Polar anisotropic magnet, rotor using polar anisotropic magnet, rotating machine, and method for manufacturing polar anisotropic magnet
By aligning neodymium magnet powder in a quasi-cylindrical mold using orientation magnetic fields, the method achieves high surface magnetic flux density in polar anisotropic magnets, enhancing rotating machine performance and reducing costs.
Patent Information
- Application Number
- JP2021026007
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-28
- Filing Date
- 2021-02-22
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2041-02-22
AI Technical Summary
Conventional methods for manufacturing polar anisotropic magnets are costly due to the use of core rods and often result in deviations in orientation direction, leading to insufficient surface magnetic flux density.
A quasi-cylindrical mold cavity is used with specific lubricant application and orientation magnetic fields to align neodymium magnet powder, ensuring high surface magnetic flux density and reducing costs.
The method produces cylindrical polar anisotropic magnets with high surface magnetic flux density, enabling high-performance rotating machines that can rotate at higher speeds and reduce eddy current losses, resulting in smaller, lighter, and more efficient motors and generators.
Smart Images

Figure 0007561056000004 
Figure 0007561056000005 
Figure 0007561056000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a polar anisotropic magnet, a rotor using a polar anisotropic magnet, a rotating machine, and a method for manufacturing a polar anisotropic magnet. [Background technology]
[0002] Conventionally, polar anisotropic magnets have been considered for use in rotors used in rotating machines such as motors and generators in order to reduce their size and weight. However, due to difficulties in achieving the desired shape, orientation, and cost reduction, practical polar anisotropic magnets have hardly been realized. Patent Document 1 describes a magnetic field molding apparatus used to manufacture polar anisotropic magnets, in which the magnetization direction is normal at the magnetic pole position and tangential at the intermediate position between adjacent magnetic poles, and when the magnetic pole position and the intermediate position adjacent to it are divided into elements with equal angular pitch, the magnetization directions of adjacent elements have a substantially constant angular difference. The magnetic field molding apparatus has a molding die having a gap with a circular cross section, a cylindrical core rod placed at the center of the circular cross section gap of the molding die to form a ring-shaped cavity, a plurality of gaps opening to the inner surface of the molding die, and a plurality of coils placed in each gap, the plurality of coils are arranged along the cavity, and the ratio of the central angle θ1 formed by the plurality of coils along the cavity in each gap to the central angle θ2 formed by the coils in adjacent gaps is 0.8 to 1.2. It is also described that such a magnetic field molding apparatus can produce polar-anisotropic ring magnets that have a stably high sine wave matching rate of the surface magnetic flux density distribution and that generate virtually no cogging torque when incorporated into a motor. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 3997427 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the manufacturing method of using a magnetic field molding device to produce ring-shaped magnets as described in Patent Document 1 requires a core rod, which makes it costly, and there can be a misalignment between the direction of the magnetic field generated by the magnetizer and the orientation direction of the magnet powder, resulting in a problem that sufficient surface magnetic flux density of the polar anisotropic magnet cannot be obtained.
[0005] The present invention has been made in view of the above circumstances in order to solve the following technical problems. A first object of the present invention is to provide a cylindrical or columnar polar anisotropic magnet that has a higher surface magnetic flux density while being less expensive than conventional magnets. A second object of the present invention is to provide a rotor that uses a polar anisotropic magnet with a large surface magnetic flux density, and that is capable of supplying a large magnetic flux to the stator while keeping costs low. A third object of the present invention is to provide a rotating machine such as a motor or generator that employs a polar anisotropic magnet that generates a large surface magnetic flux density, and that has higher performance and is capable of rotating at higher speeds than conventional machines. [Means for solving the problem]
[0006] Through extensive research, the inventors came up with the idea of a pseudo-cylindrical mold cavity that takes into consideration the fact that the shrinkage rate due to sintering differs greatly between the direction of the easy magnetization axis and the direction perpendicular to it. By filling this cavity with neodymium magnet powder of a specific particle size to which a specific amount of lubricant has been added so as to achieve a specific packing density, and then applying an aligning magnetic field within a specific range, the neodymium magnet powder can be aligned along its easy magnetization axis, i.e., the cubic phase that constitutes the main phase of the powder, NdFe 14 They discovered that the c-axis of the B phase can be oriented along the magnetic flux flow, and that by sintering the resulting material together with the mold, a cylindrical or columnar polar anisotropic magnet with a high surface magnetic flux density can be obtained, thus completing the present invention.
[0007] The present invention relates to the following (1) to (14). (1) A cylindrical or columnar polar anisotropic magnet with 2N poles, where N is a multiple of the natural number. (2) A polar anisotropic magnet according to (1) above, characterized in that the surface magnetic flux density at the magnetic pole positions in the circumferential direction of the cylindrical or columnar shape is 450 mT or more. (3) A polar-anisotropic magnet as described in (1) or (2) above, characterized in that the amount of magnetic flux leaking in the circumferential direction of the cylindrical or columnar shape is formed into a sine wave synchronized with the number of poles, and when the sine wave is taken as the primary component, the overall ratio of harmonic components excluding the primary component is 10% or less. (4) A polar anisotropic magnet according to any one of (1) to (3) above, characterized in that the variation in the amount of leakage magnetic flux in the axial direction of the cylindrical or columnar shape is within ±5% of the average value of the amount of leakage magnetic flux throughout the top and bottom of the coaxial shape. (5) A rotor in which the outer surface of the polar anisotropic magnet according to any one of (1) to (4) above is covered with a protective tube. (6) A rotor according to (5) above, having a shaft on the outside of both end faces of the polar anisotropic magnet. (7) A rotor according to (5) or (6) above, which is rotatable at 20,000 rpm or more. (8) A rotating machine comprising the rotor according to any one of (5) to (7) above and a stator with concentrated winding or distributed winding. (9) The rotating machine according to (8) above, which is mounted on a moving body for use. (10) A neodymium magnet powder having an average particle size of 1.0 to 5.0 μm and containing 1.0 mass % or less of a lubricant is added at a concentration of 3.4 to 4.0 g / cm 3 a filling step of filling the powder into a quasi-cylindrical mold cavity with a packing density of 0.1 to 0.5 to obtain a powder-filled mold; an orientation step of loading the powder-filled mold into an orientation device and applying an orientation magnetic field of 1.0 to 5.0 T to the filled neodymium magnet powder without applying pressure to orient the neodymium magnet powder to obtain an oriented mold; a sintering step of inserting the oriented mold into a sintering furnace and sintering the mold together to obtain a sintered body; A method for manufacturing a cylindrical or columnar polar anisotropic magnet, comprising: (11) A method for producing a polar anisotropic magnet as described in (10) above, characterized in that the shape of the mold cavity is designed so that the sintered body has a cylindrical or columnar shape. (12) A method for producing a polar anisotropic magnet as described in (10) or (11) above, characterized in that in the orientation step, an orientation device capable of orienting the magnet to have an anisotropy of 2N poles, where the number of poles is a multiple of the natural number N, is used. (13) The orientation step comprises: the step of loading the powder-filled mold into an orientation device, applying a magnetic field in a direction perpendicular to the orientation direction without applying pressure to the filled neodymium magnet powder, and then applying an orientation magnetic field of 1.0 to 5.0 T in the orientation direction to orient the neodymium magnet powder and obtain the oriented mold; A method for producing a polar anisotropic magnet according to any one of (10) to (12) above. (14) A method for producing a polar anisotropic magnet, comprising contacting the surface of a polar anisotropic magnet produced by the method according to any one of (10) to (13) above with a heavy rare earth metal (R) or an R-based alloy containing a heavy rare earth metal (wherein R is at least one element selected from Dy, Tb and Ho), and then heat treating the magnet to diffuse the R element into the magnet. Effect of the Invention
[0008] According to the present invention, a cylindrical or columnar polar anisotropic magnet having a high surface magnetic flux density can be obtained at low cost. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic perspective view of a mold for producing a cylindrical two-pole polar anisotropic magnet. [Diagram 2] FIG. 1 is a schematic perspective view of a mold for producing a cylindrical four-pole polar anisotropic magnet. [Diagram 3] FIG. 13 is a schematic perspective view of another mold for producing a cylindrical four-pole polar anisotropic magnet. [Figure 4]FIG. 2 is a schematic top view showing the state in which a powder-filled mold, which is formed by filling a mold with neodymium magnet powder when producing a cylindrical two-pole polar anisotropic magnet, is loaded into an orientation device. [Diagram 5] FIG. 2 is a schematic top view showing the state in which a powder-filled mold, which is formed by filling a mold with neodymium magnet powder when producing a cylindrical four-pole polar anisotropic magnet, is loaded into an orientation device. [Figure 6] FIG. 2 is a schematic top view showing another powder-filled mold, obtained by filling a mold with neodymium magnet powder when producing a cylindrical four-pole polar anisotropic magnet, loaded into an orientation device. [Figure 7] FIG. 1 is a schematic perspective view showing a two-pole polar anisotropic magnet obtained by the manufacturing method of the present invention. [Figure 8] FIG. 1 is a schematic perspective view showing a four-pole polar anisotropic magnet obtained by the manufacturing method of the present invention. [Figure 9] 10A and 10B are diagrams for explaining a method for measuring the variation in the amount of leakage magnetic flux in the axial direction. [Figure 10] 1 is a schematic cross-sectional view showing a magnet of the present invention with two shafts arranged thereon and further covered with a protective tube. [Figure 11] FIG. 2 is a schematic cross-sectional view of a motor. [Figure 12] 1 is a graph showing waveforms of surface magnetic flux density in the circumferential direction in Example 1 and Comparative Examples 1, 2, and 4. [Figure 13] 4 is a graph showing variation in the amount of magnetic flux in the central axis direction in Example 1. [Figure 14] This figure shows the positional relationship between the magnet center point O, the magnet end X parallel to O, and the magnet end Y perpendicular to O in the upper right quarter of the magnet obtained in Example 9 when viewed from above (axial direction). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The manufacturing method of the present invention will now be described. The present invention provides a neodymium magnet powder having an average particle size of 1.0 to 5.0 μm and containing 1.0 mass % or less of a lubricant, at a concentration of 3.4 to 4.0 g / cm. 3 and an orienting step of loading the powder-filled mold into an orienting device and applying an orienting magnetic field of 1.0 to 5.0 T to the filled neodymium magnet powder without applying pressure to orient the neodymium magnet powder to obtain an oriented mold. The method of manufacturing a cylindrical or columnar polar anisotropic magnet includes the steps of: filling a pseudo-cylindrical mold cavity with the powder at a filling density of 1.0 to 5.0 T to obtain a powder-filled mold; and sintering the oriented mold into a sintering furnace and sintering the mold together to obtain a sintered body. This method of manufacturing a cylindrical or columnar polar anisotropic magnet is hereinafter referred to as the "manufacturing method of the present invention."
[0011] <Filling process> In the filling step of the manufacturing method of the present invention, neodymium magnet powder is prepared.
[0012] Neodymium magnet powder is a powder whose main components are neodymium, a transition element (T), and boron (B). Here, the term "main component" means that the total content is 90% by mass or more, and the total content is more preferably 95% by mass or more. The transition element (T) preferably contains Fe, Co, Ni, etc. In particular, Nd-Fe-B based neodymium magnet powder is preferred.
[0013] The average particle size of the neodymium magnet powder is 1.0 to 5.0 μm, and preferably 2.5 to 3.5 μm. Neodymium magnet powder consists of an Nd-rich phase, which is the grain boundary phase component, and an NdFe 14It is preferable that the main phase is composed of single crystal particles of phase A and phase B. If the main phase is single crystal, the particles have one easy axis of magnetization, so the particles tend to be oriented in the direction of the generated magnetic flux, resulting in a magnet with a higher magnetic flux density. If the average particle size is 1.0 to 5.0 μm, it is considered that almost all of the particles are single crystal particles. Here, the average particle size is defined as the median (D 50 ) was decided.
[0014] There is no particular limitation on the method for preparing the neodymium magnet powder, for example, a method in which a molten master alloy is sprayed onto a rotating roll and quenched to obtain a ribbon with a fine crystal structure, and then the ribbon is crushed to an average particle size of 1.0 to 5.0 μm to obtain the neodymium magnet powder can be used.
[0015] Such neodymium magnet powders contain a lubricant at a content of 1.0 mass% or less. The lubricant content in the neodymium magnet powders is preferably 0.01 mass% or more, and more preferably 0.05 to 1.0 mass%.
[0016] As the lubricant, methyl caprylate, methyl laurate, zinc stearate, etc. can be used.
[0017] The above-mentioned lubricant is added to the neodymium magnet powder, and after thorough mixing, the mixture is filled into a quasi-cylindrical mold cavity.
[0018] The filling density when filling the neodymium magnet powder into the mold cavity is 3.4 to 4.0 g / cm 3 The packing density is 3.5 to 3.9 g / cm 3 It is preferable to set the above.
[0019] In the manufacturing method of the present invention, in the filling step, neodymium magnet powder is filled into the mold cavity to achieve a specific filling density to obtain a neodymium magnet powder compact, which is then oriented and sintered to obtain a cylindrical or columnar polar anisotropic magnet. However, when a cylindrical or columnar neodymium magnet powder compact is formed in the filling step, the shape of the polar anisotropic magnet obtained by orienting and sintering this will not be cylindrical or columnar. This is because, when the compact is sintered, the shrinkage rate in the direction of the easy magnetization axis is significantly different from that in the direction perpendicular thereto. Therefore, the present inventors conducted extensive research as described below into the shape of the compact of neodymium magnet powder that would enable the polar anisotropic magnet obtained by the manufacturing method of the present invention to have a cylindrical or columnar shape, i.e., the shape of the mold cavity.
[0020] First, the inventors of the present invention prepared a neodymium magnet powder having an average particle size of 1.0 to 5.0 μm and containing 1.0 mass % or less of a lubricant at a concentration of 3.4 to 4.0 g / cm. 3 The neodymium magnet powder was then filled into a cylindrical mold cavity at a packing density of 1000g / m² / g, and the mold filled with the neodymium magnet powder was then subjected to the orientation step and sintering step in the manufacturing method of the present invention to obtain a polar anisotropic magnet. As a result, the shape of the obtained polar anisotropic magnet was not cylindrical, but rather resembled a prism with two end faces that were nearly square in shape with rounded corners. This suggests that when a compact of the neodymium magnet powder is sintered, shrinkage is less likely to occur in the direction perpendicular to the direction of the easy axis of magnetization.
[0021] Therefore, the present inventors conducted repeated experiments and investigated the relationship between the amount of shrinkage in the direction of the easy magnetization axis during sintering and the amount of shrinkage in the direction perpendicular thereto. Here, the amount of shrinkage due to sintering is affected by various factors such as the composition of the magnet powder, particle size, the amount and type of lubricant, packing density, etc. Therefore, the present inventors conducted extensive research and discovered that a neodymium magnet powder with an average particle size of 1.0 to 5.0 μm and containing 1.0 mass % or less of lubricant can be produced at a packing density of 3.4 to 4.0 g / cm. 3It has been found that, when a compact filled at a packing density of 1000 to 10000 mm is subjected to the orientation step and sintering step in the manufacturing method of the present invention, the amount of shrinkage (b) in the direction of easy magnetization during sintering is larger than the amount of shrinkage (a) in the direction perpendicular thereto, and the ratio (b / a) is 1.25 to 1.37, preferably 1.28 to 1.34, more preferably 1.30 to 1.32, and even more preferably about 1.31. As mentioned above, the amount of shrinkage caused by sintering varies depending on various factors, so this ratio (b / a) should be determined by conducting several preliminary experiments so that the end faces of the resulting polar anisotropic magnet will be perfectly round. However, the inventors have found that the approximate range of this ratio (b / a) is as described above when using the manufacturing method of the present invention.
[0022] Next, based on the findings from the measurement results of the ratio (b / a) above, the present inventors investigated the shape of the mold cavity. The mold cavity is a space defined by the inner surface of the mold that contains the neodymium magnet powder.
[0023] Figure 1 shows a mold 10 used to produce a cylindrical two-pole polar anisotropic magnet. Mold 10 has two end faces 12, 14, a side face 16, and an inner face 18. The portion formed by inner face 18 corresponds to mold cavity 19, into which neodymium magnet powder is filled. The cross section and end faces of mold cavity 19 are elliptical, as shown in Figure 1. As shown in FIG. 1, the length of the major axis of mold cavity 19 at two end faces 12, 14 is b, the length of the minor axis is a, and the ratio thereof (b / a) is set to 1.25 to 1.37 (preferably about 1.31). When manufacturing a polar anisotropic magnet that is cylindrical rather than columnar, this can be achieved, for example, by previously providing an elongated cylinder, elliptical cylinder, rectangular cylinder, etc., or by arranging a core rod at the center of the mold cavity shaped as shown in Figure 1 (the intersection of the direction in which length b is measured and the direction in which length a is measured).
[0024] Fig. 2 shows a mold 20 used to obtain a cylindrical four-pole polar anisotropic magnet. Mold 20 has two end faces 22, 24, a side face 26, and an inner face 28. The portion formed by inner face 28 is mold cavity 29, into which neodymium magnet powder is filled. At end faces 22, 24, the cross section and end faces of mold cavity 29 have a shape formed by two ellipses crossing at right angles, as shown in Fig. 2. As shown in FIG. 2, for each of the two end faces 22, 24 of the mold cavity 29, the length between the two farthest points on the outer circumference is defined as b, and the length in the direction forming 45 degrees with respect to both directions in which the length b is measured is defined as a, with the ratio of these (b / a) being 1.25 to 1.37 (preferably about 1.31). When manufacturing a polar anisotropic magnet that is cylindrical rather than columnar, this can be achieved, for example, by previously providing an elongated cylinder, elliptical cylinder, rectangular cylinder, etc., or by arranging a core rod at the center of the mold cavity shaped as shown in Figure 2 (the intersection of the direction in which length b is measured and the direction in which length a is measured).
[0025] FIG. 3 shows a mold 30 used to obtain a cylindrical four-pole polar anisotropic magnet. The mold 30 shown in FIG. 3 has a slightly different shape from the mold 20 shown in FIG. 2, but both are molds used to obtain cylindrical four-pole polar anisotropic magnets. The mold 30 has two end faces 32, 34, a side face 36, and an inner face 38. The inner face 38 defines a mold cavity 39 into which neodymium magnet powder is filled. At the end faces 32, 34, the cross section and end faces of the mold cavity 39 have a square shape with rounded corners, as shown in FIG. Comparing mold cavity 29 shown in Fig. 2 with mold cavity 39 shown in Fig. 3, it can be seen that mold cavity 29 shown in Fig. 2 has a recessed (or protruding) portion that is more inward than mold cavity 39 shown in Fig. 3. By controlling the shape of this portion and the strength of the magnetic field applied in the orientation step described below, it is possible to obtain the intended polar anisotropic orientation. As shown in FIG. 3, for each of the two end faces 32, 34 of the mold cavity 39, the length between the two farthest points on the outer circumference is defined as b, and the length in the direction forming 45 degrees with respect to both directions in which the length b is measured is defined as a, with the ratio of these (b / a) being 1.25 to 1.37 (preferably about 1.31). When manufacturing a polar anisotropic magnet that is cylindrical rather than columnar, this can be achieved, for example, by previously providing an elongated cylinder, elliptical cylinder, rectangular cylinder, etc., or by arranging a core rod at the center of the mold cavity shaped as shown in Figure 3 (the intersection of the direction in which length b is measured and the direction in which length a is measured).
[0026] Note that Figure 1 shows an example of a mold for producing a two-pole polar anisotropic magnet, and Figures 2 and 3 show an example of a mold for producing a four-pole polar anisotropic magnet, but a mold for producing six or more poles polar anisotropic magnets can also be designed using the same concept.
[0027] In the manufacturing method of the present invention, the mold cavity shapes exemplified in Figures 1, 2, and 3 are defined as pseudo-cylindrical. In other words, a mold cavity shape that is not cylindrical but close to cylindrical, and that results in a polar anisotropic magnet obtained by the manufacturing method of the present invention having a cylindrical or cylindrical shape, is defined as pseudo-cylindrical.
[0028] The mold is preferably made of a non-magnetic material, such as graphite carbon.
[0029] Although the outer diameters of the molds 10, 20 and 30 in Figs. 1, 2 and 3 are cylindrical, this shape is not particularly limited.
[0030] In the manufacturing method of the present invention, as described above, it is preferable that the shape of the mold cavity is designed so that the sintered body obtained by the sintering step described below has a cylindrical or columnar shape, because the sintered body can be used as a rotor as it is without processing it.
[0031] In the filling step of the manufacturing method of the present invention, the neodymium magnet powder is filled into such a quasi-cylindrical mold cavity to achieve the above-mentioned filling density. The mold thus obtained, filled with the neodymium magnet powder, is referred to as a powder-filled mold. Moreover, the mold 10 shown in Fig. 1 after being filled with the neodymium magnet powder is referred to as a powder-filled mold 40. Moreover, the mold 20 shown in Fig. 2 after being filled with the neodymium magnet powder is referred to as a powder-filled mold 50. Furthermore, the mold 30 shown in Fig. 3 after being filled with the neodymium magnet powder is referred to as a powder-filled mold 60.
[0032] <Orientation process> In the orienting step in the manufacturing method of the present invention, the powder-filled mold is loaded into an orienting device and an orienting magnetic field is applied thereto. In the orientation step, an orientation device capable of orienting the film to have anisotropy of 2N poles, where the number of poles is a multiple of a natural number N, can be used.
[0033] For example, when a two-pole polar anisotropic magnet is to be obtained by the manufacturing method of the present invention, a powder-filled mold 40 is loaded into an orientation device as shown in FIG. FIG. 4 is a diagram (schematic diagram) seen from above showing a state in which a powder-filled mold 40 obtained by filling the mold cavity 19 in the mold 10 illustrated in FIG. 1 with the neodymium magnet powder is loaded into an orientation device. As shown in Fig. 4, two coils 42 are arranged at positions sandwiching the powder-filled mold 40 from the short axis direction. The coils 42 can generate a magnetic field whose polarity is shown by the dotted lines in Fig. 4. In the state shown in Figure 4, by applying an aligning magnetic field of 1.0 to 5.0 T without applying pressure to the filled neodymium magnet powder, the magnetization easy axis of the neodymium magnet powder can be oriented so as to be parallel to the dotted line shown in Figure 4. In other words, the dotted line is the orientation direction. In this way, a polar anisotropic magnet can be obtained in which the orientation direction is normal to the magnetic pole positions in the circumferential direction, tangential to the intermediate positions between adjacent magnetic poles, and curved at these intermediate positions.
[0034] Also, for example, when a four-pole polar anisotropic magnet is obtained by the manufacturing method of the present invention, a powder-filled mold 50 is loaded into an orientation device as shown in FIG. FIG. 5 is a diagram (schematic diagram) seen from above showing a state in which a powder-filled mold 50 obtained by filling the mold cavity 29 in the mold 20 illustrated in FIG. 2 with the neodymium magnet powder is loaded into an orientation device. As shown in Fig. 5, a total of four coils 52 are arranged at positions sandwiching the powder-filled mold 50 from each of its two short diameter directions (the direction in which the length a is measured). The coils 52 can generate a magnetic field whose polarity and dotted lines are shown in Fig. 5. In the state shown in Figure 5, by applying an aligning magnetic field of 1.0 to 5.0 T without applying pressure to the filled neodymium magnet powder, the magnetization easy axis of the neodymium magnet powder can be oriented so as to be parallel to the dotted line shown in Figure 5. In other words, the dotted line is the orientation direction.
[0035] Also, for example, when a four-pole polar anisotropic magnet is to be obtained by the manufacturing method of the present invention, a powder-filled mold 60 is loaded into an orientation device as shown in FIG. FIG. 6 is a diagram (schematic diagram) seen from above showing a state in which a powder-filled mold 60 obtained by filling the mold cavity 39 in the mold 30 illustrated in FIG. 3 with the neodymium magnet powder is loaded into an orientation device. As shown in Figure 6, a total of four coils 62 are placed on the powder-filled mold 60 in the same position as in Figure 5. The coils 62 can generate a magnetic field whose polarity and dotted lines are shown in Figure 6. In the state shown in Figure 6, by applying an aligning magnetic field of 1.0 to 5.0 T without applying pressure to the filled neodymium magnet powder, the magnetization easy axis of the neodymium magnet powder can be oriented so as to be parallel to the dotted line shown in Figure 6. In other words, the dotted line is the orientation direction.
[0036] Note that Figure 4 illustrates an orientation device for obtaining a two-pole polar anisotropic magnet using the manufacturing method of the present invention, and Figures 5 and 6 illustrate orientation devices for obtaining a four-pole polar anisotropic magnet using the manufacturing method of the present invention, but orientation devices for obtaining six or more poles polar anisotropic magnets can also be designed using the same concept.
[0037] In the orienting step, the orienting magnetic field applied to the neodymium magnet powder is 1.0 to 5.0 T, but this orienting magnetic field is preferably 1.5 to 3.0 T, and more preferably about 2.0 to 2.5 T.
[0038] In the orientation step, the liquid crystal is oriented in the orientation direction as described above. However, it is preferable to apply a magnetic field in a direction perpendicular to the orientation direction before the orientation step, and then apply an aligning magnetic field in the orientation direction as described above to align the liquid crystal. In other words, the orientation step is preferably a step of loading the powder-filled mold into an orientation device, applying pressure to the filled neodymium magnet powder in a direction perpendicular to the orientation direction without applying pressure to the neodymium magnet powder, and then applying an orientation magnetic field of 1.0 to 5.0 T in the orientation direction to orient the neodymium magnet powder and obtain the oriented mold. In this case, the present inventors have found that a polar anisotropic magnet with fewer cracks can be obtained by the manufacturing method of the present invention.
[0039] Here, the direction perpendicular to the orientation direction usually coincides with the depth direction in the mold cavity, and also usually coincides with the direction parallel to the central axis of the resulting cylindrical or columnar polar anisotropic magnet.
[0040] The magnetic field applied in the direction perpendicular to the orientation direction may be of the same order as the magnetic field applied in the orientation direction (orientation magnetic field) described above. That is, the magnetic field applied in the direction perpendicular to the orientation direction may be 1.0 to 5.0 T, preferably 1.5 to 3.0 T, and more preferably about 2.0 to 2.5 T.
[0041] By this orientation process, a mold can be obtained in which the oriented neodymium magnet powder is filled into the mold cavity. Such a mold is called an oriented mold.
[0042] <Sintering process> In the sintering step in the manufacturing method of the present invention, the oriented mold obtained in the orientation step is loaded into a sintering furnace and sintered together with the mold.
[0043] The sintering method is not particularly limited. For example, the oriented mold can be placed in a conventionally known sintering furnace and sintered. The sintering is preferably carried out in a vacuum.
[0044] The sintering temperature must be optimally selected depending on the components of the magnet. The sintering temperature is preferably set to 900 to 1100°C.
[0045] The sintering time is preferably from 1 to 20 hours, more preferably from 2 to 15 hours, and further preferably from about 4 to 10 hours.
[0046] The oriented mold is then loaded into a sintering furnace and sintered together with the mold, to obtain a sintered body. The sintered body has a cylindrical or columnar shape. For example, using the mold 10 shown in Figure 1, the neodymium magnet powder is filled therein as described above, and then the powder is oriented using the orienting device shown in Figure 4, followed by sintering. After that, by applying a magnetic field along the orientation direction of the crystal grains, a cylindrical two-pole polar anisotropic magnet magnetized in the orientation direction as shown in Figure 7 can be obtained. Furthermore, for example, by using the mold 20 and mold 30 shown in Figures 2 and 3 and filling them with the neodymium magnet powder as described above, followed by orienting using the orienting device shown in Figures 5 and 6 and sintering, and then applying a magnetic field along the orientation direction of the crystal grains, a cylindrical four-pole polar anisotropic magnet magnetized in the orientation direction as shown in Figure 8 can be obtained.
[0047] There is no particular limit to the size of the resulting polar anisotropic magnet. It is sufficient to manufacture the magnet in the shape required for the rotor in a rotating machine. If necessary, a process of diffusing heavy rare earth elements from the surface of the sintered body into the sintered body can be carried out to increase the coercive force of the sintered body and, in turn, the heat resistance of the magnet. Any process can be used as the specific grain boundary diffusion process, but for example, if the method described in Japanese Patent No. 6180507 is used, heavy rare earth elements can be efficiently introduced into the magnet, improving the magnetic properties.
[0048] <Circumferential surface magnetic flux density distribution> Such polar anisotropic magnets obtained by the manufacturing method of the present invention (hereinafter also referred to as "magnets of the present invention") have a magnetization direction that coincides with the magnetic path, so the magnetization potential of the magnet can leak magnetic flux to the outside with high efficiency. Therefore, the magnetic flux density generated in a rotating machine, for example, at the cap of the stator / rotor that affects the motor performance, is high. In addition, the amount of magnetic flux leaking in the circumferential direction of a circular or cylindrical shape is formed in a sine wave that is synchronized with the number of poles. In other words, the surface magnetic flux density distribution in the circumferential direction forms a sine wave. Here, the magnetic flux density leaking in the circumferential direction is measured using a magnetic measuring device (for example, UHS-1DS, manufactured by Nippon Denji Sokki Co., Ltd.) Specifically, the magnetic field sensor probe of the magnetic measuring device is set with a gap of about 0.5 mm from the surface of the magnet of the present invention, and the surface magnetic flux is measured around one revolution along the circumference perpendicular to the central axis, and then the magnetic field sensor probe is lowered 1 mm downward along the central axis, and the surface magnetic flux density is measured around one revolution in the same manner.
[0049] When the circumferential surface magnetic flux density waveform thus obtained is subjected to frequency analysis (Fast Fourier Transform (FFT)) to determine the harmonic content, in the case of the magnet of the present invention, it can be 10% or less. In frequency analysis of the waveform of the circumferential surface magnetic flux density, a sine wave is considered to be the primary wave, and other harmonics are considered to be non-sinusoidal waves. Therefore, when the harmonic content is 0%, the circumferential surface magnetic flux density is considered to be a perfect sine wave. In this way, the magnet of the present invention is preferably such that the amount of magnetic flux leaking in the circumferential direction of the cylindrical or columnar shape is formed into a sine wave synchronized with the number of poles, and when the sine wave is considered to be the primary component, the overall ratio of harmonic components excluding the primary component is 10% or less. The higher the amplitude of this sine wave, the better, but from the viewpoint of obtaining sufficient output characteristics as a rotating machine, it is preferable that it be 450 mT or more, more preferably 600 mT or more, and even more preferably 700 mT or more. In this way, it is preferable that the magnet of the present invention has a surface magnetic flux density of 450 mT or more at the magnetic pole positions in the circumferential direction of the cylindrical or columnar shape. When the harmonic content obtained by frequency analysis (Fourier transform) of the circumferential surface magnetic flux density waveform of the magnet of the present invention is 10% or less (preferably 5% or less, more preferably 4% or less, and even more preferably 3% or less), the waveform of the surface magnetic flux density can be said to be roughly sinusoidal, and therefore the magnetic flux leaking in the circumferential direction can be said to be formed in a sinusoidal shape.
[0050] The magnitude of the magnetic flux density of the magnet of the present invention means the amplitude of a sine wave.
[0051] <Variations in the amount of leakage magnetic flux in the axial direction> The magnet of the present invention preferably has a variation in the amount of leakage magnetic flux in the central axis direction of ±10% or less of the average amount of leakage magnetic flux from above and below on the same axis of a cylindrical or columnar shape.
[0052] The method for measuring this variation will be described with reference to FIG. FIG. 9 shows a cylindrical magnet of the present invention as an example, but the same can be considered for a cylindrical shape. First, as shown in Figure 9, the magnet 68 of the present invention is divided into 10 equal parts parallel to the axis X (the normal direction of the two end faces). The surface magnetic flux density in the circumferential direction is then measured at each part. In this case, as mentioned above, the waveform is roughly a sine wave. The amplitude of the sine wave is then taken as the magnitude of the magnetic flux density at that part. By carrying out this procedure, the magnetic flux density at all 10 locations is determined, and the simple average value is calculated. Then, the ratio (percentage) of the magnetic flux density values at all points to the simple average value is calculated. Each ratio calculated here is preferably within ±5% (i.e., 95 to 105%), and more preferably within ±3% (i.e., 97 to 103%).
[0053] <About through holes, etc.> The magnet of the present invention may have a through hole along the central axis (e.g., axis X in FIG. 9). In this case, a rotating shaft can be attached to the magnet of the present invention by passing the rotating shaft through the through hole.
[0054] <Rotor> Furthermore, the magnet of the present invention does not need to have a through hole. In this case, it may be used as shown in FIG. FIG. 10 is a cross-sectional perspective view showing a rotor of the present invention in which two shafts are disposed on the outside of both end faces of a magnet, and which is further covered with a protective tube. In the rotor shown in FIG. 10, a magnet 70 of the present invention has both end faces in contact with two shafts 72 . The shaft 72 has a circular cross section, and is formed so that its cross-sectional diameter is the same as that of the magnet 70 of the present invention. The magnet 70 of the present invention is completely covered by a protective tube 74. The inner diameter of the protective tube 74 is configured to be approximately the same as the outer diameter of the magnet 70 of the present invention and the shaft 72. By providing such protective tube 74, when the rotor shown in Fig. 10 rotates, it is possible to provide resistance to centrifugal force, such as preventing damage to the magnets. The rotor shown in Fig. 10 can then rotate at, for example, 20,000 rpm or more.
[0055] <Motor> For example, a motor as shown in FIG. 11 can be formed by using a magnet of the present invention with a rotating shaft attached to the through hole thereof or by using magnet 70 of the present invention in the embodiment shown in FIG. Fig. 11 shows a motor 80 using, as a rotor, the magnet 70 of the present invention shown in Fig. 10. Fig. 11 is a cross-sectional view of the motor 80 in a direction perpendicular to the rotation axis. The motor 80 has coils 84 spaced at regular intervals in the circumferential direction inside a cylindrical stator 82, and has the magnet 70 of the present invention at the center. A fixed gap 86 is formed between the magnet 70 of the present invention and the coils 84. Although the motor shown in FIG. 11 has a concentrated winding stator, a distributed winding stator can also be used.
[0056] The magnet 70 of the present invention generates a large magnetic flux density, so the gap 86 can be made relatively large. Conversely, even if the gap 86 is made large, sufficient magnetic flux can be generated in the coil 84. The electrical conductivity of the magnet material is high, and when high-frequency magnetic flux changes are applied to the magnet material, large eddy currents are generated, reducing the motor efficiency. To suppress these eddy currents, a method is often used in which the magnet is divided and the eddy current paths are offset. However, in this case, a huge increase in costs occurs, such as magnet processing / magnet assembly / magnet insertion into the rotor. Another method is to reduce the magnitude of the high-frequency magnetic flux change, but there is no magnet that generates a large magnetic flux (1.5 to 3.0 times larger than the conventional one) in a limited rotor area, and it has been difficult to achieve this. When the magnet 70 rotates as a rotor, the current flowing to the stator coil is driven by an inverter that controls the voltage / current including harmonics. This high-frequency current causes high-frequency magnetic flux changes in the coil, and the high-frequency magnetic flux changes are applied to the magnet, generating eddy currents. In the case of the present invention, even if eddy currents are generated, the influence is extremely minor because the distance from the stator can be made large. If we assume that the gap of a typical small motor is 0.5 mm, it can be widened to 1.5 mm. Assuming that this reduces the magnitude of the high-frequency magnetic flux to 1 / 10, the eddy current loss will be 1 / 100. Therefore, in the past, the generation of eddy currents caused large heat losses, and the energy losses led to thermal damage, so designs using magnets, especially for high-speed motors, were not realized. However, a motor using the magnet of the present invention can achieve a smaller, lighter motor with the same output and higher speeds, which was not possible with the past.
[0057] <Motor using two-pole anisotropic cylindrical magnets> As the two-pole polar anisotropic magnet shown in Fig. 7 has a polar anisotropic orientation, when installed in a motor, the waveform of the induced voltage becomes closer to a sine wave compared to a parallel orientation (the harmonic content is reduced by more than 30% by approaching a sine wave from a square wave). The motor's magnet torque is proportional to the product of the magnetic flux generated by the coil and the magnetic flux generated in the gap. Here, with inverter control, the current to the coil is usually a sine wave, so the closer the magnet-generated magnetic flux is to a sine wave, the greater the magnet torque will be improved by about 1.2 to 1.8 times compared to magnets of other orientations, assuming the same magnet material is used. Furthermore, when applied to a high-speed motor, the centrifugal force of rotation becomes a problem in the high-speed motor. Also, the smaller the rotor diameter, the less the centrifugal force influence. First, as a countermeasure against centrifugal force, a protective tube is formed around the rotor outer diameter as a strength member. Furthermore, in a high-speed motor, assuming inverter drive, the drive control frequency is high, about 300 to 5000 Hz, depending on the high speed. By increasing the control frequency, a high-frequency magnetic flux change that does not contribute to torque is applied from the stator to the rotor, and eddy currents are generated in the protective tube / rotor. When a polar anisotropic cylindrical magnet is used, a large magnet torque can be generated for the above reasons. Therefore, it is possible to secure a wide gap between the rotor and the stator. By applying the magnet according to the present invention, it is possible to widen the gap between the rotor and the stator from the conventional 0.5 mm to 1.5 mm. Also, by widening the gap between the rotor and the stator, the amount of high-frequency magnetic flux generated in the rotor is reduced, thereby reducing eddy currents. If the high-frequency magnetic flux density generated in the rotor could be reduced to one-tenth, it would be possible to reduce eddy currents to about one-hundredth, resulting in a high-speed motor. In addition, if a 10,000 rpm motor were to be increased to 20,000 rpm while maintaining the same output, the rotor diameter could potentially be reduced to one-fourth, making it possible to miniaturize the motor.
[0058] <Motors using polar anisotropic cylindrical magnets with four or more poles> A four-pole polar anisotropic magnet as shown in FIG. 8 or a polar anisotropic magnet with four or more poles can have a longer magnetization path length compared to a radial / parallel oriented cylindrical / segment magnet rotor. As with a two-pole polar anisotropic magnet, when the motor is installed, the waveform of the induced voltage becomes closer to a sine wave (the harmonic content decreases). When a two-pole rotor is changed to a four-pole rotor, the same induced voltage can be generated even if the rotor speed is reduced by half. Therefore, the required motor performance can be ensured even if the rotation speed is reduced. Furthermore, high-speed motors often aim to improve motor output [proportional to the product of generated torque and rotation] by increasing speed. However, in high-speed motors, centrifugal force applies stress to magnets, etc., making it difficult to implement. When using polar anisotropic cylindrical magnets with four or more poles, two methods can be applied compared to conventional magnets: improving magnet torque and reducing rotor rotation speed. This reduces eddy currents generated in the rotor, making it possible to realize a small, lightweight motor at high speed with unprecedented output.
[0059] Such a motor using the magnet of the present invention can be mounted on a moving object such as a car or an airplane.
[0060] For aeronautical applications, generators using turbines with speeds of over 100,000 rpm as their energy source are expected, and a high power-to-weight ratio is important for aeronautical applications. The magnet of the present invention is capable of generating a large magnetic flux, which allows for miniaturization, weight reduction, and high efficiency, and can also be used to form high-output generators for aviation applications, for example.
[0061] <Generator> The magnet of the present invention can also be used as a driving source for a compressor or as a generator that uses a turbine as its power source. EXAMPLES
[0062] <Example 1> A neodymium magnet powder with an average particle size of 3.2 μm and the composition shown in [1] in Table 1 was prepared. Then, methyl caprylate was added as a lubricant to this powder so that the amount was 0.07 mass%, and mixed thoroughly. After that, the neodymium magnet powder with the lubricant added was mixed at 3.6 g / cm 3The powder was filled into a carbon quasi-cylindrical mold cavity shown in FIG. 2 at a filling density of 1000 g / m2 to obtain a powder-filled mold. Next, the mold filled with powder was loaded into an orientation device, and an orientation magnetic field of 2.0 T was applied to the filled neodymium magnet powder as shown in FIG. 5 without applying pressure to the powder, thereby obtaining an oriented mold. Next, the oriented mold was placed in a sintering furnace and sintered together with the mold in a vacuum at 1000°C for 4 hours to obtain a sintered body. The obtained sintered body was then subjected to aging treatment at 800°C for 30 minutes and at 520°C for 1 hour. A magnetic field was applied along the orientation direction to this to obtain a cylindrical four-pole polar anisotropic magnet as shown in FIG. The surface magnetic flux density (mT), harmonic component ratio (%), and axial variation (%) of the surface magnetic flux density were measured for the obtained polar anisotropic magnet using the methods described above. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, the surface magnetic flux density (mT) was high (450 mT or more), the harmonic component ratio (%) was low (10% or less), and the axial surface magnetic flux density variation (%) was also 5% or less, confirming good performance in all respects. Moreover, the waveform of the surface magnetic flux density in the circumferential direction in the case of Example 1 is shown in FIG. Furthermore, the variation in the amount of magnetic flux in the central axis direction in the case of Example 1 is shown in FIG.
[0063] <Example 2> In Example 1, methyl caprylate was added as a lubricant to the neodymium magnet powder, but in Example 2, methyl laurate was used as a lubricant instead of methyl caprylate and added to the neodymium magnet powder. In addition, in Example 1, the oriented mold was placed in a sintering furnace and sintered at 1000°C, whereas in Example 2, it was sintered at 1020°C. Otherwise, the same operations as in Example 1 were carried out, and the surface magnetic flux density (mT), harmonic component ratio (%), and axial surface magnetic flux density variation (%) of the obtained polar anisotropic magnet were measured in the same manner as in Example 1. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, the surface magnetic flux density (mT) was high (450 mT or more), the harmonic component ratio (%) was low (10% or less), and the axial surface magnetic flux density variation (%) was also 5% or less, confirming good performance in all respects.
[0064] <Example 3> In Example 1, a neodymium magnet powder having the composition shown in Table 1 [1] and an average particle size of 3.2 μm was used, while in Example 3, a neodymium magnet powder having the composition shown in Table 1 [2] and an average particle size of 4.9 μm was used. Otherwise, the same operations as in Example 1 were carried out, and the surface magnetic flux density (mT), harmonic component ratio (%), and axial surface magnetic flux density variation (%) of the obtained polar anisotropic magnet were measured in the same manner as in Example 1. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, the surface magnetic flux density (mT) was high (450 mT or more), the harmonic component ratio (%) was low (10% or less), and the axial surface magnetic flux density variation (%) was also 5% or less, confirming good performance in all respects. The neodymium magnet powder used in Example 3 contains Dy. This is presumably the main reason why the polar anisotropic magnet obtained in Example 3 has different performance from that obtained in Example 1.
[0065] <Example 4> In Example 1, the mold filled with powder was loaded into the orienting device and an orienting magnetic field of 2.0 T was applied, whereas in Example 4, the mold filled with powder was loaded into the orienting device and an orienting magnetic field of 1.0 T was applied. Otherwise, the same operations as in Example 1 were carried out, and the surface magnetic flux density (mT), harmonic component ratio (%), and axial surface magnetic flux density variation (%) of the obtained polar anisotropic magnet were measured in the same manner as in Example 1. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, the surface magnetic flux density (mT) was high (450 mT or more), the harmonic component ratio (%) was low (10% or less), and the axial surface magnetic flux density variation (%) was also 5% or less, confirming good performance in all respects. The oriented magnetic field in Example 4 is different from that in Example 1. This is presumably the main reason why the polar anisotropic magnet obtained in Example 1 has different performance.
[0066] <Example 5> In Example 1, the mold filled with powder was loaded into the orienting device and an orienting magnetic field of 2.0 T was applied, whereas in Example 5, the mold filled with powder was loaded into the orienting device and an orienting magnetic field of 3.0 T was applied. Otherwise, the same operations as in Example 1 were carried out, and the surface magnetic flux density (mT), harmonic component ratio (%), and axial surface magnetic flux density variation (%) of the obtained polar anisotropic magnet were measured in the same manner as in Example 1. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, the surface magnetic flux density (mT) was high (450 mT or more), the harmonic component ratio (%) was low (10% or less), and the axial surface magnetic flux density variation (%) was also 5% or less, confirming good performance in all respects. The oriented magnetic field in Example 5 is different from that in Example 1. This is presumably the main reason why the polar anisotropic magnet obtained in Example 1 has different performance.
[0067] <Example 6> In Example 1, a pseudo-cylindrical carbon mold cavity as shown in FIG. 2 was used, and an aligning magnetic field was applied as shown in FIG. 5 to obtain a cylindrical four-pole polar anisotropic magnet as shown in FIG. 8. In Example 6, a pseudo-cylindrical carbon mold cavity as shown in FIG. 1 was used, and an aligning magnetic field was applied as shown in FIG. 4 to obtain a cylindrical two-pole polar anisotropic magnet as shown in FIG. 7. Otherwise, the same operations as in Example 1 were carried out, and the surface magnetic flux density (mT), harmonic component ratio (%), and axial surface magnetic flux density variation (%) of the obtained polar anisotropic magnet were measured in the same manner as in Example 1. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, the surface magnetic flux density (mT) was high (450 mT or more), the harmonic component ratio (%) was low (10% or less), and the axial surface magnetic flux density variation (%) was also 5% or less, confirming good performance in all respects. The sixth embodiment differs from the first embodiment in the number of poles of the polar anisotropic magnet.
[0068] <Example 7> The polar anisotropic magnet obtained in Example 1 was further subjected to GBD. GBD is a process in which a TbNiAl alloy is deposited on the surface of the polar anisotropic magnet (Tb deposition amount 1 wt% / mm 2 ), and then heat treatment is performed in an Ar atmosphere at 900°C for 15 hours to diffuse the Tb element into the magnet. Otherwise, the same operations as in Example 1 were carried out, and the surface magnetic flux density (mT), harmonic component ratio (%), and axial surface magnetic flux density variation (%) of the obtained polar anisotropic magnet were measured in the same manner as in Example 1. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, the surface magnetic flux density (mT) was high (450 mT or more), the harmonic component ratio (%) was low (10% or less), and the axial surface magnetic flux density variation (%) was also 5% or less, confirming good performance in all respects.
[0069] <Example 8> A neodymium magnet powder with an average particle size of 3.2 μm and the composition shown in [1] in Table 1 was prepared. Then, methyl caprylate was added as a lubricant to this powder so that the amount was 0.07 mass%, and mixed thoroughly. After that, the neodymium magnet powder with the lubricant added was mixed at 3.6 g / cm 3 The powder was filled into a carbon pseudo-cylindrical mold cavity shown in FIG. 3 at a filling density of 1000 g / m2 to obtain a powder-filled mold. Next, the powder-filled mold was loaded into an orientation device, and an orientation magnetic field of 2.0 T was applied without applying pressure to the filled powder, as shown in FIG. 6, to obtain an oriented mold. Next, the oriented mold was placed in a sintering furnace and sintered together with the mold in a vacuum at 1000°C for 4 hours to obtain a sintered body. The obtained sintered body was then subjected to aging treatment at 800°C for 30 minutes and at 520°C for 1 hour. A magnetic field was applied along the orientation direction to this to obtain a cylindrical four-pole polar anisotropic magnet as shown in FIG. In FIG. 6, there is no pointed portion on the inside as shown in FIG. 5, but by controlling the shape of this portion and the strength of the applied magnetic field, the intended polar anisotropic orientation can be obtained. The surface magnetic flux density (mT), harmonic component ratio (%), and axial variation (%) of the surface magnetic flux density were measured for the obtained polar anisotropic magnet using the methods described above. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, the surface magnetic flux density (mT) was high (450 mT or more), the harmonic component ratio (%) was low (10% or less), and the axial surface magnetic flux density variation (%) was also 5% or less, confirming good performance in all respects.
[0070] <Example 9> In Example 8, methyl caprylate was added as a lubricant to the neodymium magnet powder, but in Example 9, methyl laurate was used as a lubricant instead of methyl caprylate and added to the neodymium magnet powder. In addition, in Example 8, the oriented mold was placed in a sintering furnace and sintered at 1000°C, whereas in Example 9, it was sintered at 1020°C. In Example 8, as shown in FIG. 5, a magnetic field was applied in a direction parallel to the paper surface of FIG. 5, but in Example 9, a magnetic field of 2.0 T was applied in a direction perpendicular to the magnet's orientation direction (the axial direction of the magnet) to orient the magnet, and then an aligning magnetic field of 4.8 T was applied in the magnet's orientation direction. As a result, in the above-mentioned Example 8, slight cracks were confirmed in several places on the magnet surface, but in Example 9, no similar cracks were confirmed at all. From this result, it can be seen that by applying a magnetic field in the axial direction of the magnet, the strength of the magnet can be made stronger (the appearance can be made neater). This is thought to be mainly due to the fact that the powder density is increased by applying a magnetic field in the axial direction of the magnet in advance, and that the powder becomes more easily oriented by applying a magnetic field in advance to make it magnetic.
[0071] Additionally, the orientation angle and degree of orientation were measured at each measurement point on the magnet surface in Example 9. Fig. 14 is a diagram showing the positional relationship between magnet center point O, magnet end X parallel to O, and magnet end Y perpendicular to O in the upper right quarter of the magnet obtained in Example 9 when viewed from above (axial direction). Table 3 shows the measured values of the positional relationship (distance and angle), as well as the orientation angle and degree of orientation. In Table 3, X is the distance in the X direction from the center point of the magnet, Y is the distance in the Y direction from the center point of the magnet, R is the distance from the center point of the magnet to each measurement point, and θ is the angle between the line OX and the line O- each measurement point when the line OX is set to 0°. The orientation angle in Table 3 is the angle calculated by XRD (X-ray diffraction). The orientation degree in Table 3 is the result of Br / Js calculated from the result of XRD and that measured by XRD. XRD measures the degree to which the crystal orientation in the magnet is oriented in the intended direction (crystallographic orientation degree). The result of Br / Js was calculated from the correlation between XRD and Br / Js (comparison of the calibration curves of the two) by performing a preliminary experiment on magnets having the same composition and obtaining the XRD value. As shown in Table 3, Example 9 shows the orientation shown in FIG. 8 at a high rate. Specifically, at each measurement point, the results of XRD and Br / Js are both 80% or more.
[0072] <Comparative Example 1> In Example 1, a neodymium magnet powder having the composition shown in composition [1] in Table 1 and an average particle size of 3.2 μm was used, while in Comparative Example 1, a neodymium magnet powder having a similar composition but an average particle size of 0.8 μm was used. Otherwise, the same operations as in Example 1 were carried out, and the surface magnetic flux density (mT), harmonic component ratio (%), and axial surface magnetic flux density variation (%) of the obtained polar anisotropic magnet were measured in the same manner as in Example 1. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, the surface magnetic flux density (mT) deteriorated (less than 450mT), the harmonic component ratio (%) deteriorated (more than 10%), and the axial variation in surface magnetic flux density (%) also deteriorated to more than 5%. This is presumably because the particle size of the neodymium magnet powder was small, which increased the surface area and caused poor packing, resulting in defects inside the obtained polar anisotropic magnet. Moreover, the waveform of the surface magnetic flux density in the circumferential direction in the case of Comparative Example 1 is shown in FIG.
[0073] <Comparative Example 2> In Example 1, a neodymium magnet powder having the composition shown in composition [1] in Table 1 and an average particle size of 3.2 μm was used, while in Comparative Example 2, a neodymium magnet powder having a similar composition but an average particle size of 8.2 μm was used. Furthermore, in Example 1, methyl caprylate was added as a lubricant to the neodymium magnet powder, but in Comparative Example 2, methyl laurate was used as a lubricant instead of methyl caprylate, and this was added to the neodymium magnet powder. Otherwise, the same operations as in Example 1 were carried out, and the surface magnetic flux density (mT), harmonic component ratio (%), and axial surface magnetic flux density variation (%) of the obtained polar anisotropic magnet were measured in the same manner as in Example 1. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, the surface magnetic flux density (mT) deteriorated (less than 450 mT), the harmonic component ratio (%) deteriorated (more than 10%), and the axial variation in surface magnetic flux density (%) also deteriorated to more than 5%. This is presumably because the particle size of the neodymium magnet powder is large, which results in a large amount of non-single crystal grains, resulting in poor orientation. Moreover, the waveform of the surface magnetic flux density in the circumferential direction in the case of Comparative Example 2 is shown in FIG.
[0074] <Comparative Example 3> In Example 1, the neodymium magnet powder to which the lubricant was added was 3.6 g / cm 3 In Comparative Example 3, the filling density was 3.2 g / cm 3 The mold cavity was filled at a packing density of 0.1 g / mol. Otherwise, the same operations as in Example 1 were carried out, and the surface magnetic flux density (mT), harmonic component ratio (%), and axial surface magnetic flux density variation (%) of the obtained polar anisotropic magnet were measured in the same manner as in Example 1. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, it was not possible to measure the surface magnetic flux density (mT), the harmonic component ratio (%), or the axial variation of the surface magnetic flux density (%). This was because the packing density was insufficient, and it was not possible to fabricate a proper solid cylindrical shape.
[0075] <Comparative Example 4> In Example 1, the neodymium magnet powder to which the lubricant was added was 3.6 g / cm 3 In Comparative Example 4, the filling density was 4.2 g / cm 3 The mold cavity was filled at a packing density of 0.1 g / mol. Otherwise, the same operations as in Example 1 were carried out, and the surface magnetic flux density (mT), harmonic component ratio (%), and axial surface magnetic flux density variation (%) of the obtained polar anisotropic magnet were measured in the same manner as in Example 1. The results are shown in Table 2 together with the measurement conditions. As shown in Table 2, the surface magnetic flux density (mT) deteriorated (less than 450mT), the harmonic component ratio (%) deteriorated (more than 10%), and the axial variation in surface magnetic flux density (%) also deteriorated to more than 5%. This is presumably due to the high packing density, which made it difficult to orient the material. Moreover, the waveform of the surface magnetic flux density in the circumferential direction in the case of Comparative Example 4 is shown in FIG.
[0076] [Table 1]
[0077] [Table 2]
[0078] [Table 3] [Explanation of symbols]
[0079] 10 Mold 12, 14 End face 16 Side 18 Inner Surface 19 Mold Cavity 20 Mold 22, 24 end face 26 Side 28 Inner Surface 29 Mold Cavity 30 Mold 32, 34 end face 36 Side 38 Inside 39 Mold Cavity 40 Powder filled mold 42 Coil 50 Powder-filled molds 52 Coil 60 Powder-filled mold 62 Coil 68, 70 Magnet of the present invention 72 Shaft 74 Protection tube 80 Motor 82 Stator 84 Coil 86 Gap
Claims
1. Neodymium magnet powder having an average particle size of 1.0 to 5.0 μm and containing 1.0 mass % or less of a lubricant is added at 3.4 to 4.0 g / cm 3 a filling step of filling the powder into a quasi-cylindrical mold cavity with a packing density of 0.1 to 0.5 to obtain a powder-filled mold; an orientation step of loading the powder-filled mold into an orientation device and applying an orientation magnetic field of 1.0 to 5.0 T to the filled neodymium magnet powder without applying pressure to orient the neodymium magnet powder to obtain an oriented mold; A sintering step of inserting the oriented mold into a sintering furnace and sintering the mold together to obtain a sintered body, the mold cavity is designed so that the sintered body has a cylindrical or columnar shape, and the cross-sectional shape of the mold cavity has a ratio (b / a) of 1.25 to 1.37, where b is the length of the major axis of the mold cavity and a is the length of the minor axis of the mold cavity; In the sintering step, the ratio of the amount of shrinkage in the direction of easy magnetization during sintering to the amount of shrinkage in the direction perpendicular thereto (amount of shrinkage in the direction of easy magnetization during sintering / amount of shrinkage in the direction perpendicular thereto) is 1.25 to 1.37; The surface magnetic flux density at the magnetic pole position in the circumferential direction of the cylindrical or columnar shape is 450 mT or more, A method for manufacturing a cylindrical or columnar polar anisotropic magnet, in which the variation in the amount of leakage magnetic flux in the axial direction of the cylindrical or columnar shape is within ±5% of the average amount of leakage magnetic flux through the top and bottom of the coaxial shape.
2. 2. The method for producing a polar anisotropic magnet according to claim 1, characterized in that in the orientation step, an orientation device capable of orienting the magnet to have an anisotropy of 2N poles, the number of poles being a multiple of a natural number N, is used.
3. The orientation step includes: a step of loading the powder-filled mold into an orientation device, applying a magnetic field in a direction perpendicular to the orientation direction without applying pressure to the filled neodymium magnet powder, and then applying an orientation magnetic field of 1.0 to 5.0 T in the orientation direction to orient the neodymium magnet powder and obtain the oriented mold; A method for producing a polar anisotropic magnet according to claim 1 or 2.
4. A method for manufacturing a polar anisotropic magnet, comprising contacting the surface of a polar anisotropic magnet manufactured by the method of any one of claims 1 to 3 with a heavy rare earth metal (R) or an R-based alloy containing a heavy rare earth metal (wherein R is at least one element selected from Dy, Tb and Ho), performing a heat treatment, and diffusing the R element into the magnet.
Citation Information
Patent Citations
Manufacture of anisotropic magnet roll
JP1985246614A
Read-after-write magnetic head
JP1986080507A
High-speed rotation brushless motor
JP2006217740A
Rotor for motor and brushless motor
JP2009022096A
Permanent magnet and method of producing permanent magnet
JP2015153790A