Method for producing titanium-based sintered body, and titanium-based sintered body
A two-stage mixing and pressing process uniformly disperses ceramic precipitates in a titanium alloy matrix, enhancing mechanical properties and durability of titanium-based sintered bodies.
Patent Information
- Application Number
- JP2023006375
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-01-19
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-01-19
AI Technical Summary
Existing methods for producing titanium-based sintered bodies face challenges in uniformly dispersing fine ceramic precipitates in a titanium alloy matrix, leading to variations in mechanical properties and potential local damage.
A two-stage mixing process involving a ball mill or attritor for ceramic powder and a V-type mixer for titanium alloy powders, followed by cold isostatic pressing and hot isostatic pressing, ensures uniform dispersion of ceramic-derived precipitates in a titanium alloy matrix, enhancing mechanical properties.
The method produces a titanium-based sintered body with uniformly dispersed precipitates, improving mechanical properties and reducing local damage, resulting in a more robust and long-lasting material.
Smart Images

Figure 0007561894000003 
Figure 0007561894000004 
Figure 0007561894000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a titanium-based sintered body, and a titanium-based sintered body. [Background technology]
[0002] Titanium alloys containing titanium have excellent mechanical properties, and therefore titanium-based ingots and sintered bodies made of titanium alloys are used in the components of various machines.
[0003] Patent Document 1 discloses a method for producing a sintered powder impeller, in which raw material powder containing metal and ceramic powders is pressure-molded to produce a molded body, and the molded body is sintered to produce a sintered powder impeller. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 8-120307 Summary of the Invention [Problem to be solved by the invention]
[0005] The powder sintered impeller described in Patent Document 1 has a structure known as a metal matrix composite (hereinafter, MMC). MMC has a matrix containing a metal and a plurality of precipitates dispersed in the matrix. The precipitates are compounds derived from ceramic powder.
[0006] In MMC, it is difficult to uniformly disperse fine precipitates in the matrix, and the uneven distribution of precipitates in the matrix reduces the mechanical properties of the MMC.
[0007] An object of the present disclosure is to provide a method for producing a titanium-based sintered body, which is capable of producing a titanium-based sintered body in which a plurality of precipitates are uniformly dispersed in a matrix. [Means for solving the problem]
[0008] The method for producing a titanium-based sintered body according to the present disclosure includes the steps of: mixing the first powder and the ceramic powder to prepare a mixed powder; mixing the mixed powder with a second powder to prepare a raw material powder; A step of press-molding the raw material powder to produce a powder compact; and a step of sintering the powder compact to produce a titanium-based sintered body. The combination of the first powder and the second powder is the following (A) or (B). (A) The first powder is a powder composed of titanium or a titanium alloy, and the second powder is a powder containing an element capable of alloying with titanium. (B) The second powder is a powder constituted by titanium or a titanium alloy, and the first powder is a powder containing an element capable of alloying with titanium. Effect of the Invention
[0009] The method for producing a titanium-based sintered body according to the present disclosure can produce a titanium-based sintered body in which a plurality of precipitates are uniformly dispersed in the matrix. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a flow chart showing steps of a method for producing a titanium-based sintered body according to an embodiment. [Diagram 2] FIG. 2 is a graph showing the test results of Sample No. 21 described in Test Example 2. [Diagram 3] FIG. 3 is a graph showing the test results of Sample No. 22 described in Test Example 2. [Figure 4] FIG. 4 is a cross-sectional photograph of the titanium-based sintered body of Sample No. 31 described in Test Example 3. [Diagram 5] FIG. 5 is a cross-sectional photograph of the titanium-based sintered body of Sample No. 32 described in Test Example 3. [Figure 6] FIG. 6 is a cross-sectional photograph of the titanium-based sintered body of Sample No. 33 described in Test Example 3. [Figure 7] FIG. 7 is a cross-sectional photograph of the titanium-based sintered body of Sample No. 34 described in Test Example 3. [Figure 8] FIG. 8 is a cross-sectional photograph of the titanium-based sintered body of Sample No. 35 described in Test Example 3. [Figure 9] FIG. 9 is a schematic diagram showing a test piece for the tensile test described in Test Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described.
[0012] <1> The method for producing a titanium-based sintered body according to the present disclosure includes the steps of: mixing the first powder and the ceramic powder to prepare a mixed powder; mixing the mixed powder with a second powder to prepare a raw material powder; A step of press-molding the raw material powder to produce a powder compact; and a step of sintering the powder compact to produce a titanium-based sintered body. The combination of the first powder and the second powder is the following (A) or (B). (A) The first powder is a powder composed of titanium or a titanium alloy, and the second powder is a powder containing an element capable of alloying with titanium. (B) The second powder is a powder constituted by titanium or a titanium alloy, and the first powder is a powder containing an element capable of alloying with titanium.
[0013] By mixing ceramic powder with the raw powder, a titanium-based sintered body consisting of a metal matrix composite (MMC) with a structure in which compounds derived from the ceramic powder are precipitated in a titanium alloy matrix can be obtained. MMCs are lightweight and have excellent heat resistance and wear resistance.
[0014] In the above manufacturing method, the raw material powder is composed of multiple types of powder, and the mixing is divided into two stages. By mixing multiple types of powder in stages in this way, multiple fine precipitates are uniformly dispersed in the matrix of the titanium-based sintered body. In addition, by producing a powder compact using the raw material powder in which multiple types of powder are mixed in stages, the relative density of the titanium-based sintered body obtained by sintering the powder compact can be dramatically improved.
[0015] <2> the above <1> In the method for producing a titanium-based sintered body described in The first powder is made of an alloy containing aluminum and vanadium, The second powder may be comprised of titanium.
[0016] the above <2> According to the method for producing a titanium-based sintered body described in the above, the matrix of the titanium-based sintered body is made of a titanium alloy containing titanium (Ti), aluminum (Al) and vanadium (V). The titanium alloy is, for example, Ti-6Al-4V, so-called 64 titanium. 64 titanium has extremely excellent strength.
[0017] <3> the above <1> In the method for producing a titanium-based sintered body described in The first powder is composed of titanium, The second powder may be made of an alloy containing aluminum and vanadium.
[0018] the above <3> According to the method for producing a titanium-based sintered body described in the above, the matrix of the titanium-based sintered body is made of a titanium alloy containing Ti, Al, and V. The titanium alloy is, for example, titanium 64. Titanium 64 has extremely excellent strength.
[0019] <4> the above <1> from <3> 2. The method for producing a titanium-based sintered body according to claim 1, The ceramic powder may be comprised of titanium diboride.
[0020] Titanium diboride (TiB2) precipitates as titanium boride (TiB) in titanium-based sintered bodies. Titanium-based sintered bodies containing titanium boride as a precipitate are lightweight and have excellent wear resistance and heat resistance.
[0021] <5> the above <1> from <4> In the method for producing a titanium-based sintered body described in The first powder and the ceramic powder may be mixed using a ball mill, an attritor, or a jet mill.
[0022] The ball mill, the attritor, and the jet mill can mix the first powder and the ceramic powder while applying a large stress to the ceramic powder. Therefore, the ceramic powder is easily dispersed uniformly in a fine state in the mixed powder. As a result, the ceramic-derived precipitates are easily dispersed uniformly in the matrix of the titanium-based sintered body.
[0023] <6> the above <1> from <5> 2. The method for producing a titanium-based sintered body according to claim 1, The mixed powder and the second powder may be mixed by a V-type mixer.
[0024] The V-type mixer can mix the mixed powder and the second powder uniformly. The first powder and the second powder contained in the mixed powder form a matrix titanium alloy. Therefore, by uniformly mixing the mixed powder and the second powder, a homogeneous matrix is easily obtained.
[0025] <7> the above <1> from <6> 2. The method for producing a titanium-based sintered body according to claim 1, In the step of producing the powder compact, the powder compact may be manufactured by cold isostatic pressing.
[0026] Because the cold isostatic press mold is not made of metal, the titanium contained in the raw powder does not stick to the mold, making it easier to increase the pressure and increase the density of the green compact.
[0027] <8> the above <1> from <7> 2. The method for producing a titanium-based sintered body according to claim 1, The method may further include a step of compressing the titanium-based sintered body by hot isostatic pressing.
[0028] Hot isostatic pressing further increases the density of the titanium-based sintered body, improving the strength of the titanium-based sintered body.
[0029] <9> The titanium-based sintered body of the present disclosure is A matrix including titanium; A plurality of precipitates are formed from a compound derived from a ceramic powder and dispersed in the matrix; The average value R0, the maximum value R1, and the minimum value R2 of the plurality of abundance ratios obtained from each of 50 or more different measurement ranges in the cross section satisfy the following formula, R1≦R0+4.5 R2≧R0-4.5 Each of the multiple presence ratios is an area ratio of the multiple precipitates when the total area of the matrix and the multiple precipitates in each of the multiple measurement ranges is taken as 100%.
[0030] The titanium-based sintered body of the present disclosure is typically an MMC having a structure in which ceramic precipitates are precipitated in a titanium alloy matrix. MMCs are lightweight and have excellent heat resistance and wear resistance.
[0031] The units for the average value R0, maximum value R1, and minimum value R2 are % (percent). That is, R1≦R0+4.5 means that the maximum value R1 is the average value R0 plus 4.5% or less, and R2≧R0-4.5 means that the minimum value R2 is the average value R0 minus 4.5% or more. For example, if the average value R0 is 10%, the maximum value R1 is 14.5% or less, and the minimum value R2 is 5.5% or more. The fact that the maximum value R1 and minimum value R2 of the precipitate abundance ratio satisfy the above formula means that the abundance ratio in each measurement range does not deviate significantly from the average value R0. In other words, the above formula specifies that there is little variation in the precipitate abundance ratio in multiple measurement ranges. of Therefore, in the titanium-based sintered body of the present disclosure, a plurality of precipitates are uniformly dispersed throughout the entire area of the titanium-based sintered body. Therefore, the mechanical properties of the entire titanium-based sintered body are uniform. Such a titanium-based sintered body is less likely to be locally damaged during use and has a long life.
[0032] <10> the above <9> In the titanium-based sintered body described in The matrix may be made of an alloy containing titanium, aluminum and vanadium.
[0033] Titanium alloys containing Ti, Al and V have excellent strength. An example of such a titanium alloy is titanium 64. Titanium 64 has extremely excellent strength.
[0034] <11> the above <9> or <10> In the titanium-based sintered body described in The precipitate may be constituted by titanium boride.
[0035] Titanium boride improves the heat resistance and wear resistance of the titanium-based sintered body.
[0036] [Details of the embodiment of the present disclosure] Hereinafter, specific examples of the manufacturing method of the titanium-based sintered body of the present disclosure will be described with reference to the drawings. The same reference numerals in the drawings indicate the same or corresponding parts. The size of the members shown in each drawing is expressed for the purpose of clarifying the description, and does not necessarily represent the actual size. Note that the present invention is not limited to these examples, but is indicated by the claims, and it is intended to include all modifications within the meaning and scope equivalent to the claims.
[0037] <Embodiment 1> As shown in the flow chart of FIG. 1, the method for producing a titanium-based sintered body according to the embodiment includes the following steps. First mixing step Second mixing process The process of compressing and molding the raw powder - A process for cutting powder compacts Lubricant removal process - Sintering the powder compact - A process of compressing titanium-based sintered bodies using hot isostatic presses. Finishing process Each step will be described in detail below.
[0038] <First mixing process> In the first mixing step, a first powder and a ceramic powder are mixed among a plurality of kinds of raw powders to prepare a mixed powder. The first powder may be a powder made of pure titanium or a powder made of a titanium alloy. The first powder may be a powder containing a first element that can be alloyed with titanium. The first element is, for example, aluminum (Al), vanadium (V), tin (Sn), chromium (Cr), molybdenum (Mo), or zirconium (Zr). The first element is appropriately selected depending on the composition of the titanium-based sintered body to be prepared. An example of the first powder containing the first element is Al-V powder made of a compound of aluminum and vanadium. The ceramic powder is, for example, titanium diboride (TiB2).
[0039] The first mixing step of mixing the first powder and the ceramic powder can be carried out, for example, by a ball mill, an attritor, or a jet mill. By mixing two or more types of powder including the ceramic powder by a method of applying high energy, the ceramic powder can be easily dispersed finely.
[0040] <Second mixing process> In the second mixing step, the mixed powder obtained in the first mixing step is mixed with a second powder to produce a raw material powder. The second powder may be a powder made of pure titanium, a powder made of a titanium alloy, or a powder containing the first element. Here, when the first powder is a powder made of titanium or a titanium alloy, the second powder is a powder containing the first element. When the first powder is a powder containing the first element, the second powder is a powder made of titanium or a titanium alloy.
[0041] The second mixing step of mixing the mixed powder and the second powder can be carried out, for example, by a V-type mixer. The V-type mixer has excellent powder mixing ability. Therefore, the mixed powder and the second powder are mixed uniformly. The mixing method using the V-type mixer is a mixing method in which the energy given to the raw material powder is relatively low.
[0042] The particle size of the raw material powder, i.e., the particle size of the first powder, the particle size of the second powder, and the particle size of the ceramic powder, is, for example, 0.1 μm or more and 100 μm or less. When the fine raw material powder is pressure-molded, air is likely to be trapped in the gaps between the particles constituting the powder compact, and the oxygen concentration of the powder compact is likely to be high. The oxygen contained in the powder compact may deteriorate the mechanical properties of the titanium-based sintered body obtained by sintering the powder compact. If the particle size of the raw material powder is 0.1 μm or more, aggregation during mixing can be suppressed. If the particle size of the raw material powder is 100 μm or less, the density of the powder compact and the titanium-based sintered body is likely to be high. The particle size of the raw material powder may be, for example, 0.5 μm or more and 90 μm or less.
[0043] In the second mixing step, a lubricant may be further mixed with the mixed powder and the second powder. The lubricant improves the cutting workability of the green compact. If the green compact is not cut, it is not necessary to include a lubricant in the green compact. The lubricant is, for example, stearic acid, zinc stearate, stearic acid amide, or ethylene bis-stearic acid amide.
[0044] The amount of lubricant mixed with respect to the raw material powder is, for example, 0.05% by mass or more and 0.5% by mass or less when the raw material powder is 100% by mass. If the amount of lubricant mixed with respect to 100% by mass of the raw material powder is 0.05% by mass or more, the powder compact can be easily cut in the step of cutting the powder compact described below. If the amount of lubricant mixed with respect to 100% by mass of the raw material powder is 0.5% by mass or less, the amount of lubricant relative to the raw material powder is not too large, and the density of the powder compact can be easily increased. The amount of lubricant mixed may be 0.2% by mass or more and 0.5% by mass or less, or 0.3% by mass or more and 0.4% by mass or less.
[0045] <Process of compressing raw powder> The pressure molding is performed, for example, by cold isostatic pressing. The molding temperature is from 0°C to 50°C. The mold for cold isostatic pressing is made of a nonmetallic elastic material, such as urethane rubber, acrylic resin, acrylic resin containing elastomer, or polylactic acid (PLA) resin. Since the mold for cold isostatic pressing is not metal, titanium does not seize onto the mold. The shape of the green compact obtained by cold isostatic pressing is relatively simple. For example, the shape of the green compact is columnar or cylindrical.
[0046] The molding pressure is appropriately selected depending on the material of the raw material powder and the density of the green compact. For example, the molding pressure is 200 MPa or more. The molding pressure may be 350 MPa or more, or 500 MPa or more. The upper limit of the molding pressure depends on the capacity of the equipment. For example, the upper limit of the molding pressure is 800 MPa. The higher the molding pressure, the higher the density of the green compact tends to be.
[0047] <Step of cutting the powder compact> The cutting process is performed, for example, by a lathe or a machining center. The cutting process may be continuous cutting using a cutting tool or intermittent cutting using a rotary tool. Since the powder compact contains a lubricant, the cutting tool is less likely to be damaged during the cutting process. Since the cutting tool is less likely to be damaged, the increase in the cost of the cutting process associated with the replacement of the cutting tool can be suppressed. In addition, the cutting accuracy is less likely to decrease, and the surface quality of the cut powder compact is improved.
[0048] The greater the content of the lubricant in the powder compact, the less likely the cutting tool is to be damaged and the easier it is to improve the surface properties of the powder compact. The content of the lubricant relative to the raw material powder in the powder compact may be considered to be the same as the amount of lubricant mixed with the raw material powder when the raw material powder and the lubricant are mixed.
[0049] The step of cutting the powder compact is not essential, and the powder compact may be sintered without being cut.
[0050] <Process for removing lubricant> In the step of removing the lubricant, the powder compact is heat-treated in an inert atmosphere at 400°C or less. The inert atmosphere is, for example, a nitrogen atmosphere or an argon atmosphere. In an inert atmosphere at 400°C or less, titanium contained in the powder compact is difficult to nitride. Since titanium nitride is brittle, if titanium nitride is generated in the powder compact, the mechanical properties of the titanium-based sintered body obtained by sintering the powder compact may be deteriorated. In addition, titanium nitride may inhibit the sintering of the powder compact and deteriorate the mechanical properties of the titanium-based sintered body. Here, even if the powder compact is heat-treated in an argon atmosphere, titanium nitride may be generated in an argon atmosphere above 400°C because the powder compact may contain air.
[0051] Stearic acid vaporizes at 270°C or higher. Therefore, a powder compact containing stearic acid as a lubricant is heat treated, for example, in an inert atmosphere at 270°C or higher and 380°C or lower. If the temperature range of the inert atmosphere is 270°C or higher and 380°C or lower, most of the stearic acid is removed from the powder compact. Furthermore, within the above temperature range, the generation of titanium nitride in the powder compact can be effectively suppressed.
[0052] The time for which the powder compact is maintained within the above temperature range, i.e., the heat treatment time, is, for example, 10 minutes or more and 8 hours or less. If the heat treatment time is 10 minutes or more, the temperature at the center of the powder compact becomes sufficiently high, and the lubricant is easily removed from the entire powder compact. If the heat treatment time is 8 hours or less, the production time of the titanium-based sintered body is not too long. The heat treatment time may be 3 hours or more and 6 hours or less. After the heat treatment, the powder compact is cooled to room temperature in a furnace.
[0053] If the powder compact does not contain a lubricant, the step of removing the lubricant is not necessary.
[0054] <Step of sintering the powder compact> In the step of sintering the powder compact, the powder compact is sintered in a vacuum atmosphere. The atmospheric pressure is, for example, 0.1 Pa or less. The atmospheric temperature is appropriately selected depending on the material of the raw material powder. For example, the atmospheric temperature is 1100°C or more and 1400°C or less.
[0055] The sintering time is, for example, 1 hour or more and 25 hours or less. If the sintering time is 1 hour or more, the entire powder compact is likely to be sintered sufficiently. If the sintering time is 25 hours or less, the production time of the titanium-based sintered body is not too long. The sintering time may be 8 hours or more and 18 hours or less. The titanium-based sintered body is cooled to room temperature in the furnace.
[0056] Even in a vacuum atmosphere, there is a small amount of air. Therefore, there is a risk that the nitrogen in the air will react with the titanium contained in the powder compact when it is sintered. The amount of titanium nitride in the titanium-based sintered body can be reduced by embedding the powder compact in zirconia balls and further placing a getter made of titanium pieces on top of the zirconia balls.
[0057] The relative density of the titanium-based sintered body is, for example, 95% by volume or more. In this example, the relative density is the volume ratio of the solid portion to the volume of the object to be measured. Here, even if the relative density of the powder compact before sintering is the same, if the method of manufacturing the powder compact is different, the relative density of the titanium-based sintered body will change. For example, when a powder compact made of a raw material powder made of a prealloy powder is sintered, the relative density of the titanium-based sintered body is unlikely to be high. The prealloy powder is a powder having the same composition as the titanium alloy that makes up the titanium-based sintered body. On the other hand, when a powder compact made of a raw material powder in which a plurality of types of powders are mixed is sintered, the relative density of the titanium-based sintered body is likely to be high.
[0058] <Step of compressing titanium-based sintered body by hot isostatic pressing> Hot isostatic pressing further increases the relative density of titanium-based sintered bodies. The relative density of titanium-based sintered bodies subjected to hot isostatic pressing is 95% or more. It is difficult to increase the density of titanium-based sintered bodies with a relative density of less than 95% by hot isostatic pressing.
[0059] The temperature of the hot isostatic press is appropriately selected depending on the composition of the titanium-based sintered body. For example, the temperature of the hot isostatic press is 800°C or higher and 1100°C or lower. The processing time is, for example, 30 minutes or longer and 6 hours or shorter. If the processing time is 30 minutes or longer, the relative density of the titanium-based sintered body is sufficiently high. If the processing time is 6 hours or shorter, the manufacturing time of the titanium-based sintered body is not too long. The processing time may be 1 hour or longer and 4 hours or shorter. The titanium-based sintered body is cooled to room temperature in the hot isostatic press device. The pressure is, for example, 150 MPa or higher.
[0060] <Finishing process> In the finish processing step, for example, the surface of the titanium-based sintered body is ground. Grinding allows the titanium-based sintered body to have the desired dimensions and makes the surface of the titanium-based sintered body smooth. In addition, impurities concentrated on the surface of the titanium-based sintered body are removed from the surface of the titanium-based sintered body by grinding. Examples of impurities include titanium oxide, titanium carbide, and titanium nitride. Removing impurities from the surface of the titanium-based sintered body improves the mechanical properties of the titanium-based sintered body.
[0061] <Titanium-based sintered body> As shown in Fig. 4, the titanium-based sintered body 1 of this example is an MMC including a matrix 2 and a plurality of precipitates 3 dispersed in the matrix 2. Fig. 4 is a cross-sectional photograph of the titanium-based sintered body produced in Test Example 3 described later. The MMC is excellent in tensile strength, heat resistance, and wear resistance.
[0062] The matrix 2 includes titanium. For example, the matrix 2 is made of a titanium alloy. For example, the titanium alloy is Ti-5Al-2.5Sn, Ti-6Al-4V, Ti-3Al-2.5V, Ti-6Al-4V-2Sn, Ti-15V-3Cr-3Sn-3A. l , Ti-13V-11Cr-3Al, or Ti-3Al-8V-6Cr-4Mo-4Zr. In particular, Ti-6Al-4V has excellent strength.
[0063] The precipitate 3 is composed of ceramics. The precipitate 3 is, for example, TiB. The precipitate 3 derived from the ceramic powder contributes to improving the tensile strength, wear resistance, and heat resistance of the titanium-based sintered body.
[0064] In the titanium-based sintered body 1 of this example, a plurality of precipitates 3 are uniformly dispersed throughout the entire titanium-based sintered body 1, and the mechanical properties of the entire titanium-based sintered body 1 are uniform. Therefore, the titanium-based sintered body 1 of this example is less likely to be locally damaged during use and has a long life.
[0065] The homogeneity of the titanium-based sintered body 1 can be evaluated based on the variation in the abundance ratio of the precipitates 3 at multiple locations in the titanium-based sintered body 1. In this example, the evaluation index is that the average value R0, the maximum value R1, and the minimum value R2 of the abundance ratios satisfy the following formula. R1≦R0+4.5 R2≧R0-4.5
[0066] Each of the plurality of abundance ratios is the area ratio of the plurality of precipitates when the total area of the matrix 2 and the plurality of precipitates 3 in each of the plurality of measurement ranges is taken as 100%. The plurality of measurement ranges are obtained from a cross section of the titanium-based sintered body 1. The number of measurement ranges is 10 or more. The maximum value R1 and the minimum value R2 of the abundance ratio of the precipitates 3 satisfying the above formula means that the abundance ratio in each measurement range does not deviate significantly from the average value R0. In other words, the provision of the above formula indicates that the variation in the abundance ratio in the plurality of measurement ranges is small.
[0067] <Test Example> <Test Example 1> In Test Example 1, the influence of the presence or absence of a lubricant and the amount of the lubricant on the machinability of the powder compact was examined. The samples prepared in Test Example 1 were as follows.
[0068] [Sample No. 1] A first powder made of an Al-V alloy was prepared. The particle size of the first powder was 20 μm or more and 90 μm or less. The first powder was obtained by classifying a commercially available Al-V alloy powder.
[0069] A second powder made of pure titanium was prepared. The particle size of the second powder was 20 μm or more and 45 μm or less. The second powder was obtained by classifying a commercially available titanium powder.
[0070] Ceramic powder made of titanium diboride (TiB2) was prepared. The particle size of the ceramic powder was 0.7 μm or more and 10 μm or less.
[0071] 1221 g of the first powder and 77.9 g of the ceramic powder were mixed in a ball mill to produce a mixed powder consisting of the first powder and the ceramic powder. The container of the ball mill was made of tungsten carbide. The grinding balls put into the container of the ball mill were also made of tungsten carbide. The diameter of the grinding balls was 10 mm, and the number of grinding balls was 50. The mixing conditions were 300 rpm for 1 hour. "rpm" refers to the number of rotations per minute.
[0072] 154 g of the mixed powder and 846 g of the second powder were mixed in a V-type mixer to produce raw powder. This raw powder was pressurized by a cold isostatic press to produce a cylindrical green compact. The pressing pressure was 390 MPa, and the holding time was 30 seconds. The green compact had an outer diameter of 40 mm, an inner diameter of 20 mm, and a height of 30 mm. The green compact did not contain any lubricant.
[0073] [Sample No. 2 to Sample No. 5] The powder compacts of Sample No. 2 to Sample No. 5 contain a lubricant. The only difference between Sample No. 2 to Sample No. 5 and Sample No. 1 is the presence or absence of a lubricant. The lubricant was stearic acid. The lubricant was fed into the V-type mixer together with the mixed powder and the second powder. The amount of lubricant mixed in Sample No. 2 was 0.05 mass% when the raw material powder was taken as 100 mass%. The amount of lubricant mixed in Sample No. 3 was 0.1 mass%, the amount of lubricant mixed in Sample No. 4 was 0.3 mass%, and the amount of lubricant mixed in Sample No. 5 was 0.5 mass%.
[0074] [Sample No. 100] Sample No. 100 is a sintered material obtained by heat treating a powder compact produced by the same method as sample No. 3 in a nitrogen atmosphere at 380°C for 4 hours and then sintering in a vacuum atmosphere at 1300°C for 12 hours.
[0075] [Cutting test] The surfaces of the sintered material of sample No. 100 and the green compacts of sample No. 1 to No. 5 were machined using a lathe. The cutting was dry machining. The peripheral speed S was 180 m / min, the feed F was 0.2 mm / rev, and the cutting depth D was 0.5 mm / rev. The wear of the cutting tools after the cutting test was measured using a measuring device attached to a microscope. As a result, the wear of the cutting tools used in cutting sample No. 2 to No. 5 was smaller than that of sample No. 1 and sample No. 100. In addition, the wear of the cutting tools decreased as the amount of lubricant mixed increased. However, there was almost no difference in the wear between sample No. 4, which contained 0.3 mass% of lubricant, and sample No. 5, which contained 0.5 mass% of lubricant.
[0076] <Test Example 2> In Test Example 2, the effect of the mixing method of the raw material powders on the relative density of the titanium-based sintered body was examined. The samples prepared in Test Example 2 are as follows:
[0077] [Sample No. 21] First, a powder compact of sample No. 21 was produced using the same materials and manufacturing method as sample No. 3. Therefore, the powder compact of sample No. 21 contains a powder of pure titanium, a powder of an Al-V alloy, a ceramic powder of TiB2, and a lubricant.
[0078] The green compact was placed in an inert oven and the stearic acid was removed from the green compact by heat treatment. The atmosphere in the inert oven was a nitrogen atmosphere, the heat treatment temperature was 380°C, and the heat treatment time was 4 hours. The temperature rise rate of the inert oven was 5°C / min.
[0079] The lubricant-removed green compact was placed in a sintering furnace, and titanium-based sintered compacts were produced by sintering. The sintering furnace atmosphere was a vacuum atmosphere of 0.1 Pa or less, the sintering temperature was 1300°C, and the sintering time was 12 hours. The heating rate of the sintering furnace was 6.7°C / min up to 1290°C, and 1°C / min from 1290°C to 1300°C. The titanium-based sintered compact was an MMC with a matrix containing titanium and multiple precipitates dispersed in the matrix. The composition of the matrix was Ti-6Al-4V alloy, a so-called 64 titanium alloy. The composition of the precipitates derived from TiB2 was titanium boride (TiB).
[0080] In Test Example 2, the relative density of the powder compact was measured before sintering the powder compact, and the relative density of the titanium-based sintered body was also measured. The relative density is the volume ratio of the solid part to the volume of the measurement object. The unit of relative density is volume %. The relative density was measured by Archimedes' method.
[0081] The relationship between the relative density of powder compacts and the relative density of titanium-based sintered bodies is shown in the graph of Figure 2. The plot of white circles indicates the relative density of powder compacts, and the plot of black circles indicates the relative density of titanium-based sintered bodies. The horizontal axis of Figure 2 is compacting pressure, and the vertical axis is relative density. The unit of compacting pressure is MPa (megapascals). Figure 2 also shows the relative densities of powder compacts with compacting pressures of 100 MPa, 200 MPa, 300 MPa, and 390 MPa, as well as the relative densities of titanium-based sintered bodies.
[0082] As shown in FIG. 2, it was found that the higher the molding pressure, the higher the relative density of the powder compact. In addition, the relative density of the titanium-based sintered body was increased by 15% or more by volume compared to the relative density of the powder compact before sintering. The relative density of all titanium-based sintered bodies shown in FIG. 2 was 95% or more by volume. From these findings, it was found that even if the relative density of the powder compact is low, a titanium-based sintered body having a relative density of 95% or more by sintering can be produced. On the other hand, when cutting the powder compact, if the relative density of the powder compact is low, the powder compact may chip or crack. From the viewpoint of suppressing cracking or chipping of the powder compact, it is desirable that the relative density of the powder compact is 75% or more by volume. The molding pressure for obtaining a thick powder compact having a relative density of 75% or more by volume is, for example, 300 MPa or more.
[0083] [Sample No. 22] The green compact of sample No. 22 was obtained by pressing a mixture of prealloy powder, ceramic powder, and stearic acid. The prealloy powder was a powder made of Ti-6Al-4V alloy. The pressing pressure was the same as that of sample No. 21. The lubricant was removed from the green compact by heat treatment, and a titanium-based sintered compact was produced by sintering. The heat treatment and sintering conditions were the same as those of sample No. 21. The titanium-based sintered compact of sample No. 22 was also an MMC with multiple precipitates dispersed in the matrix.
[0084] The relationship between the relative density of the powder compact and the relative density of the titanium-based sintered body is shown in the graph of Figure 3. The graph of Figure 3 can be read in the same way as the graph of Figure 2. As shown in Figure 3, it was found that the higher the compacting pressure, the higher the relative density of the powder compact. However, the relative density of the titanium-based sintered body was only about 5% higher by volume than the relative density of the powder compact before sintering. The relative density of all of the titanium-based sintered bodies shown in Figure 3 was 85% by volume or less.
[0085] [summary] The results of Test Example 2 show that in order to produce an MMC with a relative density of 95% by volume or more, it is effective to produce a green compact from raw material powders made up of multiple types of powder.
[0086] <Test Example 3> In Test Example 3, the effect of the raw material powder mixing method on the structure of titanium-based sintered bodies was investigated. In Test Example 3, samples No. 31 to No. 35 were produced using different raw material powder mixing methods. In producing samples No. 31 to No. 34, the raw material powder was mixed in two batches. In producing sample No. 35, the raw material powder was mixed all at once. The mixing conditions for each sample using the ball mill were 300 rpm x 1 hour, and the mixing time using the V-type mixer was 1 hour.
[0087] [Sample No. 31] In the first mixing, Al-V alloy powder and TiB2 ceramic powder were mixed in a ball mill to produce a mixed powder. In the second mixing, the mixed powder, pure titanium powder, and stearic acid were mixed in a V-type mixer to produce a raw powder. The amount of stearic acid mixed was 0.3 mass%.
[0088] [Sample No.32] In the first mixing, pure titanium powder and TiB2 ceramic powder were mixed in a ball mill to produce a mixed powder. In the second mixing, the mixed powder, Al-V alloy powder, and stearic acid were mixed in a V-type mixer to produce a raw powder.
[0089] [Sample No. 33] In the first mixing, Al-V alloy powder and pure titanium powder were mixed in a ball mill to produce a mixed powder. In the second mixing, the mixed powder, ceramic powder made of TiB2, and stearic acid were mixed in a V-type mixer to produce a raw powder.
[0090] [Sample No. 34] In the first mixing, Al-V alloy powder and pure titanium powder were mixed in a ball mill to produce a mixed powder. In the second mixing, the mixed powder, ceramic powder made of TiB2, and stearic acid were mixed in a ball mill to produce a raw powder.
[0091] [Sample No. 35] The raw powder was prepared by mixing Al-V alloy powder, pure titanium powder, and TiB2 ceramic powder in a V-type mixer. Sample No. 35 does not contain stearic acid.
[0092] Titanium-based sintered bodies were produced from the raw powders of samples No. 31 to No. 35. The cold isostatic pressing pressure, the heat treatment conditions to remove the lubricant, and the sintering conditions for each sample were the same. The molding pressure was 390 MPa, the heat treatment conditions were 380°C x 4 hours in a nitrogen atmosphere, and the sintering conditions were 1300°C x 12 hours in a vacuum atmosphere.
[0093] The cross section of each sample was observed, and the area ratio of precipitates consisting of TiB was measured. Cross-sectional photographs of the titanium-based sintered compacts of sample No. 31 to sample No. 35 are shown in Figures 4 to 8, respectively. The gray parts in the cross-sectional photographs are a matrix consisting of 64 titanium, and the black parts are precipitates consisting of TiB. Comparing Figures 4 to 8, it was found that TiB precipitates were uniformly dispersed in sample No. 31 and sample No. 32. On the other hand, in sample No. 33 to sample No. 35, numerous spotted areas with few black precipitates were observed, indicating that the precipitates were dispersed non-uniformly.
[0094] Next, the dispersion state of TiB was quantitatively evaluated. The observation field of 13.2 mm × 9.5 mm was divided into 64, and the matrix and TiB in each divided field were distinguished by binarization processing. Then, the area ratio of TiB was calculated using image analysis software when the total area of the matrix and precipitates in each divided field was taken as 100%. The area ratio of TiB is the abundance ratio of TiB, and is expressed in %,. The average value R0, maximum value R1, and minimum value R2 of the abundance ratios obtained from each divided field were calculated. The average value R0, maximum value R1, and minimum value R2 for each sample are shown in Table 1. Samples that satisfy R1≦R0+4.5 and R2≧R0-4.5 were evaluated as ``A'', and samples that do not satisfy these were evaluated as ``B''. Samples that satisfy R1≦R0+4.5 and R2≧R0-4.5 were judged to be samples in which TiB precipitates are uniformly dispersed in the matrix.
[0095] [Table 1]
[0096] As shown in Table 1, TiB was uniformly dispersed in the matrix in Sample No. 31 and Sample No. 32. These samples were prepared by mixing the ceramic powders in a ball mill in the first mixing step.
[0097] In samples No. 33 and No. 34, the dispersion state of TiB in the matrix was not uniform. These samples were obtained by mixing the ceramic powder in the second mixing process. Mix This is a combined sample.
[0098] There was variation in the dispersion state of TiB in the matrix in sample No. 35. This sample was made by mixing all the raw materials constituting the titanium-based sintered body at once using a ball mill.
[0099] From these results, it was found that in order to uniformly disperse precipitates in the matrix, it is important to mix the raw materials constituting the titanium-based sintered body in several batches, and that it is also important that the ceramic powder is mixed in the first mixing step using a mixing method that applies high stress to the ceramic powder.
[0100] <Test Example 4> The mechanical properties of the MMC were examined in Test Example 4. The samples prepared in Test Example 4 were as follows:
[0101] [Sample No. 40] Sample No. 40 is a cast body made of titanium alloy 64.
[0102] [Sample No. 41 to Sample No. 44] Sample No. 41, Sample No. 42, Sample No. 43, Sample No. 44, and Sample No. 45 are titanium-based sintered bodies having the same configuration as Sample No. 31, Sample No. 32, Sample No. 33, Sample No. 34, and Sample No. 35 of Test Example 3, respectively.
[0103] [Tensile test] A test piece was prepared from each sample, and a tensile test was performed. FIG. 9 is a schematic diagram showing the shape of the test piece 5. The test piece 5 includes a first grip portion 51, a second grip portion 52, and an intermediate portion 50. The diameter of the intermediate portion 50 is 6.35 mm (millimeters), and the gauge length d between the first gauge point 50A and the second gauge point 50B set in the intermediate portion 50 is 25.4 mm. The temperature of the tensile test was room temperature, the strain rate until the 0.2% yield strength was 1.2 mm / min, and the strain rate after the 0.2% yield strength was 12.8 mm / min. The unit of tensile strength was MPa. The test results are shown in Table 2.
[0104] [Table 2]
[0105] As shown in Table 2, the tensile strength of the titanium-based sintered compacts of Samples No. 41 to 45 was equal to or greater than that of the ingot made of titanium 64. From these results, it was found that the titanium-based sintered compacts of this example are useful as materials for components of machines such as automobiles. [Explanation of symbols]
[0106] 1 Titanium-based sintered body 2. Matrix 3 Precipitates 5. Test Pieces 50 Middle 50A First gauge 50B Second gauge point 51 First grip part 52 Second grip part d Gauge length
Claims
1. mixing the first powder and the ceramic powder to prepare a mixed powder; mixing the mixed powder with a second powder to prepare a raw material powder; A step of press-molding the raw material powder to produce a powder compact; and a step of sintering the powder compact to produce a titanium-based sintered body. The first powder is made of an alloy containing aluminum and vanadium, The second powder is composed of titanium. A method for producing a titanium-based sintered body.
2. mixing the first powder and the ceramic powder to prepare a mixed powder; mixing the mixed powder with a second powder to prepare a raw material powder; A step of press-molding the raw material powder to produce a powder compact; and a step of sintering the powder compact to produce a titanium-based sintered body. The first powder is composed of titanium, The second powder is composed of an alloy containing aluminum and vanadium. A method for producing a titanium-based sintered body.
3. 3. The method for producing a titanium-based sintered body according to claim 1, wherein the ceramic powder is constituted by titanium diboride.
4. 3. The method for producing a titanium-based sintered body according to claim 1, wherein the first powder and the ceramic powder are mixed by a ball mill, an attritor, or a jet mill.
5. The method for producing a titanium-based sintered body according to claim 4, wherein the mixed powder and the second powder are mixed by a V-type mixer.
6. 3. The method for producing a titanium-based sintered body according to claim 1, wherein in the step of producing the powder compact, the powder compact is produced by cold isostatic pressing.
7. 3. The method for producing a titanium-based sintered body according to claim 1, further comprising a step of compressing the titanium-based sintered body by hot isostatic pressing.
8. a matrix made of an alloy containing titanium, aluminum, and vanadium; A plurality of precipitates are formed from a compound derived from a ceramic powder and dispersed in the matrix; The average value R0, the maximum value R1, and the minimum value R2 of the plurality of abundance ratios obtained from each of 50 or more different measurement ranges in the cross section satisfy the following formula: R1≦R0+4.5 R2≧R0−4.5 Each of the plurality of presence ratios is an area ratio of the plurality of precipitates when a total area of the matrix and the plurality of precipitates in each of the plurality of measurement ranges is set to 100%. Titanium-based sintered body.
9. 9. The titanium-based sintered body according to claim 8, wherein the precipitates are constituted by titanium boride.
Citation Information
Patent Citations
Re2O3, TiB and TiC doped reinforced titanium-base composite material and method for making same
CN101135016A
Preparation method of orientation controllable TiB whisker reinforcement titanium-based composite material
CN109136608A
Gradient alloy composite material and preparation method thereof
CN114182125A
Manufacture of sintered co superalloy
JP1982171644A
Production of powder sintered impeller
JP1996120307A