Method for rolling high toughness low alloy high strength steel bars

The rolling method for low-alloy high-strength steel integrates microalloy elements and controlled cooling to enhance strength and toughness, eliminating offline normalizing and reducing costs, achieving superior mechanical properties.

JP7562018B2Active Publication Date: 2024-10-04DAYE SPECIAL STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023569599
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-12
Filing Date
2022-05-11
Publication Date
2024-10-04
Estimated Expiration
2042-05-11

AI Technical Summary

Technical Problem

Conventional steel rolling methods for low-alloy high-strength steel fail to combine strength and toughness, require an offline normalizing step, and are costly, lacking energy efficiency and green manufacturing practices.

Method used

A rolling method involving a four-stage heating process, continuous rolling with controlled cooling, and online thermomechanical processing to produce high-toughness low-alloy high-strength steel, eliminating offline normalizing and incorporating microalloy elements like vanadium to enhance hardenability and grain refinement.

Benefits of technology

The method achieves high tensile and yield strengths, fine grain size, and improved impact toughness, reducing production costs and time while maintaining excellent mechanical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562018000009
    Figure 0007562018000009
  • Figure 0007562018000010
    Figure 0007562018000010
  • Figure 0007562018000011
    Figure 0007562018000011
Patent Text Reader

Abstract

The present invention provides a rolling method for producing a high-strength, low-alloy steel with high toughness, which sequentially includes a heating step, a phosphorus removal step, a rough rolling step, a continuous rolling step, a first water cooling step, a finish rolling step, a second water cooling step, and a cold bed cooling step, and which uses a converter continuous cast billet as a raw material, and the chemical components and contents thereof in the continuous cast billet, in mass%, are C≦0.20, Si≦0.60, Mn1.00-1.70, Cr≦0.30, P≦0.020, S≦0.020, V0.05-0.10, Al≦0.03, N≦0.025, and the remainder being Fe and unavoidable impurities. Using this rolling method, the actual grain size of the low alloy high strength steel can be refined, and the comprehensive performance of the low alloy high strength steel is excellent, the metallurgical structure is fine ferrite and pearlite, the grain size reaches 9.0 grade or above, the -20°C impact energy is greater than 100J, and the -40°C impact energy is greater than 80J.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of steel rolling, and in particular to a method for rolling high toughness, low alloy, high strength steel. [Background technology]

[0002] With the economic development of society and the progress of science and technology, steel materials have been widely applied in various fields, among which low alloy high strength steel has high strength, good plasticity and toughness, and is therefore widely used in high-end fields such as aerospace and ships, especially infrastructure facilities such as oil pipelines, bridges, large buildings, vehicles, containers and machinery, chemical industry, medical care, light industrial equipment, etc. Low alloy high strength steel has high strength, excellent formability and stable comprehensive performance, and is therefore widely used in machinery equipment, vehicles, pipe manufacturing and other fields.

[0003] At present, the methods for increasing the strength of steel materials include solid solution strengthening, dislocation strengthening, fine grain strengthening, and second phase particle precipitation strengthening, among which the effect of fine grain strengthening is the most prominent, and the steel material after fine grain strengthening has relatively good strength and toughness. With the refinement of grains and the improvement of crack extension resistance, the fatigue strength of steel increases, toughness improves, and the brittle turning point temperature decreases. Fine grain steel has good strength and toughness combination and is widely used in the fields of automobiles, ships, bridges, engineering machinery and other fields.

[0004] The prior art has been unable to achieve both the strength and toughness of low alloy high strength steels. The prior art only relates to the rolling methods of steel plates and strips, and does not relate to the rolling methods of round bar steel. In addition, an offline normalizing step is required during the rolling process, which increases production costs and is disadvantageous to energy saving, cost reduction and green manufacturing. Summary of the Invention [Problem to be solved by the invention]

[0005] In response to the shortcomings of the prior art, the present invention provides a rolling method for producing a high toughness low alloy high strength steel, and through the micro-alloying element and rolling control and cooling control process technology, a reasonable production process control is established, and a rolling method for producing a high toughness low alloy high strength steel is successfully developed, and in the production process of the product, the step of off-line normalizing is eliminated, the process production flow is reduced, and the production cost is saved. The low alloy high strength steel produced by using this process and method has a metallurgical structure of fine ferrite and pearlite, a tensile strength of more than 630 MPa, a yield strength of more than 500 MPa, a fine and uniform grain size after rolling, and a grain size of 9.0 or more, and the comprehensive mechanical performance far exceeds that of ordinary rolling processes. [Means for solving the problem]

[0006] In order to achieve the above object, the present invention provides the following technical solutions: A rolling method for producing a high-toughness low-alloy high-strength steel, the rolling method including a heating step, a phosphorus removal step, a rough rolling step, a continuous rolling step, a first water cooling step, a finish rolling step, a second water cooling step, and a cold bed cooling step in sequence. The raw material is a converter continuous casting billet, and the chemical components and contents, in mass%, of the continuous casting billet of the high toughness low alloy high strength steel are C≦0.20, Si≦0.60, Mn 1.00~1.70, Cr≦0.30, P ≦0.020, S ≦0.020, V 0.05~0.10, Al ≦0.03, N ≦0.025, and the remainder is Fe and unavoidable impurities. In a preferred embodiment of the rolling method for the high toughness low alloy high strength steel, the heating step is divided into four stages, namely, a preheating stage, a heating 1 stage, a heating 2 stage and a soaking stage. In the above-mentioned method for rolling a high-toughness low-alloy high-strength steel, in a preferred embodiment, the temperature in the preheating stage is 750° C. or less. In the above-mentioned method for rolling a high-toughness low-alloy high-strength steel, as a preferred embodiment, the temperature in the first heating stage is 900 to 1050°C. In the above-mentioned method for rolling a high-toughness low-alloy high-strength steel, as a preferred embodiment, the temperature in the two heating stages is 1050 to 1150°C. In the above-mentioned method for rolling a high-toughness low-alloy high-strength steel, as a preferred embodiment, the temperature of the soaking stage is 1150 to 1210°C. In the above-mentioned method for rolling a high-toughness low-alloy high-strength steel, as a preferred embodiment, the total heating time of the heating step is 3 to 5 hours. In a preferred embodiment of the rolling method for producing a high-toughness low-alloy high-strength steel, the soaking time in the soaking stage is 30 to 80 minutes. In the above-mentioned rolling method for high toughness low alloy high strength steel, as a preferred embodiment, the heating step is carried out in a four-stage stepping heating furnace. In a preferred embodiment of the rolling method for producing a high toughness low alloy high strength steel, in the rough rolling step, the rough rolling inlet temperature is 950 to 1050°C, the rough rolling passes are 5 to 7 passes, and preferably, in the rough rolling step, the number of rough rolling mills is 6. In the above-mentioned rolling method for producing a high toughness low alloy high strength steel, in a preferred embodiment, the continuous rolling step includes intermediate rolling and pre-finish rolling. In the above-mentioned method for rolling a high-toughness low-alloy high-strength steel, as a preferred embodiment, the entrance temperature of the intermediate rolling is 900 to 1000°C. In a preferred embodiment of the rolling method for producing a high toughness low alloy high strength steel, the intermediate rolling is performed with six intermediate rolling mills and with five to seven passes, preferably six passes. In the above-mentioned method for rolling a high-toughness low-alloy high-strength steel, as a preferred embodiment, the exit temperature of the pre-finish rolling is 850 to 950°C. In a preferred embodiment of the rolling method for producing a high toughness low alloy high strength steel, the pre-finish rolling includes four pre-finish rolling mills and three to five passes, preferably four passes. In a preferred embodiment of the rolling method for producing the high toughness low alloy high strength steel, the raw material after the continuous rolling step is subjected to a first water cooling, in which the water cooling rate is 25-50°C / s and the water pressure is 0.2-0.6 MPa. In a preferred embodiment of the above-mentioned method for rolling a high-toughness low-alloy high-strength steel, the entrance rolling temperature of the finish rolling is 800 to 850°C in the finish rolling step. In a preferred embodiment of the rolling method for producing the high-toughness low-alloy high-strength steel, finish rolling is carried out using an RS mill (reducing sizing mill). In the above-mentioned rolling method for high toughness low alloy high strength steel, as a preferred embodiment, the RS mill is a 3-roll RS mill. In a preferred embodiment of the rolling method for producing the high toughness low alloy high strength steel, in the second water cooling step, the steel material after the finish rolling step is subjected to second water cooling, in which the water cooling rate is 25 to 100°C / s and the water pressure is 0.2 to 0.6 MPa. In a preferred embodiment of the rolling method for producing a high-toughness low-alloy high-strength steel, the phosphorus removal step employs high-pressure water phosphorus removal for the purpose of removing iron oxide scale, and the water pressure of the high-pressure water is 15 to 20 MPa. More preferably, the water pressure of the high pressure water is 17 to 20 MPa. In a preferred embodiment, the rolling method for producing a high-toughness low-alloy high-strength steel is a low-alloy high-strength steel bar having a high toughness, the steel bar having a size of φ60 to 120 mm. In a preferred embodiment of the rolling method for producing a high-toughness low-alloy high-strength steel, the cold bed cooling refers to air-cooling the steel material obtained after the second water-passing cooling in a cold bed.

[0007] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The addition of microalloy element vanadium V to the chemical composition of continuous casting billet improves the hardenability of steel, reduces the deformation of steel, avoids the occurrence of cracks, and further improves impact toughness. Microalloy element vanadium V has a retarding effect on recrystallization only below 900℃, so that after austenite transformation, microalloy element vanadium V is almost completely dissolved, and microalloy element N further strengthens the impact toughness of microalloy element. Make full use of the precipitation strengthening effect of microalloy element vanadium V and nitrogen N, and increase the content of microalloy element V to improve impact toughness, and dissolving microalloy element vanadium V in ferrite has a strengthening effect, forming stable carbides and refining grains. At the same time, the online TMCP process is adopted to control the nitride precipitation process and form ferrite and pearlite structures. By adopting a relatively low final rolling temperature and cooling rate, the grains are refined again. In the process of refining the grains, the strength of the steel is increased and its plasticity and impact toughness are improved, thereby achieving high strength control of mechanical properties. Using this rolling method, the actual grain size of the low alloy high strength steel can be refined, and the comprehensive performance of the obtained low alloy high strength steel is excellent, the metallographic structure is fine ferrite and pearlite, the tensile strength is greater than 630 MPa, the yield strength is greater than 500 MPa, the grain size after rolling is fine and uniform, the grain size reaches above grade 9.0, the -20°C impact energy is greater than 100J, and the -40°C impact energy is greater than 80J, and its comprehensive mechanical performance far exceeds the ordinary rolling process. (2) No offline normalizing treatment is required during rolling, and the mechanical properties can meet the requirements for use, which not only saves processing time, but also reduces costs and improves efficiency. [Brief description of the drawings]

[0008] [Figure 1] This is the metallographic structure obtained in Comparative Example 2 using a rolling diameter of 80 mm. [Diagram 2] This is the grain size (7.5 class) obtained in Comparative Example 2 using a rolling diameter of 80 mm. [Diagram 3] This is a metallographic structure obtained for a rolling mill of φ80 mm standard in Example 2 of the present invention. [Figure 4] This is the grain size (9.0 class) obtained in Example 2 of the present invention using a rolling mill with a rolling diameter of 80 mm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The technical solutions in the embodiments of the present invention will be described below clearly and completely with reference to the drawings in the embodiments of the present invention, but obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative labor, belong to the scope of protection of the present invention.

[0010] The rolling method disclosed in the present invention is designed based on the continuous rolling process parameters, and by combining the solid phase transition and plastic deformation of the rolling principle, plastic sawing is performed through a four-stage stepping heating furnace heating process regime and rolling reduction regime, and the lumber is sawn through the rough rolling, intermediate rolling and finish rolling deformation regimes, and finally the metal solid phase transition is controlled through the cooling control process, so as to obtain the required product with good microstructural morphology and excellent microstructural mechanical performance.

[0011] The technical solution of the present invention will be described in more detail below by examples with reference to the drawings.

[0012] A rolling method for producing a high-strength, low-alloy steel with high toughness, the rolling method sequentially includes a heating step, a phosphorus removal step, a rough rolling step, a continuous rolling step, a first water cooling step, a finish rolling step, a second water cooling step, and a cold bed cooling step, in which a converter continuous cast billet is used as a raw material, and the chemical components and contents thereof in mass% in the continuous cast billet are: C≦0.20, Si≦0.60, Mn 1.00-1.70, Cr≦0.30, P≦0.020, S≦0.020, V 0.05-0.10, Al≦0.03, N≦0.025, and the remainder being Fe and unavoidable impurities.

[0013] The addition of micro-alloy element vanadium V to the chemical composition of the continuous casting billet improves the hardenability of the steel, reduces the deformation and cracking of the steel, and further improves the impact toughness. The micro-alloy element vanadium V has a retarding effect on recrystallization only below 900℃, so that after the austenite transformation, the micro-alloy element vanadium V is almost completely dissolved, and the micro-alloy element N further strengthens the impact toughness of the micro-alloy element vanadium V, and makes full use of the precipitation strengthening effect of the micro-alloy element vanadium V and nitrogen N.

[0014] The reason why the refinement of grains can improve plasticity and toughness is that fine grains provide better conditions for the occurrence and extension of plastic deformation. Any factor that reduces the austenite to ferrite transition temperature Ar3 tends to refine grains. The addition of the microalloy element V content increases impact toughness, and the microalloy element vanadium V dissolves in ferrite to strengthen it, form stable carbides, and refine grains.

[0015] The rolling method includes the following steps in sequence: (1)Heating The heating step is carried out in a four-stage stepping heating furnace, and the heating step is divided into four stages, namely, a pre-heating stage, a heating stage 1, a heating stage 2, and a soaking stage. The temperature of the pre-heating stage is below 750°C (for example, 600°C, 650°C, 665°C, 700°C, 750°C, and an interval or interval point between any two of these temperatures). That is, if the furnace temperature exceeds 750°C, the thermal conductivity of the billet will be too fast and the temperature difference between the billet and the heating furnace will be too large, which may further cause cracks to occur on the surface of the cast billet or final rolled material. The temperature of the first heating stage is 900 to 1050°C (for example, 900°C, 950°C, 980°C, 1000°C, 1010°C, 1050°C, and a section or point between any two of these temperatures). The temperature of the second heating stage is 1050 to 1150°C (for example, 1050°C, 1080°C, 1100°C, 1110°C, 1130°C, 1150°C, and a section or point between any two of these temperatures). The main functions of the first and second heating stages are to reduce energy consumption and reduce oxidation burnout of the billet. The temperature of the soaking stage is 1150 to 1210°C (e.g., 1150°C, 1160°C, 1165°C, 1170°C, 1185°C, 1190°C, 1205°C, 1210°C, and a section or section point between any two of these temperatures). The main functions of the soaking stage are to reduce energy consumption, reduce oxidation burnout of the billet, and reduce decarbonization of the billet. The total heating time of the heating step is 3 to 5 h (e.g., 3.5 h, 4 h, 4.5 h, 4.8 h, or any time between any two of those time periods), and the soaking time of the soaking stage is 30 to 80 min (e.g., 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, 70 min, 75 min, 80 min, or any time between any two of those time periods). The heating steps achieve four goals: first, omitting the offline normalizing step reduces energy consumption and saves costs, second, the four-stage heating process reduces the oxidation burnout of the billet, third, reduces the decarbonization of the billet, and fourth, reduces the surface cracks of the final rolled material caused by too long a heating time.

[0016] (2) Phosphorus removal For the heated billet, high-pressure water dephosphorization is used to remove the iron oxide scale, and the pressure of the high-pressure water is 15-20 MPa (for example, 15 MPa, 16.5 MPa, 17 MPa, 18 MPa, 20 MPa, or a pressure value between any two of these pressure values), and the pressure value of the high-pressure water is preferably 17-20 MPa. When high-pressure water is used to remove the iron oxide scale on the steel surface, if the pressure is lower than 15 MPa, the cleaning of the surface iron oxide scale will be dirty and incomplete, which will affect the rolling effect of the steel.

[0017] (3)Rough rolling The rough rolling step preferably has 6 rough rolling mills, the inlet temperature of the rough rolling is 950-1050°C (for example, 950°C, 980°C, 1000°C, 1020°C, 1035°C, 1050°C, and intervals or interval points between any two of these temperatures), the rough rolling passes are 5-7 passes, and the rough rolling passes are preferably 6 passes. The rough rolling step adopts a rolling method of continuous rolling, mainly changing the size of the blank surface of the billet by plastic deformation, and the groove design adopts a box-shaped groove design, and the blank cross-sectional shape is changed and reduced by a large reduction process.

[0018] (4) Continuous rolling The continuous rolling step includes intermediate rolling and pre-finish rolling, the inlet temperature of intermediate rolling is 900-1000°C (for example, 905°C, 920°C, 940°C, 950°C, 970°C, 1000°C, and intervals or interval points between any two temperatures therein), it is preferable to install 6 intermediate rolling mills in the intermediate rolling step, the number of passes of intermediate rolling is 5-7 passes, and 6 passes of intermediate rolling are preferred. The caliber design mainly adopts elliptical and circular caliber design, and the blank cross-sectional shape is made closer to the finished product shape through the rolling process. The exit temperature of the pre-finish rolling is 850-950°C (for example, 855°C, 870°C, 890°C, 900°C, 910°C, 920°C, 930°C, 940°C, 950°C, and intervals or intervals between any two of these temperatures), and it is preferable to install four pre-finish rolling mills in the pre-finish rolling step, and the number of passes of the pre-finish rolling is 3-5, and the number of passes of the pre-finish rolling is preferably 4. The caliber design mainly adopts elliptical and circular caliber designs, and the blank cross-sectional shape is made closer to the finished product shape through the rolling process.

[0019] (5) 1st water cooling The raw material after the continuous rolling step is subjected to a first water cooling, and the temperature after the first water cooling step is 750 to 800°C (for example, 750°C, 765°C, 780°C, 795°C, 798°C, 800°C, and an interval or interval point between any two of these temperatures), in which the water cooling rate of the first water cooling is 25 to 50°C / s and the water pressure is 0.2 to 0.6 MPa. By controlling the temperature and water cooling rate of the first water cooling, the steel temperature before finish rolling is controlled and a target temperature required for finish rolling is obtained.

[0020] (6) Finish rolling The rolled material obtained in step (5) is fed into an RS finishing rolling mill for rolling, and the RS finishing rolling mill is preferably a 3-roll RS mill, i.e., a KOCKS RS finishing rolling mill, and the inlet rolling temperature is 800 to 850°C (e.g., 800°C, 810°C, 820°C, 824°C, 832°C, 850°C, and an interval or interval point between any two of these temperatures). Finish rolling using a 3-roll RS mill can better perform low-temperature rolling, thereby improving the grain size and overall mechanical performance of the non-heat treated steel, and providing its excellent performance for the production of non-heat treated steel.

[0021] (7)Second water cooling The steel material after finish rolling is subjected to a second water cooling, and the temperature of the second water cooling of the steel material after the finish rolling step is 600 to 700°C (for example, 600°C, 625°C, 640°C, 662°C, 683°C, 700°C, and an interval or interval point between any two of these temperatures), in which the water cooling rate is 25 to 100°C / s and the water pressure is 0.2 to 0.6MPa. The second water cooling is performed after finish rolling, and the temperature and water cooling rate of the second water cooling are controlled to control the steel material temperature, thereby obtaining the final required metallographic structure and mechanical properties of the steel material.

[0022] (8) Cold frame cooling, i.e. cold frame air cooling The steel obtained after the second water cooling was air-cooled in a cold bed to finally obtain the finished steel product.

[0023] The controlled rolling and controlled cooling techniques described in steps (1) to (8) are the main steps for refining the grain size of high carbon steels, and the heating temperature, deformation degree and cooling rate are comprehensively controlled to refine the actual grain size and achieve the purpose of improving the stiffness and toughness of the steel.

[0024] At the same time, the online TMCP process (i.e., thermomechanical control process) is adopted to control the nitride precipitation process and form uniform ferrite and pearlite structures. By adopting a relatively low final rolling temperature and cooling rate, the grains are refined again. In the process of refining the grains, the strength of the steel is increased and its plasticity and impact toughness are improved, thereby achieving high strength control of mechanical properties.

[0025] The rolling method of the high toughness low alloy high strength steel of the present invention is unique, and uses the cooperation of micro-alloying elements and rolling cooling control technology of thermomechanical control process to realize online control, and the actual grain size of the high toughness low alloy high strength steel can be refined by using this process method, and the high toughness low alloy high strength steel has excellent comprehensive performance, fine ferrite and pearlite metallurgy structure, tensile strength is greater than 630MPa, yield strength is greater than 500MPa, the grain size after rolling is fine and uniform, the grain size reaches above grade 9.0, -20°C Charpy V impact energy is greater than 100J, and -40°C Charpy V impact energy is greater than 80J, and its comprehensive mechanical performance far exceeds that of ordinary rolling methods.

[0026] The high toughness low alloy high strength steel does not require offline normalizing treatment during the manufacturing process, and the mechanical properties can meet the requirements for use, thus not only saving processing time, but also reducing costs and improving efficiency.

[0027] Example 1 Example 1 provides a rolling method for high toughness low alloy high strength steel, in which the required finished product specification is φ65mm, and a continuous cast billet with a cross section of 300×400mm is selected, in which the chemical components in the continuous cast billet are shown in Table 2 in mass%, and the mass fraction totals 100%. The rolling method for the high toughness low alloy high strength steel includes the following steps: (1) Heating: After the cross-section continuous casting billet is cut, it is heated in a four-stage stepping heating furnace by using a cold transfer method. The temperature of the pre-heating stage is 685°C, the temperature of the first heating stage is 1005°C, the temperature of the second heating stage is 1086°C, and the temperature of the soaking stage is 1175°C. The total heating time of this heating step is 3.8h, and the soaking time of the soaking stage is 43min. (2) Phosphorus removal: After heating, the billet is subjected to high-pressure water phosphorus removal to remove the iron oxide scale, and the pressure of the high-pressure water is 18.0 MPa. (3) Rough rolling: The billet after phosphorus removal is put into a high-rigidity rough rolling mill (6 units) for rough rolling to obtain a rough rolled billet. The rough rolling inlet temperature is 1015°C, and the rough rolling pass is 6 passes. (4) Continuous rolling: The rough rolled billet obtained in step (3) is fed into a continuous rolling unit, the intermediate rolling entrance temperature is 925°C, the intermediate rolling passes are 6 passes, the pre-finished rolled billet exit temperature is 910°C, and the pre-finished rolled billet passes are 4 passes. (5) First water cooling: The rolled material after the preliminary finish rolling is subjected to the first water cooling to cool the temperature to 790°C, the water cooling rate is 40°C / s, and the water pressure is 0.5MPa. (6) Finish rolling: The rolled material having a standard of φ80 mm obtained after the preliminary finish rolling is rolled by a KOCKS RS mill. The inlet temperature of the rolled material during rolling in the RS mill is 845°C, and a steel bar having a standard of φ65 mm is obtained. (7) Second water cooling: The rolled material after finish rolling is subjected to the second water cooling to cool the temperature to 685°C, the water cooling rate is 75°C / s, and the water pressure is 0.6MPa. (8) Cold bed cooling (cold bed air cooling): The steel bar having a size of φ65 mm obtained in step (7) is air-cooled in a cold bed to finally obtain the finished steel bar.

[0028] The hot-rolled structure of the high-toughness low-alloy high-strength steel obtained in Example 1 is uniform ferrite and pearlite, the actual grain size is 9.0 class, and the mechanical properties of the steel product are shown in Table 3. The hot-rolled structure of the high-toughness low-alloy high-strength steel obtained in Example 1 is uniform ferrite and pearlite, the actual grain size is 9.0 class, and as can be seen from Table 3, the mechanical properties of the steel product are excellent.

[0029] Example 2 Example 2 provides a rolling method for high toughness low alloy high strength steel, the required finished product specification is φ80mm, and a 300×400mm cross section continuous cast billet is selected, in which the chemical components in the continuous cast billet are shown in Table 2 in mass%, and the mass fraction totals 100%. The rolling method includes the steps of (1) heating, (2) phosphorus removal, (3) rough rolling, (4) continuous rolling, (5) first water cooling, (6) finish rolling, (7) second water cooling, and (8) cold bed cooling (cold bed air cooling), in order. The processing steps of Example 2 are the same as those of Example 1, and the processing parameters of the specific steps are shown in Table 1, and the mechanical properties of the steel product are shown in Table 3.

[0030] The hot-rolled structure of the high-toughness low-alloy high-strength steel obtained in Example 2 is uniform ferrite and pearlite as shown in Figure 3, and the actual grain size is 9.0 class as shown in Figure 4. As can be seen from Table 3, the steel product has excellent mechanical properties.

[0031] Example 3 Example 3 provides a rolling method for high toughness low alloy high strength steel, the required finished product specification is φ100mm, and a 300×400mm cross section continuous cast billet is selected, in which the chemical components in the continuous cast billet are shown in Table 2 in mass%, and the mass fraction totals 100%. The rolling method includes the steps of (1) heating, (2) phosphorus removal, (3) rough rolling, (4) continuous rolling, (5) first water cooling, (6) finish rolling, (7) second water cooling, and (8) cold bed cooling (cold bed air cooling), in order. The processing steps of Example 3 are the same as those of Example 1, and the processing parameters of the specific steps are shown in Table 1, and the mechanical properties of the steel product are shown in Table 3.

[0032] The hot-rolled structure of the high-toughness low-alloy high-strength steel obtained in Example 3 is uniform ferrite and pearlite, and the actual grain size is 9.0 class. As can be seen from Table 3, the steel product has excellent mechanical properties.

[0033] The specific processing step parameters for Examples 1 to 3 are shown in Table 1.

[0034] [Table 1]

[0035] The chemical compositions of the continuous cast billets selected in Examples 1 to 3 are shown in Table 2.

[0036] [Table 2]

[0037] Table 3 shows the performance in each item of the high-toughness, low-alloy, high-strength steels obtained in Examples 1 to 3.

[0038] [Table 3]

[0039] Examples 4 to 7 Examples 4 to 7 provide a rolling method for high toughness low alloy high strength steel, which includes the steps of (1) heating, (2) phosphorus removal, (3) rough rolling, (4) continuous rolling, (5) first water cooling, (6) finish rolling, (7) second water cooling, and (8) cold bed cooling (cold bed air cooling) in sequence. The processing steps and machine parameters of Examples 4 to 7 are the same as those of Example 1. The contents of each chemical component in the continuous casting billet used in Examples 4 to 7 are shown in Table 4 in mass%, and the mass fractions total 100%.

[0040] [Table 4]

[0041] Table 5 shows the performance in each item of the high-toughness, low-alloy, high-strength steels obtained in Examples 4 to 7.

[0042] [Table 5]

[0043] As can be seen from Table 5, the hot-rolled structure of the high-toughness low-alloy high-strength steels obtained in Examples 4 to 7 is uniform ferrite and pearlite, the actual grain size is 9.0 class, and the steel products have excellent mechanical properties.

[0044] Comparative Example 1 The required finished product specification is φ65mm, and a 300×400mm cross-section continuous casting billet is selected. The chemical components and contents of the continuous casting billet are C0.45, Si0.28, Mn1.46, Cr0.16, V0.06, N0.010, Al0.020, P≦0.020, S≦0.020, and the rest is Fe and unavoidable impurities. The alloy steel processing steps and parameters are shown in Table 7.

[0045] As shown in Table 6, the C content in the chemical composition of the continuous casting billet is 0.45%, that is, C>0.20; therefore, as shown in Table 8, the elongation of the rolled steel is 18%, the -20℃ Charpy V impact energy is 32J, and the -40℃ Charpy V impact energy is 17J.

[0046] Comparative Example 2 The required finished product specification is φ80mm, and a 300×400mm cross-section continuous casting billet is selected. The chemical components and contents of the continuous casting billet are C0.16, Si0.30, Mn0.8, Cr0.15, V0.07, N0.012, Al0.020, P≦0.020, S≦0.020, and the rest is Fe and unavoidable impurities. The alloy steel processing steps and parameters are shown in Table 7.

[0047] As shown in Table 6, the manganese (Mn) content in the chemical composition of the continuous casting billet is 0.8, i.e., Mn<1.0; therefore, as shown in Table 8, the elongation of the rolled steel is 26%, the Charpy V impact energy at -20°C is 54J, and the Charpy V impact energy at -40°C is 25J.

[0048] Comparative Example 3 The required finished product specification is φ100mm, and a 300×400mm cross-section continuous casting billet is selected. The chemical components and contents of the continuous casting billet are C0.16, Si0.30, Mn1.40, Cr0.15, N0.011, Al0.022, P≦0.020, S≦0.020, and the rest is Fe and unavoidable impurities. The alloy steel processing steps and parameters are shown in Table 7.

[0049] As shown in Table 6, vanadium V is not added to the chemical composition of the continuous casting billet, so as shown in Table 8, the elongation of the rolled steel is 25%, the -20℃ Charpy V impact energy is 35J, and the -40℃ Charpy V impact energy is 19J.

[0050] Comparative Example 4 The required finished product specification is φ90mm, and a 300×400mm cross-section continuous casting billet is selected. The chemical components and contents of the continuous casting billet are C0.16, Si0.32, Mn1.47, Cr0.15, V0.06, N0.040, Al0.020, P≦0.020, S≦0.020, and the rest is Fe and unavoidable impurities. The alloy steel processing steps and parameters are shown in Table 7.

[0051] As shown in Table 6, the nitrogen N content in the chemical composition of the continuous casting billet is 0.040, i.e., N>0.025; therefore, as shown in Table 8, the elongation of the rolled steel is 27%, the Charpy V impact energy at -20°C is 62J, and the Charpy V impact energy at -40°C is 37J.

[0052] As can be seen from Table 8, in terms of the mechanical properties of the steel materials obtained by the rolling methods of Comparative Examples 1 to 4 compared to the rolling method disclosed in the present application, the -20°C Charpy V-type impact energy was all less than 100 J, the -40°C Charpy V-type impact energy was all less than 80 J, and the grain size of the alloy steel material after rolling did not reach grade 9.0 or more.

[0053] [Table 6]

[0054] The alloy steel processing steps and parameters of Comparative Examples 1 to 4 are shown in Table 7.

[0055] [Table 7]

[0056] Table 8 shows the performances of the alloy steel materials obtained in Comparative Examples 1 to 4.

[0057] [Table 8]

[0058] Although the preferred embodiments of the present invention have been described, other changes and modifications to these embodiments may be made by those skilled in the art. Therefore, the appended claims should be interpreted to include the preferred embodiments and all such changes and modifications that fall within the scope of the present invention.

[0059] The above is only a preferred embodiment of the present invention, and is not used to limit the present invention, and those skilled in the art can make various modifications and variations to the present invention. Any amendments, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. The method includes a heating step, a phosphorus removal step, a rough rolling step, a continuous rolling step, a first water cooling step, a finish rolling step, a second water cooling step, and a cold bed cooling step in sequence; A converter continuous casting billet is used as a raw material, and the chemical components and contents in the continuous casting billet are, in mass%, C≦0.20, Si≦0.60, Mn 1.37-1.70, Cr≦0.30 (excluding 0%), P≦0.020, S≦0.020, V 0.07-0.10, Al≦0.03, N 0.008-0.025, and the remainder is Fe and unavoidable impurities, The heating step is divided into four stages, namely, a preheating stage, a first heating stage, a second heating stage, and a soaking stage, The temperature of the preheating stage is equal to or lower than 750° C. The temperature of the first heating stage is 900 to 1050° C. The temperature of the second heating stage is 1050 to 1150° C. The temperature of the soaking stage is 1150 to 1210° C. The total heating time of the heating step is 3 to 5 h, and the soaking time of the soaking stage is 30 to 80 min; In the phosphorus removal step, high pressure water phosphorus removal is used to remove iron oxide scale, and the water pressure of the high pressure water is 15-20 MPa; In the rough rolling step, the rough rolling inlet temperature is 950 to 1050 ° C., and the rough rolling pass is 5 to 7 passes; The continuous rolling step includes intermediate rolling and preliminary finishing rolling, The inlet temperature of the intermediate rolling is 900 to 1000° C., and the number of passes of the intermediate rolling is 5 to 7 passes. The exit temperature of the pre-finish rolling is 850 to 950° C., and the number of passes of the pre-finish rolling is 3 to 5 passes. The first water cooling is a first water cooling of the raw material after the continuous rolling step, in which the water cooling rate is 25-50°C / s, the water pressure is 0.2-0.6MPa, and the temperature after the first water cooling is 765-800°C; In the finish rolling step, the entrance rolling temperature of the finish rolling is 832 to 850 ° C., The second water cooling is performed on the steel material after the finish rolling step at a temperature of 600°C to 700°C, wherein the water cooling rate is 25 to 100°C / s and the water pressure is 0.2 to 0.6 MPa; The cold bed cooling is to air-cool the steel material obtained after the second water cooling in a cold bed, The method for rolling a high-strength low-alloy steel bar having high toughness is characterized in that the obtained steel material has a metallurgical structure of fine ferrite and pearlite, a tensile strength of more than 630 MPa, a yield strength of more than 500 MPa, and a grain size of 9.0 class or more.

2. The heating step is carried out in a four-stage stepping furnace.

2. The method for rolling a high-strength low-alloy steel bar having high toughness according to claim 1.

3. In the rough rolling step, the number of rough rolling mills is set to 6, and the number of passes of the rough rolling is 6.

2. The method for rolling a high-strength low-alloy steel bar having high toughness according to claim 1.

4. In the intermediate rolling, the number of intermediate rolling mills is set to 6, and the number of passes of the intermediate rolling is 6 passes.

2. The method for rolling a high-strength low-alloy steel bar having high toughness according to claim 1.

5. In the pre-finish rolling, the number of pre-finish rolling machines is set to four, and the number of passes of the pre-finish rolling is four.

2. The method for rolling a high-strength low-alloy steel bar having high toughness according to claim 1.

6. Finish rolling is performed using an RS mill.

2. The method for rolling a high-strength low-alloy steel bar having high toughness according to claim 1.

7. The RS mill is a 3-roll RS mill.

7. The method for rolling a high-strength low-alloy steel bar having high toughness according to claim 6.

8. The water pressure of the high-pressure water is 17 to 20 MPa.

2. The method for rolling a high-strength low-alloy steel bar having high toughness according to claim 1.

9. The rolling method provides a high-toughness low-alloy high-strength steel bar.

3. The method for rolling a high-strength low-alloy steel bar having high toughness according to claim 1 or 2.

10. The standard of the steel bar is φ60 to 120 mm.

10. The method for rolling a high-strength low-alloy steel bar having high toughness according to claim 9.

Citation Information

Patent Citations

  • Rolling production method capable of reducing hardness of 42CrMo

    CN106216391A

  • Low-temperature rolling production method of high-performance 20CrMnTi gear steel

    CN108906884A

  • Production of rolled steel material having excellent homogeneity

    JP1987050411A

  • Production of reinforcing steel product having high strength and low yield ratio

    JP1997125143A