Industrial furnace and construction method thereof
Patent Information
- Application Number
- JP2020199933
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-01
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-12-01
AI Technical Summary
【0010】 請求項1に記載の工業炉は、施工作業(築炉作業あるいは補修作業)が容易であり、短期間で施工することができる。その上、枠体が外壁の内面に固着されており、耐火レンガの周方向のずれが抑えられることで、熱電対の周囲の耐火レンガが剥落しにくいので、必要な補修の頻度を低く抑えることができる上、熱電対の損傷も防止できるので、炉の安定操業につながる(寄与する)。
Smart Images

Figure 0007562392000001 
Figure 0007562392000002 
Figure 0007562392000003
Abstract
Description
[Technical field]
[0001] This relates to various industrial furnaces in which a layer of fireproof bricks is laminated on the inside of a metal peripheral wall (exterior wall) and a thermocouple is installed to detect the internal temperature, and to their construction methods. [Background technology]
[0002] A rotary kiln, which has a long cylindrical kiln body that can rotate around an axis along the longitudinal direction, is known as an industrial furnace used for manufacturing cement, etc. (Patent Document 1). The outer periphery of such a rotary kiln is covered with an outer wall (iron shell) made of metal (carbon steel, etc.) having a predetermined thickness, and a firebrick layer is formed by assembling firebricks inside the outer wall. In addition, a number of rod-shaped thermocouples for detecting the internal temperature are covered by a cylindrical protective tube and are provided so as to be perpendicular to the outer wall surface of the kiln body (Patent Document 2).
[0003] Conventionally, when constructing a rotary kiln, firebricks are assembled inside the outer wall, and when the installation location of the thermocouple and protective tube is reached, the overlapping firebricks are cut to match the shapes of the thermocouple and protective tube protruding inward, and then assembled. In addition, when repairing a rotary kiln, all remaining firebricks after melting are removed, and new firebricks are assembled in the same way. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 7-159042 [Patent Document 2] JP 2018-173358 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the conventional rotary kiln construction or repair method, since the refractory bricks must be individually drilled and cut to fit the protruding position of the thermocouple at the installation position, the installation (laying) work of the refractory bricks at the installation position of the thermocouple is very time-consuming. In addition, in the rotary kiln, the thermocouple may be bent together with the protective tube during use, so the refractory bricks must be individually drilled and cut to fit the bent shape, which makes the construction or repair work even more time-consuming. In addition, if the refractory bricks are drilled and cut to fit the bent shape of the thermocouple, cracks will occur at the drilled and cut parts during use. If the refractory bricks are displaced in the circumferential direction due to the rotation of the rotary kiln, the refractory bricks will easily fall off from the cracked parts. If the refractory bricks fall off, repairs will be required again at short intervals. Furthermore, the thermocouple may be damaged as the rotary kiln rotates, especially if the refractory bricks around the thermocouple are displaced in the circumferential direction, and if the thermocouple is damaged, it will be impossible to measure the temperature inside the kiln, causing problems in the operation of the kiln.
[0006] The object of the present invention is to provide a method of constructing an industrial furnace that solves the problems of the above-mentioned conventional methods of constructing or repairing an industrial furnace (an industrial furnace equipped with an internal temperature detection function using a thermocouple), that makes the construction or repair work very easy, extends the service life of the furnace after construction or repair, reduces the frequency of repairs, and enables stable operation of the furnace. It is also to provide an industrial furnace that requires less repairs and enables stable operation when constructed by such a method. [Means for solving the problem]
[0007] Among the present inventions, the invention described in claim 1 is an industrial furnace in which a layer of fireproof bricks is laminated inside a metal outer wall, and a thermocouple and a protective tube for detecting the internal temperature are provided so as to penetrate the outer wall and the fireproof brick layer, characterized in that a metal frame is fixed to the inner surface of the outer wall so as to cover the thermocouple and protective tube protruding into the interior, the inside of the frame is filled with amorphous refractory material, and fireproof bricks are assembled in the parts other than the frame.
[0008] The invention described in claim 2 is the invention described in claim 1, characterized in that an anchor is fixed to the outer wall inside the frame body.
[0009] The invention described in claim 3 is a construction method for an industrial furnace in which a fireproof brick layer is laminated inside a metal outer wall, and a thermocouple and a protective tube for detecting the internal temperature are arranged to penetrate the outer wall and the fireproof brick layer, and is characterized by having a thermocouple covering process for fixing a metal frame to the inner surface of the outer wall so as to cover the thermocouple and protective tube protruding inward, an amorphous refractory filling process for filling amorphous refractory inside the metal frame, and a fireproof brick assembly process for assembling fireproof bricks to the parts other than the metal frame. Effect of the Invention
[0010] The industrial furnace described in claim 1 is easy to install (furnace construction or repair) and can be installed in a short time. In addition, the frame is fixed to the inner surface of the outer wall, and the circumferential displacement of the firebricks is suppressed, so that the firebricks around the thermocouples are less likely to fall off, which reduces the frequency of necessary repairs and prevents damage to the thermocouples, leading to (contributing to) stable operation of the furnace.
[0011] In the industrial furnace described in claim 2, anchors are fixed to the outer wall inside the frame, so that the amorphous refractory material around the thermocouple is less likely to fall off from the inner surface of the outer wall, thereby more effectively preventing damage to the thermocouple.
[0012] According to the industrial furnace construction method (furnace construction method or repair method) described in claim 3, it is possible to efficiently construct, in a short period of time, an industrial furnace that is unlikely to damage thermocouples and can operate stably and requires less frequent repairs. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is an explanatory diagram (perspective view) showing a kiln body of a rotary kiln. [Diagram 2] FIG. 2 is an explanatory diagram showing a vertical cross section of the kiln body. [Diagram 3] FIG. 3 is an explanatory diagram showing an installation site (part A in FIG. 2) of a thermocouple (a is a cross-sectional view, and b is a front view seen from the inner surface side). [Figure 4] FIG. 1 is an explanatory diagram showing a frame (a is a perspective view, b is a front view seen from the inner surface side, c is a right side view, and d is a cross-sectional view taken along line BB in b). [Diagram 5] FIG. 2 is an explanatory diagram (front view) showing an anchor. [Figure 6] FIG. 1 is an explanatory diagram showing how a rotary kiln is constructed (a is a front view seen from the inside side, and b is a cross-sectional view). [Figure 7] FIG. 1 is an explanatory diagram showing how a rotary kiln is constructed (a is a front view seen from the inside side, and b is a cross-sectional view). [Figure 8] FIG. 1 is an explanatory diagram showing how a rotary kiln is constructed (a is a front view seen from the inside side, and b is a cross-sectional view). [Figure 9] FIG. 1 is an explanatory diagram showing how a rotary kiln is constructed (a is a front view seen from the inside side, and b is a cross-sectional view). [Figure 10] FIG. 1 is an explanatory diagram showing how a rotary kiln is constructed (a is a front view seen from the inside side, and b is a cross-sectional view). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] An embodiment of an industrial furnace and its construction method (construction or repair method) according to the present invention will be described in detail below with reference to the drawings. Fig. 1 shows a kiln body, which is a part of a rotary kiln for manufacturing cement. In the rotary kiln, a kiln body 1 that functions as a combustion chamber is formed in a long cylindrical shape, and the kiln body 1 can be rotated around a central axis along the longitudinal direction by a rotary drive device (not shown).
[0015] 2 shows a vertical cross section (vertical cross section perpendicular to the longitudinal direction) of the kiln body 1. The kiln body 1 is covered on its outer periphery with an outer wall 2 made of metal (carbon steel), and firebricks 3, 3... are assembled (laid) inside the outer wall 2, forming a stack of layers of firebricks. Furthermore, the kiln body 1 is provided with long cylindrical thermocouples 4, 4... for measuring the internal temperature, which are provided at predetermined intervals along the longitudinal direction and penetrate the outer wall 2 and the firebricks 3. The thermocouples 4, 4... are covered with cylindrical metal tubes (protective tubes).
[0016] 3 is an enlarged view of the installation portion of the thermocouple 4. In the installation portion of the thermocouple 4, a metal frame 5 is welded to the inner surface of the outer wall 2, and the tip end (temperature detection portion) of the thermocouple 4 protruding inward is covered by the frame 5.
[0017] 4 shows a frame 5 covering a thermocouple 4. The frame 5 is formed into a hollow rectangular prism shape with the top and bottom heights of the rear side higher than the front side by welding two metal plates (steel plates) 5a, 5a in a substantially fan shape for forming the side surfaces and two metal plates (steel plates) 5b, 5b in a substantially rectangular shape for forming the top and bottom surfaces. Furthermore, the outer peripheral edge and inner peripheral edge of the rear side have inclined grooves (see FIG. 4(d)). The frame 5 is fixed to the inner surface of the outer wall 2 by welding the outer peripheral edge and inner peripheral edge of the rear side where the grooves are formed.
[0018] Furthermore, inside the frame 5, a Y-shaped anchor 6 is welded to the inner surface of the outer wall 2 and is adjacent to the thermocouple 4. Figure 5 shows the anchor 6, which is formed by welding two cylindrical bodies, one long and one short, bent into a V shape. The anchor 6 is fixed to the inner surface of the outer wall 2 by welding the outer periphery of its tip into a circular shape.
[0019] Furthermore, the inside of the frame 5 welded to the exterior wall 2 as described above is filled with an amorphous refractory 7, and the anchor 6 and the periphery of the thermocouple 4 except for the tip surface are covered with the amorphous refractory 7. Furthermore, the firebricks 3, 3... are assembled with mortar (the main ingredient is the same as the firebricks) on the inner surface of the exterior wall 2 except for the part where the frame 5 is installed. The firebricks 3, 3... are formed into a substantially rectangular parallelepiped (quadratic pyramid) shape with the top and bottom heights of the back side being higher than the top and bottom heights of the front side. In the part adjacent to the frame 5, the firebricks 3, 3... are cut to a predetermined left and right width, and the length and width are adjusted according to the installation state of the surrounding firebricks 3, 3.... In addition, the tip surface of the thermocouple 4 is exposed to the surface of the amorphous refractory material 7, and the front edge of the frame body 5 is positioned approximately 20 mm inside the surface of the amorphous refractory material 7 (buried).
[0020] <Industrial furnace construction method> The construction method (construction or repair method) of the rotary kiln configured as described above will be described below. The construction method of the rotary kiln involves three steps: a. refractory brick assembly step, b. thermocouple coating step, and c. monolithic refractory packing step. Each step will be described below.
[0021] [a. Firebrick assembly process] Figures 6 to 10 show how to construct (build or repair) a rotary kiln. When constructing a rotary kiln, first, as shown in Figure 6, firebricks 3, 3... are attached to the inner surface of the outer wall (steel shell) 2 (except for the areas where the thermocouples 4, 4... are installed) using mortar and bonded to the outer wall 2. When repairing a rotary kiln after use, the (melted and damaged) firebricks 3, 3... attached to the inner surface of the outer wall 2 are peeled off to expose the inner surface of the outer wall 2, and new firebricks 3, 3... are then installed.
[0022] In constructing (building or repairing) a rotary kiln, it is preferable to assemble the firebricks 3, 3... successively from the bottom up with the kiln body 1 fixed at a predetermined rotational phase so that the firebricks 3, 3... do not peel off from the inner surface of the outer wall 2 during assembly. In addition, after the firebricks 3, 3... of a certain vertical width have been assembled, it is preferable to rotate the kiln body 1 appropriately so that the gravity of the firebricks 3, 3... that are not yet bonded to the outer wall 2 (the mortar has not yet hardened) does not act in a direction that would peel them off from the inner surface of the outer wall 2. In addition, various types of firebricks 3, 3... can be used.
[0023] [b. Thermocouple coating process] In the process of assembling the refractory bricks 3, 3... as described above, when the installation portion of the thermocouple 4 is reached (i.e., when the distance between the topmost assembled refractory brick 3 and the thermocouple 4 becomes less than a predetermined length (e.g., the height of the refractory brick 3)), the frame 5 is welded to the inner surface of the outer wall 2 so as to cover the thermocouple 4. At this time, the lower metal plate 5b of the frame 5 is placed on the upper surface of the assembled topmost refractory brick 3, 3.... When welding the frame 5 to the inner surface of the outer wall 2, the frame 5 is abutted against the inner surface of the outer wall 2 so as to cover the thermocouple 4, and in this state, the inner and outer peripheral edges of the rear side of each of the metal plates 5a, 5b... of the frame 5 with the grooves formed therein are welded to the inner surface of the outer wall 2.
[0024] The frame 5 is not particularly limited in shape as long as it is cylindrical, but a hollow rectangular columnar shape as shown in FIG. 4 is preferable because it is easy to assemble the refractory bricks 3, 3... around it. The frame 5 is preferably 10 to 50 mm shorter in width from front to back than the refractory bricks 3, 3... to be laid around it. If the difference between the front and back widths of the frame 5 and the refractory bricks 3, 3... is less than 10 mm, the frame 5 is likely to melt due to heat during use of the rotary kiln after construction, which is undesirable. Conversely, if the difference between the front and back widths of the frame 5 and the refractory bricks 3, 3... exceeds 50 mm, it is undesirable because it is not possible to sufficiently prevent unexpected stress from being applied to the thermocouples 4.
[0025] After welding the frame 5 to the inner surface of the outer wall 2 so as to cover the thermocouples 4, an anchor 6 having a Y-shape or the like is welded to the inside of the frame 5 (i.e., the outer periphery of the base end of the anchor 6 is welded to the inner surface of the outer wall 2). As the anchor 6, an anchor bent into an L-shape or an anchor branched into a Y-shape or the like can be suitably used. Then, after welding the frame 5 to the inner surface of the outer wall 2 so as to cover the thermocouples 4 as described above, the firebricks 3, 3... are assembled around the frame 5. When assembling the firebricks 3, 3... around the frame 5, the firebricks 3, 3... are divided into upper and lower or left and right as necessary.
[0026] [c. Monolithic refractory filling process] Then, the frames 5, 5·· are welded to the inner surface of the outer wall 2 so as to cover all the thermocouples 4, 4··, and the firebricks 3, 3·· are assembled to the entire inner surface of the outer wall 2. Then, the inside of each frame 5, 5·· welded to the outer wall 2 is filled with an amorphous refractory 7. The type of the amorphous refractory 7 is not particularly limited, and castables using hydrated cement bonds of alumina cement, low cement castables using ultrafine powders such as dispersants and silica fume, lightweight castables mixed with porous lightweight aggregates and cement materials, plastic materials in which plastic materials are added to refractory aggregates, ramming materials with lower plasticity than plastic materials, etc. can be suitably used. When the amorphous refractory 7 is filled inside the frame 5, care should be taken so that the tip surfaces of the thermocouples 4 are not covered by the amorphous refractory 7.
[0027] As described above, after the interior of the frames 5, 5... covering the thermocouples 4, 4... is filled with the monolithic refractory 7, the construction (building or repair) of the rotary kiln is completed by sufficiently curing the monolithic refractory 7. When constructing a rotary kiln, it is possible to weld the frame 5 to the installation position of the thermocouple 4 when the installation position of the thermocouple 4, 4... is reached while the firebricks 3, 3... are being assembled from the bottom up, as described above, or it is also possible to assemble the firebricks 3, 3... to the inner surface of the outer wall 2 after welding the frame 5, 5... at the installation positions of all the thermocouples 4, 4....
[0028] <Effects of industrial furnaces (rotary kilns)> As described above, the rotary kiln has metal frames 5,5... fixed to the inner surface of the outer wall 2 so as to cover the thermocouples (covered with protective tubes) 4,4... protruding inward, the interiors of the frames 5,5... filled with monolithic refractories 7, and the firebricks 3,3... assembled to the parts other than the frames 5,5..., so that construction work (furnace construction or repair work) is easy and can be completed in a short time. In addition, because the frames 5,5... are fixed to the inner surface of the outer wall 2 and the circumferential displacement of the firebricks 3,3... is suppressed, the firebricks 3,3... around the thermocouples 4,4... are less likely to fall off, so that the frequency of necessary repairs can be kept low and damage to the thermocouples 4,4... can be prevented, leading to stable operation of the furnace.
[0029] In addition, in the rotary kiln, since the anchors 6 are fixed to the outer wall 2 inside each frame 5, 5..., the amorphous refractory material 7 around each thermocouple 4, 4... is less likely to fall off from the inner surface of the outer wall 2, so that damage to each thermocouple 4, 4... can be more effectively prevented.
[0030] On the other hand, the construction method (furnace construction or repair method) for a rotary kiln described above includes a thermocouple covering process in which metal frames 5, 5·· are fixed to the inner surface of the outer wall 2 so as to cover the thermocouples 4 (covered with protective tubes), 4·· protruding inward, an amorphous refractory filling process in which amorphous refractory 7 is filled inside the metal frames 5, 5··, and a refractory brick assembling process in which refractory bricks 3, 3·· are assembled to the parts other than the metal frames 5, 5··. Therefore, a rotary kiln that is capable of stable operation and in which the thermocouples 4, 4·· are less likely to be damaged and require less frequent repairs can be efficiently constructed in a short period of time.
[0031] <Examples of changes to industrial furnaces and their construction methods> The industrial furnace according to the present invention is not limited to the above-mentioned embodiment, and the materials, shapes, structures, etc. of the outer wall, refractory bricks, thermocouples, frame, anchors, monolithic refractories, etc. can be appropriately changed as needed without departing from the spirit of the present invention. The construction method of the industrial furnace according to the present invention is also not limited to the above-mentioned embodiment, and the contents of each step of the thermocouple covering step, monolithic refractory filling step, and refractory brick assembly step can be appropriately changed as needed without departing from the spirit of the present invention.
[0032] For example, the industrial furnace according to the present invention is not limited to the above embodiment in which an anchor for preventing the amorphous refractory from falling off is welded to the outer wall inside the frame, but may be one in which one or more projections or anchors are welded to the inner surface of the iron plate constituting the frame. Furthermore, the anchor for preventing the amorphous refractory from falling off inside the frame is not limited to a Y-shaped one formed by welding two long and short cylindrical bodies bent into a V-shape as in the above embodiment, but can be changed to an L-shaped one or a trifurcated one. Furthermore, the material of the firebricks and the amorphous refractory filled in the frame can be appropriately changed depending on the use of the industrial furnace, etc.
[0033] In addition, the industrial furnace according to the present invention is not limited to a rotary kiln as in the above embodiment, but can be applied to various industrial furnaces as long as they have an internal temperature detection function using a thermocouple. When the industrial furnace according to the present invention is a rotary kiln, there is an advantage in that it is possible to more effectively prevent damage to the thermocouple caused by the refractory bricks being displaced in the circumferential direction as the kiln body rotates. [Industrial Applicability]
[0034] Since the industrial furnace according to the present invention has the above-mentioned excellent effects, it can be suitably used as an industrial furnace equipped with an internal temperature detection function using a thermocouple. Also, the industrial furnace construction method according to the present invention can be suitably used as a method for constructing or repairing an industrial furnace equipped with an internal temperature detection function using a thermocouple. [Explanation of symbols]
[0035] 1. Kiln body 2. Exterior wall (iron shell) 3. Firebricks 4. Thermocouple 5...Frame 6. Anchor 7. Monolithic refractories
Claims
1. An industrial furnace having a metal outer wall on which a refractory brick layer is laminated, and a thermocouple and a protective tube for detecting an internal temperature are provided so as to penetrate the outer wall and the refractory brick layer, An industrial furnace characterized in that a metal frame is fixed to the inner surface of the outer wall so as to cover the thermocouple and protective tube protruding inward, the inside of the frame is filled with amorphous refractory material, and firebricks are assembled to the part other than the frame.
2. 2. The industrial furnace according to claim 1, wherein an anchor is fixed to the outer wall inside the frame.
3. A method for constructing an industrial furnace in which a refractory brick layer is laminated inside a metal outer wall, and a thermocouple and a protective tube for detecting an internal temperature are provided so as to penetrate the outer wall and the refractory brick layer, a thermocouple covering step of fixing a metal frame to the inner surface of the outer wall so as to cover the thermocouple and the protective tube protruding inward; a monolithic refractory filling step of filling the inside of the metal frame with a monolithic refractory; and a refractory brick assembling step of assembling refractory bricks to the portion other than the metal frame.
Citation Information
Patent Citations
Repairing method of rotary kiln
JP1995159042A
Blast furnace bottom thermometer installing method
JP2006176828A
Method for measuring temperature of inside of furnace and method for monitoring inside of furnace
JP2018173358A