The composition for sliding members, utilizing ethylene propylene diene rubber and polyolefin resin with silicone oil and fluororesin additives, addresses the issue of high-temperature sliding property degradation in weatherstrips, ensuring stable and low-friction performance.
Patent Information
- Application Number
- JP2021126714
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-02
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2041-08-02
AI Technical Summary
Weatherstrips for car windows experience a decrease in sliding properties and may generate abnormal noises or require greater force to operate when exposed to high temperatures due to increased friction coefficients.
A composition for sliding members using a resin component containing ethylene propylene diene rubber, polyolefin resin, and a crosslinking agent, without silicone oil or fluororesin, with specific proportions and additives like silicone oil and fluororesin, to form a dynamic crosslinked product dispersed in a polyolefin resin matrix.
The composition maintains stable sliding properties and reduces friction even in high-temperature environments, preventing abnormal noises and maintaining low sliding resistance over time.
Smart Images

Figure 0007561710000005 
Figure 0007561710000006 
Figure 0007561710000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition for a sliding member, a method for producing the same, and a sliding member. [Background technology]
[0002] Weatherstrips attached to the sashes of automobile doors are automobile parts used to seal the outer edges of the window glass, thereby firmly holding the window glass in place and preventing rain, wind, foreign objects, etc. from entering the vehicle interior, while also allowing the window glass to be opened and closed smoothly. Weatherstrips are generally made of a composition for sliding members containing a dynamically crosslinked thermoplastic elastomer (Thermoplastic Vulcanizates: TPV). In order to improve the sliding properties, silicone compounds such as silicone oil are sometimes added to the TPV. For example, Patent Document 1 discloses a sliding material in which a high content of silicone compounds is added to a dynamically crosslinked olefin-based thermoplastic elastomer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5167128 Summary of the Invention [Problem to be solved by the invention]
[0004] When the window glass is opened and closed in an automobile exposed to the hot summer sun, the hot weather strip slides against the window glass. When sliding in such a high-temperature environment, the friction coefficient of the weather strip surface increases and remains high, causing a problem of reduced sliding properties. When the sliding properties decrease, abnormal noise is generated and greater force is required when opening and closing the window glass. The present invention has been made in view of the above circumstances, and provides a slide member in which the deterioration of sliding properties after sliding in a high-temperature environment is reduced, a composition for a slide member, and a method for producing the same. [Means for solving the problem]
[0005] In order to achieve the above object, the present invention employs the following configuration. [1] A resin component including a dynamically crosslinked body (A) and a polyolefin resin (B) (but not including silicone oil or fluororesin; the same applies below), a silicone oil, and a fluororesin; The dynamically crosslinked body (A) is obtained by kneading and crosslinking raw materials including an ethylene propylene diene rubber (A1), a polyolefin resin (A2) containing 60 mass% or more of structural units based on ethylene, a polyolefin resin (A3) containing 60 mass% or more of structural units based on propylene, and a crosslinking agent (A4); A ratio of the dynamically crosslinked body (A) to the total mass of the resin components is 50 to 92 mass%, and a ratio of the polyolefin resin (B) to the total mass of the resin components is 8 to 50 mass%, A composition for a sliding member, comprising 5 to 20 parts by mass of the silicone oil and 1 to 22 parts by mass of the fluororesin relative to 100 parts by mass of the resin component. [2] The composition for a sliding member according to [1], wherein a proportion of the ethylene propylene diene rubber (A1) is 15 to 40 mass%, a proportion of the polyolefin resin (A2) is 25 to 60 mass%, a proportion of the polyolefin resin (A3) is 15 to 40 mass%, and a proportion of the crosslinking agent (A4) is 1 to 10 mass%, based on the total mass of raw materials for obtaining the dynamically crosslinked body (A). [3] The composition for a sliding member according to [1] or [2], wherein the average particle size of the fluororesin is 50 μm or less. [4] The composition for a sliding member according to any one of [1] to [3], wherein the dynamically crosslinked product (A) forms domains and is dispersed in a matrix containing the polyolefin resin (B). [5] A method for producing the composition for a sliding member according to any one of [1] to [4], comprising the steps of: a dynamic crosslinking step of kneading and crosslinking raw materials containing the ethylene propylene diene rubber (A1), the polyolefin resin (A2), the polyolefin resin (A3), and the crosslinking agent (A4) to obtain the dynamically crosslinked body (A); a mixing step of mixing the dynamically crosslinked product (A) obtained, the resin component other than the dynamically crosslinked product (A), the silicone oil, and the fluororesin. [6] A sliding member formed from the composition for a sliding member according to any one of [1] to [4]. Effect of the Invention
[0006] In the sliding member of the present invention, the deterioration of the sliding property after sliding in a high-temperature environment is reduced. According to the composition for a sliding member of the present invention and the method for producing the same, it is possible to form a sliding member in which the deterioration of the sliding property after sliding in a high-temperature environment is reduced. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic cross-sectional view of a weather strip equipped with a sliding member of the present invention. [Diagram 2] FIG. 2 shows fluorine atom concentration distribution maps obtained by an electron probe microanalyzer (EPMA) of a molded article made of the composition of Example 1, in which (a) is a fluorine atom concentration distribution map of a cross section near the surface, and (b) is a fluorine atom concentration distribution map of the surface. [Diagram 3] 4A and 4B are fluorine atom concentration distribution maps obtained by an electron probe microanalyzer (EPMA) of a molded article made of the composition of Example 2, in which (a) is a fluorine atom concentration distribution map of a cross section near the surface, and (b) is a fluorine atom concentration distribution map of the surface. [Figure 4] FIG. 2 shows fluorine atom concentration distribution diagrams obtained by an electron probe microanalyzer (EPMA) of a molded product made of the composition of Comparative Example 2, in which (a) is a fluorine atom concentration distribution diagram of a cross section near the surface, and (b) is a fluorine atom concentration distribution diagram of the surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <Composition for Sliding Members> The composition for a sliding member of the present invention contains a resin component containing a dynamically crosslinked product (A) and a polyolefin resin (B), a silicone oil, and a fluororesin. The resin component may optionally contain a dynamically crosslinked product (C) other than the dynamically crosslinked product (A).
[0009] [Dynamic crosslinked body (A)] The dynamically crosslinked material (A) is obtained by kneading and crosslinking raw materials including an ethylene propylene diene rubber (A1), a polyolefin resin (A2) containing 60% by mass or more of structural units based on ethylene, a polyolefin resin (A3) containing 60% by mass or more of structural units based on propylene, and a crosslinking agent (A4).
[0010] Ethylene propylene diene rubber (A1) is a ternary copolymer of ethylene, propylene, and diene. As the diene, 5-ethylidene-2-norbornene, dicyclopentadiene, and 1,4-hexadiene are mainly used. Among them, ethylene propylene diene rubber (A1) is easy to manufacture, so the diene portion of most of the commercially available ethylene propylene diene rubber (A1) is 5-ethylidene-2-norbornene.
[0011] The proportion of units derived from ethylene in all constituent units of the ethylene propylene diene rubber (A1) is preferably 50 to 80 mass%, more preferably 60 to 70 mass%. When the proportion of units derived from ethylene is equal to or more than the lower limit of the preferred range, the abrasion resistance is improved. When the proportion is equal to or less than the upper limit of the preferred range, the processability is improved.
[0012] The proportion of the units derived from propylene in the total constituent units of the ethylene propylene diene rubber (A1) is preferably 15 to 45 mass%, more preferably 25 to 35 mass%. When the proportion of the units derived from propylene is equal to or more than the lower limit of the preferred range, processability is improved. When the proportion is equal to or less than the upper limit of the preferred range, abrasion resistance is improved.
[0013] The ratio of the units derived from diene to all the constituent units of the ethylene propylene diene rubber (A1) is preferably 1 to 20 mass%, more preferably 1 to 11 mass%. When the ratio of the units derived from diene is equal to or more than the lower limit of the preferred range, toughness is improved. When the ratio is equal to or less than the upper limit of the preferred range, processability is improved.
[0014] The Mooney viscosity of the ethylene propylene diene rubber (A1) is preferably 40 to 80, more preferably 50 to 70. When the molecular weight of the ethylene propylene diene rubber (A1) is equal to or higher than the lower limit of the preferred range, the abrasion resistance is improved. When the molecular weight of the ethylene propylene diene rubber (A1) is equal to or lower than the upper limit of the preferred range, the processability is improved. The Mooney viscosity of the ethylene propylene diene rubber (A1) is a viscosity measured at 125° C., with 1 minute of residual heat, and 4 minutes after the rotor started rotating.
[0015] The proportion (mixture amount) of the ethylene propylene diene rubber (A1) to the total mass of the raw materials for obtaining the dynamically crosslinked product (A) is preferably 15 to 40 mass%, more preferably 18 to 30 mass%, and even more preferably 24 to 30 mass%, where the total mass is the total mass of the resin and crosslinking agent contained in the raw materials, and other additives added as necessary (hereinafter the same). When the amount of the ethylene propylene diene rubber (A1) is at least the lower limit of the preferred range, the elongation is improved, and when the amount is at most the upper limit of the preferred range, the processability is improved. The ethylene propylene diene rubber (A1) may be used in combination of two or more kinds.
[0016] The polyolefin resin (A2) is a polyolefin resin containing 60 mass % or more of structural units based on ethylene. The proportion of units derived from ethylene in all structural units of the polyolefin resin (A2) is preferably 60% by mass or more, more preferably 80% by mass or more, and particularly preferably 100% by mass. When the proportion of units derived from ethylene is equal to or more than the lower limit of the preferred range, the abrasion resistance is improved.
[0017] Examples of the structural units other than the ethylene-based structural units constituting the polyolefin resin (A2) include structural units based on propylene and α-olefins (such as 1-butene, 1-octene, or longer chain structural units). These may be contained alone or in combination of two or more.
[0018] The polyolefin resin (A2) may be any of high density polyethylene (HDPE), low density polyethylene (LDPE) and linear low density polyethylene (LLDPE), but since it is a wear-resistant sliding member, high density polyethylene (HDPE) is preferred.
[0019] The melt flow rate (hereinafter referred to as "MFR value") of the polyolefin resin (A2) is preferably 50 g / 10 min or less, more preferably 30 g / 10 min or less. When the MFR value of the polyolefin resin (A2) is equal to or higher than the lower limit of the preferred range, the abrasion resistance is improved. When the MFR value of the polyolefin resin (A2) is equal to or lower than the upper limit of the preferred range, the processability is improved. The MFR value of the polyolefin resin (A2) is the converted mass (g / 10 min) of the resin flowing out of an orifice having a diameter of 2.095 mm and a length of 8,000 mm at 190° C. and a load of 10.0 kg in a cut-off flow tester in accordance with JIS K 7210.
[0020] The proportion (blending amount) of the polyolefin resin (A2) relative to the total mass of the raw materials for obtaining the dynamically crosslinked body (A) is preferably from 25 to 60 mass %, more preferably from 31 to 52 mass %, and even more preferably from 31 to 45 mass %. When the blending amount of the polyolefin resin (A2) is at least the lower limit of the preferred range, the abrasion resistance is improved, and when the blending amount is at most the upper limit of the preferred range, the processability is improved. The polyolefin resin (A2) may be used in combination of two or more kinds.
[0021] The polyolefin resin (A3) is a polyolefin resin containing 60 mass % or more of structural units based on propylene. The proportion of propylene-derived units in all constituent units of the polyolefin resin (A3) is preferably 60% by mass or more, more preferably 80% by mass, and particularly preferably 100% by mass. When the proportion of propylene-derived units is equal to or more than the lower limit of the preferred range, processability is improved.
[0022] Examples of the structural units other than the propylene-based structural units constituting the polyolefin resin (A3) include structural units based on ethylene and α-olefins (1-butene, 1-octene, or longer chains, etc.), which may be contained alone or in combination of two or more kinds. When the polyolefin resin (A3) is a propylene homopolymer, there is no particular limitation on the stereoregularity, and isotactic polypropylene, syndiotactic polypropylene, atactic polypropylene, or a mixture thereof can be appropriately used.
[0023] The MFR value of the polyolefin resin (A3) is preferably 50 g / 10 min or less, more preferably 30 g / 10 min or less. When the MFR value of the polyolefin resin (A3) is equal to or greater than the lower limit of the preferred range, the processability is improved. When the MFR value of the polyolefin resin (A3) is equal to or less than the upper limit of the preferred range, the abrasion resistance is improved. The MFR value of the polyolefin resin (A3) is the converted mass (g / 10 min) of the resin flowing out of an orifice having a diameter of 2.095 mm and a length of 8,000 mm at 230° C. and a load of 2.16 kg in a cut-off flow tester in accordance with JIS K 7210.
[0024] The proportion (blending amount) of the polyolefin resin (A3) relative to the total mass of the raw materials for obtaining the dynamically crosslinked body (A) is preferably from 15 to 40 mass %, more preferably from 20 to 36 mass %, and even more preferably from 29 to 36 mass %. When the blending amount of the polyolefin resin (A3) is at least the lower limit of the preferred range, processability is improved, and when the blending amount is at most the upper limit of the preferred range, abrasion resistance is improved. The polyolefin resin (A3) may be used in combination of two or more kinds.
[0025] Examples of the crosslinking agent (A4) include organic peroxides, hydrosilylation agents (and hydrosilylation catalysts), phenolic resin curing agents, sulfur, sulfur-containing compounds, organic polyamines, metal oxides, etc. Among these, it is preferable to use organic peroxides. Organic peroxides can cause radical crosslinking based on hydrogen abstraction from hydrocarbon moieties such as methyl groups and methylene groups, and therefore can form crosslinked bodies with high viscosity. When forming a crosslinked body using an organic peroxide, it is preferable to use an organosiloxane (hydrosilylation agent) containing a hydrosilyl group (Si-H) in combination, which improves the crosslinking efficiency and prevents "resin burning" during dynamic crosslinking accompanied by heat treatment.
[0026] Suitable organic peroxides include peroxyketals, dialkyl peroxides, peroxyesters, diacyl peroxides, and peroxydicarbonates. Specifically, 1,1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-hexylperoxy)3,3,5-trimethylcyclohexane, 1,1-di(t-butylperoxy)cyclohexane, n-butyl-4,4-di(t-butylperoxy)valerate, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, di(2-t-butylperoxyisopropyl)benzene, t-butylcumyl peroxide, di-t-hexyl Examples of peroxyalkylene oxides include tert-butyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane-3, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-hexyl peroxybenzoate, t-butylperoxy-3-methylbenzoate, diisopropyl peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, and 1,6-bis(t-butylperoxycarbonyloxy)hexane.
[0027] Examples of hydrosilylation agents include silicon hydride compounds such as methylhydrogenpolysiloxane, methylhydrogenalkylmethylpolysiloxane, etc. Examples of hydrosilylation catalysts include platinum-containing catalysts such as hexachloroplatinic acid, platinum chloride, platinum oxide, platinum complexes, etc.
[0028] Phenolic resin curing agents include halogenated phenolic resins such as alkylphenol formaldehyde resins, methylolated alkylphenolic resins, and brominated alkylphenolic resins. In general, non-halogenated phenolic resins are used with a halogen donor such as stannic chloride as a catalyst, and a hydrogen halide scavenger such as zinc oxide. Halogenated phenolic resins are used with a hydrogen halide scavenger, if necessary.
[0029] The proportion (blending amount) of the crosslinking agent (A4) relative to the total mass of the raw materials for obtaining the dynamically crosslinked product (A) is preferably from 1 to 10 mass %, more preferably from 2 to 6 mass %, and even more preferably from 3 to 4 mass %. The degree of crosslinking of the dynamically crosslinked product (A) can be controlled by the amount of the crosslinking agent (A4) added. When the amount of the crosslinking agent (A4) is at least the lower limit of the preferred range, the abrasion resistance is improved, and when the amount is at most the upper limit of the preferred range, the processability is improved. The crosslinking agent (A4) may be used in combination of two or more kinds.
[0030] The raw materials for obtaining the dynamically crosslinked product (A) may contain known additives as appropriate. Examples of the additives include crosslinking assistants.
[0031] The degree of crosslinking of the dynamically crosslinked product (A) is preferably such that the residual ratio after refluxing with hot xylene is 20 to 80%, more preferably 30 to 75%. When the residual ratio is equal to or more than the lower limit of the preferred range, the abrasion resistance is improved. When the residual ratio is equal to or less than the upper limit of the preferred range, the processability is improved. The residual ratio mainly reflects the content of crosslinked bodies and the degree of crosslinking. In other words, the higher the residual ratio, the higher the content of crosslinked bodies and the higher the degree of crosslinking. The residual ratio can be measured by the following "Method for measuring residual ratio by hot xylene reflux".
[0032] "Method for measuring the residue ratio by refluxing hot xylene" Approximately 3 g of a sample of the dynamically crosslinked product (A) is weighed to obtain an accurate weight (W1). The sample is placed in a cylindrical filter paper, set in a Soxhlet extractor, and refluxed with xylene for 6 hours. After extraction, the filter paper containing the sample is taken out and placed on a hot plate at 120°C for 5 hours to thoroughly evaporate the xylene. After cooling, the accurate weight (W2) of the sample is measured. The heating time for evaporation is appropriately adjusted so that the xylene evaporates and the sample weight is sufficiently stabilized. For example, if the heating time is 5 hours, if the rate of change in the "residual ratio % due to hot xylene reflux" between 5 hours of heating and another 5 hours of heating (total of 10 hours) is within the range of +5% to -8%, the heating time of 5 hours is deemed appropriate. If the rate of change is large, the heating time is extended so that the rate of change is within the range of +5% to -8% compared to the first 5 hours of heating. The "residual ratio due to hot xylene reflux" is calculated as 100 x W2 / W1.
[0033] Dynamic crosslinked material (A) shear rate-melt viscosity measurement at 200°C and a shear rate of 121.6 sec -1 The viscosity is preferably 300 to 3,000 Pa·s, and more preferably 800 to 2,500 Pa·s. When the viscosity is equal to or higher than the lower limit of the preferred range, processability is improved. When the viscosity is equal to or lower than the upper limit of the preferred range, abrasion resistance is improved.
[0034] The dynamically crosslinked material (A) may be used alone or in combination of two or more kinds. In the composition for sliding members of the present invention, the proportion (blending amount) of the dynamically crosslinked material (A) in the total mass of the resin components is 50 to 92 mass%, preferably 55 to 87 mass%, and more preferably 60 to 82 mass%. When the content of the dynamically crosslinked material (A) is 50% by mass or more, the abrasion resistance is improved, and when the content is 92% by mass or less, the processability is improved.
[0035] [Polyolefin resin (B)] The polyolefin resin (B) is preferably a polyolefin resin (B1) containing 60% by mass or more of structural units based on ethylene, or a polyolefin resin (B2) containing 60% by mass or more of structural units based on propylene, and it is more preferable to use polyolefin resin (B1) and polyolefin resin (B2) in combination.
[0036] The polyolefin resin (B1) may be the same as the polyolefin resin (A2) described above, and the preferred embodiments are also the same. The polyolefin resin (B2) may be the same as the polyolefin resin (A3) described above, and the preferred embodiments are also the same. The polyolefin resin (B) may be used alone or in combination of two or more kinds.
[0037] In the composition for sliding members of the present invention, the proportion (blending amount) of the polyolefin resin (B) in the total mass of the resin components is 8 to 50 mass%, preferably 13 to 45 mass%, and more preferably 18 to 40 mass%. When the blending amount of the polyolefin resin (B) is 8% by mass or more, the moldability of the composition for a sliding member is improved, and when it is 50% by mass or less, the wear resistance is improved.
[0038] [Thermoplastic elastomer (C)] The composition for a sliding member of the present invention may contain a thermoplastic elastomer (C) other than the dynamically crosslinked product (A) as a resin component. Examples of the thermoplastic elastomer (C) include styrene-based thermoplastic elastomers and dynamically crosslinked olefin-based thermoplastic elastomers. Styrene-based thermoplastic elastomers have a hard segment of polystyrene, and depending on the soft segment, they are broadly classified into SBS (S: styrene, B: butadiene), SIS (I: isoprene), and hydrogenated versions of these, such as SEBS (E: ethylene, B: butylene), SEPS (P: propylene), etc. Among these, SEBS (hydrogenated TPS) is preferred due to its superior abrasion resistance. Dynamically crosslinked olefin-based thermoplastic elastomers are advantageous in terms of moldability and surface sliding properties, and therefore preferably have a structure in which EPDM crosslinked particles are dispersed in an olefin-based resin. The thermoplastic elastomer (C) may be used alone or in combination of two or more kinds.
[0039] In the composition for sliding member of the present invention, the proportion (blended amount) of the thermoplastic elastomer (C) in the total mass of the resin components is preferably 0 to 10 mass %, more preferably 2 to 8 mass %. By making the blending amount of the thermoplastic elastomer (C) 2% by mass or more, an improvement in elongation can be expected, and by making it 10% by mass or less, the sliding property is improved.
[0040] [Other resin components] The composition for a sliding member of the present invention may contain, as a resin component, other resin components than the dynamically crosslinked product (A), the polyolefin resin (B), and the thermoplastic elastomer (C) within a range that does not impair the effects of the present invention.
[0041] [Silicone oil] Examples of silicone oils include straight silicone oils and modified silicone oils in which organic groups have been introduced into the side chains or ends. Examples of straight silicone oils include dimethyl silicone oil, methyl phenyl silicone oil, and methyl hydrogen silicone oil.
[0042] Modified silicone oils are classified into side chain type, both end type, one end type, and side chain both end type depending on the bonding position of the substituted organic group. Modified silicone oils are also classified into reactive silicone oils and non-reactive silicone oils depending on the nature of the organic groups introduced.
[0043] Examples of reactive silicone oils include various modified types of reactive silicone oils such as amino-modified, epoxy-modified, carboxy-modified, carbinol-modified, methacryl-modified, mercapto-modified, phenol-modified, and heterogeneous functional group-modified. Examples of non-reactive silicone oils include reactive silicone oils of various modified types, such as polyether-modified, methylstyryl-modified, alkyl-modified, higher fatty acid ester-modified, specially hydrophilic modified, higher fatty acid-containing, and fluorine-modified.
[0044] As the silicone oil used in the composition for a sliding member of the present invention, straight silicone oil is preferred, and dimethyl silicone oil is more preferred, because of its superior chemical stability. The silicone oil may be used alone or in combination of two or more kinds.
[0045] The dynamic viscosity of the silicone oil used in the composition for sliding members of the present invention is 10 to 10 6 mPa·s is preferable, and 10 2 ~10 5 It is more preferable that the dynamic viscosity of the silicone oil is equal to or higher than the lower limit of the preferred range, thereby improving the long-term sliding properties. It is more preferable that the dynamic viscosity of the silicone oil is equal to or lower than the upper limit of the preferred range, thereby reducing the initial coefficient of friction. In this specification, the dynamic viscosity is a viscosity measured at 25°C using a Brookfield viscometer.
[0046] The molecular weight of the silicone oil used in the composition for a sliding member of the present invention is preferably 1000 to 15000, and more preferably 6000 to 100000. When the molecular weight of the silicone oil is within the preferred range, the dynamic viscosity of the silicone oil can be easily adjusted to the preferred range described above. The molecular weight of the silicone oil is measured by gel permeation chromatography using polystyrene standard polymer as a reference.
[0047] The composition for a sliding member of the present invention contains 5 to 20 parts by mass of silicone oil per 100 parts by mass of the resin component. The composition for a sliding member of the present invention contains preferably 6 to 16 parts by mass, more preferably 7 to 13 parts by mass of silicone oil per 100 parts by mass of the resin component. By including 5 parts by mass or more of silicone oil per 100 parts by mass of the resin component, the long-term sliding properties are improved. By including 20% by mass or less of silicone oil, bleeding out of the silicone oil is easily suppressed.
[0048] [Fluororesin] Examples of fluororesins include homopolymers and copolymers of polytetrafluoroethylene, perfluoroalkoxyalkane, perfluoroethylenepropene copolymer, ethylene-tetrafluoroethylene copolymer, polyvinylidene fluoride, polychlorotrifluoroethylene, polyvinyl fluoride, etc. Among these, polytetrafluoroethylene is preferred because it is a resin having self-lubricating properties. Two or more types of fluororesins may be used in combination.
[0049] The average particle size of the fluororesin is preferably 50 μm or less, and more preferably 3 to 25 μm. When the average particle size of the fluororesin is equal to or greater than the lower limit of the preferred range, the initial sliding resistance is likely to decrease, and when the average particle size is equal to or less than the upper limit of the preferred range, long-term sliding properties are likely to be ensured. The average particle size of the fluororesin is the volume-based median diameter (D50) measured by a laser diffraction / scattering method.
[0050] The composition for a sliding member of the present invention contains 1 to 22 parts by mass of a fluororesin relative to 100 parts by mass of a resin component. The composition for a sliding member of the present invention contains preferably 3 to 22 parts by mass, more preferably 3 to 19 parts by mass of a fluororesin relative to 100 parts by mass of a resin component. By including 3 parts by mass or more of fluororesin per 100 parts by mass of the resin component, the increase in the coefficient of sliding resistance can be suppressed, the effect of improving long-term sliding properties (durability) can be obtained, and the coefficient of friction after a heated sliding test can be kept low. By keeping the content of fluororesin at 22% by mass or less, processability is improved.
[0051] [Additives] The composition for a sliding member of the present invention may contain other additives as appropriate, such as reinforcing agents such as pigments, silica, and carbon black, antioxidants, weather resistance improvers, thermoplastic resins, elastomers, antifungal agents, antibacterial agents, flame retardants, softeners such as paraffin-based agents, and lubricants. The amount of other additives to be added may be, for example, 0.1 to 10 parts by mass per 100 parts by mass of the resin component, taking into consideration the effect on sliding properties.
[0052] [Structure of the composition for sliding members] In the composition for a sliding member, the dynamically crosslinked material (A) forms domains and has a structure in which it is dispersed in a matrix containing the polyolefin resin (B).
[0053] Microscopic gaps are generated between the dynamically crosslinked material (A) and the matrix due to the difference in physical properties between the two. It is considered that the silicone oil in the composition for sliding members fills the gap between the dynamically crosslinked body (A) and the matrix, thereby suppressing bleeding out. It is also considered that the silicone oil dispersed and exposed on the surface of the composition for sliding members improves the sliding properties of the composition for sliding members.
[0054] On the other hand, the solid fluororesin is dispersed throughout the matrix, not in the gaps. Since the fluororesin has a small cohesive force, it can maintain a good dispersion state in the matrix, which is thought to suppress partial aggregation. In addition, the fluororesin dispersed and exposed on the surface of the composition for sliding member is thought to improve the slidability of the composition for sliding member.
[0055] When the composition for a sliding member is extruded from an extruder, the average particle size of the domains in a cross section parallel to the extrusion direction is preferably 0.5 to 50 μm, and more preferably 1 to 30 μm. By setting the average particle size of the domains to be equal to or larger than the lower limit of the preferred range, it is easy to suppress the bleeding out of the silicone oil, and by setting the average particle size of the domains to be equal to or smaller than the upper limit of the preferred range, it is easy to improve the mechanical properties.
[0056] The average grain size of the domains can be calculated by taking an electron micrograph of the cross section in an area of 0.5 x 0.5 mm, calculating the grain size of each domain by image processing, and then calculating the overall average. Here, the grain size of the domain is the diameter calculated by converting the observed domain area into a perfect circle.
[0057] [Physical Properties of Composition for Sliding Member] The MFR value of the composition for sliding member of the present invention is preferably 2 to 41 g / 10 min, more preferably 7 to 36 g / 10 min, and further preferably 12 to 31 g / 10 min. When the MFR value is equal to or higher than the lower limit of the preferred range, melt fracture is easily suppressed. When the MFR value is equal to or lower than the upper limit of the preferred range, processability is improved. The MFR value of the composition for sliding members is the converted mass (g / 10 min) of the resin flowing out of an orifice having a diameter of 2.095 mm and a length of 8,000 mm at 230° C. under a load of 5.00 kg in a cut-off flow tester in accordance with JIS K 7210.
[0058] The hardness (Shore D) of the composition for sliding member of the present invention is preferably 35 to 60, more preferably 40 to 57, and even more preferably 45 to 55. When the hardness is equal to or higher than the lower limit of the preferred range, the sliding properties are likely to be improved. When the hardness is equal to or lower than the upper limit of the preferred range, the handleability of the molded product is improved. In this specification, the hardness is a durometer hardness measured in accordance with JIS K 6253.
[0059] The breaking strength of the composition for a sliding member of the present invention is preferably 3 MPa or more, more preferably 5 MPa or more, and even more preferably 10 MPa or more. If the breaking strength is equal to or more than the lower limit of the preferred range, the handleability of the molded product is improved. In this specification, the breaking strength is a tensile property value measured in accordance with JIS K 6251.
[0060] The elongation at break of the composition for use in a sliding member of the present invention is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more. When the elongation at break is equal to or more than the lower limit of the preferred range, the handleability of the molded product is improved. In this specification, the elongation at break is a tensile property value measured in accordance with JIS K 6251.
[0061] The composition for a sliding member of the present invention can provide a sliding member which has low dynamic and static friction coefficients, which are unlikely to increase even after heating, and which maintains its sliding properties for a long period of time.
[0062] <Method of producing the composition for sliding member> The method for producing a composition for a sliding member of the present invention includes a dynamic crosslinking step and a mixing step.
[0063] [Dynamic crosslinking process] The dynamic crosslinking step is a step of obtaining a dynamically crosslinked body (A) by crosslinking raw materials containing an ethylene propylene diene rubber (A1), a polyolefin resin (A2), a polyolefin resin (A3), and a crosslinking agent (A4) while kneading them.
[0064] The specific method of the dynamic crosslinking step is not particularly limited as long as it is a method that can crosslink the ethylene propylene diene rubber (A1), the polyolefin resin (A2), and the polyolefin resin (A3) in the raw materials while kneading, and a known dynamic crosslinking method for producing TPV can be adopted. For example, the raw materials can be dynamically crosslinked by kneading them in a twin-screw extruder and heating them as necessary. The crosslinked TPV formed by dynamic crosslinking can be obtained in the form of pellets, for example.
[0065] [Mixing process] The mixing step is a step of mixing the dynamically crosslinked material (A), resin components other than the dynamically crosslinked material (A) (including at least the polyolefin resin (B)), silicone oil, fluororesin, and other additives added as necessary.
[0066] The mixing method is not particularly limited, and a general method for kneading a resin composition can be adopted. For example, a mixing method using a kneader such as a twin screw extruder, a single screw extruder, a kneader, or a Banbury mixer can be used. The composition for a sliding member formed by mixing can be obtained in the form of, for example, pellets.
[0067] <Sliding parts> The sliding member of the present invention is a sliding member formed from the composition for a sliding member of the present invention. An example of an application of a sliding member is a weatherstrip 10 shown in Fig. 1. The weatherstrip 10 is composed of a weatherstrip main body 20 and a sliding member 30 made of the above-mentioned composition for sliding members. The weatherstrip main body 20 is composed of a base 20a, sidewalls 20b on both sides, and lip portions 20c extending inward from the tips of the sidewalls 20b, and the sliding member 30 is formed so as to cover the sliding contact portion of the lip portion 20c that comes into sliding contact with the window glass 18 and the surface of the base 20a that comes into sliding contact with the outer peripheral edge face of the window glass 18. In the weatherstrip 10, since a sliding member made of the composition for sliding member of the present invention is used, bleeding of the silicone compound is reduced, and the deterioration of sliding properties after sliding in a high-temperature environment is reduced. Therefore, even when wet with water, a stable low sliding resistance is maintained, and the generation of abnormal noise is also suppressed. EXAMPLES
[0068] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the description of these examples.
[0069] <Raw materials> Details of the raw materials used in each of the examples and comparative examples are as follows. "EPDM": Ethylene-propylene-diene rubber manufactured by Mitsui Chemicals, product name: Mitsui EPT (grade: 3092PM) "PE": Polyethylene homopolymer manufactured by Prime Polymer, product name: Hi-Zex (grade: 2200J) "PP": Polypropylene homopolymer manufactured by Japan Polypropylene Corporation, product name: Novatec PP (grade: MA3H) "Cross-linking agent": NOF Corporation, organic peroxide (cross-linking agent), product name: Perhexa (grade: 25B) "TPE": Dynamic crosslinking olefin-based thermoplastic elastomer manufactured by JSR Corporation, product name: Excellink (grade: 1300B) "Silicone oil": Silicone oil manufactured by Shin-Etsu Chemical Co., Ltd., dynamic viscosity 10,000 mPa·s, molecular weight 60,000 (grade: KF96) "PTFE (1)": Kitamura Co., Ltd., polytetrafluoroethylene resin, product name: KTL (grade: 450), average particle size 22 μm "PTFE (2)": Kitamura Co., Ltd., polytetrafluoroethylene resin, product name: KTL (grade: 620), average particle size 11 μm "PTFE (3)": Kitamura Co., Ltd., polytetrafluoroethylene resin, product name: KTL (grade: 8FH, average particle size 3.5 μm)
[0070] <Preparation of Composition for Sliding Member> Among "Material 1" in Tables 1 to 4, EPDM, PE, and PP were kneaded in the amounts (parts by mass) listed in each table using a Banbury mixer, and pellets were made by passing through a rudder. Next, the pellets and the amount (parts by mass) of a crosslinking agent listed in "Material 1" in each table were put into a twin-screw extruder, and dynamic crosslinking was performed by crosslinking while kneading, to obtain pellets of the dynamically crosslinked body (A). Pellets of the dynamically crosslinked body (A) and the amounts (parts by mass) of PE, PP, and TPE listed in "Material 2" in each table, and the amount (parts by mass) of PTFE listed in "Material 3" in each table were fed into a twin-screw extruder and kneaded, while injecting silicone oil in the amount (parts by mass) listed in "Material 3" in each table from the middle part of the twin-screw extruder using a metering pump and kneading, to prepare pellets of the composition for sliding members of each example. Note that blank spaces in the table indicate that the material was not added.
[0071] 2 to 4 show fluorine atom concentration distribution diagrams of the pellets of the compositions for the sliding member of Example 1, Example 2, and Comparative Example 2. In Figures 2 to 4, (a) is an image of the surface vicinity of a cross section obtained by cutting the middle part of a pellet with a microtome in the direction perpendicular to the extrusion direction, taken with an electron probe microanalyzer (EPMA). (b) is an image of the pellet surface taken with an electron probe microanalyzer (EPMA).
[0072] 2 to 4, the white areas (eg, areas marked with the symbol F) are areas where fluorine atoms were detected. 2 and 3, fluorine atoms were dispersed evenly throughout in Examples 1 and 2. No fluorine atoms were observed in Comparative Example 2, in which no fluororesin was added.
[0073] <Physical Properties of Composition for Sliding Member> The compositions for sliding members of each example were measured for MFR (unit: g / 10 min), hardness, breaking strength (unit: MPa), and elongation at break (unit: %). The results are shown in 1 to 4.
[0074] <Production of two-layer molded products> Two extruders were connected to a flat two-layer molding die, and a commercially available olefin-based TPV (Milastomer, manufactured by Mitsui Chemicals, Inc.) serving as a base material was extruded from one extruder, and each example of a sliding member composition was extruded from the other extruder, to obtain a two-layer molded product consisting of a base and a sliding member layer laminated on the base. The thickness of the base layer of the two-layer molded product was approximately 2 mm, and the thickness of the sliding material layer was 170±70 μm.
[0075] <Sliding test> The two-layer molded product was used as a sample and fixed with a jig so that the part coated with the sliding material layer was flexible. This was fixed to a sliding tester, and a load of 17 N was applied to the sample. A glass plate (length 50 mm) was moved horizontally (average 150 mm / sec) while driving the motor, and the sliding material layer of the two-layer molded product was slid 5,000 times with the glass plate. After that, the static friction coefficient and dynamic friction coefficient were measured with a HEIDON friction and wear tester manufactured by Shinto Scientific Co., Ltd. Tables 1 to 4 show the results of measurements taken in a room temperature environment of 25°C (before heat sliding), and the results of measurements taken after the sample was left to stand for 60 minutes in a heated environment of 80°C, sliding was performed after the sample reached 80°C, and then the sample was cooled to 25°C and then measured (after heat sliding).
[0076] In addition, the sliding resistance value was measured using a load cell when the sliding member layer of the two-layer molded product was slid against the glass plate using a sliding tester. The measured values immediately after the start (initial value), 2,500 times, 5,000 times, and 10,000 times of sliding were taken as the sliding resistance coefficient, and the extent to which the sliding resistance changed depending on the number of times of sliding was measured. The results are shown in Tables 1 to 4.
[0077] [Table 1]
[0078] [Table 2]
[0079] [Table 3]
[0080] [Table 4]
[0081] As described above, the composition for a sliding member according to the present invention not only exhibits excellent sliding properties before sliding in a high-temperature environment, but also reduces deterioration of the sliding properties after sliding in a high-temperature environment. In addition, the composition also exhibits excellent long-term sliding properties. On the other hand, the compositions for sliding members of Comparative Examples 1 and 2, which did not contain a fluororesin, had a large dynamic friction coefficient before sliding in a high-temperature environment, and the sliding properties were significantly deteriorated after sliding in a high-temperature environment. In addition, the sliding properties did not last for a long time. In addition, in Comparative Example 3, which contained an excessive amount of fluororesin, pelletization was not possible. [Explanation of symbols]
[0082] 10...weather strip, 20...weather strip main body, 30...sliding member 18…Window glass
Claims
1. A resin component including a dynamically crosslinked body (A) and a polyolefin resin (B) (but not including silicone oil or fluororesin; the same applies below), a silicone oil, and a fluororesin, The dynamically crosslinked body (A) is obtained by kneading and crosslinking raw materials including an ethylene propylene diene rubber (A1), a polyolefin resin (A2) containing 60 mass% or more of structural units based on ethylene, a polyolefin resin (A3) containing 60 mass% or more of structural units based on propylene, and a crosslinking agent (A4), a ratio of the dynamically crosslinked body (A) to the total mass of the resin components is 50 to 92 mass%, and a ratio of the polyolefin resin (B) to the total mass of the resin components is 8 to 50 mass%, The composition for a sliding member comprises 5 to 20 parts by mass of the silicone oil and 1 to 22 parts by mass of the fluororesin relative to 100 parts by mass of the resin component.
2. 2. The composition for a sliding member according to claim 1, wherein a ratio of the ethylene propylene diene rubber (A1) to a total mass of raw materials for obtaining the dynamically crosslinked body (A) is 15 to 40 mass%, a ratio of the polyolefin resin (A2) to a total mass of 25 to 60 mass%, a ratio of the polyolefin resin (A3) to a total mass of 15 to 40 mass%, and a ratio of the crosslinking agent (A4) to a total mass of 1 to 10 mass%.
3. 3. The composition for a sliding member according to claim 1, wherein the fluororesin has an average particle size of 50 μm or less.
4. The composition for a sliding member according to any one of claims 1 to 3, wherein the dynamically crosslinked product (A) forms domains and is dispersed in a matrix containing the polyolefin resin (B).
5. A method for producing the composition for a sliding member according to any one of claims 1 to 4, comprising the steps of: a dynamic crosslinking step of kneading and crosslinking raw materials containing the ethylene propylene diene rubber (A1), the polyolefin resin (A2), the polyolefin resin (A3), and the crosslinking agent (A4) to obtain the dynamically crosslinked body (A); a mixing step of mixing the dynamically crosslinked product (A) obtained, the resin component other than the dynamically crosslinked product (A), the silicone oil, and the fluororesin.
6. A sliding member formed from the composition for a sliding member according to any one of claims 1 to 4.
Citation Information
Patent Citations
Kakusantenshashashinkamera
JP1976067128A
Polyolefin resin composition for skinning member and its laminate
JP1997176408A
Resin composition for facing member and laminate containing the same
JP2000095900A
Thermoplastic elastomer composition
JP2002294002A
Olefinic thermoplastic elastomer and its molded product
JP2003155387A