Method for designing mixture of iron-containing raw materials and method for operating blast furnace
The mixture design method for blast furnaces optimizes the composition of iron-containing raw materials by setting a lower limit for the weighted average reduction rate and variation, improving air permeability and reducing ventilation resistance.
Patent Information
- Application Number
- JP2021049276
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-23
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2041-03-23
AI Technical Summary
Existing methods for designing iron-containing raw material blends for blast furnaces do not effectively utilize the reduction rate at the start of fusion (Rs) to optimize the composition of the ore layer, leading to poor air permeability due to cohesive zone formation.
A mixture design method that sets a lower limit for the weighted average reduction rate (Rs) and variation (σRs) of multiple types of iron-containing raw materials to improve air permeability by ensuring stable cohesive zone formation.
Enhances air permeability in blast furnaces by optimizing the composition of iron-containing raw materials, promoting indirect and direct reduction rates, and reducing ventilation resistance.
Smart Images

Figure 0007560735000011 
Figure 0007560735000012 
Figure 0007560735000013
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for designing a blending ratio of iron-containing raw materials for forming an ore layer in a blast furnace, and a method for operating a blast furnace in which iron-containing raw materials blended by this blending ratio design method are charged into a blast furnace to form an ore layer. [Background technology]
[0002] In a blast furnace, iron-containing ore raw materials (sintered ore, pellets, lump ore, etc.) and coke as a reducing agent and fuel are charged alternately from the top of the furnace, and hot air is blown in from the tuyeres at the bottom of the furnace together with auxiliary fuel such as pulverized coal. The ore raw materials and coke (hereinafter collectively referred to as "charge") charged from the top of the furnace form ore layers and coke layers that are layered alternately. As the ore raw materials and coke are lowered in the blast furnace, they gradually descend toward the bottom of the furnace, and are heated by the reducing gas rising from the bottom of the furnace, raising their temperature.
[0003] The ore raw materials descend while being heated and reduced in the blast furnace. When they reach the bottom of the furnace, they begin to soften and fuse, forming a fusion layer. In the fusion layer, the gaps between the ore raw materials decrease, and the permeability of the reducing gas deteriorates. For this reason, the reducing gas passes through the coke layer adjacent to the fusion layer and rises toward the top of the furnace. The area in the blast furnace where the fusion layer exists (including the coke layer adjacent to the fusion layer) is called the fusion zone. Therefore, the shape of the fusion zone has a significant impact on the permeability of the blast furnace.
[0004] Therefore, in the past, the gas permeability inside the blast furnace was controlled by focusing on the reducibility of the raw ore.
[0005] For example, Patent Document 1 discloses a method of operating a blast furnace in which the weighted average value of the coke reactivity index (CRI) of all charged coke, the weighted average value of the sinter reducibility index (RI) of all charged sinter ore, and the amount of blast furnace slag per ton of molten iron are all kept within predetermined ranges, thereby suppressing deterioration of coke strength and powdering in the blast furnace and ensuring good permeability within the furnace.
[0006] Furthermore, Patent Document 2 discloses a blast furnace operation method in which the reduction rate of iron ores is maintained at 50% or more by adjusting one or more of the component ratios of FeO and Al2O3 in the sintered ore charged to the blast furnace, the slag ratio of the blast furnace charge, and the blast moisture in the hot air blown from the tuyere of the blast furnace, thereby improving the permeability in the lower part of the furnace, stabilizing the blast furnace conditions, and reducing the fuel rate.
[0007] In addition, a method is known that focuses on and manages the S value (area of the portion where the pressure drop is 200 mmH2O or more in a time-pressure drop curve obtained by heating and reducing sintered ore), which is one of the indexes that represent the high-temperature properties of iron-containing raw materials such as raw ore (hereinafter also referred to as "high-temperature property evaluation index") (Patent Document 3). More specifically, Patent Document 3 discloses a method of charging sintered ore into a blast furnace, in which sintered ore is divided into two types based on its high-temperature properties (S value), and the sintered ore with poor high-temperature properties is charged as a lower layer and the sintered ore with excellent high-temperature properties is charged above it as an upper layer, thereby improving the reducibility of the entire ore layer. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2005-272968 A [Patent Document 2] Japanese Patent Application Publication No. 6-256818 [Patent Document 3] JP 2002-309306 A [Non-patent literature]
[0009] [Non-Patent Document 1] Iron and Steel, Vol. 83 (1997), pp. 97-102, "Development of a method for evaluating the softening and melting properties of sintered ore" Summary of the Invention [Problem to be solved by the invention]
[0010] The high-temperature properties of iron-containing raw materials such as ore are one of the important factors that determine the shape of the cohesive zone. Conventionally, in addition to the above-mentioned S value, the fusion start temperature (Ts), the dripping start temperature (Te, Td), or the difference between the dripping start temperature and the fusion start temperature (ΔT=Te-Ts) have been known as high-temperature property evaluation indices (e.g., Non-Patent Document 1).
[0011] On the other hand, from the viewpoint of reducibility of the iron-containing raw materials, the reduction degree at the melting start temperature (Ts) is important, and therefore, in the present invention, this is defined as the reduction degree at the melting start temperature (Rs). A blending design method for designing the blending of the iron-containing raw materials that form the iron-containing raw material layer in the blast furnace using the reduction degree at the melting start temperature (Rs) has not been reported so far.
[0012] An object of the present invention is to provide a method for designing a blend of iron-containing raw materials that form an iron-containing raw material layer in a blast furnace by using the reduction degree at the start of fusion (Rs). [Means for solving the problem]
[0013] In order to solve the above-mentioned problems, the blending design method of the present invention is (1) a blending design method for designing a blending of a plurality of types of iron-containing raw materials that form an iron-containing raw material layer in a blast furnace, and the blending design method is a weighted average value Rs of the reduction rates at the start of fusion of the plurality of types of iron-containing raw materials represented by the following formula (I). av is the lower limit Rs min The mixture of the plurality of types of iron-containing raw materials is designed so that the lower limit Rs min is at least one parameter selected from the air permeability index, the coke ratio, and the productivity of the blast furnace, which are determined in advance based on the results of stable operation of the blast furnace, and the weighted average value Rs av The weighted average value Rs corresponding to the target value of the parameter in correlation with av It is characterized in that:
number
[0014] (2) The weighted average values Rs corresponding to the target values of two or more of the parameters, respectively av The highest value among them is the lower limit Rs min The method for designing a blend of iron-containing raw materials according to (1), characterized in that the blend is determined as follows:
[0015] (3) The blending design method of the iron-containing raw materials according to (1) or (2), further comprising designing a blend of the plurality of types of the iron-containing raw materials so that a variation σRs of reduction rates at the start of fusion of the plurality of types of the iron-containing raw materials, represented by the following formula (II), is 10% or less.
number
[0016] (4) One of the plurality of types of iron-containing raw materials is composed of a plurality of lump ores of different brands, and the reduction rate Rs of the lump ores at the start of fusion is i is the reduction rate at the start of fusion for each brand, and the blending ratio M i The method for designing a blend of iron-containing raw materials according to any one of (1) to (3), wherein R is a blend ratio for each brand.
[0017] (5) One of the plurality of types of iron-containing raw materials is composed of a plurality of pellets of different brands, and the reduction rate at the start of fusion of the pellets Rs i is the reduction rate at the start of fusion for each brand, and the blending ratio M iThe method for designing a blend of iron-containing raw materials according to any one of (1) to (4), wherein R is a blend ratio for each brand.
[0018] (6) One of the plurality of iron-containing raw materials is composed of a plurality of sintered ores having different sintering raw materials and / or sintering conditions, and the reduction rate Rs of the sintered ores at the start of fusion is set to 0.05 to 0.05. i is the reduction rate at the start of fusion for each of the sintered ores having different sintering raw materials and / or firing conditions, and the blending ratio M i The method for designing a blend of iron-containing raw materials according to any one of (1) to (5), characterized in that R is a blending ratio of the sintered raw materials and / or the sintered ore having different firing conditions.
[0019] (7) A method for operating a blast furnace, comprising charging into the blast furnace a plurality of types of iron-containing raw materials whose blending ratios are designed by the method for designing a blending ratio of iron-containing raw materials according to any one of (1) to (6) to form an iron-containing raw material layer. Effect of the Invention
[0020] According to the present invention, it is possible to provide a blending design method for designing a blending of iron-containing raw materials that form an iron-containing raw material layer in a blast furnace by using the reduction degree (Rs) at the start of fusion. [Brief description of the drawings]
[0021] [Figure 1] FIG. [Diagram 2] FIG. 2 is a diagram showing an apparatus for measuring a reduction rate at the start of fusion. [Diagram 3] FIG. 2 is a diagram showing conditions for measuring the reduction rate at the start of fusion. [Figure 4] FIG. 2 is a diagram showing an example of high-temperature properties of sintered ore. [Diagram 5] 13 is a diagram illustrating the correlation between the corrected airflow resistance index K2cor and the weighted average value Rsav (lower limit value Rsmin). FIG. [Figure 6] FIG. 2 is a diagram illustrating the correlation between the coke ratio CR and the weighted average value Rsav (lower limit value Rsmin). [Figure 7] FIG. 2 is a diagram illustrating the correlation between the productivity and the weighted average value Rsav (lower limit value Rsmin). [Figure 8] FIG. 2 is a diagram illustrating the relationship between the reduction rate Rs at the start of fusion and the air permeability in a blast furnace. [Figure 9] This is a graph showing the relationship between the corrected air resistance index K2cоr and the weighted average value Rsav before and after mix design. [Figure 10] FIG. 1 is a diagram showing the relationship between the coke ratio CR and the weighted average value Rsav before and after the blend design. [Figure 11] FIG. 1 is a diagram showing the relationship between the productivity and the weighted average value Rsav before and after the blend design. [Figure 12] FIG. 13 is a graph showing the relationship between the corrected airflow resistance index K2cоr and the variation σRs in the reduction rate at the start of fusion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] First, the process by which the present invention was completed will be described with reference to FIG.
[0023] FIG. 1 is a diagram showing the inside of a blast furnace. As shown in FIG. 1, a charge 2 is charged into the blast furnace 1. The charge 2 is mainly coke and iron-containing raw materials (including ore raw materials described later), and the coke and iron-containing raw materials are charged alternately to form a coke layer 3 and an iron-containing raw material layer 4 that are alternately stacked. The iron-containing raw material layer 4 does not have to be composed of only iron-containing raw materials. For example, the iron-containing raw material layer 4 may contain coke. In the iron-containing raw material layer 4 that is heated and reduced and descends in the blast furnace, the iron-containing raw materials begin to soften and fuse, forming a fusion layer 5. The molten pig iron 9 that drips from the fusion layer 5 is stored in the hearth 10. The hot air blown into the blast furnace from the tuyere 7 burns the pulverized coal and coke in the raceway 8 in front of the tuyere, generating reducing gas (CO, H2), which rises in the furnace. In the cohesive zone 5, the iron-containing raw materials are fused together, so there are few gaps between the iron-containing raw materials, and the permeability of the reducing gas is poor. Therefore, the reducing gas passes through the coke layer 6 adjacent to the cohesive zone 5 and rises in the blast furnace 1. In other words, the permeability of the furnace gas in the cohesive zone is limited to the coke layer 6 adjacent to the cohesive zone 5, so the shape of the cohesive zone has a significant effect on the permeability of the blast furnace 1. Note that the cohesive zone refers to the region in which the cohesive layer 5 exists, including the coke layer 6 between the cohesive layers 5.
[0024] The inventors considered that the high-temperature properties of the iron-containing raw materials affect the shape of the cohesive zone, and considered it important to grasp the high-temperature properties. As a result of extensive research focusing on an index (high-temperature property evaluation index) that indicates the high-temperature properties, they found that the reduction ratio Rs at the start of fusion of the iron-containing raw materials forming the iron-containing raw material layer 4 was weighted according to the blending ratio (mass%) of each iron-containing raw material, and the weighted average value Rs av (Hereinafter, simply "weighted average value Rs av " has been found to be correlated with the gas permeability inside a blast furnace, and this has led to the completion of the present invention.
[0025] In this specification, the reduction ratio Rs at the start of fusion refers to the reduction ratio of the iron-containing raw material when a fusion layer is formed in a load-softening test described later. Whether or not a fusion layer is formed can be determined based on whether or not the pressure loss of the iron-containing raw material layer reaches a predetermined value in a load-softening test described later. For example, it can be determined that a fusion layer is formed when the pressure loss of the iron-containing raw material layer reaches 200×9.8 Pa.
[0026] (First embodiment) A first embodiment of the present invention will now be described.
[0027] The blending design method of this embodiment is a method for designing the blending of multiple types of ore raw materials that form an ore layer (corresponding to the above-mentioned iron-containing raw material layer). The ore raw material is a raw material containing 50 mass% or more of iron. At least two types of ore raw materials are used for the ore raw materials whose blending is designed by the blending design method of this embodiment, and for example, two or more types of ore raw materials selected from the group consisting of sintered ore, lump ore, and pellets are used.
[0028] In the blending design method of this embodiment, the weighted average value Rs of the reduction rate Rs at the start of fusion of multiple types of ore raw materials is av However, the lower limit Rs min The mixture of multiple types of ore raw materials is designed so that the weighted average value Rs av is expressed by the following formula (1).
[0029]
number
[0030] In the above formula (1), the reduction ratio Rs of the ore raw material type i at the start of fusion iThe reduction ratio Rs at the start of fusion is measured for each type of ore raw material. The reduction ratio Rs at the start of fusion is measured using the load-softening test described in Non-Patent Document 1, and the following measuring device and measuring conditions are used.
[0031] (Measuring device for reduction rate Rs at the start of fusion) FIG. 2 shows an apparatus for measuring the reduction ratio Rs at the start of fusion. In this measuring apparatus, as shown in FIG. 2, two Tammann electric furnaces are arranged in two stages, one above the other, and the two furnaces (upper furnace 12 and lower furnace 11) are connected by a flange. Gas 17 is introduced from the lower part of the lower furnace 11. In the lower furnace 11, the lower furnace heater H' is controlled by the lower furnace heater control means 16, and the gas 17 is preheated. Then, the gas 17 preheated to a high temperature is introduced into the upper reduction furnace (upper furnace 12). The gas 17 introduced into the upper furnace 12 is introduced into a graphite crucible 13 (inner diameter approximately 85 mm) with a hole in the bottom, and heats and reduces the ore raw material in the ore layer 14 sandwiched between two coke layers 21. A load is applied to the coke layer 21 and the ore layer 14 by a load machine 19. When the gas 17 is introduced into the upper furnace 12 and the lower furnace 11 to heat and reduce the raw ore, the upper furnace heater H is controlled by the upper furnace heater control means 15 to perform adiabatic control so that the difference between the outer wall temperature of the reaction tube of the upper furnace 12 (the reaction tube provided between the graphite crucible 13 and the upper furnace heater H) and the temperature of the top of the sample layer (the layer consisting of the coke layer 21 and the ore layer 14) is constant. The upper furnace heater control means 15 also performs heating control as described later. The post-reduced gas 18 is discharged from the top of the upper furnace 12. The molten iron generated by heating and reducing the raw ore in the ore layer 14 is received in the dripping molten iron receiver 20. According to this device, the reduction and melting behavior of the raw ore in an actual furnace can be accurately grasped by introducing the gas 17 preheated to a high temperature and performing adiabatic control.
[0032] (Conditions for measuring reduction rate Rs at the start of fusion) The ore raw material forming the ore layer 14 is any one of a plurality of types of ore raw materials for which the blending is designed. A load-softening test is performed for each type of ore raw material for which the blending is designed, so that the reduction degree Rs at the start of fusion can be measured for each type of ore raw material. The ore raw material forming the ore layer 14 is made of ore raw material sized to 10 mm to 15 mm. The ore layer 14 is formed to have a layer thickness of approximately 70 mm. The coke forming the coke layer 21 is made of coke sized to 10 mm to 15 mm. The coke layers 21 sandwiching the ore layer 14 are each made to have a layer thickness of approximately 20 mm.
[0033] The composition and temperature conditions of the gas 17 introduced into the above-mentioned measuring device are as shown in FIG. 3. Specifically, the heating rate of the gas 17 in the lower furnace 11 is set to 10°C / min, which is the maximum capacity of the furnace, and after the temperature of the gas 17 reaches the maximum normal temperature of the furnace (1700°C), this temperature is maintained. The heating rate of the gas 17 in the upper furnace 12 is set to 10°C / min up to 1000°C, and is set to 5°C / min, which is the average heating rate of an actual furnace, at 1000°C or higher. Regarding the composition of the gas 17, N2 is introduced up to 800°C, and reducing gas (CO: 29.4 volume %-H2: 3.6 volume %-N2: 67.0 volume %) is introduced at 800°C or higher. The gas flow rate is constant at 34 Nl / min, and a standard superficial velocity of 10 cm / sec is ensured. The composition of the gas 17 is set to 10°C / min, 15×10 -3 kg / Nm 3 Based on the bosh gas composition when the pulverized coal ratio was 100 kg / t-pig, the reduction rate of the ore raw material at 1000°C was determined by adjusting the N2 ratio while keeping the H2 / CO ratio constant so that it would be 30%, which is almost the same as the results of an actual dismantling investigation (the results of an investigation after dismantling an actual furnace).
[0034] As shown in Fig. 3, the load applied to the ore layer 14 and the coke layer 21 is 0.098 MPa when the temperature of the gas 17 is 800°C or higher. At this load (0.098 MPa) or higher, the load dependency on shrinkage and permeability is extremely small, so the above-mentioned condition is used. When the temperature is less than 800°C, no load is applied to the ore layer 14 and the coke layer 21. The upper furnace 12 performs heating control at the start of the test, switches to adiabatic control at around 1200°C, and switches back to heating control after molten iron has dripped into most of the sample layer (ore layer 14).
[0035] Fig. 4 shows an example of the high-temperature property evaluation index of sintered ore measured by the load-softening test described in Non-Patent Document 1 using the above-mentioned measuring device and measuring conditions. In this embodiment, of the high-temperature property evaluation indexes shown in Fig. 4, the reduction degree when the cohesive layer is formed (when the pressure loss in the ore layer reaches 200 × 9.8 Pa), that is, the reduction degree at the start of cohesiveness Rs, is used.
[0036] In addition, in Fig. 4, in addition to the reduction rate Rs at the start of fusion, the maximum pressure drop in the ore layer (maximum pressure drop value △P max ), the temperature when the fusion layer is formed (when the pressure loss in the ore layer reaches 200×9.8 Pa) (fusion start temperature Ts), the temperature range of the ore layer when the fusion layer is formed (when the pressure loss in the ore layer is 200×9.8 Pa or more) (temperature range △T), the integral value of the pressure loss when the fusion layer is formed (when the pressure loss in the ore layer is 200×9.8 Pa or more (i.e., within the temperature range △T)), the dripping start temperature of the ore raw material (dripping start temperature Td), and the temperature when the pressure loss in the ore layer drops to the pressure loss when the fusion layer is formed (200×9.8 Pa).
[0037] In this embodiment, the above-mentioned test is performed for each type of ore raw material, and the reduction ratio Rs at the start of fusion of each measured ore raw material is calculated by the reduction ratio Rs at the start of fusion in the above formula (1). i Used as.
[0038] The blending ratio M of type i of ore raw material in the above formula (1) i The blending ratio MR (the mass ratio of each type of ore raw material to 100 mass% of all types of ore raw materials for which the blend is designed) obtained for each type of ore raw material is used for R. The method of obtaining the blending ratio MR is not particularly limited, and the mass of each type of ore raw material may be actually measured or the mass of each type of ore raw material may be predicted.
[0039] (Lower limit Rs min About Lower limit Rs min is determined based on at least one parameter of the air permeability resistance index K2 in the blast furnace, the coke ratio CR, and the productivity. A specific description will be given below, but first, the air permeability resistance index K2 will be described.
[0040] The airflow resistance index K2 is a known index indicating airflow resistance (for example, see "Iron and Steel Physical Properties Handbook, Steelmaking Edition," p. 250, published by the Iron and Steel Institute of Japan and the Japan Society for the Promotion of Science, 54th Committee on Ironmaking, 2006), and the higher the airflow resistance (in other words, the lower the air permeability), the higher the airflow resistance index K2. The airflow resistance index K2 can be calculated from the following formula (2).
[0041]
number
[0042] Next, the lower limit Rs from the airflow resistance index K2 min This section explains how to determine the
[0043] Weighted average value Rs avIf the correlation between the airflow resistance index K2 and the airflow resistance index K2 is determined in advance, the weighted average value Rs corresponding to the airflow resistance index K2 (target value) can be determined by specifying the target value of the airflow resistance index K2. av The lower limit is Rs min The weighted average value Rs av The correlation between the airflow resistance index K2 and the airflow resistance index K2 can be determined by the method described below.
[0044] Weighted average value Rs av In a coordinate system with the coordinate axes of the index K2 and the air permeability resistance index K2, the operation performance of the blast furnace is plotted, and the area where the operation performance of the blast furnace when stable operation is performed (hereinafter referred to as the "stable operation area") and the area where the operation performance of the blast furnace when stable operation is not performed (hereinafter referred to as the "unstable operation area") are plotted are identified. Then, the boundary line dividing the stable operation area and the unstable operation area is determined by the weighted average value Rs av and the airflow resistance index K2. The term "division" here does not mean to strictly divide the stable operation region and the unstable operation region, but may be anything that can roughly divide the stable operation region and the unstable operation region.
[0045] The boundary between the stable operation region and the unstable operation region can be created, for example, by the following procedure. Among the operational records in which stable operation was performed, the operational record with the smallest value of the air permeability resistance index K2 is calculated as the weighted average value Rs av Next, the extracted operation results and weighted average value Rs av An approximation formula is created based on this, and this is used as the boundary line. As described above, since it is not necessary to strictly divide the stable operation region and the unstable operation region, the stable operation region does not have to be determined as the region in which all operational results in which stable operation was performed are plotted. In roughly dividing the stable operation region and the unstable operation region, for example, the region in which 90% or more of all operational results in which stable operation was performed are plotted can be regarded as the stable operation region.
[0046] In Fig. 5, the results of stable operation of the four blast furnaces 1 to 4 are plotted, and the weighted average Rs av and corrected ventilation resistance index K2 cоr In FIG. 5, instead of the airflow resistance index K2, the corrected airflow resistance index K2 cоr The "airflow resistance index" in this invention refers to the airflow resistance index K2 or the corrected airflow resistance index K2. cоr Includes:
[0047] Corrected ventilation resistance index K2 cоr is a value obtained by correcting the air permeability index K2 expressed by the above formula (2) based on the coke ratio CR and coke strength DI in blast furnace operation. Since the air permeability index K2 is affected by the coke ratio CR and coke strength DI, the weighted average value Rs av Therefore, instead of the airflow resistance index K2, the corrected airflow resistance index K2 cоr Here, the permeability index K2 was set to the value when the coke ratio CR was 320 kg / t (standard value) and the coke strength DI was 86% (standard value).
[0048] Corrected ventilation resistance index K2 cоr In the calculation of the above, a correction was made by adding 3[-] to the permeability resistance index K2 in response to an increase of 1 kg / t in the coke ratio CR in blast furnace operation from the reference value (320 kg / t). In addition, a correction was made by subtracting 3[-] from the permeability resistance index K2 in response to a decrease of 1 kg / t in the coke ratio CR in blast furnace operation from the reference value (320 kg / t). On the other hand, a correction was made by adding 120[-] to the permeability resistance index K2 in response to an increase of 1% in the coke strength DI in blast furnace operation from the reference value (86%). In addition, a correction was made by subtracting 120[-] from the permeability resistance index K2 in response to a decrease of 1% in the coke strength DI in blast furnace operation from the reference value (86%).
[0049] According to Figure 5, the weighted average value Rs av and corrected ventilation resistance index K2 cоrThe correlation is at the lower limit Rs min The lower limit Rs is defined by the straight line (dotted line) shown as min According to the straight line (dotted line), the corrected ventilation resistance index K2 cоr The higher the lower limit Rs min The corrected ventilation resistance index K2 is lower. cоr The lower the lower limit Rs min The lower limit Rs min Corrected ventilation resistance index K2 for the straight line (dotted line) cоr The higher region is the stable operation region, and the lower limit Rs min Corrected ventilation resistance index K2 for the straight line (dotted line) cоr The region with a low Rs includes the unstable operation region. All the operational results plotted in Figure 5 are stable operation results, but some operational results are excluded and the lower limit Rs min A straight line (dotted line) is determined.
[0050] As shown in Figure 5, the weighted average value Rs av and corrected ventilation resistance index K2 cоr Correlation of (i.e., lower limit Rs min If the line (straight line) is determined, the corrected ventilation resistance index K2 cоr The lower limit Rs corresponding to the target value min For example, the corrected airflow resistance index K2 cоr When the target value is 800[-], the lower limit Rs min becomes 58[%].
[0051] In the example shown in FIG. 5, the weighted average value Rs av and corrected ventilation resistance index K2 cоr The correlation between the two is a linear function (lower limit Rs min As mentioned above, the weighted average value Rs av and corrected ventilation resistance index K2 cоr The correlation between the above may be defined as a boundary line dividing a stable operation region and an unstable operation region.
[0052] Next, the coke ratio CR is reduced to the lower limit Rs minThis section explains how to determine the
[0053] Weighted average value Rs av If the correlation between the coke ratio CR and the weighted average value Rs corresponding to the coke ratio CR (target value) is determined in advance, the weighted average value Rs corresponding to the coke ratio CR (target value) can be obtained by specifying the target value of the coke ratio CR. av The lower limit is Rs min The weighted average value Rs av The correlation between the carbon dioxide and the coke ratio CR can be determined by the method described below.
[0054] Weighted average value Rs av The operation record of the blast furnace is plotted in a coordinate system with the coke ratio CR as the coordinate axis, and the stable operation region and the unstable operation region are identified as described above. Then, the boundary line dividing the stable operation region and the unstable operation region is drawn by the weighted average value Rs av and coke ratio CR.
[0055] The boundary between the stable operation region and the unstable operation region can be created, for example, by the following procedure. The operation record with the lowest coke ratio CR among the stable operation records is calculated as the weighted average value Rs av Next, the extracted operation results and weighted average value Rs av An approximation equation is created based on this and used as the boundary line.
[0056] In Fig. 6, the results of stable operation of the four blast furnaces 1 to 4 are plotted, and the weighted average Rs av The correlation between the weighted average value Rs and the coke ratio CR is shown in Fig. 6. av The correlation between the coke ratio and the coke ratio CR is as follows: min This lower limit Rs min According to the line, the lower limit Rs when the coke ratio CR is 330 [kg / t] min is 56% and the lower limit Rs min will increase by 2%.
[0057] The lower limit Rs shown in Figure 6 min According to the line, the higher the coke ratio CR, the lower limit Rs min The lower the coke ratio CR, the lower limit Rs min The lower limit Rs min The region with a high coke ratio CR is the stable operation region, and the lower limit Rs min The area where the coke ratio CR is low on the line of the line includes the unstable operation area. All the operational results plotted in Fig. 6 are operational results where stable operation was performed, but some operational results were excluded and the lower limit Rs min A straight line (dotted line) is determined.
[0058] As shown in Figure 6, the weighted average value Rs av and the correlation with the coke ratio CR (i.e., the lower limit Rs min Once the line (Rs) is determined, the lower limit Rs corresponding to the target value of the coke ratio CR can be calculated. min For example, when the target value of the coke ratio CR is set to 290 [kg / t], the lower limit Rs min becomes 64[%].
[0059] In the example shown in FIG. 6, the weighted average value Rs av The correlation between the coke ratio CR and the coke ratio CR is expressed as a linear function (lower limit Rs min As mentioned above, the weighted average value Rs av The correlation between the carbon content and the coke rate CR may be defined as a boundary line dividing the stable operation region and the unstable operation region.
[0060] Next, the lower limit Rs min This section explains how to determine the
[0061] Weighted average value Rs av If the correlation between the productivity and the target value of the productivity is determined in advance, the weighted average value Rs corresponding to the productivity (target value) can be obtained by specifying the target value of the productivity. av The lower limit is Rs minThe weighted average value Rs av The correlation between the productivity and the amount of molten iron can be determined by the method described below.
[0062] Weighted average value Rs av The operation results of the blast furnace are plotted in a coordinate system with the iron production rate and productivity as the coordinate axes, and the stable operation region and the unstable operation region are identified as described above. Then, the boundary line dividing the stable operation region and the unstable operation region is drawn by the weighted average value Rs av and productivity.
[0063] The boundary between the stable operation region and the unstable operation region can be created, for example, by the following procedure. The operation results with the highest productivity among the stable operation results are calculated as the weighted average value Rs av Next, the extracted operation results and weighted average value Rs av An approximation equation is created based on this and used as the boundary line.
[0064] In Fig. 7, the results of stable operation of the four blast furnaces 1 to 4 are plotted, and the weighted average Rs av According to Figure 6, the weighted average value Rs av The correlation between the productivity and the lower limit Rs min This lower limit Rs min According to the line, the lower limit Rs when the productivity is 1.8[-] min is 56[%], and the lower limit Rs min will increase by 1%.
[0065] Lower limit Rs min According to the line, the higher the productivity, the lower limit Rs min The lower the productivity, the lower the lower limit Rs min The lower limit Rs min The area with low productivity relative to the line is the stable operation area, and the lower limit Rs minThe unstable operation region is included in the high productivity region of the line. All the operational results plotted in Fig. 7 are stable operation results, but some operational results are excluded and the lower limit value Rs min A straight line (dotted line) is determined.
[0066] As shown in Figure 7, the weighted average value Rs av and productivity (i.e., lower limit Rs min If the line (Rs) is determined, the lower limit Rs corresponding to the target value of the productivity can be obtained. min For example, when the target value of the productivity is set to 2.0 [-], the lower limit Rs min becomes 58[%].
[0067] In the example shown in FIG. 7, the weighted average value Rs av The correlation between the productivity and the iron production rate is expressed as a linear function (lower limit Rs min As mentioned above, the weighted average value Rs av The correlation between the temperature and productivity may be defined as a boundary line dividing a stable operation region and an unstable operation region.
[0068] Lower limit Rs min can be determined based on two or more parameters of the air permeability index K2, the coke ratio CR, and the productivity. In this case, the lower limit Rs for each parameter is determined based on the above-mentioned method. min is determined, and the lower limit Rs min (Candidate value) occurs. The lower limit value Rs min The lower limit Rs, which is the highest value among the (candidate values) min The lower limit Rs in the mix design method of this embodiment min This results in a weighted average value of Rs av is the lower limit Rs min When the ore raw material mix is designed so that the weighted average value Rs av All lower limits Rs min (candidate value) or more. Note that the lower limit Rs minAs multiple lower limits Rs min It can also be the average value of (candidate values).
[0069] (Regarding the mix design of mineral ore materials) In the mix design method of this embodiment, the weighted average value Rs av is the lower limit Rs min The blend of multiple types of ore raw materials is designed so that the weighted average value Rs av When the ore raw materials with different blend ratios were used in an actual blast furnace as raw materials for forming the ore layer (hereinafter also referred to as "blast furnace raw materials"), the weighted average value Rs av is the lower limit Rs min If this is the case, the air flow resistance inside the blast furnace will be low and stable.
[0070] Weighted average value Rs av As can be understood from the above formula (1), the blending ratio M i R and reduction rate at the start of fusion Rs i It can be adjusted by changing the mixture ratio M i R can be changed by changing the blending ratio of each ore raw material. i can be changed by changing the type of ore raw material. Therefore, the weighted average value Rs av is the lower limit Rs min In other words, the weighted average value Rs av is the lower limit Rs min This means determining the blending ratio of the raw ore materials and the types of the raw ore materials that satisfy the above requirements.
[0071] The weighted average value of Rs av An example of the blending of the ore raw materials when calculating is shown in FIG. 4. The results shown in FIG. 4 were obtained using the sintered ore shown in Table 1 below. Also, σRs shown in Table 1 below is the variation in the reduction ratio Rs at the start of fusion of multiple types of ore raw materials, and the details will be described later.
[0072] [Table 1]
[0073] The blending design method of this embodiment can be used when changing the blending ratio of the ore raw materials used in the blast furnace or when changing the type of ore raw materials used in the blast furnace, as shown below.
[0074] When changing the blending ratio of the ore raw materials used in the blast furnace, for example, the reduction ratio Rs at the start of fusion of each ore raw material already in use is measured in advance, and when the blending ratio to be changed is set, the weighted average value Rs av is the lower limit Rs min It is judged whether it is more than the weighted average value Rs av is the lower limit Rs min If it is more than this, the mix ratio of the ore raw material to be changed is adopted and the mix is designed (decided). Weighted average value Rs av is the lower limit Rs min If it is less than the weighted average value of Rs av is the lower limit Rs min The mix ratio will be reviewed again and the mix will be designed so that the weighted average value is Rs av is the lower limit Rs min If it is less than the weighted average value of Rs av is the lower limit Rs min The types of ore raw materials may be reviewed and the blending may be designed so as to satisfy the above.
[0075] When changing the type of raw ore used in a blast furnace, the reduction ratio Rs at the start of fusion of the raw ore to be changed (if there is raw ore that is not changed, the reduction ratio Rs at the start of fusion of the raw ore) is measured in advance, and when the type of raw ore is changed without changing the blending ratio, the weighted average value Rs av is the lower limit Rs min It is judged whether it is more than the weighted average value Rs av is the lower limit Rs min If it is above this, the mix is designed (decided) by adopting the change in type without changing the mix ratio already in use. Weighted average value Rs av is the lower limit Rs min If it is less than the weighted average value of Rs avis the lower limit Rs min The blend ratio of the ore raw materials will be reviewed and the blending ratio will be designed so that the weighted average value Rs av is the lower limit Rs min In order to achieve the above, the type of ore raw material to be changed may be reviewed and the blend may be designed.
[0076] The ore raw material, the composition of which is designed by the blending design method of this embodiment, is used as blast furnace raw material. The blast furnace raw material may be composed only of the ore raw material, the composition of which is designed by the blending design method of this embodiment, but may also contain, in addition to the ore raw material, for example, coke, ferro coke, carbon-containing agglomerates, and auxiliary materials. In this case, as described above, the weighted average value Rs av is the lower limit Rs min The blending ratio of the ore raw materials may be designed so as to satisfy the above. By using the ore raw materials whose blending ratio is designed by the blending ratio design method of this embodiment as blast furnace raw materials in blast furnace operation, the permeability inside the blast furnace is improved. The reason for this will be explained with reference to FIG.
[0077] FIG. 8 is a diagram explaining the relationship between the reduction ratio Rs at the start of fusion and the permeability in the blast furnace. As mentioned above, the fusion layer has poor permeability, so almost no reducing gas flows through the fusion layer, but passes through the coke layer adjacent to the fusion layer. In the process of the fusion layer being formed from the ore layer, the main reduction form transitions from indirect reduction by reducing gas (FeO+CO(g)→Fe+CO2(g) (exothermic reaction)) to direct reduction by solid carbon (FeO+C→Fe+CO(g) (endothermic reaction)). An increase in the reduction ratio Rs at the start of fusion means that the indirect reduction ratio (exothermic reaction) until the fusion layer is formed increases, and the direct reduction ratio (endothermic reaction) in the lower part of the furnace decreases. For this reason, if the reduction ratio Rs at the start of fusion increases, the amount of heat absorbed in the lower part of the furnace decreases (the endothermic reaction decreases), and the temperature rise of the ore raw material is promoted. When the temperature rise of the ore raw material is accelerated, the carburization of the ore (iron) is accelerated and the dripping of the molten iron is accelerated. As a result, the area of the cohesive zone on the furnace center side is reduced, and the reducing gas can easily pass through the cohesive layer. Then, the weighted average reduction rate Rs of the ore raw material used as the blast furnace raw material at the start of fusion Rs is av is the lower limit Rs min If the temperature is more than this, the phenomenon occurs significantly, and it is considered that the permeability inside the blast furnace is likely to be improved.
[0078] In the mix design method of this embodiment, the weighted average value Rs av is the lower limit Rs min In addition to the above, it is preferable to design the blending of the multiple types of raw ore materials so that the variation σRs of the reduction rates Rs at the start of fusion of the multiple types of raw ore materials (hereinafter, simply referred to as "variation σRs") expressed by the following formula (3) is 10% or less. The condition that the variation σRs is 10% or less has also been determined by the present inventors based on the examples described later.
[0079]
number
[0080] In the above formula (3), the weighted average value Rs av , Reduction rate at the start of fusion Rs i and mixing ratio M i R is the weighted average value Rs in the above formula (1). av , Reduction rate at the start of fusion Rs i and mixing ratio M i Since these are the same as R, detailed explanations will be omitted.
[0081] The variation σRs is the weighted average value Rs av Similarly, it can be adjusted by changing the amount of each ore raw material and the type of ore raw material. In other words, the weighted average value Rs av is the lower limit Rs min In addition, designing the mix of ore raw materials so that the variation σRs is 10% or less is the weighted average value Rs av is the lower limit Rs min In addition to the above, this means determining the blending ratio of the raw ore materials and the types of the raw ore materials so that the variation σRs is 10% or less.
[0082] Weighted average value Rs av is the lower limit Rs min In addition to the above, when the variation σRs is 10% or less, the permeability in the blast furnace is more likely to be improved than when the variation σRs exceeds 10%.
[0083] In the above-described embodiment, the reduction rate Rs at the start of fusion is set for each type of raw ore. i and mixing ratio M iHowever, there are multiple brands of ore raw materials such as lump ore and pellets, and even if the type of ore raw material is the same (lump ore or pellets), the reduction ratio Rs at the start of fusion may differ between different brands. Therefore, in the blending design method of this embodiment, when multiple brands of ore raw materials are used as at least one type of ore raw material among lump ore and pellets, it is preferable to use the reduction ratio Rs at the start of fusion and the blending ratio MR set for each brand as the reduction ratio Rs at the start of fusion and the blending ratio MR of the ore raw material of that type.
[0084] Specifically, for example, when sinter, lump ore, and pellets are used as the ore raw material, and lump ore of brand a and lump ore of brand b are used as the lump ore, the reduction ratio Rs at the start of fusion and the blending ratio MR set for the lump ore of brand a and the lump ore of brand b are the reduction ratio Rs at the start of fusion in the above formulas (1) and (3). i and mixing ratio M i R. In other words, the subscript i in the above formulas (1) and (3) is defined not only to distinguish between types of mineral ore, but also to distinguish between multiple brands that belong to the same type.
[0085] In addition, for example, when sinter, lump ore, and pellets are used as the ore raw material, and when pellets of brand a and brand b are used as the pellets, the reduction ratio Rs at the start of fusion and the blending ratio MR set for the pellets of brand a and the pellets of brand b are calculated based on the reduction ratio Rs at the start of fusion in the above formulas (1) and (3). i and mixing ratio M i R. In other words, the subscript i in the above formulas (1) and (3) is defined not only to distinguish between types of mineral ore, but also to distinguish between multiple brands that belong to the same type.
[0086] The brands include those named after the place of origin (mine) of the ore raw material or the company name of the manufacturer. The blending ratio MR set for each brand is the mass ratio of each brand of ore raw material to 100% by mass of all types and brands (by type), and is not the mass ratio of each brand of lump ore to all brands of lump ore (i.e., the mass ratio of each brand of lump ore to 100% by mass of lump ore) or the mass ratio of each brand of pellets to all brands of pellets (i.e., the mass ratio of each brand of pellets to 100% by mass of pellets).
[0087] Similarly, there are multiple sintered ores with different sintering raw materials and / or firing conditions, and the reduction ratio Rs at the start of fusion may differ between sintered ores with different sintering raw materials and / or firing conditions. When the sintering raw materials are different, the components and particle size of the sintering raw materials themselves may be different, or the blending ratio of the sintering raw materials may be different. When the sintering raw materials are different, for example, the components of the sintered ore will be different, so the reduction ratio Rs at the start of fusion may be different. On the other hand, an example of a firing condition is the fuel ratio. When the firing conditions are different, the pore structure of the sintered ore will be different, so the reduction ratio Rs at the start of fusion may be different.
[0088] Therefore, in the blending design method of this embodiment, when a plurality of sintered ores having different sintering raw materials and / or firing conditions are used as the sintered ore, the reduction rate at the start of fusion Rs shown in the above formulas (1) and (3) is i and mixing ratio M i It is preferable to use the reduction ratio Rs at the start of fusion and the blending ratio MR set for each sintered ore with different sintering raw materials and / or firing conditions as R. In addition, the blending ratio MR set for each sintered ore with different sintering raw materials and / or firing conditions is the mass ratio of each sintered ore with different sintering raw materials and firing conditions to 100 mass% of all types of ore raw materials, and is not the mass ratio of each sintered ore with different sintering raw materials and firing conditions to all sintered ores with different sintering raw materials and firing conditions.
[0089] Even if the ore raw materials are the same type, by setting the reduction ratio Rs at the start of fusion and the blending ratio MR for each sinter raw material and / or ore raw material with different firing conditions (sintered ore) and for each brand of ore raw material (lump ore, pellets), the actual high-temperature properties of the ore raw material (reduction ratio Rs at the start of fusion) can be more accurately reflected by the weighted average value Rs av And the variation σRs becomes easier to find.
[0090] Weighted average value Rs for sintered raw materials and / or ore raw materials with different firing conditions (sintered ore) and ore raw materials of different brands (lump ore, pellets) av When adjusting the variation σRs to perform the blending design, in addition to the blending ratio of each type of ore raw material, it is possible to change the blending ratio of each sintering raw material and / or ore raw material with different firing conditions (sintered ore) and each brand of ore raw material (lump ore, pellets), as well as the type of ore raw material, the sintering raw material and / or firing conditions and brand.
[0091] (Blast furnace operation method) In blast furnace operation, multiple types of ore raw materials whose mixes are designed by the mix design method of this embodiment are charged into the blast furnace to form an ore layer (corresponding to the iron-containing raw material layer in the present invention) in the blast furnace.
[0092] Second embodiment Next, a second embodiment of the present invention will be described.
[0093] This embodiment is a method for designing a blend of multiple types of iron-containing raw materials that form an iron-containing raw material layer. The iron-containing raw materials are raw materials that contain 15 mass% or more of iron, and specifically include sintered ore, pellets, lump ore, carbon-containing agglomerated ore, ferro-coke, etc. The iron-containing raw materials are a concept that includes ore raw materials. In addition, the types of iron-containing raw materials refer to classifications such as sintered ore, pellets, lump ore, carbon-containing agglomerated ore, and ferro-coke.
[0094] As described above, the cohesive zone is formed by softening and fusing the ore material contained in the iron-containing raw material layer. However, when the iron-containing raw material layer contains iron-containing raw materials other than the ore material, the iron-containing raw materials may also contribute to the formation of the cohesive zone. In other words, the shape of the cohesive zone may be affected. Therefore, in this embodiment, the reduction ratio Rs at the start of fusing is set for each type of iron-containing raw material, and the weighted average reduction ratio Rs is calculated. av is the lower limit Rs min The blend of multiple types of iron-containing raw materials is designed so as to satisfy the above.
[0095] As the iron-containing raw material for which the blending design method of the present embodiment is used, two or more types of iron-containing raw materials are used. For example, two or more types of iron-containing raw materials selected from the group consisting of sintered ore, lump ore, pellets, ferro coke, and carbon-containing agglomerated ore can be used.
[0096] In the blending design method of this embodiment, the weighted average value Rs of the reduction ratios Rs at the start of fusion of multiple types of iron-containing raw materials is calculated using the following formula (4): av is the lower limit Rs min The mixture of multiple types of iron-containing raw materials is designed so that the lower limit Rs min As described in the first embodiment, the ventilation resistance index K2 (or the corrected ventilation resistance index K2 cоr ), coke ratio CR and iron production rate, or based on any one of the air permeability index K2 (or corrected air permeability index K2 cоr ), the coke ratio CR, and the productivity may be determined based on two or more parameters.
[0097]
number
[0098] The reduction ratio Rs of the iron-containing raw material of type i at the start of fusion in the above formula (4) i The reduction ratio Rs at the start of fusion measured for each type of iron-containing raw material is used for this purpose. The load-softening test described in Non-Patent Document 1 can be used to measure the reduction ratio Rs at the start of fusion of the iron-containing raw material, as in the first embodiment. The load-softening test described in Non-Patent Document 1 and the device and conditions used for the test are the same as those in the first embodiment, and therefore a detailed description will be omitted. Also, the blending ratio M of the iron-containing raw material of type i in the above formula (4) i R is the blending ratio M of the first embodiment i R (the blending ratio M of the above formula (1) i R), so detailed explanation is omitted.
[0099] The weighted average value Rs expressed by the above formula (4) av can be adjusted by changing the blending amount of each iron-containing raw material or the type of iron-containing raw material. Therefore, in this embodiment, the weighted average value Rs av is the lower limit Rs min It is necessary to design the mixture of iron-containing raw materials so that the weighted average value Rs av is the lower limit Rs min This means that the blending ratio of the iron-containing raw materials and the types of the iron-containing raw materials are determined so as to satisfy the above.
[0100] The blending design method of this embodiment can be used when changing the blending ratio of the iron-containing raw materials used in the blast furnace or when changing the type of the iron-containing raw materials used in the blast furnace, similar to the blending design method of the first embodiment. The specific method is the same as that of the first embodiment, so a detailed description will be omitted.
[0101] The iron-containing raw materials, the composition of which is designed by the blending design method of this embodiment, are used as raw materials (blast furnace raw materials) for forming an iron-containing raw material layer. The blast furnace raw materials may be composed only of the iron-containing raw materials, the composition of which is designed by the blending design method of this embodiment, but may also contain, for example, coke and auxiliary raw materials in addition to the iron-containing raw materials. In this case, as described above, the weighted average value Rs av is the lower limit Rs min The blending ratio of the iron-containing raw materials may be designed so as to satisfy the above. By using the iron-containing raw materials whose blending ratio is designed by the blending ratio design method of this embodiment as blast furnace raw materials in blast furnace operation, the gas permeability in the blast furnace is improved. As described in the first embodiment, one of the reasons for this is considered to be that the cohesive zone on the furnace center side shrinks, and the phenomenon that the reducing gas in the furnace easily passes through the coke layer adjacent to the cohesive layer occurs significantly.
[0102] In the mix design method of this embodiment, the weighted average value Rs av is the lower limit Rs min In addition to the above, the reduction ratio Rs at the start of fusion of multiple types of iron-containing raw materials is expressed by the following formula (5). i It is preferable to design the blend of the multiple types of iron-containing raw materials so that the variation σRs (hereinafter also simply referred to as "variation σRs") of is 10% or less.
[0103]
number
[0104] In the above formula (5), the weighted average value Rs av , Reduction rate at the start of fusion Rsi and mixing ratio M i R is the weighted average value Rs in the above formula (4). av , Reduction rate at the start of fusion Rs i and mixing ratio M i Since these are the same as R, detailed explanations will be omitted.
[0105] The variation σRs can be adjusted by changing the amount of each iron-containing raw material or the type of iron-containing raw material. In other words, the weighted average value Rs av is the lower limit Rs min In addition, designing the mix of iron-containing raw materials so that the variation σRs is 10% or less is the weighted average value Rs av is the lower limit Rs min This means that the blending ratio of the iron-containing raw materials and the type of the iron-containing raw materials are determined so that the above is satisfied and the variation σRs is 10% or less.
[0106] Regarding the composition of iron-containing raw materials, the weighted average value of Rs av is the lower limit Rs min In addition to the above, by having the variation σRs be 10% or less, the permeability in the blast furnace is more likely to be improved than when the variation σRs exceeds 10%.
[0107] In the blending design method of this embodiment, as in the first embodiment, when using iron-containing raw materials (sintered ore) with different sintering raw materials and / or firing conditions or different brands of iron-containing raw materials (lump ore, pellets, carbon-containing agglomerated ore, ferro-coke) even if they are the same type of iron-containing raw materials, it is preferable to set the reduction ratio Rs at the start of fusion and the blending ratio MR for each iron-containing raw material with different sintering raw materials and / or firing conditions or for each iron-containing raw material with different brands. In this case, the weighted average value Rs that more accurately reflects the actual high-temperature properties (reduction ratio Rs at the start of fusion) of the iron-containing raw materials is used. av And the variation σRs becomes easier to find.
[0108] (Blast furnace operation method) In blast furnace operation, a plurality of types of iron-containing raw materials whose mixes are designed by the mix design method of the present embodiment are charged into a blast furnace to form an iron-containing raw material layer in the blast furnace. EXAMPLES
[0109] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to these examples.
[0110] The weighted average reduction rate Rs at the start of fusion for the ore used as blast furnace raw material av The ore raw materials with the designed blends were used as raw materials for the blast furnace, and the internal volume was 3000 to 5500 m 3 The ore raw materials used in each blast furnace were sintered ore, lump ore, and pellets.
[0111] (Combination design 1) The mix design of the blast furnace raw materials (ore raw materials) was carried out for blast furnace A. When carrying out this mix design, the weighted average value Rs av and corrected ventilation resistance index K2 cоr Using the correlation (see Figure 5), the corrected airflow resistance index K2 cоr The lower limit Rs corresponding to the target value min Here, the corrected ventilation resistance index K2 cоr The target value was set at 550[-], and the lower limit Rs min The rate was 65%.
[0112] Weighted average value Rs av is the lower limit Rs min The ore raw material mix was designed so that the reduction ratio Rs at the start of fusion was 65% or more. Specifically, of the three types of ore raw materials mentioned above, the mix ratio MR of the lump ore with a low reduction ratio Rs at the start of fusion was reduced, and the ore was changed to sintered ore with a higher reduction ratio Rs at the start of fusion than the sintered ore before the mix design. The weighted average value Rs before the mix design av is the lower limit Rs min (65%), but the weighted average value after mix design was Rs av is the lower limit Rs min(65%). That is, the weighted average value after mix design Rs av is the weighted average value before mix design Rs av As shown in Figure 9, the corrected air resistance index K2 cоr The results shown in Fig. 9 confirm that the permeability of the blast furnace can be improved by the mix design.
[0113] (Combination design 2) The mix design of the blast furnace raw materials (ore raw materials) was carried out for blast furnace A. When carrying out this mix design, the weighted average value Rs av Using the correlation between the coke ratio CR and the coke ratio CR (see Fig. 6), the lower limit Rs min Here, the target value of the coke ratio CR was set at 285 [kg / t], and the lower limit Rs min The rate was 65%.
[0114] Weighted average value Rs av is the lower limit Rs min The ore raw material mix was designed so that the reduction ratio Rs at the start of fusion was 65% or more. Specifically, of the three types of ore raw materials mentioned above, the mix ratio MR of the lump ore with a low reduction ratio Rs at the start of fusion was reduced, and the ore was changed to sintered ore with a higher reduction ratio Rs at the start of fusion than the sintered ore before the mix design. The weighted average value Rs before the mix design av is the lower limit Rs min (65%), but the weighted average value after mix design was Rs av is the lower limit Rs min (65%). That is, the weighted average value after mix design Rs av is the weighted average value before mix design Rs av This mix design allows the coke ratio (CR) to be reduced, and this reduction in the coke ratio (CR) is due to improved permeability in the blast furnace.
[0115] (Mixture design 3) The mix design of the blast furnace raw materials (ore raw materials) was carried out at blast furnace C. When carrying out this mix design, the weighted average value Rsav Using the correlation between the productivity and the target value of the productivity (see Fig. 7), the lower limit Rs min Here, the target value of the productivity was set at 2.7 [-], and the lower limit Rs min The rate was 65%.
[0116] Weighted average value Rs av is the lower limit Rs min The ore raw material mix was designed so that the reduction ratio Rs at the start of fusion (65%) or more was achieved. Specifically, of the three types of ore raw materials mentioned above, the ore was changed to sintered ore with a higher reduction ratio Rs at the start of fusion than the sintered ore before the mix design, and the mix ratio of the sintered ore after the change was increased. The weighted average value Rs before the mix design av is the lower limit Rs min (65%), but the weighted average value after mix design was Rs av is the lower limit Rs min (65%). That is, the weighted average value after mix design Rs av is the weighted average value before mix design Rs av This mix design allows for an increase in productivity, which is due to improved permeability in the blast furnace.
[0117] On the other hand, for blast furnaces B and C, the weighted average value Rs after mix design was av Although the corrected permeability resistance index K2 of blast furnace B is higher than that of blast furnace C, cоr Therefore, regarding the blending of ore raw materials in blast furnaces B and C, the variation in the reduction rate at the start of melting of the ore raw materials, σRs, and the corrected permeability resistance index, K2 cоr The relationship between these two is shown in Figure 12.
[0118] As shown in Fig. 12, in blast furnace C, the variation σRs was 10% or less for all blends, whereas in blast furnace B, the variation σRs exceeded 10% for most blends. av is the lower limit Rs minIn addition to the above, it was found that by designing the mix of ore raw materials so that the variation σRs is 10% or less, it is easier to further improve the permeability inside the blast furnace compared to when the mix of ore raw materials is designed so that the variation σRs exceeds 10%. [Explanation of symbols]
[0119] 1 blast furnace 2 Charge 3 Coke layer 4. Iron-containing raw material layer 5 Fusion layer 6. Cohesive layer and adjacent coke layer 7 Tuyere 8 Raceway 9 Dripping molten iron 10 hearth bottom 11 Lower Furnace 12 Upper Furnace 13 Graphite crucible 14 Ore Layer 15 Upper furnace heater control means 16 Lower furnace heater control means 17 Gas 18 Post-reduction gas 19 Loading machine 20 Dripping molten iron receiver 21 Coke layer H Upper Furnace Heater H' Lower Furnace Heater
Claims
1. A method for designing a mixture of a plurality of types of iron-containing raw materials forming an iron-containing raw material layer in a blast furnace, comprising: The weighted average value Rs of the reduction rates at the start of fusion of the plurality of types of iron-containing raw materials is represented by the following formula (I): av is the lower limit Rs min The composition of the iron-containing raw materials is designed so as to satisfy the above. The lower limit value Rs min is at least one parameter selected from the air permeability index, the coke ratio, and the productivity of the blast furnace, which are determined in advance based on the track record of stable operation of the blast furnace, and the weighted average value Rs av The weighted average value Rs corresponding to the target value of the parameter in correlation with av A method for designing a blend of iron-containing raw materials, comprising: [0010] In the above formula (I), i is the type of iron-containing raw material, Rs i is the reduction rate [%] of the iron-containing raw material of type i at the start of fusion, M i R is the blending ratio [mass %] of type i of iron-containing raw material to all types of iron-containing raw materials.
2. The weighted average values Rs each corresponding to the target values of two or more of the parameters av The highest value among them is the lower limit Rs min The method for designing a blend of iron-containing raw materials according to claim 1, characterized in that the blend is determined as follows:
3. The blending design method of the iron-containing raw materials according to claim 1 or 2, further comprising designing a blend of the plurality of types of the iron-containing raw materials so that a variation σRs of the reduction rates at the start of fusion of the plurality of types of the iron-containing raw materials, represented by the following formula (II), is 10% or less. [0025] In the above formula (II), i is the type of iron-containing raw material, Rs i is the reduction rate [%] of the iron-containing raw material of type i at the start of fusion, Rs av is the weighted average value [%] of the reduction rates at the start of fusion of the plurality of types of iron-containing raw materials, M i R is the blending ratio [mass %] of type i of iron-containing raw material to all types of iron-containing raw materials.
4. One type of the iron-containing raw material among the plurality of types of iron-containing raw materials is composed of a plurality of lump ores of different brands, The reduction rate Rs of the lump ore at the start of fusion i is the reduction rate at the start of fusion for each brand, The blending ratio M of the lump ore i R is the blending ratio for each brand, 4. The method for designing a blend of iron-containing raw materials according to claim 1 .
5. One type of iron-containing raw material among the plurality of types of iron-containing raw materials is composed of a plurality of pellets of different brands, The reduction rate Rs of the pellets at the start of fusion i is the reduction rate at the start of fusion for each brand, The blending ratio M of the pellets i R is the blending ratio for each brand, 5. The method for designing a blend of iron-containing raw materials according to claim 1 .
6. One type of iron-containing raw material among the plurality of types of iron-containing raw materials is composed of a plurality of sintered ores having different sintering raw materials and / or sintering conditions, The reduction rate Rs of the sintered ore at the start of fusion i is the reduction rate at the start of fusion for each of the sintered ores having different sintering raw materials and / or firing conditions, The blending ratio M of the sintered ore i R is the blending ratio of the sintered ore having different sintering raw materials and / or firing conditions; 6. The method for designing a blend of iron-containing raw materials according to claim 1 .
7. A method for operating a blast furnace, comprising charging a plurality of types of iron-containing raw materials, the composition of which is designed by the method for designing the composition of iron-containing raw materials according to any one of claims 1 to 6, into the blast furnace to form an iron-containing raw material layer.
Citation Information
Patent Citations
Ore quality judgement and blast furnace operation
JP1979131519A
Operation of blast furnace
JP1994256818A
Method for charging sintered ore into blast furnace
JP2002309306A
Method for operating blast furnace
JP2005272968A
Blast furnace operation method
JP2011099150A