Acid-resistant steel sheet and its manufacturing method
A steel plate with controlled composition and manufacturing process forms a Si-enriched surface layer, addressing corrosion resistance and workability issues in acidic environments without expensive alloys, achieving low corrosion rates and high elongation.
Patent Information
- Application Number
- JP2021531253
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-11-30
- Filing Date
- 2019-11-26
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2039-11-26
AI Technical Summary
Existing steel plates lack sufficient corrosion resistance and workability in acidic environments, particularly when exposed to strong acids, and methods to enhance these properties often involve expensive alloying elements or suffer from limitations in effectiveness or economic efficiency.
A steel plate composition with controlled amounts of C, Si, Mn, Al, P, S, and N, and optionally Cr, Ni, Cu, Nb, Ti, and Mo, combined with a manufacturing process that includes hot rolling, acid treatment, and controlled cooling to create a Si-enriched surface layer, enhancing corrosion resistance without expensive alloys.
The steel plate achieves excellent corrosion resistance and workability in acidic conditions, with a corrosion rate less than 3.5 mg/cm²·h in a 1% sulfuric acid solution at 70°C and an elongation rate of 30% or more, while avoiding the need for costly alloying elements.
Smart Images

Figure 0007561126000003 
Figure 0007561126000001 
Figure 0007561126000002
Abstract
Description
[Technical field]
[0001] TECHNICAL FIELD The present invention relates to an acid-resistant steel sheet and a manufacturing method thereof, and more particularly to a steel sheet having excellent corrosion resistance against corrosion caused by various acids and excellent workability, and a manufacturing method thereof. [Background technology]
[0002] In the process of burning fossil fuels to generate thermal energy, water vapor is generated along with toxic exhaust gases such as sulfuric acid gas and nitric acid gas, and in the process of cooling these, condensed water containing various strong acids such as sulfuric acid, hydrochloric acid, and nitric acid is generated, which can corrode the exhaust system. In addition, acid solutions are often used as solutions for cleaning and other purposes in various industrial facilities, which can induce corrosion by acids.
[0003] When a steel sheet is exposed to such an acid environment, the steel sheet may rapidly corrode and lose its thickness, causing it to lose its function as a structural material. Therefore, steel sheets used in environments where they may come into contact with acid must have improved corrosion resistance to acids in order to extend their life. Also, in order to be used as structures with desired shapes, the steel sheet must have a certain level of mechanical properties for forming.
[0004] To complement the corrosion resistance of cold-rolled steel sheets, a method has been proposed to improve the corrosion resistance of steel sheets by hot-dip plating with aluminum. Aluminum-plated steel sheets are made by plating aluminum on ordinary carbon steel, and have corrosion resistance due to the Al2O3 passivation film, and have the advantage of being particularly resistant to corrosion by salt. However, aluminum is easily dissolved and removed in a low-pH, strongly acidic environment, so there is a limit to how much corrosion resistance can be achieved.
[0005] To solve these problems, a method has been proposed in which copper is added to steel sheets to suppress corrosion in low-pH, strongly acidic environments. When copper is added, it concentrates on the surface during the corrosion process, reducing the corrosion rate, but there is a limit to the level of corrosion resistance that can be achieved by adding copper, and a method to further improve corrosion resistance is needed. Also, adding large amounts of copper has the disadvantage of inducing cracks on the surface during the steel sheet production process.
[0006] As a method to greatly improve the corrosion resistance of steel sheets, a method of manufacturing stainless steel sheets by adding large amounts of various alloying elements including Cr has been proposed. Stainless steel sheets also have corrosion resistance due to the Cr2O3 passivation film in a certain range of pH, but in a strong acidic environment with a low pH, the Cr2O3 passivation film becomes activated and the corrosion resistance is lost. In addition, there is a disadvantage that the cost is reduced by adding large amounts of expensive alloying elements. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention provides an acid-resistant steel sheet and a manufacturing method thereof. Specifically, the present invention provides a steel sheet having excellent corrosion resistance against corrosion caused by various acids and excellent workability, and a manufacturing method thereof. [Means for solving the problem]
[0008] An acid-resistant steel sheet according to one embodiment of the present invention contains, by weight, C: 0.1% or less (excluding 0%) and Si: 2.0 to 4.0%, with the remainder being Fe and other unavoidable impurities, and the Si content in the surface portion from the steel sheet surface to a depth of 10 μm inward is 15% or more by weight.
[0009] It may further contain one or more of Mn: 0.1 to 0.5 wt %, Al: 0.1 wt % or less, P: 0.01 wt % or less, S: 0.01 wt % or less, and N: 0.01 wt % or less.
[0010] It may further contain one or more of Cr: 0.1 wt % or less, Ni: 0.1 wt % or less, Cu: 0.1 wt % or less, Nb: 0.1 wt % or less, Ti: 0.1 wt % or less, and Mo: 0.1 wt % or less.
[0011] When immersed in a 1% by weight aqueous sulfuric acid solution at 70°C for 1 hour, the average corrosion rate is 3.5mg / cm 2 h or less. The elongation can be 30% or more.
[0012] A method for producing an acid-resistant steel sheet according to one embodiment of the present invention includes a step of heating a slab containing, by weight, C: 0.1% or less (excluding 0%) and Si: 2.0 to 4.0%, with the remainder being Fe and other unavoidable impurities, a step of hot rolling the slab to produce a hot-rolled steel sheet, and a step of acid-treating the hot-rolled steel sheet in an acid aqueous solution of 25% by weight or more for 10 seconds or more.
[0013] In the step of heating the slab, the slab may be heated to 1200° C. or greater. In the stage of producing hot-rolled steel sheet, the finish rolling temperature can be Ar3 or higher.
[0014] The Ar3 temperature can be calculated by the following formula: Ar3=910-310×[C]-80×[Mn]-20×[Cu]-15×[Cr]-55×[Ni]-80×[Mo]-(0.35×(25.4-8))
[0015] After the step of producing the hot-rolled steel sheet, the method may further include a step of coiling the hot-rolled steel sheet at 550 to 750°C. After the step of producing the hot-rolled steel sheet, the method may further include a step of cold rolling the hot-rolled steel sheet. After the step of producing the hot-rolled steel sheet, the method may further include a step of annealing the hot-rolled steel sheet. Effect of the Invention
[0016] The acid-resistant steel sheet according to one embodiment of the present invention is excellent in acid resistance and workability. The acid-resistant steel sheet according to one embodiment of the present invention can obtain excellent acid resistance and workability without adding expensive alloy components such as Cr. The acid-resistant steel sheet according to one embodiment of the present invention has a Si-enriched layer formed thereon, and has excellent corrosion resistance in an acid corrosive environment, thereby effectively extending the life of the material. [Brief description of the drawings]
[0017] [Figure 1] 1 is a schematic cross-sectional view of an acid-resistant steel plate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, a first part, component, region, layer or section described below may be referred to as a second part, component, region, layer or section without departing from the scope of the present invention.
[0019] The terminology used herein is merely for the purpose of referring to particular embodiments and is not intended to limit the present invention. As used herein, the singular forms include the plural forms unless the context clearly indicates otherwise. As used in the specification, the term "comprising" refers to the specification of certain features, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements and / or components.
[0020] Moreover, unless otherwise specified, % means % by weight, and 1 ppm is 0.0001% by weight.
[0021] In one embodiment of the present invention, the term "additionally contain an additional element" refers to the inclusion of an additional amount of the additional element in place of the remaining iron (Fe).
[0022] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted as having a meaning consistent with the relevant technical literature and the presently disclosed content, and are not interpreted as being overly ideal or formal unless otherwise defined.
[0023] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.
[0024] The acid-resistant steel plate according to an embodiment of the present invention relates to a steel plate used in an environment where corrosion by acid occurs. The material for this application must have corrosion resistance in an acid environment to extend its life, and also have workability to be molded into a desired shape.
[0025] When expensive alloy elements are added in excessive amounts to increase acid resistance, not only does the cost of the material increase, reducing its economic viability, but it also results in reduced workability. Therefore, a method is needed that can ensure both corrosion resistance and workability without adding large amounts of expensive alloy elements.
[0026] The acid-resistant steel sheet according to one embodiment of the present invention has a Si-enriched layer formed on the surface thereof, and has excellent corrosion resistance in an acid corrosive environment, thereby effectively extending the life of the material.
[0027] Fig. 1 shows a schematic cross section of an acid-resistant steel plate according to an embodiment of the present invention. As shown in Fig. 1, a surface portion 20 is present from the surface of the acid-resistant steel plate 10 toward the inside. Although Fig. 1 shows that the surface portion 20 is located on one side, it is also possible for the surface portion 20 to be located on both sides.
[0028] An acid-resistant steel sheet 10 according to one embodiment of the present invention contains, by weight, C: 0.1% or less (excluding 0%), Si: 2.0 to 4.0%, and the balance Fe and unavoidable impurities. Each component will be described in detail below.
[0029] Carbon (C): 0.1% by weight or less Since the higher the C content, the greater the strength, an appropriate amount of C is added to obtain the desired yield strength and tensile strength. However, if the C content is too high, the elongation decreases and formability may deteriorate. Therefore, C may be contained in an amount of 0.1% by weight or less. More specifically, C may be contained in an amount of 0.001 to 0.1% by weight. Even more specifically, C may be contained in an amount of 0.01 to 0.09% by weight.
[0030] Silicon (Si): 2.0 to 4.0% by weight Si is an element that can be used as a decarburizing agent when added in small amounts, and can contribute to improving strength through solid solution strengthening. In one embodiment of the present invention, Si is a very important additive element, and can greatly improve corrosion resistance against acids by forming a Si-based oxide layer on the surface through the addition of Si and surface concentration. If too little Si is added, it is difficult to obtain the above-mentioned effects. Conversely, if too much Si is added, the workability may be greatly reduced due to the formation of a B2 or DO3 ordered phase. Therefore, Si may be contained in an amount of 2.0 to 4.0 wt %. More specifically, Si may be contained in an amount of 2.5 to 3.5 wt %.
[0031] The acid-resistant steel plate 10 according to one embodiment of the present invention may further contain one or more of Mn: 0.1 to 0.5 wt %, Al: 0.1 wt % or less, P: 0.01 wt % or less, S: 0.01 wt % or less, and N: 0.01 wt % or less.
[0032] Manganese (Mn): 0.1 to 0.5% by weight Manganese (Mn) is an element that prevents hot shortness caused by dissolved S in steel by combining with the dissolved S and precipitating as MnS. To achieve this effect, Mn may be contained in an amount of 0.1 wt% or more. However, if the Mn content exceeds 0.5 wt%, the material may become hard and the softness may decrease. More specifically, Mn may be contained in an amount of 0.15 to 0.35 wt%.
[0033] Aluminum (Al): 0.1% by weight or less Al is an element with a very large deoxidizing effect, and can be further contained since it reacts with N in the steel to precipitate AlN, thereby preventing the deterioration of formability due to solute N. However, when a large amount is added, the softness decreases rapidly, so the content is limited to 0.1 wt% or less. More specifically, 0.01 to 0.05 wt% of Al can be further contained.
[0034] Phosphorus (P): 0.01% by weight or less The addition of P up to a certain amount can increase the strength of steel without significantly decreasing its softness, but if it is added in excess of 0.01% by weight, it segregates at the grain boundaries and hardens the steel, so the amount should be limited to 0.01% by weight or less. More specifically, P can be contained in an amount of 0.001 to 0.01% by weight.
[0035] Sulfur (S): 0.01% by weight or less Since S is an element that induces red shortness when in solid solution, the addition of Mn must induce the precipitation of MnS. However, excessive precipitation of MnS is undesirable because it hardens the steel. Therefore, the upper limit of S is limited to 0.01 wt%. More specifically, S may be further contained at 0.001 to 0.01 wt%.
[0036] Nitrogen (N): 0.01% by weight or less N is often contained in steel as an unavoidable element, and N that exists in a solid solution state without being precipitated reduces softness, deteriorates aging resistance, and also reduces workability. In addition, when N combines with elements such as Ti and Nb to form precipitates, it significantly deteriorates corrosion resistance, so the upper limit is limited to 0.01 wt%. More specifically, N may be further contained at 0.001 to 0.005 wt%.
[0037] The acid-resistant steel sheet 10 according to one embodiment of the present invention contains C: 0.01% by weight or less, Si: 2.0 to 4.0% by weight, Mn: 0.1 to 0.5% by weight, Al: 0.1% by weight or less, P: 0.01% by weight or less, S: 0.01% by weight or less, and N: 0.01% by weight or less, with the balance being Fe and other inevitable impurities. Specifically, the acid-resistant steel sheet 10 according to one embodiment of the present invention contains C: 0.01% by weight or less, Si: 2.0 to 4.0% by weight, Mn: 0.1 to 0.5% by weight, Al: 0.1% by weight or less, P: 0.01% by weight or less, S: 0.01% by weight or less, and N: 0.01% by weight or less, with the balance being Fe and other inevitable impurities.
[0038] In addition to the above-mentioned alloy composition, the balance includes Fe and inevitable impurities. However, this does not exclude the addition of other compositions in one embodiment of the present invention. The inevitable impurities may be unintentionally mixed from raw materials or the surrounding environment during normal steel manufacturing processes, and cannot be excluded. The inevitable impurities can be understood by engineers in the field of normal steel manufacturing. For example, Cr: 0.1 wt% or less, Ni: 0.1 wt% or less, Cu: 0.1 wt% or less, Nb: 0.1 wt% or less, Ti: 0.1 wt% or less, and Mo: 0.1 wt% or less.
[0039] In one embodiment of the present invention, the Si content of the surface portion 20 from the surface of the steel sheet to a depth of 10 μm in the inner direction may be 15 wt % or more.
[0040] The above-mentioned alloy composition is the alloy composition of the entire steel plate 10 including the surface portion 20, and not excluding the surface portion 20.
[0041] The remaining contents in the surface portion 20 besides the Si content are the same as the alloy composition of the steel sheet 10, except that the surface portion 20 may further contain 5 to 50 wt% of O. A concentration gradient of Si may exist even in the surface portion 20, and the expression that the Si content is 15% or more means the average over the entire thickness of the surface portion 20.
[0042] In one embodiment of the present invention, corrosion resistance can be ensured by ensuring that the Si content of the surface portion 20 is 15% by weight or more. More specifically, the Si content of the surface portion 20 can be 20% by weight or more. Even more specifically, the Si content can be 20 to 35% by weight.
[0043] The method for forming the surface portion 20 will be described in detail in the method for manufacturing an acid-resistant steel plate described later, so a duplicated description will be omitted.
[0044] As described above, the presence of the surface portion 20 can ensure excellent corrosion resistance as well as excellent workability.
[0045] Specifically, when immersed in a 1% by weight aqueous sulfuric acid solution at 70°C for 1 hour, the average corrosion rate is 3.5mg / cm 2 ·h or less. Also, the elongation rate may be 30% or more. More specifically, when immersed in a 1 wt% aqueous sulfuric acid solution at 70°C for 1 hour, the average corrosion rate may be 1.0 to 3.0 mg / cm 2 The elongation rate may be 30 to 40%.
[0046] A method for manufacturing an acid-resistant steel sheet according to an embodiment of the present invention includes the steps of heating a slab, hot rolling the slab to manufacture a hot-rolled steel sheet, and acid-treating the hot-rolled steel sheet in an acid solution of 25% by weight or more for 10 seconds or more.
[0047] Each step will be described in detail below. First, heat the slab. The alloy composition of the slab has been described above in relation to the acid-resistant steel plate, so a duplicated description will be omitted. Since the alloy components do not substantially change during the manufacturing process of the acid-resistant steel plate, the alloy composition of the acid-resistant steel plate and the alloy composition of the slab are substantially the same.
[0048] The heating temperature of the slab may be 1200°C or higher. A temperature of 1200°C or higher is necessary because most of the precipitates present in the steel must be redissolved. More specifically, the heating temperature of the slab may be 1250°C or higher.
[0049] The slab is then hot rolled to produce a hot rolled steel sheet. At this time, the finish rolling temperature can be Ar3 or higher.
[0050] The Ar3 temperature is calculated using the following formula: Ar3=910-310×[C]-80×[Mn]-20×[Cu]-15×[Cr]-55×[Ni]-80×[Mo]-(0.35×(25.4-8))
[0051] This is because the rolling is carried out in the austenite single phase region.
[0052] After the step of producing the hot-rolled steel sheet, the method may further include a step of coiling the hot-rolled steel sheet at 550 to 750°C. By coiling at 550°C or higher, N remaining in a solid solution state can be additionally precipitated as AlN, thereby ensuring excellent aging resistance. If coiling is performed at less than 550°C, there is a risk that workability will decrease due to the remaining solid solution N that has not been precipitated as AlN. If coiling is performed at 750°C or higher, crystal grains will become coarse, which will cause a decrease in cold rolling ability.
[0053] The method may further include a step of cold rolling the hot rolled steel sheet after the step of producing the hot rolled steel sheet. Also, the method may further include a step of annealing the hot rolled steel sheet after the step of producing the hot rolled steel sheet. The steps of cold rolling and annealing are widely known in the relevant field, so detailed description thereof will be omitted.
[0054] Next, the hot-rolled steel sheet is subjected to an acid treatment in an acid aqueous solution of 25% by weight or more for 10 seconds or more. In one embodiment of the present invention, excellent acid resistance can be ensured by concentrating Si in the surface portion 20 by acid treatment.
[0055] The acid may be an inorganic acid or an organic acid. Specifically, one or more of sulfuric acid, hydrochloric acid, and nitric acid may be used. More specifically, hydrochloric acid may be used.
[0056] The acid concentration must be 25% by weight or more, and the treatment time must be 10 seconds or more. If the acid concentration is low or the treatment time is short, Si is not properly concentrated, and it is difficult to ensure corrosion resistance. More specifically, the acid concentration is 25 to 50% by weight, and the treatment time can be 10 to 60 seconds. EXAMPLES
[0057] The present invention will be described in more detail below with reference to examples. However, these examples are merely for the purpose of illustrating the present invention, and the present invention is not limited thereto.
[0058] (Example) Steel having the composition shown in Table 1 below was manufactured, and the components are shown as actual values. The steel slab having the composition shown in Table 1 was reheated at 1250°C, hot-rolled at 900°C or higher, coiled at 620°C, and surface-treated with hydrochloric acid under the acid treatment conditions shown in Table 1, to finally obtain a hot-rolled steel sheet having a thickness of 3 mm.
[0059] [Table 1]
[0060] The Si content in the surface region of each hot-rolled steel sheet from the surface to a depth of 10 μm was measured using an EDS (Energy Dispersive Spectrometer). Acid resistance was evaluated by measuring the average corrosion rate after corroding in a 1 wt% sulfuric acid solution at 70° C. for 1 hour, and mechanical properties were evaluated by a room temperature tensile test. The measured Si content in the surface region, average corrosion rate, and elongation are shown in Table 2 below.
[0061] [Table 2]
[0062] As shown in Table 2 above, the invention steels 1 to 16, which satisfy the composition and manufacturing conditions of the present invention, have a Si content of 15% or more by weight in the surface portion, and are excellent in average corrosion rate and elongation in a sulfuric acid corrosion test.
[0063] It can be seen that comparative steel 1 has poor workability due to its excessively high C content.
[0064] Comparative steels 2 and 3 have low Si content, and the Si content in the surface area is also low. As a result, it can be confirmed that the corrosion rate increases significantly. In contrast, comparative steels 4 and 5 have high Si content, and the Si content in the surface area is also high. It can be confirmed that the corrosion rate is excellent, but the elongation is very poor. This is due to the formation of B2 or DO3 phases due to the regular arrangement of Si and Fe, and it is analyzed that when these phases are formed, dislocations cannot move freely and the elongation decreases significantly.
[0065] It can be seen that the average corrosion rate of comparative steels 6 to 8 is very poor because the concentration of the acid solution is low and the concentration of Si in the surface portion is insufficient.
[0066] It can be seen that the average corrosion rate of comparative steels 9 to 11 is very poor because the acid treatment time is very short and the concentration of Si in the surface portion is insufficient.
[0067] The present invention is not limited to the above embodiment, and can be manufactured in various different forms, and a person skilled in the art to which the present invention belongs can understand that the present invention can be embodied in other specific forms without changing the technical idea or essential features of the present invention. Therefore, it should be understood that the above embodiment is illustrative in all respects and not limiting. [Explanation of symbols]
[0068] 10 Acid-resistant steel plate 20 Surface area
Claims
1. containing C: 0.1 wt % or less (excluding 0 wt %), Si: 2.0 to 4.0 wt %, Mn: 0.1 to 0.5 wt %, Al: 0.1 wt % or less, P: 0.01 wt % or less, S: 0.01 wt % or less, and N: 0.01 wt % or less, with the balance being Fe and unavoidable impurities; An acid-resistant steel plate having a Si content of 15% by weight or more in a surface portion extending from the surface of the steel plate to a depth of 10 μm inward.
2. 2. The acid-resistant steel sheet according to claim 1, further comprising one or more of Cr: 0.1 wt. % or less, Ni: 0.1 wt. % or less, Cu: 0.1 wt. % or less, Nb: 0.1 wt. % or less, and Mo: 0.1 wt. % or less.
3. When immersed in a 1 wt % aqueous sulfuric acid solution at 70° C. for 1 hour, the average corrosion rate is 3.5 mg / cm 2 The acid-resistant steel sheet according to claim 1 or 2, wherein the hardness is 0.05-0.05 h or less.
4. 4. The acid-resistant steel sheet according to claim 1, having an elongation of 30% or more.
5. A method for producing an acid-resistant steel sheet according to any one of claims 1 to 4, comprising the steps of: a step of heating a slab containing C: 0.1 wt% or less (excluding 0 wt%), Si: 2.0 to 4.0 wt%, Mn: 0.1 to 0.5 wt%, Al: 0.1 wt% or less, P: 0.01 wt% or less, S: 0.01 wt% or less, and N: 0.01 wt% or less, with the balance being Fe and unavoidable impurities, or a slab further containing one or more of Cr: 0.1 wt% or less, Ni: 0.1 wt% or less, Cu: 0.1 wt% or less, Nb: 0.1 wt% or less, and Mo: 0.1 wt% or less; hot rolling the slab to produce a hot rolled steel sheet; and subjecting the hot-rolled steel sheet to an acid treatment in an acid solution of 25% by weight or more for 10 seconds or more. A method for producing an acid-resistant steel sheet, comprising:
6. Heating the slab, The method for producing an acid-resistant steel sheet according to claim 5, wherein the slab is heated to 1200°C or higher.
7. In the step of producing the hot-rolled steel sheet, The finishing rolling temperature is Ar 3 The method for producing an acid-resistant steel sheet according to claim 5 or 6.
8. After the step of producing the hot rolled steel sheet, The method for producing an acid-resistant steel sheet according to any one of claims 5 to 7, further comprising a step of coiling the hot-rolled steel sheet at 550 to 750°C.
9. After the step of producing the hot rolled steel sheet, The method for producing an acid-resistant steel sheet according to claim 5 , further comprising a step of cold rolling the hot-rolled steel sheet.
10. After the step of producing the hot rolled steel sheet, The method for producing an acid-resistant steel sheet according to any one of claims 5 to 9, further comprising a step of annealing the hot-rolled steel sheet.