Concrete Composition
The concrete composition, using specific admixtures without setting retarding or reducing performance, addresses the instability of fluidity and strength in existing compositions, ensuring stable fluidity, freshness retention, and high strength development.
Patent Information
- Application Number
- JP2021021897
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-15
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2041-02-15
AI Technical Summary
Existing concrete compositions struggle to stably combine initial fluidity, fluidity retention, and strength development, with dispersants exhibiting excessive or insufficient setting retardation, affecting concrete strength and workability.
A concrete composition incorporating a water reducing agent without setting retarding performance, a setting retarding agent without water reducing performance, and a thickener, along with a nonionic surfactant, to maintain fluidity, freshness retention, and underwater inseparability, while ensuring appropriate strength development.
The composition achieves stable fluidity during pouring, retains freshness, exhibits excellent underwater inseparability, and develops high strength after hardening, improving workability and construction efficiency.
Abstract
Description
[Technical field]
[0001] The present invention relates to a concrete composition. [Background technology]
[0002] When constructing concrete structures such as tunnels, various properties such as fluidity, freshness retention, and underwater segregation resistance during concrete pouring may be required in addition to the strength of the concrete, depending on external factors such as water pressure from the ground at the planned construction site of the structure and the construction method adopted. An example of a concrete structure requiring such properties is lining concrete poured on-site in shield tunnel construction below the groundwater level.
[0003] Patent Document 1 discloses a concrete composition that contains cement, aggregate, water, and at least two types of dispersants for the purpose of maintaining and adjusting fresh properties, and in which the initial slump flow value and the time to reach 50 cm have a predetermined relationship. According to this document, it is possible to adjust the initial fluidity and fluidity retention by using an agent classified as a delayed type and an agent classified as a standard type as dispersants. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-23148 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the dispersants used in the technology described in Patent Document 1 all have both initial fluidity and set retardation as fluidity retention (specified in JIS A6204), and they tend to have excessive or insufficient initial fluidity or set retardation, adversely affect strength development, and make it extremely difficult to adjust these physical properties. In addition, the above-mentioned dispersants adsorb to cement particles and act to repel the particles, and the excess water trapped by cement aggregation is released, and this water reacts with the thickener, which tends to affect viscosity. In this way, the technology described in Patent Document 1 was unable to stably combine the strength of concrete with various performance properties such as fluidity when pouring the concrete, freshness retention, and anti-segregation underwater.
[0006] Therefore, an object of the present invention is to stably provide a concrete composition which has good fluidity, freshness retention, and anti-segregation properties when poured, and which can exhibit excellent strength after hardening. [Means for solving the problem]
[0007] The present invention includes water, cement, aggregates and admixtures, The concrete composition includes, as the admixtures, a water-reducing agent or a superplasticizer having no set-retarding performance, a set retarder having no water-reducing performance, and a viscosity enhancer. Effect of the Invention
[0008] According to the present invention, there is provided a concrete composition which has excellent fluidity, freshness retention and anti-segregation properties when poured, and which can stably exhibit excellent strength after hardening. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described below based on preferred embodiments. The concrete composition of the present invention contains water, cement, aggregate and admixture. In the following description, unless otherwise specified, the concrete composition in this specification includes both mortar containing only fine aggregate as an aggregate and concrete containing both fine and coarse aggregate. Depending on the context, the concrete composition may refer to a fluid before hardening (so-called fresh concrete) or a hardened product after hardening (so-called hardened concrete).
[0010] The water used can be any water commonly used in the present technical field, such as tap water, well water, distilled water, purified water, etc., without any particular limitations.
[0011] The cement may be any of various types of Portland cement, such as ordinary Portland cement, high-early-strength Portland cement, and moderate-heat Portland cement; mixed cements, such as blast-furnace cement, silica cement, and fly ash cement; and special cements, such as ecocement and alumina cement. These may be used alone or in combination. As these cements, for example, cements specified in JIS R5210 to R5214 may be used.
[0012] The aggregate may be fine aggregate or coarse aggregate. Depending on the properties of the desired composition, the aggregate may be in the form of mortar using only fine aggregate or in the form of concrete using both fine and coarse aggregate.
[0013] Examples of fine aggregates include natural aggregates such as river sand, mountain sand, and sea sand, artificial aggregates such as crushed stone, crushed sand, and fine blast furnace slag aggregate, and recycled aggregates extracted from concrete waste. These can be used alone or in combination. Examples of the coarse aggregate include river gravel, sea gravel, mountain gravel, crushed stone, slag crushed stone, etc. These can be used alone or in combination. Coarse aggregates specified in JIS A 5005 can also be used.
[0014] One of the features of the concrete composition of the present invention is that it contains, as an admixture, which is a type of admixture, a water-reducing agent or a superplasticizer that does not have set retardation performance, and a set retarder that does not have water-reducing performance. Examples of water-reducing agents or fluidizing agents include those specified in JIS A6204, which are intended to increase the fluidity of a concrete composition by increasing the water dispersibility of cement particles in the concrete composition. The setting retarder is intended to delay the hardening of a concrete composition. However, the present inventor's study has revealed that some water-reducing agents or fluidizing agents have a setting retardation performance in addition to the main performance of fluidity improvement performance, depending on the type. Similarly, the present inventor's study has revealed that some types of setting retarders have a fluidity improvement performance such as water reduction performance in addition to the main performance of setting retardation performance. Due to this, depending on the mixing ratio of the fluidity improvement performance and the setting retarder and the combination of their types, the intended fluidity improvement performance and retardation performance are excessively expressed. As a result, the various physical properties required during construction, such as the handleability of the concrete composition, filling ability, and retention in the pipe, are deteriorated, and the strength of the concrete after hardening is adversely affected.
[0015] The present inventors have conducted extensive research into how to improve these points, and have found that by selecting and using a water-reducing agent or a superplasticizer that does not have set-retarding properties, and by selecting and using a set-retarder that does not have water-reducing properties, it is possible to develop a suitable fluidity in the concrete composition while maintaining the fresh properties of the composition for a suitable period of time, and to develop good strength after hardening. In other words, the present invention allows the water-reducing agent or superplasticizer itself to develop fluidity-improving properties, and allows the set-retarder itself to develop set-retarding properties, thereby making it possible to easily adjust the desired physical properties of the concrete composition and to effectively develop said properties.
[0016] As described above, the concrete composition contains a water-reducing agent or a superplasticizer that does not have a set retarding property. Note that the water-reducing agent or the superplasticizer in the present invention is excluded from the set retarders described above. In this specification, "not having set retardation performance" includes both not having any set retardation performance in the strict sense and the set retardation performance exhibited by the water reducing agent or superplasticizer being negligibly small compared to the set retardation performance exhibited by the set retarder. In the above-mentioned water reducing agent or superplasticizer, the set acceleration performance is not prevented from being exhibited, but from the viewpoint of appropriately controlling the setting property by the set retarder, it is preferable that it does not have the set acceleration performance.
[0017] Specifically, "not having retardation properties" means that the difference in the initial setting time measured according to JIS A6204 is +90 minutes or less, preferably less than +60 minutes, more preferably +30 minutes or less, even more preferably 0 minutes or less, and preferably -60 minutes or more, more preferably -30 minutes or more, even more preferably 0 minutes or more. In JIS A6204, retardation of setting time is indicated by the sign "+", and acceleration of setting time is indicated by the sign "-". By using a water-reducing agent or a fluidizing agent having such a setting time, the fluidity of the concrete composition can be appropriately expressed, and the composition can be filled without gaps within the formwork or between the ground and the formwork, thereby improving workability.
[0018] As the water reducing agent or superplasticizer without setting retardation performance, one or more of the superplasticizers, water reducing agents, AE water reducing agents, superplasticizers, and superplasticizers specified in JIS A6204, other than the retardation type, can be used. Of these, it is preferable to use a superplasticizer, a superplasticizer standard type, or a superplasticizer standard type as the water reducing agent or superplasticizer, and it is more preferable to use a superplasticizer. By using such a water reducing agent or superplasticizer, the concrete composition can be made to have an appropriate fluidity, and the composition can be easily filled without gaps in the formwork or between the ground and the formwork. As a result, concrete with high density and strength after hardening can be efficiently obtained. In addition, since the above-mentioned condition of not having the setting retardation performance can be easily achieved without using other raw materials, it is also advantageous in that the costs required for production and construction can be reduced.
[0019] As described above, the concrete composition contains a set retarder that does not have water-reducing properties. Note that the set retarder is excluded from the above-mentioned water-reducing agent or superplasticizer. In this specification, "having no water-reducing performance" includes both having absolutely no water-reducing performance in the strict sense and the water-reducing performance exhibited by the setting retarder being negligibly small compared to the water-reducing performance exhibited by the above-mentioned water-reducing agent or superplasticizer. Specifically, "not having set retardation performance" means that the water reduction rate measured according to JIS A6204 is less than 4%, preferably 2% or less, and realistically 0% or more. By using a set retarder having such a water reduction rate, the concrete composition can be pumped to the intended casting site while maintaining the fresh properties of the concrete composition in the delivery pipe for a predetermined time by maintaining the fresh properties of the concrete composition in the delivery pipe. As a result, the handling and workability of the concrete composition are improved.
[0020] Examples of the setting retarder include, provided that they do not have water reducing properties, organic setting retarders such as saccharides such as sucrose and raffinose, oxycarboxylic acids such as gluconic acid, citric acid, tartaric acid, and malic acid and their salts, lignin sulfonic acid and their salts, and inorganic setting retarders such as silicon fluorides. These can be used alone or in combination. Of these, from the viewpoint of further exerting the setting retardation effect, it is preferable to use a setting retarder containing oxycarboxylic acid and its salt as the main component. In addition, it is preferable that the setting retarder in this specification excludes retarders classified as "delayed type" as defined in JIS A6204.
[0021] The concrete composition further contains a thickener as an admixture, which is a type of admixture. Note that the thickener is excluded from the above-mentioned setting retarder, water reducing agent, and superplasticizer. By containing the thickener, the concrete composition can exhibit appropriate fluidity and appropriate viscosity. As a result, excellent underwater non-separation properties can be exhibited even under conditions of water pressure and water flow.
[0022] The thickener in the present invention is capable of exhibiting non-separation properties in water, and is classified as a so-called non-separation admixture in water. Examples of such thickeners include cellulose-based thickeners, biopolymer-based thickeners, acrylic-based thickeners, and special thickeners. These can be used alone or in combination. Among these, from the viewpoint of further improving the pumpability and fluidity of the final concrete composition, it is preferable to use a special thickener containing an alkylarylsulfonate and an alkylammonium salt as main components as the thickener.
[0023] The water-cement ratio in the concrete composition (percentage of the mass of water relative to the mass of cement) is preferably 30-60%, more preferably 30-45%. With such a water-cement ratio, even when the concrete composition contains the above-mentioned various admixtures, the concrete composition effectively exhibits the fluidity, freshness retention, and non-separation in water, and has excellent strength after hardening. In addition, the concrete composition can be demolded earlier, so that the construction speed can be increased and the construction period can be shortened. Furthermore, the concrete composition can easily and efficiently exhibit a compressive strength measured in accordance with JIS A1107 that is equal to or higher than the required level. The above-mentioned water-cement ratio is preferably determined by determining the correlation between the reciprocal of the water-cement ratio, i.e., the cement-water ratio, and the strength developed at a specified time in a preliminary test, and also by taking into account a safety factor, in order to develop excellent strength after hardening at an appropriate casting location.
[0024] The content of the water reducing agent or fluidizing agent in the concrete composition is preferably 1.4 to 3.3 mass%, more preferably 1.7 to 3.0 mass%, expressed as a mass ratio relative to the cement. When two or more water reducing agents or fluidizing agents are contained, the total amount may be within the above-mentioned range. By setting the content of the water reducing agent or fluidizing agent within such a range, even when the concrete composition contains the above-mentioned various admixtures, excellent fluidity can be imparted to the concrete composition, and the handling property, filling property at the casting site, and workability are further improved.
[0025] The content of the set retarder in the concrete composition is preferably 0.3 to 1.7 mass%, more preferably 0.5 to 1.5 mass%, expressed as a mass ratio relative to the cement. When two or more types of set retarders are contained, the total amount may be within the above-mentioned range. By setting the content of the set retarder within such a range, even when the concrete composition contains the above-mentioned various admixtures, unintended setting does not occur during pumping of the concrete composition, and the concrete composition can be pumped while maintaining the retention and freshness in the delivery pipe in an appropriate state, thereby further improving the handling and workability of the concrete composition.
[0026] The content of the thickener in the concrete composition is preferably 3.5 to 5.5 mass %, more preferably 4.0 to 5.0 mass %, expressed as a mass ratio to water. When two or more types of thickeners are contained, the total amount may be within the above-mentioned range. By setting the content of the thickener within this range, even when the above-mentioned various admixtures are contained, excellent underwater non-separation properties can be more effectively exhibited under water pressure conditions and under water conditions.
[0027] The concrete composition preferably further contains a nonionic surfactant. The nonionic surfactant mainly functions to control the viscosity of the concrete composition as a viscosity adjuster that adjusts the thickening effect of the thickener to a moderate degree. By containing a nonionic surfactant, it is possible to moderately alleviate the viscosity change caused by the thickener, and to improve the handleability and workability of the concrete while allowing the concrete to exhibit non-separation properties in water. Note that the nonionic surfactant in this specification is excluded from the above-mentioned water reducing agent, superplasticizer, setting retarder, and thickener.
[0028] Examples of nonionic surfactants include alkyl ethers such as polyethylene oxide alkyl ethers (polyoxyethylene alkyl ethers), polyoxypropylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, and polyoxypropylene alkyl phenyl ethers; polyhydric alcohol ethers such as alkyl glycosides; fatty acid esters such as glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxypropylene fatty acid esters, sucrose fatty acid esters, and sorbitan fatty acid esters; and amides such as fatty acid alkanolamides. These can be used alone or in combination of two or more.
[0029] Among these nonionic surfactants, it is preferable to use at least one of alkyl ethers and fatty acid esters, and it is more preferable to use at least one of polyethylene oxide alkyl ethers and fatty acid esters. By using such a nonionic surfactant, the agent has high stability, and the viscosity change caused by the thickener is moderately mitigated, so that the concrete exhibits anti-separation properties underwater while obtaining good fluidity and fresh retention of the concrete.
[0030] The mass ratio of the nonionic surfactant to the thickener is preferably 0.5 to 4.5 mass%, more preferably 1.0 to 4.0 mass%, and further preferably 2.0 to 3.5 mass%. By blending the nonionic surfactant in such a ratio, the viscosity change caused by the thickener can be appropriately mitigated, and the concrete can be made to exhibit anti-separation properties in water while further improving the handleability and workability of the concrete.
[0031] The concrete composition in the above-mentioned embodiment can be prepared by a known mixing method, such as adding water, cement, aggregate, and admixtures in any order or simultaneously and kneading them. As long as the effects of the present invention are achieved, other admixtures than the above-mentioned cement, water, aggregate, and admixtures may be further added as necessary. Examples of other admixtures include siliceous admixtures, gypsum, calcium carbonate, limestone, etc., as specified in JIS R5212.
[0032] The concrete composition thus obtained has a strength index of preferably 15 N / mm2 or less in uniaxial compressive strength 24 hours after mixing, measured in accordance with JIS A1107. 2 More preferably, 20N / mm 2 More preferably, 25N / mm 2 That's all. The higher the unconfined compressive strength, the higher the strength of the concrete after hardening. Such strength can be easily achieved, for example, by setting the water-cement ratio within the above-mentioned preferred range. In addition, it can also be achieved by setting the type and content of each mixed material within the above-mentioned range.
[0033] The concrete composition preferably has a slump flow value within the range of 650±50 mm as an index of its fluidity, measured according to JIS A1150. A slump flow value within such a range means that the concrete composition has excellent fluidity. Such a slump flow value can be easily achieved, for example, by setting the water-cement ratio within the above-mentioned preferred range, or by setting the type and content of each admixture, such as a water-reducing agent or a fluidizing agent, within the above-mentioned range.
[0034] As an index of freshness retention, the concrete composition has a 500 mm flow time measured in accordance with JSCE-F516 4 hours after mixing, which is preferably within 180 seconds. The shorter the flow time, the longer the freshness is maintained, and the better the pumpability and workability. Such a flow time can be easily achieved, for example, by setting the water-cement ratio within the above-mentioned preferred range, or by setting the type and content of each mixed material, such as the setting retarder, within the above-mentioned range.
[0035] The concrete composition preferably has a pH of 12 or less as an index of its underwater non-separation property measured according to JSCE-D104 (Appendix 2). This index is an indirect index of the amount of suspended solids dispersed in fresh water, considering that cement milk is strongly alkaline. Therefore, if the above-mentioned pH is less than a predetermined value, it means that even if the casting site is under severe conditions such as under water pressure or under water, the concrete composition has resistance to these conditions and can exhibit strength after hardening. Such a pH can be easily achieved, for example, by setting the water-cement ratio to the above-mentioned suitable range, or by setting the type and content of each mixed material such as a thickener to the above-mentioned range. It goes without saying that the above-mentioned pH will not fall below the neutral range of fresh water, and is generally 10 or more.
[0036] The above concrete composition has good fluidity, freshness retention, and underwater non-segregation properties when poured, and can stably exhibit excellent strength after hardening. According to a preferred embodiment of the present invention, even if a construction method different from a normal pouring method is adopted, or the construction site is under water conditions such as under water pressure or under water flow, or under harsh environmental conditions compared to normal construction sites such as high or low temperatures during mixing or curing, the concrete composition is less susceptible to the influence of these external factors by using a combination of admixtures that are easy to adjust in proportion, and can quickly and effectively exhibit excellent strength after hardening while maintaining the desired properties of fluidity, freshness retention, and underwater non-segregation properties when poured.
[0037] Such a concrete composition is preferably used as a construction material for concrete structures in the presence of water, such as tunnels and undersea tunnels constructed in ground with a large amount of groundwater, as underwater concrete or underwater non-segregating concrete. The concrete composition is further preferably used as a material for primary lining concrete used in a cast-in-place support system using a shield. Furthermore, the concrete composition is particularly preferably used as a material for lining concrete cast at the construction site, rather than precast, in shield tunnel construction below the groundwater level, as concrete in which the above-mentioned system is employed.
[0038] Although the present invention has been described based on the preferred embodiments, the present invention is not limited to the above-mentioned embodiments. For example, the present invention provides a method for adjusting the amount of each raw material used in the production of concrete so that the physical property values of concrete related to the fluidity, freshness, anti-segregation in water, and strength after hardening are equal to or greater than the above-mentioned preferable values, based on the correlation between external factors such as the temperature of the casting site (external air temperature, tunnel temperature, etc.), the temperature at which concrete is mixed, or the temperature at which concrete is cured, and at least one of the properties of the concrete, such as the fluidity, freshness, anti-segregation in water, and strength after hardening. Also provided is a method for predicting the above-mentioned properties of concrete based on the correlation between the external factors and the amounts of each raw material of the concrete composition. It is also preferable to obtain the above-mentioned correlations in advance by preliminary studies.
Claims
1. Contains water, cement, aggregates and admixtures A concrete composition comprising a water reducing agent or a plasticizer, a setting retarder, and a viscosity enhancer as the admixture, The water-reducing agent or superplasticizer is a high-performance water-reducing agent, a high-performance AE water-reducing agent standard form, or a superplasticizer standard form as specified in JIS A6204, and the initial difference in setting time measured in accordance with JIS A6204 is less than +60 minutes; The concrete composition, wherein the set retarder has a water reduction rate of less than 4% as measured in accordance with JIS A6204.
2. The concrete composition according to claim 1, wherein the water-cement ratio is 30 to 60%.
3. 3. The concrete composition according to claim 1, wherein the water-reducing agent or the fluidizing agent is a high-performance water-reducing agent as defined in JIS A6204.
4. The thickener comprises an alkyl aryl sulfonate and an alkyl ammonium salt, The concrete composition according to any one of claims 1 to 3, further comprising a nonionic surfactant.
5. A method for producing a concrete composition comprising water, cement, aggregate, and admixtures, the admixtures comprising a water-reducing agent or a superplasticizer, a setting retarder, and a viscosity enhancer, The water-reducing agent or superplasticizer is a high-performance water-reducing agent, a high-performance AE water-reducing agent standard form, or a superplasticizer standard form as specified in JIS A6204, and the setting retarder has a water reduction rate measured in accordance with JIS A6204 of less than 4%, The method for producing a concrete composition includes adjusting the content ratio of the water-reducing agent or superplasticizer and the set retarder so that the water-cement ratio of the concrete composition is within the range of 30 to 60%, the slump flow value measured in accordance with JIS A1150 is within the range of 650±50 mm, and the 500 mm flow time measured in accordance with JSCE-F516 4 hours after the concrete is mixed is within 180 seconds.
6. The thickener comprises an alkyl aryl sulfonate and an alkyl ammonium salt, The method for producing a concrete composition according to claim 5, wherein the content of the thickener is adjusted so that the pH measured in accordance with JSCE-D104 (Appendix 2) is 12 or less.
7. The admixture further comprises a nonionic surfactant, The method for producing a concrete composition according to claim 5 or 6, wherein the content ratio of the nonionic surfactant is adjusted so that the pH measured in accordance with JSCE-D104 (Appendix 2) is 12 or less.
Citation Information
Patent Citations
High water-reducing rate ready mixed concrete composition
JP1986132554A
Production of water-permeable cellular mortar and the mortar and mortar material used therefor
JP2000128661A
Agent for improving workability of cement composition and water-reducing admixture for cement containing the same
JP2003165755A
Admixture for concrete
JP2010037129A
Vehicular pop-up hood device
JP2013023148A