Glass composition for glass fiber, glass fiber, glass fiber fabric, and glass fiber reinforced resin composition
A glass composition with optimized SiO2, B2O3, Al2O3, MgO, CaO, SrO, and TiO2 ratios addresses striae and dielectric loss issues, ensuring stable glass fiber production with reduced breakage and enhanced mechanical properties.
Patent Information
- Application Number
- JP2022514310
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-10
- Filing Date
- 2020-12-24
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2040-12-24
AI Technical Summary
Glass fibers produced from certain compositions break during spinning due to striae formation, which is caused by variations in temperature and composition within the glass melting furnace, leading to reduced production efficiency and increased dielectric loss.
A glass composition with specific ratios of SiO2, B2O3, Al2O3, MgO, CaO, SrO, and TiO2, formulated to satisfy certain mathematical relationships, which reduces dielectric loss, suppresses phase separation, and minimizes striae formation, allowing for stable fiber production even with large bushings.
The composition achieves low dielectric loss, suppresses phase separation, and reduces striae, enabling efficient production of glass fibers with improved mechanical strength and reduced breakage during spinning.
Smart Images

Figure 0007560761000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass composition for glass fibers, a glass fiber made of the glass composition for glass fibers, a glass fiber fabric containing the glass fiber, and a glass fiber reinforced resin composition containing the glass fiber. [Background technology]
[0002] Glass fibers are produced by melting glass raw materials prepared to obtain a glass composition for glass fibers having a desired composition in a glass melting furnace to obtain molten glass (a melt of the glass composition for glass fibers), discharging the molten glass from a container (bushing) having a nozzle plate with several to several thousand nozzle tips, and winding it up at high speed to stretch it while cooling and solidifying it into a fiber (hereinafter, this operation may be referred to as "spinning"). The bushing is made of a precious metal such as platinum.
[0003] Conventionally, glass fibers have been widely used in various applications to improve the strength of resin molded articles, and the resin molded articles are increasingly being used in housings or parts of electronic devices such as servers, smartphones, and notebook computers.
[0004] Generally, glass absorbs energy from an alternating current as heat, and therefore, when the resin molded article is used for the housing or parts of the electronic device, the resin molded article generates heat, which is a problem.
[0005] Here, the dielectric loss energy absorbed by glass is proportional to the dielectric constant and dielectric loss tangent determined by the components and structure of the glass, and is expressed by the following formula (A).
[0006] W=kfv 2 ×ε 1 / 2 ×tan δ (A) where W is the dielectric loss energy, k is a constant, f is frequency, and v 2is the potential gradient, ε is the dielectric constant, and tan δ is the dielectric tangent. From formula (A), it can be seen that the larger the dielectric constant and the dielectric tangent, and the higher the frequency, the larger the dielectric loss and the greater the heat generation of the resin molded product.
[0007] In recent years, in response to an increase in the frequency (f in the formula (A)) of the alternating current used in the housings or parts of the electronic devices, a lower dielectric constant and a lower dielectric loss tangent are required for the glass fibers used in the housings or parts of the electronic devices in order to reduce dielectric loss energy. In particular, a low dielectric loss tangent is required because it has a greater effect on the formula (A) than the dielectric constant raised to the power of 1 / 2.
[0008] In response to such demands, the applicant proposed a glass composition for glass fiber that has a low dielectric constant and a low dielectric loss tangent, and in order to enable efficient glass fiberization, the occurrence of phase separation is suppressed, and further, the viscosity at high temperatures is reduced, the glass composition for glass fiber containing, relative to the total amount of the glass composition for glass fiber, SiO2 in the range of 52.0 to 59.5 mass%, B2O3 in the range of 17.5 to 25.5 mass%, Al2O3 in the range of 9.0 to 14.0 mass%, SrO in the range of 0.5 to 6.0 mass%, MgO in the range of 1.0 to 5.0 mass%, CaO in the range of 1.0 to 5.0 mass%, and F2 and Cl2 in the range of 0.1 to 3.0 mass% in total (see Patent Document 1). Note that phase separation is a phase separation phenomenon in which a single-phase glass forms a glass phase with a different composition due to heat or the like. When phase separation occurs, the chemical durability of the glass fiber decreases, and when the phase separation occurs significantly, it becomes difficult to fiberize the molten glass. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Patent No. 6468409 Summary of the Invention [Problem to be solved by the invention]
[0010] However, when glass fibers formed from the glass composition for glass fibers of Patent Document 1 are industrially mass-produced using a glass melting furnace equipped with a bushing that requires a nozzle plate having 100 or more nozzle tips formed thereon, there is a problem in that the glass fibers are broken during spinning, reducing production efficiency.
[0011] The present inventors have conducted extensive research into the reasons for the above-mentioned inconveniences and found that the breakage of glass fibers during spinning is due to the occurrence of striae. Here, in a glass melting furnace equipped with a small bushing having a nozzle plate with less than 100 nozzle tips, the volume of the glass melting furnace is small according to the size of the bushing, and the temperature in the glass melting furnace and the amount of volatilization of glass raw materials are relatively uniform. On the other hand, when a glass melting furnace equipped with a large bushing requiring a nozzle plate with 100 or more nozzle tips is used, the volume of the glass melting furnace is also large according to the size of the bushing, so that the temperature in the glass melting furnace and the amount of volatilization of glass raw materials may vary, and these variations cause deviations in the glass composition. Different types of glass created by this deviation become streaky during the melting process, and striae appear as differences in the refractive index in the glass. When striae occur, when the molten glass is discharged from the bushing and drawn by being wound up at high speed, a difference in viscosity is generated due to a difference in composition in the portion where the striae occur, and this difference in viscosity inhibits the drawing of the molten glass, presumably making the glass fibers more susceptible to breakage during spinning.
[0012] The present invention aims to provide a glass composition for glass fiber that overcomes these disadvantages, has a low dielectric tangent, inhibits the occurrence of phase separation, reduces viscosity at high temperatures, and further reduces the occurrence of striae. Another object of the present invention is to provide a glass fiber formed from the glass composition for glass fiber, a glass fiber fabric containing the glass fiber, and a glass fiber reinforced resin composition using the glass fiber. [Means for solving the problem]
[0013] In order to achieve this object, the glass composition for glass fiber of the present invention contains SiO2 in a range of 52.0 mass % or more and 57.5 mass % or less based on the total amount of the glass composition for glass fiber, 23.8 The composition contains B2O3 in a range of 25.5% by mass or more, Al2O3 in a range of 8.0% by mass or more and 13.0% by mass or less, MgO in a range of 0% by mass or more and 2.0% by mass or less, CaO in a range of 0% by mass or more and 6.0% by mass or less, SrO in a range of 0.5% by mass or more and 6.5% by mass or less, and TiO2 in a range of 0.1% by mass or more and 3.0% by mass or less, and the ratio of the Al2O3 content (mass%) to the B2O3 content (mass%) is in a range of 0.35 to 0.54, and the SiO2 content (mass%) SI, the B2O3 content (mass%) B, the MgO content (mass%) M, the CaO content (mass%) C, the SrO content (mass%) SR, and the TiO2 content (mass%) T satisfy the following formula (1).
[0014] 6.90≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2 / 3 ×{T / (M+T)} 1 / 2 ≦12.30 (1) According to the glass composition for glass fiber of the present invention, when it contains SiO2, B2O3, Al2O3, MgO, CaO, SrO, and TiO2 in the above-mentioned ranges, and the ratio of the Al2O3 content to the B2O3 content is in the above-mentioned range, and the above formula (1) is satisfied, it has a low dielectric tangent, the occurrence of phase separation is suppressed, the viscosity at high temperatures is reduced, and further the occurrence of striae is reduced.
[0015] Here, "having a low dielectric tangent" means that the dielectric tangent is 0.0018 or less at a frequency of 10 GHz, and "having reduced viscosity at high temperatures" means that the 1000 poise temperature (the temperature at which the viscosity of molten glass is 1000 poise (100 Pa s)) is 1375°C or less.
[0016] In the glass composition for glass fiber of the present invention, it is preferable that the SI, B, M, C, SR and T satisfy the following formula (2). 9.56≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2 / 3 ×{T / (M+T)} 1 / 2 ≦11.77 (2) When the SI, B, M, C, SR and T satisfy the formula (2), the glass composition for glass fiber of the present invention has a low dielectric tangent more reliably, the occurrence of phase separation is more reliably suppressed, the viscosity at high temperatures is more reliably reduced, and further, the occurrence of striae is more reliably reduced.
[0017] In the glass composition for glass fiber of the present invention, it is more preferable that the SI, B, M, C, SR and T satisfy the following formula (3).
[0018] 10.00≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2 / 3 ×{T / (M+T)} 1 / 2 ≦11.35 (3) When the SI, B, M, C, SR, and T satisfy the above formula (3), the glass composition for glass fiber of the present invention has a lower dielectric tangent, the occurrence of phase separation is more reliably suppressed, the viscosity at high temperatures is more reliably reduced, and the occurrence of striae is further reduced.
[0019] Here, having a lower dielectric tangent means that the dielectric tangent is 0.0017 or less at a frequency of 10 GHz.
[0020] In the glass composition for glass fiber of the present invention, it is particularly preferable that the SI, B, M, C, SR and T satisfy the following formula (4).
[0021] 10.15≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2 / 3 ×{T / (M+T)} 1 / 2 ≦10.85 (4) When the SI, B, M, C, SR, and T satisfy the above formula (4), the glass composition for glass fiber of the present invention more reliably has a lower dielectric tangent, more reliably suppresses the occurrence of phase separation, more reliably reduces the viscosity at high temperatures, and more reliably reduces the occurrence of striae.
[0022] Here, the viscosity at high temperatures being further reduced means that the 1000 poise temperature (the temperature at which the viscosity of the molten glass is 1000 poise (100 Pa·s)) is less than 1370°C.
[0023] Furthermore, in the glass composition for glass fiber of the present invention, it is most preferable that the SI, B, M, C, SR and T satisfy the following formula (5).
[0024] 10.35≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2 / 3 ×{T / (M+T)} 1 / 2 ≦10.78 (5) When the SI, B, M, C, SR, and T satisfy the formula (5), the glass composition for glass fiber of the present embodiment more reliably has a lower dielectric tangent, more reliably suppresses the occurrence of phase separation, more reliably reduces the viscosity at high temperatures, and more reliably reduces the occurrence of striae.
[0025] The glass fiber of the present invention is made of the glass composition for glass fiber of the present invention described above. The glass fiber of the present invention can be obtained, for example, by melting the glass composition for glass fiber of the present invention described above, discharging the resulting molten material from a bushing having 1 to 8,000 nozzle tips or a nozzle plate having holes formed therein, and cooling and solidifying the material while stretching it by winding it up at high speed to form it into a fibrous shape. Therefore, the glass fiber of the present invention has the same glass composition as the glass composition for glass fiber of the present invention described above.
[0026] The glass fiber fabric of the present invention contains the above-mentioned glass fiber of the present invention.
[0027] The glass fiber reinforced resin composition of the present invention contains the above-mentioned glass fiber of the present invention. For example, the glass fiber reinforced resin composition of the present invention contains 10 to 90 mass % of glass fiber with respect to the total amount of the glass fiber reinforced resin composition in a glass fiber reinforced resin composition containing a resin (thermoplastic resin or thermosetting resin), glass fiber, and other additives. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Next, the embodiment of the present invention will be described in more detail.
[0029] The glass composition for glass fiber of the present embodiment contains SiO2 in a range of 52.0 mass% or more and 57.5 mass% or less based on the total amount of the glass composition for glass fiber, 23.8 % or more and 25.5% or less by mass, Al2O3 in the range of 8.0% by mass or more and 13.0% by mass or less, MgO in the range of 0% by mass or more and 2.0% by mass or less, CaO in the range of 0% by mass or more and 6.0% by mass or less, SrO in the range of 0.5% by mass or more and 6.5% by mass or less, and TiO2 in the range of 0.1% by mass or more and 3.0% by mass or less, wherein a ratio of the Al2O3 content (mass%) to the B2O3 content (mass%) is in the range of 0.35 to 0.54, and the SiO2 content (mass%) SI, the B2O3 content (mass%) B, the MgO content (mass%) M, the CaO content (mass%) C, the SrO content (mass%) SR, and the TiO2 content (mass%) T satisfy the above formula (1). In addition, according to the glass composition for glass fiber, when it contains SiO2, B2O3, Al2O3, MgO, CaO, SrO, and TiO2 in the above-mentioned ranges, and the ratio of the Al2O3 content to the B2O3 content is in the above-mentioned range, and the above formula (1) is satisfied, it has a low dielectric tangent, the occurrence of phase separation is suppressed, the viscosity at high temperatures is reduced, and further the occurrence of striae is reduced.
[0030] In the glass composition for glass fiber of this embodiment, if the content of SiO2 is less than 52.0% by mass based on the total amount of the glass composition for glass fiber, the mechanical strength of the glass fiber formed from the glass composition for glass fiber is significantly reduced, and the function of the glass fiber as a reinforcing material in the glass fiber reinforced resin composition is impaired. In addition, the glass fiber is easily deteriorated when placed in an acidic environment. On the other hand, if the content of SiO2 is more than 57.5% by mass based on the total amount of the glass composition for glass fiber, the viscosity at high temperatures increases, so the temperature for melting the glass raw material increases, and from the viewpoint of production costs, it becomes unsuitable for industrial glass fiber production using a glass melting furnace equipped with a bushing that requires a nozzle plate formed with 100 or more nozzle tips.
[0031] In the glass composition for glass fiber of this embodiment, the content of SiO2 relative to the total amount of the glass composition for glass fiber is preferably 52.5 mass% or more and 55.5 mass% or less, more preferably 53.1 mass% or more and 55.0 mass% or less, even more preferably 53.3 mass% or more and 54.7 mass% or less, particularly preferably 53.5 mass% or more and 54.3 mass% or less, and most preferably 53.6 mass% or more and 54.2 mass% or less.
[0032] The glass composition for glass fiber of the present embodiment has a B2O3 content relative to the total amount of the glass composition for glass fiber. 23.8 If the content of B2O3 is less than 25.5% by mass, the dielectric loss tangent of the glass composition for glass fiber cannot be sufficiently reduced. On the other hand, if the content of B2O3 exceeds 25.5% by mass based on the total amount of the glass composition for glass fiber, the occurrence of phase separation cannot be sufficiently suppressed regardless of the contents of other components.
[0033] In the glass composition for glass fiber of this embodiment, the content of B2O3 relative to the total amount of the glass composition for glass fiber is: 23.8 It is preferable that the content is 24.8% by mass or more and 24.8% by mass or less. 23.8 More preferably, the content is 24.7% by mass or more and 24.7% by mass or less. 23.8 It is more preferable that the content is 24.6% by mass or more and 24.6% by mass or less.23.8 It is particularly preferable that the content is 24.5% by mass or more and 24.5% by mass or less. 23.8 It is most preferable that the content is 24.4% by mass or more and 24.4% by mass or less.
[0034] In the glass composition for glass fiber of this embodiment, if the content of Al2O3 is less than 8.0 mass% relative to the total amount of the glass composition for glass fiber, the occurrence of phase separation cannot be sufficiently suppressed regardless of the contents of other components. On the other hand, if the content of Al2O3 is more than 13.0 mass% relative to the total amount of the glass composition for glass fiber, the dielectric loss tangent of the glass composition for glass fiber cannot be sufficiently reduced.
[0035] In the glass composition for glass fiber of this embodiment, the content of Al2O3 relative to the total amount of the glass composition for glass fiber is preferably 11.1 mass% or more and 12.9 mass% or less, more preferably 11.4 mass% or more and 12.8 mass% or less, even more preferably 11.6 mass% or more and 12.7 mass% or less, particularly preferably 11.9 mass% or more and 12.6 mass% or less, and most preferably 12.0 mass% or more and 12.5 mass% or less.
[0036] In the glass composition for glass fiber of this embodiment, if the content of MgO exceeds 2.0 mass % based on the total amount of the glass composition for glass fiber, the occurrence of striae cannot be sufficiently reduced regardless of the contents of other components.
[0037] In the glass composition for glass fiber of this embodiment, the content of MgO relative to the total amount of the glass composition for glass fiber is preferably 0 mass% or more and 1.4 mass% or less, more preferably 0 mass% or more and 1.1 mass% or less, even more preferably 0 mass% or more and 0.9 mass% or less, particularly preferably 0 mass% or more and 0.7 mass% or less, and most preferably 0 mass% or more and 0.5 mass% or less.
[0038] In the glass composition for glass fiber of this embodiment, if the CaO content exceeds 6.0 mass% based on the total amount of the glass composition for glass fiber, the dielectric tangent of the glass composition for glass fiber cannot be sufficiently reduced while suppressing the occurrence of phase separation.
[0039] In the glass composition for glass fiber of this embodiment, the content of CaO relative to the total amount of the glass composition for glass fiber is preferably 1.5 mass% or more and 5.5 mass% or less, more preferably 2.0 mass% or more and 5.3 mass% or less, even more preferably 2.5 mass% or more and 5.2 mass% or less, particularly preferably 2.8 mass% or more and 5.1 mass% or less, especially preferably 3.0 mass% or more and 5.0 mass% or less, and most preferably 3.0 mass% or more and 4.9 mass% or less.
[0040] In the glass composition for glass fiber of this embodiment, if the content of SrO relative to the total amount of the glass composition for glass fiber is less than 0.5 mass % or exceeds 6.5 mass %, the dielectric tangent of the glass composition for glass fiber cannot be sufficiently reduced.
[0041] In the glass composition for glass fiber of this embodiment, the content of SrO relative to the total amount of the glass composition for glass fiber is preferably 1.5 mass% or more and 6.0 mass% or less, more preferably 2.0 mass% or more and 5.5 mass% or less, even more preferably 2.2 mass% or more and 5.3 mass% or less, particularly preferably 2.3 mass% or more and 5.2 mass% or less, especially preferably 2.5 mass% or more and 4.7 mass% or less, and most preferably 2.8 mass% or more and 4.5 mass% or less.
[0042] In the glass composition for glass fiber of this embodiment, if the content of TiO2 is less than 0.1 mass% relative to the total amount of the glass composition for glass fiber, the viscosity at high temperatures increases, so that the temperature for melting the glass raw material increases, and from the viewpoint of production costs, the glass composition is not suitable for industrial glass fiber production using a glass melting furnace equipped with a bushing that requires a nozzle plate having 100 or more nozzle tips. On the other hand, if the content of TiO2 exceeds 3.0 mass% relative to the total amount of the glass composition for glass fiber, the dielectric loss tangent of the glass composition for glass fiber cannot be sufficiently reduced.
[0043] In the glass composition for glass fiber of this embodiment, the content of TiO2 relative to the total amount of the glass composition for glass fiber is preferably 0.2 mass% or more and 2.8 mass% or less, more preferably 0.2 mass% or more and 2.7 mass% or less, even more preferably 0.3 mass% or more and 2.6 mass% or less, particularly preferably 0.4 mass% or more and 2.5 mass% or less, and most preferably 0.5 mass% or more and 2.0 mass% or less.
[0044] The glass composition for glass fiber of this embodiment may contain F2 and Cl2 in a total amount within a range of 0.1 mass % or more and 2.0 mass % or less based on the total amount of the glass composition for glass fiber. When F2 and Cl2 are contained in this range in the glass composition for glass fiber of this embodiment, they contribute to reducing viscosity at high temperatures. On the other hand, if the glass composition for glass fiber contains F2 and Cl2 in a total amount exceeding 2.0 mass %, the chemical durability of the glass composition for glass fiber may be deteriorated.
[0045] When the glass composition for glass fiber of the present embodiment contains F2 and Cl2, the total content of F2 and Cl2 relative to the total amount of the glass composition for glass fiber is preferably 0.2 mass% or more and 1.8 mass% or less, more preferably 0.5 mass% or more and 1.5 mass% or less, even more preferably 0.6 mass% or more and 1.4 mass% or less, particularly preferably 0.7 mass% or more and 1.3 mass% or less, especially preferably 0.8 mass% or more and 1.2 mass% or less, and most preferably 0.8 mass% or more and 1.0 mass% or less.
[0046] When the glass composition for glass fiber of this embodiment contains F2, the content of F2 relative to the total amount of the glass composition for glass fiber is preferably 0.2 mass% or more and 1.8 mass% or less, more preferably 0.5 mass% or more and 1.5 mass% or less, even more preferably 0.6 mass% or more and 1.4 mass% or less, particularly preferably 0.7 mass% or more and 1.3 mass% or less, especially preferably 0.8 mass% or more and 1.2 mass% or less, and most preferably 0.8 mass% or more and 1.0 mass% or less.
[0047] When the glass composition for glass fiber of the present embodiment contains 0.4 mass % or more of F2, it may not contain substantially any Cl2 (that is, the content of Cl2 may be less than 0.01 mass %).
[0048] The glass composition for glass fiber of the present embodiment may contain ZnO in a range of 0 to 3.0 mass % based on the total amount of the glass composition for glass fiber. When the glass composition for glass fiber of the present embodiment contains ZnO, if the ZnO content exceeds 3.0 mass %, devitrification is likely to occur, making it impossible to stably produce glass fibers.
[0049] When the glass composition for glass fiber of the present embodiment contains ZnO, the content of ZnO relative to the total amount of the glass composition for glass fiber is preferably 2.5 mass% or less, more preferably 1.5 mass% or less, and even more preferably 0.5 mass% or less.
[0050] The glass composition for glass fiber of this embodiment may contain Fe2O3 in a range of 0 mass % or more and 1.0 mass % or less based on the total amount of the glass composition for glass fiber. When the glass composition for glass fiber of this embodiment contains Fe2O3, it is effective to set the content of Fe2O3 in a range of 0.1 mass % or more and 0.6 mass % or less from the viewpoint of suppressing bubbles contained in the glass fiber.
[0051] The glass composition for glass fiber of this embodiment may contain SnO2 in a range of 0 mass % or more and 1.0 mass % or less based on the total amount of the glass composition for glass fiber. When the glass composition for glass fiber of this embodiment contains SnO2, it is effective to set the SnO2 content in a range of 0.1 mass % or more and 0.6 mass % or less from the viewpoint of suppressing bubbles contained in the glass fiber.
[0052] In the glass composition for glass fiber of this embodiment, so long as the total content of Na2O, K2O and Li2O is less than 1.0 mass% and the content of each component is less than 0.4 mass% based on the total amount of the glass composition for glass fiber, Na2O, K2O or Li2O may be contained. If the total content of Na2O, K2O and Li2O is 1.0 mass% or more, or the content of each component is 0.4 mass% or more based on the total amount of the glass composition for glass fiber, the dielectric constant and dielectric loss tangent of the glass composition for glass fiber are significantly deteriorated.
[0053] In the glass composition for glass fiber of this embodiment, ZrO2 may be contained as long as the content of ZrO2 is less than 0.4 mass% based on the total amount of the glass composition for glass fiber. If the content of ZrO2 is 0.4 mass% or more based on the total amount of the glass composition for glass fiber, devitrification is likely to occur, making it impossible to stably manufacture glass fibers.
[0054] In the glass composition for glass fiber of this embodiment, Cr2O3 may be contained as long as the Cr2O3 content is less than 0.05 mass% based on the total amount of the glass composition for glass fiber. If the Cr2O3 content is 0.05 mass% or more based on the total amount of the glass composition for glass fiber, devitrification is likely to occur, making it impossible to stably manufacture glass fibers.
[0055] The glass composition for glass fiber of this embodiment may contain oxides of Ba, P, Mn, Co, Ni, Cu, Mo, W, Ce, Y, and La in total, relative to the total amount of the glass composition for glass fiber, as impurities derived from raw materials. In particular, when the glass composition for glass fiber of this embodiment contains BaO, P2O5, CeO2, Y2O3, or La2O3 as an impurity, the content thereof is preferably less than 0.40 mass%, more preferably less than 0.20 mass%, even more preferably less than 0.10 mass%, particularly preferably less than 0.05 mass%, and most preferably less than 0.01 mass%.
[0056] Furthermore, when the glass composition for glass fiber of this embodiment contains Bi2O3, Gd2O3, Pr2O3, Sc2O3, or Yb2O3 as an impurity derived from the raw materials, the content thereof is each independently preferably less than 0.10 mass%, more preferably less than 0.05 mass%, and even more preferably less than 0.01 mass%.
[0057] In the glass composition for glass fiber of this embodiment, the total content of SiO2, B2O3, Al2O3, MgO, CaO, SrO and TiO2 is 97.0 mass% or more, preferably 97.5 mass% or more, more preferably 98.0 mass% or more, even more preferably 98.5 mass% or more, particularly preferably 98.8 mass% or more, and most preferably 99.0 mass%.
[0058] In the glass composition for glass fiber of this embodiment, the ratio (Al2O3 / B2O3) of the Al2O3 content (mass%) to the B2O3 content (mass%) is in the range of 0.35 to 0.54. If the ranges of the B2O3 content and the Al2O3 content are within the above-mentioned ranges and Al2O3 / B2O3 is less than 0.35, the occurrence of phase separation cannot be sufficiently suppressed. On the other hand, if the ranges of the B2O3 content and the Al2O3 content are within the above-mentioned ranges and Al2O3 / B2O3 is more than 0.54, the dielectric tangent cannot be sufficiently reduced or the occurrence of striae cannot be sufficiently reduced.
[0059] In the glass composition for glass fiber of this embodiment, the ratio of the Al2O3 content (mass%) to the B2O3 content (mass%) (Al2O3 / B2O3) is preferably in the range of 0.49 to 0.53, more preferably in the range of 0.50 to 0.53, and even more preferably in the range of 0.50 to 0.52.
[0060] In the glass composition for glass fiber of this embodiment, the SiO2 content (mass%) SI, the B2O3 content (mass%) B, the MgO content (mass%) M, the CaO content (mass%) C, the SrO content (mass%) SR, and the TiO2 content (mass%) T satisfy the following formula (1).
[0061] 6.90≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2 / 3 ×{T / (M+T)} 1 / 2 ≦12.30 (1) When the SI, B, M, C, SR, and T satisfy the formula (1), the glass composition for glass fiber of the present embodiment has a low dielectric tangent, the occurrence of phase separation is suppressed, the viscosity at high temperatures is reduced, and further, the occurrence of striae is reduced.
[0062] In the glass composition for glass fiber of the present embodiment, it is preferable that the SI, B, M, C, SR and T satisfy the following formula (2).
[0063] 9.56≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2 / 3 ×{T / (M+T)} 1 / 2 ≦11.77 (2) When the SI, B, M, C, SR, and T satisfy the formula (2), the glass composition for glass fiber of the present embodiment is more reliably provided with a low dielectric tangent, the occurrence of phase separation is more reliably suppressed, the viscosity at high temperatures is more reliably reduced, and further, the occurrence of striae is more reliably reduced.
[0064] When the SI, B, M, C, SR, and T satisfy the formula (2), the glass composition for glass fiber of the present embodiment contains SiO2 in a range of 53.1 mass% or more and 55.0 mass% or less based on the total amount of the glass composition for glass fiber, 23.8 It is preferable that the composition contains B2O3 in the range of 24.8% by mass or more, Al2O3 in the range of 11.1% by mass or more and 12.9% by mass or less, MgO in the range of 0% by mass or more and 1.4% by mass or less, CaO in the range of 1.5% by mass or more and 5.5% by mass or less, SrO in the range of 1.5% by mass or more and 6.0% by mass or less, and TiO2 in the range of 0.4% by mass or more and 2.5% by mass or less, and the ratio of the Al2O3 content (mass%) to the B2O3 content (mass%) (Al2O3 / B2O3) is in the range of 0.49 to 0.53.
[0065] In the glass composition for glass fiber of the present embodiment, it is more preferable that SI, B, M, C, SR and T satisfy the following formula (3).
[0066] 10.00≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2 / 3 ×{T / (M+T)} 1 / 2 ≦11.35 (3) When the SI, B, M, C, SR, and T satisfy the formula (3), the glass composition for glass fiber of the present embodiment has a lower dielectric tangent, the occurrence of phase separation is more reliably suppressed, the viscosity at high temperatures is more reliably reduced, and further, the occurrence of striae is more reliably reduced.
[0067] When the SI, B, M, C, SR, and T satisfy the formula (3), the glass composition for glass fiber of the present embodiment contains SiO2 in a range of 53.1 mass% or more and 55.0 mass% or less based on the total amount of the glass composition for glass fiber, 23.8It is preferable that the composition contains B2O3 in the range of 24.8% by mass or more, Al2O3 in the range of 11.1% by mass or more and 12.9% by mass or less, MgO in the range of 0% by mass or more and 1.4% by mass or less, CaO in the range of 2.5% by mass or more and 5.5% by mass or less, SrO in the range of 2.5% by mass or more and 4.7% by mass or less, and TiO2 in the range of 0.4% by mass or more and 2.5% by mass or less, and the ratio of the Al2O3 content (mass%) to the B2O3 content (mass%) (Al2O3 / B2O3) is in the range of 0.50 to 0.53.
[0068] In the glass composition for glass fiber of the present embodiment, it is particularly preferable that the SI, B, M, C, SR and T satisfy the following formula (4).
[0069] 10.15≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2 / 3 ×{T / (M+T)} 1 / 2 ≦10.85 (4) When the SI, B, M, C, SR, and T satisfy the formula (4), the glass composition for glass fiber of the present embodiment more reliably has a lower dielectric tangent, more reliably suppresses the occurrence of phase separation, more reliably reduces the viscosity at high temperatures, and more reliably reduces the occurrence of striae.
[0070] When the SI, B, M, C, SR, and T satisfy the formula (4), the glass composition for glass fiber of the present embodiment contains SiO2 in a range of 53.1 mass% or more and 54.3 mass% or less based on the total amount of the glass composition for glass fiber, 23.8 It is preferable that the composition contains B2O3 in the range of 24.5% by mass or more, Al2O3 in the range of 11.6% by mass or more and 12.7% by mass or less, MgO in the range of 0% by mass or more and 1.1% by mass or less, CaO in the range of 2.5% by mass or more and 5.5% by mass or less, SrO in the range of 2.5% by mass or more and 4.7% by mass or less, and TiO2 in the range of 0.4% by mass or more and 2.5% by mass or less, and the ratio of the Al2O3 content (mass%) to the B2O3 content (mass%) (Al2O3 / B2O3) is in the range of 0.50 to 0.53.
[0071] In the glass composition for glass fiber of the present embodiment, it is most preferable that SI, B, M, C, SR and T satisfy the following formula (5).
[0072] 10.35≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2 / 3 ×{T / (M+T)} 1 / 2 ≦10.78 (5) When the SI, B, M, C, SR, and T satisfy the formula (5), the glass composition for glass fiber of the present embodiment more reliably has a lower dielectric tangent, more reliably suppresses the occurrence of phase separation, more reliably reduces the viscosity at high temperatures, and more reliably reduces the occurrence of striae.
[0073] When the SI, B, M, C, SR, and T satisfy the formula (5), the glass composition for glass fiber of the present embodiment contains SiO2 in a range of 53.1 mass% or more and 54.2 mass% or less based on the total amount of the glass composition for glass fiber, 23.8 It is preferable that the composition contains B2O3 in the range of 24.4% by mass or more, Al2O3 in the range of 11.6% by mass or more and 12.5% by mass or less, MgO in the range of 0% by mass or more and 1.1% by mass or less, CaO in the range of 2.5% by mass or more and 5.0% by mass or less, SrO in the range of 3.0% by mass or more and 4.7% by mass or less, and TiO2 in the range of 0.5% by mass or more and 2.5% by mass or less, and that the ratio of the Al2O3 content (mass%) to the B2O3 content (mass%) (Al2O3 / B2O3) is in the range of 0.50 to 0.52.
[0074] In the glass composition for glass fiber of the present embodiment, the content of each of the above-mentioned components can be measured by using an ICP optical emission spectrometer for the light element Li, and by using a wavelength dispersive X-ray fluorescence analyzer for the other elements.
[0075] The measurement method is as follows: first, a glass batch (mixed and prepared by mixing glass raw materials) or glass fiber (when organic matter is attached to the surface of the glass fiber or when the glass fiber is mainly contained as a reinforcing material in the organic matter (resin), the organic matter is removed by, for example, heating in a muffle furnace at 300 to 650 ° C for 0.5 to 24 hours) is placed in a platinum crucible, and in an electric furnace, the glass batch is kept at a temperature of 1550 ° C, and the glass fiber is kept at a temperature of 1400 ° C for 6 hours while being stirred, thereby obtaining homogeneous molten glass. Next, the obtained molten glass is poured onto a carbon plate to produce glass cullet, which is then crushed and powdered to obtain glass powder. For Li, which is a light element, the glass powder is heated and decomposed with acid, and then quantitatively analyzed using an ICP emission spectrometer. For other elements, the glass powder is formed into a disk shape using a press machine, and then quantitatively analyzed using a wavelength dispersive X-ray fluorescence analyzer. The results of these quantitative analyses are converted into oxides to calculate the contents and total amounts of each component, and the contents of each of the above-mentioned components can be obtained from these values.
[0076] The glass composition for glass fiber of the present embodiment can be obtained by melting a glass raw material (glass batch) prepared so as to have the above-mentioned composition after melting and solidifying, and then cooling and solidifying it.
[0077] In the glass composition for glass fiber of the present embodiment, the 1000 poise temperature is in the range of 1330 to 1400°C, preferably in the range of 1340 to 1390°C, more preferably in the range of 1345 to 1380°C, and even more preferably in the range of 1350 to 1375°C. In the glass composition for glass fiber of the present invention, the liquidus temperature (the temperature at which crystals are first precipitated when the temperature of the molten glass is lowered) is in the range of 1050 to 1240°C, preferably in the range of 1100 to 1210°C, more preferably in the range of 1130 to 1200°C, and even more preferably in the range of 1150 to 1195°C. In the glass composition for glass fiber of the present invention, the temperature range between the 1000 poise temperature and the liquidus temperature (working temperature range) is 200°C or higher, preferably in the range of 200 to 400°C, and more preferably in the range of 210 to 360°C.
[0078] When forming the glass fiber of this embodiment from the glass composition for glass fiber of this embodiment, first, the glass raw material prepared as described above is supplied to a glass melting furnace and melted at a temperature range of 1000 poise temperature or higher, specifically, at a temperature in the range of 1450 to 1550° C. Then, the molten glass melted at the above temperature is discharged from 100 to 8000 nozzle tips or holes controlled at a predetermined temperature, and cooled and solidified while being stretched by winding at high speed, thereby forming the glass fiber.
[0079] Here, a glass filament (glass filament) discharged from one nozzle tip or hole and cooled and solidified usually has a perfect circular cross-sectional shape and a diameter of 3.0 to 35.0 μm. For applications requiring low dielectric properties, the glass filament preferably has a diameter of 3.0 to 6.0 μm, more preferably a diameter in the range of 3.0 to 4.5 μm. On the other hand, when the nozzle tip has a non-circular shape and has a protrusion or a notch for quenching the molten glass, a glass filament having a non-circular (e.g., elliptical or oval) cross-sectional shape can be obtained by controlling the temperature conditions. When the glass filament has an elliptical or oval cross-sectional shape, the ratio of the major axis to the minor axis of the cross-sectional shape (major axis / minor axis) is, for example, in the range of 2.0 to 10.0, and the fiber diameter (equivalent fiber diameter) when the cross-sectional area is converted to a perfect circle is in the range of 3.0 to 35.0 μm.
[0080] The glass fiber of the present embodiment is usually in the form of a glass fiber bundle (glass strand) in which 10 to 8000 glass filaments are bundled together, and has a weight in the range of 1 to 10000 tex (g / km). Note that the glass filaments discharged from a plurality of nozzle tips or holes may be bundled into one glass fiber bundle or into a plurality of glass fiber bundles.
[0081] The glass fiber of the present embodiment can take various forms, such as yarn, woven fabric, knitted fabric, nonwoven fabric (including chopped strand mat and multiaxial nonwoven fabric), chopped strand, roving, powder, etc., obtained by further processing the glass strand in various ways.
[0082] The glass fiber of the present embodiment may be coated on its surface with an organic material for the purpose of improving the bundling of glass filaments, improving the adhesion between glass fibers and resin, and improving the uniform dispersion of glass fibers in a mixture of glass fibers and resin or inorganic material. Examples of such organic materials include starch, urethane resin, epoxy resin, vinyl acetate resin, acrylic resin, modified polypropylene (particularly carboxylic acid-modified polypropylene), and copolymers of (poly)carboxylic acid (particularly maleic acid) and unsaturated monomers. The glass fiber of the present embodiment may be coated with a resin composition containing a silane coupling agent, a lubricant, a surfactant, and the like in addition to these resins. The glass fiber of the present embodiment may be coated with a treatment composition containing a silane coupling agent, a surfactant, and the like without containing the above-mentioned resin. Such a resin composition or treatment composition coats the glass fiber at a ratio of 0.03 to 2.0 mass % based on the mass of the glass fiber of the present embodiment in a state in which it is not coated with the resin composition or treatment composition. The coating of glass fibers with an organic substance can be carried out, for example, in the glass fiber manufacturing process by applying a resin solution or a resin composition solution to the glass fibers using a known method such as a roller-type applicator, and then drying the glass fibers to which the resin solution or the resin composition solution has been applied. Alternatively, the coating can be carried out by immersing the glass fibers of the present embodiment in the form of a woven fabric in a treatment composition solution, and then drying the glass fibers to which the treatment composition has been applied.
[0083] Here, examples of the silane coupling agent include aminosilane (γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-N'-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-anilinopropyltrimethoxysilane, etc.), chlorosilane (γ-chloropropyltrimethoxysilane, etc.), epoxysilane (β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, etc.), mercaptosilane (γ-mercaptotrimethoxysilane, etc.), vinylsilane (vinyltrimethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, etc.), and (meth)acrylicsilane (γ-methacryloxypropyltrimethoxysilane, etc.). In this embodiment, the silane coupling agent may be used alone or in combination of two or more.
[0084] Examples of lubricants include modified silicone oils, animal oils (beef tallow, etc.) and their hydrogenated products, vegetable oils (soybean oil, coconut oil, rapeseed oil, palm oil, castor oil, etc.) and their hydrogenated products, animal waxes (beeswax, lanolin, etc.), vegetable waxes (candelilla wax, carnauba wax, etc.), mineral waxes (paraffin wax, montan wax, etc.), condensates of higher saturated fatty acids and higher saturated alcohols (stearic acid esters such as lauryl stearate, etc.), polyethyleneimine, polyalkylpolyamine alkylamide derivatives, fatty acid amides (for example, dehydration condensates of polyethylene polyamines such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, etc., and fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, etc.), and quaternary ammonium salts (alkyltrimethylammonium salts such as lauryltrimethylammonium chloride, etc.). In this embodiment, the lubricants may be used alone or in combination of two or more.
[0085] Examples of the surfactant include a nonionic surfactant, a cationic surfactant, an anionic surfactant, and an amphoteric surfactant. In this embodiment, the surfactant may be used alone or in combination of two or more kinds.
[0086] Examples of nonionic surfactants include ethylene oxide propylene oxide alkyl ethers, polyoxyethylene alkyl ethers, polyoxyethylene-polyoxypropylene-block copolymers, alkyl polyoxyethylene-polyoxypropylene-block copolymer ethers, polyoxyethylene fatty acid esters, polyoxyethylene fatty acid monoesters, polyoxyethylene fatty acid diesters, polyoxyethylene sorbitan fatty acid esters, glycerol fatty acid ester ethylene oxide adducts, polyoxyethylene castor oil ethers, hydrogenated castor oil ethylene oxide adducts, alkylamine ethylene oxide adducts, fatty acid amide ethylene oxide adducts, glycerol fatty acid esters, polyglycerin fatty acid esters, pentaerythritol fatty acid esters, sorbitol fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, polyhydric alcohol alkyl ethers, fatty acid alkanolamides, acetylene glycol, acetylene alcohol, ethylene oxide adducts of acetylene glycol, and ethylene oxide adducts of acetylene alcohol.
[0087] Examples of cationic surfactants include alkyl dimethyl benzyl ammonium chloride, alkyl trimethyl ammonium chloride, alkyl dimethyl ethyl ammonium ethyl sulfate, higher alkyl amine salts (acetates, hydrochlorides, etc.), ethylene oxide adducts of higher alkyl amines, condensates of higher fatty acids and polyalkylene polyamines, salts of esters of higher fatty acids and alkanolamines, salts of higher fatty acid amides, imidazoline-type cationic surfactants, and alkyl pyridinium salts.
[0088] Examples of anionic surfactants include higher alcohol sulfates, higher alkyl ether sulfates, α-olefin sulfates, alkylbenzene sulfonates, α-olefin sulfonates, reaction products of fatty acid halides and N-methyltaurine, dialkyl sulfosuccinates, higher alcohol phosphates, and phosphates of higher alcohol ethylene oxide adducts.
[0089] Examples of the amphoteric surfactant include amino acid type amphoteric surfactants such as alkali metal salts of alkylaminopropionic acid, betaine type amphoteric surfactants such as alkyldimethylbetaine, and imidazoline type amphoteric surfactants.
[0090] The glass fiber fabric of this embodiment contains the glass fiber of this embodiment described above. Specifically, the glass fiber fabric of this embodiment can be obtained by weaving the glass fiber of this embodiment described above as at least a part of the warp or weft using a loom known per se. Examples of the loom include a jet loom such as an air jet or water jet loom, a shuttle loom, and a rapier loom. Examples of the weaving method using the loom include a plain weave, a satin weave, a tanabae weave, and a twill weave, and from the viewpoint of manufacturing efficiency, a plain weave is preferred. The glass fiber fabric of this embodiment preferably uses the glass fiber of this embodiment described above as the warp and weft.
[0091] In the glass fiber fabric of the present embodiment, the glass fiber of the present embodiment described above is preferably formed by bundling 35 to 400 glass filaments having a filament diameter of 3.0 to 9.0 μm, having a twist of 0 to 1.0 turns / 25 mm, and having a mass of 0.9 to 69.0 tex (g / 1000 m).
[0092] In the glass fiber fabric of this embodiment, when the above-described glass fibers of this embodiment are used as warp or weft, the warp weave density is preferably 40 to 120 threads / 25 mm, and the weft weave density is preferably 40 to 120 threads / 25 mm.
[0093] After being woven, the glass fiber fabric of the present embodiment may be subjected to a de-oiling treatment, a surface treatment, and a fiber-opening treatment.
[0094] The deoiling treatment may be performed by placing the glass fiber fabric in a heating furnace with an atmospheric temperature of 350° C. to 400° C. for 40 to 80 hours to thermally decompose the organic matter adhering to the glass fibers.
[0095] The surface treatment may be a treatment in which a glass fiber fabric is immersed in a solution containing the silane coupling agent or the silane coupling agent and the surfactant, excess water is squeezed out, and then the fabric is dried by heating at a temperature in the range of 80 to 180°C for 1 to 30 minutes.
[0096] Examples of the opening process include a process in which a tension of 30 to 200 N is applied to the warp yarns of a glass fiber fabric, and the warp yarns and weft yarns are opened by water flow pressure, opened by high-frequency vibration using a liquid as a medium, opened by pressure of a fluid having surface pressure, or opened by pressure applied by a roll, thereby expanding the yarn width.
[0097] The glass fiber fabric of the present embodiment has a fiber thickness of 7.0 to 190.0 g / m 2 and preferably has a thickness in the range of 8.0 to 200.0 μm.
[0098] In the glass fiber fabric of this embodiment, the yarn width of the warp yarns is preferably 110 to 600 μm, and the yarn width of the weft yarns is preferably 110 to 600 μm.
[0099] The glass fiber fabric of the present embodiment may have a surface treatment layer containing the silane coupling agent, or the silane coupling agent and the surfactant. When the glass fiber fabric of the present embodiment includes the surface treatment layer, the surface treatment layer may have a mass of, for example, 0.03 to 1.50 mass% based on the total mass of the glass fiber fabric including the surface treatment layer.
[0100] The glass fiber reinforced resin composition of this embodiment contains the glass fiber of this embodiment described above. Specifically, the glass fiber reinforced resin composition of this embodiment contains 10 to 90 mass% of glass fiber with respect to the total amount of the glass fiber reinforced resin composition in a glass fiber reinforced resin composition containing a resin (thermoplastic resin or thermosetting resin), glass fiber, and other additives. Moreover, the glass fiber reinforced resin composition of this embodiment contains 90 to 10 mass% of resin with respect to the total amount of the glass fiber reinforced resin composition, and contains other additives in the range of 0 to 40 mass%.
[0101] Here, examples of the thermoplastic resin include polyethylene, polypropylene, polystyrene, styrene / maleic anhydride resin, styrene / maleimide resin, polyacrylonitrile, acrylonitrile / styrene (AS) resin, acrylonitrile / butadiene / styrene (ABS) resin, chlorinated polyethylene / acrylonitrile / styrene (ACS) resin, acrylonitrile / ethylene / styrene (AES) resin, acrylonitrile / styrene / methyl acrylate (ASA) resin, styrene / acrylonitrile (SAN) resin, methacrylic resin, polyvinyl chloride (PVC), polyvinylidene chloride (PVDC), polyamide, polyacetal, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polycarbonate, and the like. Examples of suitable resins include carbonate, polyarylene sulfide, polyethersulfone (PES), polyphenylsulfone (PPSU), polyphenylene ether (PPE), modified polyphenylene ether (m-PPE), polyaryletherketone, liquid crystal polymer (LCP), fluororesin, polyetherimide (PEI), polyarylate (PAR), polysulfone (PSF), polyamideimide (PAI), polyaminobismaleimide (PABM), thermoplastic polyimide (TPI), polyethylene naphthalate (PEN), ethylene / vinyl acetate (EVA) resin, ionomer (IO) resin, polybutadiene, styrene / butadiene resin, polybutylene, polymethylpentene, olefin / vinyl alcohol resin, cyclic olefin resin, cellulose resin, and polylactic acid.
[0102] Specifically, examples of polyethylene include high density polyethylene (HDPE), medium density polyethylene, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), and ultra-high molecular weight polyethylene.
[0103] Examples of polypropylene include isotactic polypropylene, atactic polypropylene, syndiotactic polypropylene, and mixtures thereof.
[0104] Examples of polystyrene include general-purpose polystyrene (GPPS), which is an atactic polystyrene having an atactic structure, high impact polystyrene (HIPS), which is GPPS with a rubber component added, and syndiotactic polystyrene having a syndiotactic structure.
[0105] Examples of the methacrylic resin include a homopolymer of one of acrylic acid, methacrylic acid, styrene, methyl acrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, and a fatty acid vinyl ester, or a copolymer of two or more of them.
[0106] Examples of polyvinyl chloride include vinyl chloride homopolymers polymerized by conventional methods such as emulsion polymerization, suspension polymerization, microsuspension polymerization, and bulk polymerization, copolymers of vinyl chloride monomers with monomers copolymerizable therewith, and graft copolymers in which vinyl chloride monomers are graft polymerized onto a polymer.
[0107] Polyamides include polycaproamide (nylon 6), polyhexamethylene adipamide (nylon 66), polytetramethylene adipamide (nylon 46), polytetramethylene sebacamide (nylon 410), polypentamethylene adipamide (nylon 56), polypentamethylene sebacamide (nylon 510), polyhexamethylene sebacamide (nylon 610), polyhexamethylene dodecamide (nylon 612), polydecamethylene adipamide (nylon 106), polydecamethylene adipamide (nylon 106), polytetramethylene sebacamide (nylon 106), polypentamethylene adipamide (nylon 56), polypentamethylene sebacamide (nylon 510), polyhexamethylene sebacamide (nylon 610), polyhexamethylene dodecamide (nylon 612), polydecamethylene adipamide (nylon 106), polytetramethylene sebac ... Polyethylene sebacamide (nylon 1010), polydecamethylene dodecamide (nylon 1012), polyundecane amide (nylon 11), polyundecamethylene adipamide (nylon 116), polydodecanamide (nylon 12), polyxylene adipamide (nylon XD6), polyxylene sebacamide (nylon XD10), polymeta-xylylene adipamide (nylon MXD6), polypara-xylylene adipamide (nylon PXD6), polytetramethylene terephthalamide (nylon 4T), polypentamethylene terephthalamide (nylon 5T), polyhexamethylene terephthalamide (nylon 6T), polyhexamethylene isophthalamide (nylon 6I), polynonamethylene terephthalamide (nylon 9T), polydecamethylene terephthalamide (nylon 10T), polyundecamethylene terephthalamide (nylon 11T), polydodecamethylene terephthalamide (nylon 12T), polytetramethylene isophthalamide (nylon 4I), polybis( Examples of the polybis(3-methyl-4-aminohexyl)methane terephthalamide (nylon PACMT), polybis(3-methyl-4-aminohexyl)methane isophthalamide (nylon PACMI), polybis(3-methyl-4-aminohexyl)methanendodecamide (nylon PACM12), polybis(3-methyl-4-aminohexyl)methane tetradecamide (nylon PACM14), and the like, or copolymers of two or more of these components, or mixtures thereof, can be mentioned.
[0108] Examples of polyacetals include homopolymers having oxymethylene units as the main repeating units, and copolymers mainly composed of oxymethylene units and containing oxyalkylene units having 2 to 8 adjacent carbon atoms in the main chain.
[0109] Examples of polyethylene terephthalate include polymers obtained by polycondensation of terephthalic acid or a derivative thereof with ethylene glycol.
[0110] Examples of polybutylene terephthalate include polymers obtained by polycondensation of terephthalic acid or a derivative thereof with 1,4-butanediol.
[0111] Examples of polytrimethylene terephthalate include polymers obtained by polycondensation of terephthalic acid or a derivative thereof with 1,3-propanediol.
[0112] Examples of polycarbonates include polymers obtained by a transesterification method in which a dihydroxydiaryl compound is reacted with a carbonate ester such as diphenyl carbonate in a molten state, and polymers obtained by a phosgene method in which a dihydroxyaryl compound is reacted with phosgene.
[0113] Examples of polyarylene sulfide include linear polyphenylene sulfide, crosslinked polyphenylene sulfide which has been polymerized and then cured, polyphenylene sulfide sulfone, polyphenylene sulfide ether, and polyphenylene sulfide ketone.
[0114] Examples of polyphenylene ether include poly(2,3-dimethyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-chloromethyl-1,4-phenylene ether), poly(2-methyl-6-hydroxyethyl-1,4-phenylene ether), poly(2-methyl-6-n-butyl-1,4-phenylene ether), poly(2-ethyl-6-isopropyl-1,4-phenylene ether), poly(2-ethyl-6-n-propyl-1,4-phenylene ether), poly(2,3,6-trimethyl-1,4-phenylene ether), poly[2-(4'-methylphenyl)-1,4-phenylene ether], poly(2-bromo-6-phenyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), poly(2-phenyl-1,4-phenylene ether), poly(2-chloro-1,4-phenylene ether), poly(2-methyl-1,4-phenylene ether), poly(2-chloro-6-ethyl-1,4-phenylene ether), poly(2-chloro-6-bromo-1,4-phenylene ether), poly(2,6-di-n-propyl-1,4-phenylene ether), poly(2-methyl-6-isopropyl-1,4-phenylene ether), poly(2-chloro-6-methyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2,6-dibromo-1,4-phenylene ether), poly(2,6-dichloro-1,4-phenylene ether), poly(2,6-diethyl-1,4-phenylene ether), poly(2,6-dimethyl-1,4-phenylene ether), and the like.
[0115] Examples of modified polyphenylene ethers include a polymer alloy of poly(2,6-dimethyl-1,4-phenylene) ether and polystyrene, a polymer alloy of poly(2,6-dimethyl-1,4-phenylene) ether and a styrene / butadiene copolymer, a polymer alloy of poly(2,6-dimethyl-1,4-phenylene) ether and a styrene / maleic anhydride copolymer, a polymer alloy of poly(2,6-dimethyl-1,4-phenylene) ether and a polyamide, a polymer alloy of poly(2,6-dimethyl-1,4-phenylene) ether and a styrene / butadiene / acrylonitrile copolymer, the polyphenylene ether having a functional group such as an amino group, an epoxy group, a carboxy group, or a styryl group introduced at the polymer chain end, and the polyphenylene ether having a functional group such as an amino group, an epoxy group, a carboxy group, a styryl group, or a methacryl group introduced at the polymer chain side chain.
[0116] Examples of polyaryletherketones include polyetherketone (PEK), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), and polyetheretherketoneketone (PEEKK).
[0117] Examples of liquid crystal polymers (LCPs) include thermotropic liquid crystal polyesters, such as (co)polymers composed of one or more structural units selected from aromatic hydroxycarbonyl units, aromatic dihydroxy units, aromatic dicarbonyl units, aliphatic dihydroxy units, aliphatic dicarbonyl units, and the like.
[0118] Examples of fluororesins include polytetrafluoroethylene (PTFE), perfluoroalkoxy resin (PFA), fluorinated ethylene propylene resin (FEP), fluorinated ethylene tetrafluoroethylene resin (ETFE), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), and ethylene / chlorotrifluoroethylene resin (ECTFE).
[0119] Examples of ionomer (IO) resins include copolymers of olefin or styrene with unsaturated carboxylic acid, in which a portion of the carboxyl groups is neutralized with metal ions.
[0120] Examples of the olefin / vinyl alcohol resin include an ethylene / vinyl alcohol copolymer, a propylene / vinyl alcohol copolymer, a saponified ethylene / vinyl acetate copolymer, and a saponified propylene / vinyl acetate copolymer.
[0121] Examples of the cyclic olefin resin include monocyclic compounds such as cyclohexene, polycyclic compounds such as tetracyclopentadiene, and polymers of cyclic olefin monomers.
[0122] Examples of polylactic acid include poly-L-lactic acid, which is a homopolymer of the L-form, poly-D-lactic acid, which is a homopolymer of the D-form, and stereocomplex polylactic acid, which is a mixture thereof.
[0123] Examples of the cellulose resin include methyl cellulose, ethyl cellulose, hydroxy cellulose, hydroxy methyl cellulose, hydroxy ethyl cellulose, hydroxy ethyl methyl cellulose, hydroxy propyl methyl cellulose, cellulose acetate, cellulose propionate, and cellulose butyrate.
[0124] Examples of the thermosetting resin include unsaturated polyester resin, vinyl ester resin, epoxy (EP) resin, melamine (MF) resin, phenolic resin (PF), urethane resin (PU), polyisocyanate, polyisocyanurate, polyimide (PI), urea (UF) resin, silicone (SI) resin, furan (FR) resin, benzoguanamine (BR) resin, alkyd resin, xylene resin, bismaleimide triazine (BT) resin, and diallyl phthalate resin (PDAP).
[0125] Specifically, the unsaturated polyester resin may be a resin obtained by subjecting an aliphatic unsaturated dicarboxylic acid and an aliphatic diol to an esterification reaction.
[0126] Examples of the vinyl ester resin include bis-based vinyl ester resins and novolac-based vinyl ester resins.
[0127] Epoxy resins include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol E type epoxy resin, bisphenol S type epoxy resin, bisphenol M type epoxy resin (4,4'-(1,3-phenylenediisopridiene) bisphenol type epoxy resin), bisphenol P type epoxy resin (4,4'-(1,4-phenylenediisopridiene) bisphenol type epoxy resin), bisphenol Z type epoxy resin (4,4'-cyclohexydiene bisphenol type epoxy resin), phenol novolac type epoxy resin, cresol novolac type epoxy resin, and tetraphenol group ethane type novolac. type epoxy resins, novolac type epoxy resins having a condensed ring aromatic hydrocarbon structure, biphenyl type epoxy resins, aralkyl type epoxy resins such as xylylene type epoxy resins and phenylaralkyl type epoxy resins, naphthylene ether type epoxy resins, naphthol type epoxy resins, naphthalene diol type epoxy resins, difunctional to tetrafunctional epoxy type naphthalene resins, binaphthyl type epoxy resins, naphthalene aralkyl type epoxy resins, anthracene type epoxy resins, phenoxy type epoxy resins, dicyclopentadiene type epoxy resins, norbornene type epoxy resins, adamantane type epoxy resins, and fluorene type epoxy resins.
[0128] The melamine resin may be a polymer obtained by polycondensation of melamine (2,4,6-triamino-1,3,5-triazine) and formaldehyde.
[0129] Examples of the phenol resin include novolac-type phenol resins such as phenol novolac resin, cresol novolac resin, and bisphenol A-type novolac resin; resol-type phenol resins such as methylol-type resol resin and dimethylene ether-type resol resin; and aryl alkylene-type phenol resins; and the like. One or a combination of two or more of these may be used.
[0130] Urea resins include resins obtained by condensation of urea and formaldehyde.
[0131] The thermoplastic resins or thermosetting resins may be used alone or in combination of two or more kinds.
[0132] Since the glass fiber reinforced resin composition of the present embodiment is used for applications requiring low dielectric properties, the resin is preferably an epoxy resin, a modified polyphenylene ether, a polybutylene terephthalate, a polypropylene, a fluororesin, or a liquid crystal polymer (LCP).
[0133] Examples of the other additives include reinforcing fibers other than glass fibers (e.g., carbon fibers and metal fibers), fillers other than glass fibers (e.g., glass powder, talc and mica), flame retardants, ultraviolet absorbers, heat stabilizers, antioxidants, antistatic agents, flow improvers, antiblocking agents, lubricants, nucleating agents, antibacterial agents and pigments.
[0134] The glass fiber reinforced resin composition of the present embodiment may be a prepreg obtained by impregnating the glass fiber fabric of the present embodiment with the resin by a method known per se and semi-curing the same.
[0135] The glass fiber reinforced resin composition of this embodiment can be molded by known molding methods such as injection molding, injection compression molding, two-color molding, hollow molding, foam molding (including supercritical fluid), insert molding, in-mold coating molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, blow molding, stamping molding, infusion, hand lay-up, spray-up, resin transfer molding, sheet molding compound method, bulk molding compound method, pultrusion method, filament winding method, etc. to obtain various glass fiber reinforced resin molded products. In addition, a glass fiber reinforced resin molded product can also be obtained by curing the prepreg.
[0136] Applications of such molded articles include, for example, electronic device housings, electronic components (printed wiring boards), vehicle exterior parts (bumpers, fenders, bonnets, air dams, wheel covers, etc.), vehicle interior parts (door trims, ceiling materials, etc.), vehicle engine peripheral parts (oil pans, engine covers, intake manifolds, exhaust manifolds, etc.), muffler-related parts (sound-absorbing parts, etc.), high-pressure tanks, etc.
[0137] The glass fiber of the present embodiment can be suitably used as a reinforcing material for inorganic materials such as gypsum, cement, etc., other than the glass fiber reinforced resin composition of the present embodiment. For example, when used as a reinforcing material for gypsum (particularly, a gypsum board having a thickness of 4 to 60 mm), the glass fiber having the above range can be contained in a range of 0.1 to 4.0 mass% with respect to the total mass of the gypsum.
[0138] Next, examples of the present invention and comparative examples will be described. EXAMPLES
[0139] First, the glass composition after melting and solidifying was the same as that of Examples 1 to 4 shown in Table 1. 2. Reference Examples 1~3 Glass raw materials were mixed so as to obtain each composition of Comparative Examples 1 to 5, to obtain glass batches.
[0140] Next, Examples 1 to 2. Reference Examples 1~3 Or, a glass batch corresponding to the glass composition for glass fiber of Comparative Examples 1 to 5 was melted at 1550°C for 6 hours to obtain a homogeneous glass cullet. Then, the glass cullet was placed in a platinum crucible with a diameter of 80 mm, melted at 1500°C for 4 hours, and removed from the crucible to obtain a glass bulk. Then, the obtained glass bulk was annealed at 580°C for 8 hours to obtain a test piece. The dielectric tangent and phase separation characteristics of the obtained test piece were measured or evaluated by the method shown below. In addition, the 1000 poise temperature was measured using the glass cullet obtained in the test piece preparation process.
[0141] In addition, Examples 1 to 2. Reference Examples 1~3 Or, the glass batch corresponding to the glass composition for glass fiber of Comparative Examples 1 to 5 or the above-mentioned glass cullet was melted at 1550°C in a glass melting furnace, and the obtained melt was discharged from a bushing having a nozzle plate formed with 200 nozzle tips, cooled and solidified to obtain glass beads. The obtained glass beads were gradually cooled under the condition of 580°C and 8 hours, and at least 40 pieces of the gradually cooled glass beads were used to evaluate the striae characteristics by the method shown below.
[0142] The evaluation results are shown in Table 1.
[0143] [Method of measuring dielectric tangent] The test piece was polished to prepare a polished test piece of 80 mm x 3 mm (thickness 1 mm). The polished test piece obtained was then dried and stored in a room at 23°C and 60% humidity for 24 hours. The dielectric loss tangent (dissipation factor Df) at 10 GHz was measured for the polished test piece obtained using a cavity resonator method dielectric constant measuring device ADMS01Oc1 (product name) manufactured by AET Corporation in accordance with JIS C 2565:1992.
[0144] [Method of evaluating phase separation characteristics] A disk-shaped test piece was placed on the boundary between the black and white plates, and the boundary between the black and white plates was observed from the top of the test piece through the test piece. If no turbidity (phase separation) was observed within the test piece and the boundary was clearly observed, the test piece was rated as "A." If slight turbidity was observed within the test piece but the boundary was clearly observed, the test piece was rated as "B." If the boundary could not be clearly observed due to turbidity within the test piece, the test piece was rated as "C."
[0145] [How to measure 1000 poise temperature] A high-temperature electric furnace equipped with a rotational viscometer (manufactured by Shibaura Systems Co., Ltd.) was used to melt glass cullet in a platinum crucible, and the viscosity of the molten glass was continuously measured while changing the melting temperature using a rotational Brookfield viscometer, and the viscosity was determined by measuring the temperature corresponding to the rotational viscosity of 1000 poise.
[0146] [Method of evaluating striae characteristics] The glass beads were observed under an optical microscope at a magnification of 20 to 50 times, and the number of glass beads with striae was counted. If 40% or less of the total number of beads observed had striae, they were rated as "A", if more than 40% but not more than 60%, they were rated as "B", and if more than 60%, they were rated as "C".
[0147] [Table 1] As shown in Table 1, Examples 1 to 2 SiO2 in the range of 52.0 mass% or more and 57.5 mass% or less with respect to the total amount of the glass composition for glass fiber, 23.8% or more and 25.5% or less by mass, Al2O3 in the range of 8.0% by mass or more and 13.0% by mass or less, MgO in the range of 0% by mass or more and 2.0% by mass or less, CaO in the range of 0% by mass or more and 6.0% by mass or less, SrO in the range of 0.5% by mass or more and 6.5% by mass or less, and TiO2 in the range of 0.1% by mass or more and 3.0% by mass or less, wherein a ratio (Al2O3 / B2O3) of the content (mass%) of Al2O3 to the content (mass%) of B2O3 is in the range of 0.35 to 0.54, The glass composition for glass fiber of the present invention, in which the SiO2 content (mass%) SI, the B2O3 content (mass%) B, the MgO content (mass%) M, the CaO content (mass%) C, the SrO content (mass%) SR, and the TiO2 content (mass%) T satisfy the following formula (1), has a low dielectric tangent (a dielectric tangent of 0.0018 or less), inhibits the occurrence of phase separation, has reduced viscosity at high temperatures (has a 1000 poise temperature of 1375°C or less), and further has reduced occurrence of striae.
[0148] 6.90≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2 / 3 ×{T / (M+T)} 1 / 2 ≦12.30 (1) On the other hand, the glass compositions for glass fiber of Comparative Examples 1 to 5 did not satisfy the formula (1), and therefore had any of the following disadvantages: the dielectric tangent was high (dielectric tangent was greater than 0.0018), phase separation occurred, the viscosity at high temperatures was not reduced (1000 poise temperature was greater than 1375°C), or striae occurred. [Example 3 ] The glass raw materials were mixed so that the glass composition after melting and solidifying would be the same as that of Example 1, to obtain a glass batch. Next, the glass batch was melted at 1550°C, and the obtained molten material was discharged from a bushing having a nozzle plate formed with 200 nozzle tips, and was cooled and solidified while being stretched by winding at a predetermined speed, to form glass fibers (glass filaments) having a perfect circular cross section and a fiber diameter of 5 μm. A bundling agent was applied to the obtained 200 glass filaments with an applicator to bundle them, and the filaments were wound around a collet to obtain a glass fiber bundle. A series of operations (spinning) was continued for 6 hours, but no breakage of the glass fibers occurred. [Comparative Example 6] The glass raw materials were mixed so that the glass composition after melting and solidifying was the same as that of Comparative Example 5, to obtain a glass batch. Next, the glass batch was melted at 1550°C, and the obtained molten material was discharged from a bushing having a nozzle plate formed with 200 nozzle tips, and was cooled and solidified while being stretched by winding at a predetermined speed, to form glass fibers (glass filaments) having a perfect circular cross section and a fiber diameter of 5 μm. A bundling agent was applied to the obtained 200 glass filaments with an applicator to bundle them, and the filaments were wound around a collet to obtain a glass fiber bundle. A series of operations (spinning) was continued for 6 hours, and the glass fibers were broken 15 times.
[0149] Working Example 3 From Comparative Example 1 and Comparative Example 6, it was confirmed that the glass composition for glass fiber of the present invention can produce glass fibers and glass fiber bundles while suppressing their breakage. In addition, it was confirmed that the glass composition for glass fiber of the present invention satisfies the standard for industrial production if the number of breaks of the glass fiber when spinning is continued for 6 hours is 7 times or less. In addition, when producing glass fiber industrially, the number of breaks of the glass fiber when spinning is continued for 6 hours is preferably 5 times or less, more preferably 3 times or less, and even more preferably 1 time or less.
Claims
1. SiO in the range of 52.0 mass% to 57.5 mass% based on the total amount 2 and B in the range of 23.8% by mass or more and 25.5% by mass or less. 2 O 3 and Al in the range of 8.0 mass% to 13.0 mass%. 2 O 3 %, MgO in the range of 0% by mass to 2.0% by mass, CaO in the range of 0% by mass to 6.0% by mass, SrO in the range of 0.5% by mass to 6.5% by mass, and TiO in the range of 0.1% by mass to 3.0% by mass. 2 and B 2 O 3 Al content (mass%) 2 O 3 The content (mass%) of Al 2 O 3 / B 2 O 3 ) is in the range of 0.35 to 0.54; The SiO 2 The content (mass%) of SI, 2 O 3 the content (mass%) B of the MgO, the content (mass%) M of the CaO, the content (mass%) C of the SrO, and the content (mass%) SR of the TiO 2 A glass composition for glass fiber, characterized in that the content (mass%) T of satisfies the following formula (1): 6.90≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2/3 ×{T / (M+T)} 1/2 ≦12.30 ・・・(1)
2. 2. The glass composition for glass fiber according to claim 1, wherein SI, B, M, C, SR and T satisfy the following formula (2): 9.56≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2/3 ×{T / (M+T)} 1/2 ≦11.77 ・・・(2)
3. 3. The glass composition for glass fiber according to claim 2, wherein SI, B, M, C, SR and T satisfy the following formula (3): 10.00≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2/3 ×{T / (M+T)} 1/2 ≦11.35 ・・・(3)
4. 4. The glass composition for glass fiber according to claim 3, wherein SI, B, M, C, SR and T satisfy the following formula (4): 10.15≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2/3 ×{T / (M+T)} 1/2 ≦10.85 ・・・(4)
5. 5. The glass composition for glass fiber according to claim 4, wherein SI, B, M, C, SR and T satisfy the following formula (5): 10.35≦ 100×(B / SI) 2 ×{SR / (C+SR)} 2/3 ×{T / (M+T)} 1/2 ≦10.78 ・・・(5)
6. A glass fiber comprising the glass composition for glass fiber according to any one of claims 1 to 5.
7. A woven glass fiber fabric comprising the glass fiber according to claim 6.
8. A glass fiber reinforced resin composition comprising the glass fiber according to claim 6.
Citation Information
Patent Citations
Production of globular metal powder
JP1989068409A
Glazing of glass or glass ceramic and glass composition for ornament containing no lead and cadmium
JP1999043352A
Low dielectric constant low dielectric dissipation factor glass fiber
JP2004107112A
Glass composition resistant to chemical media for the manufacture of glass-reinforced yarn
JP2010507557A
Glass fiber-reinforced resin molding
JP2019081909A