Cement Composition

The cement composition with a polyoxyalkylene compound and fatty acid metal salt effectively addresses shrinkage and cracking issues, ensuring high strength and reduced shrinkage in cement products.

JP7561659B2Active Publication Date: 2024-10-04TAIHEIYO CEMENT CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021034984
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-31
Filing Date
2021-03-05
Publication Date
2024-10-04
Estimated Expiration
2041-03-05

AI Technical Summary

Technical Problem

Existing cement compositions fail to effectively reduce shrinkage and prevent cracking, particularly in high-strength applications, necessitating improved shrinkage reducing agents.

Method used

A cement composition incorporating a polyoxyalkylene compound containing a fatty acid metal salt, specifically a divalent metal salt of a fatty acid with 2 to 10 carbon atoms, and a polyoxyalkylene compound, with a specific mass proportion and amount, along with other additives like silica fume and high-performance water reducers, to enhance shrinkage reduction and strength.

Benefits of technology

The cement composition significantly reduces shrinkage and suppresses cracking in cured products, maintaining high strength and fluidity while optimizing cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561659000005
    Figure 0007561659000005
  • Figure 0007561659000001
    Figure 0007561659000001
  • Figure 0007561659000002
    Figure 0007561659000002
Patent Text Reader

Abstract

To provide a cement composition excellent in shrinkage reduction effect.SOLUTION: A cement composition is provided, including: a shrinkage reduction agent including a fatty acid metal salt (preferably, a magnesium salt of 2-ethylhexanoic acid) and a polyoxyalkylene compound, and satisfying the following (A) to (B); and a cement. In the cement composition, the amount of the shrinkage reduction agent with respect to 100 pts.mass of the cement is 0.1-10 pts.mass. (A) The fatty acid metal salt is a metal salt of 2-10C fatty acid, and (B) the ratio of the fatty aid metal salt to the total amount of the fatty acid metal salt and the polyoxyalkylene compound is 10-27 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cement composition. [Background technology]

[0002] From the viewpoint of extending the service life of concrete structures, shrinkage cracks have been of increasing interest, and methods for preventing and reducing shrinkage cracks are being sought. A common method for preventing and reducing shrinkage cracks is to use a shrinkage reducing agent. Patent Document 1 describes an autogenous shrinkage reducing agent for cement compositions that exhibits a good autogenous shrinkage reducing effect and exhibits the effect with a small amount added, and that is characterized by comprising a fatty acid metal salt of a fatty acid having 2 to 10 carbon atoms and a divalent metal. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-81687 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a cement composition having an excellent shrinkage reducing effect. [Means for solving the problem]

[0005] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned object can be achieved by a shrinkage-reducing agent comprising a fatty acid metal salt, which is a divalent metal salt of a fatty acid having 2 to 10 carbon atoms, and a polyoxyalkylene compound, wherein the proportion of the fatty acid metal salt in the total amount of the fatty acid metal salt and the polyoxyalkylene compound is 10 to 27 mass %, and a cement composition comprising cement, wherein the amount of the shrinkage-reducing agent is 0.1 to 10 parts by mass per 100 parts by mass of the cement, and have completed the present invention. That is, the present invention provides the following [1] to [4]. [1] A cement composition comprising a shrinkage-reducing agent that contains a fatty acid metal salt and a polyoxyalkylene compound and satisfies the following (A) to (B), and cement, wherein the amount of the shrinkage-reducing agent per 100 parts by mass of the cement is 0.1 to 10 parts by mass. (A) The fatty acid metal salt is a divalent metal salt of a fatty acid having 2 to 10 carbon atoms. (B) the proportion of the fatty acid metal salt in the total amount of the fatty acid metal salt and the polyoxyalkylene compound is 10 to 27 mass %. [2] The above cement composition has a BET specific surface area of ​​15 to 25 m 2 / g of silica fume, an inorganic powder having a 50% volume cumulative particle size of 0.8 to 5 μm, aggregate A having a maximum particle size of 1.2 mm or less, a high-performance water reducing agent, a defoaming agent, and water. [3] The cement composition according to [1] or [2], wherein the fatty acid metal salt is a magnesium salt of 2-ethylhexanoic acid. [4] The cement composition according to any one of the above [1] to [3], wherein the polyoxyalkylene compound is a compound represented by the following chemical formula (1): R 1 O-(AO) n -R 2 (1) (In the above formula (1), R 1 is a hydrocarbon group having 1 to 30 carbon atoms or a hydrogen atom, and R 2 is a methyl group or a hydrogen atom, AO is an oxyalkylene group having 2 to 4 carbon atoms, and n is the average number of moles of the oxyalkylene group AO added, which is a number from 1 to 100. Effect of the Invention

[0006] According to the cement composition of the present invention, shrinkage of a hardened product of the cement composition can be reduced, and the occurrence of cracks due to shrinkage can be suppressed. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1A is a cross-sectional view showing a formwork into which mortar was poured when measuring the change in length in the examples, cut vertically at approximately the center in the short direction, and FIG. 1B is a cross-sectional view showing the formwork cut vertically at approximately the center in the long direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The cement composition of the present invention is a cement composition containing a shrinkage-reducing agent that contains a fatty acid metal salt and a polyoxyalkylene compound and satisfies the following (A) and (B), and also contains cement, in which the amount of the shrinkage-reducing agent is 0.1 to 10 parts by mass per 100 parts by mass of cement. (A) The fatty acid metal salt is a divalent metal salt of a fatty acid having 2 to 10 carbon atoms. (B) the proportion of the fatty acid metal salt in the total amount of the fatty acid metal salt and the polyoxyalkylene compound is 10 to 27 mass %. Specifically, the fatty acid metal salt is represented by the following chemical formula (2). (RCOO)2M ···(2) In the above formula (2), R is a hydrocarbon group having 1 to 9 carbon atoms, and M is a divalent metal.

[0009] Here, the fatty acid (RCOOH) constituting the fatty acid metal salt may be either a straight-chain fatty acid or a branched-chain fatty acid, but from the viewpoint of further reducing shrinkage, a branched-chain fatty acid is preferable. The fatty acid may be either a saturated fatty acid or an unsaturated fatty acid, but from the viewpoint of further reducing shrinkage, a saturated fatty acid is preferred. The fatty acid has 2 to 10 carbon atoms, preferably 4 to 9 carbon atoms, and more preferably 6 to 8 carbon atoms, from the viewpoint of further reducing shrinkage. Examples of the fatty acid include straight-chain fatty acids such as butanoic acid, pentanoic acid, caproic acid, caprylic acid, nonanoic acid, etc., and branched-chain fatty acids such as dimethylacetic acid, 3-methylbutanoic acid, 2-ethylhexanoic acid, isononanoic acid, etc. Among them, 2-ethylhexanoic acid is preferable from the viewpoint of further reducing shrinkage. The divalent metal constituting the fatty acid metal salt is preferably an alkaline earth metal, more preferably magnesium, from the viewpoint of further reducing shrinkage.

[0010] The ratio of the fatty acid metal salt in the total amount (100% by mass) of the fatty acid metal salt and the polyoxyalkylene compound is 10 to 27% by mass, preferably 12 to 26% by mass, more preferably 14 to 22% by mass, and particularly preferably 18 to 21% by mass. If the ratio is less than 10% by mass, the shrinkage of the hardened body of the cement composition cannot be sufficiently reduced. If the ratio exceeds 27% by mass, the cost becomes excessively high. In addition, the effect of reducing the shrinkage of the hardened body of the cement composition may be reduced.

[0011] A preferred example of the polyoxyalkylene compound contained in the shrinkage reducing agent is a polyoxyalkylene compound represented by the following chemical formula (1). R 1 O-(AO) n -R 2 (1) In the above formula (1), R 1 is a hydrocarbon group having 1 to 30 carbon atoms or a hydrogen atom, and R 2 is a methyl group or a hydrogen atom, AO is an oxyalkylene group having 2 to 4 carbon atoms, and n is the average number of moles of the oxyalkylene group AO added, which is a number of 1 to 100, preferably 2 to 50, more preferably 3 to 40, further preferably 4 to 30, and particularly preferably 5 to 20.

[0012] In the above formula (1), R 1is a hydrocarbon group having 1 to 30 carbon atoms or a hydrogen atom. From the viewpoint of reducing shrinkage and achieving excellent handleability, the carbon number of the hydrocarbon group is 1 to 30, preferably 3 to 25, more preferably 5 to 22, further preferably 8 to 20, and particularly preferably 10 to 18. Examples of the hydrocarbon group having 1 to 30 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, and an isostearyl group. In the above formula (1), R 2 is a hydrogen atom or a methyl group. Among these, a hydrogen atom is preferred from the viewpoint of further reducing shrinkage and excellent handleability.

[0013] In the above formula (1), AO is an oxyalkylene group having a carbon number of 2 to 4. Among them, from the viewpoint of further reducing shrinkage and excellent handleability, an oxyalkylene group having a carbon number of 2 or 3 is preferable. Examples of the oxyalkylene group having 2 to 4 carbon atoms include an oxyethylene group, an oxypropylene group, an oxybutylene group, and an oxytetramethylene group. The oxyalkylene groups may be added randomly or in blocks.

[0014] The polyoxyalkylene compound may be used alone or in combination of two or more kinds (R 1 , AO, or R 2 (combinations of different types) may be used. From the viewpoint of further reducing shrinkage, the proportion of the polyoxyalkylene compound in the total amount of the fatty acid metal salt and the polyoxyalkylene compound is preferably 73 to 90 mass%, more preferably 74 to 88 mass%, even more preferably 78 to 86 mass%, and particularly preferably 79 to 82 mass%. The polyalkylene compound is preferably liquid at 25° C., from the viewpoint of further reducing shrinkage and excellent handling.

[0015] The shrinkage reducing agent used in the present invention may contain other components in addition to the fatty acid metal salt and the polyoxyalkylene compound. As the other components, general shrinkage reducing agents (excluding the above-mentioned two components used in the present invention) can be used. Examples of general shrinkage reducing agents include alkylene oxide adducts of lower alcohols, alcohol-based shrinkage reducing agents, glycol ether / amino alcohol derivative-based shrinkage reducing agents, polyether-based shrinkage reducing agents, low molecular weight alkylene oxide copolymer-based shrinkage reducing agents, and shrinkage reducing agents consisting of a mixture of polyoxyalkylene alcohol ether and inorganic filler. The proportion of other components in the shrinkage-reducing agent is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably 5% by mass or less.

[0016] The cement composition of the present invention is a cement composition containing the above-mentioned shrinkage-reducing agent and cement, in which the amount of the shrinkage-reducing agent is 0.1 to 10 parts by mass per 100 parts by mass of cement. Examples of cement include various Portland cements such as ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement, low-heat Portland cement, and sulfate-resistant Portland cement; various mixed cements obtained by mixing various Portland cements with blast furnace slag, fly ash, or siliceous admixtures (e.g., silica fume); ecocement, white cement, and ultra-fast hardening cement. The amount of shrinkage reducing agent relative to 100 parts by mass of cement is 0.1 to 10 parts by mass, preferably 0.2 to 8 parts by mass, more preferably 0.3 to 6 parts by mass, even more preferably 0.4 to 4 parts by mass, and particularly preferably 0.6 to 2 parts by mass. If the amount is less than 0.1 parts by mass, the effect of reducing shrinkage is small. If the amount exceeds 10 parts by mass, the amount of shrinkage reducing agent is large, and the cost becomes excessively high.

[0017] When preparing the cement composition, the shrinkage-reducing agent may be dissolved in advance in the water for mixing and then mixed with the other materials, or may be added to and mixed with the other materials simultaneously with the water, or may be added and mixed during or after mixing the other materials and water.

[0018] The cement composition may contain other materials as necessary. The other materials are not particularly limited as long as they are generally used as materials for mortar or concrete, and examples thereof include various admixtures such as aggregate, water, fly ash, silica fume, and ground granulated blast furnace slag. Examples of aggregates contained in the cement composition include fine aggregates such as river sand, mountain sand, land sand, sea sand, crushed sand, silica sand, slag fine aggregate, lightweight fine aggregate, or mixtures thereof; and coarse aggregates such as river gravel, mountain gravel, land gravel, sea gravel, crushed stone, blast furnace slag crushed stone, artificial lightweight coarse aggregate, recycled aggregate, or mixtures thereof. The amount of aggregate to be mixed (the total amount when fine aggregate and coarse aggregate are used in combination) is not particularly limited, and may be a general amount used in concrete or the like. The blending amounts of various admixtures such as fly ash, silica fume, and ground granulated blast furnace slag are not particularly limited, and may be the general blending amounts in concrete, etc. For example, the ratio of the admixtures in the total of 100 mass% of cement and admixtures is preferably 5 to 30 mass%, more preferably 10 to 20 mass%.

[0019] The amount of water used in preparing the cement composition may be appropriately determined depending on the application of the cement composition, and is, for example, preferably 10 to 70 parts by mass, more preferably 12 to 60 parts by mass, even more preferably 15 to 50 parts by mass, even more preferably 16 to 45 parts by mass, and particularly preferably 18 to 30 parts by mass, relative to 100 parts by mass of cement. If the amount is 10 parts by mass or more, the fluidity of the cement composition before hardening is further improved. If the amount is 70 parts by mass or less, the strength development of the cement composition is further improved.

[0020] The cement composition may contain various additives (additives) as necessary within the scope of not impairing the object of the present invention. Examples of the various additives include water reducing agents, high-performance water reducing agents, air-entraining agents, air-entraining water reducing agents, high-performance air-entraining water reducing agents, antifoaming agents, air content regulators, setting retarders, setting accelerators, expansive agents, fluidizing agents, foaming agents, separation inhibitors, water retention agents, thickening agents, waterproofing agents, etc.

[0021] According to the above-mentioned cement composition, the cementitious hardened body using the cement composition has high strength (for example, the compressive strength of the mortar measured in accordance with "JIS R 5201 (Physical Testing Method for Cement)" is 80 N / mm 2 More than 90N / mm 2 More preferably, 100N / mm 2 Even if the above conditions are met, shrinkage (particularly autogenous shrinkage) of the cementitious hardened body can be suppressed. Furthermore, in the production of precast products, even when there is a rise in temperature before the cement composition hardens, such as in steam curing that is performed after pouring the unhardened cement composition into a formwork, or in a temperature rise due to the heat of hydration of a mass concrete member, the cement composition of the present invention can suppress shrinkage of the resulting cementitious hardened body.

[0022] The cement composition of the present invention further contains, in addition to the above-mentioned shrinkage reducing agent and cement, a cement having a BET specific surface area of ​​15 to 25 m. 2 / g of silica fume, inorganic powder with a 50% cumulative volume particle size of 0.8 to 5 μm, aggregate A with a maximum particle size of 1.2 mm or less, a high-performance water reducing agent, a defoaming agent, and water. A hardened product of a cement composition containing such materials (hereinafter also referred to as an "ultra-high strength cement composition") has a high strength (for example, 300 N / mm 2 The hardened body of a cement composition having high strength is more susceptible to autogenous shrinkage than a cementitious hardened body having ordinary strength, but the cement composition of the present invention can suppress the shrinkage of the hardened body while maintaining the strength development. As the cement contained in the ultra-high strength cement composition, various Portland cements such as ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement, low-heat Portland cement, and sulfate-resistant Portland cement are preferred, and from the viewpoint of improving fluidity, moderate-heat Portland cement and low-heat Portland cement are more preferred.

[0023] The BET specific surface area of ​​the silica fume contained in the ultra-high strength cement composition is 15 to 25 m 2 / g, preferably 17 to 23 m 2 / g, particularly preferably 18 to 22 m 2 / g. The specific surface area is 15 m 2 If the specific surface area is less than 25 m / g, the strength development of the ultra-high strength cement composition is reduced. 2 If the viscosity exceeds 1 / g, the fluidity of the ultra-high strength cement composition decreases.

[0024] Examples of inorganic powders having a 50% cumulative volume particle size of 0.8 to 5 μm contained in the ultra-high strength cement composition include quartz powder (silica powder), volcanic ash, fly ash (classified or crushed), slag powder, limestone powder, feldspar powder, mullite powder, alumina powder, silica sol, carbide powder, nitride powder, etc. These may be used alone or in combination of two or more. Among these, it is preferable to use quartz powder or fly ash from the viewpoint of improving the fluidity and strength development of the ultra-high strength cement composition. In this specification, the inorganic powder having a 50% volume cumulative particle size of 0.8 to 5 μm does not include cement.

[0025] The 50% volume cumulative particle size of the inorganic powder is 0.8 to 5 μm, preferably 1 to 4 μm, more preferably 1.1 to 3.5 μm, and particularly preferably 1.2 μm or more and less than 3 μm. If the particle size is less than 0.8 μm, the fluidity of the ultra-high strength cement composition decreases. If the particle size exceeds 5 μm, the strength development of the ultra-high strength cement composition decreases. The 50% volume cumulative particle size of the inorganic powder can be determined using a commercially available particle size distribution measuring device (for example, product name "Microtrac HRA Model 9320-X100" manufactured by Nikkiso Co., Ltd.). Specifically, a particle size distribution measuring device is used to create a cumulative particle size curve, and the 50% volume cumulative particle size can be calculated from the cumulative particle size curve. 3 0.06 g of a sample is added to each of the samples, and the mixture is ultrasonically dispersed for 90 seconds using an ultrasonic dispersing device (for example, product name "US300" manufactured by Nippon Seiki Seisakusho Co., Ltd.), and then the measurement is performed.

[0026] The maximum particle size of the inorganic powder is preferably 15 μm or less, more preferably 14 μm or less, and particularly preferably 13 μm or less, from the viewpoint of further improving the strength development of the ultra-high strength cement composition. The 95% volume cumulative particle size of the inorganic powder is preferably 8 μm or less, more preferably 7 μm or less, and particularly preferably 6 μm or less, from the viewpoint of further improving the strength development of the ultra-high strength cement composition.

[0027] The inorganic powder is preferably one containing SiO2 as a main component (for example, quartz powder). The content of SiO2 in the inorganic powder is preferably 50 mass% or more, more preferably 60 mass% or more, and particularly preferably 70 mass% or more. If the content is 50 mass% or more, the strength development of the ultra-high strength cement composition is further improved.

[0028] In the ultra-high strength cement composition, the proportion of cement is preferably 55 to 65 volume %, more preferably 57 to 63 volume %, in the total amount of cement, silica fume, and the inorganic powder (100 volume %). If the proportion is 55 volume % or more, the strength development of the ultra-high strength cement composition is further improved. If the proportion is 65 volume % or less, the fluidity of the ultra-high strength cement composition is further improved. In the total amount of cement, silica fume and the inorganic powder (100% by volume), the proportion of silica fume is preferably 5 to 25% by volume, more preferably 7 to 23% by volume. If the proportion is 5% by volume or more, the strength development of the ultra-high strength cement composition is further improved. If the proportion is 25% by volume or less, the fluidity of the ultra-high strength cement composition is further improved. The proportion of the inorganic powder is preferably 15 to 35 volume %, more preferably 17 to 33 volume %, of the total amount of cement, silica fume and the inorganic powder (100 volume %). If the proportion is 15 volume % or more, the strength development of the ultra-high strength cement composition is further improved. If the proportion is 35 volume % or less, the fluidity of the ultra-high strength cement composition is further improved.

[0029] Examples of the aggregate A used in the ultra-high strength cement composition include river sand, land sand, sea sand, crushed sand, silica sand, artificial fine aggregate (for example, slag fine aggregate or fired fine aggregate obtained by firing fly ash, etc.), recycled fine aggregate, and mixtures thereof. The maximum particle size of the aggregate A is 1.2 mm or less, preferably 1.1 mm or less, and particularly preferably 1.0 mm or less. If the maximum particle size is 1.2 mm or less, the strength development of the ultra-high strength cement composition is further improved. From the viewpoint of improving the fluidity and strength development of the ultra-high strength cement composition, the particle size distribution of the above aggregate A is preferably such that the proportion of aggregate A having a particle size of 0.6 mm or less is 95 mass% or more, the proportion of aggregate A having a particle size of 0.3 mm or less is 40 to 50 mass%, and the proportion of aggregate A having a particle size of 0.15 mm or less is 6 mass% or less. The proportion of aggregate A in the ultra-high strength cement composition is preferably 20-40% by volume, more preferably 22-38% by volume, even more preferably 30-37% by volume, and particularly preferably 32-36% by volume. If the proportion is 20% by volume or more, the heat generation amount of the ultra-high strength cement composition is small, and the shrinkage amount of the hardened body of the ultra-high strength cement composition is small. If the proportion is 40% by volume or less, the strength development of the ultra-high strength cement composition is further improved.

[0030] The high performance water reducing agent contained in the ultra-high strength cement composition may be a naphthalenesulfonic acid-based, melamine-based, polycarboxylic acid-based, etc. Among them, from the viewpoint of further improving the fluidity and strength development of the ultra-high strength cement composition, a polycarboxylic acid-based high performance water reducing agent is preferred. The amount of the high-performance water reducing agent is preferably 0.5 to 5.0 parts by mass, more preferably 1.0 to 4.0 parts by mass, and particularly preferably 2.0 to 3.0 parts by mass in the case of a liquid, and is preferably 0.1 to 2.0 parts by mass, more preferably 0.2 to 1.5 parts by mass, and particularly preferably 0.4 to 1.2 parts by mass in the case of a solid such as a powder, relative to 100 parts by mass of the total amount of cement, silica fume, and the above inorganic powder. If the amount is 0.5 parts by mass or more in the case of a liquid (0.2 parts by mass or more in the case of a solid), the water reducing performance is improved and the fluidity of the ultra-high strength cement composition is improved. If the amount is 5.0 parts by mass or less in the case of a liquid (1.5 parts by mass or less in the case of a solid), the strength development of the ultra-high strength cement composition is further improved.

[0031] As the defoaming agent contained in the ultra-high strength cement composition, a commercially available product can be used. The amount of the antifoaming agent is preferably 0.001 to 0.5 parts by mass, more preferably 0.01 to 0.4 parts by mass, and particularly preferably 0.1 to 0.3 parts by mass, based on 100 parts by mass of the total amount of cement, silica fume, and the inorganic powder. If the amount is 0.001 parts by mass or more, the strength development of the ultra-high strength cement composition is improved. If the amount exceeds 0.5 parts by mass, the effect of improving the strength development of the ultra-high strength cement composition reaches a plateau.

[0032] The amount of water contained in the ultra-high strength cement composition is preferably 10 to 20 parts by mass, more preferably 11 to 18 parts by mass, and particularly preferably 14 to 16 parts by mass, based on 100 parts by mass of the total amount of cement, silica fume, and the inorganic powder. If the amount is 10 parts by mass or more, the fluidity of the ultra-high strength cement composition is improved. If the amount is 20 parts by mass or less, the strength development of the ultra-high strength cement composition is further improved.

[0033] In addition, the compressive strength of the hardened body obtained by hardening the mortar made of the ultra-high strength cement composition (not including aggregate B described later) is preferably 100 N / mm 2 More preferably, 120N / mm 2 More preferably, 280N / mm 2 More preferably, 300N / mm 2 That's all.

[0034] The ultra-high strength cement composition may include aggregate B having a maximum particle size greater than 1.2 mm and not greater than 13 mm. Examples of aggregate B include river sand, mountain sand, land sand, sea sand, crushed sand, silica sand, artificial fine aggregate (for example, slag fine aggregate, burned fine aggregate obtained by burning fly ash, etc.), recycled fine aggregate, river gravel, mountain gravel, land gravel, crushed stone, artificial coarse aggregate (for example, slag coarse aggregate, burned coarse aggregate obtained by burning fly ash, etc.), recycled coarse aggregate, and mixtures of these. The maximum particle size of the aggregate B is 13 mm or less, preferably 12 mm or less, more preferably 11 mm or less, and particularly preferably 10 mm or less. If the maximum particle size is 13 mm or less, the strength development of the cement composition is improved. From the viewpoint of cost reduction and the like, the maximum particle size of aggregate B is a value exceeding 1.2 mm, preferably 3 mm or more, more preferably 5 mm or more, and particularly preferably 7 mm or more. In this specification, when the maximum particle size of aggregate B is 5 mm or more, the "maximum particle size" refers to the particle size of aggregate B indicated by the nominal size of the smallest sieve among those through which 90% or more by mass of the total aggregate B passes (generally known as the definition of the maximum particle size of coarse aggregate).

[0035] The minimum particle size of aggregate B is preferably greater than the maximum particle size of aggregate A, and is more preferably 2 mm or more, even more preferably 3 mm or more, even more preferably 4 mm or more, and particularly preferably 5 mm or more (in this case, it corresponds to coarse aggregate). In this specification, the minimum particle size of aggregate B refers to the particle size of aggregate B when it reaches 15 mass% of the total particle size of aggregate B when accumulating from the smallest particle size to the larger particle sizes.

[0036] In the present invention, the total amount of aggregate A and aggregate B in the ultra-high strength cement composition is preferably 25-40% by volume, more preferably 28-38% by volume, and particularly preferably 30-36% by volume. If the amount is 25% by volume or more, the heat generation amount of the ultra-high strength cement composition is small, and the shrinkage amount of the hardened body of the ultra-high strength cement composition is small. If the amount is 40% by volume or less, the strength development of the ultra-high strength cement composition can be improved. The ratio of aggregate B to the total amount of aggregate A and aggregate B is preferably 40% by volume or less, more preferably 30% by volume or less, and particularly preferably 25% by volume or less. If the ratio is 40% by volume or less, the strength development of the ultra-high strength cement composition is further improved. The compressive strength of a cementitious hardened body obtained by hardening an ultra-high strength cement composition (e.g., concrete) containing aggregate B is preferably 300 N / mm 2 More preferably, 320N / mm 2 More preferably, 340N / mm 2 More preferably, 360N / mm 2 That's all.

[0037] An example of a method for producing a hardened body of the above-mentioned ultra-high strength cement composition includes a molding step of pouring the ultra-high strength cement composition into a formwork to obtain an unhardened molded body; a room temperature curing step of sealingly curing or air curing the unhardened molded body at 10 to 40°C for 24 hours or more and then removing it from the formwork to obtain a hardened molded body; a heat curing step of subjecting the hardened molded body to either steam curing or hot water curing at 70°C or more and less than 100°C for 6 hours or more and autoclave curing at 100 to 200°C for 1 hour or more to obtain a hardened body after heat curing; and a high temperature heating step of heating the heat-cured hardened body at 150 to 200°C for 24 hours or more (excluding heating due to autoclave curing) to obtain a hardened body of the ultra-high strength cement composition.

[0038] [Molding process] This step is a step of casting the ultra-high strength cement composition into a formwork to obtain an unhardened molded body. The method of kneading the ultra-high strength cement composition before casting is not particularly limited. The device used for kneading is also not particularly limited, and a conventional mixer such as an omni mixer, a pan mixer, a twin-shaft mixer, or a tilting mixer can be used. Furthermore, the casting (molding) method is also not particularly limited. The unhardened molded body in this step may be made of an ultra-high strength cement composition in which air bubbles have been reduced or removed. By reducing or removing air bubbles in the ultra-high strength cement composition, the strength development of the ultra-high strength cement composition can be further improved. Methods for reducing or removing air bubbles in an ultra-high-strength cement composition include (1) mixing the ultra-high-strength cement composition under reduced pressure, (2) reducing the pressure of the mixed ultra-high-strength cement composition before pouring it into a formwork to degas it, and (3) reducing the pressure of the ultra-high-strength cement composition after pouring it into a formwork to degas it.

[0039] [Room temperature curing process] This step involves subjecting the uncured molded body to sealed curing or air curing at 10 to 40°C (preferably 15 to 30°C) for 24 hours or more (preferably 24 to 72 hours, more preferably 24 to 48 hours), and then removing it from the formwork to obtain a cured molded body. When the curing temperature is 10° C. or higher, the curing time can be shortened. When the curing temperature is 40° C. or lower, the strength development of the ultra-high strength cement composition is improved. If the curing time is 24 hours or more, defects such as chips and cracks are less likely to occur in the hardened molded body when it is demolded.

[0040] [Heat curing process] This step is a step in which the hardened molded body obtained in the previous step is subjected to either or both of steam curing or hot water curing at 70°C or higher but lower than 100°C (preferably 75 to 95°C, more preferably 80 to 92°C) for 6 hours or more, and autoclave curing at 100 to 200°C (preferably 160 to 190°C) for 1 hour or more, to obtain a hardened body after heat curing. In this step, when only steam curing or hot water curing is performed, the curing time is preferably 24 hours or more, more preferably 24 to 96 hours, and particularly preferably 36 to 72 hours. When only autoclave curing is performed, the curing time is preferably 8 to 60 hours, and more preferably 12 to 48 hours. When both steam curing or hot water curing and autoclave curing are performed (for example, when steam curing or hot water curing is performed and then autoclave curing is performed), the curing time for steam curing or hot water curing is preferably 6 to 72 hours, and more preferably 12 to 48 hours, and the curing time for autoclave curing is preferably 1 to 24 hours, and more preferably 4 to 18 hours. In this step, when the curing temperature is within the above range, the curing time can be shortened and the strength development of the ultra-high strength cement composition can be further improved. In addition, in this step, if the curing time is within the above range, the strength development of the ultra-high strength cement composition is further improved.

[0041] [High temperature heating process] This step is a step in which the hardened body after heat curing is heated (excluding heating in an autoclave) at 150 to 200°C (preferably 170 to 190°C) for 24 hours or more (preferably 24 to 72 hours, more preferably 36 to 48 hours) to obtain a cementitious hardened body by hardening the ultra-high strength cement composition. The heating in this step is usually carried out in a dry atmosphere (in other words, in a state where water or water vapor is not artificially supplied). If the heating temperature is 150° C. or higher, the heating time can be shortened. If the heating temperature is 200° C. or lower, the strength of the cementitious hardened body becomes greater. If the heating time is 24 hours or longer, the strength of the hardened cementitious body will be greater.

[0042] [Water absorption process] A water absorbing step may be included between the room temperature curing step and the heat curing step, in which the hardened molded body obtained in the room temperature curing step is allowed to absorb water. As a method for making the hardened molded body absorb water, a method of immersing the molded body in water can be mentioned. In addition, in the method of immersing the molded body in water, from the viewpoint of increasing the amount of water absorption in a short time and further improving the strength development of the ultra-high strength cement composition, the following methods are preferred: (1) a method of immersing the molded body in water under reduced pressure, (2) a method of immersing the molded body in boiling water, and then lowering the water temperature to 40°C or less while the molded body is still immersed, (3) a method of immersing the molded body in boiling water, and then removing the molded body from the boiling water and then immersing the molded body in water at 40°C or less, (4) a method of immersing the molded body in water under pressure, or (5) a method of immersing the molded body in an aqueous solution in which an agent for improving the water permeability of the molded body is dissolved.

[0043] The above-mentioned molded body can be immersed in water under reduced pressure by using equipment such as a vacuum pump or a large reduced pressure vessel. The above molded article can be immersed in boiling water by using equipment such as a high-temperature, high-pressure container or a hot water bath. The time for immersing the hardened molded body in water under reduced pressure or boiling water is preferably 3 minutes or more, more preferably 8 minutes or more, and particularly preferably 20 minutes or more, from the viewpoint of increasing the water absorption rate. The upper limit of the time is preferably 60 minutes, more preferably 45 minutes, from the viewpoint of increasing the compressive strength of the cementitious hardened body. EXAMPLES

[0044] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Materials used 1] (1) Ordinary Portland cement; manufactured by Taiheiyo Cement Corporation; density: 3.16 g / cm 3 (2) Silica fume; Tomoe Engineering Co., Ltd., product name "EFACO" (3) Fine aggregate; Surface dry density: 2.57g / cm 3 , Maximum particle size: 1.2mm or less (4) Shrinkage reducing agent A; magnesium metal salt of 2-ethylhexanoic acid (fatty acid metal salt): 25% by mass, C 18 H 37 O-(C3H6O) 10 -H (propylene oxide (10 moles) adduct of stearyl alcohol: polyoxyalkylene compound represented by the above-mentioned chemical formula (1): 75% by mass (5) Shrinkage reducing agent B; magnesium metal salt of 2-ethylhexanoic acid (fatty acid metal salt): 20% by mass, C 18 H 37 O-(C3H6O) 10 -H (propylene oxide (10 moles) adduct of stearyl alcohol: polyoxyalkylene compound represented by the above-mentioned chemical formula (1): 80% by mass (6) Shrinkage reducing agent C; magnesium metal salt of 2-ethylhexanoic acid (fatty acid metal salt): 15% by mass, C 18 H 37 O-(C3H6O) 10 -H (propylene oxide (10 moles) adduct of stearyl alcohol: polyoxyalkylene compound represented by the above-mentioned chemical formula (1): 85% by mass (7) Shrinkage reducer D; alkylene oxide adduct of lower alcohol, manufactured by Pacific Materials Corporation, trade name "Tetraguard AS21" (6) High-performance water-reducing agent; manufactured by Frolic Co., Ltd., product name "SF500U", liquid (7) Defoamer 1; product name "Sydox DEF-001" manufactured by NOF Corporation (8) Defoamer 2; BASF Japan, trade name "Master Air 404" (9) Water; tap water

[0045] [Examples 1 to 3] The mixed cement, which was made by mixing ordinary Portland cement and silica fume in advance in a bag, and the fine aggregate were charged into a 5-liter Hobart mixer and dry mixed for 15 seconds. Next, mixing water, which was made by mixing a shrinkage reducing agent, a high-performance water reducing agent, an antifoaming agent, and water of the types shown in Table 1, was charged into the mixer and mixed for 240 seconds to prepare mortar. The mixing ratio of each material is shown in Table 1. In Tables 1 and 3, the symbol "-" indicates that the material was not used. The flow value, time to reach 200 mm, air content, and length change of the obtained mortar were measured according to the following methods.

[0046] (1) Measurement of mortar flow value and time to reach 200 mm In accordance with "JIS R 5201:2015 (Physical Testing Methods for Cement)", the flow values ​​of the mortar after 90 seconds and 180 seconds were measured without performing the 15 drop motions. In measuring the flow value, the time from when the slump cone was completely pulled up until the flow value of the mortar reached 200 mm (time to reach 200 mm) was measured. (2) Measurement of air volume The air content of the mortar was measured in accordance with "JIS A 1128:2005 (Test method for air content of fresh concrete by pressure - Air chamber pressure method)". The volume of the mortar air meter used for the measurement was 500 milliliters.

[0047] (3) Measurement of length change In order to restrain the free deformation of the test specimen and to prevent the loss of moisture, a Teflon sheet 3 was laid on the bottom of the inside of formwork 2 as shown in Figure 1, and a polystyrene board 4 was laid on the 100 x 100 mm side of the inside of the formwork. Formwork 2 had an inner dimension of 400 x 100 x 100 mm, and a polyester film 5 was further laid inside formwork 2. Mortar was then poured into formwork 2 to prepare test specimen 1. After pouring, the concrete was compacted, and the entire specimen 1 was wrapped in a polyester film 5 to perform sealing and curing at room temperature (20°C). Teflon is a registered trademark. An embedded strain gauge 6 was embedded in the approximate center of the test specimen 1, and shrinkage strain was measured from the initial setting time at material ages of 7 days, 14 days, and 28 days. The initial setting time was measured in accordance with "JIS A 1147:2007 (Test method for setting time of concrete)". In addition, instead of performing sealed curing, pre-curing was performed at 20°C for 12 hours, then the temperature was raised to 45°C at a heating rate of 2.1°C / hour, held at 45°C for 12 hours, and then cooled to 20°C at a cooling rate of 4.5°C / hour. Except for this, specimens were prepared in the same manner, and the shrinkage strain from the initial setting time of the specimens to an age of 7 days (shown as "thermal history 7 days" in Table 2) was measured.

[0048] (4) Measurement of compressive strength of mortar The compressive strength of the mortar at ages of 7 and 14 days was measured in accordance with JIS R 5201:2015 (Physical testing methods for cement).

[0049] [Comparative Example 1] A mortar was prepared in the same manner as in Example 1, except that no shrinkage reducing agent was used and antifoaming agent 2 was used instead of antifoaming agent 1, and the flow value and other properties of the obtained mortar were measured in the same manner as in the examples. [Comparative Example 2] A mortar was prepared in the same manner as in Example 1 except that shrinkage-reducing agent D was used, and the flow value and other properties of the obtained mortar were measured in the same manner as in the Examples. The results are shown in Table 2.

[0050] [Table 1]

[0051] [Table 2]

[0052] From Table 2, comparing Examples 1 to 3 with Comparative Examples 1 to 2, the shrinkage strain (material age 7 days: -507 to -365 × 10 -6 , 14 days old: -532~-395×10 -6 , 28 days old: -565~-430×10 -6 Temperature history was performed for 7 days: -705 to -609 x 10 -6 ) is the shrinkage strain in Comparative Examples 1 and 2 (7 days: -866 to -604 × 10 -6 , 14 days old: -943~-618×10 -6 , 28 days old: -1,042~-653×10 -6 Temperature history was performed for 7 days: -1301 to -924 x 10 -6 ) is smaller than

[0053] In addition to the above-mentioned material 1, the following material 2 was further used to carry out Examples 4 to 12 and Comparative Examples 3 to 7. [Materials used 2] (10) Shrinkage reducing agent E; magnesium metal salt of 2-ethylhexanoic acid (fatty acid metal salt): 25% by mass, ethylene oxide / propylene oxide adduct of butanol: polyoxyalkylene compound represented by the above-mentioned chemical formula (1): 75% by mass (11) Shrinkage reducing agent F (having a different structure from shrinkage reducing agent A); magnesium metal salt of 2-ethylhexanoic acid (fatty acid metal salt): 25% by mass, C 18 H 37 O-(C3H6O) 15 -H (propylene oxide (15 moles) adduct of stearyl alcohol: polyoxyalkylene compound represented by the above-mentioned chemical formula (1): 75% by mass (12) Shrinkage reducing agent G (having a different structure from shrinkage reducing agent C); magnesium metal salt of 2-ethylhexanoic acid (fatty acid metal salt): 15% by mass, C 18 H 37 O-(C3H6O) 15 -H (propylene oxide (15 moles) adduct of stearyl alcohol: polyoxyalkylene compound represented by the above-mentioned chemical formula (1): 85% by mass (13) Shrinkage reducer H; 2-ethyl-1-hexanol with 3.5 moles of ethylene oxide (14) PFC (non-porous concrete) powder; low heat Portland cement: 60% by volume, silica fume (BET specific surface area: 20 m 2 / g): 10% by volume, inorganic powder (silica powder, 50% cumulative particle size by volume: 2 μm, maximum particle size: 12 μm, 95% cumulative particle size by volume: 5.8 μm): 30% by volume

[0054] [Examples 4 to 7, Comparative Examples 3 to 4] The mixed cement, which was made by mixing ordinary Portland cement and silica fume in advance in a bag, and the fine aggregate were charged into a 5-liter Hobart mixer and dry mixed for 15 seconds. Next, mixing water, which was made by mixing a shrinkage reducing agent, a high-performance water reducing agent, an antifoaming agent, and water of the types shown in Table 3 in advance, was charged into the mixer and mixed for 240 seconds to prepare mortar. The mixing ratio of each material is shown in Table 3. In the same manner as in the measurement of the change in length in Example 1, a mortar specimen was prepared and subjected to sealed curing at room temperature (20°C) for 9 days. The specimen was then demolded and the polyester film that had been wrapped around it was removed to obtain a hardened cement composition. The hardened cement composition was then left to stand in an environment at room temperature (20°C) and a relative humidity of 60%. After standing, the shrinkage strain was measured at ages of 28 and 91 days from the time when setting began. The measured shrinkage strain was mainly due to drying shrinkage. The compressive strength of the mortar at 28 days of age was measured in the same manner as in Example 1. The results are shown in Table 4. The values ​​in parentheses for shrinkage strain in Table 4 indicate the shrinkage strain reduction rate ((shrinkage strain value-shrinkage strain value of Comparative Example 4) / shrinkage strain value of Comparative Example 4×100%) when the shrinkage strain value of Comparative Example 4 is taken as 100%.

[0055] [Examples 8 to 10, Comparative Example 5] Mortar specimens were prepared in the same manner as in Example 4, except that PFC powder was used instead of the blended cement, and the shrinkage strain at ages of 28 days and 91 days, and the compressive strength at age 28 days were measured in the same manner as in Example 1. The measured shrinkage strain was mainly due to drying shrinkage. The results are shown in Table 4. The values ​​in parentheses for shrinkage strain in Table 4 indicate the shrinkage strain reduction rate ((shrinkage strain value-shrinkage strain value of Comparative Example 5) / shrinkage strain value of Comparative Example 5×100%) when the shrinkage strain value of Comparative Example 5 is taken as 100%.

[0056] [Examples 11 to 12, Comparative Examples 6 to 7] A mortar specimen was prepared in the same manner as in the measurement of the change in length in Example 1, except that the PFC powder was used instead of the mixed cement, and the specimen was subjected to sealed curing at room temperature (20°C) for two days. The specimen was then demolded, and the polyester film that had been wrapped around the specimen was removed to obtain a hardened cement composition. The hardened body was immersed in water in a desiccator with reduced pressure for 30 minutes. The pressure was reduced using an "Aspirator (AS-01)" manufactured by AS ONE Corporation. After immersion, the molded body was heated to 90°C at a heating rate of 15°C / hour, steam cured at a maximum temperature of 90°C for 48 hours, and then cooled to 20°C at a heating rate of 15°C / hour. After that, the molded body was heated to 180°C at a heating rate of 60°C / hour, heated at a maximum temperature of 180°C for 48 hours, and then cooled to room temperature at a heating rate of 60°C / hour. The compressive strength of the mortar after heating was measured in accordance with JIS R 5201:2015 (Physical testing methods for cement). The results are shown in Table 4. The values ​​in parentheses for shrinkage strain in Table 4 indicate the shrinkage strain reduction rate ((shrinkage strain value-shrinkage strain value of Comparative Example 6) / shrinkage strain value of Comparative Example 6×100%) when the shrinkage strain value of Comparative Example 6 is taken as 100%.

[0057] [Table 3]

[0058] [Table 4]

[0059] From Table 4, comparing Examples 4 to 7 with Comparative Examples 3 to 4, the shrinkage strain in Examples 4 to 7 (28 days: -826 to -671 x 10 -6 , 91 days old: -998~-840×10 -6 ) is the shrinkage strain in Comparative Examples 3 and 4 (28 days: -1086 to -910 × 10 -6 , 91 days old: -1,265~-1084×10 -6 ) is smaller than In addition, when comparing Examples 8 to 10 with Comparative Example 5, the shrinkage strain (28 days: −875 to −756 × 10 -6 , 91 days old: -1002~-864×10 -6 ) is the shrinkage strain in Comparative Example 5 (28 days: -1185 x 10 -6 , 91 days old: -1,271×10 -6 ) is smaller than Furthermore, when comparing Examples 11 and 12 with Comparative Examples 6 and 7, the shrinkage strain (-675 to -629 × 10 -6 ) is the shrinkage strain (-881 to -334 × 10 -6 ) is smaller than [Explanation of symbols]

[0060] 1. Test specimen (mortar) 2 Formwork 3 Teflon sheet 4. Polystyrene boards 5. Polyester film 6 Embedded strain gauge

Claims

1. A cement composition comprising a shrinkage-reducing agent which contains a fatty acid metal salt and a polyoxyalkylene compound and satisfies the following (A) and (B), cement, silica fume having a BET specific surface area of ​​15 to 25 m 2 / g, an inorganic powder having a 50% volume cumulative particle size of 0.8 to 5 μm, aggregate A having a maximum particle size of 1.2 mm or less, a high-performance water-reducing agent, an antifoaming agent, and water, wherein the amount of the shrinkage-reducing agent per 100 parts by mass of the cement is 0.1 to 10 parts by mass, A cement composition, wherein the polyoxyalkylene compound is a compound represented by the following chemical formula (1): (A) The fatty acid metal salt is a magnesium salt of a saturated fatty acid and a branched chain fatty acid having 6 to 9 carbon atoms. (B) the ratio of the fatty acid metal salt to the total amount of the fatty acid metal salt and the polyoxyalkylene compound is 10 to 15 mass %. R 1 O-(AO)n-R 2 ... (1) (In the above formula (1), R 1 is a hydrocarbon group having 10 to 20 carbon atoms, R 2 is a methyl group or a hydrogen atom, AO is an oxyalkylene group having 2 to 4 carbon atoms, and n is the average number of moles of the oxyalkylene group AO added, which is a number from 5 to 10.)

2. 2. The cement composition according to claim 1, wherein said fatty acid metal salt is a magnesium salt of 2-ethylhexanoic acid.

Citation Information

Patent Citations

  • Cement admixture and cement composition

    JP2005089228A

  • Shrinkage reduction agent for hydraulic material

    JP2005187279A

  • Ultra-high-strength high-fluidity concrete and cement composition

    JP2014169213A

  • Self-shrinkage reducing agent for cement composition and cement composition