Multilayer films, laminates and airbags

By integrating a thermoplastic elastomer with a melt tension of 7.5 mN or more in the multilayer film layers, molding stability is significantly improved, addressing issues of neck-in and non-uniform bubble formation, resulting in consistent film production.

JP7562251B2Active Publication Date: 2024-10-07ZF AUTOMOTIVE GERMANY GMBH

Patent Information

Application Number
JP2019221659
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-12-06
Publication Date
2024-10-07
Estimated Expiration
2039-12-06

AI Technical Summary

Technical Problem

Multilayer films experience poor molding stability during film molding, leading to issues such as the neck-in phenomenon and non-uniform bubble formation during inflation molding.

Method used

Incorporating a thermoplastic elastomer with a melt tension of 7.5 mN or more in at least one layer of the multilayer film, specifically the adhesive and second layers, enhances molding stability by maintaining a stable form during various molding methods like inflation and T-die methods.

Benefits of technology

The multilayer film achieves excellent molding stability, preventing deformation and ensuring consistent film width during molding, thereby improving yield and reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562251000005
    Figure 0007562251000005
  • Figure 0007562251000006
    Figure 0007562251000006
  • Figure 0007562251000007
    Figure 0007562251000007
Patent Text Reader

Abstract

To provide a multilayer film capable of having excellent molding stability.SOLUTION: There is provided a multilayer film which is bonded to a base fabric and comprises a first layer bonded to the base fabric and a second layer provided on the first layer, wherein either or both of the first layer and the second layer contain a thermoplastic elastomer and the thermoplastic elastomer is at least one kind selected from a group consisting of a polyester-based elastomer, a polyurethane-based elastomer and a polyamide-based elastomer and has melt tension of 7.5 mN or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to multilayer films, laminates and airbags. [Background technology]

[0002] A multilayer film is generally constructed by laminating a plurality of resin layers, and is widely used in products that undergo shape changes, such as vehicle airbags, outdoor products, packaging, etc., due to its excellent flexibility. A base fabric that is easily deformed may be used in such products. In such cases, in order to protect the base fabric, a multilayer film having a resin layer that has adhesive strength to the base fabric is used on the surface of the base fabric.

[0003] As such a multilayer film, for example, a laminated molded body has been disclosed which is constructed by laminating an adhesive polymer composition layer made of a modified polyester-based elastomer and a gas barrier resin layer made of a polyamide resin or an ethylene-vinyl alcohol copolymer (see, for example, Patent Document 1).

[0004] This laminated molded product is produced by melting the adhesive polymer composition and the thermoplastic resin, which are the molding materials for the layers constituting the laminated molded product, and using various molding methods such as (co)extrusion molding, inflation molding, blow molding, rotational molding, and injection molding. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-144486 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the multilayer film described in Patent Document 1 has poor molding stability during film molding, and may not be molded into a desired shape. For example, when the T-die method is used, the molten resin extruded from the T-die may become narrow, which is called the neck-in phenomenon. When the inflation molding method is used, the molten resin may not blow up uniformly, and stable bubbles may not be formed.

[0007] An object of one aspect of the present invention is to provide a multilayer film that can have excellent molding stability. [Means for solving the problem]

[0008] One embodiment of the multilayer film according to the present invention is a multilayer film adhered to a base fabric, A first layer adhered to the base fabric; a second layer disposed on the first layer, One or both of the first layer and the second layer comprises a thermoplastic elastomer; the thermoplastic elastomer is at least one selected from the group consisting of polyester-based elastomers, polyurethane-based elastomers, and polyamide-based elastomers, The melt tension is 7.5 mN or more. Effect of the Invention

[0009] One embodiment of the multilayer film according to the present invention can have excellent molding stability. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view of a multilayer film according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing an example of an inflation molding machine equipped with a plurality of melt-kneading devices. [Diagram 3] FIG. 2 is a top view of the annular die. [Figure 4] FIG. 1 is a diagram showing an example of a T-die extrusion molding machine equipped with a plurality of melt-kneading devices. [Diagram 5] FIG. 2 is an explanatory diagram showing a state in which a molten multilayer film is discharged from a discharge port of a multi-manifold die. [Figure 6] FIG. 2 is an explanatory diagram of a state in which a molten material is extruded from a T-die. [Figure 7] FIG. 2 is a cross-sectional view illustrating an example of a laminate. [Figure 8] FIG. 2 is a diagram illustrating an example of a laminate manufacturing apparatus. [Figure 9] FIG. 11 is a cross-sectional view showing an example in which the base fabric is OPW. [Figure 10] FIG. 2 is a schematic cross-sectional view showing another example of a multilayer film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiment of the present invention will be described in detail. In order to facilitate understanding of the description, the same components in each drawing are given the same reference numerals, and duplicated description will be omitted. In addition, the scale of each member in the drawing may differ from the actual one. In this specification, a three-dimensional orthogonal coordinate system with three axial directions (X-axis, Y-axis, and Z-axis) is used, and the coordinates on the main surface of the first layer are defined as the X-axis direction and the Y-axis direction, and the height direction (thickness direction) is defined as the Z-axis direction. The direction from the bottom to the top of the first layer (the direction from the main surface of the first layer to the second layer) is defined as the +Z-axis direction, and the opposite direction is defined as the -Z-axis direction. In the following description, the +Z-axis direction may be referred to as up, and the -Z-axis direction may be referred to as down. In this specification, a tilde "~" indicating a numerical range means that the numerical values ​​before and after it are included as the lower and upper limits, unless otherwise specified.

[0012] <Multilayer film> A multilayer film according to an embodiment of the present invention will be described. Fig. 1 is a schematic cross-sectional view of the multilayer film according to this embodiment. As shown in Fig. 1, the multilayer film 1 includes an adhesive layer 10 as a first layer, and a second layer 20 adhered (bonded) to the adhesive layer 10, and is configured by laminating the second layer 20 on the adhesive layer 10. The multilayer film 1 can be used by adhering it to a fibrous article such as a base fabric 2. Details of the base fabric 2 will be described later.

[0013] The multilayer film 1A contains a thermoplastic elastomer in any of the layers constituting the multilayer film 1 (the adhesive layer 10 and the second layer 20), and has a melt tension of 7.5 mN or more. The melt tension of the multilayer film 1A is preferably 8.0 mN or more, more preferably 9.0 mN or more, even more preferably 10 mN or more, and most preferably 20.0 mN or more. If the melt tension is 7.5 mN or more, the multilayer film 1A can maintain a stable shape in a molten state that allows it to be stretched during molding when various molding methods such as the inflation method and the T-die method are used.

[0014] In this embodiment, the melt tension is a value when a molten resin extruded from a specified die at a specified temperature and extrusion speed is taken up in a spun state while gradually pulling it up from a specified take-up speed using a specified device, and the spun thread breaks. In this embodiment, the melt tension is a value when a resin extruded from a capillary having a diameter of 1 mm, a length of 10 mm, and an inlet angle of 180° at a constant speed of 8.8 mm / min is taken up in a spun state while gradually pulling it up from a take-up speed of 5 m / min using a Capillary Extrusion Rheometer manufactured by Malvern, and the spun thread breaks.

[0015] The melt tension is a value measured at a temperature higher than the melting points of the adhesive layer 10 and the second layer 20 constituting the multilayer film 1A. The layers constituting the multilayer film 1A do not enter a molten state at temperatures below their melting points, and become completely fluid at temperatures significantly higher than the melting points, making it impossible to measure the melt tension. The melting points of each layer (adhesive layer 10 and second layer 20) constituting the multilayer film 1A are the melting peak temperatures measured with a differential scanning calorimeter.

[0016] Each layer constituting the multilayer film 1A will now be described.

[0017] [Adhesive layer] The adhesive layer 10 is a layer that is adhered to the base fabric 2, and has an adhesive function when adhering the multilayer film 1 to the base fabric 2. The adhesive layer 10 can adhere the multilayer film 1 to the base fabric 2 under predetermined conditions when adhering the multilayer film 1 to the base fabric 2. The adhesive layer 10 exerts its adhesive function, so that the multilayer film 1 can be well adhered to the base fabric 2 without using a separate adhesive or the like. Therefore, the effort and cost involved in using an adhesive when adhering the multilayer film 1 to the base fabric 2 can be reduced. In addition, when the multilayer film 1 is used for a long period of time, for example, the multilayer film 1 can be prevented from peeling off from the base fabric 2 due to deterioration of the adhesive.

[0018] The predetermined conditions may be any conditions that allow the adhesive layer 10 to exhibit adhesion to the base fabric 2, for example, by increasing at least one of the temperature and pressure so that the adhesive layer 10 can be softened or melted.

[0019] The adhesive layer 10 may have a function of preventing gas from circulating inside and outside the layer (hereinafter also referred to as an airtight function). When the adhesive layer 10 exerts an airtight function, leakage of gas such as air from inside the base fabric 2 to the outside can be suppressed when the multilayer film 1 is adhered to the base fabric 2.

[0020] The adhesive layer 10 may contain thermoplastic elastomers, ethylene-vinyl alcohol copolymers (EVOH), polyolefin resins, polyester resins, polyamide resins, acrylic resins, polyurethanes, polyvinyl chloride, polycarbonates, etc. (hereinafter, may be simply referred to as thermoplastic elastomers, etc.) These may be used alone or may contain two or more types.

[0021] (Thermoplastic elastomer) The thermoplastic elastomer is preferably a block copolymer containing a hard segment (also called a high melting point segment or crystalline segment) and a soft segment (also called a low melting point segment or non-crystalline segment).Thermoplastic elastomer softens and becomes fluid when heated, and can exhibit rubber-like elasticity when not heated.

[0022] The thermoplastic elastomer is at least one selected from the group consisting of polyester elastomers (also called polyester thermoplastic elastomers), polyurethane elastomers (also called polyurethane thermoplastic elastomers), and polyamide elastomers (also called polyamide thermoplastic elastomers). Among these, polyester elastomers are preferred because they are easy to form block copolymers having a branched structure.

[0023] The adhesive layer 10 contains at least one of a polyester-based elastomer, a polyurethane-based elastomer, and a polyamide-based elastomer, and thereby the adhesiveness between the adhesive layer 10 and the base fabric 2 and the adhesive layer 10 and the second layer 20 of the resulting multilayer film 1 can be improved even under conditions including at least any one of room temperature, high temperature, and high humidity. In addition, the flexibility and mechanical strength of the multilayer film 1 can be improved. The level of adhesiveness can be evaluated from the presence or absence of delamination, and when delamination occurs, it can be determined that the adhesiveness is high.

[0024] In this embodiment, high temperature refers to a temperature higher than room temperature, and high humidity refers to a humidity higher than room humidity. Room temperature refers to a temperature range of 5 to 35° C., and room humidity refers to a relative humidity range of 45 to 85%.

[0025] Preferred polyester-based elastomers include polyester-polyether copolymers containing aromatic polyesters as hard segments and aliphatic polyethers as soft segments, and polyester-polyester copolymers containing aromatic polyesters as hard segments and aliphatic polyesters as soft segments.

[0026] The hard segment of the polyester-based elastomer preferably contains an aromatic polyester, for example, a polyester formed from an aromatic dicarboxylic acid and a diol.

[0027] Examples of aromatic polycarboxylic acids include phthalic acid, terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, anthracene dicarboxylic acid, 4,4'-biphenyldicarboxylic acid, diphenoxyethanedicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 5-sulfoisophthalic acid, and sodium 3-sulfoisophthalate. The aromatic polycarboxylic acids may be contained alone or in combination of two or more in the aromatic polyester. In addition, a part of the aromatic dicarboxylic acids may be replaced with an alicyclic or aliphatic carboxylic acid.

[0028] Examples of diols include aliphatic diols such as 1,4-butanediol, ethylene glycol, polypropylene glycol, trimethylene glycol, pentamethylene glycol, hexamethylene glycol, neopentyl glycol, and decamethylene glycol; alicyclic diols such as 1,1-cyclohexanedimethanol, 1,4-dicyclohexanedimethanol, and tricyclodecane dimethanol; and aromatic diols such as xylylene glycol, bis(p-hydroxy)diphenyl, bis(p-hydroxy)diphenylpropane, 2,2'-bis[4-(2-hydroxyethoxy)phenyl]propane, bis[4-(2-hydroxyethoxy)phenyl]sulfone, 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 4,4'-dihydroxy-p-terphenyl, and 4,4'-dihydroxy-p-quarterphenyl. The above diols may be contained alone or in combination in the aromatic polyester.

[0029] From the viewpoint of heat resistance and gas barrier properties, the polyester contained in the hard segment is preferably polybutylene terephthalate, polypropylene terephthalate, polybutylene isophthalate, polyethylene terephthalate, polyethylene isophthalate, or polytrimethylene terephthalate. These may be contained alone or in combination of two or more. These may also be contained as a copolymer or a mixture.

[0030] The soft segment of the polyester elastomer preferably contains at least one of an aliphatic polyether and an aliphatic polyester. Examples of the aliphatic polyether include poly(ethylene oxide) glycol, poly(propylene oxide) glycol, poly(tetramethylene oxide) glycol (polytetramethylene ether glycol), poly(hexamethylene oxide) glycol, copolymers of ethylene oxide and propylene oxide, ethylene oxide addition polymers of poly(propylene oxide) glycol, and copolymer glycols of ethylene oxide and tetrahydrofuran. Examples of the aliphatic polyester include poly(ε-caprolactone), polyenantholactone, polycaprylolactone, polybutylene adipate, and polyethylene adipate.

[0031] Among these aliphatic polyethers and aliphatic polyesters, from the viewpoint of elasticity and moldability, poly(tetramethylene oxide) glycol, ethylene oxide addition polymer of poly(propylene oxide) glycol, copolymer glycol of ethylene oxide and tetrahydrofuran, poly(ε-caprolactone), polybutylene adipate, polyethylene adipate, and the like are preferred, and among these, poly(tetramethylene oxide) glycol, ethylene oxide addition polymer of poly(propylene oxide) glycol, and copolymer glycol of ethylene oxide and tetrahydrofuran are particularly preferred.

[0032] The number average molecular weight of the soft segment is preferably about 300 to 6,000 in a copolymerized state.

[0033] The polyester elastomer may be modified with an unsaturated carboxylic acid such as acrylic acid, maleic acid, or fumaric acid or a derivative thereof in the presence of a radical generator. The amount of the unsaturated carboxylic acid or a derivative thereof added for modification is preferably 0.1 to 30 parts by mass per 100 parts by mass of the thermoplastic polyester elastomer. The type and amount of the component used for such modification can be appropriately selected depending on the material and application of the base fabric 2 to be bonded.

[0034] The content of the hard segment in the polyester elastomer in the adhesive layer 10 is preferably 10% by mass to 70% by mass, more preferably 20% by mass to 60% by mass, and even more preferably 25% by mass to 55% by mass, based on 100% by mass of the thermoplastic polyester elastomer. When the content of the hard segment is within the above preferred range, the mechanical strength, heat resistance, and durability under high temperature and high humidity conditions of the multilayer film 1 can be improved, and the multilayer film 1 can be ensured to have appropriate elasticity, flexibility, and formability.

[0035] The content of the soft segment in the polyester elastomer in the adhesive layer 10 is preferably 30% by mass to 90% by mass, more preferably 40% by mass to 80% by mass, and even more preferably 45% by mass to 75% by mass, relative to 100% by mass of the polyester elastomer. When the content of the soft segment is within the above preferred range, appropriate elasticity, flexibility, and formability of the multilayer film 1 can be ensured, and the mechanical strength of the multilayer film 1 can be improved.

[0036] The content of the soft segment in the polyester elastomer is related to the melting point and softening point of the polyester elastomer. In general, the greater the content of the soft segment in the polyester elastomer, the lower the melting point and softening point of the polyester elastomer. By adjusting the content of the soft segment in the polyester elastomer in the adhesive layer 10, the melting point of the polyester elastomer can be adjusted, and therefore the melting point of the adhesive layer 10 can be adjusted.

[0037] The melting point of the adhesive layer 10 is appropriately adjusted, and is preferably lower than the melting points of the intermediate layer 21 and the airtight layer 22. The melting point of the adhesive layer 10 may be a temperature lower than the melting points of the intermediate layer 21 and the airtight layer 22 constituting the second layer 20, and is preferably 80° C. to 250° C., more preferably 100° C. to 200° C., and even more preferably 130° C. to 190° C. The melting point of the adhesive layer 10 is adjusted according to the type and content of the polyester-based elastomer used in the adhesive layer 10, the type and content of the hard segment and soft segment constituting the polyester-based elastomer, and the like.

[0038] By making the melting point of the adhesive layer 10 higher than the melting points of the intermediate layer 21 and the airtight layer 22, when the multilayer film 1 is heated to adhere to the base fabric 2, the adhesive layer 10 can be softened or melted to a softness suitable for adhesion to the base fabric 2 while suppressing softening of the intermediate layer 21 and the airtight layer 22. Therefore, even if the heating temperature and pressure conditions of the multilayer film 1 vary during production, the multilayer film 1 can be reliably adhered to the base fabric 2.

[0039] Commercially available polyester elastomers include "Hytrel (registered trademark)" manufactured by DuPont-Toray Co., Ltd., "MODIC (registered trademark)" manufactured by Mitsubishi Chemical Corporation, "Pelprene (registered trademark)" manufactured by Toyobo Co., Ltd., "Arnitel (registered trademark)" manufactured by DSM, and "Flexmar" series manufactured by Nippon Synthetic Chemical Industry Co., Ltd.

[0040] The polyurethane-based elastomer is preferably a polyurethane-based copolymer containing, as a hard segment, a urethane that is a condensation product of a diisocyanate compound and a short-chain glycol, and containing, as a soft segment, a polyester or a polyether, etc. The polyurethane-based elastomer may contain, as a hard segment, a single urethane or two or more kinds of urethane.

[0041] Examples of the polyurethane copolymer include those represented by the formula (I):

[0042] [ka] (In the formula, A is a hard segment, which is a condensation block of a diisocyanate compound and a short-chain glycol, B is a soft segment, which is a polyester or polyether, and Y is a residue of a diisocyanate compound.) Examples of the copolymer include those represented by the following formula:

[0043] As the diisocyanate compound, known and commonly used compounds such as phenylene diisocyanate, tolylene diisocyanate, xylene diisocyanate, 4,4'-diphenylmethane diisocyanate, hexamethylene diisocyanate, etc. The diisocyanate compounds of the hard segment and the soft segment may be the same or different.

[0044] Examples of the short-chain glycol include alkylene glycols having 2 to 5 carbon atoms, such as ethylene glycol, propylene glycol, and 1,4-butanediol.

[0045] Examples of polyesters include polyalkylene adipates, polycaprolactones, and polycarbonates.

[0046] The polyether may be a poly(alkylene oxide) glycol having a molecular weight of 400 to 6000. Examples of the poly(alkylene oxide) glycol having a molecular weight of 400 to 6000 include poly(alkylene oxide) glycols having a molecular weight of 400 to 6000, such as polyethylene glycol, poly(1,2- and 1,3-propylene oxide) glycol, poly(tetramethylene oxide) glycol, and poly(hexamethylene oxide) glycol.

[0047] The polyesters and polyethers may contain condensation bonds with the diisocyanate compounds.

[0048] The soft segment of the polyurethane elastomer may be made of the same material as the soft segment of the thermoplastic polyester elastomer, and therefore a detailed description of the soft segment of the polyurethane elastomer will be omitted.

[0049] The content of the hard segment in the polyurethane-based elastomer can be the same as the content of the hard segment in the polyester-based elastomer described above, and therefore, the description of the content of the hard segment in the polyester-based elastomer is omitted.

[0050] The content of the soft segment in the polyurethane-based elastomer can be the same as the content of the soft segment in the polyester-based elastomer described above, and therefore, the description of the content of the soft segment in the polyester-based elastomer is omitted.

[0051] The melting point of the polyurethane elastomer can be the same as that of the polyester elastomer, and therefore a description of the melting point of the polyester elastomer is omitted.

[0052] Commercially available polyurethane elastomers include "Elastran (registered trademark)" (manufactured by BASF Japan Ltd.), "Miractran" (manufactured by Nippon Miractoran Co., Ltd.), "Rezamin P Series" (manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.), and "U-Fine P" (manufactured by Asahi Glass Co., Ltd.).

[0053] The polyamide-based elastomer is preferably a polyamide-based copolymer containing a polyamide as a hard segment and a polyether or polyester as a soft segment. The polyamide-based elastomer may contain a single polyamide or two or more types of polyamide as the hard segment.

[0054] Examples of the polyamide block include nylon 6, nylon 6,6, nylon 11, and nylon 12, with nylon 12 being preferred.

[0055] The polyether block is preferably an aliphatic polyether block, similar to the soft segment of the polyester-based elastomer.

[0056] The polyamide-polyether copolymer may, for example, be a copolymer represented by the formula (II):

[0057] [ka] (In the formula, PA represents a polyamide which is a hard segment, and PG represents a polyether which is a soft segment.) Examples of the copolymer include those represented by the following formula:

[0058] Polyamide-polyether copolymers can be obtained, for example, by polycondensing a salt of a diamine and a dicarboxylic acid, a lactam, or an aminodicarboxylic acid (PA component), a polyoxyalkylene glycol (PG component) such as polyoxyethylene glycol or polyoxypropylene glycol, and a dicarboxylic acid.

[0059] Commercially available polyamide-polyether copolymers include "Pebax (registered trademark)" (Arkema), "Diamid-PAE" (Daicel-Degussa Co., Ltd.), "UBE Polyamide Elastomer" (Ube Industries, Ltd.), "Novamid PAE" (Mitsubishi Engineering Plastics Corporation), "Grilux" (Toyobo Co., Ltd.), and "Grilon ELX, ELY" (M-Chemie Japan Co., Ltd.).

[0060] The soft segment of the polyamide-based elastomer may be made of the same material as the soft segment of the thermoplastic polyester-based elastomer, and therefore a description of the soft segment of the polyamide-based elastomer will be omitted.

[0061] The content of the hard segment in the polyamide-based elastomer can be the same as the content of the hard segment in the polyester-based elastomer described above, and therefore the description of the content of the hard segment in the polyamide-based elastomer is omitted.

[0062] The content of the soft segment in the polyamide-based elastomer can be the same as the content of the soft segment in the polyester-based elastomer described above, and therefore the description of the content of the soft segment in the polyamide-based elastomer is omitted.

[0063] The melting point of the polyamide-based elastomer can be the same as that of the polyester-based elastomer, and therefore a description of the melting point of the polyamide-based elastomer is omitted.

[0064] (Branched component) When the adhesive layer 10 includes a thermoplastic elastomer, it may include a branched component.

[0065] The branched component is a polyvalent component having two or more functional groups. By including the branched component, the thermoplastic elastomer included in the adhesive layer 10 can have a branched structure. By including the branched component in the adhesive layer 10, the thermoplastic elastomer forming the adhesive layer 10 can have a branched structure, which makes it easier to increase the stability of the shape when molding the adhesive layer 10. In this embodiment, the polyvalent component may have two or more functional groups, but preferably has three or more functional groups.

[0066] When the thermoplastic elastomer is a polyester-based elastomer, the branched component can be at least one of an aromatic polycarboxylic acid having two or more carboxyl groups in the molecule and a polyhydric alcohol having two or more hydroxyl groups in the molecule.

[0067] In addition, when the thermoplastic elastomer is a polyurethane-based elastomer, the branched component can be at least one of a polyisocyanate-based compound having two or more isocyanate groups in the molecule and a polyol-based compound having two or more hydroxyl groups in the molecule.

[0068] Furthermore, when the thermoplastic elastomer contains a polyester-based elastomer and a polyurethane-based elastomer, the branched component can contain a polyester-based elastomer and a polyurethane-based elastomer having a branched structure by using at least one of a polyvalent isocyanate-based compound and a polyol-based compound in the polyester-based elastomer.

[0069] Examples of aromatic polycarboxylic acids include aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, orthophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, anthracene dicarboxylic acid, 4,4'-biphenyldicarboxylic acid, diphenoxyethanedicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 5-sulfoisophthalic acid, and sodium 3-sulfoisophthalate; propane-1,2,3-tricarboxylic acid, 2-methylpropane-1,2,3-triscarboxylic acid, butane-1,2,4-tricarboxylic acid, butane-1,2,4-tricarboxylic acid, and butane-1,2,5-tricarboxylic acid. Examples of the aromatic polycarboxylic acid include benzene-1,2,3,4-tetracarboxylic acid, trimellitic acid, trimesic acid, hemimellitic acid, pyromellitic acid, benzenepentacarboxylic acid, cyclohexane-1,2,4-tricarboxylic acid, cyclohexane-1,3,5-tricarboxylic acid, cyclohexane-1,2,4,5-tetracarboxylic acid, naphthalene-1,2,4-tricarboxylic acid, naphthalene-2,5,7-tricarboxylic acid, pyridine-2,4,6-tricarboxylic acid, naphthalene-1,2,7,8-tetracarboxylic acid, and naphthalene-1,4,5,8-tetracarboxylic acid. Among these, trimellitic acid is preferred. The aromatic polycarboxylic acid may be contained alone or in combination of two or more in the aromatic polyester. In addition, in the hard segment, a part of the aromatic polycarboxylic acid component may be replaced with an alicyclic or aliphatic carboxylic acid.

[0070] Examples of polyhydric alcohols include aliphatic diols such as 1,4-butanediol, ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, trimethylene glycol, pentamethylene glycol, hexamethylene glycol, neopentyl glycol, and decamethylene glycol; alicyclic diols such as 1,1-cyclohexanedimethanol, 1,4-dicyclohexanedimethanol, and tricyclodecane dimethanol, xylylene glycol, bis(p-hydroxy)diphenyl, and bis(p-hydroxy)diphenylpropane, Aromatic diols such as 2,2'-bis[4-(2-hydroxyethoxy)phenyl]propane, bis[4-(2-hydroxyethoxy)phenyl]sulfone, 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 4,4'-dihydroxy-p-terphenyl, 4,4'-dihydroxy-p-quaterphenyl; 1,2,4-butanetriol, 1,2,5-pentanetriol, 1,2,6-hexanetriol, 1,2,3,6-hexanetetrol, glycerin, diglycerin, triglycerin, tetraglycerin, pentaglycerin, etc. Serine, hexaglycerin, triethanolamine, trimethylolethane, trimethylolpropane, ditrimethylolpropane, tritrimethylolpropane, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, pentaerythritol, dipentaerythritol, tripentaerythritol, methyl glucoside, sorbitol, mannitol, sucrose, 1,3,5-trihydroxybenzene, 1,2,4-trihydroxybenzene, (poly)oxyethylene glycerin, (poly)oxypropylene glycerin, (poly ) oxyethylene diglycerin, (poly)oxypropylene diglycerin, (poly)oxyethylene trimethylolpropane, (poly)oxypropylene trimethylolpropane, (poly)oxyethylene ditrimethylolpropane, (poly)oxypropylene ditrimethylolpropane, erythritol (also called erythritol), (poly)oxyethylene pentaerythritol, (poly)oxypropylene pentaerythritol, (poly)oxyethylene dipentaerythritol, (poly)oxypropylene dipentaerythritol, and the like.Among these, pentaerythritol, trimethylolpropane, ditrimethylolpropane, and dipentaerythritol are preferable. The polyhydric alcohols may be contained in the aromatic polyester either alone or in combination of two or more kinds.

[0071] Examples of the polyisocyanate compound include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, polyphenylmethane polyisocyanate, modified diphenylmethane diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, phenylene diisocyanate, and naphthalene diisocyanate; aliphatic polyisocyanates such as hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, lysine diisocyanate, and lysine triisocyanate; alicyclic polyisocyanates such as hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, and norbornene diisocyanate; and isocyanurate compounds or polymer compounds of these polyisocyanates, allophanate polyisocyanates, biuret polyisocyanates, and water-dispersible polyisocyanates. These may be used alone or in combination of two or more.

[0072] Commercially available polyisocyanate compounds include, for example, "Coronate" (manufactured by Tosoh Corporation), "Duranate" (manufactured by Asahi Kasei Corporation), and "Takenate" (manufactured by Mitsui Chemicals, Inc.).

[0073] Examples of polyol compounds include aliphatic polyols, alicyclic polyols, polyether polyols, polyester polyols, polycarbonate polyols, polyolefin polyols, polybutadiene polyols, polyisoprene polyols, (meth)acrylic polyols, polysiloxane polyols, etc. These may be used alone or in combination of two or more.

[0074] Examples of the aliphatic polyols include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, trimethylene glycol, dimethylolpropane, neopentyl glycol, 2,2-diethyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,4-tetramethylenediol, 1,3-tetramethylenediol, 2-methyl-1,3-trimethylenediol, 1,5-pentamethylenediol, 1, Examples of the alcohol include aliphatic alcohols containing two hydroxyl groups, such as 6-hexamethylenediol, 3-methyl-1,5-pentamethylenediol, 2,4-diethyl-1,5-pentamethylenediol, pentaerythritol diacrylate, 1,9-nonanediol, and 2-methyl-1,8-octanediol; sugar alcohols, such as xylitol and sorbitol; and aliphatic alcohols containing three or more hydroxyl groups, such as glycerin, trimethylolpropane, and trimethylolethane.

[0075] Examples of the alicyclic polyol include cyclohexanediols such as 1,4-cyclohexanediol and cyclohexyldimethanol, hydrogenated bisphenols such as hydrogenated bisphenol A, and tricyclodecane dimethanol.

[0076] Examples of polyether polyols include alkylene structure-containing polyether polyols such as polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polybutylene glycol, polypentamethylene glycol, and polyhexamethylene glycol, and random or block copolymers of these polyalkylene glycols.

[0077] Examples of polyester-based polyols include condensation polymers of polyhydric alcohols and polycarboxylic acids; ring-opening polymers of cyclic esters (lactones); and reaction products of three components, a polyhydric alcohol, a polycarboxylic acid, and a cyclic ester.

[0078] Examples of polycarbonate-based polyols include reaction products of polyhydric alcohols and phosgene; ring-opening polymers of cyclic carbonates (such as alkylene carbonates); and the like.

[0079] Examples of the polyhydric alcohol include the polyhydric alcohols exemplified above, and examples of the alkylene carbonate include ethylene carbonate, trimethylene carbonate, tetramethylene carbonate, and hexamethylene carbonate.

[0080] The polycarbonate-based polyol may be any compound having a carbonate bond in the molecule and a hydroxyl group at the end, and may have an ester bond in addition to the carbonate bond.

[0081] Examples of polyolefin polyols include those having a homopolymer or copolymer of ethylene, propylene, butene, or the like as a saturated hydrocarbon skeleton and having hydroxyl groups at the molecular terminals.

[0082] The polybutadiene-based polyol may be a polybutadiene having a butadiene copolymer as a hydrocarbon skeleton and a hydroxyl group at the molecular end. The polybutadiene-based polyol may be a hydrogenated polybutadiene polyol in which all or a part of the ethylenically unsaturated groups contained in the structure are hydrogenated.

[0083] The polyisoprene-based polyol may be a polyol having a copolymer of isoprene as a hydrocarbon skeleton and having hydroxyl groups at the molecular terminals. The polyisoprene-based polyol may be a hydrogenated polyisoprene polyol in which all or a part of the ethylenically unsaturated groups contained in the structure are hydrogenated.

[0084] Examples of (meth)acrylic polyols include those having at least two hydroxy groups in the molecule of a (meth)acrylic acid ester polymer or copolymer. Examples of (meth)acrylic acid esters include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate.

[0085] Examples of polysiloxane-based polyols include dimethylpolysiloxanepolyol and methylphenylpolysiloxanepolyol.

[0086] The content of the branched component is preferably 0.1% by mass to 10% by mass, more preferably 0.3% by mass to 5% by mass, and even more preferably 0.5% by mass to 3% by mass. If the content of the branched component is 0.1% by mass to 10% by mass, the thermoplastic elastomer contained in the adhesive layer 10 can have a branched structure and the flexibility of the adhesive layer 10 can be maintained.

[0087] The thermoplastic elastomer may include at least one of a polyester-based elastomer, a polyurethane-based elastomer, and a polyamide-based elastomer, a polyolefin-based elastomer, a polystyrene-based elastomer, a polybutadiene-based elastomer, and the like.

[0088] (EVOH) EVOH is a water-insoluble thermoplastic resin obtained by copolymerizing ethylene and a vinyl ester monomer and then saponifying the copolymer. Vinyl acetate is generally used as the vinyl ester monomer from an economical point of view. The polymerization method may be a known polymerization method such as solution polymerization, suspension polymerization, or emulsion polymerization, and generally, solution polymerization using methanol as a solvent is used. The ethylene-vinyl ester copolymer obtained may also be saponified by a known method. That is, EVOH is mainly composed of ethylene structural units and vinyl alcohol structural units, and contains a small amount of vinyl ester structural units remaining without being saponified.

[0089] The content of the ethylene structural unit contained in the EVOH is preferably within a range of 20 mol% to 60 mol%. If the content is within a range of 20 mol% to 60 mol%, flexibility can be exhibited. The content of the ethylene structural unit can be measured, for example, in accordance with ISO14663-1 (1999).

[0090] The saponification degree of the vinyl ester component in the EVOH is preferably within a range of 80 mol% to 100 mol%. If the saponification degree is within the above range, flexibility can be exhibited. The saponification degree of the vinyl ester component can be measured, for example, in accordance with JIS K6726 (1994) (wherein EVOH is a solution uniformly dissolved in a water / methanol solvent (water:methanol=9:1 (mass ratio))).

[0091] The melt flow rate (MFR) of EVOH (210° C., load 2,160 g) is preferably within the range of 1 g / 10 min to 50 g / 10 min. If the MFR is within the above range, flexibility can be exhibited.

[0092] The EVOH may be used alone, or two or more kinds of EVOH having different ethylene contents, saponification degrees, and MFRs may be used in combination.

[0093] When the adhesive layer 10 does not contain a thermoplastic elastomer, a branched component, or EVOH, it may contain, instead of these, a polyolefin resin, a polyester resin, a polyamide resin, an acrylic resin, a polyurethane, a polyvinyl chloride, a polycarbonate, etc. (hereinafter, sometimes simply referred to as a polyolefin resin, etc.). These may be used alone or may contain two or more types.

[0094] Examples of polyolefin resins include polyethylene, polypropylene, ethylene-propylene copolymer, polybutylene, polymethylpentene, etc. Examples of polyethylene include low-density polyethylene (LPDE), high-density polyethylene (HDPE), and linear low-density polyethylene (L-LDPE). The polyolefin resin may also be a modified polyolefin resin obtained by bonding unsaturated carboxylic acid or its anhydride by addition reaction, graft reaction, or the like.

[0095] Examples of polyester resins include aromatic polyester resins such as polyethylene terephthalate (PET), polytrimethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate.

[0096] Examples of polyamide-based resins include aliphatic polyamides such as polyamide 6, polyamide 66, polyamide 610, polyamide 10, polyamide 12, and polyamide 6-12, and copolymers thereof, and semi-aromatic polyamides synthesized from aromatic dicarboxylic acids and aliphatic diamines.

[0097] Examples of the acrylic resin include acrylic acid and methacrylic acid.

[0098] Examples of polyurethane include polycarbonate-based polyurethane, polyether-based polyurethane, polyester-based polyurethane, and modified products thereof.

[0099] Examples of polyvinyl chloride include vinyl chloride homopolymers polymerized by conventional methods such as emulsion polymerization, suspension polymerization, microsuspension polymerization, and bulk polymerization, copolymers of vinyl chloride monomers with monomers copolymerizable therewith, and graft copolymers in which vinyl chloride monomers are graft polymerized onto a polymer.

[0100] The polycarbonate includes aromatic polycarbonate resins, aliphatic polycarbonate resins, and aromatic-aliphatic polycarbonate resins.

[0101] (Secondary ingredient) The adhesive layer 10 may contain, as a secondary component, for example, ethylene-vinyl acetate copolymer (EVA), polyolefin resin, polyester resin, polyamide resin, acrylic resin, polyurethane, polyvinyl chloride, polycarbonate, etc. (hereinafter, simply referred to as EVA, etc.). Among these, EVA and polyolefin resin are preferable. These may be used alone or may contain two or more kinds. Polyolefin resin, polyester resin, polyamide resin, acrylic resin, polyurethane, polyvinyl chloride, polycarbonate, etc. are the same as the above-mentioned polyolefin resin, polyester resin, polyamide resin, acrylic resin, polyurethane, polyvinyl chloride, polycarbonate, etc., and therefore detailed description thereof will be omitted.

[0102] The content of the secondary component can be appropriately designed depending on the types of thermoplastic elastomer and secondary component. When the secondary component is EVA, the content ratio of the thermoplastic elastomer to EVA is preferably 90:10 to 50:50, and more preferably 80:20 to 60:40.

[0103] In addition to the above components, the adhesive layer 10 may contain additives such as pigments, fillers, antioxidants, hydrolysis stabilizers, and antiblocking agents.

[0104] The content of the thermoplastic elastomer in the adhesive layer 10 is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and still more preferably 99.5% by mass or more, based on the total amount of the adhesive layer 10. The adhesive layer 10 may be composed of a thermoplastic elastomer.

[0105] The total thickness of the adhesive layer 10 can be designed appropriately and is, for example, preferably from 1 μm to 50 μm, and more preferably from 5 μm to 40 μm.

[0106] The adhesive layer 10 preferably has a melt tension of 7.5 mN or more, more preferably 8.0 mN or more, even more preferably 9.0 mN or more, even more preferably 10 mN or more, and most preferably 20.0 mN or more. If the melt tension of the adhesive layer 10 is 7.5 mN or more, the adhesive layer 10 can have a stable shape in a molten state that allows it to be stretched during molding when various molding methods such as the inflation method and the T-die method are used.

[0107] [Second layer] The second layer 20 is provided on the adhesive layer 10 (in the +Z-axis direction) and has an airtight function. The second layer 20 includes an intermediate layer 21 and an airtight layer 22, and is configured by laminating the intermediate layer 21 and the airtight layer 22 in this order on the adhesive layer 10.

[0108] (Middle class) The intermediate layer 21 is provided between the adhesive layer 10 and the airtight layer 22, and has the function of bonding the adhesive layer 10 and the airtight layer 22. The composition of the intermediate layer 21 can be selected depending on the composition and thickness of the adhesive layer 10 and the airtight layer 22, the application of the multilayer film 1, and the like. By providing the intermediate layer 21, the bonding force between the adhesive layer 10 and the airtight layer 22 can be strengthened, and thus delamination within the multilayer film 1 can be suppressed. Furthermore, by providing the intermediate layer 21, properties such as mechanical strength can also be improved.

[0109] The intermediate layer 21 may contain a thermoplastic elastomer or the like. These may be used alone or may contain two or more types. As the thermoplastic elastomer or the like, the same thermoplastic elastomer or the like as the thermoplastic elastomer or the like used in the adhesive layer 10 may be used. Therefore, detailed description of the thermoplastic elastomer or the like is omitted.

[0110] The content of the hard segment in the thermoplastic elastomer in the intermediate layer 21 is preferably 30% by mass to 95% by mass, more preferably 35% by mass to 90% by mass, and even more preferably 40% by mass to 85% by mass, relative to 100% by mass of the thermoplastic elastomer. By setting the content of the hard segment within the preferred range, the mechanical strength, heat resistance, and durability under high temperature and high humidity conditions of the multilayer film 1 can be improved, and the multilayer film 1 can have appropriate elasticity, flexibility, and formability.

[0111] The content of the soft segment in the thermoplastic elastomer in the intermediate layer 21 is preferably 5% by mass to 70% by mass, more preferably 10% by mass to 65% by mass, and even more preferably 15% by mass to 60% by mass, relative to 100% by mass of the thermoplastic elastomer. By setting the content of the soft segment within a preferred range, it is possible to ensure appropriate elasticity, flexibility, and formability of the multilayer film 1 and the resulting laminate, and to improve the mechanical strength of the multilayer film and the resulting laminate.

[0112] The melting point of the intermediate layer 21 is preferably higher than the melting point of the adhesive layer 10. While ensuring that the melting point of the intermediate layer 21 is higher than the melting point of the adhesive layer 10, the melting point of the intermediate layer 21 is preferably, for example, 90°C to 300°C, more preferably 130°C to 250°C or higher, and even more preferably 150°C to 220°C. The melting point of the intermediate layer 21 is adjusted depending on the type and content of the thermoplastic elastomer used in the intermediate layer 21, and the types and contents of the hard segment and soft segment constituting the thermoplastic elastomer, etc.

[0113] As described above, the melting point of the intermediate layer 21 is preferably higher than the melting point of the adhesive layer 10. The difference between the melting point of the intermediate layer 21 and the melting point of the adhesive layer 10 is preferably 10°C to 150°C, more preferably 20°C to 100°C. When the multilayer film 1 is bonded to the base fabric 2 using heat, by setting the difference between the melting point of the intermediate layer 21 and the melting point of the adhesive layer 10 within the above range, even if the heating temperature during production varies slightly, the bonding performance between the adhesive layer 10 and the airtight layer 22 can be maintained. Therefore, it is possible to reduce the occurrence of defective products in which the adhesive layer 10 is not sufficiently softened to be bonded to the base fabric 2 and cannot be bonded well, or the intermediate layer 21 is deformed or altered, resulting in impaired bonding between the adhesive layer 10 and the airtight layer 22, and thus improve production stability.

[0114] The intermediate layer 21 may contain a branched component in addition to a thermoplastic elastomer, similar to the adhesive layer 10. The branched component may be the same as that of the adhesive layer 10, and therefore a detailed description of the branched component will be omitted. By including a branched component in the intermediate layer 21, the thermoplastic elastomer forming the intermediate layer 21 can have a branched structure, which makes it easier to improve the stability of the shape when the intermediate layer 21 is molded.

[0115] The content of the branched components can be the same as that of the adhesive layer 10. When the content of the branched components is 0.1% by mass to 10% by mass, the thermoplastic elastomer contained in the intermediate layer 21 can have a branched structure and the flexibility of the intermediate layer 21 can be maintained.

[0116] When the intermediate layer 21 does not contain a thermoplastic elastomer, a branched component, or EVOH, like the adhesive layer 10, it may contain, instead of these, a polyolefin resin, a polyester resin, a polyamide resin, an acrylic resin, a polyurethane, a polyvinyl chloride, a polycarbonate, or the like. These may be used alone or may contain two or more types. As the polyolefin resin, etc., the same polyolefin resin as that of the adhesive layer 10 can be used, so detailed description of the polyolefin resin, etc. will be omitted.

[0117] The intermediate layer 21, like the adhesive layer 10, can contain, as a secondary component, EVA, polyolefin resin, polyester resin, polyamide resin, acrylic resin, polyurethane, polyvinyl chloride, polycarbonate, etc. Among these, EVA and polyolefin resin are preferred. These may be used alone or in combination of two or more.

[0118] The content of the auxiliary components may be the same as that of the adhesive layer 10 .

[0119] Like the adhesive layer 10, the intermediate layer 21 may contain additives such as pigments, fillers, antioxidants, hydrolysis stabilizers, and antiblocking agents in addition to the above-mentioned components.

[0120] The content of the thermoplastic elastomer in the intermediate layer 21 is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and still more preferably 99.5% by mass or more, based on the total amount of the intermediate layer 21. The intermediate layer 21 may be made of a thermoplastic elastomer.

[0121] The total thickness of the intermediate layer 21 can be designed appropriately and is, for example, preferably from 1 μm to 50 μm, and more preferably from 3 μm to 30 μm.

[0122] The intermediate layer 21 preferably has a melt tension of 7.5 mN or more, more preferably 8.0 mN or more, even more preferably 9.0 mN or more, even more preferably 10 mN or more, and most preferably 20.0 mN or more. If the melt tension of the intermediate layer 21 is 7.5 mN or more, the intermediate layer 21 can stably maintain its shape in a molten state that allows it to be stretched when various molding methods such as an inflation method or a T-die method are used.

[0123] The intermediate layer 21 may be composed of two or more layers. When the intermediate layer 21 is composed of multiple layers, the compositions of the layers may be the same or different. When the intermediate layer 21 is composed of multiple layers, the material of each intermediate layer 21 can be appropriately selected so as to improve the adhesiveness between the layers in the multilayer film 1, thereby making the bond between the layers stronger and further suppressing delamination within the multilayer film 1.

[0124] (Airtight layer) As described above, the airtight layer 22 is provided on the intermediate layer 21 (in the +Z-axis direction) and has an airtight function. Therefore, for example, when the multilayer film 1 is formed into a bag shape, it is possible to more reliably prevent air stored inside the bag from leaking out.

[0125] The airtight layer 22 may contain a thermoplastic elastomer or the like. These may be used alone or may contain two or more types. As the thermoplastic elastomer or the like, the same thermoplastic elastomer or the like as the thermoplastic elastomer or the like used in the adhesive layer 10 may be used. Therefore, detailed description of the thermoplastic elastomer or the like will be omitted.

[0126] The content of the hard segment in the thermoplastic elastomer in the airtight layer 22 is preferably 30% by mass to 95% by mass, more preferably 35% by mass to 90% by mass, and even more preferably 40% by mass to 85% by mass, based on 100% by mass of the thermoplastic elastomer. By setting the content of the hard segment within the preferred range, the mechanical strength, heat resistance, and durability under high temperature and high humidity conditions of the multilayer film 1 can be improved, and the multilayer film 1 can have appropriate elasticity, flexibility, and formability.

[0127] The content of the soft segment in the thermoplastic elastomer in the airtight layer 22 is preferably 5% by mass to 70% by mass, more preferably 10% by mass to 65% by mass, and even more preferably 15% by mass to 60% by mass, relative to 100% by mass of the thermoplastic elastomer. By setting the content of the soft segment within a preferred range, it is possible to ensure appropriate elasticity, flexibility, and formability of the multilayer film 1 and the resulting laminate, and to improve the mechanical strength of the multilayer film 1 and the resulting laminate.

[0128] The melting point of the airtight layer 22 is preferably higher than that of the adhesive layer 10, similarly to the intermediate layer 21. While ensuring the condition that the melting point of the airtight layer 22 is higher than that of the adhesive layer 10, the melting point is preferably 90° C. or higher, more preferably 150° C. or higher, and even more preferably 180° C. or higher. The upper limit of the melting point of the airtight layer 22 is sufficient to be higher than the melting point of the adhesive layer 10, and is preferably 300° C. or lower, more preferably 250° C. or lower, and even more preferably 230° C. or lower. The melting point of the airtight layer 22 is adjusted, similarly to the intermediate layer 21, according to the type and content of the thermoplastic elastomer used in the intermediate layer 21, the type and content of the hard segment and soft segment constituting the thermoplastic elastomer, and the like.

[0129] As described above, the melting point of the airtight layer 22 is preferably higher than the melting point of the adhesive layer 10. The difference between the melting point of the airtight layer 22 and the melting point of the adhesive layer 10 is preferably 10°C to 150°C, more preferably 20°C to 100°C. When the multilayer film 1 is bonded to the base fabric 2 by using heat, the difference between the melting point of the airtight layer 22 and the melting point of the adhesive layer 10 is set within the above range, so that the airtight function of the airtight layer 22 and the adhesive function of the adhesive layer 10 can be ensured even if the heating temperature during production varies slightly. Therefore, it is possible to reduce the occurrence of defective products in which the adhesive layer 10 is not sufficiently softened and cannot be well bonded to the base fabric 2, or the airtight layer 22 is deformed or altered, and thus the production stability can be improved.

[0130] The airtight layer 22 may contain a branched component in addition to the thermoplastic elastomer, similar to the adhesive layer 10. The branched component may be the same as that of the adhesive layer 10, and therefore a detailed description of the branched component will be omitted. When the airtight layer 22 contains a branched component, the thermoplastic elastomer forming the airtight layer 22 can have a branched structure, which makes it easier to improve the stability of the shape when the airtight layer 22 is molded.

[0131] The content of the branched components can be the same as that of the adhesive layer 10. When the content of the branched components is 0.1% by mass to 10% by mass, the thermoplastic elastomer contained in the airtight layer 22 can have a branched structure and the flexibility of the airtight layer 22 can be maintained.

[0132] When the airtight layer 22 does not contain a thermoplastic elastomer, a branched component, or EVOH, like the adhesive layer 10, it may contain, instead of these, a polyolefin resin, a polyester resin, a polyamide resin, an acrylic resin, a polyurethane, a polyvinyl chloride, a polycarbonate, or the like. These may be used alone or may contain two or more types. As the polyolefin resin, etc., the same polyolefin resin as the adhesive layer 10 can be used, so a detailed description of the polyolefin resin, etc. will be omitted.

[0133] The airtight layer 22 can contain, as a secondary component, EVA, polyolefin resin, polyester resin, polyamide resin, acrylic resin, polyurethane, polyvinyl chloride, polycarbonate, etc., similar to the adhesive layer 10. Among these, EVA and polyolefin resin are preferred. These may be used alone or in combination of two or more.

[0134] The content of the auxiliary components may be the same as that of the adhesive layer 10 .

[0135] Like the intermediate layer 21, the airtight layer 22 may contain additives such as pigments, fillers, antioxidants, hydrolysis stabilizers, and antiblocking agents in addition to the above-mentioned components.

[0136] The content of the thermoplastic elastomer in the airtight layer 22 is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and still more preferably 99.5% by mass or more, based on the total amount of the airtight layer 22. The airtight layer 22 may be made of a thermoplastic elastomer.

[0137] The total thickness of the airtight layer 22 can be designed appropriately and is, for example, preferably 1 μm to 50 μm, and more preferably 3 μm to 30 μm.

[0138] The airtight layer 22 preferably has a melt tension of 7.5 mN or more, more preferably 8.0 mN or more, even more preferably 9.0 mN or more, even more preferably 10 mN or more, and most preferably 20.0 mN or more. If the airtight layer 22 has a melt tension of 7.5 mN or more, the airtight layer 22 can stably maintain its shape in a molten state that allows it to be stretched when various molding methods such as an inflation method or a T-die method are used.

[0139] The airtight layer 22 may be composed of two or more layers. When the airtight layer 22 is composed of multiple layers, the compositions of the layers may be the same or different. When the airtight layer 22 is composed of multiple layers, the material of each airtight layer 22 can be appropriately selected so as to improve the adhesiveness between the layers in the multilayer film 1, thereby making the bond between the layers stronger and preventing delamination within the multilayer film 1.

[0140] When any one or more of the adhesive layer 10, intermediate layer 21, and airtight layer 22 constituting the multilayer film 1 contains a thermoplastic elastomer, the other layers not containing a thermoplastic elastomer may contain EVOH, polyolefin resin, polyester resin, polyamide resin, acrylic resin, polyurethane, polyvinyl chloride, polycarbonate, etc. Among them, it is preferable to contain EVOH. These may be used alone or may contain two or more kinds. As for EVOH, polyolefin resin, polyester resin, polyamide resin, acrylic resin, polyurethane, polyvinyl chloride, polycarbonate, etc., the same as the adhesive layer 10 described above, EVOH, polyolefin resin, polyester resin, polyamide resin, acrylic resin, polyurethane, polyvinyl chloride, polycarbonate, etc. can be used.

[0141] (Manufacturing of multi-layer films) An example of a method for producing the multilayer film 1 will be described. The materials (raw materials) of the adhesive layer 10, intermediate layer 21, and airtight layer 22 are each melted using a melt kneading machine such as an extruder or a pressure kneader, extruded simultaneously (co-extrusion), and molded using a known molding method such as an inflation method or a T-die method. As a result, the adhesive layer 10, intermediate layer 21, and airtight layer 22 can be obtained as separate sheets. Then, the adhesive layer 10 and the intermediate layer 21 are bonded, and the intermediate layer 21 and the airtight layer 22 are bonded, and these layers are laminated on the adhesive layer 10 in the order of the intermediate layer 21 and the airtight layer 22. As a result, the multilayer film 1 is obtained. Among them, it is preferable to use the inflation method, which allows for a large area and has excellent productivity.

[0142] When the inflation method is used, for example, an inflation molding machine equipped with a plurality of melt kneading devices (three in this embodiment) can be used. Fig. 2 is a diagram showing an example of an inflation molding machine equipped with a plurality of melt kneading devices. As shown in Fig. 2, an inflation molding machine 30 includes three melt kneading devices 31A, 31B, and 31C, an annular die 32, an air ring (cooling ring) 33, a pair of guide plates 34, a pinch roll 35, a guide roll 36, and a trimming 37.

[0143] The materials constituting the adhesive layer 10, the intermediate layer 21, and the airtight layer 22 are inserted into three melt-kneading devices 31A, 31B, and 31C, respectively, and melted in the three melt-kneading devices 31A, 31B, and 31C. When the melts of the materials constituting the adhesive layer 10, the intermediate layer 21, and the airtight layer 22 are extruded from the melt-kneading devices 31A, 31B, and 31C, respectively, into the annular die 32, the melts are extruded into a cylindrical film shape from the annular discharge port 321 of the annular die 32, as shown in FIG.

[0144] As shown in Fig. 2, air 38 is supplied from the bottom of the annular die 32, and as shown in Fig. 3, the air 38 is discharged upward from an air discharge port 322 provided in the center of the annular die 32 in a plan view. As shown in Fig. 2, the film-like molten material extruded into a cylindrical shape from the annular die 32 is inflated by the air flow of the air 38 discharged from the top of the annular die 32. At the same time, the molten material inflated into a tubular shape is air-cooled and solidified by air supplied from an air ring 33. As a result, the molten material is pulled upward as it becomes a cylindrical inflation film (bubble) 39.

[0145] The cylindrical inflation film 39 is taken up by the pinch rolls 35 along a pair of guide plates 34 located above the annular die 32 while squeezing out the air inside the inflation film 39. The inflation film 39 is pressed flat by the pinch rolls 35. The flattened inflation film 39 passes through a guide roll 36 located downstream of the pinch rolls 35, and is separated into two pieces at the interface between the adhesive layers 10A and 10B by trimming 37. The separated inflation film 39 passes through various guide rolls 36 and is taken up by a pair of take-up rolls 40. As a result, two multilayer films 1 are collected in a rolled state.

[0146] When the T-die method is used, for example, a T-die extrusion molding machine equipped with a plurality of (three in this embodiment) melt kneading devices can be used. Fig. 4 is a diagram showing an example of a T-die extrusion molding machine equipped with a plurality of melt kneading devices. As shown in Fig. 4, a T-die extrusion molding machine 50 includes three melt kneading devices 51A, 51B, and 51C, a three-kind three-layer distribution type feed block 52, a multi-manifold type die (multi-manifold type die) 53, a cooling roll 54, and a guide roll 55.

[0147] The materials constituting the adhesive layer 10, the intermediate layer 21, and the airtight layer 22 are melt-kneaded in the melt kneading devices 51A, 51B, and 51C, respectively. The melted and kneaded adhesive layer 10, intermediate layer 21, and airtight layer 22 are supplied to a three-kind, three-layer distribution type feed block 52 and distributed to form a three-layer structure. Then, as shown in FIG. 5, a molten multilayer film 56 formed from the melted adhesive layer 10, intermediate layer 21, and airtight layer 22 is discharged in a film shape from a discharge port (die lip) 53a of a multi-manifold type die 53. The discharged molten multilayer film 56 is cooled while being wound around a cooling roll 54. In this way, a multilayer film 1 is manufactured in which the intermediate layer 21 and the airtight layer 22 are laminated on the adhesive layer 10. Then, as shown in FIG. 4, the multilayer film 1 is passed through various guide rolls 55 and taken up by a take-up roll 57. In this way, the multilayer film 1 is collected in a roll state.

[0148] As another molding method, an extrusion lamination method may be used in which a melt of any of the adhesive layer 10, the intermediate layer 21, and the airtight layer 22 is extruded onto a molded sheet of any of the adhesive layer 10, the intermediate layer 21, and the airtight layer 22. This makes it possible to produce a multilayer film 1 in which the intermediate layer 21 and the airtight layer 22 are laminated in this order on the adhesive layer 10.

[0149] The produced multilayer film 1 can be cut into a desired shape and size depending on the application. The multilayer film 1 may be wound around a roll or the like, and may be unwound and cut to the required length when used. Furthermore, the multilayer film 1 may be provided with a release sheet at least on the adhesive layer 10 side. This allows the adhesive layer 10 to be protected until immediately before use.

[0150] As described above, the multilayer film 1 includes the adhesive layer 10 and the second layer 20, and either or both of the adhesive layer 10 and the second layer 20 contain a thermoplastic elastomer. The adhesive layer 10 or the second layer 20 uses at least one selected from the group consisting of polyester-based elastomers, polyurethane-based elastomers, and polyamide-based elastomers as the thermoplastic elastomer, and the melt tension of the multilayer film 1 is set to 7.5 mN or more. By using at least a polyester-based elastomer, a polyurethane-based elastomer, or a polyamide-based elastomer as the thermoplastic elastomer used in each layer constituting the multilayer film 1, the multilayer film 1A can stably maintain its shape in a molten state that allows it to be stretched during molding. Therefore, the multilayer film 1 can have excellent molding stability. Therefore, the multilayer film 1 can be effectively used in various molding methods such as the inflation method and the T-die method.

[0151] In the case of molding using the inflation method, the shape stability of the multilayer film 1 can be evaluated by observing the molding state of the inflation film drawn from the annular die 32 of the inflation molding machine 30 as shown in FIG. 2. In the case of molding using the T-die method, the shape stability can be evaluated by measuring the neck-in ratio (unit: %) of the film-like melt extruded from the discharge port 53a of the multi-manifold die 53 of the T-die extrusion molding machine 50 as shown in FIG. 4. As shown in FIG. 6, the neck-in width W1 of the film-like melt is the difference between the width W0 of the discharge port 53a and the width (film width) W2 of the film-like melt (neck-in width W1 = width W0 of the discharge port 53a - film width W2). The neck-in ratio is a percentage value obtained by dividing the sum of the two widths generated at both ends of the discharge port 53a by the width of the discharge port 53a ((sum of neck-in widths / width of discharge port) × 100 (%)). The higher the neck-in ratio, the easier the film-like melt is to deform, and the thickness of both ends of the film-like melt tends to increase.

[0152] Therefore, the multilayer film 1 can maintain good stability during molding, for example, even when molded using an inflation method. Also, the multilayer film 1 can prevent the width of the film extruded from the T-die from narrowing and prevent an increase in the neck-in width, for example, even when molded using a T-die method. Therefore, the multilayer film 1 can achieve good yield during molding.

[0153] Furthermore, since the multilayer film 1 can be prevented from being deformed during molding, the area and associated burden required to cut out the deformed portion can be reduced, and therefore the cost required during production can be reduced.

[0154] In the multilayer film 1, the melt tension of at least one of the adhesive layer 10 and the second layer 20 can be set to 7.5 mN or more. This allows the adhesive layer 10 and the second layer 20 in the multilayer film 1 to have a stable shape in a molten state that allows stretching during molding, and therefore the multilayer film 1 can be stably molded even when various molding methods such as an inflation method or a T-die method are used.

[0155] In the multilayer film 1, the second layer 20 can include an airtight layer 22. This allows the multilayer film 1 to maintain molding stability while having airtightness.

[0156] In the multilayer film 1, the second layer 20 can include an intermediate layer 21 between the adhesive layer 10 and the airtight layer 22. This can increase the bonding strength between the adhesive layer 10 and the airtight layer 22, thereby suppressing the occurrence of interlayer peeling within the multilayer film 1 and maintaining molding stability.

[0157] In the multilayer film 1, at least one of the adhesive layer 10, the intermediate layer 21, and the airtight layer 22 can have a melt tension of 7.5 mN or more. This allows the adhesive layer 10, the intermediate layer 21, and the airtight layer 22 to have a stable shape in a molten state that allows stretching during molding, so that the adhesive layer 10, the intermediate layer 21, and the airtight layer 22 can be molded while stably maintaining their respective shapes even when various molding methods such as an inflation method or a T-die method are used.

[0158] In the multilayer film 1, at least one of the adhesive layer 10 and the second layer 20 contains a branched component, and the thermoplastic elastomer contained in the adhesive layer 10 or the second layer 20 can have a branched structure. When the thermoplastic elastomer has a branched structure, it is easier to suppress deformation during molding compared to thermoplastic elastomers that generally have a linear structure such as olefin-based thermoplastic elastomers. Therefore, in the multilayer film 1, when at least one of the adhesive layer 10 and the second layer 20 contains a branched component and the thermoplastic elastomer has a branched structure, the multilayer film 1 can maintain a more stable molded state even when various molding methods are used.

[0159] The content of the branched component in the multilayer film 1 can be 0.1% by mass to 10% by mass. Depending on the content of the branched component, the content of the thermoplastic elastomer having a branched structure in the adhesive layer 10 and the second layer 20 can be adjusted. This allows the multilayer film 1 to maintain a more stable molded state using various molding methods such as an inflation method or a T-die method, and also allows it to have flexibility.

[0160] In the multilayer film 1, either or both of the adhesive layer 10 and the second layer 20 may contain an ethylene-vinyl alcohol copolymer. By containing an ethylene-vinyl alcohol copolymer as a component other than the thermoplastic elastomer, the adhesive layer 10 and the second layer 20 can easily adjust the melt tension of the adhesive layer 10 and the second layer 20 to a desired value. This allows the multilayer film 1 to maintain a more stable molded state and have flexibility even when various molding methods such as an inflation method or a T-die method are used.

[0161] The multilayer film 1 can use the base fabric 2 as an airbag base fabric, and thus the multilayer film 1 can be effectively used as a protective film provided on the surface of the base fabric of an airbag formed into a bag shape.

[0162] <Laminate> Next, a laminate to which the multilayer film 1 according to the present embodiment is applied will be described. Fig. 7 is a cross-sectional view showing a schematic example of a laminate. As shown in Fig. 7, the laminate 100 includes multilayer films 1A and 1B and a base fabric 2, and the multilayer films 1A and 1B are bonded to the base fabric 2.

[0163] Multilayer film 1A is provided on the upper surface side (+Z axis direction) of base fabric 2, and multilayer film 1B is provided on the lower surface side (-Z axis direction) of base fabric 2.

[0164] (base fabric) The base fabric 2 functions as a support for ensuring the mechanical strength of the laminate 100, and is formed in a sheet shape. The sheet shape includes a planar shape, as well as a shape formed in a cylindrical or bag shape when viewed as a whole.

[0165] The base fabric 2 preferably contains fibers, and may be a woven fabric, knitted fabric, nonwoven fabric, or the like. The base fabric 2 may be sewn partially or entirely. When the base fabric 2 is formed in a flat shape, the base fabric 2 may be a flat woven fabric such as plain weave, twill weave, or satin weave. When the base fabric 2 is formed in a bag shape, the base fabric 2 may be a one piece woven (OPW) woven seamlessly into a tube or bag shape so that it can have a curved surface according to the shape of the product.

[0166] The fibers contained in the base fabric 2 may be synthetic fibers, natural fibers, regenerated fibers, semi-synthetic fibers, inorganic fibers, or combinations thereof (including blends and weaves). These may be used alone or in combination of two or more. Among these, synthetic fibers are preferred. As the fibers, composite fibers such as core-sheath type fibers, side-by-side type fibers, and split type fibers may be used.

[0167] Polymers constituting synthetic fibers include polyester, polyolefin, aramid, acrylic, vinylon, polyurethane, copolymers in which the acid components constituting the repeating units of polyester are copolymerized with aliphatic dicarboxylic acids such as isophthalic acid, 5-sodium sulfoisophthalic acid, or adipic acid, nylon 6·6, nylon 6, nylon 12, nylon 4·6, and nylon 6-nylon 66 copolymers, polyamides in which nylon is copolymerized with polyalkylene glycol, dicarboxylic acids, amines, etc., aramids such as paraphenylene terephthalamide and copolymers with aromatic ethers, sulfone resins such as paraphenylene sulfone and polysulfone, rayon, ultra-high molecular weight polyethylene, polyether ketone, etc. These may be used alone or in combination of two or more types.

[0168] Examples of polyesters include polyalkylene terephthalates such as polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), polybutylene terephthalate (PBT), and polyethylene naphthalate (PEN); polyalkylene naphthalates such as polybutylene naphthalate (PBN), etc. These may be used alone or in combination of two or more.

[0169] In particular, when the adhesive layer 10 constituting the multilayer film 1 contains a polyester-based elastomer, the base fabric 2 preferably contains a fiber made of polyester (polyester fiber) or a fiber containing polyester. The base fabric 2 may contain polyester fiber mixed with other fibers by interweaving or the like, may contain a blended fiber of polyester and a material other than polyester, or may contain a composite fiber of polyester and a material other than polyester, such as a core-sheath type, a side-by-side type, or a split type, made of polyester and a material other than polyester. When the adhesive layer 10 contains a polyester-based elastomer, the base fabric 2 contains polyester, which improves the adhesive strength between the multilayer film 1 and the base fabric 2, so that the laminate 100 can have even better durability. In addition, the laminate 100 can be manufactured relatively inexpensively while ensuring mechanical strength and weather resistance. Furthermore, when the base fabric 2 is made of polyester fiber, the above effect is even more pronounced.

[0170] When the base fabric 2 has a structure including threads extending in a plurality of different directions, different types of fibers may be used for the threads extending in each direction.

[0171] The yarns contained in the base fabric 2 may be monofilament or multifilament. When the yarns are multifilament, the total yarn fineness (single yarn fineness x number of yarns) is preferably 100 dtex to 700 dtex. The single yarn fineness of the fibers used in the base fabric 2 is preferably 1 dtex to 10 dtex. When the base fabric 2 is a plain weave fabric, the weaving density is preferably 5 warp yarns / cm and 5 weft yarns / cm. 2 ~30 pieces / cm 2It is preferable that:

[0172] Base fabric 2 unit weight (1m 2 The mass per unit area is preferably 30 g / m2 in order to ensure the mechanical strength of the laminate 100, improve the storage property of the laminate 100, and reduce the cost. 2 ~300g / m 2 and more preferably 50 g / m 2 ~200g / m 2 and more preferably 70 g / m 2 ~150g / m 2 More preferably, 80 g / m 2 ~100g / m 2 The following is the result.

[0173] The base fabric 2 may be densely woven. In this case, the laminate 100 can be made stronger. The base fabric 2 may have openings. When the base fabric 2 has openings, the laminate 100 can be made lighter. The laminate 100 is formed by laminating a preformed multilayer film 1 onto the base fabric 2. Therefore, even if the base fabric 2 has openings, the laminate 100 can have sufficient mechanical strength and airtightness without causing inconveniences such as the relatively low-viscosity polymer composition penetrating through the openings.

[0174] (Method of manufacturing laminate) An example of a method for producing the laminate 100 will be described. Fig. 8 is a schematic diagram showing an example of a laminate production apparatus applied to the method for producing the laminate. As shown in Fig. 8, the laminate production apparatus 60 includes a heating / pressurizing section 61 and a cooling section 62.

[0175] The heating and pressing unit 61 includes, for example, a pair of opposing rolls (nip rolls or the like) 611, a pair of opposing belts 612, and a heating unit (not shown). At least one of the pair of rolls 611 or the belt 612 can be heated by the heating unit (not shown).

[0176] The heating temperature can be appropriately designed according to the melting points of the adhesive layer 10, the intermediate layer 21, and the airtight layer 22. When the melting point of the adhesive layer 10 is lower than that of the intermediate layer 21 and the airtight layer 22, the heating temperature is preferably a temperature lower than the melting points of the intermediate layer 21 and the airtight layer 22, at which the adhesive layer 10 is softened or melted. By setting the heating temperature to a temperature lower than the melting points of the intermediate layer 21 and the airtight layer 22, the functions of the intermediate layer 21 and the airtight layer 22 can be more reliably ensured. In addition, the adhesive layer 10 can be softened or melted without melting (melting) the intermediate layer 21 and the airtight layer 22. The heating temperature may be any temperature at which the intermediate layer 21 and the airtight layer 22 do not lose their airtight function due to the influence of heat.

[0177] The heating temperature depends on the melting points of the adhesive layer 10, the intermediate layer 21 and the airtight layer 22, but is preferably from 100°C to 250°C, and more preferably from 120°C to 200°C, for example.

[0178] The pressure applied can be appropriately designed depending on the layer structure of the laminate 100, the thickness of the adhesive layer 10, the intermediate layer 21 and the airtight layer 22, etc. The pressure applied is, for example, 5 N / cm. 2 ~700N / cm 2 is preferred, and 10 N / cm 2 ~500N / cm 2 More preferably, 15 N / cm 2 ~50N / cm 2 is more preferred.

[0179] The cooling section 62 can lower the temperature of the laminate 100, preferably to room temperature. The cooling section 62 includes a pair of opposing rolls (nip rolls or the like) 621, a pair of opposing belts 622, a cooling section (not shown) containing a cooling medium, and an intake section (shown). At least one of the pair of rolls 621 or the belts 622 can be cooled by the cooling section (not shown).

[0180] In the laminate manufacturing apparatus 60, the base fabric 2 and the multilayer films 1A and 1B, which have been wound up in advance on a roll 611 or the like, are unwound, and the multilayer films 1A and 1B are superimposed on both sides (upper and lower surfaces) of the base fabric 2. The superimposed multilayer film 1A, base fabric 2, and multilayer film 1B are sent to a heating and pressing section 61, where the multilayer films 1A and 1B are heated and pressed.

[0181] In the heating and pressurizing section 61, at least one of the pair of rolls 611 or the belt 612 is heated, and the superimposed multilayer film 1A, base fabric 2, and multilayer film 1B are passed between the pair of belts 612, thereby performing heating and pressurization.

[0182] The heating temperature is preferably, for example, a temperature at which the adhesive layer 10 softens or melts, but at which the intermediate layer 21 and the airtight layer 22 do not melt (dissolve). This allows the adhesive layer 10 to be pressed against the base fabric 2 in a state in which the adhesive layer 10 is sufficiently softened or melted, while ensuring the functions of the intermediate layer 21 and the airtight layer 22. The softened or melted adhesive layer 10 also penetrates into the recesses of the uneven surface of the base fabric 2, allowing the adhesive layer 10 to be tightly adhered to the base fabric 2. This allows the multilayer films 1A and 1B to be adhered to the base fabric 2, respectively, and a laminate 100 including the multilayer film 1A, the base fabric 2, and the multilayer film 1B is formed and transported.

[0183] The laminate 100 that has passed through the heating and pressing section 61 is transported to a cooling section 62 .

[0184] In the cooling section 62, at least one of the pair of rolls 621 or the belts 622 is cooled, and the laminate 100 is passed between the pair of belts 622, thereby performing cooling and pressurization. The temperature of the laminate 100 is preferably lowered to room temperature. Note that the cooling section 62 does not necessarily have to pressurize the laminate 100 using the pair of opposing belts 622.

[0185] The laminate 100 that has passed through the cooling section 62 is taken up by a roll 63 .

[0186] By including the multilayer film 1, the laminate 100 is less susceptible to misalignment or distortion between the multilayer film 1 and the base fabric 2, and the multilayer film 1 can be stably bonded to the base fabric 2. As a result, the laminate 100 is less susceptible to interlayer peeling between the multilayer film 1 and the base fabric 2, and has excellent durability.

[0187] The laminate 100 can be bonded to the base fabric 2 by at least one of heating and pressing the multilayer film 1 in the heating and pressing section 61. This allows the adhesive layer 10 to be impregnated into the base fabric 2 while bonding, thereby further improving the durability of the laminate 100.

[0188] Since the laminate 100 has excellent formability even when the multilayer film 1 is adhered to the base fabric 2, it can be suitably used as the base fabric 2, for example, for a seamless tubular or bag-shaped OPW.

[0189] Fig. 9 is a cross-sectional view showing an example in which the base fabric is OPW. As shown in Fig. 9, the laminate 100 comprises multilayer films 1A and 1B, and an OPW 2A that contains air in its internal space and is inflated like a bag, with multilayer films 1 provided on the upper and lower surfaces of the OPW 2A. The edges of the multilayer films 1A and 1B are bonded to each other by applying heat and pressure.

[0190] When a laminate 100 including an OPW 2A is manufactured using a laminate manufacturing apparatus 60 shown in FIG. 8, the OPW 2A is used after the air has been removed from inside and the OPW 2A is rolled up in a flat state. The laminate 100 is pressed from both sides by a pair of rolls 621 in a heating and pressing section 61. As a result, the multilayer films 1A and 1B are bonded to the upper and lower surfaces of the OPW 2A, respectively, and the edges of the multilayer films 1A and 1B are bonded to each other by heating and pressing. This makes it possible to obtain a laminate 100 as shown in FIG. 9. The obtained laminate 100 can inflate the air in the internal space of the OPW 2A into a bag shape.

[0191] The adhesive layers 10A and 10B may be bonded so as to cover the entire edge of the OPW 2A. Any excess edge of the laminate 100 may be removed by cutting or the like. This allows the multilayer film 1 to be formed on the entire surface of the OPW 2A formed in a bag shape.

[0192] The obtained laminate 100 can be used in a state where the multilayer film 1 is stably adhered to the surface of the OPW 2A that can be inflated and used in a state where air is stored inside, and therefore can be suitably used for vehicle airbags, outdoor products, packaging applications, and the like. The laminate 100 can be particularly suitably used for vehicle airbags, especially curtain airbags. The curtain airbag is attached to the roof line or the like above the side window of the vehicle, and is stored in a casing or the like in a folded or rolled state. When a high load is applied during a collision or the like, the curtain airbag inflates into a bag shape and deploys vertically downward in a curtain shape along the side window. Therefore, the OPW used for the curtain airbag has a complex curved surface with multiple chambers formed therein, and tends to have an uneven structure when inflated. The laminate 100 includes the multilayer film 1 according to this embodiment, and can maintain a state where the multilayer film 1 is well adhered to the OPW 2A that forms a curved surface when inflated into a bag shape and may have unevenness on the surface. Therefore, the laminate 100 can suppress interlayer delamination between the multilayer film 1 and the OPW 2A, and the occurrence of damage and the like is suppressed, resulting in excellent durability.

[0193] (Modification) In this embodiment, at least one of the adhesive layer 10, the intermediate layer 21, and the airtight layer 22 may be formed of two or more layers. For example, the multilayer film 1 may be configured with the adhesive layer 10 and the intermediate layer 21 as multiple layers (e.g., two layers) and the airtight layer 22 as a single layer.

[0194] In this embodiment, the second layer 20 may be formed of an intermediate layer 21 or an airtight layer 22 .

[0195] In this embodiment, the laminate 100 may have the multilayer film 1 laminated only on one side of the base fabric 2. For example, as shown in Fig. 10, the laminate 100 may have the multilayer film 1 laminated only on the upper surface (+Z-axis direction) of the base fabric 2.

[0196] In this embodiment, the laminate 100 may be produced by adhering the multilayer film 1, supplied at room temperature or below, to the base fabric 2 while heating the multilayer film 1 at a temperature below the melting point of the airtight layer 22 using a heating means. The laminate 100 may also be produced, for example, by adhering a polymer extruded into a film shape by an extruder to the base fabric 2. Furthermore, the laminate 100 may be produced by adhering the multilayer film 1 and the base fabric 2 by applying pressure to the multilayer film 1 and the base fabric 2 while heating at a temperature at which the airtight layer 22 does not melt. EXAMPLES

[0197] The embodiments will be described in more detail below with reference to examples and comparative examples, but the embodiments are not limited to these examples and comparative examples.

[0198] <Preparation of raw materials> Raw materials that can be used for the layers (adhesive layer, intermediate layer, airtight layer) that form the multilayer film were prepared. As the raw materials, single materials and mixtures of multiple materials were prepared. The single materials and mixtures are shown below. (Material alone) Polyester-based thermoplastic elastomer (TPEE-1) Polyester-based thermoplastic elastomer (TPEE-2) Polyester-based thermoplastic elastomer (TPEE-3) Thermoplastic polyurethane elastomer (TPU): "Estane® 58277", manufactured by Lubrizol, melting point 130°C Ethylene-vinyl acetate copolymer (EVA: "Evatane® 28-05", Arkema, melting point 72°C) (mixture) Mixture 1: Mixture of TPEE-2 (80% by mass) and EVA (20% by mass) Mixture 2: Mixture of TPEE-2 (70% by mass) and EVA (30% by mass) Mixture 3: Mixture of TPEE-2 (60% by mass) and EVA (40% by mass) Mixture 4: Mixture of TPEE-3 (70% by mass) and EVA (30% by mass)

[0199] TPEE-1, TPEE-2 and TPEE-3 were prepared as follows. The melting points of the prepared raw materials were the melting peak temperatures measured by a differential scanning calorimeter (DSC). (TPEE-1) A polyester-polyether block copolymer, TPEE-1, was prepared by using polybutylene terephthalate (PBT) as a hard segment and polytetramethylene ether glycol (PTMG) as a soft segment. In the copolymer, the content of PBT was 85% by mass, and the content of PTMG was 15% by mass. The melting point of the obtained polyester-polyether block copolymer was 210°C. (TPEE-2) TPEE-2, a polyester-polypropylene block copolymer, was prepared with PBT as the hard segment, polypropylene glycol (PPG) as the soft segment, and trimellitic acid as the branching component. In the copolymer, the PBT content was 49.5% by mass, the PPG content was 50% by mass, and the trimellitic acid content was 0.5% by mass. The melting point of the obtained polyester-polypropylene block copolymer was 210°C. (TPEE-3) A polyester-polyether block copolymer, TPEE-3, was prepared by using PBT as the hard segment and PTMG as the soft segment. In the copolymer, the content of PBT was 55% by mass and the content of PTMG was 45% by mass. The melting point of the obtained polyester-polyether block copolymer was 150°C.

[0200] <Melt tension measurement> The melt tension of each of the prepared materials and the mixture was measured. (Melt tension measurement of single material) After making pellets of the individual materials, each individual material was heated to 230°C to melt. Using a Malvern Panalytical capillary rheometer (ROSAND RH7), the molten individual materials were extruded from a capillary (diameter: 1 mm, length: 10 mm, inlet angle: 180°) at a constant speed of 8.8 mm / min. The extruded molten individual material was taken up at a gradually increasing take-up speed from 5 m / min, and the tension at which the resin broke was recorded as the melt tension. The measurement results are shown in Table 1. (Melt tension measurement of mixture) Pellets of the individual materials constituting the mixture were melt-mixed to prepare pellets of the mixture, which were then heated to 230°C to melt them. The melt tension of the molten mixture was measured in the same manner as for the individual materials. The measurement results are shown in Table 1.

[0201] [Table 1]

[0202] <Example 1> [Making multilayer films] (Preparation of multi-layer films using the inflation method) The three prepared raw materials (TPEE-1, TPEE-2, and TPEE-3) were fed into the extruders of an inflation extrusion apparatus (VAREX II, manufactured by Windmoeller & Hoelscher) having five extruders (extruder 1 to extruder 5), with TPEE-1 being fed into extruder 1, TPEE-2 into extruders 2 and 3, and TPEE-3 into extruders 4 and 5. Each raw material was melted at a temperature equal to or higher than the melting point of the respective raw material, and the molten material of each resin in each extruder was extruded from the extruder into a die having a circular discharge port. The extrusion rate of the molten material of each resin was 10 g / m for each extruder. 2The extruded molten material was pulled up into a cylindrical inflation film (bubble), and a multilayer film with a three-layer structure was produced, with the airtight layer being TPEE-1, the middle layer being TPEE-2, and the adhesive layer being TPEE-3.

[0203] (Production of multi-layer film using the T-die method) As shown in FIG. 5, a three-layered multilayer film was produced by feeding three prepared raw materials (TPEE-1, TPEE-2, and TPEE-3) into three extruders using a simultaneous extruder (FILMIX II, manufactured by Windmoeller & Hoelscher). Each raw material was melted at a temperature equal to or higher than the melting point of each raw material, and the melt of each resin in each extruder was fed to a die having three outlets (ports). The raw materials were simultaneously extruded into a film shape from the outlet of the T-die, laminated, and cooled to produce a multilayer film in which an adhesive layer 10, an intermediate layer 21, and an airtight layer 22 were laminated. The screw speed of each extruder was set so that a film-like melt having a desired thickness was extruded from the T-die in a normal manner.

[0204] [evaluation] The multilayer film was evaluated by measuring the melt tension, the bubble stability when the inflation method was used with an inflation molding machine, and the neck-in ratio when the T-die method was used.

[0205] (Melt tension measurement) The multilayer film was melted and mixed to prepare pellets in which each layer of the multilayer film was uniformly distributed, and then heated to 230°C to melt the pellets. The melt tension of the molten multilayer film was measured in the same manner as for the single material.

[0206] (Stability of bubbles when using the inflation method) The multilayer films obtained using the inflation method were checked for wrinkles, and the stability of the bubbles when the bubbles of the molten resin were pulled up and molded was evaluated. If no wrinkles were found in the multilayer film, it was judged as excellent (indicated as A in Table 2), if wrinkles were found in the multilayer film but were not problematic as a product, it was judged as good (indicated as B in Table 2), and if a multilayer film could not be formed, it was judged as poor (indicated as C in Table 2).

[0207] (Neck-in rate when using the T-die method) The molten multilayer film produced in the same manner as in the measurement of melt tension was extruded from the discharge port of a T-die using the T-die method, and the neck-in ratio (unit: %) around the discharge port was measured (see Figure 6). The neck-in ratio was calculated as a percentage obtained by dividing the sum of the two widths at both ends of the discharge port by the width of the discharge port ((sum of neck-in widths / width of discharge port) x 100). If the neck-in ratio was at a level that did not pose a problem as a product, it was judged to be good (represented as A in Table 2), and if it was problematic as a product or a multilayer film could not be formed, it was judged to be bad (represented as B in Table 2).

[0208] <Example 2> The same procedure as in Example 1 was repeated, except that the airtight layer was changed from TPEE-3 to Mixture 4.

[0209] <Example 3> The procedure of Example 1 was repeated, except that the adhesive layer was changed from TPEE-1 to TPEE-2, the intermediate layer was changed from TPEE-2 to Mixture 4, and the airtight layer was changed from TPEE-3 to Mixture 4.

[0210] <Comparative Example 1> The same procedure as in Example 1 was repeated, except that the adhesive layer was changed from TPEE-1 to TPU and the intermediate layer was changed from TPEE-2 to TPU.

[0211] <Comparative Example 2> The same procedure as in Example 1 was repeated, except that the intermediate layer was changed from TPEE-2 to TPU.

[0212] Table 2 shows the measurement results of the melt tension of the multilayer film, the stability of the bubble shape when the inflation method was used, and the neck-in ratio when the T-die method was used for each of the examples and comparative examples.

[0213] [Table 2]

[0214] As shown in Table 1, TPEE-2 had a melt tension of 20 mN or more. In addition, in the case of a mixture containing TPEE-2, when the content of TPEE-2 was 40% or more, the melt tension was 8.0 mN or more. On the other hand, TPEE-1 had a melt tension of 5.6 mN, and the melt tension of TPEE-3 could not be measured. Therefore, it was confirmed that a polyester-based thermoplastic elastomer or a mixture containing a polyester-based thermoplastic elastomer has a melt tension of 8.0 mN or more. It was also confirmed that if the polyester-based thermoplastic elastomer has a branched structure, the melt tension can be made higher.

[0215] As shown in Table 2, in Examples 1 to 3, the melt tension was 8.0 mN or more, the bubble shape was good when the inflation method was used, and the neck-in ratio was 30% or less when the T-die method was used. Therefore, it was confirmed that if a single material or a mixture of materials with high melt tension is used in the adhesive layer or intermediate layer of a multilayer film, the melt tension of the multilayer film itself can be increased and excellent molding stability can be achieved.

[0216] As described above, the embodiment has been described, but the above embodiment is presented as an example, and the present invention is not limited to the above embodiment. The above embodiment can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]

[0217] 1 Multilayer film 10 Adhesive layer (1st layer) 20 2nd layer 21 Middle Class 22 Airtight layer 2 Base fabric 2A OPW 100 Laminate

Claims

1. A multilayer film adhered to a fabric substrate, a first layer adhered to the backing; a second layer disposed on the first layer; and the second layer comprises an airtight layer and an intermediate layer between the first layer and the airtight layer; One or both of the first layer and the second layer comprises a thermoplastic elastomer; the thermoplastic elastomer is at least one selected from the group consisting of polyester-based elastomers, polyurethane-based elastomers, and polyamide-based elastomers, A multilayer film having a melt tension of 7.5 mN or more, wherein The first layer is a polyester-polyether block copolymer TPEE-3 having polybutylene terephthalate (PBT) as a hard segment and polytetramethylene ether glycol (PTMG) as a soft segment; the airtight layer is a polyester-polyether block copolymer TPEE-1 having PBT as a hard segment and PTMG as a soft segment; and the intermediate layer is a polyester-polypropylene block copolymer TPEE-2 having PBT as a hard segment, polypropylene glycol (PPG) as a soft segment, and a branched component being trimellitic acid; or The first layer is the TPEE-3, the airtight layer is a mixture 4 of the TPEE-3 (70% by mass) and ethylene-vinyl acetate copolymer (EVA) (30% by mass), and the intermediate layer is the TPEE-2; or The first layer is the TPEE-2, and the airtight layer and the intermediate layer are the mixture 4. Multilayer film.

2. 2. The multilayer film according to claim 1, wherein at least one of the first layer and the second layer has a melt tension of 7.5 mN or more.

3. 2. The multilayer film according to claim 1, wherein at least one of the first layer, the intermediate layer and the airtight layer has a melt tension of 7.5 mN or more.

4. A multilayer film as described in claim 1, wherein the content of branched components in the thermoplastic elastomer is 0.1 mass % to 10 mass %.

5. The multilayer film according to any one of claims 1 to 4, wherein the base fabric is an airbag base fabric.

6. The multilayer film according to any one of claims 1 to 5, A base fabric; A laminate comprising:

7. An airbag comprising the laminate according to claim 6.

Citation Information

Patent Citations

  • Thermoplastic resin composition

    JP1997221588A

  • Polyester resin, polyester resin composition and extrusion molding

    JP2001200038A

  • Laminated molded body

    JP2002144486A

  • Thermoplastic polyurethane resin and its manufacturing method

    JP2003026755A

  • Ethylene-vinyl alcohol copolymer resin composition and its manufacturing method