Method for nitriding rare earth magnetic material and nitrided rare earth magnetic material
A three-step heat treatment process addresses nitrogen content and distribution issues in rare earth magnetic materials, enhancing magnetic performance through uniform nitrogen distribution.
Patent Information
- Application Number
- JP2023514950
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-16
- Filing Date
- 2021-04-19
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2041-04-19
Smart Images

Figure 0007561974000001
Abstract
Description
[Technical field]
[0001] The present application belongs to the technical field of magnetic materials, and relates to a method for nitriding a rare earth magnetic material and a nitrided rare earth magnetic material. [Background technology]
[0002] In recent years, with the progress and development of science and technology, the scope of use of magnetic materials has become wider, and people's lives are inseparable from magnetic materials. Magnetic materials are divided into permanent magnetic materials and soft magnetic materials, and their applications vary according to their performance. Rare earth magnetic materials are widely used due to their excellent magnetic performance.
[0003] The most commonly used rare earth permanent magnetic material is NdFeB, which is currently the rare earth permanent magnetic material with the highest permanent magnetic performance, magnetic energy product. However, due to the low content of rare earth elements in the earth's crust and the high cost of mining and refining, NdFeB material has high performance but also high cost.
[0004] Samarium iron nitrogen magnets avoid the defects of neodymium iron boron magnets, such as low Curie temperature, easy oxidation, and high cost, and have become a research hotspot of next-generation rare earth permanent magnetic materials. The introduction of nitrogen atoms does not change the crystal structure of samarium iron alloys, but causes lattice expansion, enhances the ferromagnetic coupling exchange action of the alloy, greatly improves the Curie temperature of the alloy, enhances the anisotropic field, and is the key to improving the permanent magnetic performance of samarium iron alloys. Therefore, the nitriding process plays an important role in the production of samarium iron nitrogen magnets. At present, the relatively mature nitriding process at home and abroad first obtains alloy powder by mechanical methods and then performs nitriding, but the solid powder nitriding has defects such as uneven and incomplete nitriding, poor efficiency, and easy oxidation of powder.
[0005] Rare earth-iron-nitrogen materials include SmFeN, NdFeN, CeFeN, etc. Some utilize the permanent magnetic properties of the material, while others utilize the soft magnetic properties of the material. However, all of the manufacturing methods for these materials involve forming a rare earth-iron alloy and then nitriding the alloy during the manufacturing process.
[0006] Modern communication computers, mobile phones, network equipment, etc. will generate electromagnetic interference and electromagnetic radiation during use. In order to effectively reduce and eliminate electromagnetic interference and radiation, it is necessary to use absorbers with high complex permeability. At present, the widely used ferrite materials have defects such as narrow frequency band and low complex permeability at high frequencies, while metal soft magnetic materials have poor soft magnetic performance at high frequencies due to the existence of eddy current loss. Materials such as CeFeN can ensure high permeability and wide resonance frequency at high frequencies, as well as realize electromagnetic shielding within a wide frequency band and reduction of signal noise, meeting the needs of modern technology and being widely used in instruments, meters, communications and other fields.
[0007] Rare earth transition metal magnetic materials exhibit excellent magnetic performance after nitriding, but the insufficient nitrogen content and non-uniform distribution of nitrogen element generated during the nitriding process greatly affect the performance of the materials.
[0008] CN101699578A has the chemical formula R2Fe 17 N 3-δ The paper discloses a rare earth iron nitrogen high frequency soft magnetic material, its composite material and manufacturing method, which discloses that a material containing 10-30%wt of rare earth elements and 70-90%wt of iron is first melted and smelted into an iron-based alloy, which is then crushed into small particles, ground into powder and subjected to nitriding treatment, with the treatment temperature being 250-550°C. However, there is room for further improvement in the nitrogen content and uniformity of the product obtained by this method.
[0009] CN107557551A discloses a method for producing samarium-iron-nitrogen-based permanent magnetic materials, which discloses that a metastable samarium-iron alloy is subjected to large plastic deformation, followed by nitriding and annealing crystallization, and the defects caused by the large plastic deformation are utilized to promote the intrusion and diffusion of nitrogen atoms, thereby significantly improving the amount and uniformity of nitriding of the alloy. However, the process of this method is too complicated, which increases the manufacturing cost. Summary of the Invention [Problem to be solved by the invention]
[0010] The present application aims to provide a method for nitriding a rare earth magnetic material and a nitrided rare earth magnetic material, which can solve the problems of insufficient nitrogen content and non-uniform distribution of nitrogen elements after nitriding the rare earth magnetic material. [Means for solving the problem]
[0011] In order to achieve this object, the present application provides the following technical solutions.
[0012] In a first aspect, the present application provides a method for producing a method for manufacturing a semiconductor device comprising: (1) evacuating the reactor containing the rare earth magnetic material, adding a nitrogen source, and performing a three-stage heating process to obtain a semi-finished product, and the heating temperature of the three-stage heating process is increased stepwise; (2) a method for nitriding a rare earth magnetic material, comprising the steps of: heating the semi-finished product in step (1) to a first set temperature, adjusting the temperature to a second set temperature, drawing a vacuum, introducing an inert gas, and maintaining the temperature at the second set temperature to obtain a nitrided rare earth magnetic material, the second set temperature being lower than the first set temperature.
[0013] In the method of the present application, the three-step heat treatment is the main nitriding process, which can ensure that the nitrogen-containing gas molecules adsorbed on the surface of the alloy diffuse into the alloy (rare earth magnetic material) to form a nitrogen-containing alloy (i.e., a semi-finished product), thereby making it possible to improve the nitrogen content by rationally utilizing the diffusion kinetics and improving the penetration depth of the nitrogen element after the nitrogen element is adsorbed on the powder surface. Heating at the first set temperature is a homogenization treatment step, which can further promote the adsorption of nitrogen and the diffusion into the alloy, thereby making the distribution of the nitrogen element in the alloy more uniform. Heating at the second set temperature can make the diffusion of the nitrogen element in the alloy uniform.
[0014] In the method according to the present application, in step (2), the temperature is adjusted to the second set temperature and a vacuum is drawn, which may be performed by directly cooling to the second set temperature and then drawing a vacuum, or by first cooling to room temperature, drawing a vacuum, and then heating to the second set temperature.
[0015] In the method according to the present application, three different locations are selected from the obtained rare earth nitride magnetic material, and the mass fraction of nitrogen is measured using a nitrogen content detector, thereby making it possible to consider whether the nitrogen distribution is uniform or not.
[0016] In the present application, in step (1), the rare earth magnetic material may be in the form of a lump or powder, and it is preferable to use the powder since it has a better effect.
[0017] The following is a preferred technical solution of the present application, which is not intended to limit the technical solution of the present application, and can better achieve and realize the technical objectives and beneficial effects of the present application.
[0018] In the preferred technical solution of the present application, in step (1), the rare earth magnetic material has a general formula of ReTm, where Re is a rare earth metal and Tm is a 3d transition element and / or a 4d transition element. The 3d transition element includes at least one of Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, or Zn. The 4d transition element refers to at least one of Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, or Cd.
[0019] Preferably, the general formula of the rare earth nitride magnetic material is ReTmN. In the present application, the specific ratio of Re and Tm is not limited as long as a phase can be formed.
[0020] Preferably, in step (1), the pressure in the reactor is reduced to 1000 Pa or less, for example, 900 Pa, 500 Pa, 100 Pa, 50 Pa, 10 Pa, 5 Pa, etc., and preferably reduced to 10 Pa or less, by the evacuation.
[0021] Preferably, in step (1), the nitrogen source comprises a gaseous nitrogen source and / or a solid nitrogen source.
[0022] Preferably, the gaseous nitrogen source is a nitrogen-containing gas.
[0023] Preferably, the gaseous nitrogen source includes nitrogen gas and / or ammonia gas.
[0024] Preferably, the gaseous nitrogen source further comprises hydrogen gas.
[0025] Preferably, the solid nitrogen source includes ammonium bicarbonate.
[0026] Preferably, in step (1), the nitrogen source is a gaseous nitrogen source, and the pressure of the gaseous nitrogen source in the reactor is 0.001-10 MPa, such as 0.001 MPa, 1 MPa, 2 MPa, 5 MPa, 8 MPa or 10 MPa, and preferably 0.01-2 MPa.
[0027] Preferably, in step (1), the nitrogen source is a solid nitrogen source, and before the three-stage heat treatment, a protective gas is introduced into the reactor until the pressure is 0.001-10 MPa, for example, 0.001 MPa, 1 MPa, 2 MPa, 5 MPa, 8 MPa or 10 MPa, preferably 0.01-2 MPa.
[0028] As a preferred technical solution of the present application, in step (1), the temperature in the first stage of the three-stage heat treatment is 330-470K, for example, 330K, 350K, 380K, 400K, 420K, 450K or 470K, and preferably 370-420K.
[0029] Preferably, in step (1), the incubation time in the first stage of the three-stage heat treatment is 0 to 24 hours (excluding 0), for example, 0.1 hour, 0.5 hours, 1 hour, 5 hours, 10 hours, 20 hours or 24 hours, and preferably 0.1 to 5 hours.
[0030] In the present application, the purpose of the first heating step of the three-stage heating in step (1) is to exhaust gases, particularly oxygen gas, adsorbed in the ReTm alloy in order to prevent the alloy from being oxidized during the subsequent nitriding.
[0031] As a preferred technical solution of the present application, in step (1), the temperature in the second stage of the three-stage heat treatment is 670 to 730K (but excluding 730K), for example, 670K, 680K, 690K, 700K, 710K or 720K, and is preferably 690 to 710K.
[0032] Preferably, in step (1), the incubation time in the second stage of the three-stage heat treatment is 0 to 24 hours (excluding 0), for example, 0.1 hours, 0.5 hours, 1 hour, 5 hours, 10 hours, 20 hours or 24 hours, and preferably 0.1 to 5 hours.
[0033] In the present application, the function of the second heating stage among the three heating stages in step (1) is to preheat and adsorb the ReTm and N element atmosphere, and to allow the nitrogen-containing atmosphere to be sufficiently adsorbed on the surface of ReTm.
[0034] As a preferred technical proposal of the present application, in step (1), the temperature in the third stage of the three-stage heat treatment is 730 to 830K (but excluding 830K), for example, 730K, 740K, 750K, 760K, 770K, 780K, 790K, 800K, 810K or 820K, and is preferably 750 to 780K.
[0035] Preferably, in step (1), the incubation time in the third stage of the three-stage heat treatment is 0 to 24 hours (excluding 0), for example, 0.1 hours, 0.5 hours, 1 hour, 5 hours, 10 hours, 20 hours or 24 hours, and preferably 0.1 to 5 hours.
[0036] In the present application, the purpose of the third heating step among the three heating steps in step (1) is to cause the gas molecules adsorbed on the surface of the alloy to penetrate into the alloy by diffusion, thereby forming a ReTmN alloy.
[0037] In the preferred technical solution of the present application, in step (2), the first set temperature is 830 to 860 K (but does not include 860 K), such as 830 K, 835 K, 840 K, 845 K, or 850 K, and is preferably 830 to 840 K. In the present application, if the first set temperature is too high, ReTmN decomposes into ReN and Tm phases, and the product deviates from the desired composition. If the first set temperature is too low, the N content is low and non-uniform.
[0038] Preferably, in step (2), the temperature rise time to the first set temperature is 0 to 24 hours (however, not including 0), for example, 1 hour, 5 hours, 10 hours, 15 hours, 20 hours or 24 hours, and is preferably 0.5 to 5 hours.
[0039] As a preferred technical solution of the present application, in step (2), the pressure in the reactor is reduced to 1000 Pa or less, for example, 900 Pa, 500 Pa, 100 Pa, 50 Pa, 10 Pa, 5 Pa, etc., by the evacuation, and it is preferable to reduce the pressure to 10 Pa or less.
[0040] Preferably, in step (2), the pressure in the reactor is adjusted to 0.001 to 1 MPa, such as 0.001 MPa, 0.01 MPa, 0.1 MPa, 0.5 MPa or 1 MPa, by introducing the inert gas.
[0041] Preferably, in step (2), the second set temperature is 600 to 700K, for example, 600K, 610K, 620K, 630K, 640K, 650K, 660K, 670K, 680K, 690K or 700K, and is preferably 620 to 670K.
[0042] Preferably, in step (2), the incubation time for maintaining the temperature at the second set temperature is 0 to 24 hours (excluding 0), for example, 1 hour, 5 hours, 10 hours, 15 hours, 20 hours or 24 hours, and is preferably 0.5 to 5 hours.
[0043] In a preferred technical solution of the present application, step (2) further includes cooling to room temperature after maintaining the temperature at the second set temperature.
[0044] As a further preferred technical solution of the method according to the present application, the method comprises: (1) placing a rare earth magnetic material in a reactor, evacuating to 1000 Pa or less, introducing a nitrogen-containing gas, heating to 370-420 K and keeping the temperature for 0.1-5 hours, heating to 690-710 K and keeping the temperature for 0.1-5 hours, heating to 750-780 K and keeping the temperature for 0.1-5 hours, and obtaining a semi-finished product; (2) heating the semi-finished product in step (1) to 830-840K for 0.5-5 hours, adjusting the temperature to 620-670K, drawing a vacuum, reducing the pressure in the reactor to 1000 Pa or less, introducing an inert gas to adjust the pressure in the reactor to 0.001-1 MPa, maintaining the temperature at the second set temperature for 0.5-5 hours, and cooling to room temperature to obtain a nitride-type rare earth magnetic material.
[0045] In a second aspect, the present application provides a nitrided rare earth magnetic material obtained by the method for nitriding a rare earth magnetic material according to the first aspect. Effect of the Invention
[0046] Compared with the prior art, the present application has the following beneficial effects:
[0047] The method for nitriding a rare earth magnetic material according to the present application can distribute the nitrogen element more uniformly in the magnetic material while improving the nitrogen content, thereby resolving the problems of insufficient nitrogen content and non-uniform distribution of the nitrogen element after nitriding rare earth magnetic material in the prior art. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0048] In order to better explain the present application and facilitate understanding of the technical solution of the present application, the present application will be described in more detail below, however, the following examples are merely simple examples of the present application and do not represent or limit the scope of protection of the present application, which is subject to the scope of protection of the present application.
[0049] The following are typical but non-limiting examples of the present application.
[0050] Example 1
[0051] In this embodiment, the rare earth magnetic material is nitrided according to the following method.
[0052] (1) SmFe 17The alloy ingot was placed in a nitriding furnace, the pressure was reduced to 95 Pa by evacuation, the evacuation system was closed, and ammonia gas at 1.2 MPa was introduced.
[0053] (2) The temperature was raised to 450 K and kept at that temperature for 2 hours.
[0054] (3) After the temperature was kept at 450K, the temperature was increased to 710K and kept at that temperature for 1 hour.
[0055] (4) After the temperature was kept at 710K, the temperature was increased to 780K and kept at that temperature for 5 hours to obtain a semi-finished product.
[0056] (5) After the temperature was kept at 780K, the temperature was increased to 850K in one hour.
[0057] (6) After the temperature was maintained at 850K, the furnace was cooled to 680K, the gas in the nitriding furnace was extracted, the pressure was reduced to 90 Pa by evacuation, argon gas at 0.05 MPa was introduced, and the furnace was maintained at the same temperature for 3 hours.
[0058] (7) After the heating at 680K was completed, the alloy was cooled to room temperature, and the nitrided SmFeN alloy was taken out and samples were taken from three different locations to measure the mass fraction of nitrogen using a nitrogen content detector. The test results are shown in Table 1.
[0059] Example 2
[0060] In this embodiment, the rare earth magnetic material is nitrided according to the following method.
[0061] (1) Sm2Fe17 alloy powder (powder particle size: 0.1 μm to 10 mm) was charged into a nitriding furnace, the pressure was reduced to 9 Pa by evacuation, the evacuation system was closed, and ammonia gas at 1.2 MPa was introduced.
[0062] (2) The temperature was raised to 420 K and kept at that temperature for 2 hours.
[0063] (3) After the temperature was kept at 420K, the temperature was increased to 680K and kept at that temperature for 1 hour.
[0064] (4) After the temperature was kept at 680K, the temperature was increased to 750K and kept at that temperature for 4 hours.
[0065] (5) After the temperature was kept at 750K, the temperature was increased to 830K in one hour to obtain a semi-finished product.
[0066] (6) After the temperature was maintained at 830 K, the furnace was cooled to 670 K, the gas in the nitriding furnace was extracted, the pressure was reduced to 9 Pa by evacuation, argon gas at 0.03 MPa was introduced, and the furnace was maintained at the same temperature for 1 hour.
[0067] (7) After the heating at 670K was completed, the alloy was cooled to room temperature, and the nitrided SmFeN alloy powder was taken out and sampled from three different locations to measure the mass fraction of nitrogen using a nitrogen content detector. The test results are shown in Table 1.
[0068] Example 3
[0069] Other than step (6), the rest were the same as in Example 2. In step (6) in this example, after the heat retention at 830 K was completed, the furnace was cooled to room temperature, the gas in the nitriding furnace was extracted, the pressure was reduced to 10 Pa or less by evacuation, argon gas of 0.03 MPa was introduced, the temperature was raised to 670 K, and the furnace was kept at that temperature for 1 hour.
[0070] Example 4
[0071] Other than step (1), the rest were the same as in Example 2. In step (1) of this example, the vacuum system was closed, and a mixed gas of ammonia gas and hydrogen gas (mixture molar ratio 1:1) at 1.2 MPa was introduced.
[0072] Example 5
[0073] SmFe 17 A SmFeN alloy was produced under the same conditions as in Example 2, except that the alloy powder was replaced with SmFe9 alloy powder.
[0074] Example 6
[0075] SmFe 17 The alloy powder was Ce2Fe 17 A CeFeN alloy was produced under the same conditions as in Example 2, except that the alloy powder was replaced.
[0076] Example 7
[0077] SmFe 17 The alloy powder is Nd2Fe 17 A NdFeN alloy was produced under the same conditions as in Example 2, except that the alloy powder was substituted.
[0078] Example 8
[0079] SmFe 17 The alloy powder is NdFe 12 A NdFeN alloy was produced under the same conditions as in Example 2, except that the alloy powder was substituted.
[0080] Example 9
[0081] In this embodiment, the rare earth magnetic material is nitrided according to the following method.
[0082] (1) SmFe 17 Alloy powder (powder particle size 0.1 μm to 10 mm) was charged into a nitriding furnace, the pressure was reduced to 5 Pa by evacuation, the evacuation system was closed, and a mixed gas of nitrogen gas and ammonia gas (mixture molar ratio 1:1) at 0.01 MPa was introduced.
[0083] (2) The temperature was raised to 400 K and kept at that temperature for 0.1 hours.
[0084] (3) After the temperature was kept at 400 K, the temperature was increased to 700 K and kept at that temperature for 0.1 hours.
[0085] (4) After the temperature was kept at 700 K, the temperature was increased to 770 K and kept at that temperature for 0.1 hours.
[0086] (5) After the temperature was kept at 770 K, the temperature was increased to 840 K in 0.5 hours to obtain a semi-finished product.
[0087] (6) After the temperature was maintained at 840K, the furnace was cooled to 650K, the gas in the nitriding furnace was extracted, the pressure was reduced to 5 Pa by evacuation, argon gas at 0.01 MPa was introduced, and the furnace was maintained at the same temperature for 0.5 hours.
[0088] (7) After the heating at 650K was completed, the alloy was cooled to room temperature, and the nitrided SmFeN alloy powder was taken out and sampled from three different locations to measure the mass fraction of nitrogen using a nitrogen content detector. The test results are shown in Table 1.
[0089] Example 10
[0090] In this embodiment, the rare earth magnetic material is nitrided according to the following method.
[0091] (1) SmFe 17 Alloy powder (powder particle size: 0.1 μm to 10 mm) was charged into a nitriding furnace, the pressure was reduced to 5 Pa by evacuation, the evacuation system was closed, and ammonia gas at 2 MPa was introduced.
[0092] (2) The temperature was raised to 370 K and kept at that temperature for 5 hours.
[0093] (3) After the temperature was kept at 370K, the temperature was increased to 690K and kept at that temperature for 5 hours.
[0094] (4) After the temperature was kept at 690K, the temperature was increased to 770K and kept at that temperature for 5 hours.
[0095] (5) After the temperature was kept at 770K, the temperature was increased to 835K in 5 hours to obtain a semi-finished product.
[0096] (6) After the temperature was maintained at 835K, the furnace was cooled to 620K, the gas in the nitriding furnace was extracted, the pressure was reduced to 5 Pa by evacuation, argon gas of 1 MPa was introduced, and the furnace was maintained at the same temperature for 5 hours.
[0097] (7) After the heating at 620K was completed, the alloy was cooled to room temperature, and the nitrided SmFeN alloy powder was taken out and sampled from three different locations to measure the mass fraction of nitrogen using a nitrogen content detector. The test results are shown in Table 1.
[0098] Example 11
[0099] In step (1), SmFe 17 The alloy powder (powder particle size: 0.1 μm to 10 mm) was mixed with a certain amount of ammonium bicarbonate and charged into a nitriding furnace. The pressure was reduced to 9 Pa by evacuation, the evacuation system was closed, and argon gas at 1.2 MPa was introduced. Except for this, a SmFeN alloy was produced under the same conditions as in Example 2.
[0100] Comparative Example 1
[0101] The difference between this comparative example and Example 2 is that steps (2) and (3) are not performed, and instead the temperature is raised to 750K in step (3) and maintained at that temperature for 4 hours.
[0102] Comparative Example 2
[0103] The difference between this comparative example and Example 2 is that the operation in step (5) is not carried out, and cooling is carried out directly from 750K to room temperature in step (6).
[0104] Comparative Example 3
[0105] The difference between this comparative example and Example 2 is that the operation in step (3) is not performed, the temperature in step (4) is changed to and maintained at 420 K, and after the temperature is maintained at 420 K, the temperature is increased to 750 K and maintained at that temperature for 4 hours.
[0106] How we tested
[0107] In each of the examples and comparative examples, samples were taken from three different locations of the obtained rare earth nitride magnetic material, and the mass fraction of nitrogen was measured using a nitrogen content detector. The test results are shown in Table 1.
[0108] [Table 1]
[0109] As can be seen from the above-mentioned examples and comparative examples, the nitriding method of the rare earth magnetic material according to the examples makes it possible to distribute the nitrogen element more uniformly in the magnetic material while improving the nitrogen content, thereby resolving the problems in the prior art that the nitrogen content is insufficient and the distribution of the nitrogen element is non-uniform after the rare earth magnetic material is nitrided.
[0110] The low nitrogen content in the products of Examples 7 and 8 is due to the different rare earth elements used compared to Example 1. Their nitrogen contents are not comparable to those of Example 1.
[0111] In Comparative Example 1, only one-stage heating was performed instead of multi-stage heating when producing the semi-finished product, which resulted in incomplete exhaust and insufficient adsorption of nitrogen elements, resulting in an extremely low nitrogen content after nitriding and a poor nitriding effect.
[0112] In Comparative Example 2, the nitrogen content varies greatly and is not uniform because the homogenization treatment is not performed (that is, heating is not performed at the first set temperature).
[0113] In Comparative Example 3, the nitrogen content after nitriding is low due to insufficient adsorption of nitrogen element caused by only two-stage heating being performed in producing the semi-finished product.
[0114] The present application describes the detailed method of the present application through the above examples, but the applicant declares that the present application is not limited to the above detailed method, that is, it does not mean that the present application cannot be implemented without depending on the above detailed method.
Claims
1. (1) evacuating the reactor containing the rare earth magnetic material, adding a nitrogen source, and performing a three-stage heating process to obtain a semi-finished product, and the heating temperature of the three-stage heating process is increased step by step; (2) heating the semi-finished product in step (1) to a first set temperature, adjusting the temperature to a second set temperature, drawing a vacuum, introducing an inert gas, and maintaining the temperature at the second set temperature to obtain a rare earth nitride magnetic material, the second set temperature being lower than the first set temperature; A method for nitriding a rare earth magnetic material, wherein each step of the three-stage heat treatment includes heat retention, and the next step of heating is performed after the heat retention is completed.
2. 2. The method of claim 1, wherein in step (2), the first set temperature is between 830 and 860 K (but not including 860 K).
3. 3. The method of claim 1 or 2, wherein in step (1), the rare earth magnetic material has a general formula of ReTm, where Re is a rare earth metal and Tm is a 3d transition element and / or a 4d transition element.
4. The method according to claim 3 , wherein the rare earth nitride magnetic material has a general formula of ReTmN.
5. In step (1), the pressure in the reactor is reduced to 1000 Pa or less by evacuation, In step (1), the nitrogen source includes a gaseous nitrogen source and / or a solid nitrogen source; the gaseous nitrogen source is a nitrogen-containing gas; The method of any one of claims 1 to 4, wherein the solid nitrogen source comprises ammonium bicarbonate and / or ammonium chloride.
6. The method of claim 5 , wherein the gaseous nitrogen source comprises nitrogen gas and / or ammonia gas.
7. The method of claim 5 or 6, wherein the gaseous nitrogen source further comprises hydrogen gas.
8. 2. The method according to claim 1, wherein in step (1), the nitrogen source is a gaseous nitrogen source, and the pressure of the gaseous nitrogen source in the reactor is 0.001 to 10 MPa.
9. 2. The method of claim 1, wherein in step (1), the nitrogen source is a solid nitrogen source, and after the three-stage heat treatment, a protective gas is introduced into the reactor until the pressure is 0.001-10 MPa, and the protective gas is argon gas.
10. In step (1), the temperature in the first stage of the three-stage heat treatment is 330 to 470 K; In step (1), the warming time in the first stage of the three-stage heat treatment is 0 to 24 hours (excluding 0); In step (1), the temperature in the second stage of the three-stage heat treatment is 670 to 730 K (but does not include 730 K); In step (1), the warming time in the second stage of the three-stage heat treatment is 0 to 24 hours (but does not include 0); In step (1), the temperature in the third stage of the three-stage heat treatment is 730 to 830 K (but does not include 830 K); The method according to any one of claims 1 to 9, wherein in step (1), the incubation time in the third stage of the three-stage heat treatment is 0 to 24 hours (excluding 0).
11. In step (2), the first set temperature is 830 to 840 K; The method according to any one of claims 2 to 10, wherein in step (2), the temperature rise time to the first set temperature is 0 to 24 hours (but does not include 0).
12. In step (2), the pressure in the reactor is reduced to 1000 Pa or less by evacuation, In step (2), the inert gas is introduced to adjust the pressure of the reactor to 0.001 to 1 MPa; In step (2), the second set temperature is 600 to 700 K; The method according to any one of claims 1 to 11, wherein in step (2), the incubation time for keeping the temperature at the second set temperature is 0 to 24 hours (but does not include 0).
13. The method according to any one of claims 1 to 12, further comprising cooling to room temperature after keeping at the second set temperature in step (2).
14. (1) Putting a rare earth magnetic material into a reactor, evacuating to 1000 Pa or less, introducing a nitrogen-containing gas, heating to 370-420 K and keeping the temperature for 0.1-5 h, heating to 690-710 K and keeping the temperature for 0.1-5 h, heating to 750-780 K and keeping the temperature for 0.1-5 h, and obtaining a semi-finished product; (2) heating the semi-finished product in step (1) to 830-840K for 0.5-5h, adjusting the temperature to 620-670K, drawing a vacuum, reducing the pressure in the reactor to 1000Pa or less, introducing an inert gas to adjust the pressure in the reactor to 0.001-1MPa, keeping the temperature at the second set temperature for 0.5-5h, and cooling to room temperature to obtain a nitride-type rare earth magnetic material. The method according to any one of claims 1 to 13, further comprising the steps of:
15. A nitrided rare earth magnetic material obtained by the method for nitriding a rare earth magnetic material according to any one of claims 1 to 14.
Citation Information
Patent Citations
Manufacture of molded product made of sm - fe - n group anisotropic magnet material
JP1992233709A
Manufacture of magnetic material
JP1995029715A
Method for producing rare earth magnet powder, and rare earth bond magnet
JP2008106325A
Method for producing rare earth-iron-nitrogen-based magnet powder
JP2014122392A
Process for the production of shaped body from an anisotropic magnetic material based on the Sm-Fe-N system
US5137587A