Hydrophilic coating composition
The hydrophilic coating composition addresses uneven hydrophilization and durability issues by using a silane coupling agent and compounds with sulfonic acid and quaternary ammonium groups, providing effective dirt prevention and durability on ceramic surfaces.
Patent Information
- Application Number
- JP2020044430
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-13
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-03-13
AI Technical Summary
Existing hydrophilic treatment agents for ceramics struggle with uneven surface hydrophilization and insufficient durability against various cleaning detergents, leading to issues with calcium deposition and stain adhesion.
A hydrophilic coating composition comprising a silane coupling agent, a hydrophilic compound with sulfonic acid groups or alkali metal salts, and a hydrophilic compound with quaternary ammonium cationic groups, along with a radical polymerization initiator, to enhance surface hydrophilicity and durability.
The composition effectively prevents calcium deposition and enhances durability against common cleaning detergents, ensuring excellent dirt adhesion prevention and washability.
Smart Images

Figure 0007562068000001 
Figure 0007562068000002 
Figure 0007562068000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a hydrophilic treatment coating composition and a hydrophilic treatment method using the same. [Background technology]
[0002] 2. Description of the Related Art Conventionally, various surface treatments have been carried out on ceramics and other items installed around water, such as toilets and wash basins, in order to make the surfaces easier to clean.
[0003] Although not intended for cleaning surfaces, a method and specific compounds have been disclosed in which the surface of a substance mainly containing silicon oxide is treated with a silane coupling agent, and then a reactive surfactant having a reactive group such as an acryloyl group or a vinyl group in the side chain or in the middle of a hydrophobic group is reacted with the surface in order to impart anti-fogging and anti-fouling properties to glass products (see JP-A-8-259270 (Patent Document 1)).
[0004] JP 2016-20461 A (Patent Document 2) discloses a hydrophilic treatment coating composition which is prepared by treating a surface layer containing an inorganic compound with a silane coupling agent containing a radical reactive functional group, and then reacting the surface layer with the radical reactive functional group of the silane coupling agent, the hydrophilic treatment coating composition containing a radical reactive functional group and an alkali metal salt of a sulfonic acid group, a hydrophilic compound which does not contain a hydrophilic portion other than the ends of the molecular chain and no branched chains, a radical polymerization initiator, and a polar compatibilizer. JP 2016-20462 A (Patent Document 3) discloses a hydrophilic treatment coating composition which comprises treating a surface layer containing an inorganic compound with a silane coupling agent containing at least one reactive functional group selected from an isocyanate group, an epoxy group, an amino group, and a mercapto group, and then reacting with the reactive functional group of the silane coupling agent, the composition containing a functional group which is at least one selected from an amino group, a hydroxyl group, a mercapto group, and an epoxy group and which reacts with the reactive functional group of the silane coupling agent, a hydrophilic compound which contains a sulfonic acid group or an alkali metal salt of a sulfonic acid group and does not contain a hydrophilic portion other than at the ends of the molecular chain, and a polar compatibilizer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-259270 [Patent Document 2] JP 2016-20461 A [Patent Document 3] JP 2016-20462 A Summary of the Invention [Problem to be solved by the invention]
[0006] In the method using the compound described in Patent Document 1, since the compound has a branched chain structure, the hydrophilic portion is unlikely to aggregate on the surface, and there is a concern that the compound may not have sufficient cleaning properties even when used on pottery that is frequently washed with water, such as toilet bowls and washbasins. On the other hand, when a compound without a branched structure is used, the hydrophilic group is highly hydrophilic, so that the compound is likely to crystallize, making it difficult to uniformly hydrophilize the surface of pottery, etc.
[0007] It is described that the hydrophilic treatment agents described in Patent Documents 2 and 3 prevent calcium deposition and facilitate cleaning of oily dirt that causes bacterial growth and odors when used on ceramics such as toilets and washstands that contain inorganic compounds such as silicon oxide. On the other hand, the ceramics are often cleaned using cleaning detergents in ordinary households, and a wide variety of cleaning detergents are commercially available. There is a demand for the development of new detergents with higher cleaning capabilities, and various new products have actually appeared. The hydrophilic treatment agents that can be used on the ceramics are required to have excellent durability against various new cleaning detergents.
[0008] The present invention is to solve the above-mentioned conventional problems, and its object is to provide a hydrophilic coating composition which imparts dirt-repellent properties to substrates such as ceramics and has excellent durability of dirt-repellent properties. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention provides the following aspects. [1] A hydrophilic coating composition for inorganic substrates surface-treated with a silane coupling agent (S), A hydrophilic compound (A), and Hydrophilic compound (B) Including, The hydrophilic compound (A) is a compound having at least one of a sulfonic acid group and an alkali metal salt of a sulfonic acid group, The hydrophilic compound (B) is a compound having a quaternary ammonium cationic group. Hydrophilic coating composition. [2] A hydrophilic treatment coating composition for inorganic substrates, comprising: Silane coupling agent (S), A hydrophilic compound (A), and Hydrophilic compound (B) Including, The hydrophilic compound (A) is a compound having at least one of a sulfonic acid group and an alkali metal salt of a sulfonic acid group, The hydrophilic compound (B) is a compound having a quaternary ammonium cationic group. Hydrophilic coating composition. [3] The silane coupling agent (S) has a radical reactive functional group (R S ) The hydrophilic compound (A) has a radical reactive functional group (R A ), and The hydrophilic compound (B) has a radical reactive functional group (R B ) Further, the composition includes a radical polymerization initiator. [1] or [2]. A hydrophilic coating composition according to the present invention. [4] The silane coupling agent (S) has one condensation type reactive functional group (R S2 ) is a monofunctional silane coupling agent having The hydrophilic compound (A) has a condensation type reactive functional group (R A2 ) The hydrophilic compound (B) has a condensation type reactive functional group (R B2 ) [1] or [2]. A hydrophilic coating composition according to the present invention. [5] The radical reactive functional group (R A ) and (R B) is at least one selected from an acrylamide group, an acryloyl group, a methacryloyl group, an allyl group, a vinyl group, a styryl group, and a mercapto group. [6] The hydrophilic treatment coating composition according to any one of [1] to [5], wherein the hydrophilic compound (A) has no hydrophilic moieties other than at the ends of the molecular chain. [7] The hydrophilic treatment coating composition according to any one of [1] to [6], wherein the hydrophilic compound (B) has no hydrophilic moiety other than at the end of the molecular chain. [8] The number average molecular weight of the hydrophilic compound (A) is 70 to 500, The number average molecular weight of the hydrophilic compound (B) is 70 to 500. The hydrophilic treatment coating composition according to any one of [1] to [7]. [9] The radical reactive functional group (R A The average number of carbon atoms between the alkyl group and the sulfonic acid group is (n1), The radical reactive functional group (R B ) and the quaternary ammonium cationic functional group, the average number of carbon atoms present between them is (n2); The above (n1) and (n2) are (n2)>(n1) The hydrophilic treatment coating composition according to any one of [3] and [5] to [8], which has the relationship:
[10] The condensed reactive functional group (R A2 The average number of carbon atoms between the sulfonic acid group and the 12 )year, The condensed reactive functional group (R B2 The average number of carbon atoms between the quaternary ammonium cationic functional group and the quaternary ammonium cationic functional group is (n 22 )year, The above (n 12 ) and the above (n 22 )but, (n 22 )>(n 12 ) The hydrophilic treatment coating composition according to any one of [4] and [6] to [8], which has the relationship:
[11] [1]-
[10] , in the hydrophilic treatment coating composition according to any one of the above, the hydrophilic compound (A) and the hydrophilic compound (B) are stored separately from each other. Hydrophilic treatment paint composition set.
[12] A step of surface-treating a surface of an inorganic substrate with a silane coupling agent (S); Applying the hydrophilic treatment coating composition according to any one of [1] and [3] to
[11] to the inorganic substrate treated with the silane coupling agent (S), The silane coupling agent (S) and and reacting the hydrophilic compound (A) with at least one of the hydrophilic compounds (B).
[13] [2] to
[11] , exposing the hydrophilic treatment coating composition according to any one of the above to light or heat; The method includes reacting the silane coupling agent (S) with at least one of the hydrophilic compound (A) and the hydrophilic compound (B), The hydrophilic treatment coating composition after the reaction is applied to a surface of an inorganic substrate. A method for hydrophilizing inorganic substrates.
[14] A hydrophilic treatment coating composition according to any one of [2] to
[11] is applied to a surface of an inorganic substrate, The method includes reacting the silane coupling agent (S) with at least one of the hydrophilic compound (A) and the hydrophilic compound (B) by light irradiation or heating. A method for hydrophilizing inorganic substrates.
[15] The method for hydrophilization of an inorganic substrate according to any one of
[12] to
[14] , comprising reacting the silane coupling agent (S) with at least one of the hydrophilic compound (A) and the hydrophilic compound (B) by light irradiation.
[16] The inorganic substrate is sanitary ware.
[12] ~
[15] 10. The hydrophilization treatment method according to any one of the above. Effect of the Invention
[0010] By using the above-mentioned hydrophilic treatment coating composition, it is possible to effectively prevent deposition of calcium and the like on ceramics that contain inorganic compounds such as silicon oxide and are installed around water such as toilets and washstands. The above-mentioned hydrophilic treatment coating composition further has the advantage of excellent durability of such dirt adhesion prevention performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The above hydrophilic treatment coating composition, hydrophilic treatment coating composition set, and hydrophilic treatment method will be described below.
[0012] The hydrophilic treatment coating composition in this specification can be roughly divided into the following first and second embodiments. First aspect A hydrophilic treatment coating composition for an inorganic substrate surface-treated with a silane coupling agent (S), the hydrophilic treatment coating composition comprising: A hydrophilic compound (A), and Hydrophilic compound (B) Including, The hydrophilic compound (A) is a compound having at least one of a sulfonic acid group and an alkali metal salt of a sulfonic acid group, The hydrophilic compound (B) is a compound having a quaternary ammonium cationic group. Hydrophilic coating composition. Second aspect A hydrophilic treatment coating composition for an inorganic substrate, the hydrophilic treatment coating composition comprising: Silane coupling agent (S), A hydrophilic compound (A), and Hydrophilic compound (B) Including, The hydrophilic compound (A) is a compound having at least one of a sulfonic acid group and an alkali metal salt of a sulfonic acid group, The hydrophilic compound (B) is a compound having a quaternary ammonium cationic group. Hydrophilic coating composition.
[0013] In both the first and second embodiments, the silane coupling agent (S), the hydrophilic compound (A) and the hydrophilic compound (B) are used. Each component will be described below.
[0014] Silane coupling agent (S) The silane coupling agent (S) used in the hydrophilic treatment coating composition is a compound having both a reactive silyl group and an organic functional group in the molecule. The reactive silyl group may be a group that generates a silanol group by hydrolysis. Specific examples of the reactive silyl group include a trialkoxysilyl group (the number of carbon atoms contained in the alkoxy group is preferably 1 to 7), a dialkoxyalkyl group (the number of carbon atoms contained in the alkoxy group is preferably 1 to 7, and the number of carbon atoms contained in the alkyl group is preferably 1 to 7), and more specifically, a trimethoxysilyl group, a triethoxysilyl group, a tripropoxysilyl group, a tris(2-methoxyethoxy)silyl group, a dimethoxyalkylsilyl group, a diethoxyalkylsilyl group, a dipropoxyalkylsilyl group, and a bis(2-methoxyethoxy)alkylsilyl group (the alkyl group may be a linear or branched alkyl group having 1 to 7 carbon atoms).
[0015] An example of the organic functional group is a radical reactive functional group (R S ) can be mentioned. SExamples of the organic functional groups include an acrylamide group, an acryloyl group, a methacryloyl group, an allyl group, a vinyl group, a styryl group, a mercapto group, etc. These organic functional groups may include only one type, or may include two or more types.
[0016] Another example of the organic functional group is a condensation type reactive functional group (R S2 Condensation type reactive functional groups (R S2 Examples of the organic functional groups include a carboxy group, a hydroxy group, an amino group, an epoxy group, a ureido group, an isocyanate group, an isocyanurate group, etc. These organic functional groups may be contained alone or in combination with one or more kinds.
[0017] Specific examples of the silane coupling agent (S) include: vinyltriethoxysilane, vinyltrimethoxysilane, vinyltris(2-methoxyethoxy)silane, Vinylmethyldimethoxysilane, p-Styryltrimethoxysilane, p-steel R triethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-acryloxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-octanoylthio-1-propyltriethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-(N-phenyl)aminopropyltrimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, Tris-(trimethoxysilylpropyl)isocyanurate, etc.
[0018] The silane coupling agent (S) may be used alone or in combination of two or more kinds.
[0019] As an example of a silane coupling agent (S), the silane coupling agent (S) may be a silane coupling agent having two or more radical reactive functional groups (R S In this embodiment, at least one radical reactive functional group (R S ) and the hydrophilic compound (A) have a bonding property, and further, at least one other radical reactive functional group (R S) and the hydrophilic compound (B) have a bonding property. This effectively prevents basic cleaning ingredients such as quaternary ammonium salts, which may be contained in commercially available detergents, from forming ionic bonds with the sulfonic acids contained in the hydrophilic compound (A), and has the advantage of providing better durability in preventing dirt adhesion.
[0020] Commercially available silane coupling agents (S) may be used. Commercially available silane coupling agents include those available from Shin-Etsu Chemical Co., Ltd., Momentive Corporation, Toagosei Co., Ltd., Asahi Kasei Corporation, and the like.
[0021] It is believed that the silane coupling agent (S) undergoes a bonding reaction with the surface of an inorganic substrate, which is a substrate having an inorganic surface, via a silanol group generated by hydrolysis of a reactive silyl group.
[0022] In the first embodiment, the amount of the silane coupling agent (S) used is preferably within a range of 0.1 to 10 parts by mass, and more preferably within a range of 1 to 5 parts by mass, relative to 100 parts by mass of the total amount of the hydrophilic compounds. In the second embodiment, the amount of the silane coupling agent (S) contained in the hydrophilic treatment coating composition is preferably within the range of 0.1 to 10 parts by mass, more preferably within the range of 0.2 to 7 parts by mass, relative to 100 parts by mass of the total amount of the hydrophilic compounds. Here, the "total amount of the hydrophilic compounds" means the total amount of the hydrophilic compounds (A) and (B) when the hydrophilic compounds include the hydrophilic compounds (A) and (B).
[0023] In the above first and second embodiments, a catalyst may be used in combination with the silane coupling agent (S). Examples of the catalyst include acidic catalysts such as aqueous hydrochloric acid solutions, aqueous sulfuric acid solutions, aqueous nitric acid solutions, aqueous phosphoric acid solutions, and aqueous solutions of compounds having carboxylic acids such as formic acid, acetic acid, and propionic acid, and basic catalysts such as aqueous ammonia solutions, morpholine, N-methylmorpholine, N-ethylmorpholine, piperazine, hydroxyethylpiperazine, 2-methylpiperazine, trans 2,5-dimethylpiperazine, cis 2,6-dimethylpiperazine, triethylamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N-(β-aminoethyl)ethanolamine, N-methyldiethanolamine, Nn-butylethanolamine, Nn-butyldiethanolamine, Nt-butylethanolamine, Nt-butyldiethanolamine, N-(β-aminoethyl)isopropanolamine, N,N-diethylisopropanolamine, 2-amino-2-methyl-1-propanol, aqueous sodium hydroxide solutions, and aqueous potassium hydroxide solutions.
[0024] Hydrophilic compound (A) The hydrophilic compound (A) is a compound having at least one of a sulfonic acid group and an alkali metal salt of a sulfonic acid group (hereinafter sometimes abbreviated as "sulfonic acid groups"). By including the hydrophilic compound (A) in the hydrophilic treatment coating composition, a sulfonic acid group and / or its salt can be introduced into the inorganic substrate, thereby exerting a hydrophilic function.
[0025] The hydrophilic compound (A) preferably has, in addition to the sulfonic acid group, a functional group that reacts with the silane coupling agent (S). S ), the hydrophilic compound (A) has a radical reactive functional group (R A It is preferable that the compound has a radical reactive functional group (R AExamples of the radical reactive functional group include an acrylamide group, an acryloyl group, a methacryloyl group, an allyl group, a vinyl group, a styryl group, a mercapto group, etc. These radical reactive functional groups may include only one type, or may include two or more types.
[0026] In addition, the silane coupling agent (S) has a condensation type reactive functional group (R S2 ), the hydrophilic compound (A) has a condensation type reactive functional group (R A2 It is preferable that the condensation type reactive functional group (R A2 Examples of the reactive functional groups include a carboxy group, a hydroxy group, an amino group, an epoxy group, a ureido group, an isocyanate group, an isocyanurate group, etc. These condensation type reactive functional groups may include only one type, or may include two or more types.
[0027] The hydrophilic compound (A) preferably does not have a hydrophilic portion other than the end of the molecular chain. The "hydrophilic portion" in the hydrophilic compound (A) means sulfonic acid groups and other hydrophilic groups that the hydrophilic compound (A) has. By the hydrophilic compound (A) having such a structure, the hydrophilic groups of the hydrophilic compound (A) can be concentrated on the coating surface that is not on the inorganic substrate side, and this has the advantage that sufficient cleanability and cleaning durability can be imparted even when used for members that are frequently washed with water, such as sanitary ware.
[0028] Specific examples of the hydrophilic compound (A) include, for example, Sodium vinyl sulfonate, vinyl sulfonic acid, Nt-butylacrylamidosulfonate lithium, Sodium Nt-butylacrylamidosulfonate, Nt-butylacrylamidosulfonic acid potassium salt, 2-Sodium sulfoethyl methacrylate, Sodium allylsulfonate, Sodium p-styrenesulfonate, Sodium sulfonate-containing urethane acrylate, Nt-butylacrylamidosulfonic acid, The hydrophilic compound (A) may be used alone or in combination of two or more. The hydrophilic compound (A) may be neutralized by adding an aqueous solution of an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide to the hydrophilic compound (A) to form a sulfonate.
[0029] A commercially available product may be used as the hydrophilic compound (A). Examples of commercially available products include ATBS (registered trademark)-Na from Toa Gosei Co., Ltd., N-SVS-25 from Asahi Kasei Finechem Co., Ltd., Antox MS-2N from Nippon Nyukazai Co., Ltd., and Spinomer (registered trademark) NaSS from Tosoh Organic Chemical Co., Ltd. The hydrophilic compound (A) may also be prepared by a commonly used method. For example, sodium sulfonate-containing urethane acrylate can be prepared by a commonly used method by those skilled in the art.
[0030] The hydrophilic compound (A) preferably has a number average molecular weight within the range of 70 to 500. Having a number average molecular weight within the above range has the advantage of being able to impart hydrophilicity more satisfactorily.
[0031] Hydrophilic compound (B) The hydrophilic compound (B) is a compound having a quaternary ammonium cationic group. The hydrophilic treatment coating composition contains the hydrophilic compound (B) in addition to the hydrophilic compound (A), which is advantageous in that it can provide good dirt adhesion prevention and good durability of dirt adhesion prevention performance. Without being bound by theory, it is believed that the inclusion of the hydrophilic compound (B) in addition to the hydrophilic compound (A) can effectively prevent basic cleaning components such as quaternary ammonium salts, which may be contained in commercially available detergents, from forming ionic bonds with the sulfonic acids possessed by the hydrophilic compound (A), thereby providing good durability of dirt adhesion prevention performance.
[0032] The hydrophilic compound (B) preferably has, in addition to the quaternary ammonium cationic group, a functional group that reacts with the silane coupling agent (S). S ), the hydrophilic compound (B) has a radical reactive functional group (R B It is preferable that the compound has a radical reactive functional group (R B Examples of the radical reactive functional group include an acrylamide group, an acryloyl group, a methacryloyl group, an allyl group, a vinyl group, a styryl group, a mercapto group, etc. These radical reactive functional groups may include only one type, or may include two or more types.
[0033] In addition, the silane coupling agent (S) has a condensation type reactive functional group (R S2 ), the hydrophilic compound (B) has a condensation type reactive functional group (R B2 It is preferable that the condensation type reactive functional group (R B2 Examples of the reactive functional groups include a carboxy group, a hydroxy group, an amino group, an epoxy group, a ureido group, an isocyanate group, an isocyanurate group, etc. These condensation type reactive functional groups may include only one type, or may include two or more types.
[0034] The hydrophilic compound (B) preferably does not have a hydrophilic portion other than the end of the molecular chain. The "hydrophilic portion" in the hydrophilic compound (B) means the quaternary ammonium cationic group and other hydrophilic groups that the hydrophilic compound (B) has. By the hydrophilic compound (B) having such a structure, the hydrophilic groups of the hydrophilic compound (B) can be concentrated on the coating surface that is not on the inorganic substrate side, and this has the advantage that sufficient cleanability and cleaning durability can be imparted even when used for members that are frequently washed with water, such as sanitary ware.
[0035] Specific examples of the hydrophilic compound (B) include, for example, (3-acrylamidopropyl)trimethylammonium chloride, (3-acrylamidopropyl)trimethylammonium bromide, [3-(methacryloylamino)propyl]trimethylammonium chloride, 2-(acryloyloxy)-N,N,N-trimethylethanaminium chloride, 2-(methacryloyloxy)ethyltrimethylammonium chloride, The hydrophilic compound (B) may be used alone or in combination of two or more kinds.
[0036] A commercially available product may be used as the hydrophilic compound (B). The hydrophilic compound (B) may also be prepared by a commonly used method.
[0037] The hydrophilic compound (B) preferably has a number average molecular weight within the range of 70 to 500. Having a number average molecular weight within the above range has the advantage of being able to impart hydrophilicity more satisfactorily.
[0038] The ratio of the amount of the hydrophilic compound (A) and the hydrophilic compound (B) contained in the hydrophilic treatment coating composition is preferably within the range of (A):(B)=15:85 to 85:15, more preferably within the range of 30:70 to 70:30, and even more preferably within the range of 40:60 to 60:40. By having the ratio (A):(B) within the above range, there is an advantage that good durability of the dirt adhesion prevention performance can be obtained.
[0039] In the case where the hydrophilic compound (A) and the hydrophilic compound (B) each have a radical reactive functional group, the radical reactive functional group (R A The average number of carbon atoms between the sulfonic acid group and the radical reactive functional group (R B ) and the quaternary ammonium cationic functional group, the average number of carbon atoms present between them is (n2); The above (n1) and (n2) are (n2)>(n1) It is preferable that the relationship be: When the average carbon number (n1) and the average carbon number (n2) have a relationship of (n2)>(n1), after the hydrophilic treatment coating composition is applied to an inorganic substrate and reacted, the quaternary ammonium cationic functional group of the hydrophilic compound (B) is considered to be present at a higher rate on the surface side than the sulfonic acid of the hydrophilic compound (A). This is considered to enable the achievement of better durability of the dirt adhesion prevention performance. The difference between the average carbon number (n1) and the average carbon number (n2) is more preferably 1 or more, and even more preferably 2 or more.
[0040] Similarly, when the hydrophilic compound (A) and the hydrophilic compound (B) each have a condensation type reactive functional group, the condensation type reactive functional group (R A2 The average number of carbon atoms between the sulfonic acid group and the 12 ) and the condensation type reactive functional group (R B2 The average number of carbon atoms between the quaternary ammonium cationic functional group and the quaternary ammonium cationic functional group is (n 22 )year, The above (n 12 ) and the above (n 22 )but, (n 22 )>(n 12 ) It is preferable that the average carbon number (n 12 ) and the average number of carbon atoms (n 22 ) is more preferably 1 or more, and even more preferably 2 or more.
[0041] In another embodiment of the hydrophilic treatment coating composition, for example, The hydrophilic compound (A) and the hydrophilic compound (B) each have copolymerizability, and these compounds are compounds that form at least one type of linear polymer selected from the group consisting of an alternating copolymer, a random copolymer, and a block copolymer, and At least one of the hydrophilic compound (A) and the hydrophilic compound (B) further has a binding ability with a silane coupling agent. In one embodiment, the composition is a hydrophilic coating composition. Even in this embodiment, there is an advantage that good stain adhesion prevention properties can be imparted to an inorganic substrate having a surface layer containing an inorganic compound.
[0042] Hydrophilic compound (C) The hydrophilic treatment coating composition may contain a hydrophilic compound (C) as necessary. Here, the hydrophilic compound (C) is a hydrophilic compound having a nonionic group. However, even if the hydrophilic compound has a nonionic group, the hydrophilic compound (C) does not include a compound corresponding to the hydrophilic compound (A) or (B).
[0043] Radical Polymerization Initiator When the silane coupling agent (S), the hydrophilic compound (A) and the hydrophilic compound (B) have a radical reactive functional group, the hydrophilic treatment coating composition preferably further contains a radical polymerization initiator. The radical polymerization initiator is a compound that decomposes by light or heat to generate radicals. The radical polymerization initiator is classified into a photoradical polymerization initiator that decomposes by light and a thermal radical polymerization initiator that decomposes by heat. The radical polymerization initiator is preferably water-soluble.
[0044] As the photoradical polymerization initiator, benzophenone, 1-hydroxy-cyclohexyl-phenyl-ketone, a mixture of 1-hydroxy-cyclohexyl-phenyl-ketone and benzophenone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 2-hydroxy-1-[4-{4-(2-hydroxy-2-methyl-propionyl)-benzyl}phenyl]-2-methyl-1-propan-1-one, oxyphenylacetic acid, a mixture of 2-[2-oxo-2-phenylacetoxyethoxy]ethyl ester and oxyphenylacetic acid, 2-(2-hydroxyethoxy)ethyl ester, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and the like are preferred. If necessary, a sensitizer such as ethyl p-dimethylaminobenzoate (Kayacure EPA manufactured by Nippon Kayaku Co., Ltd.) can be added to the photoradical polymerization initiator. Commercially available products of this type include Omnirad (registered trademark) 184, Omnirad (registered trademark) 500, Omnirad (registered trademark) 2959, DAROCURE (registered trademark) 1173, Omnirad (registered trademark) 127, Omnirad (registered trademark) 754, and Omnirad (registered trademark) 819DW manufactured by IGM RESINS.
[0045] Thermal radical polymerization initiators include 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride. Bazo compounds such as 2,2'-azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis(propane-2-carboxamidine) dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] n-hydrate, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], and 4,4'-azobis(4-cyanopentanoic acid); persulfates such as ammonium persulfate, sodium persulfate, and potassium persulfate; hydrogen peroxide; cumyl perneodecanoate; and 1,1,3,3-tetramethylbutylperoxyneodecanoate. mosquito Noate, t-Hexylperoxyneode mosquito Noate, t-Butylperoxyneode mosquito Peroxides such as tert-hexyl peroxypivalate, tert-butyl peroxypivalate, etc. are preferred. In addition, water, etc. can be added to the thermal radical polymerization initiator as necessary. As commercial products thereof, VA-044, VA-046B, VA-061, V-50, VA-057, VA-086, V-501 from Wako Pure Chemical Industries, Ltd., Percumyl ND-50E, Perocta ND-50E, Perhexyl ND-50E, Perbutyl ND-50E, Perhexyl PV-50E, Perbutyl PV-40E from NOF Corporation, and reagents from each company can be used.
[0046] The amount of the radical polymerization initiator is preferably within a range of 1 to 75 parts by mass, and more preferably within a range of 5 to 60 parts by mass, per 100 parts by mass of the total amount (solid content mass) of the hydrophilic compounds.
[0047] Other Ingredients The hydrophilic coating composition may be, if necessary, depending onA solvent may be included. By including a solvent, there is an advantage that the hydrophilic compound can be dissolved or dispersed well. Preferable solvents include, for example, water, methanol, ethanol, isopropyl alcohol, n-propyl alcohol, etc. These solvents can be appropriately selected according to the type and content of each of the above-mentioned hydrophilic compounds.
[0048] The hydrophilic coating composition may contain additives as necessary in addition to the above components. Examples of additives include surface conditioners, compatibilizers, leveling agents, plasticizers, defoamers, UV absorbers, antioxidants, and viscosity control agents. These additives may contain only one type, or may contain two or more types.
[0049] Examples of compatibilizers that can be used as additives include amide compounds such as urea, melamine, acryloylmorpholine, dimethylacrylamide, dimethylaminopropylacrylamide, isopropylacrylamide, diethylacrylamide, and hydroxyethylacrylamide; aprotic polar solvents such as dimethylsulfoxide, acetonitrile, and N,N-dimethylformamide; polyhydric alcohols such as ethylene glycol, glycerin, trimethylolpropane, ditrimethylolpropane, erythritol, erythritol, and dipentaerythritol; trioses, tetroses, pentoses, hexoses, Sedoheptulose Examples of the compatibilizer include sugars such as glucose, maltose, sucrose (cane sugar), lactose, cellobiose, raffinose, acarbose, oligosaccharides, cyclodextrin, dextrin, and starch, polar resins such as sodium carboxymethylcellulose, polyvinylpyrrolidone, sodium polyacrylate, and modified urea, and inorganic salts such as sodium hydrogen carbonate, sodium carbonate, sodium hydrogen sulfate, and sodium sulfate. The content of the compatibilizer is preferably 10 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the total amount of the hydrophilic compounds.
[0050] The solid content of the hydrophilic compound is preferably within the range of 0.1 to 60% by mass. The solid content within the above range has the advantage that good stain adhesion prevention properties can be obtained.
[0051] Another embodiment of the hydrophilic treatment coating composition is, for example, a hydrophilic treatment coating composition set in which the hydrophilic compound (A) and the hydrophilic compound (B) are stored separately. In addition, the second embodiment is a hydrophilic treatment coating composition set in which the silane coupling agent (S), the hydrophilic compound (A), and the hydrophilic compound (B) are stored separately. These embodiments can be appropriately selected according to the storage stability and reactivity of each component.
[0052] Method for hydrophilizing inorganic substrate The present specification provides a hydrophilization treatment of an inorganic substrate using the above-mentioned hydrophilic treatment coating composition. The hydrophilization treatment method includes the following two aspects. First aspect of hydrophilic treatment method A hydrophilic treatment method using the hydrophilic treatment coating composition of the first aspect, The surface of the inorganic substrate is treated with a silane coupling agent (S), Applying the hydrophilic treatment coating composition of the first embodiment to an inorganic substrate treated with the silane coupling agent (S), reacting the silane coupling agent (S) with at least one of the hydrophilic compound (A) and the hydrophilic compound (B) by light or heat; The present invention relates to a method for hydrophilizing an inorganic substrate. Second aspect of hydrophilic treatment method (1) The hydrophilic treatment coating composition of the second embodiment is exposed to light or heat, The method includes reacting a silane coupling agent (S) with at least one of the hydrophilic compound (A) and the hydrophilic compound (B), The hydrophilic treatment coating composition after the reaction is applied to a surface of an inorganic substrate. A method for hydrophilizing inorganic substrates. Second aspect of hydrophilic treatment method (2) Applying the hydrophilic treatment coating composition of the second embodiment to the surface of an inorganic substrate, The method includes reacting a silane coupling agent (S) with at least one of a hydrophilic compound (A) and a hydrophilic compound (B) by light irradiation or heating. A method for hydrophilizing inorganic substrates.
[0053] In any of the above hydrophilic treatment methods, the object (substrate) to which the hydrophilic treatment method using the hydrophilic treatment coating composition is applied is an inorganic substrate. In this specification, the term "inorganic substrate" refers to a substrate having a surface layer containing an inorganic compound (substrate having an inorganic surface). Examples of the surface layer containing an inorganic compound include glass, metal and metal oxide, and silicon dioxide other than glass. Specific examples of inorganic substrates include sanitary ware, tiles, enamel, glass, siding materials, sashes, walls, mirrors, bathtubs, and other housing-related components. An example of a substrate suitable for the above hydrophilic treatment method is sanitary ware. Sanitary ware is a water-related housing equipment such as a toilet, washbasin, and hand washing basin, and is a component that is mostly or partly made of pottery. Such sanitary ware is generally a component in which a glassy layer is formed on the surface by applying a glaze to a base (e.g., unglazed pottery, etc.) made of raw materials such as clay, pottery stone, and feldspar, and firing the glaze.
[0054] In the first embodiment of the hydrophilic treatment method, the surface of the inorganic substrate is treated with the silane coupling agent (S) by applying the silane coupling agent (S) to the surface of the inorganic substrate. More specifically, the silanol group generated by hydrolysis of the reactive silyl group reacts with the inorganic surface of the inorganic substrate to bond thereto.
[0055] Next, the hydrophilic treatment coating composition of the first embodiment is applied to the inorganic substrate treated with the silane coupling agent (S). After the hydrophilic treatment coating composition is applied, the silane coupling agent (S) is reacted with at least one of the hydrophilic compound (A) and the hydrophilic compound (B) by light or heat. For example, when the silane coupling agent (S), the hydrophilic compound (A) and the hydrophilic compound (B) have radical reactive functional groups, the radical reactive functional groups of the silane coupling agent (S), the hydrophilic compound (A) and the hydrophilic compound (B) can be radical-reacted by irradiating with light or heating. In addition, when the silane coupling agent (S), the hydrophilic compound (A) and the hydrophilic compound (B) have condensation reactive functional groups, the condensation reactive functional groups of the silane coupling agent (S), the hydrophilic compound (A) and the hydrophilic compound (B) can be condensed by heating.
[0056] The above reaction can hydrophilize the surface of the inorganic substrate. The hydrophilization treatment obtained by using the above hydrophilic treatment coating composition has the advantage that the hydrophilic treatment coating composition contains both the hydrophilic compound (A) and the hydrophilic compound (B), and thus can obtain good dirt adhesion prevention properties and good dirt adhesion prevention performance durability.
[0057] In the second embodiment (1) of the hydrophilic treatment method, the hydrophilic treatment coating composition of the second embodiment, i.e., the hydrophilic treatment coating composition containing at least the silane coupling agent (S), the hydrophilic compound (A) and the hydrophilic compound (B), is irradiated with light or heat to cause the silane coupling agent (S) to react with at least one of the hydrophilic compound (A) and the hydrophilic compound (B). In the case where the silane coupling agent (S), the hydrophilic compound (A) and the hydrophilic compound (B) have a radical reactive functional group, the radical reactive functional group of the silane coupling agent (S), the hydrophilic compound (A) and the hydrophilic compound (B) can be radically reacted by irradiating with light or heating. In addition, when the above-mentioned silane coupling agent (S), hydrophilic compound (A) and hydrophilic compound (B) have a condensation type reactive functional group, the condensation type reactive functional groups of the silane coupling agent (S), hydrophilic compound (A) and hydrophilic compound (B) can be subjected to a condensation reaction by heating.
[0058] By applying the above-mentioned reacted composition to the inorganic surface of the inorganic substrate, the silanol group generated by hydrolysis of the reactive silyl group of the silane coupling agent (S) reacts with the inorganic surface of the inorganic substrate, thereby making it possible to hydrophilize the surface of the inorganic substrate.
[0059] In the second embodiment (2) of the hydrophilic treatment method, the hydrophilic treatment coating composition of the second embodiment, i.e., the hydrophilic treatment coating composition containing at least a silane coupling agent (S), a hydrophilic compound (A) and a hydrophilic compound (B), is applied to the inorganic surface of the inorganic substrate, and then light or heat is applied. Here, the radical reactive functional group in the silane coupling agent (S) reacts with at least one of the radical reactive functional groups of the hydrophilic compound (A) and the hydrophilic compound (B), or the condensation reactive functional group in the silane coupling agent (S) reacts with at least one of the condensation reactive functional groups of the hydrophilic compound (A) and the hydrophilic compound (B). Meanwhile, the silanol group generated by hydrolysis of the reactive silyl group of the silane coupling agent (S) reacts with the inorganic surface of the inorganic substrate, and the silanol group generated by hydrolysis of the reactive silyl group undergoes a bonding reaction. This allows the surface of the inorganic substrate to be hydrophilized.
[0060] In the reaction between the silane coupling agent (S) and the hydrophilic compound (A) and the hydrophilic compound (B), one of the hydrophilic compounds (A) and (B) may be reacted preferentially, and then the other may be reacted. As a method for controlling the reaction order of the hydrophilic compounds (A) and (B), for example, a method of using a compound having higher reactivity as one of the hydrophilic compounds (A) and (B) may be mentioned.
[0061] The light irradiation may be performed by irradiating with active energy rays. More specifically, the light irradiation may be performed by irradiating with active energy rays, more preferably with ultraviolet rays having a wavelength of 220 to 450 nm, using a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, an ultraviolet LED lamp, or the like. The heating conditions may be, for example, heating using a commonly used heating furnace, a hot air dryer, or an IR heater, or thermal irradiation using an infrared heat irradiation device, or the like. The heating conditions may be, for example, a heating temperature of 80°C or higher and 150°C or lower. EXAMPLES
[0062] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited thereto. In the examples, "parts" and "%" are by weight unless otherwise specified.
[0063] Synthesis Example 1 Synthesis of sodium sulfonate-containing urethane acrylate 45.2 parts by mass of aminoethylsulfonic acid, 14.8 parts by mass of sodium hydroxide, and 40 parts by mass of ion-exchanged water were reacted at room temperature of 20 to 25°C. 42.5 parts by mass of the resulting reaction product was kept at a temperature of 5 to 10° C., and a solution prepared by mixing and dissolving 24.5 parts by mass of 2-isocyanatoethyl acrylate (Karenzu AOI (registered trademark) manufactured by Showa Denko K.K.) in 33 parts by mass of 1-methoxy-2-propanol was added dropwise thereto over a period of 5 minutes. Intermittent stirring The reaction was confirmed to have ended because no absorption due to isocyanate groups was observed in the infrared absorption spectrum, yielding a sodium sulfonate-containing urethane acrylate.
[0064] Example 1-1 Preparation of hydrophilic coating composition 27.5 parts by weight of ion-exchanged water and 10 parts by weight of urea were mixed and stirred until the urea was dissolved, and then 30 parts by weight of sodium vinyl sulfonate, 70 parts by weight of (3-acrylamidopropyl)trimethylammonium chloride, 50 parts by weight of 2-hydroxy-2-methyl-1-phenylpropanone, and 100 parts by weight of isopropyl alcohol were added and stirred until a transparent homogenous solution was obtained, thereby preparing a hydrophilic treatment coating composition.
[0065] Hydrophilic treatment 1 part of 3-methacryloxypropyltrimethoxysilane as the silane coupling agent (S) and 98 parts by mass of 1-methoxy-2-propanol were mixed with stirring at room temperature, and then 1 part by mass of a 3% aqueous hydrochloric acid solution was added and stirred for an additional 30 minutes to carry out hydrolysis. The solution obtained above was applied to a ceramic having silicon oxide on the surface, dried at 60° C. for 30 minutes in an electric oven, and then left to stand at room temperature for 30 minutes. Next, the hydrophilic treatment coating composition prepared above was applied, and then a high-pressure mercury lamp was used to illuminate the surface with an integrated light dose of 1000 mJ / cm 2 . 2 The hydrophilization treatment was carried out by irradiating the surface with ultraviolet light, which provides energy of 10 ...
[0066] Examples 1-2 to 1-42 and Comparative Examples 1-1 to 1-16 In Examples 1-2 to 1-42 and Comparative Examples 1-1 to 1-16, hydrophilic coating compositions were prepared and hydrophilic treatment was performed in the same manner as in Example 1-1, except that the type and amount of the silane coupling agent (S), and the types and amounts of the hydrophilic compounds (A) and (B) and the polymerization initiator were changed according to Tables 1 and 2 below.
[0067] Example 2-1 Preparation of hydrophilic coating composition 27.5 parts by weight of ion-exchanged water and 10 parts by weight of urea were mixed and stirred until the urea was dissolved, and then 30 parts by weight of sodium vinyl sulfonate, 70 parts by weight of (3-acrylamidopropyl)trimethylammonium chloride, 5 parts by weight of potassium persulfate, and 100 parts by weight of isopropyl alcohol were added and stirred until a transparent homogenous solution was obtained, thereby preparing a hydrophilic treatment coating composition.
[0068] Hydrophilic treatment 1 part of 3-methacryloxypropyltrimethoxysilane as the silane coupling agent (S) and 98 parts by mass of 1-methoxy-2-propanol were mixed with stirring at room temperature, and then 1 part by mass of a 3% aqueous hydrochloric acid solution was added and stirred for an additional 30 minutes to carry out hydrolysis. The solution obtained above was applied to a ceramic having silicon oxide on the surface, dried at 60° C. for 30 minutes in an electric oven, and then left to stand at room temperature for 30 minutes. Next, the hydrophilic treatment coating composition prepared above was applied, and then heating was performed using an electric oven to perform a hydrophilic treatment.
[0069] Examples 2-2 to 2-32 and Comparative Examples 2-1 to 2-15 In Examples 2-2 to 2-32 and Comparative Examples 2-1 to 2-15, hydrophilic coating compositions were prepared and hydrophilic treatment was performed in the same manner as in Example 2-1, except that the type of silane coupling agent (S), and the types and amounts of hydrophilic compounds (A) and (B) and polymerization initiator were changed according to the table below.
[0070] The hydrophilic treatments carried out in the above Examples and Comparative Examples were evaluated as follows. The evaluation results are shown in the table below.
[0071] Durability evaluation As a standard for evaluating the durability of the hydrophilic treatment, the contact angle of a water droplet on the surface was used in accordance with JIS R 3257 "Test method for wettability of glass substrate surface" (the sessile drop method was used as the type of test method). Specifically, the contact angle of a water droplet was measured using a DMo-701 manufactured by Kyowa Interface Science Co., Ltd., where 4 μL of distilled water was dropped onto the coating film and the contact angle was measured 60 seconds later. This utilizes the fact that the contact angle of a water droplet changes when a physical or chemical change occurs due to physical or chemical treatment of the surface. The surface of the substrate that had not been subjected to any treatment after the hydrophilization treatment was designated as "initial". After the hydrophilization treatment, 1 mL of Sanpol (trade name), a cationic surfactant, was dropped onto the coated surface of the substrate, which was then washed with water and designated as "detergent resistance (cationic)". After the hydrophilization treatment, 1 mL of a nonionic surfactant, Bathmagiclean (trade name), was dropped onto the coated surface of the substrate, which was then washed with water and designated as "detergent resistance (nonionic)". After the hydrophilization treatment, 1 mL of Mama Lemon (trade name), an anionic surfactant, was dropped onto the coated surface of the substrate, which was then washed with water to determine "detergent resistance (anionic)." Under each of the above conditions, the contact angle of a water droplet was measured and evaluated according to the following criteria: ◯ and Δ were judged as good, and × was judged as bad. ○: The contact angle of the water droplet is greater than 10° and less than 20° △: The contact angle of the water droplet is greater than 20° and less than 40° ×: The contact angle of the water droplet is greater than 40°
[0072] Mineral removal evaluation (evaluation of cleaning ability against inorganic substances) After the hydrophilic treatment, 150 μL of water was dropped onto the coating surface of the coated object, and the surface was dried at 40°C for 24 hours to create white water droplet spots. After that, the surface was immersed in water at 20 to 25°C and then dried with 3M Scotch-Brite. (商標) Using the antibacterial urethane sponge S-21KS, a load of 500 gf was applied and the sponge was moved back and forth 20 times, and the remaining water droplet spots were visually observed and evaluated according to the following criteria. In the following criteria, ○ and △ were considered to be acceptable, and × was considered to be defective. ○: After 20 round trips, no water droplets were visible. △: After 20 round trips, some water droplets are visible. ×: After 20 round trips, water droplets are clearly visible
[0073] [Table 1]
[0074] [Table 2]
[0075] [Table 3]
[0076] [Table 4]
[0077] It was confirmed that when the hydrophilic treatment compositions of the Examples were used, good durability and mineral removal were obtained. Comparative Examples 1-1 and 2-1 are examples in which the silane coupling agent (S) was not used. In these examples, it was confirmed that both durability and mineral removal properties were inferior. In all the other comparative examples, only one of the hydrophilic compounds (A) and (B) was used. In these examples, it was confirmed that at least one of the cationic detergent resistance, anionic detergent resistance, and mineral removal ability was poor. [Industrial Applicability]
[0078] The present disclosure provides a hydrophilic treatment coating composition that imparts dirt-adhesion prevention properties and has excellent durability of the dirt-adhesion prevention performance.
Claims
1. A hydrophilic treatment coating composition for an inorganic substrate surface-treated with a silane coupling agent (S), comprising: A hydrophilic compound (A), and Hydrophilic compound (B) Including, The hydrophilic compound (A) is a compound having at least one of a sulfonic acid group and an alkali metal salt of a sulfonic acid group, The hydrophilic compound (B) is a compound having a quaternary ammonium cationic group, The silane coupling agent (S) has a radical reactive functional group (R S ), At least one of the hydrophilic compound (A) and the hydrophilic compound (B) further has a radical reactive functional group that reacts with a silane coupling agent, At least one of the radical reactive functional groups is at least one selected from an acrylamide group, an acryloyl group, a methacryloyl group, an allyl group, a vinyl group, a styryl group, and a mercapto group. Hydrophilic treatment coating composition.
2. A hydrophilic treatment coating composition for an inorganic substrate, the hydrophilic treatment coating composition comprising: A silane coupling agent (S), A hydrophilic compound (A), and Hydrophilic compound (B) Including, The hydrophilic compound (A) is a compound having at least one of a sulfonic acid group and an alkali metal salt of a sulfonic acid group, The hydrophilic compound (B) is a compound having a quaternary ammonium cationic group, The silane coupling agent (S) has a radical reactive functional group (R S ), At least one of the hydrophilic compound (A) and the hydrophilic compound (B) further has a radical reactive functional group that reacts with the silane coupling agent (S); At least one of the radical reactive functional groups is at least one selected from an acrylamide group, an acryloyl group, a methacryloyl group, an allyl group, a vinyl group, a styryl group, and a mercapto group. Hydrophilic treatment coating composition.
3. The composition further comprises a radical polymerization initiator. The hydrophilic coating composition according to claim 1 or 2.
4. The hydrophilic coating composition according to any one of claims 1 to 3, wherein the hydrophilic compound (A) has no hydrophilic moiety other than at the ends of the molecular chain.
5. The hydrophilic coating composition according to any one of claims 1 to 4, wherein the hydrophilic compound (B) has no hydrophilic moiety other than at the ends of the molecular chain.
6. The number average molecular weight of the hydrophilic compound (A) is 70 to 500, The number average molecular weight of the hydrophilic compound (B) is 70 to 500. The hydrophilic coating composition according to any one of claims 1 to 5.
7. The hydrophilic compound (A) and the hydrophilic compound (B) each have the radical reactive functional group that reacts with the silane coupling agent (S), The radical reactive functional group (R A The average number of carbon atoms between the sulfonic acid group and the 1 )year, The radical reactive functional group (R B The average number of carbon atoms present between the quaternary ammonium cationic functional group and the quaternary ammonium cationic functional group is (n 2 )year, The (n 1 ) and the above (n 2 )but, (n 2 )>(n 1 ) The hydrophilic coating composition according to any one of claims 1 to 6, wherein
8. The hydrophilic compound (A) and the hydrophilic compound (B) in the hydrophilic treatment coating composition according to any one of claims 1 to 7 are stored separately from each other. Hydrophilic treatment paint composition set.
9. The surface of the inorganic substrate is surface-treated with a silane coupling agent (S); The hydrophilic treatment coating composition according to any one of claims 1 and 3 to 7 is applied to the inorganic substrate treated with the silane coupling agent (S), The silane coupling agent (S) and A method for hydrophilizing an inorganic substrate, comprising reacting at least one of the hydrophilic compound (A) and the hydrophilic compound (B).
10. The hydrophilic treatment coating composition according to any one of claims 2 to 7 is exposed to light or heat, The method includes reacting the silane coupling agent (S) with at least one of the hydrophilic compound (A) and the hydrophilic compound (B), The hydrophilic treatment coating composition after the reaction is applied to a surface of an inorganic substrate. A method for hydrophilizing inorganic substrates.
11. A hydrophilic treatment coating composition according to any one of claims 2 to 7 is applied to a surface of an inorganic substrate, The method includes reacting the silane coupling agent (S) with at least one of the hydrophilic compound (A) and the hydrophilic compound (B) by light irradiation or heating. A method for hydrophilizing inorganic substrates.
12. The hydrophilic treatment method for an inorganic substrate according to any one of claims 9 to 11, comprising reacting the silane coupling agent (S) with at least one of the hydrophilic compound (A) and the hydrophilic compound (B) by light irradiation.
13. The hydrophilic treatment coating composition according to any one of claims 1 to 7, wherein the inorganic substrate is sanitary ware.
Citation Information
Patent Citations
Production of antifogging coated article
JP1996027290A
Optical product having anti-fogging function
JP1996259270A
Hydrophilic coating composition, hydrophilic coating film, water section product and manufacturing method of hydrophilic coating film
JP2014111745A
Hydrophilic treatment coating composition and hydrophilic treatment method
JP2016020461A
Hydrophilic treatment coating composition and hydrophilic treatment method
JP2016020462A