Laminated film and roll body

The laminated film with controlled CN-, Si-, and OH- peak ratios on the insulating resin layer surface addresses lifting, wrinkles, and resin peeling issues, maintaining film integrity in long rolls.

JP7560998B2Active Publication Date: 2024-10-03SEKISUI CHEMICAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020180719
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-28
Publication Date
2024-10-03
Estimated Expiration
2040-10-28

AI Technical Summary

Technical Problem

Conventional laminated films experience issues such as lifting, wrinkles, and resin peeling when unwound from rolls, particularly when the roll length is long or stored for extended periods, which can damage the insulating resin layer.

Method used

A laminated film configuration with specific ion count ratios of CN-, Si-, and OH- peaks on the insulating resin layer surface, achieved by controlling chemical adhesion functional groups, is used to suppress lifting, wrinkles, and resin peeling.

Benefits of technology

The laminated film effectively prevents lifting and wrinkles, and resin peeling even in long rolls stored for extended periods, ensuring the integrity of the insulating resin layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560998000006
    Figure 0007560998000006
  • Figure 0007560998000007
    Figure 0007560998000007
  • Figure 0007560998000008
    Figure 0007560998000008
Patent Text Reader

Abstract

To provide a laminate film wound from a roll body which can suppress occurrences of floating and wrinkles, and can suppress occurrence of resin peeling at the time of peeling of a protective film.SOLUTION: A laminate film has a base material film, an insulating resin layer arranged on a surface of the base material film, and a protective film laminated on a surface opposite to the base material film side of the insulating resin layer, in which the insulating resin layer is used for forming the insulating layer in a multilayer printed wiring board, and when a surface of the insulating resin layer exposed by peeling the protective film after the protective film has been peeled is analyzed by flight-time secondary ion mass spectrometry, a CN-peak and an Si-peak exist, an OH- peak exists or does not exist, and a ratio (count number of CN-ion of CN-peak / count number of Si-ion of Si-peak) is more than 50 and less than 6,000.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate film including a base film, an insulating resin layer, and a protective film, and also to a roll body using the laminate film. [Background technology]

[0002] Conventionally, various resin materials have been used to obtain electronic components such as semiconductor devices, laminates, and printed wiring boards. For example, in multilayer printed wiring boards, resin materials are used to form insulating layers for insulating between internal layers and to form insulating layers located on the surface. To form the insulating layers, laminate films including a base film and an insulating resin layer are used.

[0003] The following Patent Document 1 discloses an adhesive sheet (laminate film) with a protective film, which includes an adhesive sheet consisting of a support having a first and second surface and a resin composition layer bonded to the second surface of the support, and a protective film having a first and second surface and provided so that the second surface is bonded to the resin composition layer of the adhesive sheet. This adhesive sheet with a protective film has an arithmetic average roughness (Ra p1 ) is 100 nm or more, and the arithmetic mean roughness (Ra p2 ) is 100 nm or more. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-20480 A Summary of the Invention [Problem to be solved by the invention]

[0005] A laminate film including a base film, an insulating resin layer, and a protective film may be wound into a roll and stored in the form of a roll. When using the laminate film, the protective film is peeled off and the exposed insulating resin layer is laminated on a member to be laminated.

[0006] In a conventional laminate film, when the laminate film is unwound from a roll, peeling (so-called lifting) or wrinkles may occur at the interface between the insulating resin layer and the protective film.

[0007] Furthermore, in conventional laminated films, a phenomenon may occur in which a part of the insulating resin layer is peeled off together with the protective film when the protective film is peeled off (so-called resin peeling). In the laminated film described in Patent Document 1, the arithmetic mean roughness of the surface of the resin composition layer (insulating resin layer) side of the protective film is controlled, so that the occurrence of resin peeling can be suppressed to a certain extent. However, even with the laminated film described in Patent Document 1, it may be difficult to sufficiently suppress resin peeling. When resin peeling occurs, the insulating resin layer may be partially damaged after the protective film is peeled off.

[0008] In particular, in conventional laminate films such as those described in Patent Document 1, when the roll is long (e.g., 20 m or more) or when the roll is stored at room temperature for a long period of time, lifting, wrinkles, and resin peeling are likely to occur due to tight winding.

[0009] An object of the present invention is to provide a laminate film that can suppress the occurrence of lifting and wrinkles in the laminate film unwound from a roll body, and can suppress the occurrence of resin peeling when a protective film is peeled off. Another object of the present invention is to provide a roll body using the above laminate film. [Means for solving the problem]

[0010] According to a broad aspect of the present invention, there is provided a multilayer printed wiring board comprising a base film, an insulating resin layer disposed on a surface of the base film, and a protective film laminated on a surface of the insulating resin layer opposite to the base film side, the insulating resin layer being used to form an insulating layer in a multilayer printed wiring board, and when the surface of the insulating resin layer exposed by peeling off the protective film is analyzed by time-of-flight secondary ion mass spectrometry after peeling off the protective film, - Peak and Si - Peaks and OH - The peak may or may not be present, and the CN - Peak CN - The number of ion counts, - Peak Si - A laminated film is provided having an ion to count ratio of greater than 50 and less than 6000.

[0011] In a specific aspect of the laminated film according to the present invention, the CN - Peak CN - The number of ion counts, - Peak Si - The ratio of ion counts is less than 5,000.

[0012] In a specific aspect of the laminated film according to the present invention, the CN - Peak CN - The number of ion counts, - Peak Si - The ratio of ion counts is less than 4000.

[0013] In a specific aspect of the laminated film according to the present invention, the OH - The OH peak is present. - Peak OH - The number of ion counts, - Peak Si - The ratio of the ion counts is less than 2000.

[0014] In a specific aspect of the laminated film according to the present invention, the OH - Peak OH - The number of ion counts, - Peak Si - The ratio of the ion counts is less than 1000.

[0015] According to a broad aspect of the present invention, there is provided a roll body including a winding core and the above-mentioned laminate film, the laminate film being wound around the outer periphery of the winding core. Effect of the Invention

[0016] The laminated film according to the present invention comprises a base film, an insulating resin layer disposed on a surface of the base film, and a protective film laminated on the surface of the insulating resin layer opposite to the base film side. In the laminated film according to the present invention, the insulating resin layer is used to form an insulating layer in a multilayer printed wiring board. In the laminated film according to the present invention, when the surface of the insulating resin layer exposed by peeling off the protective film is analyzed by time-of-flight secondary ion mass spectrometry after peeling off the protective film, CN - Peak and Si - Peaks and OH - In the laminated film according to the present invention, the CN - Peak CN - The number of ion counts is the above Si - Peak Si - The ratio of the number of ions counted to the number of ions counted is more than 50 and less than 6000. Since the laminated film according to the present invention has the above-mentioned configuration, the laminated film unwound from the roll can be prevented from floating and wrinkling, and the resin can be prevented from peeling off when the protective film is peeled off. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a laminated film according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a perspective view that typically illustrates a roll around which the laminate film shown in FIG. 1 is wound. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates a multilayer printed wiring board using a laminate film according to one embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram showing the configuration of a laminated film manufacturing apparatus used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will be described in detail below.

[0019] The laminated film according to the present invention includes a base film, an insulating resin layer disposed on a surface of the base film, and a protective film laminated on the surface of the insulating resin layer opposite to the base film side. The insulating resin layer is used to form an insulating layer in a multilayer printed wiring board.

[0020] In the laminated film according to the present invention, the protective film is peeled off when the insulating resin layer is used. In the laminated film according to the present invention, when the surface of the insulating resin layer exposed by peeling off the protective film is analyzed by time-of-flight secondary ion mass spectrometry after peeling off the protective film, CN - Peak and Si - Peaks and OH - Peaks are either present or absent.

[0021] In the laminated film according to the present invention, the above-mentioned CN - Peak CN - The number of ion counts is the above Si - Peak Si - Ratio of ion counts (CN - Peak CN - Ion counts / Si - Peak Si - The number of ion counts is greater than 50 and less than 6,000.

[0022] Since the laminated film according to the present invention has the above-mentioned configuration, the laminated film unwound from the roll can be prevented from floating and wrinkling, and the resin peeling can be prevented from occurring when the protective film is peeled off. In the present invention, the chemical adhesion functional groups on the surface of the insulating resin layer in contact with the protective film are sufficiently controlled, so that the laminated film unwound from the roll can be prevented from floating and wrinkling, and the resin peeling can be prevented from occurring when the protective film is peeled off.

[0023] The laminate film according to the present invention can exhibit the above-mentioned effects of the present invention even when the roll body is long (for example, 20 m or more) or when the storage period of the roll body is long.

[0024] In the laminated film according to the present invention, after the protective film is peeled off, the above ratio (CN - Peak CN - Ion counts / Si - Peak Si - The number of ion counts satisfies the above range.

[0025] The above ratio (CN - Peak CN - Ion counts / Si - Peak Si - The ratio (CN ion count number) on the surface of the insulating resin layer before the protective film is peeled off (before the protective film is laminated) does not match the ratio on the surface of the insulating resin layer before the protective film is peeled off. - Peak CN - Ion counts / Si - Peak Si - Even if the ion count satisfies the above-mentioned range, the ratio on the surface of the insulating resin layer exposed by peeling off the protective film does not satisfy the above-mentioned range.

[0026] In the present invention, the above ratio (CN - Peak CN - Ion counts / Si - Peak Si - It is significant that the ratio is set in the above-mentioned range, focusing on the number of counts of ions.

[0027] FIG. 1 is a cross-sectional view that illustrates a laminated film according to one embodiment of the present invention.

[0028] The laminated film 1 includes a base film 3, an insulating resin layer 2, and a protective film 4. The insulating resin layer 2 is laminated on a surface of the base film 3. A first surface of the insulating resin layer 2 A base film 3 is laminated on the first surface 2a of the insulating resin layer 2. A protective film 4 is laminated on a second surface 2b opposite to the first surface 2a of the insulating resin layer 2. When using the laminated film 1, the protective film 4 is peeled off, and the laminated film 1 is laminated on a target member from the second surface 2b side of the insulating resin layer 2.

[0029] FIG. 2 is a perspective view that typically illustrates a roll around which the laminate film shown in FIG. 1 is wound.

[0030] 2, the laminate film 1 is wound into a roll shape in the roll body 51. The roll body 51 includes a winding core 61 and the laminate film 1. The laminate film 1 is wound around the outer periphery of the winding core 61.

[0031] In the laminated film according to the present invention, when the surface of the insulating resin layer exposed by peeling off the protective film is analyzed by time-of-flight secondary ion mass spectrometry (TOF-SIMS), CN - Peak and Si - Peaks and OH - Peaks are either present or absent.

[0032] The above CN -The peak can be made to exist by, for example, making the insulating resin layer contain a compound having an amino bond or a compound having an amine bond. - The OH peak can be made to exist by, for example, adding silica as an inorganic filler to the insulating resin layer. - The peak can be made to exist by, for example, including a phenol compound in the insulating resin layer.

[0033] From the viewpoint of exerting the effects of the present invention, in the laminated film according to the present invention, the above-mentioned CN - Peak CN - The number of ion counts is the above Si - Peak Si - Ratio of ion counts (CN - Peak CN - Ion counts / Si - Peak Si - The number of ion counts is greater than 50 and less than 6,000.

[0034] The above CN - Peak CN - The number of ion counts is the above Si - Peak Si - Ratio of ion counts (CN - Peak CN - Ion counts / Si - Peak Si - The CN ion count is preferably 100 or more, and more preferably 200 or more. - Peak CN - The number of ion counts is the above Si - Peak Si - Ratio of ion counts (CN - Peak CN - Ion counts / Si - Peak Si - The ion count) is preferably less than 5000, more preferably 4000 or less, even more preferably less than 4000, and particularly preferably 3500 or less. - Peak CN -Ion counts / Si - Peak Si - When the count number of ions satisfies the above lower limit and upper limit, the effects of the present invention can be more effectively exhibited.

[0035] From the viewpoint of more effectively exerting the effects of the present invention, particularly from the viewpoint of more effectively suppressing the occurrence of lifting and wrinkles, the above OH - It is preferable that the OH peak exists. - Even if no peak exists, the effect of the present invention can be exerted.

[0036] Above OH - If a peak is present, - Peak OH - The number of ion counts is the above Si - Peak Si - Ratio to ion counts (OH - Peak OH - Ion counts / Si - Peak Si - The OH ion count is preferably 100 or more, and more preferably 200 or more. - If a peak is present, - Peak OH - The number of ion counts is the above Si - Peak Si - Ratio to ion counts (OH - Peak OH - Ion counts / Si - Peak Si - The OH ion count is preferably less than 2000, more preferably less than 1000. - Peak OH - Ion counts / Si - Peak Si - When the number of counts of ions satisfies the above lower limit and upper limit, the effects of the present invention can be exhibited even more effectively, and in particular, the occurrence of lifting and wrinkles can be suppressed even more effectively.

[0037] Specifically, the analysis by the time-of-flight secondary ion mass spectrometry (TOF-SIMS) is carried out as follows.

[0038] The protective film in the laminated film is peeled off. The surface of the insulating resin layer exposed by peeling off the protective film is measured using a time-of-flight secondary ion mass spectrometer (for example, "TOF-SIMS5" manufactured by ION-TOF) under the measurement conditions described in the Examples section below.

[0039] The above CN - Peak CN - Ion counts, above Si - Peak Si - The number of ion counts and the above OH - Peak OH - The ion count is preferably an average value of the ion counts at three arbitrary locations that are 500 μm or more apart from each other. - Peak CN - Ion counts, above Si - Peak Si - The number of ion counts and the above OH - Peak OH - The number of ions counted is preferably measured at a position 1 mm or more inward from the edge of the laminated film.

[0040] Above ratio (CN - Peak CN - Ion counts / Si - Peak Si - ion counts), and the above ratio (OH - Peak OH - Ion counts / Si - Peak Si -The following methods can be used to control the ratio (CN ion count) within the above-mentioned preferred range. (1) A method of adjusting the drying temperature and drying speed of the solvent used when forming the insulating resin layer. (2) A method of adjusting the particle size and surface treatment method of the inorganic filler. (3) A method of adjusting the content of the resin having an alkyl structure and a nitrogen atom-containing group or an OH group. (4) A method of adjusting the content of the compound having a triazine skeleton, an imide skeleton, a carbodiimide skeleton, or a maleimide skeleton. By appropriately combining these methods, the above ratio (CN - Peak CN - Ion counts / Si - Peak Si - ion counts), and the above ratio (OH - Peak OH - Ion counts / Si - Peak Si - The number of ion counts can be controlled within the above preferred range.

[0041] Each layer constituting the laminate film according to the present invention will be described in detail below.

[0042] (Base film) Examples of the base film include metal foil, polyester resin film such as polyethylene terephthalate film and polybutylene terephthalate film, olefin resin film such as polyethylene film and polypropylene film, and polyimide film. The surface of the base film may be subjected to a release treatment as necessary. The base film may be a metal foil or a resin film. The base film is preferably a resin film. When a metal foil is used as the base film, the metal foil is preferably a copper foil.

[0043] From the viewpoint of improving the operability of the laminated film and improving the lamination properties of the insulating resin layer, the thickness of the above-mentioned base film is preferably 10 μm or more, more preferably 20 μm or more, and preferably 300 μm or less, more preferably 250 μm or less.

[0044] (insulating resin layer) The insulating resin layer is laminated on the surface of the base film. The insulating resin layer preferably contains an epoxy compound, an inorganic filler, and a curing agent, which will be described later. By curing the insulating resin layer containing the epoxy compound and the curing agent, an insulating layer that is a cured product can be formed in the multilayer printed wiring board.

[0045] [Epoxy compounds] The insulating resin layer preferably contains an epoxy compound. As the epoxy compound, a conventionally known epoxy compound can be used. The epoxy compound refers to an organic compound having at least one epoxy group. The epoxy compound may be used alone or in combination of two or more kinds.

[0046] Examples of the epoxy compound include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, phenol novolac type epoxy compounds, biphenyl type epoxy compounds, biphenyl novolac type epoxy compounds, biphenol type epoxy compounds, naphthalene type epoxy compounds, fluorene type epoxy compounds, phenol aralkyl type epoxy compounds, naphthol aralkyl type epoxy compounds, dicyclopentadiene type epoxy compounds, anthracene type epoxy compounds, epoxy compounds having an adamantane skeleton, epoxy compounds having a tricyclodecane skeleton, naphthylene ether type epoxy compounds, and epoxy compounds having a triazine nucleus in the skeleton.

[0047] From the viewpoint of further increasing the adhesive strength between the cured product and the metal layer, the epoxy compound preferably has an aromatic skeleton, preferably has a biphenyl skeleton, and is preferably a biphenyl-type epoxy compound.

[0048] From the viewpoint of further increasing the adhesive strength between the cured product and the metal layer, the content of the epoxy compound in 100% by weight of the insulating resin layer is preferably 10% by weight or more, more preferably 20% by weight or more, preferably 70% by weight or less, more preferably 65% ​​by weight or less, even more preferably 60% by weight or less, and particularly preferably 55% by weight or less.

[0049] The molecular weight of the epoxy compound is more preferably not more than 1000. In this case, when the insulating resin layer is laminated onto a base film, the inorganic filler can be uniformly present.

[0050] The molecular weight of the epoxy compound and the molecular weight of the curing agent described later refer to the molecular weight that can be calculated from the structural formula when the epoxy compound or the curing agent is not a polymer and when the structural formula of the epoxy compound or the curing agent can be specified, and refer to the weight average molecular weight when the epoxy compound or the curing agent is a polymer.

[0051] [Inorganic filler] The insulating resin layer preferably contains an inorganic filler. The use of the inorganic filler reduces the dimensional change of the cured product due to heat. Furthermore, the surface roughness of the cured product is further reduced, and the adhesive strength between the cured product and the metal layer is increased.

[0052] Examples of the inorganic filler include silica, talc, clay, mica, hydrotalcite, alumina, magnesium oxide, aluminum hydroxide, aluminum nitride, and boron nitride.

[0053] From the viewpoint of reducing the surface roughness of the cured product, further increasing the adhesive strength between the cured product and the metal layer, forming finer wiring on the surface of the cured product, and imparting better insulation reliability to the cured product, the inorganic filler is preferably silica or alumina, more preferably silica, and even more preferably fused silica. By using silica, the thermal expansion coefficient of the cured product is further reduced, the surface roughness of the cured product is effectively reduced, and the adhesive strength between the cured product and the metal layer is effectively increased. The shape of the silica is preferably spherical.

[0054] From the viewpoints of promoting resin curing regardless of the curing environment, effectively increasing the glass transition temperature of the cured product, and effectively reducing the coefficient of linear thermal expansion of the cured product, it is preferable that the inorganic filler be spherical silica.

[0055] The average particle size of the inorganic filler is preferably 10 nm or more, more preferably 50 nm or more, even more preferably 100 nm or more, and preferably 5 μm or less, more preferably 3 μm or less, even more preferably 1 μm or less, and particularly preferably 0.5 μm or less. When the average particle size of the inorganic filler is equal to or more than the lower limit and equal to or less than the upper limit, the adhesive strength between the cured product and the metal layer is further increased.

[0056] The median diameter (d50) at 50% is used as the average particle diameter of the inorganic filler. The average particle diameter can be measured using a particle size distribution measuring device using a laser diffraction scattering method.

[0057] The inorganic filler is preferably spherical, more preferably spherical silica. In this case, the surface roughness of the cured product is effectively reduced, and the adhesive strength between the cured product and the metal layer is effectively increased. When the inorganic filler is spherical, the aspect ratio of the inorganic filler is preferably 2 or less, more preferably 1.5 or less.

[0058] The inorganic filler is preferably surface-treated, more preferably surface-treated with a coupling agent, and even more preferably surface-treated with a silane coupling agent, which further reduces the surface roughness of the roughened cured product, further increases the adhesive strength between the cured product and the metal layer, forms finer wiring on the surface of the cured product, and provides the cured product with better inter-wiring insulation reliability and interlayer insulation reliability.

[0059] The coupling agent includes a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, etc. The silane coupling agent includes a methacrylsilane, an acrylsilane, an aminosilane, an imidazole silane, a vinylsilane, an epoxysilane, etc.

[0060] The content of the inorganic filler in 100% by weight of the insulating resin layer is preferably 30% by weight or more, more preferably 40% by weight or more, even more preferably 50% by weight or more, particularly preferably 60% by weight or more, and most preferably 70% by weight or more. The content of the inorganic filler in 100% by weight of the insulating resin layer is preferably 90% by weight or less, more preferably 85% by weight or less, even more preferably 83% by weight or less, and particularly preferably 80% by weight or less. When the content of the inorganic filler is equal to or more than the lower limit and equal to or less than the upper limit, the surface roughness of the cured product is further reduced, the adhesive strength between the cured product and the metal layer is further increased, and finer wiring is formed on the surface of the cured product. Furthermore, with this content of the inorganic filler, it is possible to lower the thermal expansion coefficient of the cured product and at the same time improve the smear removal property. When the content of the inorganic filler is equal to or more than the lower limit, the dielectric loss tangent is effectively lowered. When the content of the inorganic filler is equal to or less than the upper limit, peeling of the resin when the protective film is peeled off can be more effectively suppressed.

[0061] [Hardening agent] The insulating resin layer preferably contains a curing agent. The curing agent is not particularly limited. As the curing agent, a conventionally known curing agent can be used. The curing agent may be used alone or in combination of two or more kinds.

[0062] Examples of the curing agent include a phenol compound (phenol curing agent), a cyanate compound (cyanate curing agent), an active ester compound, a cyanate ester compound (cyanate ester curing agent), a benzoxazine compound (benzoxazine curing agent), a carbodiimide compound (carbodiimide curing agent), an acid anhydride, an amine compound (amine curing agent), a thiol compound (thiol curing agent), a phosphine compound, and dicyandiamide. The curing agent preferably has a functional group capable of reacting with the epoxy group of the epoxy compound.

[0063] Above OH - From the viewpoint of making the peaks present well and the above ratio (OH - Peak OH - Ion counts / Si - Peak Si - From the viewpoint of controlling the ion count) within the above-mentioned preferred range, the curing agent preferably contains a phenol compound, and more preferably contains an alkylphenol compound.

[0064] Above ratio (CN - Peak CN - Ion counts / Si - Peak Si - From the viewpoint of controlling the ion count) within the above-mentioned preferred range, the curing agent preferably contains a cyanate compound, a carbodiimide compound, or a maleimide compound.

[0065] From the viewpoint of further lowering the dielectric tangent, the curing agent preferably contains a cyanate compound, a maleimide compound, or an active ester compound.

[0066] Commercially available products of the above phenol compounds include novolac phenols (DIC Corporation, "TD-2091"), biphenyl novolac phenols (Meiwa Chemical Industry Co., Ltd., "MEH-7851"), aralkyl phenol compounds (Meiwa Chemical Industry Co., Ltd., "MEH-7800"), and phenols having an aminotriazine skeleton (DIC Corporation, "LA1356" and "LA3018-50P"), etc. Commercially available products of the above alkylphenol compounds include 4-tertiary butylphenol (DIC Corporation, "DIC-PTBT") and 4-octylphenol (DIC Corporation, "DIC-POP"), etc.

[0067] Commercially available products of the cyanate compound include phenol novolac type cyanate resins (PT-30 and PT-60 manufactured by Lonza Japan) and prepolymers in which bisphenol A dicyanate is triazine-modified to form a trimer (BA230 manufactured by Lonza Japan).

[0068] An active ester compound is a compound that contains at least one ester bond in the structure and has aromatic rings bonded to both sides of the ester bond. An active ester compound is obtained, for example, by a condensation reaction between a carboxylic acid compound or a thiocarboxylic acid compound and a hydroxy compound or a thiol compound. An example of an active ester compound is a compound represented by the following formula (1).

[0069] [ka]

[0070] In the above formula (1), X1 represents a group containing an aliphatic chain, a group containing an aliphatic ring, or a group containing an aromatic ring, and X2 represents a group containing an aromatic ring. Preferred examples of the group containing an aromatic ring include a benzene ring which may have a substituent, and a naphthalene ring which may have a substituent. Examples of the substituent include a hydrocarbon group. The number of carbon atoms in the hydrocarbon group is preferably 12 or less, more preferably 6 or less, and even more preferably 4 or less.

[0071] Examples of the combination of X1 and X2 include a combination of an optionally substituted benzene ring and an optionally substituted benzene ring, and a combination of an optionally substituted benzene ring and an optionally substituted naphthalene ring.Furthermore, examples of the combination of X1 and X2 include a combination of an optionally substituted naphthalene ring and an optionally substituted naphthalene ring.

[0072] The active ester compound is not particularly limited. Commercially available products of the active ester compound include "HPC-8000-65T", "EXB9416-70BK", "EXB8100-65T", and "EXB-8000L-65MT" manufactured by DIC Corporation.

[0073] Examples of the cyanate ester compound include novolac-type cyanate ester resins, bisphenol-type cyanate ester resins, and prepolymers obtained by partially trimerizing these. Examples of the novolac-type cyanate ester resins include phenol novolac-type cyanate ester resins and alkylphenol-type cyanate ester resins. Examples of the bisphenol-type cyanate ester resins include bisphenol A-type cyanate ester resins, bisphenol E-type cyanate ester resins, and tetramethylbisphenol F-type cyanate ester resins.

[0074] Commercially available products of the cyanate ester compound include phenol novolac type cyanate ester resins ("PT-30" and "PT-60" manufactured by Lonza Japan) and prepolymers in which bisphenol type cyanate ester resins are trimerized ("BA-230S", "BA-3000S", "BTP-1000S" and "BTP-6020S" manufactured by Lonza Japan).

[0075] Examples of the benzoxazine compound include Pd-type benzoxazine and Fa-type benzoxazine.

[0076] Commercially available products of the above benzoxazine compounds include "Pd type" manufactured by Shikoku Chemical Industry Co., Ltd.

[0077] The carbodiimide compound is a compound having a structural unit represented by the following formula (2). In the following formula (2), the right end and the left end are bonding sites with other groups. The above carbodiimide compounds may be used alone or in combination of two or more kinds.

[0078] [ka]

[0079] In the above formula (2), X represents an alkylene group, a group in which a substituent is bonded to an alkylene group, a cycloalkylene group, a group in which a substituent is bonded to a cycloalkylene group, an arylene group, or a group in which a substituent is bonded to an arylene group, and p represents an integer of 1 to 5. When a plurality of Xs are present, the plurality of Xs may be the same or different.

[0080] In one preferred embodiment, at least one X is an alkylene group, a group in which a substituent is bonded to an alkylene group, a cycloalkylene group, or a group in which a substituent is bonded to a cycloalkylene group.

[0081] Commercially available examples of the carbodiimide compound include "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07", "Carbodilite V-09", "Carbodilite 10M-SP", and "Carbodilite 10M-SP (modified)" manufactured by Nisshinbo Chemical Inc., as well as "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by Rhein Chemie.

[0082] Examples of the acid anhydride include tetrahydrophthalic anhydride and alkylstyrene-maleic anhydride copolymer.

[0083] Commercially available products of the above acid anhydrides include "Rikacid TDA-100" manufactured by New Japan Chemical Co., Ltd.

[0084] The molecular weight of the curing agent is preferably not more than 1000. In this case, when the insulating resin layer is laminated onto a substrate film, the inorganic filler can be uniformly present.

[0085] The total content of the epoxy compound and the curing agent in the insulating resin layer is preferably 75% by weight or more, more preferably 80% by weight or more, preferably 99% by weight or less, more preferably 97% by weight or less, based on 100% by weight of the components excluding the inorganic filler in the insulating resin layer. When the total content of the epoxy compound and the curing agent is equal to or more than the lower limit and equal to or less than the upper limit, a better cured product can be obtained, and the dispersibility of the inorganic filler can be improved because the melt viscosity can be adjusted. Furthermore, the insulating resin layer can be prevented from spreading to unintended areas during the curing process. Furthermore, the dimensional change of the cured product due to heat can be further suppressed. Furthermore, when the total content of the epoxy compound and the curing agent is equal to or more than the lower limit, the melt viscosity does not become too low, and the insulating resin layer tends not to spread excessively to unintended areas during the curing process. Furthermore, when the total content of the epoxy compound and the curing agent is equal to or less than the upper limit, the holes or irregularities in the circuit board can be easily filled, and the inorganic filler tends not to be present unevenly.

[0086] The content of the curing agent in the insulating resin layer, based on 100% by weight of the components excluding the inorganic filler, is preferably 30% by weight or more, more preferably 40% by weight or more, and preferably 70% by weight or less, more preferably 60% by weight or less. When the content of the curing agent is equal to or more than the lower limit and equal to or less than the upper limit, a better cured product is obtained, and the dielectric loss tangent is effectively reduced.

[0087] [Cure accelerator] The insulating resin layer preferably contains a curing accelerator. The use of the curing accelerator further increases the curing speed. By quickly curing the insulating resin layer, the crosslinked structure in the cured product becomes uniform, and the number of unreacted functional groups decreases, resulting in a high crosslink density. The curing accelerator is not particularly limited, and conventionally known curing accelerators can be used. The curing accelerator may be used alone or in combination of two or more.

[0088] Examples of the curing accelerator include imidazole compounds, phosphorus compounds, amine compounds, and organometallic compounds.

[0089] Examples of the imidazole compound include 2-undecylimidazole, 2-heptadecylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1,2-dimethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and 1-cyanoethyl-2-phenylimidazolium trimethylolate. remellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-methylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-dihydroxymethylimidazole.

[0090] The phosphorus compound includes triphenylphosphine and the like.

[0091] Examples of the amine compound include diethylamine, triethylamine, diethylenetetramine, triethylenetetramine, and 4,4-dimethylaminopyridine.

[0092] Examples of the organometallic compound include zinc naphthenate, cobalt naphthenate, tin octoate, cobalt octoate, cobalt bisacetylacetonate (II), and cobalt trisacetylacetonate (III).

[0093] The content of the curing accelerator is not particularly limited. In 100% by weight of the components in the insulating resin layer excluding the inorganic filler, the content of the curing accelerator is preferably 0.005% by weight or more, more preferably 0.01% by weight or more, preferably 5% by weight or less, more preferably 3% by weight or less. When the content of the curing accelerator is equal to or more than the lower limit and equal to or less than the upper limit, the insulating resin layer is cured efficiently. When the content of the curing accelerator is within a more preferred range, the storage stability of the insulating resin layer is further increased, and a better cured product is obtained.

[0094] [Thermoplastic resin] The insulating resin layer preferably contains a thermoplastic resin. Examples of the thermoplastic resin include polyvinyl acetal resin, polyimide resin, and phenoxy resin. The thermoplastic resin may be used alone or in combination of two or more kinds.

[0095] From the viewpoint of effectively lowering the dielectric tangent and effectively increasing the adhesion of the metal wiring regardless of the curing environment, the thermoplastic resin is preferably a phenoxy resin. By using the phenoxy resin, the deterioration of the embedding property of the insulating resin layer in the hole or unevenness of the circuit board and the non-uniformity of the inorganic filler are suppressed. In addition, by using the phenoxy resin, the melt viscosity can be adjusted, so that the dispersibility of the inorganic filler is improved, and the insulating resin layer is less likely to wet and spread to unintended areas during the curing process. The phenoxy resin is not particularly limited. As the phenoxy resin, a conventionally known phenoxy resin can be used. The phenoxy resin may be used alone or in combination of two or more types.

[0096] Examples of the phenoxy resin include phenoxy resins having a skeleton such as a bisphenol A skeleton, a bisphenol F skeleton, a bisphenol S skeleton, a biphenyl skeleton, a novolac skeleton, a naphthalene skeleton, and an imide skeleton.

[0097] Commercially available examples of the phenoxy resin include "YP50", "YP55" and "YP70" manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd., and "1256B40", "4250", "4256H40", "4275", "YX6954BH30" and "YX8100BH30" manufactured by Mitsubishi Chemical Corporation.

[0098] From the viewpoint of obtaining an insulating resin layer having even more excellent storage stability, the weight average molecular weight of the thermoplastic resin is preferably 5,000 or more, more preferably 10,000 or more, and preferably 100,000 or less, more preferably 50,000 or less.

[0099] The weight average molecular weight of the thermoplastic resin is a weight average molecular weight measured by gel permeation chromatography (GPC) and calculated as polystyrene.

[0100] The contents of the thermoplastic resin and the phenoxy resin are not particularly limited. In 100% by weight of the components in the insulating resin layer excluding the inorganic filler, the content of the thermoplastic resin (the content of the phenoxy resin when the thermoplastic resin is a phenoxy resin) is preferably 1% by weight or more, more preferably 5% by weight or more, preferably 30% by weight or less, more preferably 15% by weight or less. When the content of the thermoplastic resin is equal to or more than the lower limit and equal to or less than the upper limit, the insulating resin layer is better able to fill holes or irregularities in the circuit board. When the content of the thermoplastic resin is equal to or more than the lower limit, the insulating resin layer is more easily formed, and a better insulating layer is obtained. When the content of the thermoplastic resin is equal to or less than the upper limit, the thermal expansion coefficient of the cured product is further reduced. The surface roughness of the surface of the cured product is further reduced, and the adhesive strength between the cured product and the metal layer is further increased.

[0101] [solvent] The insulating resin layer does not contain or contains a solvent. The solvent may be used to obtain a slurry containing the inorganic filler. The solvent may be used alone or in combination of two or more.

[0102] Examples of the solvent include acetone, methanol, ethanol, butanol, 2-propanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 2-acetoxy-1-methoxypropane, toluene, xylene, methyl ethyl ketone, N,N-dimethylformamide, methyl isobutyl ketone, N-methyl-pyrrolidone, n-hexane, cyclohexane, cyclohexanone, and naphtha, which is a mixture.

[0103] It is preferable that most of the solvent is removed when the insulating resin layer is formed. Therefore, the boiling point of the solvent is preferably 200° C. or less, more preferably 180° C. or less. The content of the solvent in the insulating resin layer is not particularly limited. The content of the solvent can be appropriately changed to an extent that the layer shape of the insulating resin layer can be maintained.

[0104] When the insulating resin layer is a B-stage film, the content of the solvent in 100% by weight of the B-stage film is preferably 1% by weight or more, more preferably 2% by weight or more, preferably 10% by weight or less, more preferably 5% by weight or less.

[0105] [Other ingredients] For the purpose of improving impact resistance, heat resistance, resin compatibility, workability, and the like, the insulating resin layer may contain a leveling agent, a flame retardant, a coupling agent, a colorant, an antioxidant, an ultraviolet degradation inhibitor, a defoaming agent, a thickener, a thixotropy imparting agent, and a thermosetting resin other than the epoxy compound.

[0106] The coupling agent includes a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, etc. The silane coupling agent includes a vinyl silane, an amino silane, an imidazole silane, an epoxy silane, etc.

[0107] Examples of the other thermosetting resins include polyphenylene ether resins, divinylbenzyl ether resins, polyarylate resins, diallyl phthalate resins, benzoxazole resins, bismaleimide resins, and acrylate resins.

[0108] Examples of methods for obtaining the insulating resin layer include the following methods. An extrusion molding method in which a material for forming the insulating resin layer is melt-kneaded using an extruder, extruded, and then molded into a film using a T-die or a circular die. A casting molding method in which a material for forming the insulating resin layer containing a solvent is cast into a film. Other conventionally known film molding methods. Alternatively, a material for forming the insulating resin layer can be laminated on a substrate film and dried by heating to obtain an insulating resin layer. Since the extrusion molding method or the casting molding method is suitable for thinning, the film includes a sheet.

[0109] The material for forming the insulating resin layer is formed into a film, and then heated and dried for 1 to 10 minutes at, for example, 50°C to 150°C to a degree that does not cause excessive curing by heat, to obtain an insulating resin layer that is a B-stage film.

[0110] The film-like insulating resin layer obtained by the drying process described above is called a B-stage film. The B-stage film is in a semi-cured state. The semi-cured product is not completely cured and can be further cured.

[0111] The insulating resin layer is preferably a B-stage film.

[0112] From the viewpoint of further improving the lamination properties of the insulating resin layer (the B-stage film, if the insulating resin layer is a B-stage film) and further suppressing uneven curing of the insulating resin layer, the thickness of the insulating resin layer is preferably 5 μm or more, more preferably 10 μm or more, preferably 200 μm or less, more preferably 100 μm or less.

[0113] (Protective film) The laminate film preferably has a protective film laminated on the surface of the insulating resin layer opposite to the base film side.

[0114] Examples of materials for the protective film include polyolefins such as polypropylene and polyethylene, and polyethylene terephthalate.

[0115] The material of the protective film is preferably polyolefin, more preferably polypropylene. In this case, the ratio (CN - Peak CN - Ion counts / Si - Peak Si - ion counts), and the above ratio (OH - Peak OH - Ion counts / Si - Peak Si -The number of ion counts can be easily controlled within the above preferred range.

[0116] From the viewpoint of further improving the protective properties of the insulating resin layer and further suppressing resin peeling, the thickness of the protective film is preferably 5 μm or more, more preferably 10 μm or more, preferably 70 μm or less, more preferably 50 μm or less, and even more preferably 40 μm or less.

[0117] (Other details of the laminated film) The length of the laminate film according to the present invention is preferably 20 m or more, more preferably 25 m or more, even more preferably 30 m or more, particularly preferably 50 m or more, and preferably 400 m or less, more preferably 300 m or less. With conventional laminate films, for example, when the length is 20 m or more, it is difficult to fully achieve the effects of the present invention, and when the length is 25 m or more, it is particularly difficult to fully achieve the effects of the present invention. With the laminate film according to the present invention, even when the length is 25 m or more, it is possible to fully achieve the effects of the present invention.

[0118] The laminated film according to the present invention is used to form an insulating layer in a multilayer printed wiring board. The insulating resin layer is used to form an insulating layer in a multilayer printed wiring board. The insulating layer can be formed by the insulating resin layer of the laminated film according to the present invention.

[0119] The multilayer printed wiring board includes, for example, a circuit board, a plurality of insulating layers disposed on a surface of the circuit board, and a metal layer disposed between the plurality of insulating layers, at least one of which is a cured product of the insulating resin layer.

[0120] Fig. 3 is a cross-sectional view showing a multilayer substrate using a laminate film according to one embodiment of the present invention. Specifically, Fig. 3 is a cross-sectional view showing a multilayer substrate using an insulating resin layer 2 in the laminate film 1 shown in Fig. 1.

[0121] In the multilayer printed wiring board 11 shown in FIG. 3, a plurality of insulating layers 13-16 are laminated on the upper surface 12a of the circuit board 12. The insulating layers 13-16 are cured layers. A metal layer 17 is formed on a partial region of the upper surface 12a of the circuit board 12. Of the plurality of insulating layers 13-16, the insulating layers 13-15 other than the insulating layer 16 located on the outer surface opposite to the circuit board 12 side have the metal layer 17 formed on a partial region of the upper surface. The metal layer 17 is a circuit. The metal layer 17 is disposed between the circuit board 12 and the insulating layer 13, and between each of the laminated insulating layers 13-16. The lower metal layer 17 and the upper metal layer 17 are connected to each other by at least one of a via hole connection and a through hole connection not shown.

[0122] In the multilayer printed wiring board 11, the insulating layers 13-16 are formed of a cured product of the insulating resin layer 2 (see FIG. 1). In this embodiment, the surfaces of the insulating layers 13-16 are roughened, so that fine holes (via holes) (not shown) are formed on the surfaces of the insulating layers 13-16. The metal layer 17 extends into the fine holes. In the multilayer printed wiring board 11, the width dimension (L) of the metal layer 17 and the width dimension (S) of the portion where the metal layer 17 is not formed can be reduced. In the multilayer printed wiring board 11, good insulation reliability is provided between the upper metal layer and the lower metal layer that are not connected by via hole connection and through hole connection (not shown).

[0123] (Roughening treatment and swelling treatment) The insulating resin layer is preferably used to obtain a cured product that is to be subjected to a roughening treatment or a desmear treatment. The cured product also includes a pre-cured product that can be further cured.

[0124] In order to form fine irregularities on the surface of the cured product obtained by pre-curing the insulating resin layer, the cured product is preferably subjected to a roughening treatment. The cured product is preferably subjected to a swelling treatment before the roughening treatment. The cured product is preferably subjected to a swelling treatment after the pre-curing and before the roughening treatment, and is further preferably cured after the roughening treatment. However, the cured product does not necessarily have to be subjected to a swelling treatment.

[0125] As a method of the swelling treatment, for example, a method of treating the cured product with an aqueous solution or an organic solvent dispersion solution of a compound mainly composed of ethylene glycol or the like is used. The swelling liquid used in the swelling treatment generally contains an alkali as a pH adjuster or the like. The swelling liquid preferably contains sodium hydroxide. Specifically, for example, the swelling treatment is performed by treating the cured product with a 40 wt% ethylene glycol aqueous solution or the like at a treatment temperature of 30°C to 85°C for 1 minute to 30 minutes. The temperature of the swelling treatment is preferably within the range of 50°C to 85°C. If the temperature of the swelling treatment is too low, the swelling treatment takes a long time, and the adhesive strength between the cured product and the metal layer tends to be lowered.

[0126] In the roughening treatment, a chemical oxidizing agent such as a manganese compound, a chromium compound, or a persulfate compound is used. These chemical oxidizing agents are used as an aqueous solution or an organic solvent dispersion after water or an organic solvent is added. The roughening solution used in the roughening treatment generally contains an alkali as a pH adjuster. The roughening solution preferably contains sodium hydroxide.

[0127] The manganese compounds include potassium permanganate and sodium permanganate. The chromium compounds include potassium dichromate and potassium chromate anhydride. The persulfate compounds include sodium persulfate, potassium persulfate, and ammonium persulfate.

[0128] The arithmetic mean roughness Ra of the surface of the cured product is preferably 10 nm or more, preferably less than 300 nm, more preferably less than 200 nm, and even more preferably less than 150 nm. In this case, the adhesive strength between the cured product and the metal layer is increased, and finer wiring is formed on the surface of the insulating layer. Furthermore, conductor loss can be suppressed, and signal loss can be suppressed. The arithmetic mean roughness Ra is measured in accordance with JIS B0601:1994.

[0129] (Desmear processing) A through hole may be formed in the cured product obtained by pre-curing the insulating resin layer. In the multilayer board, etc., a via or a through hole is formed as the through hole. For example, a via can be formed by irradiating a laser such as a CO2 laser. The diameter of the via is not particularly limited, but is about 60 μm to 80 μm. Due to the formation of the through hole, a smear, which is a resin residue derived from the resin component contained in the cured product, is often formed at the bottom of the via.

[0130] In order to remove the smears, the surface of the cured product is preferably subjected to a desmear treatment. The desmear treatment may also serve as a roughening treatment.

[0131] In the desmear treatment, a chemical oxidizing agent such as a manganese compound, a chromium compound, or a persulfate compound is used, as in the roughening treatment. These chemical oxidizing agents are used as an aqueous solution or an organic solvent dispersion after water or an organic solvent is added. The desmear treatment liquid used in the desmear treatment generally contains an alkali. The desmear treatment liquid preferably contains sodium hydroxide.

[0132] By using the insulating resin layer, the surface roughness of the cured product after the desmear treatment is sufficiently reduced.

[0133] The present invention will be specifically described below by way of examples and comparative examples, but the present invention is not limited to the following examples.

[0134] (Base film) Base film (polyethylene terephthalate (PET) film (Toray Industries, Inc. "XG284"), thickness 25 μm)

[0135] (Material for forming the insulating resin layer) The following materials were prepared as materials for forming the insulating resin layer.

[0136] <Epoxy compounds> Biphenyl type epoxy compound ("NC3000L" manufactured by Nippon Kayaku Co., Ltd.) Glycidylamine type epoxy compound (Mitsubishi Chemical Corporation "630") Fluorene-type epoxy compound ("PG-100" manufactured by Osaka Gas Chemicals) p-tert-Butylphenyl glycidyl ether (Nagase Chemtex Corporation "EX-146")

[0137] <Hardening agent> Active ester compound 1-containing liquid (DIC Corporation "HPC-8900-70BK", solid content 70% by weight) Active ester compound 2-containing liquid (DIC Corporation "HPC-8000L-65MT", solid content 65% by weight) Alkylphenol compound (DIC Corporation "DIC-POP") Carbodiimide compound-containing liquid (Nisshinbo Chemical's "V-03", solid content 50% by weight) Phenol compound ("H-4" manufactured by Meiwa Kasei Co., Ltd.)

[0138] <Curing accelerator> Dimethylaminopyridine ("DMAP" manufactured by Wako Pure Chemical Industries, Ltd.)

[0139] <Inorganic filler> Spherical silica 1: Spherical silica surface-treated with 0.6 parts by weight of N-phenyl-3-aminopropyl-trimethoxysilane ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd., molecular weight 255.4) per 100 parts by weight of spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd., average particle size 0.5 μm). Spherical silica 2: Spherical silica surface-treated with 0.76 parts by weight of N-phenyl-8-aminooctyl-trimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., molecular weight 325.2) per 100 parts by weight of spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd., average particle size 0.5 μm).

[0140] <Thermoplastic resin> Phenoxy resin-containing liquid (Mitsubishi Chemical Corporation "YX6954BH30", solid content 30% by weight) Polyimide resin-containing liquid: A polyimide resin-containing liquid (non-volatile content 26.8% by weight) which is a reaction product of tetracarboxylic acid and dimer diamine (synthesized in Synthesis Example 1 below)

[0141] Synthesis example 1: In a reaction vessel equipped with a stirrer, a water divider, a thermometer, and a nitrogen gas inlet tube, 300.0 g of tetracarboxylic dianhydride ("BisDA-1000" manufactured by SABIC Japan LLC) and 665.5 g of cyclohexanone were placed, and the solution in the vessel was heated to 60°C. Next, 89.0 g of dimer diamine ("PRIAMINE1075" manufactured by Croda Japan) and 54.7 g of 1,3-bisaminomethylcyclohexane (manufactured by Mitsubishi Gas Chemical Company, Inc.) were dropped. Then, 121.0 g of methylcyclohexane and 423.5 g of ethylene glycol dimethyl ether were placed, and an imidization reaction was carried out at 140°C for 10 hours, to obtain a polyimide resin-containing liquid (non-volatile content 26.8% by weight). The molecular weight (weight average molecular weight) of the obtained polyimide resin was 20,000. The molar ratio of the acid component / amine component was 1.04. The molecular weight of the polyimide resin was measured as follows.

[0142] GPC (Gel Permeation Chromatography) Measurement: The measurements were performed using a Shimadzu high-performance liquid chromatograph system with tetrahydrofuran (THF) as the developing medium at a column temperature of 40°C and a flow rate of 1.0 ml / min. The detector used was an SPD-10A, and two Shodex KF-804L columns (with an exclusion limit of 400,000) were connected in series. The standard polystyrene used was TSK Standard Polystyrene from Tosoh, with weight-average molecular weights Mw = 354,000, 189,000, 98,900, 37,200, 17,100, 9,830, 5,870, 2,500, 1,050, and 500, to create a calibration curve and calculate the molecular weight.

[0143] (Protective film) Protective film A ("MA-411" manufactured by Oji F-Tex Co., Ltd., thickness 15 μm) Protective film B (Oji F-Tex "FG-201"), thickness 30 μm)

[0144] (Examples 1 to 8 and Comparative Examples 1 to 2) (1) Preparation of insulating resin layer material The components of the insulating resin layer material shown in Tables 2 and 3 below were mixed in the amounts (solid weight) shown in Tables 2 and 3 below, and stirred at 1200 rpm for 4 hours using a stirrer to obtain the insulating resin layer material (varnish).

[0145] (2) Preparation of laminated film and roll body FIG. 4 is a schematic diagram showing the laminated film manufacturing apparatus used in the examples. The laminated film manufacturing apparatus 20 includes a feed roller 21, a coating roll 22, a first heat drying section 23, a second heat drying section 24, a roll 25, and a take-up roll 26. A base film 31 (polyethylene terephthalate film) was conveyed from the feed roller 21. On the coating roll 22, a material (varnish) for the insulating resin layer was applied to the surface of the base film 31 by a die coating method. The base film 31 coated with the material (varnish) for the insulating resin layer was conveyed at a conveying speed such that the content of the solvent in the material for the insulating resin layer was 4% by weight (the weight loss amount after heat treatment at 160°C for 30 minutes was 4% by weight), and a drying operation was performed under the drying conditions A, B, or C (first drying step, second drying step, third drying step) shown in Table 1 and below.

[0146] <First drying process> After the insulating resin layer material (varnish) was applied to the surface of the base film 31, the base film 31 coated with the insulating resin layer material (varnish) was transported and dried at room temperature (25°C) without blowing air on it.

[0147] <Second drying process> After the first drying step, the material was conveyed while being dried in the first heating and drying section 23 under the drying conditions shown in Table 1, using a blowing nozzle with a large opening area (one opening area of ​​72000 mm 2 ) at a wind speed of 1 m / s to perform heat drying. In the second drying step, the heating temperature was set as shown in Table 1 when the drying time in the second drying step was divided into three. For example, in drying condition A, the sample was heated at 80°C, then heated at 100°C, and then heated at 120°C.

[0148] <Third drying process> After the second drying step, the material was conveyed while being dried in the second heating and drying section 24 under the drying conditions shown in Table 1, using a blowing nozzle with a small opening area (one opening area of ​​3600 mm 2 ) at a speed of 1 m / s to heat and dry the sample.

[0149]

Table 1

[0150] In this way, a film was obtained in which an insulating resin layer with a thickness of 40 μm was disposed on the base film. Next, the protective film 32 unwound from the roll 25 was thermally laminated at 50° C. on the surface of the insulating resin layer opposite to the base film side, thereby obtaining a laminated film 33 including the base film, the insulating resin layer, and the protective film. Note that the obtained insulating resin layer is a B-stage film.

[0151] Next, the obtained laminated film 33 was wound around the outer periphery of a winding core (manufactured by Showa Kankyo Co., Ltd., “Plastic Core”, material ABS, inner diameter 3 inches) by a winding roll 26 under the condition of a winding tension of 50 N, thereby obtaining a roll body. Note that as the roll body, three types of roll bodies were produced: a roll body (100 m) wound with 100 m of the laminated film, a roll body (200 m) wound with 200 m of the laminated film, and a roll body (300 m) wound with 300 m of the laminated film.

[0152] (Evaluation) (1) Analysis by time-of-flight secondary ion mass spectrometry (TOF-SIMS) The protective film of the obtained laminated film was peeled off to expose the surface of the insulating resin layer. Using a time-of-flight secondary ion mass spectrometer (TOF-SIMS5 manufactured by ION-TOF), the surface of the exposed insulating resin layer was analyzed under the following measurement conditions. Note that the count number of ions at each peak was the average value of the count numbers of ions at any three locations separated from each other by 500 μm or more. Also, the count number of ions at each peak was measured at a position 1 mm or more inside from the end face of the laminated film.

[0153] <Measurement Conditions by TOF-SIMS> For the surface of the exposed insulating resin layer, Bi 3-- ion gun was used as the primary ion source, and under the following conditions, CN - peak of CN - count number of ions, Si- Peak Si - Ion counts and OH - Peak OH - The number of ions counted was measured. The analysis area was 500 μm × 500 μm.

[0154] Primary ion: 25kV, Bi 3-- , 0.1pA~0.3pA (pulse current value) Random Scan Mode Primary ion scan range (measurement area): 500μm×500μm Secondary ion detection mode: negative (uses flat gun for charge compensation) The following ratios were calculated from the counts of each ion in each peak obtained.

[0155] 1) Ratio (CN - Peak CN - Ion counts / Si - Peak Si - (Number of ion counts) 2) Ratio (OH - Peak OH - Ion counts / Si - Peak Si - (Number of ion counts)

[0156] (2) Resin peeling (a phenomenon in which part of the insulating resin layer peels off together with the protective film) (2-1) Peeling of resin from roll body after storage The obtained roll (100 m) was stored at 25° C. for 2 days. The roll after storage was set in an autocutter manufactured by Shin-Ei Kiko Co., Ltd., and the protective film was peeled off while unwinding. When the protective film was peeled off, a part of the insulating resin layer was peeled off together with the protective film, and it was observed whether the insulating resin layer was attached to the protective film.

[0157] [Evaluation criteria for peeling of resin from roll body after storage] ○: Resin peeling occurs ×: Resin does not peel off

[0158] (2-2) Peeling of resin from long roll body The protective film was peeled off from the obtained rolls (100 m), (200 m), and (300 m). When the protective film was peeled off, a part of the insulating resin layer was peeled off together with the protective film, and it was observed whether the insulating resin layer was attached to the protective film.

[0159] [Evaluation criteria for resin peeling from each roll body] A: Resin peeling occurs B: No resin peeling occurs

[0160] [Overall evaluation criteria for resin peeling from long roll body] ○○: All evaluations for roll body (100m), roll body (200m), and roll body (300m) are A ○: The evaluation for the roll body (100m) and the roll body (200m) is A, and the evaluation for the roll body (300m) is B △: The roll body (100m) was rated A, and the roll body (200m) and roll body (300m) were rated B. ×: All evaluations for roll body (100m), roll body (200m), and roll body (300m) were B

[0161] (3) Lifting and wrinkles The obtained roll (200 m) was attached to a slitter manufactured by Hagiwara Kogyo Co., Ltd., and the laminated film was unwound without slitting at a speed of 20 m / min with an unwinding force of 40 N, a winding tension of 50 N, and a roll-up tension of 20 N. The unwound laminated film was observed to check for lifting (peeling at the interface between the insulating resin layer and the protective film) and the occurrence of wrinkles.

[0162] [Float evaluation criteria] ○: 0 floats after unwinding 200m △: When 200m is unwound, there are 1 to 3 floating pieces. ×: Three or more floats are found when 200m is unwound

[0163] [Wrinkle evaluation criteria] ○○: When 200m is unwound, there are 0 wrinkles ○: When 200m is unwound, there are 1 to 3 wrinkles △: When 200m is unwound, there are 3 to 5 wrinkles ×: 5 or more wrinkles found when 200m is unwound

[0164] The composition of the laminated film and the results are shown in Tables 2 and 3 below.

[0165] [Table 2]

[0166] [Table 3] [Explanation of symbols]

[0167] 1...Laminated film 2...Insulating resin layer 2a…First surface 2b…Second surface 3...Base film 4. Protective film 11...Multilayer printed wiring board 12...Circuit board 12a…Top surface 13~16…Insulating layer 17...Metal layer 20...Laminated film manufacturing equipment 21...Feed roller 22...Coating roll 23...First heating and drying section 24...Second heating and drying section 25…Roll 26…Take-up roll 31...Base film 32…Protection film 33...Laminated film 51...Roll body 61...Core

Claims

1. A base film; an insulating resin layer disposed on a surface of the base film; a protective film laminated on a surface of the insulating resin layer opposite to the base film side, The insulating resin layer is used to form an insulating layer in a multilayer printed wiring board, When the surface of the insulating resin layer exposed by peeling off the protective film was analyzed by time-of-flight secondary ion mass spectrometry, CN - Peak and Si - Peaks are present and OH - The peak may or may not be present, and the CN - Peak CN - The number of ion counts of the Si - Peak Si - A laminated film having a ratio of ion counts greater than 50 and less than 6,000.

2. The CN - Peak CN - The number of ion counts of the Si - Peak Si - 2. The laminated film of claim 1, wherein the ratio of ions to counts is less than 5,000.

3. The CN - Peak CN - The number of ion counts of the Si - Peak Si - 2. The laminated film of claim 1, wherein the ratio of ions to counts is less than 4,000.

4. The OH - There is a peak, The OH - Peak OH - The number of ion counts of the Si - Peak Si - The laminated film according to any one of claims 1 to 3, wherein the ratio of the number of ions to the number of counts is less than 2,000.

5. The OH - Peak OH - The number of ion counts of the Si - Peak Si - 5. The laminated film according to claim 4, wherein the ratio of ions to counts is less than 1,000.

6. A winding core and The laminate film according to any one of claims 1 to 5, The laminated film is wound around the outer periphery of the winding core.

Citation Information

Patent Citations

  • Adhesive sheet with protection film

    JP2016020480A

  • Thermosetting resin composition, dry film, cured product, and electronic component

    JP2019167426A

  • Bonded joint structure and automobile component

    JP2020055144A

  • Organic insulating body, metal-clad laminate and wiring board

    WO2018016527A1