%. After the cold drawing process, a softening annealing process was carried out. In the softening annealing process, softening annealing was carried out at an annealing temperature of 720°C and with a holding time at the annealing temperature of 10 minutes. After the softening annealing process, a straightening process was carried out. In the straightening process, bending straightening was carried out on the mother pipe using a multi-roll straightening machine. Through the above processes, a seamless steel pipe of the test number K having the outer diameter and wall thickness shown in Table 2 was produced.
[0078] In test number L, a seamless steel pipe was produced by carrying out process 2 shown in FIG. 5 on a blank pipe. In process 2, a spheroidizing annealing process was carried out on a blank pipe produced in a pipe-making process. In the spheroidizing annealing process, spheroidizing annealing was carried out twice in succession with the same heat pattern as in the first spheroidizing annealing process of process 5. After the spheroidizing annealing, a first cold drawing process was carried out. In the first cold drawing process, the blank pipe was cold drawn. The area reduction rate in the first cold drawing process was 27%. After the first cold drawing process, a first softening annealing process was carried out. In the first softening annealing process, softening annealing was carried out with an annealing temperature of 720°C and a holding time at the annealing temperature of 5 minutes. After the first softening annealing process, a second cold drawing process was carried out. In the second cold drawing process, the blank pipe was cold drawn. The area reduction rate in the second cold drawing process was 24%. After the second cold drawing process, a second softening annealing process was carried out. In the second softening annealing process, softening annealing was carried out at an annealing temperature of 720°C, with a holding time at the annealing temperature of 10 minutes. After the second softening annealing process, a straightening process was carried out. In the straightening process, bending straightening was carried out on the blank pipe using a multi-roll straightener. Through the above processes, a seamless steel pipe of test number L having the outer diameter and wall thickness shown in Table 2 was produced.
[0079] In test number M, a seamless steel pipe was produced by carrying out process 3 shown in FIG. 5 on a mother pipe. In process 3, a spheroidizing annealing process was carried out on a mother pipe produced in a pipe-making process. In the spheroidizing annealing process, spheroidizing annealing was carried out twice in succession using the same heat pattern as the first spheroidizing annealing process in process 5. After spheroidizing annealing, a first cold drawing process was carried out. In the first cold drawing process, the mother pipe was cold drawn. The area reduction rate in the first cold drawing process was 27%. After the first cold drawing process, a first softening annealing process was carried out. In the first softening annealing process, softening annealing was carried out at an annealing temperature of 720°C and with a holding time at the annealing temperature of 5 minutes. After the first softening annealing process, a second cold drawing process was carried out. In the second cold drawing process, the mother pipe was cold drawn. The area reduction rate in the second cold drawing process was 24%. After the second cold drawing process, a second softening annealing process was carried out. In the second softening annealing process, softening annealing was carried out at an annealing temperature of 720°C and a holding time at the annealing temperature of 10 minutes. After the second softening annealing process, a straightening process was carried out. In the straightening process, bending straightening was carried out on the blank pipe using a multi-roll straightener. After the straightening process, a stress relief annealing process was carried out. In the stress relief annealing process, stress relief annealing was carried out at an annealing temperature of 550°C and a holding time at the annealing temperature of 30 minutes. Through the above processes, a seamless steel pipe of test number M having the outer diameter and wall thickness shown in Table 2 was produced.
[0080] In test number N, a seamless steel pipe was produced by carrying out process 4 shown in FIG. 5 on a blank pipe. In process 4, a first spheroidizing annealing process was carried out on a blank pipe produced in a pipe-making process. In the first spheroidizing annealing process, spheroidizing annealing was carried out twice in succession with the same heat pattern as in the first spheroidizing annealing process of process 5. After spheroidizing annealing, a first cold drawing process was carried out. In the first cold drawing process, the blank pipe was cold drawn. The reduction in area in the first cold drawing process was 27%. After the first cold drawing process, a second spheroidizing annealing process was carried out. In the second spheroidizing annealing process, spheroidizing annealing was carried out twice in succession with the same heat pattern as in the first spheroidizing annealing process. After the second spheroidizing annealing process, a second cold drawing process was carried out. In the second cold drawing process, the blank pipe was cold drawn. The area reduction rate in the second cold drawing process was 24%. After the second cold drawing process, a softening annealing process was carried out. In the softening annealing process, the annealing temperature was set to 720°C, and the holding time at the annealing temperature was 10 minutes. After the softening annealing process, a straightening process was carried out. In the straightening process, bending straightening was carried out on the blank pipe using a multi-roll straightener. Through the above processes, a seamless steel pipe with test number N having the outer diameter and wall thickness shown in Table 2 was produced.
[0081] [Evaluation test] The seamless steel pipes with each test number were subjected to the following evaluation tests.
[0082] [Microstructure observation test] The microstructure of the seamless steel pipe of each test number was identified by the following method. A sample was taken from the center position of the wall thickness of the seamless steel pipe of each test number. Of the surfaces of the taken samples, the cross section (surface) in the direction perpendicular to the longitudinal direction of the seamless steel pipe was used as the observation surface. After the observation surface was mirror-polished, it was etched using picric acid (picral etching solution). The etched observation surface was observed using an optical microscope at 500 times magnification, and a photographic image of one arbitrary field of view was generated. The size of the field of view was 100 μm × 100 μm. In the field of view, each phase, such as ferrite, spheroidal cementite, and bainite, has a different contrast for each phase. Therefore, each phase was identified based on the contrast. As a result of the identification, the microstructure of the seamless steel pipe of each test number was a structure consisting of ferrite and spheroidal cementite.
[0083] [Specific spheroidal cementite number ratio Ra measurement test] The percentage Ra of the number of specific spheroidal cementite in the seamless steel pipe of each test number was measured by the following method. Spheroidal cementite was identified in the visual field (100 μm × 100 μm) observed in the above-mentioned microstructure observation. The circle-equivalent diameter of each identified spheroidal cementite was obtained by well-known image processing. At this time, since it was extremely difficult to identify particles with a circle-equivalent diameter of less than 0.05 μm in the visual field, spheroidal cementite with a circle-equivalent diameter of 0.05 μm or more was identified as spheroidal cementite. Based on the circle-equivalent diameter of the identified spheroidal cementite, the number N of spheroidal cementite with a circle-equivalent diameter of more than 0.50 to 1.50 μm was determined. sp The total number of spheroidal cementite particles in the field of view, N total and the number N of spheroidal cementite with a circle equivalent diameter of more than 0.50 to 1.50 μm sp Based on this, the specific spheroidal cementite number ratio Ra (%) was calculated by the following formula. Specific spheroidal cementite number ratio Ra=N sp / N total ×100 The specific spheroidal cementite number ratios Ra (%) obtained are shown in Table 2.
[0084] [Residual stress measurement test] The residual stress of each seamless steel pipe was determined by the Crampton method. Specifically, three cylindrical test pieces 1 with a length L = 10 mm, an outer diameter D0 mm, and a wall thickness t mm were taken from the center of the length direction of each seamless steel pipe, as shown in Figure 3. The outer diameter D0 and wall thickness t of each cylindrical test piece 1 were measured. After the measurement, the cylindrical test piece 1 was cut in the axial direction to form a slit 2, as shown in Figure 4. At this time, the outer diameter D0 of the cylindrical test piece 1 was slightly expanded to an outer diameter D1 due to the formation of the slit 2. Therefore, the outer diameter D1 was measured. Based on the measured outer diameters D0, D1, and wall thickness t, the residual stress F was determined using formula (1). F = E × (1 / D0-1 / D1) × t / (1-ν 2 ) (1) Here, E in formula (1) is the Young's modulus (MPa) of the steel constituting the seamless steel pipe, and ν is the Poisson's ratio. In this example, based on the chemical composition of each test number in Table 1, Young's modulus E = 206 × 10 3 (MPa), and Poisson's ratio ν = 0.30.
[0085] The residual stress F was determined for each of the three cylindrical test pieces 1. The arithmetic mean value of the three residual stresses F was defined as the residual stress (MPa) of the seamless steel pipe.
[0086] [Dimensional accuracy test] Deep groove ball bearings (open type) were made from the seamless steel pipes of each test number. Inner rings (bearing parts) of rolling bearings were manufactured from the seamless steel pipes of each test number. Specifically, the seamless steel pipes of each test number were turned under the same conditions to produce intermediate products having a predetermined shape. The intermediate products were hardened and tempered. The hardening and tempering conditions were the same for all intermediate products. The intermediate products after hardening and tempering were polished under the same conditions to produce the inner rings (bearing parts).
[0087] A deep groove ball bearing was manufactured using the manufactured inner ring (bearing part). The material of the outer ring, the material of the balls, and the material of the cage of the deep groove ball bearing were the same for each test number. The manufactured deep groove ball bearing was used to determine the radial runout Kia of the inner ring in accordance with JIS B15515-2:2006. As shown in FIG. 6, a weight 20 for measurement load was placed on the bearing 10. A measuring device 30 was placed on the inner diameter surface of the inner ring. The bearing 10 was rotated gently once, and the difference between the maximum and minimum readings of the measuring device 30 was obtained. The obtained difference was defined as the radial runout Kia. The radial runout Kia is greatly affected by the shape error (roundness) of the inner diameter surface of the inner ring. Therefore, the radial runout Kia was used as an index of the dimensional accuracy when a bearing part (inner ring) was manufactured from a seamless steel pipe. Using the radial runout Kia of test number K as the standard, if the radial runout Kia was equivalent to that of test number K, it was judged that the dimensional accuracy was very low (indicated by "X" in the "Dimensional accuracy evaluation" column of Table 2). If the radial runout Kia was only slightly improved compared to test number K, it was judged that the dimensional accuracy was low (indicated by "△" in the "Dimensional accuracy evaluation" column of Table 2). If the radial runout Kia was significantly improved compared to test number K, it was judged that the dimensional accuracy was high (indicated by "○" in the "Dimensional accuracy evaluation" column of Table 2). If the dimensional accuracy was "○", it was judged that the dimensional accuracy of the bearing parts manufactured using that seamless steel pipe as the material was high.
[0088] [Evaluation Results] The evaluation results are shown in Table 2. Referring to Table 2, the seamless steel pipes of test numbers A to J had appropriate chemical compositions and were manufactured by appropriate methods. Therefore, the microstructure was a structure consisting of ferrite and spheroidal cementite. Furthermore, the specific spheroidal cementite number ratio Ra was 50.0% or more, and the residual stress was less than 30 MPa. As a result, in the dimensional accuracy test, the radial runout Kia was significantly smaller than that of test numbers K and L, and was also smaller than that of test numbers M and N, and the dimensional accuracy was evaluated as "○". In other words, when bearing parts were manufactured using the seamless steel pipes of these test numbers as materials, the dimensional accuracy of the bearing parts could be improved.
[0089] In the test No. K, the second spheroidizing annealing process and the second cold drawing process were not performed in the manufacturing process, and the stress relief annealing process after the straightening process was not performed either. Therefore, the specific spheroidized cementite number ratio Ra was less than 50.0%, and the residual stress was 30 MPa or more.
[0090] In test number L, a softening annealing process was performed in place of the second spheroidizing annealing process in the manufacturing process. Furthermore, a stress relief annealing process was not performed after the straightening process. Therefore, the specific spheroidized cementite number ratio Ra was less than 50.0%, and the residual stress was 30 MPa or more. Therefore, the radial runout Kia was equivalent to that of test number K, and the dimensional accuracy was evaluated as "x". Therefore, when a bearing part was manufactured using the seamless steel pipe as a material, the dimensional accuracy of the bearing part was significantly low.
[0091] In the case of test number M, a softening annealing process was performed in place of the second spheroidizing annealing process in the manufacturing process. Therefore, although the residual stress was less than 30 MPa, the specific spheroidized cementite number ratio Ra was less than 50.0%. Therefore, although the radial runout Kia was smaller than that of test number K, it was larger than that of test numbers A to J, and the dimensional accuracy was evaluated as "△". Therefore, when a bearing part was manufactured using the seamless steel pipe as a material, the dimensional accuracy of the bearing part was low.
[0092] For test number N, the stress relief annealing process after the straightening process was not performed in the manufacturing process. Therefore, the residual stress was 30 MPa or more. Therefore, although the radial runout Kia was smaller than that of test number K, it was larger than that of test numbers A to J, and the dimensional accuracy was evaluated as "△". Therefore, when bearing parts are manufactured using the seamless steel pipe as a material, the dimensional accuracy of the bearing parts is low.
[0093] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure. [Explanation of symbols]
[0094] 1 Cylindrical test piece 2 Slit 10. Bearings 20. Measurement load weight 30 Measuring instruments
Claims
1. The chemical composition, in mass%, is C: 0.60-1.40%, Si: 0.05-0.50%, Mn: 0.10-1.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.01-0.05%, N: 0.020% or less, and Cr: 0.50 to 2.00%; The balance is Fe and impurities. The microstructure consists of ferrite and spheroidal cementite, Among the spherical cementite, the number ratio of spherical cementite having an equivalent circle diameter of more than 0.50 to 1.50 μm is 50.0% or more, The residual stress is less than 30 MPa; Seamless steel tube for bearing parts.
2. The seamless steel pipe for bearing parts according to claim 1, The number ratio of the spherical cementite having a circle equivalent diameter of more than 0.50 to 1.50 μm is 52.0% or more, Seamless steel tube for bearing parts.
Citation Information
Patent Citations
Production of seamless steel pipe having excellent wear resistance
JP1989180918A
Method for softening work-hardened steel tube having spheroidized structure
JP1997078139A
Method for producing bearing race
JP2005113176A
High-carbon steel pipe excellent in cold workability, machinability and hardenability, and method for producing the same
JP2012177154A
Cold-finished seamless steel pipe
WO2005075121A1