Coating method, thermal coating, and cylinder having thermal coating
By increasing the rotational speed of the plasma gun and adjusting the powder conveyance speed, the method addresses inefficiencies in conventional thermal spraying, resulting in higher quality and faster ceramic coatings for cylinder bores.
Patent Information
- Application Number
- JP2022028816
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-05-27
- Filing Date
- 2022-02-28
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2037-05-23
AI Technical Summary
Conventional thermal spraying methods are inefficient and costly for coating curved surfaces, particularly the concave inner surfaces of cylinder bores, leading to high residual stresses, cracks, and poor quality coatings, especially with ceramic materials like Cr2O3, which limits processing speed and efficiency.
A plasma coating method that increases the rotational speed of the plasma gun beyond conventional limits and adjusts the powder conveyance speed accordingly to improve coating quality and efficiency, reducing residual stresses and cracks.
The method achieves higher quality coatings with reduced cracks and improved processing speed, allowing for more efficient and cost-effective application of ceramic coatings on cylinder bores.
Smart Images

Figure 0007561154000001 
Figure 0007561154000002 
Figure 0007561154000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating method for coating curved surfaces, in particular the concave internal surfaces of a bore wall or a cylinder wall, a thermal coating and a cylinder with a thermal coating, as described in the preambles of the independent claims of the respective categories.
[0002] Thermal spraying methods such as plasma spraying or high velocity fuel spraying (HVOF) as well as corresponding plasma spraying devices such as so-called plasma guns are generally used to coat parts subjected to high thermal or mechanical stresses by melting a suitable material, e.g. a ceramic or alloy, with the aid of an arc generated in the plasma gun and depositing it on the surface to be coated with the aid of a gas flow.
[0003] As long as the surface to be coated is easily accessible from the outside or does not have any curved surface, it can be coated by conventional thermal spraying devices. However, if the inner wall of a hole or tubular geometry is to be coated, for example, a particular problem arises. If the wall of such a geometry is coated by a conventional thermal spraying device, for example by a plasma spraying device using a plasma jet that is mainly axially ejected relative to its longitudinal axis, it is very inefficient, since only a small part of the molten coating material is effectively deposited on the wall located radially relative to the longitudinal direction of the plasma spraying device.
[0004] Such problems arise in technical applications, particularly in the thermal coating of cylinder running surfaces of internal combustion engines, so that appropriate coatings are applied by various thermal spraying methods according to the prior art.
[0005] Currently, they are widely used in engines for all kinds of automobiles, aircraft, boats and ships, among others, though not exclusively.
[0006] Today, plasma spraying devices with a rotating plasma gun are generally used to coat the concave inner surface of a cylinder, but it is also possible to rotate the liner itself. In such special plasma spraying devices, the coating jet is ejected from the plasma gun perpendicular to the axis of rotation of the plasma gun or at a specific inclination angle to the axis of rotation and is projected onto the cylindrical concave surface, for example by a pressurized gas flow (often formed by an inert gas such as a noble gas or nitrogen, or simply by air), in order to form the desired surface layer. Coating methods or plasma spraying devices that utilize a spray powder as starting material for the coating have proven to be particularly successful in practice. Such rotating plasma spraying devices as well as corresponding plasma spraying methods have already been described, for example, in EP 0601968 A1. Very modern equipment, such as the SM-F210 gun from Oerlikon Metco, has been in use for a long time and is established on the market. However, solutions that utilize a blowing wire in a rotating gun are also already known, as shown, for example, in WO 2008 / 037514.
[0007] The corresponding cylinder running surfaces are usually activated by various processes prior to the thermal coating, e.g. by corundum jet, hard casting jet, high pressure water jet, various laser processes or other well-known activation processes. Substrates made of Al- or Mg-based light metal alloys, as well as iron-based or steel, etc., are pretreated and then coated. Surface activation ensures, among other things, good adhesion of the thermal spray coating.
[0008] There are also examples of specific applications where multi-layer systems may be advantageous, where multiple layers are sprayed, either alternating from different coating materials, or composed of the same material but deposited using different spray parameters, such that the deposited coating has very specific chemical, physical, topological or other properties that can vary, for example, through the thickness of the layer.
[0009] By these and several other innovative measures, now well known to those skilled in the art, the properties of the internal coatings of cylinders in particular have been successively improved to date.
[0010] However, it has also been shown that different running surface materials require different coating application methods.
[0011] Coating material F6399 (Cr 2 O 3 Ceramic coatings such as PTFE-CuO4, PTFE-CuO4, and PTFE-CuO4 have proven to be much more difficult to process than metallic coatings such as XPT512 (low alloy carbon steel). This is reflected, among other things, in a common slowing of the layer deposition rate and, as a result, longer processing times.
[0012] It is therefore common knowledge in the prior art that at least for plasma coating with powder coating materials, the gun rotation must be limited to its maximum value, and thus the maximum powder delivery speed must be limited at the same time. The above-mentioned limitations on the rotation speed of the plasma gun unit necessarily also apply to the applicant's RotaPlasma® unit. This device is a tool manipulator that is used to rotate the APS internal gun in order to deposit the powder material inside the cylinder bore. The rotation speed limitation up to around 200 rpm does not only apply to the RotaPlasma® unit, but also applies to the same extent when using other rotary plasma guns with powder materials that are maintained in the prior art.
[0013] Such speed limitations have long been considered essential in thermal spraying to prevent excessive residual stresses, which may lead to damaging cracks or other damage to the thermal spray coating, with potentially fatal consequences, for example when cylinder liners of internal combustion engines are being coated, as is of course well known to those skilled in the art.
[0014] It has been shown that such risks not only exist but also extend to a considerable extent when ceramic coating materials are used, which leads, inter alia, to the fact that such plasma coating materials can only be applied at very low transport speeds of the plasma gun and the associated relatively low rotational speeds if a coating of sufficient quality is to be produced. This circumstance alone leads to the conclusion that ceramic coatings on the inner surface of cylinders cannot be produced economically with sufficient quality, especially on an industrial scale.
[0015] However, even if the coating is applied with a very low rotation speed of the plasma gun and a correspondingly low powder delivery speed, high residual stresses may still occur, which still cause cracks and other damage to the applied layer. This is tolerable within certain limited limits, but is of course undesirable, since even a slight crack development has a negative effect on the quality of the coating. Legislation places ever higher demands on environmental standards and fuel consumption, which plays a decisive role, especially in the case of cylinder coatings of internal combustion engines, since this is fundamentally easier to achieve with higher quality coatings. Low quality coatings also naturally lead to a shorter life of the tools in operation, which leads to shorter maintenance intervals, shorter overall service life and, ultimately, higher operating costs for the engines on which they are equipped. [Prior art documents] [Patent documents]
[0016] [Patent Document 1] European Patent Application Publication No. 0601968 [Patent Document 2] International Publication No. 2008 / 037514 Summary of the Invention [Problem to be solved by the invention]
[0017] It is therefore an object of the present invention to provide a plasma coating method for coating curved surfaces, particularly the concave inner surfaces of bore or piping walls, in particular the inner running surfaces of cylinder bores or inner walls of cylinder liners of internal combustion engines, which avoids the disadvantages known from the prior art and in particular provides a significant improvement over plasma coating coverage using powder materials, in that the resulting coating has significantly reduced residual stresses compared to the prior art, resulting in significantly reduced or no cracks or other damage, and can be applied more efficiently, more quickly and in a more cost-effective manner than using prior art methods. [Means for solving the problem]
[0018] The object of the present invention, which addresses these problems, is characterized by the features of the independent claims 1, 12 and 13.
[0019] Each dependent claim relates to particularly advantageous embodiments of the invention.
[0020] The invention therefore relates to a coating method for coating curved surfaces, in particular the concave internal surfaces of bore or cylinder walls, with a powder coating material using a thermal spraying device, in particular a plasma or HVOF thermal spraying device. In particular, a gun, in particular a plasma gun, is provided on a gun shaft of the thermal spraying device for generating a coating jet from the powder coating material by means of an arc, the gun being rotated around the shaft axis of the gun shaft at a predefined speed, with the coating jet for depositing the coating on the curved surface being directed at least to some extent radially from the shaft axis towards the curved surface. According to the invention, a gun speed is selected which is greater than the basic gun speed, and the delivery speed of the powder coating material is modified according to a predefined scheme such that the delivery speed is adapted to the gun speed.
[0021] As already mentioned above, the applicant's F6399(Cr 2 O3 Running surface materials such as XPT512 (low alloy carbon steel) are characterized by their ceramic material properties. Compared to metallic coatings such as XPT512 (low alloy carbon steel), ceramic materials are generally more difficult to machine. This is reflected, among other things, in the often slower deposition rates of the coating and the resulting longer machining times.
[0022] First of all, this problem in particular was addressed and finally solved by the present invention. Up to now, the maximum rotation speed of plasma guns such as RotaPlasma® units was limited to approximately 200 rpm, which also limited the maximum conveying speed of the powder coating material. This limitation was necessary if one did not want to risk high residual stresses in the layer. This risk is particularly problematic in the case of ceramic materials, which usually lead to the fact that they can only be applied at very low conveying speeds, which calls into question the cost-effectiveness of ceramic coatings.
[0023] Contrary to all previous assumptions of experts, it has been recognized for the first time by the present invention that the coating properties are dramatically improved by increasing the rotation speed of the plasma gun, for example up to 800 rpm or even more, and at the same time by a suitable increase in the conveying speed of the powder coating material in the coating process. A crucial finding of the present invention is therefore that, contrary to all previous assumptions, an increase in the rotation speed of the plasma gun does not necessarily lead to a deterioration of the coating properties, only if the conveying speed of the powder coating material is properly adapted. Experiments carried out by the inventors have clearly shown that increasing the relative speed between the powder jet and the surface to be coated (as a result of high rotation speeds) has a positive effect on the coating quality. This can be observed especially in the case of ceramic coatings. In addition to the improvement of the coating properties, the coating time can also be dramatically reduced. By the method according to the present invention, the coating time for coating a cylinder running surface can be easily reduced by a factor of 2 to 3 or even more.
[0024] Furthermore, the coating according to the invention is of significantly better quality than prior art coatings, particularly in the upper and lower edge regions of the internally coated cylinders. In this respect, the quality of coatings applied to the cylinder running surfaces of internal combustion engines has always been problematic, for example at the upper and lower ends of the cylinders. The edge regions were often of much lower quality, for example in terms of porosity, hardness, adhesion, etc., than the remaining part of the cylinder running surface further inside, since, for example, increased turbulence in the coating jet and / or other negative effects can occur in the edge regions during spraying. With the present invention, such defects are also largely eliminated, and a consistently high quality coating can be produced also in the edge regions of the cylinders.
[0025] In one embodiment which is particularly preferred in practice, the powder coating material is conveyed to the plasma gun at a predefined conveying speed. This conveying speed is adapted to the rotation speed of the plasma gun in such a way that the higher the rotation speed of the plasma gun, the higher the conveying speed of the powder coating material is selected as well. This means that if the rotation speed of the plasma gun is increased, the conveying speed of the powder coating material is preferably also increased. This makes it possible, for example, to obtain a similar or identical layer thickness despite a shorter treatment time with the plasma gun, i.e. despite a faster rotation of the plasma gun, as with a lower rotation speed of the plasma gun. Since the selection of the rotation speed and / or the adaptation of the conveying speed corresponding to this rotation speed is performed prior to the start of the coating pass, i.e. before the powder coating material is fed, no adaptation of the rotation speed and / or the conveying speed is necessary during the coating pass. A coating pass here can be understood as the deposition of a layer with one or more layers of powder coating material and / or other powder coating materials.
[0026] In practice, the base speed of the plasma gun and the base conveying speed for the powder coating material conveyance corresponding to the base speed are often prescribed and predetermined for technical reasons by the plasma gun to be used, such as the RotaPlasma® unit. In practice, the base speed of the plasma gun and the base conveying speed corresponding to the base speed are not only dependent on the specific plasma gun used, but are also very often determined by the coating material used or even by the geometry of the bore. It is therefore necessary to select the base speed and base conveying speed for a specific coating method, which in many cases also depends on the spray material.
[0027] The base rotational speeds and base conveying speeds are therefore nothing other than the rotational speeds and conveying speeds that have been used as standard in the prior art.
[0028] In practice, the rotational speed is usually increased above the base speed N=FM to achieve better coating and shorter coating times. N ×N 0 A particularly preferred conveying speed is also selected according to the given rotation factor F = FM F ×F 0 The base conveying speed is selected to exceed the base conveying speed by a conveying factor predetermined according to:
[0029] In particular, if the coating layer thickness does not change as the plasma gun rotates faster, the transport factor can be selected to be equal to the rotation factor. Those skilled in the art will appreciate that the thickness of the coating layer is given by FV=FM. N / FM F By suitable selection of the coefficient ratio according to FV=FM, the layer thickness can be determined as required, as well as by suitable selection of the rotation and / or transport coefficients, in particular FV=FM N / FM FIt can be understood that by suitable selection of the modulus ratio according to, other layer properties of the coating, in particular the hardness, microhardness, porosity, yield strength, elastic modulus or adhesive strength or other layer properties of the coating can also be determined. The modulus ratio FV can be in the range 0.5≦FV≦10, preferably in the range 0.75≦FV≦8, particularly preferably in the range 1≦FV≦4. However, the modulus ratio FV can also be FV=4 or FV=3 or FV=2 or FV=1.
[0030] In practice, an increased rotation speed of the powder plasma gun means, for example, a rotation speed of more than 200 rpm, preferably more than 400 rpm, or more than 600 rpm, in particular 800 rpm or more. An increased conveying speed means, for example, a conveying speed of more than 25 g / min, preferably more than 50 g / min, or more than 50 g / min, in particular 100 g / min or more. The increased rotation speeds and conveying speeds given above are particularly typically for plasma gun units of the RotaPlasma® type. However, it can be understood that these values can also be applied for other powder plasma gun units. This is because technically relevant deposition rates are determined primarily by the properties of the substrate and the spray material used, in particular whether it is ceramic or metallic or non-metallic material, and only secondarily depending on the type of rotary plasma gun.
[0031] Ceramic coating materials, especially TiO 2 or Cr 2 O 3 are preferably used as coating materials for coating cylinder running surfaces, in particular for cylinders of internal combustion engines, and / or metallic coating materials, in particular low-alloy steels, in particular Fe-1.4Cr-1.4Mn-1.2C or other coating materials are also advantageously used as coating materials.
[0032] The coating according to the invention may also be applied in a manner known per se in the form of a multi-layer coating, depending on the requirements or applications, where these layers may consist of the same or different coating materials, so that the multi-layer coating can have the same or different layer properties, in particular hardness, microhardness, porosity, yield strength, elastic modulus or adhesive strength.
[0033] The invention further relates to a thermal coating on the inner surface of the cylinder wall, in particular on the cylinder running surface of a cylinder of an internal combustion engine, which is applied by the coating method according to the invention, and also to a cylinder of an internal combustion engine having a thermal coating applied using the coating method according to the invention.
[0034] In the following, the invention will be explained in more detail with reference to the drawings.
[0035] The figures are presented diagrammatically. [Brief description of the drawings]
[0036] [Figure 1] FIG. 2 is a schematic diagram of an embodiment of the coating method according to the invention using the example of a cylinder running surface. [Diagram 2] FIG. 4 is a schematic diagram for explaining the relationship between the number of rotations and the conveying speed. [Figure 3a] Illustrated cross section of TiO2 coating sprayed at 200 rpm. [Figure 3b] Illustrated cross section of TiO2 coating sprayed at 400 rpm. [Figure 3c] Illustrated cross section of TiO2 coating sprayed at 600 rpm. [Figure 3d] Illustrated cross section of TiO2 coating sprayed at 800 rpm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0037] The present invention will now be described, by way of example only, with reference to a plasma spray process, although it will be appreciated that the present invention is not limited to plasma spray processes and may be practiced with any suitable spray process, such as, for example, an HVOF process.
[0038] FIG. 1 shows diagrammatically the implementation of a simple embodiment of the method according to the invention, using the example of coating the cylinder running surfaces of the cylinders of a passenger car engine.
[0039] In the method according to the invention shown in FIG. 1, a coating 8 is applied to a curved surface 1, which is the concave cylinder running surface of a passenger car cylinder.
[0040] In FIG. 1, a plasma gun 6 is provided in a known manner on a gun shaft 5 of a plasma spraying device 4 for generating a coating jet 7 from a powder coating material 3 by means of an electric arc. In this case, the plasma gun 6 is arranged rotatably about the shaft axis A of the gun shaft 5 for coating a curved surface 1. In the example of FIG. 1, the gun shaft 3 rotates in the direction indicated by the arrow N with a number of revolutions N. A coating jet 7 for applying a coating 8 to the curved surface 1, i.e. here the cylinder running surface of a cylinder, is directed essentially radially from the shaft axis A towards the curved surface 1, so that the curved surface 1 is applied with the coating material 3 as efficiently as possible. The basic rotation speed N of the plasma gun 6 is 1000 rpm. 0 A high rotation speed of the plasma gun 6 was selected for the plasma gun 6 (see FIG. 2) and the conveying speed F of the powder coating material 3 was changed according to certain rules, not shown in FIG. 1, in order for the conveying speed F to be appropriately adapted to the high rotation speed N of the plasma gun 6. The basic rotation speed of the plasma gun 6 is approximately 200 rpm in the case of the plasma spray unit 4 used in FIG. 1, which here comprises, for example, a RotaPlasma® unit.
[0041] In detail, in the method described in FIG. 1, the powder coating material 3 is conveyed to the plasma gun 6 at a given conveying speed F. This conveying speed F is determined by its basic rotation speed N 0The rotation speed N of the plasma gun 6 is adapted in such a way that, corresponding to a rotation speed N of the plasma gun 6 exceeding the basic conveying speed F, the high conveying speed F of the powder coating material 3 is selected as well. 0 It means bigger.
[0042] A schematic diagram illustrating the relationship between the rotation speed N and the conveying speed F is shown in FIG. 2. The conveying speed F is plotted on the ordinate axis and the rotation speed N is plotted on the abscissa axis. The curves in the graph show specific examples of how a parameter pair (conveying speed F / rotation speed N) can be appropriately selected for a given plasma spraying device 4 and powder coating material 3 to be used. The coordinates in the graph (F 0 / N 0 ) corresponds to the parameter pair used in the prior art, and the parameter pair (FM F xF 0 / FM N xN 0 ) is a specific parameter pair (F) used for coating in the thermal spray process according to the present invention, for example as described in FIG. 1 / N 1 ) is supported.
[0043] It is obviously to be understood that the curve in Fig. 2 is merely schematic: in reality, the curve shown in Fig. 2 is very often a straight line, so that for example the rotation speed N and the conveying speed F are always modified by the same factor, so that the same layer thickness D of the coating 8 is always achieved even at different rotation speeds N.
[0044] In principle, it is of course also possible to choose parameter pairs (N / F) that lie above or below the curve according to FIG. 2, in which case, for example, smaller or larger layer thicknesses D are achieved at different rotational speeds F. And / or other parameters of the coating 8, in particular the hardness, microhardness, porosity, yield strength, elastic modulus or adhesive strength or other layer properties of the coating 8, are affected by the rotational factor FM N and / or the conveying speed F FBy suitable selection of FV=FM N / FM F It can be realized that this is determined by suitable selection of the coefficient ratio FV according to
[0045] Finally, Figs. 3a to 3d show TiO 2 Illustrated are four coating cross sections, each sprayed at a different rotation speed N and a correspondingly adapted different conveying speed F.
[0046] FIG. 3a shows a coating 8 sprayed on a cylinder wall 2 by a method according to the prior art using a RotaPlasma® plasma spraying device 4. Here, conventional parameters were selected with a rotation speed of N=200 rpm and a conveying speed of F=25 g / min. As can be clearly seen, the coating 8 has fine cracks R, which were previously considered acceptable, but are not desirable in nature. In addition to the cracks R, fine pores P can also be seen in all coatings from FIG. 3a to FIG. 3d. These pores are usually desirable and even lead to a given porosity.
[0047] The coating 8 according to FIG. 3b was sprayed with twice the rotation speed N=400 rpm and twice the conveying speed F=50 g / min compared to the prior art according to FIG. 3a. It is clearly visible that the formation of cracks R in the coating 8 is reduced. The quality of the coating is therefore significantly improved.
[0048] The coating 8 according to Fig. 3c was sprayed with three times the rotation speed N=600 rpm and three times the conveying speed F=75 g / min compared to the prior art according to Fig. 3a. Indeed, no cracks R can be found in the coating 8. The quality of the coating is therefore improved.
[0049] Finally, the coating 8 according to Fig. 3d was sprayed with a rotation speed N=800 rpm and a conveying speed F=100 g / min four times higher than that of the prior art according to Fig. 3a, where no cracks are present in the coating 8. The quality of the coating is therefore improved and is considered ideal for practical use.
[0050] The invention is not limited to the described embodiments, in particular it is expressly intended that the invention encompasses all suitable combinations of the described embodiments.
Claims
1. A coating method for coating a curved surface (1) with a powder coating material (3) using a thermal spraying device (4), comprising the steps of: a gun (6) is provided on a gun shaft (5) of the thermal spraying device (4) for generating a coating jet (7) from the powder coating material (3) by means of an electric arc, the gun (6) being rotated about a shaft axis (A) of the gun shaft (5) at a predetermined number of revolutions (N); The coating method, wherein the coating jet (7) for depositing a coating (8) on the curved surface (1) is directed at least in part radially from the shaft axis (A) towards the curved surface (1), the rotational speed (N) of the gun (6) is selected to be greater than a base rotational speed (N 0 ), said base rotational speed (N 0 ) being 200 rpm; the delivery speed (F) of the powder coating material (3) is selected to be greater than the basic delivery speed (F 0 ) according to a predetermined rule so as to match the number of revolutions (N) of the gun (6) which is greater than the basic number of revolutions (N 0 ); N=FM N ×N 0 The rotation factor (FM N ) and F = FM F ×F 0 The transport coefficient (FM F ) is selected, FV = FM N / FM F wherein 1≦FV≦4.
2. 2. The coating method according to claim 1, wherein the curved surface (1) is a concave inner surface (1) of a bore or cylinder wall (2).
3. 3. A coating method according to claim 1 or 2, wherein the thermal spraying device (4) is a plasma thermal spraying device (4) or an HVOF thermal spraying device.
4. The basic rotation speed (N 0 ) corresponding to the basic conveying speed (F 0 4. The coating method according to claim 1, wherein the powder coating material (3) is delivered to the substrate by a predetermined distance from the substrate.
5. The basic rotation speed (N 0 ) corresponding to the basic conveying speed (F 0 5. The coating method according to claim 4, wherein the powder coating material (3) used is selected as a function of the powder coating material (3).
6. The thickness (D) of the layer of the coating (8) is FV = FM N / FM F 6. The coating method according to claim 4 or claim 5, wherein the coefficient ratio (FV) is determined by selecting a coefficient ratio (FV) according to
7. The rotation factor (FM N ) and / or the transport factor (FM F 7. The coating method according to claim 4, wherein the layer properties of the coating (8) are determined by suitable selection of:
8. 8. The coating method according to claim 7, wherein the layer property is hardness, microhardness, porosity, yield strength, elastic modulus or adhesive strength of the coating (8).
9. 9. The coating method according to claim 1, wherein the rotation speed (N) is greater than 400 rpm.
10. 10. The coating method according to claim 1, wherein the conveying speed (F) is greater than or equal to 25 g / min.
11. said coating material (3) being a ceramic coating material (3); and / or 11. The coating method according to any one of the preceding claims, wherein the coating material (3) is a metallic coating material (3).
12. The coating material is a ceramic coating material, and the ceramic coating material is TiO 2 or Cr 2 O 3 12. The coating method according to claim 11, wherein
13. 12. The method of claim 11, wherein the coating material is a metallic coating material, the metallic coating material being a low alloy steel.
14. 14. The method of claim 13, wherein the low alloy steel is Fe-1.4Cr-1.4Mn-1.2C.
15. A multi-layer coating (8) composed of the same or different coating materials (3) is applied, and / or 15. The coating method according to any one of the preceding claims, wherein the multi-layer coating (8) has identical or different layer properties.
16. 16. The coating method of claim 15, wherein the layer property is hardness, microhardness, porosity, yield strength, elastic modulus, or adhesive strength.
Citation Information
Patent Citations
Plasma spray gun
EP0601968A1
Thermal spray coating film forming method, and sliding member
JP2005171274A
Method for forming thermal-sprayed coating
JP2005272890A
Powder thermal spray process and powder thermal spray device
JP2006322049A
Rotating wire spraying device and a method for coating a surface of a workpiece
WO2008037514A1