Molded body, manufacturing method of molded body, and manufacturing method of sintered body
Patent Information
- Application Number
- JP2023512898
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-07
- Filing Date
- 2022-03-16
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2042-03-16
AI Technical Summary
【0009】 本発明によれば、運搬時における塑性変形を抑制することができる成形体を提供することができる。
Smart Images

Figure 0007561272000001 
Figure 0007561272000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a molded body, a method for producing a molded body, and a method for producing a sintered body. [Background technology]
[0002] Particularly precise sintered bodies or sintered bodies of complex shapes that utilize sinterable powders such as metals, ceramics, and cermets are manufactured as follows. First, a composition for sintered bodies containing sinterable powder and a binder is prepared. Next, the prepared composition for sintered bodies is heated and kneaded to obtain a raw material for sintered bodies, which is then injection molded to form a green body. Next, the green body is subjected to a debinding process, and the binder is removed from the green body by heat treatment or solvent treatment. Finally, the green body from which the binder has been removed is sintered at a predetermined temperature. In this manner, a sintered body is obtained.
[0003] In the above-mentioned sintered body manufacturing process, the green molded body obtained by injection molding the composition for sintered body may undergo plastic deformation such as distortion or breakage during transportation to the debinding step. Regarding the plastic deformation of such green molded bodies, the bending strength (green strength) of the green molded body has conventionally been used as an index to evaluate the plastic deformability of the green molded body (see, for example, Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2009-542880 [Patent Document 2] JP 2001-106581 A [Patent Document 3] JP 2005-205805 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the evaluation using bending strength as an index as described in Patent Documents 1 to 3, a green molded body that has a yield point outside the elastic region is evaluated as a non-defective product. As a result, when an external force close to the maximum bending strength is applied to the green molded body during transportation, composition deformation may occur.
[0006] The present invention has been made in view of the above problems, and an object of the present invention is to provide a molded body capable of suppressing plastic deformation during transportation. [Means for solving the problem]
[0007] As a result of intensive research into solving the above-mentioned problems, the inventors discovered that the above problems can be solved by having a green body not only have a predetermined bending yield strength but also a predetermined bending modulus, and thus completed the present invention.
[0008] That is, the present invention is as follows. [1] A molded body comprising a sinterable inorganic powder and an organic binder, The molded body has a flexural modulus (MPa) of 4,000 to 15,000 at a strain of 0.05% to 0.1%, The bending yield strength (MPa) is 10 or more. Molded body. [2] The molded article according to [1] above, wherein the product of the flexural modulus (MPa) and the flexural yield strength (MPa) is 50,000 or more. [3] When observing the cross section under a microscope, 2 The molded article according to [1] or [2] above, having 10 or less voids of 30 μm or more per unit area. [4] The molded body according to any one of the above [1] to [3], wherein the maximum particle size of the sinterable inorganic powder is 30 μm or less. [5] The molded article according to any one of the above [1] to [4], wherein the organic binder comprises a polyacetal resin. [6] The molded article according to [5] above, wherein the polyacetal resin has a melt flow rate of 70 to 200 g / 10 min. [7] The molded body according to any one of the above [1] to [6], wherein the sinterable inorganic powder is contained in an amount of 75% by mass or more and 95% by mass or less relative to 100% by mass of the molded body. [8] The molded body according to any one of the above [1] to [8], wherein the sinterable inorganic powder is a metal powder. [9] The area with a thickness of 1mm or less is 100mm 2 The molded article according to any one of the above [1] to [8],
[10] A method for producing a molded body comprising a sinterable inorganic powder and an organic binder, comprising the steps of: A kneading step of kneading a sinterable inorganic powder with an organic binder to obtain a kneaded mixture; a molding step of molding the kneaded mixture to obtain a molded body; Including, The molded body has a flexural modulus (MPa) of 4,000 to 15,000 at a strain of 0.05% to 0.1%, A method for producing a molded product, characterized in that the molded product has a bending yield strength (MPa) of 10 or more.
[11] The method for producing a molded body according to
[10] above, wherein the kneading temperature in the kneading step is 160°C to 200°C.
[12] 12. The method for producing a molded article according to claim 10, wherein a cylinder temperature in the molding step is 150°C to 190°C.
[13] 13. The method for producing a molded article according to claim 10, wherein the injection pressure in the molding step is 50 MPa or more.
[14] 14. The method for producing a molded body according to claim 10, wherein the sinterable inorganic powder is contained in an amount of 75% by mass or more and 95% by mass or less relative to 100% by mass of the molded body.
[15] a debinding step of removing the organic binder from the molded body according to any one of the above [1] to [9] or the molded body produced by the method for producing a molded body according to any one of the above
[10] to
[14] by heating or chemical treatment to obtain a sintered precursor; a sintering step of sintering the sintering precursor to obtain a sintered body; A method for producing a sintered body, comprising: Effect of the Invention
[0009] According to the present invention, it is possible to provide a molded body capable of suppressing plastic deformation during transportation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following description, and can be modified in various ways within the scope of the present invention.
[0011] [Molded body] The molded body of this embodiment contains a sinterable inorganic powder and an organic binder. The molded body of this embodiment is a preform (green molded body) obtained by injection molding a composition for a sintered body containing the inorganic powder and an organic binder, before being degreased and sintered. In this specification, the term "molded body" means a "green molded body" and is clearly distinguished from a "sintered body" obtained by degreasing and sintering a green molded body.
[0012] It is essential that the molded body of this embodiment has a flexural modulus (MPa) of 4000 to 15000 at a strain of 0.05% to 0.1%. It is also essential that the molded body of this embodiment has a flexural yield strength (MPa) value of 10 or more. If the molded body has a flexural modulus (MPa) of 4000 to 15000 at a strain of 0.05% to 0.1% and a flexural yield strength (MPa) value of 10 or more, it is possible to suppress the molded body from being subjected to plastic deformation such as distortion or breakage when being transported. The flexural modulus and flexural yield strength can be measured by the method described in the Examples below.
[0013] From the viewpoint of strength of the molded article, the flexural modulus (MPa) at a strain of 0.05% to 0.1% is preferably at least 5000, more preferably at least 6000, and even more preferably at least 7000. From the viewpoint of thin-wall formability, the upper limit is preferably at most 14500, more preferably at most 14000, and even more preferably at most 13000.
[0014] From the viewpoint of the strength of the molded body, the bending yield strength is preferably more than 10 MPa, more preferably 15 MPa or more. From the viewpoint of making the molded body less likely to break when dropped, the upper limit is preferably 40 MPa or less, more preferably 35 MPa or less.
[0015] The product of the flexural modulus (MPa) and the flexural yield strength (MPa) is preferably at least 50,000, and more preferably at least 100,000. If the product of the flexural modulus and the flexural yield strength is at least 50,000, the occurrence of plastic deformation such as distortion or breakage in the molded body during transportation can be further suppressed.
[0016] In addition, when the cross section of the molded product of this embodiment was observed under a microscope, 2It is preferable that the number of voids of 30 μm or more per unit area is 10 or less. This can further suppress the occurrence of plastic deformation such as distortion or breakage in the molded body when transporting the molded body. The observation of the cross section with the microscope can be performed by the method described in the Examples below.
[0017] The molded article of the present embodiment preferably has at least a portion having a thickness of 1 mm or less. 2 It is preferable that the number of layers is more than 100 mm. 2 Generally, the wider the thin-walled portion of a molded body that is 1 mm or less in thickness, the more likely it is that plastic deformation will occur during transportation, but the molded body of this embodiment can effectively suppress plastic deformation during transportation even when it has a wide thin-walled portion of 1 mm or less in thickness.
[0018] The molded body according to the present embodiment can be obtained by producing a composition for a sintered body, which contains a sinterable inorganic powder and an organic binder that constitute the molded body, and then injection molding the produced composition for a sintered body using a heated screw type and piston type injection molding machine. The composition for sintered body, and therefore the molded body, may further contain other additives in addition to the inorganic powder and the organic binder.
[0019] <Sinterable inorganic powder> In this embodiment, the "sinterable inorganic powder" (hereinafter, may be simply referred to as "inorganic powder") can be selected from all known suitable sinterable inorganic powders. Preferably, it is selected from metal powders, alloy powders, metal carbonyl powders, and mixtures thereof. Among them, in order to impart functionality, metal powders and ceramic powders are more preferable, and metal powders are particularly preferable. The above sinterable inorganic powders may be used alone or in combination of two or more kinds.
[0020] Specific examples of the metal powders include powders of aluminum, magnesium, barium, calcium, cobalt, zinc, copper, nickel, iron, silicon, titanium, tungsten, and metal compounds and metal alloys based on these metals, whereby not only already completed alloys but also mixtures of the individual alloy components can be used.
[0021] Examples of ceramic powders include oxides such as zinc oxide, aluminum oxide, and zirconia; hydroxides such as hydroxyapatite; carbides such as silicon carbide; nitrides such as silicon nitride and boron nitride; halides such as fluorite; silicates such as stearite; titanates such as barium titanate and lead zirconate titanate; carbonates; phosphates; ferrite; high-temperature superconducting materials; and the like.
[0022] The inorganic powders described above may be used alone, or may be used in combination with several inorganic substances such as various metals, metal alloys, ceramics, etc. Particularly preferred metals and alloys include titanium alloys and stainless steels such as SUS316L, and preferred ceramics include Al2O3 and ZrO2.
[0023] The average particle size of the inorganic powder is preferably 30 μm or less, more preferably 20 μm or less. The maximum particle size of the inorganic powder is preferably 30 μm or less, more preferably 20 μm or less. If the maximum particle size of the inorganic powder is 30 μm or less, the metal powder can be dispersed, and an injection molded body with higher strength can be obtained. The average particle size and maximum particle size can be measured, for example, by a particle size distribution measuring device using a laser diffraction method.
[0024] The mass ratio of the sinterable inorganic powder is preferably 70 to 95 mass%, more preferably 75 to 95 mass%, and particularly preferably 80 to 95 mass%, relative to 100 mass% of the molded body. When the sinterable inorganic powder is within the above range, a composition for a sintered body having a melt viscosity suitable for injection molding can be obtained, and a molded body with high strength can be obtained.
[0025] <Organic binder> The organic binder is not particularly limited, but preferably contains a polyacetal resin. By using a polyacetal resin, which is a depolymerized polymer, as an organic binder, a molded body having excellent shape retention can be obtained due to the rigidity of the polyacetal resin. The molded body has excellent shape retention even after a degreasing step by heating, and no residue remains after the degreasing step by heating. Furthermore, the degreasing step by heating can be performed quickly, thereby improving production efficiency.
[0026] (Polyacetal resin) The polyacetal resin may be a polyacetal homopolymer, a polyacetal copolymer, or a mixture thereof. Among these, the polyacetal resin is preferably a polyacetal copolymer from the viewpoint of thermal stability. The polyacetal resins may be used alone or in combination of two or more.
[0027] The polyacetal homopolymer may be a polymer having an oxymethylene unit in the main chain, and both ends of the polymer may be blocked with an ester group or an ether group. The polyacetal homopolymer may be obtained from formaldehyde and a known molecular weight regulator as raw materials, and may be obtained from these raw materials by a known slurry method using a known onium salt polymerization catalyst and a hydrocarbon as a solvent, for example, the polymerization method described in JP-B-47-6420 and JP-B-47-10059. The polyacetal homopolymer is preferably one in which 99.8 mol % or more of the main chain excluding both ends is composed of oxymethylene units, and more preferably the main chain excluding both ends is composed only of oxymethylene units.
[0028] The polyacetal copolymer includes a polymer having an oxymethylene unit and an oxyethylene unit in the main chain, and can be obtained, for example, by copolymerizing trioxane with a cyclic ether and / or a cyclic formal in the presence of a polymerization catalyst. Trioxane is a cyclic trimer of formaldehyde, and is generally obtained by reacting an aqueous formalin solution in the presence of an acid catalyst.
[0029] The trioxane may contain impurities such as water, methanol, formic acid, and methyl formate that can cause chain transfer, and it is therefore preferable to remove these impurities by, for example, distillation or other methods for purification. In this case, the total amount of impurities that can cause chain transfer is preferably 1×10 per mol of trioxane. -3 mol or less, and more preferably 0.5×10 -3 By reducing the amount of impurities to the above values, the polymerization reaction rate can be increased sufficiently for practical use, and the resulting polymer has excellent thermal stability.
[0030] The cyclic ether and / or cyclic formal are components that can be copolymerized with the above-mentioned trioxane, and examples thereof include ethylene oxide, propylene oxide, butylene oxide, epichlorohydrin, epibromohydrin, styrene oxide, oxatane, 1,3-dioxolane, ethylene glycol formal, propylene glycol formal, diethylene glycol formal, triethylene glycol formal, 1,4-butanediol formal, 1,5-pentanediol formal, and 1,6-hexanediol formal. In particular, ethylene oxide and 1,3-dioxolane are preferred. These may be used alone or in combination of two or more.
[0031] The amount of the cyclic ether and cyclic formal added is preferably 1.0 mol% or more, more preferably 3.0 mol% or more, and even more preferably 3.5 mol% or more, based on 1 mol of the trioxane. Also, the amount is preferably 8.0 mol% or less, more preferably 7.0 mol% or less, and even more preferably 5.0 mol% or less, based on 1 mol of the trioxane.
[0032] The polymerization catalyst includes boric acid, tin, titanium, phosphorus, arsenic and antimonides, which are typified by Lewis acids. In particular, boron trifluoride, boron trifluoride hydrates, and boron trifluoride coordination complexes containing organic compounds containing oxygen or sulfur atoms. For example, boron trifluoride, boron trifluoride diethyl etherate, and boron trifluoride-di-n-butyl etherate are preferred. These may be used alone or in combination of two or more.
[0033] The amount of polymerization catalyst added was 0.1×10 -5 ~0.1×10 -3 mol range is preferred, and 0.3×10 -5 ~0.5×10 -4 mol, more preferably 0.5×10 -5 ~0.4×10 -4 When the amount of the polymerization catalyst added is within the above range, the polymerization reaction can be stably carried out for a long period of time.
[0034] In the production of polyacetal copolymers, deactivation of a polymerization catalyst is carried out by putting a polyacetal resin obtained by a polymerization reaction into an aqueous solution or organic solvent liquid containing at least one catalyst neutralizing deactivator such as amines such as ammonia, triethylamine, tri-n-butylamine, or hydroxides of alkali metals or alkaline earth metals, inorganic acid salts, organic acid salts, etc., and stirring the mixture in a slurry state for generally several minutes to several hours. The slurry after catalyst neutralization and deactivation is filtered and washed to remove unreacted monomers, catalyst neutralizing deactivators, and catalyst neutralization salts, and then dried.
[0035] In addition, the polymerization catalyst can be deactivated by contacting the polyacetal copolymer with vapor of ammonia, triethylamine, or the like, or by contacting the polyacetal resin with at least one of hindered amines, triphenylphosphine, calcium hydroxide, or the like in a mixer.
[0036] Alternatively, without deactivating the polymerization catalyst, the polyacetal copolymer may be heated in an inert gas atmosphere at a temperature equal to or lower than the melting point of the polyacetal copolymer to reduce the volatilization of the polymerization catalyst, and then the terminal stabilization treatment described below may be carried out using the polyacetal copolymer. The above-mentioned deactivation operation of the polymerization catalyst and the operation of reducing the volatilization of the polymerization catalyst may be carried out after pulverizing the polyacetal resin obtained by the polymerization reaction, if necessary.
[0037] The terminal stabilization treatment of the obtained polyacetal resin involves decomposing and removing the unstable terminal moiety by the following method: For example, the unstable terminal moiety can be decomposed and removed by melting the polyacetal resin using a vented single screw extruder or a vented twin screw extruder in the presence of a known basic substance capable of decomposing unstable terminal moieties, such as ammonia, fatty acid amines such as triethylamine and tributylamine, hydroxides of alkali metals or alkaline earth metals such as calcium hydroxide, inorganic weak acid salts, or organic weak acid salts, as a notching agent.
[0038] The mass proportion of the polyacetal resin in the organic binder is preferably 5 to 95 mass %, more preferably 5 to 70 mass %, and particularly preferably 5 to 60 mass %, relative to 100 mass % of the organic binder. When the organic binder is removed from the molded body by heating, the mass ratio of the polyacetal resin is preferably 5 to 50 mass%, more preferably 5 to 45 mass%, and particularly preferably 10 to 40 mass%, relative to 100 mass% of the organic binder. By setting the ratio of the polyacetal resin in the organic binder within the above range, the shape of the green molded body tends to be well maintained.
[0039] The melt flow rate of the polyacetal resin is preferably 70 g / 10 min or more and 200 g / 10 min or less, more preferably 90 g / 10 min or more and less than 200 g / 10 min, and even more preferably 90 g / 10 min or more and less than 140 g / 10 min, as measured in accordance with ASTM-D-1238-57T at 190° C. and 2.16 kg. By setting the melt flow rate to 70 g / 10 min or more, the fluidity of the composition for sintered body is improved, and by setting the melt flow rate to 200 g / 10 min or less, the strength of the molded body can be improved. The melt flow rate of the polyacetal resin can be increased by increasing the amount of a molecular weight regulator (e.g., methylal, methanol, formic acid, methyl formate, etc.) added during polymerization.
[0040] The melting point of the polyacetal resin is preferably 100 to 200° C., and more preferably 140 to 180° C. The melting point is a peak melting temperature measured according to JIS K7121, and when multiple melting temperatures exist, it is the higher melting point.
[0041] The organic binder preferably contains a polyolefin resin, and more preferably contains a polyacetal resin and a polyolefin resin. Since polyacetal resin and polyolefin resin have different thermal decomposition starting points, it is possible to gradually remove the organic binder from the molded body during the temperature rise process when the molded body is heated and degreased. In acid degreasing, the polyacetal resin is decomposed by an acid such as nitric acid and removed from the molded body, but by blending a polyolefin resin that is not decomposed by acid, the shape of the molded body from which the polyacetal resin has been removed can be maintained.
[0042] (Polyolefin resin) The polyolefin resin is a homopolymer or copolymer having a structural unit derived from an alkene having 2 to 8 carbon atoms, preferably 2 to 4 carbon atoms.
[0043] From the viewpoints of mixability with sinterable inorganic powders when preparing a composition for a sintered body, and injection moldability when producing a molded body using the composition for a sintered body, it is desirable for the polyolefin resin to have a melt flow rate measured under conditions of 190°C and 2.16 kg of 40 g / 10 min or more.
[0044] Specific examples of the polyolefin resin include polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyisoprene, polybutadiene, etc. Polyethylene, polypropylene, and mixtures thereof are preferred, and polyethylene or polypropylene is more preferred from the viewpoint of the shape retention of the molded body when it is transported to the degreasing process and the suppression of cracking and swelling in the degreasing process. Examples of commercially available polyethylene that can be suitably used include Santech HD series (manufactured by Asahi Kasei), Santech LD series (manufactured by Asahi Kasei), Santech EVA series (manufactured by Asahi Kasei), Neozex, Ultzex, and Evolue (all manufactured by Prime Polymer), and examples of polypropylene include Sumitomo Noblen (manufactured by Sumitomo Chemical), Novatec PP (manufactured by Japan Polypropylene), Sanallomer PM series (manufactured by Sanallomer Co., Ltd.), and Prime Polypro (manufactured by Prime Polymer).
[0045] From the viewpoint of shape retention of a molded product after acid degreasing, the polyolefin resin is preferably not easily decomposed by acid. From the viewpoint of shape retention of a molded product after acid degreasing, the weight of the polyolefin resin after immersion in a 30% aqueous nitric acid solution at 23°C (room temperature) and 70°C for 24 hours according to the method described in JIS K 7114 is preferably 10% or less, more preferably 5% or less, and particularly preferably 1% or less, of the weight before immersion.
[0046] From the viewpoint of maintaining the shape of the molded body and maintaining the shape of the molded body well after acid degreasing, the mass proportion of the polyolefin resin in the organic binder is preferably 5 to 95 mass%, more preferably 5 to 70 mass%, and particularly preferably 5 to 60 mass%, relative to 100 mass% of the organic binder.
[0047] When the organic binder contains a polyacetal resin and a polyolefin resin, the mass ratio of the polyolefin resin to 100 parts by mass of the polyacetal resin is preferably 1 to 200 parts by mass, more preferably 5 to 150 parts by mass, and even more preferably 10 to 120 parts by mass.
[0048] The total mass ratio of the polyacetal resin and the polyolefin resin in 100% by mass of the organic binder is preferably 45% by mass or more, and the total mass ratio of the polyacetal resin, the polyolefin resin, and a fluidity imparting agent described below in 100% by mass of the organic binder is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more.
[0049] From the viewpoint of further reducing cracks and blistering during the degreasing step, the difference between the thermal decomposition onset point (°C) of the polyacetal resin and the thermal decomposition onset point (°C) of the polyolefin resin is preferably 30°C or more, more preferably 30 to 100°C. The thermal decomposition onset point is a temperature measured using a thermogravimetric differential thermal analyzer.
[0050] (Fluidity imparting agent) The composition for sintering to obtain a molded body preferably further contains a fluidity imparting agent. By containing the fluidity imparting agent, the fluidity of the composition for sintering can be further improved. The fluidity imparting agent is a compound other than the polyacetal resin and polyolefin resin, and examples thereof include waxes. Examples of the waxes include paraffin wax, polyethylene wax, polypropylene wax, carnauba wax, polyethylene glycol, polytetramethylene glycol, polytetraethylene glycol, polyisobutylene, microcrystalline wax, montan wax, beeswax, Japan wax, synthetic wax, poly-1,3-dioxolane, poly-1,3-dioxepane, etc. Among them, paraffin wax, polyethylene glycol, and polytetramethylene glycol are preferred from the viewpoint of providing a more excellent fluidity of the composition for sintered body in injection molding.
[0051] From the viewpoint of achieving even better fluidity of the composition for sintered body during injection molding, the mass proportion of the fluidity imparting agent is preferably 5 to 60 mass %, more preferably 5 to 50 mass %, and particularly preferably 10 to 50 mass %, relative to 100 mass % of the organic binder.
[0052] (Nitrogen-containing compounds, fatty acid metal salts) The polyacetal resin preferably further contains a nitrogen-containing compound and / or a fatty acid metal salt, and more preferably contains a nitrogen-containing compound and a fatty acid metal salt. By including the nitrogen-containing compound and the fatty acid metal salt, the extrudability, thermal stability, and suppression of foreign matter during the production of polyacetal resin can be improved. In addition, the flowability of the composition for sintered body kneaded with the metal powder and the strength of the molded body tend to be improved at the same time. By including the nitrogen-containing compound and the fatty acid metal salt, the composition for sintered body has improved thermal stability.
[0053] The nitrogen-containing compound is not particularly limited, but examples thereof include polyamide resins, amide compounds, urea derivatives, triazine derivatives, etc., and among them, polyamide resins are preferred from the viewpoint of providing a composition for sintering with better thermal stability and a molded body with better strength. These compounds may be used alone or in combination of two or more.
[0054] Examples of the polyamide resin include, but are not limited to, nylon 6, nylon 11, nylon 12, nylon 66, nylon 6·10, nylon 6 / 6·10, nylon 6 / 6·6, nylon 6·6 / 6·10, nylon 6 / 6·6 / 6·10, poly-β-alanine, and the like, which are obtained by condensation of diamines and dicarboxylic acids, condensation of amino acids, ring-opening polymerization of lactams, etc.
[0055] Examples of the amide compound include, but are not limited to, stearyl stearamide, stearyl oleamide, stearyl erucamide, ethylenediamine-distearate amide, ethylenediamine-dibehenate amide, hexamethylenediamine-distearate amide, ethylenediamine-dierucate amide, xylylenediamine-dierucate amide, di(xylylenediamine-stearate amide), and sebacate amide, which are produced from an aliphatic monocarboxylic acid, an aliphatic dicarboxylic acid, an aromatic monocarboxylic acid, or an aromatic dicarboxylic acid and an aliphatic monoamine, an aliphatic diamine, an aromatic monoamine, or an aromatic diamine.
[0056] The urea derivative is not particularly limited, but examples thereof include N-phenylurea, N,N'-diphenylurea, N-phenylthiourea, and N,N'-diphenylthiourea.
[0057] The triazine derivative is not particularly limited, but examples thereof include melamine, benzoguanamine, N-phenylmelamine, melem, N,N'-diphenylmelamine, N-methylolmelamine, N,N'-trimethylolmelamine, 2,4-diamino-6-cyclohexyltriazine, and melam.
[0058] The mass ratio of the nitrogen-containing compound is preferably 0.005 to 0.2 parts by mass, and particularly preferably 0.005 to 0.1 parts by mass, relative to 100 parts by mass of the polyacetal resin. The mass ratio of the nitrogen-containing compound within the above range is preferable from the viewpoint of improving the thermal stability of the polyacetal resin when kneading the sinterable inorganic powder and the organic binder.
[0059] The fatty acid metal salt is not particularly limited, but examples thereof include fatty acid metal salts obtained from a saturated or unsaturated fatty acid having 10 to 35 carbon atoms or a fatty acid substituted with a hydroxyl group and an alkali metal or alkaline earth metal hydroxide, oxide, or chloride.
[0060] Examples of the fatty acid of the fatty acid metal salt include capric acid, undecylic acid, lauric acid, tridecylic acid, myristic acid, pentadecylic acid, palmitic acid, heptadecylic acid, stearic acid, nonadecanoic acid, arachic acid, behenic acid, liglyceric acid, cerotic acid, heptacosanoic acid, montanic acid, undecylenic acid, oleic acid, elaidic acid, cetoleic acid, erucic acid, brassidic acid, sorbic acid, linoleic acid, linolenic acid, arachidonic acid, propiolic acid, stearic acid, 12-hydroxydodecanoic acid, 3-hydroxydecanoic acid, 16-hydroxyhexadecanoic acid, 10-hydroxyhexadecanoic acid, 12-hydroxyoctadecanoic acid, and 10-hydroxy-8-octadecanoic acid. The metal compound is a hydroxide or chloride of an alkali metal such as lithium, sodium, or potassium, an alkaline earth metal such as magnesium, calcium, strontium, or barium, or zinc or aluminum. Of these, the fatty acid is preferably myristic acid, palmitic acid, or stearic acid, and the metal compound is preferably a hydroxide, oxide, or chloride of calcium, and more preferably calcium myristate, calcium palmitate, or calcium stearate.
[0061] When the nitrogen-containing compound and the fatty acid metal salt are added to the composition for sintered body, the ratio of the mass of the fatty acid metal salt to the mass of the nitrogen-containing compound (mass of fatty acid metal salt / mass of nitrogen-containing compound) is preferably within a specific range, specifically, the ratio is 1 to 15, preferably 1 to 10. By setting the ratio to 1 to 15, it is preferable in that the thermal stability of the polyacetal resin in the organic binder can be improved.
[0062] The mass proportion of the organic binder in the composition for sintered bodies is preferably 5 to 30 parts by mass, more preferably 5 to 20 parts by mass, and even more preferably 5 to 15 parts by mass, per 100 parts by mass of the composition for sintered bodies, from the viewpoint of maintaining good moldability in injection molding and further suppressing cracks and swelling during the degreasing process.
[0063] The resin components contained in the organic binder are preferably only the polyacetal resin, the polyolefin resin, the fluidity imparting agent, and the nitrogen-containing compound (for example, polyamide resin), but may contain other additives.
[0064] (Other additives) Additives other than the above-mentioned components that can be added to the composition for sintered body are not limited as long as they do not impair the effects of the present invention. Preferred additives include antioxidants.
[0065] Examples of the antioxidant include n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, n-octadecyl-3-(3'-methyl-5'-t-butyl-4'-hydroxyphenyl)propionate, n-tetradecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, 1,6-hexanediol-bis-(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate), 1,4-butanediol-bis-(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate), 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, triethylene glycol-bis-(3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate), tetradecyl-3-(3',5'-di-t-butyl-4-hydroxyphenyl)propionate, ... Examples of the hydroxyphenyl ether include trachys(methylene 3-(3'-t-butyl-4-hydroxyphenyl)propionate)methane, N,N'-bis-(3-(3,5-di-t-butyl-4-hydroxyphenol)propionyl)hydrazine, N,N'-tetramethylene-bis-3-(3'-methyl-5'-t-butyl-4-hydroxyphenol)propionyldiamine, N,N'-bis-3-(3',5'-di-t-butyl-4-hydroxyphenol)propionylhexamethylenediamine, 3-(N-salicyloyl)amino-1,2,4-triazole, N,N'-bis-(2-(3-(3,5-dibutyl-4-hydroxyphenyl)propionyloxy)ethyl)oxyamide, and N,N'-hexamethylene-bis-(3-3,5-t-butyl-4-hydroxyphenyl)propanamide). These antioxidants may be used alone or in combination of two or more.
[0066] The content of the antioxidant is 0.01 to 1.0 part by mass, and preferably 0.05 to 0.5 part by mass, based on 100 parts by mass of the polyacetal resin. When the content is within the above range, the thermal stability is improved.
[0067] The melt flow rate of the composition for sintered body is preferably 80 g / 10 min or more and less than 200 g / 10 min, more preferably 90 g / 10 min or more and less than 180 g / 10 min, and even more preferably 90 g / 10 min or more and less than 140 g / 10 min, as measured in accordance with ASTM-D-1238-57T under conditions of 190 ° C. and 2.16 kg. By making the melt flow rate 80 g / 10 min or more, the fluidity of the composition for sintered body is improved, and by making the melt flow rate less than 200 g / 10 min, the strength of the green molded body can be improved. The melt flow rate of the composition for sintered body can be controlled within the above range, for example, by the type and mass proportion of the polyacetal resin used. The melt flow rate of the composition for sintered body tends to increase as the melt flow rate of the polyacetal resin increases.
[0068] (Method of producing a composition for sintered body) The composition for sintered bodies can be produced by a known method without any particular limitation. Specifically, the composition for sintered bodies can be produced by mixing the above-mentioned sinterable inorganic powder and organic binder with, for example, a Henschel mixer, a tumbler, a V-shaped blender, etc., and then melt-kneading the mixture in a semi-molten state with a kneader such as a single-screw extruder, a twin-screw extruder, a heating roll, a kneader, or a Banbury mixer, and can be obtained as a product in various forms such as a strand shape or a pellet shape.
[0069] [Method of manufacturing molded body] The method for producing a molded body according to the present invention is a method for producing a molded body containing a sinterable inorganic powder and an organic binder, and includes a kneading step of kneading the sinterable inorganic powder with the organic binder to obtain a kneaded mixture, and a molding step of molding the kneaded mixture to obtain a molded body. The kneading step and the molding step can be performed under desired conditions.
[0070] When kneading, it is preferable to use a kneader such as a pressure kneader, and the kneading temperature is preferably 160°C to 200°C, more preferably 160°C to 190°C, and even more preferably 160°C to 180°C. By setting the kneading temperature at 160°C or higher, kneading is performed near the melting temperature of the resin, and the dispersibility of the resin can be improved, and the bending modulus of the green molded body can be improved. In addition, by setting the kneading temperature at 200°C or lower, resin decomposition during kneading can be suppressed, and the number of voids in the cross section of the green molded body can be suppressed. In addition, even if the composition is the same, by setting the kneading temperature in the above-mentioned preferred range, the decrease in bending modulus and yield strength can be suppressed.
[0071] In injection molding, the cylinder temperature is preferably 150°C to 190°C, more preferably 160°C to 190°C, and even more preferably 165°C to 185°C. By setting the cylinder temperature at 150°C or higher, the fluidity of the resin is increased to improve moldability, and the density and strength of the green molded body can be increased, while by setting the cylinder temperature at 190°C or lower, separation of the resin during injection molding can be suppressed, and the strength of the green molded body can be increased. In addition, even if the composition is the same, by setting the kneading temperature within the above-mentioned preferred range, the decrease in the flexural modulus and yield strength can be suppressed.
[0072] The injection pressure during injection molding is preferably 50 MPa or more. By increasing the injection pressure, the voids in the resulting molded body are reduced and the adhesion between the organic binder and the metal powder is improved, so that the resin packing density is improved and a molded body with high strength can be obtained. The injection pressure is more preferably 60 MPa or more, and even more preferably 70 MPa or more. There is no particular upper limit to the injection pressure, but the injection pressure at which the molding device can be safely operated is a practical upper limit. Specifically, it is about 200 MPa. In order to increase the strength of the molded body, it is important that the injection pressure exceeds a certain value, but it is not important to make the injection pressure higher than necessary. If the strength of the obtained molded body is the same, a lower injection pressure is preferable from the standpoint of safety.
[0073] In this way, a molded article having a flexural modulus (MPa) of 4000 to 15000 at a strain of 0.05% to 0.1% and a flexural yield strength (MPa) of 10 or more can be produced.
[0074] The green body has a flexural modulus (MPa) at a strain of 0.05% to 0.1% in the range of preferably 4000 to 15000, more preferably 4000 to 12000, and particularly preferably 7000 to 12000. When the flexural modulus is within the above range, it is possible to prevent plastic deformation during transportation and to suppress damage due to impact such as dropping.
[0075] The bending strength (MPa) of the green compact is preferably 10 or more, more preferably 10 to 100, and particularly preferably 10 to 40. When the bending strength is within the above range, it is possible to obtain a compact having high strength that can withstand loads such as ejection by an ejector.
[0076] Furthermore, it is preferable that the sinterable inorganic powder is contained in an amount of 75% by mass or more and 95% by mass or less relative to 100% by mass of the molded body. If the content of the sinterable inorganic powder is 75% by mass or more, separation during injection molding can be prevented, and the strength of the molded body can be increased. Furthermore, if the content of the sinterable inorganic powder is 95% by mass or less, the molded body can be prevented from becoming brittle. It is more preferable that the sinterable inorganic powder is contained in an amount of 90% by mass or more and 95% by mass or less.
[0077] [Method of manufacturing sintered body] The method for producing a sintered body according to the present invention includes a debinding step of removing an organic binder from the above-mentioned molded body according to the present invention or a molded body produced by the method for producing a molded body according to the present invention by heating or chemical treatment to obtain a sintered precursor, and a sintering step of sintering the sintered precursor to obtain a sintered body. The debinding step and the sintering step can be performed under desired conditions. In the case of a method of degreasing by heating, degreasing is performed by increasing the temperature from room temperature to 500° C. to 600° C. in a nitrogen atmosphere. A fluidity imparting agent may be dissolved in a solvent before heating. Then, the temperature is raised to the sintering temperature of the sinterable inorganic powder, thereby obtaining a sintered body. In the case of a method of degreasing using an acid, nitric acid gas is circulated in a nitrogen atmosphere and the temperature is raised from room temperature to 110°C to 120°C to perform degreasing. Then, the temperature is raised to the sintering temperature of the sinterable inorganic powder, thereby obtaining a sintered body. EXAMPLES
[0078] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples. The terms and measurement methods for properties in the examples and comparative examples are as follows.
[0079] [Raw materials] (A Polyacetal resin) (A-1) A jacketed twin-shaft paddle-type continuous polymerization reactor (Kurimoto Iron Works, Ltd., diameter 2B, L / D=14.8) capable of passing a heat transfer medium was adjusted to a temperature of 80° C. Polymerization was carried out by continuously supplying to the polymerization reactor 69 g / hr of a catalyst preparation prepared by diluting boron trifluoride-di-n-butyl etherate to 0.26 mass % with cyclohexane as a polymerization catalyst, 3500 g / hr of trioxane, 121 g / hr of 1,3-dioxolane, and 7.9 g / hr of methylal as a molecular weight regulator. The material discharged from the polymerization reactor was put into a 0.5% by mass aqueous solution of triethylamine to deactivate the polymerization catalyst, and then filtered, washed, and dried. Next, the mixture was fed to a vented twin-screw extruder (L / D=40) set at 200°C, and a 0.8% by mass aqueous solution of triethylamine was added to the terminal stabilization zone to give a nitrogen content of 20 ppm, and the mixture was stabilized while being degassed under reduced pressure at 90 kPa, and pelletized with a pelletizer. The mixture was then dried at 100°C for 2 hours to obtain polyacetal resin (A-1). The resulting polyacetal resin (A-1) had a melting point of 164° C. and a melt flow rate of 90 g / 10 min. Details of the resulting polyacetal resin (A-1) are shown in Table 1.
[0080] [Table 1]
[0081] (A-2) A polyacetal resin (A-2) was produced in the same manner as the polyacetal resin (A-1), except that the flow rate of methylal as a molecular weight regulator was 9.4 g / hr. The resulting polyacetal resin (A-2) had a melting point of 164°C and a melt flow rate of 121 g / 10 min. Details of the resulting polyacetal resin (A-2) are shown in Table 1.
[0082] (A-3) Except for the flow rate of methylal as a molecular weight regulator being 10.6 g / hr, polyacetal resin (A-3) was produced in the same manner as polyacetal resin (A-1). The resulting polyacetal resin (A-3) had a melting point of 164°C and a melt flow rate of 180 g / 10 min. Details of the resulting polyacetal resin (A-3) are shown in Table 1.
[0083] (B Polyolefin resin) Polypropylene (Sumitomo Noblen UH501E1, manufactured by Sumitomo Chemical Co., Ltd.)
[0084] (C nitrogen-containing compounds) Nylon 66 (molecular weight 10,000)
[0085] (D Fatty acid metal salt) Calcium stearate
[0086] (E Fluidity imparting agent) Paraffin wax (Nippon Seiro Co., Ltd. Paraffin wax-14
[0087] [Preparation of composition for molding] 0.05 parts by mass of (C) nylon 66 and 0.3 parts by mass of (D) calcium stearate were uniformly added and mixed with 100 parts by mass of any one of the polyacetal resins (A-1) to (A-3), and the mixture was fed to a vented twin-screw extruder (L / D=40) set at 200°C, and pelletized while degassing under reduced pressure at 90 kPa. The mixture was then dried at 100°C for 2 hours to prepare a polyacetal resin composition (A).
[0088] The binder components were taken as 100 mass % and the binder was mixed with 25 mass % of the polyacetal resin composition (A), 25 mass % of the polyolefin resin composition (B), and 50 mass % of the fluidity imparting agent (E). The binder and SUS316L as a sinterable inorganic powder were mixed in the ratios shown in Table 1 to prepare compositions for molding used in producing the molded bodies of Comparative Examples 1 to 5 and Examples 1 to 8. In addition, except for Example 6, the SUS316L metal powder was adjusted to a maximum particle size of 30 μm using a 30 μm mesh sieve. The maximum particle size before sieving was 40 μm. Details of the composition for compact (compact) are shown in Table 2.
[0089] [Table 2]
[0090] [evaluation] (Melt Flow Rate (MI)) The MI (melt flow rate: g / 10 min) was measured under conditions of 190° C. and 2160 g using a MELT INDEXER manufactured by Toyo Seiki Co., Ltd. in accordance with ASTM-D-1238.
[0091] (Preparation of Molded Test Pieces) The prepared composition for molding was kneaded at 170 ° C. for 1 hour using a pressure kneader, and then the kneaded product was cooled and crushed to obtain a raw material for injection molding. Using an injection molding machine (ROBOSHOT α-50iA manufactured by Fanuc Corporation), the molding temperature was 170 ° C. and the injection pressure was 80 MPa, and a flat plate with a length of 60 mm, a width of 60 mm, and a thickness of 1 mm or 2 mm was molded. At that time, it was confirmed whether the composition in the mold was filled to the end. Those filled to the end were marked with ○, and those not were marked with ×. The evaluation results are shown in Table 2. From the obtained flat plate, a rectangular molded body test piece conforming to JIS K 7139 was cut out to obtain it. In addition, even for those evaluated as × in the above evaluation, molded test specimens were cut out from the flat portion filled in the mold in order to evaluate the bending yield strength and bending modulus of the molded test specimens described below. Moreover, the test pieces can be obtained not only by cutting out the flat plate but also by cutting out any molded body.
[0092] (Flexural yield strength of molded test piece) The bending yield strength of the molded product was evaluated by a three-point bending test. That is, the above-mentioned rectangular molded product test piece was measured for bending yield strength and bending modulus when the support jig was set at an interval of 50 mm on an autograph (Instron Dual column flore model 5581) and the load cell was lowered at a speed of 2 mm / min. The product of the measured bending yield strength (MPa) and bending modulus (MPa) was calculated. The measured bending yield strength, bending modulus, and calculated product values are shown in Table 2.
[0093] (Microscopic Observation) The cross section of a rectangular test piece cut from the molded plate was observed. 2 The number of voids of 30 μm or more per unit area was evaluated. Specifically, the entire cross section was observed using a Keyence digital microscope (VHX-7000) and the diameter of each void was measured. 2 The area was observed and the number of voids was counted. Areas with 10 or less voids were rated as ◯, and others were rated as ×. The evaluation results are shown in Table 2.
[0094] (Transportation test 1: Push-out test) In the above moldability evaluation, the mold in which the composition for molding had been filled up to the end of the mold was injection molded again under the same conditions, and a test was performed to see whether cracks occurred when ejected with an ejector. Specifically, the ejector thrust speed was changed to 10mm / s, 20mm / s, 30mm / s, 40mm / s, and 50mm / s, and the speed at which damage was observed in the test specimen was recorded. In addition, specimens without cracks at a thrust speed of 50mm / s were marked as having very high strength, and were marked as ◯. The speeds at which damage was observed in the test specimens are shown in Table 2.
[0095] (Transportation test 2: Drop test) In the above moldability evaluation, a mold in which the composition for a molded body had been filled up to the end of the mold was injection molded again under the same conditions, and the obtained flat plate was dropped to test whether deformation or cracking occurred. Specifically, 10 flat plates were dropped from a height of 1m and the number of deformed or cracked plates were counted. Deformation was determined by placing the flat plates on a flat metal plate and counting plates that were confirmed to be warped. Cracks were also determined by thoroughly examining the appearance and those with chipped or cracked parts were counted as cracked. The number of plates with deformation or cracks was counted and recorded. The number of plates with deformation or cracks is shown in Table 2.
[0096] <Evaluation results of transportation test 1> In the ejection test, the test pieces of the comparative examples cracked at a relatively low ejection speed, whereas the test pieces of the examples cracked at a higher ejection speed than the comparative examples. In particular, in the test pieces of Examples 2, 3, 7 and 8, no cracks occurred even at an ejection speed of 50 mm / s, and they had high strength. This result shows that the molded body according to the present invention has higher durability against breakage during transportation.
[0097] <Evaluation results of transportation test 2> In the drop test, most of the plates of the comparative examples, particularly those of Comparative Example 1 and Comparative Example 3, were deformed or cracked. In contrast, most of the plates of the examples, particularly those of Examples 1 to 5, 7 and 8, were not deformed or cracked. This result indicates that the molded product according to the present invention has higher durability against breakage during transportation.
[0098] The molded bodies of Examples 1 to 8 had an appropriate balance of organic binder, metal powder, kneading conditions, and molding conditions, and the molded bodies had a flexural modulus (MPa) of 4000 to 15000 and a flexural yield strength (MPa) of 10 or more at a strain of 0.05% to 0.1%, and all of them showed excellent results in the transportation test. On the other hand, the molded bodies of Comparative Examples 1 to 5, in which the balance of the metal powder blend amount, kneading conditions, and molding conditions was changed, had a decreased flexural modulus and flexural yield strength, and were inferior to the Examples in thin-wall formability and results of the transportation test.
Claims
1. A molded body comprising a sinterable inorganic powder and an organic binder, the organic binder contains a polyacetal resin and a polyolefin resin, a mass ratio of the polyacetal resin in the organic binder is 5 to 95% by mass with respect to 100% by mass of the organic binder; The mass ratio of the polyolefin resin in the organic binder is 5 to 95% by mass with respect to 100% by mass of the organic binder, The flexural modulus (MPa) of the molded body at a strain of 0.05% to 0.1% is 4,000 to 15,000; The bending yield strength (MPa) is 10 or more. Molded body.
2. The molded body according to claim 1, wherein the product of the flexural modulus (MPa) and the flexural yield strength (MPa) is 50,000 or more.
3. When observing the cross section under a microscope, 2 3. The molded article according to claim 1, having 10 or less voids of 30 μm or more per unit area.
4. The molded body according to any one of claims 1 to 3, wherein the maximum particle size of the sinterable inorganic powder is 30 µm or less.
5. The molded article according to claim 1, wherein the polyacetal resin has a melt flow rate of 70 to 200 g / 10 min.
6. The molded body according to any one of claims 1 to 5, comprising 75% by mass or more and 95% by mass or less of the sinterable inorganic powder relative to 100% by mass of the molded body.
7. The molded body according to any one of claims 1 to 6, wherein the sinterable inorganic powder is a metal powder.
8. The part with a thickness of 1 mm or less is 100 mm 2 The molded body according to any one of claims 1 to 7, wherein the above-mentioned components are present.
9. A method for producing a molded body comprising a sinterable inorganic powder and an organic binder, comprising the steps of: A kneading step of kneading a sinterable inorganic powder with an organic binder to obtain a kneaded mixture; a molding step of molding the kneaded mixture to obtain a molded body; Including, the organic binder contains a polyacetal resin and a polyolefin resin, a mass ratio of the polyacetal resin in the organic binder is 5 to 95% by mass with respect to 100% by mass of the organic binder; The mass ratio of the polyolefin resin in the organic binder is 5 to 95% by mass with respect to 100% by mass of the organic binder, The flexural modulus (MPa) of the molded body at a strain of 0.05% to 0.1% is 4,000 to 15,000; A method for producing a molded product, characterized in that the molded product has a bending yield strength (MPa) of 10 or more.
10. The method for producing a molded body according to claim 9, wherein the kneading temperature in the kneading step is 160°C to 200°C.
11. The method for producing a molded body according to claim 9 or 10, wherein a cylinder temperature in the molding step is 150°C to 190°C.
12. The method for producing a molded body according to any one of claims 9 to 11, wherein the injection pressure in the molding step is 50 MPa or more.
13. The method for producing a molded body according to any one of claims 9 to 12, wherein the sinterable inorganic powder is contained in an amount of 75% by mass or more and 95% by mass or less relative to 100% by mass of the molded body.
14. A degreasing step of removing the organic binder from the molded body according to any one of claims 1 to 8 or the molded body produced by the method for producing a molded body according to any one of claims 9 to 13 by heating or chemical treatment to obtain a sintered precursor; a sintering step of sintering the sintering precursor to obtain a sintered body; A method for producing a sintered body, comprising:
Citation Information
Patent Citations
Method for degreasing sinterable powder compact
JP1994192706A
Production of sintered compact
JP1996020803A
Composition for manufacturing sintered molding
JP2001106581A
Powder injection-molding composition and its sintered body
JP2005205805A
Composition for fiber reinforced resin bond type magnet, and resin bond type magnet using the same