ODS alloy powder, its production method by plasma treatment and its use
A thermal plasma treatment method for ODS alloy powders addresses the challenges of uniform oxide distribution, achieving controlled composition and size, enhancing mechanical properties and reducing costs for applications in additive manufacturing and cold spray processes.
Patent Information
- Application Number
- JP2022143945
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-05-03
- Filing Date
- 2022-09-09
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2039-05-03
AI Technical Summary
Existing methods for producing oxide dispersion strengthened (ODS) alloy powders face challenges in achieving uniform distribution and controlled composition, size, and morphology of oxide reinforcements due to wettability issues and density differences between oxides and metals, making it difficult to form ODS alloys effectively.
A production method involving mechanical synthesis followed by thermal plasma treatment is used to grind a powder mixture of base metal and auxiliary powders, exposing it to a plasma torch to achieve a metal matrix with uniformly dispersed crystalline oxide particles, optimizing the size and distribution of oxide reinforcements.
The method enables the production of ODS alloy powders with well-controlled oxide precipitate size and distribution, resulting in improved mechanical properties and reduced manufacturing costs, suitable for applications in additive manufacturing and cold spray processes.
Smart Images

Figure 0007562613000003 
Figure 0007562613000004 
Figure 0007562613000005
Abstract
Description
[Technical Field]
[0001] The present invention relates to the field of oxide dispersion strengthened alloys (also called "ODS" alloys, an acronym for "Oxides Dispersion Strengthened"), in which oxides constitute a reinforcement for a dispersed metal matrix.
[0002] More particularly, the present invention relates to ODS alloy powders and methods for producing same. [Background technology]
[0003] Atomization is the most common method for producing metal powders and consists of atomizing a molten metal stream exposed to a high-pressure gas or water jet into fine droplets to obtain a powder.
[0004] However, atomization is not suitable for producing ODS alloy powders because it is often impossible to prepare the raw material, which is essential for atomization, in the form of a massive base metal (e.g., an ingot) containing a more or less uniformly dispersed oxide strengthening material.
[0005] In practice, oxide reinforcements do not melt at the same temperature as the base metal. The oxide reinforcement would then agglomerate due to wettability problems of the reinforcement in the molten base metal and density differences between the reinforcement and the metal. Therefore, in practice, casting methods are not used to form ODS alloys.
[0006] Currently, the preferred production method for forming ODS alloys is mechanical synthesis. This powder metallurgical technique is described, for example, in the work of C. Suryanarayana, "Mechanical alloying and milling," Progress in Materials Science, 2001, Vol. 46, pp. 1-184 (Reference 1). It is based on the high-energy co-milling of a first base metal powder (optionally pre-alloyed), previously obtained by atomization, to form a metal matrix, with at least one second metal powder to form an oxide reinforcement in the metal matrix. During milling, some or all of the atoms constituting the second metal powder are incorporated into the metal matrix, optionally, and in most cases, in the form of a solid solution.
[0007] However, during this mechanical synthesis step, no oxides are formed (at best, some of the oxides may be in the form of amorphous oxides, i.e., not crystalline. However, there is debate within the scientific community as to whether this non-crystalline oxide partially corresponds to the corresponding constituent atoms that are supposed to be in solid solution in the metal matrix, and whether the corresponding reinforcement has been seeded within the milled powder particles). Only an additional densification step (e.g., by hot extrusion or hot isostatic pressing) increases the oxide reinforcement within the metal matrix to finally obtain an ODS alloy.
[0008] It is only after the formation of a sufficient amount of oxide particles constituting the reinforcement dispersed in the metal matrix that a truly strengthened alloy is formed, thus fully justifying the name "ODS alloy."
[0009] However, it is difficult to control the formation of the ODS alloy powder thus obtained, in particular its composition, size, morphology, and distribution of the oxide reinforcement in the metal matrix. [Prior art documents] [Non-patent literature]
[0010]
Non-patent document 1
Non-patent document 2
Non-patent document 3
Non-patent document 4
Non-patented document 5
Non-patent document 6
[0011] One of the objects of the present invention is therefore to avoid or attenuate one or more of the above-mentioned drawbacks by proposing a new method for producing ODS alloy powders, more particularly having optimized compositional and / or microstructural properties. [Means for solving the problem]
[0012] The present invention therefore provides a method for producing a powder of a strengthened alloy (ODS alloy) in which the grains forming the powder particles constitute a metal matrix with crystalline oxide particles dispersed in its volume, the method comprising the following successive steps: i) - a base metal powder containing a master alloy for forming a metal matrix; - an auxiliary powder comprising at least one intermediate intended to incorporate into the metal matrix, optionally in the form of a solid solution, atoms for forming dispersed oxide particles; providing a powder mixture to be milled comprising: ii) milling the powder mixture in a gaseous milling medium according to a mechanical synthesis method to produce a precursor powder comprising a metal matrix incorporating said atoms, optionally in the form of a solid solution; iii) exposing the precursor powder to a thermal plasma generated by a plasma torch containing a plasma gas to obtain a reinforced alloy powder; The present invention relates to a method, comprising:
[0013] According to the production method of the present invention, a combination of mechanically compounded milling and plasma treatment steps produces an ODS alloy powder containing crystalline oxide particles as a reinforcement for a metal matrix.
[0014] Such a result would be unexpected to one skilled in the art for the following reasons: - Treatment of powders with thermal plasma generally causes melting of said powders. Thermal plasmas (also called "high temperature plasmas") are very energetic plasmas in which electrons and ions influence the behavior of the plasma. Thermal plasmas contrast with cold plasmas, which are less energetic and in which only electrons influence the behavior of the plasma.
[0015] However, as mentioned above, melting methods are definitely not recommended for forming ODS alloys, and therefore mechanical synthesis has been developed, as mentioned in the prior art review article by DJ Lloyd, "Particle reinforced aluminum and magnesium matrix composites," International Materials Reviews, 1994, Vol. 39, No. 1, pp. 1-23 (Reference 2).
[0016] This is also why the use of hot isostatic pressing at too high a temperature is generally avoided.
[0017] In fact, oxide particles generally melt at temperatures higher than the temperature of the master alloy used to form the metal matrix. Therefore, oxide particles tend to agglomerate due to their poor wettability in the molten metal and their density being different from that of the metal. Therefore, under such conditions, it is impossible to obtain alloys reinforced with oxide reinforcements, especially nanometer-sized reinforcements, that are relatively uniformly dispersed in the metal matrix.
[0018] - although this is debated in the scientific community, after mechanical synthesis, the atoms forming the oxide particles are distributed in the metal matrix, optionally and in most cases in the form of a solid solution. It is only in the subsequent densification step that the oxide particles become seeded and then crystallize. However, this densification step, as carried out in the prior art, is not advantageous for controlling the properties of the resulting reinforcement, in particular its size, morphology, degree of crystallization and / or distribution in the metal matrix.
[0019] - A plasma torch is provided to process and obtain powders with micrometer-sized particles. To obtain nanopowders, i.e. powders with nanometer-sized particles, a quench ring must be incorporated into the plasma torch. The plasma torch processing technique is high in energy, and without an additional device of the quench ring type, a person skilled in the art would expect that the plasma torch processing would not result in the formation of nanopowders or nanoprecipitates within the powder particles, as the precipitates would likely agglomerate.
[0020] Contrary to preconceived notions that the use of a plasma treatment process that melts the powder would not result in ODS alloy powders with optimized properties, the inventors have now shown that the oxide particles do not coalesce during the plasma treatment process.
[0021] On the contrary, oxide particles undergo two steps during their precipitation: i) a seeding step during which the metal atoms migrate through the metal matrix and associate to form, in effect, oxide molecules within the powder particles; and then ii) a crystallization step, which comprises growing oxide crystals to form oxide particles. In this case, it remains individualized.
[0022] Concurrently, still during the plasma treatment step, the master alloy generally undergoes massive crystallization, either wholly or partially, to form a metallic matrix, and the crystalline oxide reinforcement thus formed is uniformly dispersed within the wholly or partially crystalline metallic matrix.
[0023] Advantageously, therefore, the production method of the present invention allows for the production of ODS alloys in which the size and distribution of oxide precipitates that strengthen the metal matrix of the ODS alloy are very well controlled.
[0024] During the first step of the production method of the invention, a powder mixture is milled according to a mechanical compounding method, the powder mixture comprising a base metal powder and an auxiliary powder.
[0025] Generally, during the mechanical synthesis step ii), when the milling conditions are adjusted, the base metal powder and the auxiliary powders are intimately mixed, but in such a way that all atoms in the intermediates for forming the dispersed oxide particles are incorporated, optionally and in most cases in the form of a solid solution, into the master alloy which then forms the metal matrix.
[0026] With regard to the properties of the powders, there are no practical limitations on the particle size of the powders that make up the powder mixture used in the production method of the invention.
[0027] In most cases, the particles of the base powder have a median diameter (d) between 1 μm and 200 μm, or even between 20 μm and 80 μm, and generally between 60 μm and 65 μm. 50 )
[0028] The median diameter of the powder (d 50 ) is the particle size distribution that 50% of the population of particles that make up this powder have. 50 It is a size having a size smaller than.
[0029] This can be determined by techniques such as laser diffraction using a granulometer, as described for example in ISO standard 13320 (edition of December 1, 2009).
[0030] The base metal powder includes a master alloy that can be selected from an iron-based alloy, a nickel-based alloy, or an aluminum-based alloy.
[0031] Iron-based alloys, by mass, - 10%~30% chromium, - 10%~30% aluminum, - 8% to 25% chromium and 3 to 8% aluminum by mass may include:
[0032] The iron-based alloy may be, for example, a steel such as an austenitic, martensitic or ferritic steel, respecting, where applicable, the composition by mass given above.
[0033] Nickel-based alloys, by mass, 10% to 40% chromium, such as for example Inconel® 600, which contains 14% to 17% chromium, 10% to 40% chromium, 0.2% to 5% aluminum, 0.3% to 5% titanium, 0% to 5% tungsten, 0% to 2% molybdenum, and 0% to 2% tantalum, such as, for example, Inconel® 625 or 718, which contain 20% to 23% or 17% to 21% chromium, respectively; - 10% to 30% aluminum may include:
[0034] Typically, the nickel-based alloy may be Inconel®.
[0035] When the master alloy is an iron-based alloy or a nickel-based alloy, the powder mixture may contain 0.1% to 2.5%, or even 0.1% to 0.5%, by mass, of auxiliary powder.
[0036] The aluminum-based alloy may contain, by mass, 0% to 1% iron (or even 0% to 0.5% iron), 0% to 1% silicon, and 0% to 1% magnesium.
[0037] For example, the following composition by mass: - Aluminum alloy 1100 containing 0.95% iron, 0.05% magnesium, 0.2% copper, and 0.1% zinc; - Aluminum alloy 6262 containing up to 0.7% iron, - aluminum alloys of the 1000 series, such as aluminum alloy 1050 containing less than 0.4% iron, less than 0.25% silicon and no magnesium, - Aluminum alloys of the 6000 series, such as aluminum alloy 6063, containing less than 0.35% iron, less than 0.6% silicon, and less than 0.9% magnesium is.
[0038] In most cases, iron is an impurity and silicon improves the fluidity of the alloy.
[0039] When the master alloy is an aluminum-based alloy, the powder mixture may contain 0.2% to 5% by mass of auxiliary powder.
[0040] Generally, the proportion of the precursor powder that precipitates in the form of oxide particles during the plasma treatment step iii) may be high due to the efficiency of the production method of the present invention. This proportion may generally be between 80% (or even 90%) and 100%. When this proportion is 100%, all atoms that form the dispersed oxide particles have precipitated in the form of reinforcement in the metal matrix of the ODS alloy. Therefore, the proportion of atoms that form the dispersed oxide particles that are present in the metal matrix of the ODS alloy in a form other than crystalline oxide particles may be reduced by an additional proportion, or even close to or equal to 0%.
[0041] This feature of the production method of the present invention therefore allows the proportion of auxiliary powders in the milled powder mixture to be reduced. During the plasma treatment step iii), this promotes the formation of oxide particles of reduced size (e.g., in the form of nanoreinforcements) and their homogeneous distribution in the metal matrix of the ODS alloy. This also reduces the cost of the production method.
[0042] Therefore, the proportion of auxiliary powder in the powder mixture to be milled may be 0.1% to 0.3%, or even 0.1% to 0.2%.
[0043] For auxiliary powders, the particles generally have a median diameter (d 50 ) Therefore, this median diameter can be smaller than the median diameter of the base powder, which promotes the incorporation of atoms for forming dispersed oxide particles into the master alloy of the base metal powder.
[0044] The intermediates intended to incorporate atoms to form dispersed oxide particles are YFe3, Y2O3, Fe2O3, Fe2Ti, FeCrWTi, TiH 2、 TiO 2、 AlO3、 HfO 2、 SiO 2、 ZrO 2、 ThO 2、 MgO, or mixtures thereof.
[0045] The non-oxide compounds (e.g. YFe3, Fe2Ti, FeCrWTi, TiH2) are precursor compounds for the formation of the corresponding metal oxides after chemical reaction during the production method of the invention, which metal oxides are present in the strengthened alloy at the end of the method, more particularly in the form of crystalline oxide particles.
[0046] Thus, the atoms for forming the dispersed oxide particles can include at least one metal atom selected from yttrium, titanium, iron, chromium, tungsten, silicon, zirconium, thorium, magnesium, aluminum, or hafnium.
[0047] In many cases, the intermediate is a metal oxide and therefore contains at least one oxygen atom for inclusion in the composition of the oxide particle.
[0048] When the intermediate does not contain oxygen atoms, for example an intermetallic compound (such as Fe2Ti or FeCrWTi) or a hydride (such as TiH2), the oxygen is provided by another intermediate of the metal oxide type, optionally supplemented with oxygen present in the master alloy.
[0049] The powder mixture to be ground is subjected to a grinding step ii) according to the mechanical compounding method.
[0050] This step may be carried out, for example, in a mill selected from a ball mill or an attritor.
[0051] The gaseous grinding media is generally an atmosphere of controlled composition, which may include hydrogen, argon, helium, nitrogen, air, or mixtures thereof.
[0052] The precursor powder obtained at the end of the grinding step ii) is then subjected to a thermal plasma treatment step iii).
[0053] The parameters of the plasma torch operated during the plasma treatment step iii) are those conventionally used in the field of powder production, for example in the following studies: - Fan, X., Gitzhofer, F., Boulos, M., "Statistical Design of Experiments for the Spheroidization of Powdered Alumina by Induction Plasma Processing," J Therm Spray Tech, 1998, 7(2), pp. 247-253 (Reference 3), - Jiang, X.-L., Boulos, M., "Induction Plasma Spheroidization of Tungsten and Molybdenum Powders", Transactions of Nonferrous Metals Society of China, 2006, 16(1), pp. 13-17 (Reference 4), - Ye, R., Ishigaki, T., Jurewicz, J., Proulx, P., Boulos, MI, "In-Flight Spheroidization of Alumina Powders in Ar-H2 and Ar-N2 Induction Plasmas", Plasma Chem Plasma Process, 2004, 24(4), pp. 555-571 (Reference 5).
[0054] These studies show that there are no strict operating parameters and that a person skilled in the art can easily adapt them, for example by iteration, as a function of the amount of powder to be processed and / or the type of powder required. However, reference operating parameters suitable for the production method of the present invention are described below.
[0055] The plasma torch used may be an induction coupled radio frequency plasma torch, a blown arc torch, or a transferred arc torch.
[0056] Radio frequency plasma operates without electrodes. Energy transfer is effected by inductive coupling. To form the plasma, a magnetic field is applied to the plasma gas circulating in an induction coil.
[0057] The power of the plasma torch may be between 10 kW and 80 kW (more particularly between 10 kW and 40 kW), or even between 20 kW and 80 kW (more particularly between 20 kW and 40 kW).
[0058] The thermal plasma used in step iii) of the production method of the invention may be, for example, a plasma as described in the document P. Fauchais, "Plasmas thermiques: aspects fondamentaux" ("Thermal plasmas: basic aspects"), Techniques de l'ingenieur, Part D2810 V1, 2005, (Reference 6).
[0059] The thermal plasma may be at a plasma temperature between 200° C. and 12000° C., for example between 700° C. and 4000° C., for melting aluminum or magnesium, or tungsten, which melts at 3500° C. Generally, this temperature is sufficient to melt these species, more particularly species containing the metal atoms that make up the precursor powder.
[0060] Thermal plasma, especially arc plasma, has an electron density of 10 14 m -3 ~10 26 m -3 Between, or even 10 18 m -3 ~10 26 m -3 It can be made to be between.
[0061] The ionization energy may be between 0.5 eV and 50 eV.
[0062] At these temperatures and / or energies of the thermal plasma, the plasma gas contained in the plasma torch is generally fully ionized. In this case, the plasma gas can be selected from argon, helium, nitrogen, or mixtures thereof. This generally constitutes the core gas of the plasma torch and can be delivered to the plasma torch at a flow rate between 10 liters / minute and 40 liters / minute.
[0063] At the start of step iii), the pressure inside the reactor of the plasma torch can be reduced (for example, less than 200 Pa) to facilitate ionization of the plasma gas, thereby promoting the formation of plasma.
[0064] However, during step iii), the pressure inside the reactor of the plasma torch is generally between 25 kPa and 100 kPa. The lower this pressure, the faster the injection flow rate, and therefore the flow rate of the precursor powder through the plasma torch is accelerated.
[0065] In the case of an inductively coupled plasma torch, the reactor corresponds to the containment tube.
[0066] When the precursor powder comes into contact with the plasma, the oxide particle precipitation reaction (i.e., seeding and subsequent growth) is thermally activated and occurs almost instantaneously.
[0067] However, the flow rate at which the precursor powder is injected into the plasma torch can be adjusted more particularly as a function of the composition and / or amount of the powder to be treated.
[0068] The precursor powder can be injected into the plasma torch at a flow rate between 10 grams / minute and 45 grams / minute, preferably between 10 grams / minute and 30 grams / minute, and even more preferably between 10 grams / minute and 19 grams / minute. This precursor powder introduction flow rate can be set independently of the core gas flow rate, although it may be increased at least in part by increasing the plasma gas and / or sheath gas flow rates.
[0069] The precursor powder may be injected into the plasma torch by vibration using a worm screw or a rotating disk.
[0070] Injection upstream of the reactor (relative to the plasma gas flow) is generally paired with a high powder flow rate, while injection downstream of the reactor is paired with a slower powder flow rate, specifically to optimize the transit time of the precursor powder through the reactor. In practice, the upstream portion of the thermal plasma in the plasma torch is at a higher temperature, which may not be optimal. Furthermore, a high powder flow rate hinders the dispersion of the powder by recirculation within the plasma.
[0071] For example, a suitable compromise may be to set the outlet height of the injectors described below so that they open into the upper third of the reactor.
[0072] It may also be advisable to pair a moderate plasma torch power with a moderate precursor powder injection flow rate in order to maximize the proportion of intermediates that precipitate in the form of oxide particles.
[0073] Typically, the power of the plasma torch is between 10 kW and 40 kW (or even between 10 kW and 30 kW) coupled with a precursor powder flow rate between 10 g / min and 30 g / min (or even between 10 g / min and 19 g / min). - the proportion of precipitated oxide particles: generally, this improved proportion is such that 80 to 100% by mass, preferably 90% to 100%, and even more preferably 100% of the metal atoms contained in the entire strengthened alloy are in the form of crystalline oxide particles; and / or - Average circularity coefficient of the strengthened alloy powder particles: generally, for 80-100% by mass of crystalline oxide particles (preferably 90-100%, even more preferably 100%), this improved average circularity coefficient is between 0.95 and 1, or even between 0.98 and 1. can be improved.
[0074] The precursor powder and / or plasma gas may be introduced into the plasma torch via an injector.
[0075] The precursor powder may be injected into the plasma torch simultaneously with the plasma gas, for example, via an injector.
[0076] A sheath gas can be flowed over the exterior surface of the injector, which can stabilize the plasma and increase the efficiency of the production method of the present invention.
[0077] The sheath gas can be delivered to the plasma torch at a flow rate between 10 liters / minute and 100 liters / minute.
[0078] The sheath gas can be selected from argon, helium, nitrogen, hydrogen, or mixtures thereof.
[0079] The sheath gas may be a mixture of at least one primary sheath gas and at least one secondary sheath gas.
[0080] The primary sheath gas (often argon) can be delivered to the plasma torch at a high flow rate, for example, between 40 liters / minute and 100 liters / minute.
[0081] The auxiliary sheath gas has suitable thermal conductivity to improve heat transfer between the plasma gas and the precursor powder. Due to its reducing properties, it limits surface oxidation of the precursor powder particles, and is, for example, helium, nitrogen, or preferably hydrogen. The auxiliary sheath gas may be injected into the plasma torch at a flow rate slower than the main sheath gas supply rate, for example, between 1 liter / min and 40 liters / min.
[0082] According to the production method, at the end of the thermal plasma treatment step iii), an ODS alloy powder is obtained.
[0083] The particles of this powder generally have a size close to or identical to that of the precursor powder obtained at the end of the grinding step ii).
[0084] With respect to this microstructure, the ODS alloy powder particles comprise wholly or partially crystallized oxide particles dispersed throughout the volume of the metal matrix of the ODS alloy.
[0085] The oxide particles may be uniformly distributed throughout the volume of the metal matrix, not just in specific regions, and in particular, the oxide particles may not be preferentially located at the grain boundaries of the ODS alloy powder particles, which would be detrimental to the mechanical properties of materials derived from the ODS alloy powder (cracking, lower toughness, etc.).
[0086] The isotropic microstructure of the strengthened alloy particularly ensures uniform mechanical properties throughout the powder, and therefore optionally in materials produced with this powder, regardless of the direction of mechanical stress in this material.
[0087] The oxide particles may include at least one oxide selected from Y2O3, TiO2, Al2O3, HfO2, SiO2, ZrO2, ThO2, MgO, Al2O3, Y2Ti2O7, and Y2TiO5.
[0088] Generally, when the auxiliary powder contains only one intermediate, typically a metal oxide, the auxiliary powder is either directly incorporated into the composition of the oxide particles dispersed in the ODS alloy, or, if some of the auxiliary powder is not precipitated, is partially disposed in the matrix.
[0089] When the auxiliary powder contains multiple intermediates, one or more types of chemical combinations may occur between these compounds, which may result in the formation of mixed oxides. For example, when the auxiliary powder contains yttrium oxide YO and titanium hydride TiH, at least one oxide selected from YTiO, YTiO, YTiO, and YTiO can constitute all or a portion of the oxide particles of the ODS alloy.
[0090] Often, when the oxide contains yttrium and / or titanium, the oxide is a pyrochlore structure oxide, such as Y2Ti2O7.
[0091] The oxide particles formed in the ODS alloy have a median diameter (d 50 ) Preferably, it is between 1 nm and 200 nm, or even between 1 nm and 150 nm. It is therefore a nanoparticle. Unexpectedly, such a result can be obtained by the production method of the present invention without using a quench ring integrated into the plasma torch.
[0092] In many cases, some or all of the strengthening alloy powder particles are spherical, or at least ellipsoidal.
[0093] Thus, the average circularity coefficient of the strengthened alloy powder particles (generally when the crystalline oxide particles are 80-100% by mass, preferably 90%-100%, even more preferably 100%) may be between 0.95 and 1, or even between 0.98 and 1. The closer the value of this coefficient for a powder is to 1, the greater the proportion of particles of this powder that have a morphology approaching spheres.
[0094] The following websites: "http: / / guilhem.mollon.free.fr / Telechargements / Mechanique_des_Materiaux_Granulaires.pdf" As described in the work of G. Mollon, "Mecanique des materiaux granulaires" (Mechanics of granular materials), INSA de Lyon, 2015 (especially pages 23 and 24) (Reference 7), available from www.insa.org.uk / granularmaterials, and according to ISO standard 9276-6 (2008 edition), the circularity factor of a particle is calculated by dividing the radius of a circle completely inscribed in the particle (R inscr ) and the radius of the circle that completely circumscribes the particle (R circ) and these radii are shown in Figure 6 from Reference 7.
[0095]
number
[0096] In practice, the average circularity coefficient of a powder can be obtained from particle photographs and automated numerical analysis. Preferably, multiple photographs of the same particle are taken at different angles. The average circularity for these different angles is then calculated. Once this operation is performed for multiple grains, the average circularity for each grain is the average for all of the grains, which is the average circularity coefficient of the powder.
[0097] From an instrumental point of view, the average circularity coefficient of a powder can be obtained automatically using an instrument such as the "Camsizer Dynamic Image Analyzer" sold by Horiba Ltd.
[0098] In terms of its composition, the strengthening alloy consists, by mass, of: - 10-5000 ppm silicon; - 10-100 ppm sulfur; - Less than 20 ppm chlorine; - 2-10 ppm phosphorus; - 0.1-10 ppm of boron; - 0.1-10 ppm calcium; - Less than 0.1 ppm of each of the elements lithium, fluorine, heavy metals, Sn, As, and Sb It may further contain at least one element selected from the group consisting of:
[0099] These elements are often initially contained in the master alloy, and since the chemical composition of the base metal powder is generally not altered during the production method of the present invention, these elements are present unchanged in the metal matrix in this case.
[0100] The metal matrix and / or all or part of the oxide particles it contains may be crystalline, so that the strengthening alloy powder itself may be wholly or partially crystalline (preferably completely crystalline).
[0101] The microstructure of the strengthening alloy powder particles may preferably be single crystal (all particles have the same crystal structure) or polycrystalline (particles may have different crystal structures).
[0102] A high proportion of strengthening alloy powders that are crystalline may be suitable for use in cold spray type manufacturing processes.
[0103] Other characteristics of the microstructure and / or composition of the strengthened alloy obtained by the production method of the present invention are described below.
[0104] The present invention also relates to strengthened alloy powders obtained or obtainable by the production method defined herein, in particular in one or more of the variations described for the method, such as, for example, the microstructure and / or composition of the strengthened alloy powder.
[0105] More particularly, the present invention relates to a strengthened alloy powder in which the crystalline grains forming the powder particles constitute a metal matrix with crystalline oxide particles dispersed within the volume thereof.
[0106] To the inventors' knowledge, ODS alloys have never been obtained directly in the form of powder, which has the particular advantage of providing adequate control over the precipitation, of being usable in cold forming processes (such as the "cold spray" type), and / or of obtaining ODS alloys (e.g., ODS steels) with improved density by additional manufacturing methods. This direct production in the form of powder (i.e., in the form of divided powdered material), rather than in the form of an already densified material, has the particular advantage of allowing the strengthened alloy powder according to the invention to be used directly, optionally continuously, such as in batch mode, in a densification process making it possible to obtain agglomerates, and more particularly components, as described below.
[0107] The proportion by mass of the crystalline oxide particles is preferably such that they comprise 80% to 100% (preferably 90% to 100%, even more preferably 100%) by mass of the metal atoms contained in the entire strengthened alloy, which correspond to the atoms originally present in the intermediate, such as yttrium, titanium, iron, chromium, tungsten, silicon, zirconium, thorium, magnesium, aluminum, or hafnium.
[0108] In other words, the metal matrix, in dissolved form (generally on an atomic scale, e.g., in solid solution) and / or in the form of amorphous oxide particles, contains, relative to the total mass of said metal atoms contained in the entire strengthened alloy: - preferably 0% to 20% by weight of said metal atoms, Even more preferably, 0% to 10%, or even 0%, of said metal atoms may include:
[0109] The mass of the metal atoms in different regions of the reinforced alloy can be measured, for example, by EDX in a transmission electron microscope (TEM) using X-ray microanalysis (e.g., relative to a control region extrapolated for the entire reinforced alloy), typically for measurements in the metal matrix. If applicable, the mass of the metal atoms contained in the amorphous oxide particles and / or the crystalline oxide particles can also be determined by chemical analysis, or can be determined taking into account that this mass complements the mass of the metal atoms contained in the metal matrix only (i.e., the sum of these two masses is equal to the total mass of the metal atoms initially present in the supplemental powder).
[0110] The strengthening alloy particles may have an average circularity coefficient between 0.95 and 1.
[0111] The metal matrix of the reinforced alloy may be crystalline.
[0112] Preferably, the oxide particles are uniformly distributed throughout the volume of the metal matrix, and in particular, the oxide particles are preferably not present at the grain boundaries of the reinforcing alloy powder particles.
[0113] The metal matrix may be comprised of an iron-based alloy, a nickel-based alloy, or an aluminum-based alloy.
[0114] Iron-based alloys, by mass, - 10%~30% chromium, - 10%~30% aluminum, - 8% to 25% chromium and 3 to 8% aluminum by mass may include:
[0115] The iron-based alloy may be, for example, a steel such as an austenitic, martensitic or ferritic steel, respecting, where applicable, the composition by mass given above.
[0116] Nickel-based alloys, by mass, 10% to 40% chromium, such as for example Inconel® 600, which contains 14% to 17% chromium, 10% to 40% chromium, 0.2% to 5% aluminum, 0.3% to 5% titanium, 0% to 5% tungsten, 0% to 2% molybdenum, and 0% to 2% tantalum, such as, for example, Inconel® 625 or 718, which contain 20% to 23% or 17% to 21% chromium, respectively; - 10% to 30% aluminum may include:
[0117] Typically, the nickel-based alloy may be Inconel®.
[0118] When the metal matrix is comprised of an iron-based or nickel-based alloy, the strengthening alloy may contain 0.1% to 2.5%, or even 0.1% to 0.5%, by mass, of oxide particles.
[0119] The aluminum-based alloy may contain, by mass, 0% to 1% iron (or even 0% to 0.5% iron), 0% to 1% silicon, and 0% to 1% magnesium.
[0120] For example, the following composition by mass: - Aluminum alloy 1100 containing 0.95% iron, 0.05% magnesium, 0.2% copper, and 0.1% zinc; - Aluminum alloy 6262 containing up to 0.7% iron, - aluminum alloys of the 1000 series, such as aluminum alloy 1050 containing less than 0.4% iron, less than 0.25% silicon and no magnesium, - Aluminum alloys of the 6000 series, such as aluminum alloy 6063, containing less than 0.35% iron, less than 0.6% silicon, and less than 0.9% magnesium is.
[0121] In most cases, iron is an impurity and silicon improves the fluidity of the alloy.
[0122] When the metal matrix is made of an aluminum-based alloy, the strengthening alloy may contain 0.2% to 5% by mass of oxide particles.
[0123] The proportion of oxide particles in the strengthened alloy is such that it can contain 0.1% to 0.5% by weight of oxide particles.
[0124] If there is still a portion of the auxiliary powder that was not precipitated during the production method of the present invention, the strengthened alloy may contain 0.1 to 2.5 mass %, preferably 0.1 to 1%, or even less than 0.1%, of atoms of intermediates (generally metal atoms) for forming oxide particles. In this case, the intermediates are generally arranged in the metal matrix. This ratio reflects the degree of precipitation of one or more intermediates in the form of oxide particles. This can be measured, in particular, by X-ray microanalysis (e.g., EDX analysis using a transmission electron microscope) focusing on the volume of the metal matrix that does not contain oxide particles.
[0125] When an intermediate for forming oxide particles is present in the strengthened alloy, the intermediate may be YFe3, Y2O3, Fe2O3, Fe2Ti, FeCrWTi, TiH2, TiO2, Al2O3, HfO2, SiO2, ZrO2, ThO2, MgO, or mixtures thereof.
[0126] Starting from this composition, the oxide particles can comprise at least one oxide selected from Y2O3, TiO2, Al2O3, HfO2, SiO2, ZrO2, ThO2, MgO, Al2O3, Y2Ti2O7, Y2TiO5.
[0127] The oxide particles have a median diameter (d 50 ).
[0128] Strengthened alloys, by mass, - 10-5000 ppm silicon; - 10-100 ppm sulfur; - Less than 20 ppm chlorine; - 2-10 ppm phosphorus; - 0.1-10 ppm of boron; - 0.1-10 ppm calcium; - Less than 0.1 ppm of each of the elements lithium, fluorine, heavy metals, Sn, As, and Sb It may further contain at least one element selected from the group consisting of:
[0129] These elements are often present in a metal matrix.
[0130] The present invention also relates to the use of the strengthened alloy powder as defined above, in one or more of the variants described herein (i.e. the strengthened alloy powder obtained or obtainable by the production method of the present invention, or the strengthened alloy powder in which the grains forming the powder particles constitute a metal matrix in whose volume crystalline oxide particles are dispersed), and to the use in which the strengthened alloy powder of the present invention is subjected to a method of densification of the strengthened alloy powder, or a coating method in which the strengthened alloy powder is coated on a substrate (more particularly, to a thickness generally between 20 μm and 50 mm) to produce an agglomerate (more particularly a component).
[0131] As mentioned above, the properties of the reinforced alloy powder according to the invention make it particularly suitable for its densification to obtain agglomerates, more particularly in the form of components or for deposition on a substrate in the form of a coating (which may also in some cases be a layer of densified material, especially if it is relatively thick).
[0132] The densification method can be selected from a wide range of methods well known to those skilled in the art for densifying powders (particularly ODS alloy powders) to produce masses, more particularly components or coatings, such as additive manufacturing methods or powder injection molding methods.
[0133] The principle of additive manufacturing (also known as "3D printing") is that of generative manufacturing methods and boils down to two steps that are repeated until the final mass product is obtained: - 1. The process of producing a layer of material to a predetermined profile and thickness, depositing the material only where it is needed; - 2. The process of producing the next layer by adding material on top of the previous layer. This manufacturing can be summarized as so-called "stepwise" manufacturing.
[0134] Additive manufacturing is described in more detail, for example, in the following documents, which are incorporated herein by reference: - (Reference 8): F. Laverne et al., "Fabrication additive - Principles generaux" (Additive manufacturing - General Principles), Techniques de l'ingenieur, Part BM7017 V2 (published February 10, 2016); - (Reference 9): H. Fayazfara et al., "Critical review of powder-based additive manufacturing of ferrous alloys: Process parameters, microstructure and mechanical properties," Materials & Design, Vol. 144, 2018, pp. 98-128. - (Reference 10): T. DebRoy et al., "Additive manufacturing of metallic components - Process, structure and properties," Progress in Materials Science, Vol. 92, 2018, pp. 112-224. - (Reference 11): Ministry of Economics and Finance, French Republic, "Prospective - future of additive manufacturing - final report", January 2017 edition, ISBN: 978-2-11-151552-9; in particular Appendix 2 (pages 205-220), which describes additive manufacturing methods, especially those using metal powders (Appendix 2, Methods of manufacture, paragraphs 3, 4 and 5).
[0135] More particularly, the additive manufacturing method is selected from Selective Laser Melting (SLM) or "Laser Powder Bed Fusion" (L-PBF), Selective Electron Beam Melting (EBM) or "Electronic Powder Bed Fusion" (E-PBF), Selective Laser Sintering (SLS), Laser Spraying ("Direct Metal Deposition" (DMD) or "Laser Cladding"), or Binder Jetting.
[0136] The principle of powder injection molding is to injection mold a component from a mixture of metal or ceramic powder and a polymer binder, followed by debinding of the component in a furnace under a controlled atmosphere (generally an atmosphere similar or identical to that of the gaseous grinding medium, excluding hydrogen), and then densification of the latter by sintering, at temperatures between 350°C and 1220°C.
[0137] Depending on the material used, it is called "Ceramic Injection Molding" (CIM) or "Metal Injection Molding" (MIM) in English.
[0138] Powder injection molding is described in more detail, for example, in the following documents, which are incorporated herein by reference: - (Reference 12): D. Moinard et al., "Procedes de frittage PIM" (PIM sintering techniques), Techniques de l'ingenieur, Part M3320 VI (published June 10, 2011).
[0139] The coating method can be selected from coating methods well known to those skilled in the art, such as cold spraying or hot spraying.
[0140] The principle of cold spraying consists in accelerating a gas (such as nitrogen, helium, or argon), typically heated to a temperature between 100°C and 700°C, to supersonic speed through a "DeLaval" type nozzle. The powder material to be sprayed (here, the reinforced ODS alloy powder according to the invention) is then fed into the high-pressure section of the nozzle (between 10 and 40 bar) and sprayed in the "unmolten state" onto the surface of the component to be coated at a speed that may range from 600 to 1200 m / s. On contact with the component, the particles undergo plastic deformation and, upon impact, form a dense, coherent coating.
[0141] The advantage of this embodiment is that there is no melting of the particles and therefore the risk of oxidation is very low and it can be incorporated in hostile media.
[0142] Cold spraying is described in more detail, for example, in the following documents, which are incorporated herein by reference: - (Reference 13): A. Papyrin, "Cold Spray Technology", ISBN-13: 978-0-08-045155-8, 2007 edition.
[0143] The hot spraying method can be selected from flame hot spraying, electric arc spraying between two wires, or blown plasma spraying.
[0144] The hot spray method is described in more detail, for example, in the following documents, which are incorporated herein by reference: - (Reference 14): A. Proner, "Revetements par projection thermique" (Hot spray coatings), Techniques de l'ingenieur, Part M1645 V2 (published September 10, 1999).
[0145] The invention is advantageously supplemented by the following features, taken alone or according to any one of their technically possible combinations:
[0146] Detailed Description of the Invention In this specification of the present invention, verbs such as "comprise," "incorporate," "include," "contain," and their conjugations are open terms and therefore do not exclude the presence of additional elements and / or steps that are described after these terms and that are in addition to the initial elements and / or steps. However, these open terms also relate to certain embodiments in which only the initial elements and / or steps are intended, to the exclusion of others, and in this case the open terms also encompass the closed terms "consist of," "comprise," "consist of," and their conjugations.
[0147] The use of the indefinite article "a" or "an" for an element or step does not exclude the presence of a plurality of elements or steps, unless the context clearly states otherwise.
[0148] In the claims, any reference signs placed between parentheses shall not be construed as limiting the scope of the invention.
[0149] Furthermore, unless otherwise specified, - The limit values are included in the range of the indicated parameters; - The temperatures indicated are taken into account for implementation at atmospheric pressure; - The proportion by mass of any component of a reinforced alloy, master alloy or powder mixture is relative to the total mass of this alloy or this mixture.
[0150] In this specification, the term "base alloy" of a metal specifically included in the composition of a master alloy or any other alloy means any alloy based on a metal whose content is at least 50% by weight, in particular more than 90% by weight, or even more than 95% by weight, of the metal of the alloy. Base metals are, for example, iron, nickel, or aluminum. The base alloy is preferably suitable for use in the nuclear industry and / or under radiation exposure.
[0151] The expression "according to one or more modifications described herein" in relation to a material / element refers in particular to modifications with regard to the chemical composition and / or proportions in the constituents of this material and in any additional chemical species that the material / element may optionally contain, in particular modifications with regard to the chemical composition, structure, geometry, spatial arrangement and / or chemical composition of this element or of the subelements that are constituents of the element, such as those described in the claims.
[0152] Other objects, features, and advantages of the present invention will now be described in the following specification of specific embodiments of the present invention, given by way of example, and not by way of limitation, with reference to the accompanying Figures 1A to 6. [Brief explanation of the drawings]
[0153] [Figure 1A] 1 is a general view of a photograph obtained by scanning electron microscopy (SEM) of the precursor powder obtained after the milling step ii) in the production method of the present invention. [Figure 1B] 2 is a cross-sectional view of a photograph obtained by scanning electron microscopy (SEM) of the precursor powder obtained after milling step ii) in the production method of the present invention. FIG. [Figure 2A] 3 is a general view of an SEM photograph of the strengthened alloy powder obtained after the plasma treatment step iii) in the production method of the present invention. [Figure 2B] 3 is a cross-sectional view of an SEM photograph of the strengthened alloy powder obtained after the plasma treatment step iii) in the production method of the present invention. [Figure 3A] 3 is a cross-sectional view of an SEM photograph of the strengthened alloy powder obtained after the plasma treatment step iii) in the production method of the present invention. [Figure 3B] FIG. 2 is an enlarged cross-section of an SEM photograph of the strengthened alloy powder obtained after plasma treatment step iii) of the production method of the present invention, focusing on the oxide precipitates. [Figure 3C] 3C is a table showing the atomic molar ratios obtained by energy dispersive X-ray spectroscopy (EDX) of oxide precipitates identified by the numbers 1 to 7 shown in FIG. 3B. [Figure 4A] 1 is a bright-field TEM photograph of an ODS alloy piece obtained by the production method of the present invention. [Figure 4B] 1 is a bright-field TEM photograph of an ODS alloy piece obtained by the production method of the present invention. [Figure 5A] 1 is a series of photographs for analyzing oxide precipitates contained in the matrix of an ODS alloy powder obtained by the production method of the present invention. The photographs focus on oxide precipitates obtained and analyzed by bright field TEM. [Figure 5B] 1 is a series of photographs for analyzing oxide precipitates contained in the matrix of an ODS alloy powder obtained by the production method of the present invention. After analysis to locate the diffraction spots corresponding to the matrix and oxide precipitates, the TEM diffraction photographs are in their raw form, obtained with the sample holder tilted at an angle of −2° relative to X. [Figure 5C] TEM diffraction images in annotated form obtained with the sample holder tilted at an angle of −2° to X after analysis to locate the diffraction spots corresponding to the matrix and oxide precipitates of the ODS alloy powder obtained by the production method of the present invention. [Figure 5D] 1 is a series of photographs for analyzing oxide precipitates contained in the matrix of an ODS alloy powder obtained by the production method of the present invention, with corresponding annotated photographs taken with the sample holder tilted at an angle of −20° relative to X. [Figure 6] FIG. 1 is a diagram illustrating the parameters Rinscr and Rcirc required to calculate the circularity of powder crystal grains from a photograph taken at a specified angle. DETAILED DESCRIPTION OF THE INVENTION
[0154] The specific embodiments presented below relate to the production method of the present invention and the composition and microstructure of the strengthened alloy obtainable thereby.
[0155] 1. Implementation of the method for producing a reinforced alloy according to the invention In a ball mill under a hydrogen atmosphere, a base metal powder made of an iron-based master alloy (mass composition: 14% Cr, 1% W, 0.3% Si, 0.3% Mn, and 0.2% Ni, 1000 ppm C, and the remaining Fe) is mixed with auxiliary powders as intermediates for forming oxide particles, which contain, by mass, 0.3% titanium hydride (TiH2) powder and 0.3% yttrium oxide (YO3) powder relative to the total amount of the powder mixture.
[0156] The powder mixture is milled for 176 hours to form a precursor powder comprising a metal matrix consisting of a master alloy incorporating titanium, yttrium, and oxygen atoms by mechanical synthesis.
[0157] At this stage in the production method of the present invention, oxide particles in the form of precipitates have not yet formed.
[0158] The precursor powder is then fed into an inductively coupled radio frequency plasma torch capable of delivering up to 80 kW of power (PL50 model sold by Tecna).
[0159] This type of torch is described, for example, in the literature: Kim, K.S., Moradian, A., Mostaghimi, J., Soucy, G., "Modeling of Induction Plasma Process for Fullerene Synthesis: Effect of Plasma Gas Composition and Operating Pressure," Plasma Chemistry and Plasma Processing, 2010, Vol. 30, pp. 91-110.
[0160] The plasma torch has a ceramic containment tube immersed in rapidly circulating cooling water along its outer wall. Cooling the tube is essential to protect it from the high heat flux generated by the plasma. Surrounding the containment tube and beyond the cooling channel is an induction coil embedded in the body of the plasma torch and connected to a radio frequency generator. This coil generates an alternating magnetic field that creates the plasma medium.
[0161] A plasma gas (also called a core gas) is continuously injected into the interior of the containment tube.
[0162] A quartz intermediate tube is installed inside the ceramic confinement tube to protect the inner wall of the tube, and a sheath gas is introduced in a vortex shape along the inner wall of the confinement tube.
[0163] The precursor powder is injected directly into the center of the plasma discharge via a water-cooled injector located in the upper third of the plasma torch's reactor. The precursor powder is then heated and melted during flight. The induction plasma operates without electrodes coming into contact with the plasma gas, ensuring a contaminant-free process.
[0164] The precursor powder obtained above is exposed to a thermal plasma according to the operating conditions shown in Table 1. The gas flow rates are as follows: - Plasma gas (argon) = 30 L / min; - Main sheath gas (argon) = 80L / min~100L / min; - Auxiliary sheath gas (helium or hydrogen) = 0 to 30 L / min.
[0165] The mass ratio of the ODS powder according to the invention (more particularly of the crystalline oxide particles, which also have an average circularity coefficient between 0.95 and 1) to the total mass of the processed powder mixture is given in the last column of Table 1. A first approximation can be estimated by SEM photographic analysis of the powder obtained at the end of the production method of the invention.
[0166] [Table 1]
[0167] Table 1 shows that the percentage of oxides deposited is higher when the power of the plasma torch is moderate (generally between 10 kW and 40 kW, or even between 10 kW and 30 kW) and the injection flow rate of the precursor powder into the plasma torch is moderate (generally less than 30 g / min).
[0168] Therefore, in Experiments 4, 12, 17, and 18, the particles were spherical and the ODS alloy powders seeded with 100% oxide nanoreinforcement were - powder flow rate of 12 g / min (Experiment 4 and Experiment 12) or 15 g / min (Experiment 17 and Experiment 18), - The plasma torch power was 25 kW (Experiment 4 and Experiment 12) or 40 kW (Experiment 17 and Experiment 18), - The reactor pressure of the plasma torch was 6 psi or 41369 Pa (Experiments 4 and 12), or 10 psi or 68947 Pa (Experiments 17 and 18), - Argon as the central gas, argon as the main sheath ... is obtained when
[0169] Comparison of Runs 4 and 12 also demonstrates the complete reproducibility of the production method of the present invention and therefore the control over the properties of the ODS alloy powder that can be advantageously obtained.
[0170] In general, to obtain iron-based ODS alloy powders whose particles are spherical (more precisely, with an average circularity coefficient between 0.95 and 1) and have a defined proportion of oxide nanoreinforcements (average size generally between 50 nm and 500 nm, preferably between 50 nm and 200 nm) uniformly dispersed in the metal matrix of the ODS alloy, a person skilled in the art can use, for example, the following operating conditions for the plasma torch, with the power of the plasma torch and the flow rate of the precursor powder being the preferred parameters acting individually or together: → When the crystalline oxide particles are 20-30% by mass relative to the initial mass of the auxiliary powder (i.e., 70%-80% of the auxiliary powder did not produce crystalline oxide particles): Plasma torch power: between 40kW and 80kW (or even between 30kW and 80kW), Flow rate of precursor powder: between 20g / min and 45g / min; and optionally at least one of the following operating conditions: - Pressure inside the plasma torch reactor: 5 psi (i.e., between 34474 Pa and 14.5 psi (i.e., atmospheric pressure) Main sheath gas flow rate: between 80L / min and 100L / min; Auxiliary sheath gas flow rate: between 10L / min and 40L / min. → When the crystalline oxide particles exceed 80% by mass relative to the initial mass of the auxiliary powder (i.e., less than 20% of the auxiliary powder did not produce crystalline oxide particles): Plasma torch power: between 20kW and 40kW (or even between 20kW and 30kW), Flow rate of precursor powder: between 10g / min and 30g / min; and optionally at least one of the following operating conditions: Plasma torch reactor pressure: between 4 psi and 8 psi (i.e., between 27.6 kPa and 55.1 kPa); Main sheath gas flow rate: between 80L / min (or even 60L / min) and 100L / min; Auxiliary sheath gas flow rate: between 10L / min and 40L / min.
[0171] 2. Composition and microstructure of the strengthened alloy according to the present invention The precursor powder and the reinforced alloy powder obtained at the last step of mechanical synthesis and then at the step of oxide precipitation in a plasma torch according to Test 4, respectively, were characterized by SEM (FIGS. 1A, 1B, 2A, 2B, 3A, and 3B), TEM (FIGS. 4A and 4B), and EDX (table in FIG. 3C).
[0172] These analyses reveal that the precursor powder particles are of various shapes (Fig. 1A) and have a disordered amorphous microstructure (Fig. 1B) that does not contain any of the oxide particles seeded to form the reinforcement of the master alloy.
[0173] However, by combining the milling step ii) and the plasma treatment step iii) according to the production method of the present invention, it is possible to obtain ODS-type reinforced alloys in which the powder particles are essentially spherical and / or ellipsoidal (Figs. 2A, 2B and 3A) and constitute grains consisting of a crystalline metal matrix in which crystalline oxide particles are uniformly embedded, appearing on a grey background in the form of black dots representing the grains of the metal matrix in various shades (Figs. 2B, 3A and 3B). The crystalline oxide particles are nanoreinforcements and have a median diameter d 50 The size of the precipitates is between 150 nm and 200 nm. There are also many precipitates smaller than 5 nm.
[0174] EDX analyses were also performed by SEM and TEM electron microscopes. These are shown in the table in Figure 3C and indicate that the nanoreinforcements present in regions 1 through 5 of the ODS alloy powder particles are enriched with titanium, yttrium, and oxygen. In contrast, the corresponding EDX analyses performed on regions 6 and 7 of the metal matrix indicate the absence of oxygen, titanium, aluminum, and yttrium in the matrix (as in the case of aluminum and yttrium, when no values are listed, the mol% is <0.1%, or even 0, including the uncertainty limits). These results demonstrate that all atoms in the auxiliary powders used to form the dispersed oxide particles were indeed precipitated within the ODS alloy powder particles in the form of nanoreinforcements, as can be seen in the magnified views in Figures 4A and 4B.
[0175] Figures 5B, 5C, and 5D were obtained by TEM diffraction of the area shown in Figure 5A centered on the oxide precipitates of the ODS alloys of the present invention, and have superlattice diffraction peaks (i.e., two spots, one brighter) that are characteristic of the pyrochlore-type oxide Y2Ti2O7 conventionally obtained in iron-based ODS alloys.
[0176] The present invention is in no way limited to the described and shown embodiments, but those skilled in the art will be able to combine them and bring about many variations and modifications based on their general knowledge.
[0177] (References) [1] C. Suryanarayana “Mechanical alloying and milling”, Progress in Materials Science, 2001, 46, 1-184. [2] D.J. Lloyd, 「Particle reinforced aluminium and magnesium matrix composites」; International materials reviews, 1994, Vol. 39, No. 1, pages 1 to 23. [3] Fan, X., Gitzhofer, F., Boulos, M. 「Statistical Design of Experiments for the Spheroidization of Powdered Alumina by Induction Plasma Processing」, J Therm Spray Tech 1998, 7 (2), 247-253. [4] Jiang, X.-L., Boulos, M. 「Induction Plasma Spheroidization of Tungsten and Molybdenum Powders」, Transactions of Nonferrous Metals Society of China 2006, 16 (1), 13-17. [5] Ye, R., Ishigaki, T., Jurewicz, J., Proulx, P., Boulos, M.I. 「In-Flight Spheroidization of Alumina Powders in Ar-H2 and Ar-N2 Induction Plasmas」, Plasma Chem Plasma Process 2004, 24 (4), 555-571. [6] P. Fauchais, 「Plasmas thermiques: aspects fondamentaux」 [「Thermal plasmas: basic aspects」], Techniques de l’ingenieur, Part D2810 V1, 2005) [7] G. Mollon 「Mecanique des materiaux granulaires」 [Mechanics of granular materials], INSA de Lyon, 2015 (in particular pages 23 and 24) [reference 7] available from the following website: 「http: / / guilhem.mollon.free.fr / Telechargements / Mechanique_des_Materiaux_Granulaires.pdf」 [8] F. Laverne et al., 「Fabrication additive - Principes generaux」 [Additive manufacturing - General Principles], Techniques de l’ingenieur, Part BM7017 V2 (published February 10, 2016); [9] H. Fayazfara et al., 「Critical review of powder-based additive manufacturing of ferrous alloys: Process parameters, microstructure and mechanical properties」, Materials & Design, Volume 144, 2018, pages 98-128.
[10] T. DebRoy et al., 「Additive manufacturing of metallic components - Process, structure and properties」, Progress in Materials Science, Volume 92, 2018, pages 112-224.
[11] Ministry of Economics and Finance, French Republic, 「Prospective - future of additive manufacturing - final report」, edition of January 2017, ISBN: 978-2-11-151552-9.
[12] D. Moinard et al., 「PIM sintering techniques」 [PIM sintering techniques], Engineering Techniques, Part M3320 VI (published June 10, 2011)
[13] A. Papyrin, 「Cold Spray Technology」, ISBN-13: 978-0-08-045155-8, 2007 edition.
[14] A. Proner, 「Thermal Spray Coatings」 [Hot spray coatings], Engineering Techniques, Part M1645 V2 (published September 10, 1999).
Claims
1. A method for producing a powder of a strengthened alloy, the grains forming the particles of the powder constituting a metallic matrix and having crystalline oxide particles dispersed in its volume, comprising the following successive steps: i) - a base metal powder comprising a master alloy for forming said metal matrix, said master alloy being selected from an iron-based alloy, a nickel-based alloy, or an aluminium-based alloy, said base metal powder having a median diameter between 1 μm and 200 μm; at least one intermediate intended to incorporate into the metal matrix the atoms for forming the dispersed oxide particles, said intermediate for forming the dispersed oxide particles being YFe 3 , Y 2 O 3 , Fe 2 O 3 , Fe 2 Ti, FeCrWTi, TiH 2 , TiO 2 , Al 2 O 3 , HfO 2 , SiO 2 , ZrO 2 , ThO 2 , MgO, or a mixture thereof; and Providing a powder mixture to be milled, comprising: ii) milling said powder mixture in a gaseous grinding medium according to a mechanical synthesis method to produce a precursor powder comprising a metal matrix incorporating said atoms; iii) exposing the precursor powder to a thermal plasma generated by a plasma torch containing a plasma gas to obtain the strengthened alloy powder, the precursor powder being injected into the plasma torch at a flow rate between 10 grams / minute and 30 grams / minute, the power of the plasma torch being between 20 kW and 40 kW, and the reactor pressure of the plasma torch being between 25 kPa and 100 kPa; A method comprising:
2. 2. The method of producing a powder according to claim 1, wherein the iron-based alloy comprises 10-30% by weight of chromium.
3. 2. The method of producing a powder according to claim 1, wherein the iron-based alloy comprises 10-30% by weight of aluminum.
4. 2. The method of producing a powder according to claim 1, wherein the iron-based alloy comprises 8 to 25% by weight chromium and 3 to 8% by weight aluminium.
5. 5. A method for producing a powder according to any one of claims 1 to 4, wherein the iron-based alloy is a steel.
6. 2. The method of producing a powder according to claim 1, wherein the nickel-based alloy comprises 10 to 40% by weight of chromium.
7. 7. The method of producing a powder according to claim 6, wherein the nickel-based alloy comprises, by weight, 10% to 40% chromium, 0.2% to 5% aluminum, 0.3% to 5% titanium, 0% to 5% tungsten, 0% to 2% molybdenum, and 0% to 2% tantalum.
8. 2. The method of producing a powder according to claim 1, wherein the nickel-based alloy comprises 10-30% by weight of aluminum.
9. A method for producing a powder according to any one of the preceding claims, wherein when the master alloy is an iron-based or nickel-based alloy, the powder mixture comprises 0.1-2.5% by weight of the auxiliary powder.
10. 2. The method of producing a powder according to claim 1, wherein the aluminum-based alloy comprises, by mass, 0% to 0.5% iron, 0% to 0.3% silicon, and 0% to 1% magnesium.
11. A method for producing a powder according to claim 1 or 10, wherein when the master alloy is an aluminium based alloy, the powder mixture comprises 0.2-5 wt. % of the auxiliary powder.
12. 12. A method for producing a powder according to any one of claims 1 to 11, wherein the powder mixture comprises 0.1% to 0.3% by weight of the auxiliary powder.
13. 13. The method of producing a powder according to any one of claims 1 to 12, wherein the atoms for forming the dispersed oxide particles comprise at least one metal atom selected from yttrium, titanium, iron, chromium, tungsten, silicon, zirconium, thorium, magnesium, aluminum, or hafnium.
14. 14. The method of producing the powder of any one of claims 1 to 13, wherein the plasma torch is an induction coupled plasma torch, a blown arc torch, or a transferred arc torch.
15. 15. A method for producing a powder according to any one of claims 1 to 14, wherein the plasma gas is selected from argon, helium, nitrogen, or mixtures thereof.
16. A method for producing a powder according to any one of claims 1 to 15, wherein the plasma gas is injected into the plasma torch at a flow rate between 10 litres / min and 40 litres / min.
Citation Information
Patent Citations
Method for preparing injection-molding nickel-base ODS (oxide dispersion strengthened) alloy
CN102251131A
Method for near-net shaping of porous Ni-based ODS (oxide dispersion strengthening) alloy
CN103060591A
Heating furnace pipe and usage therefor
JP2003139273A
Ferritic oxide dispersion reinforced alloy and manufacturing method therefor
JP2014198900A
An additional manufacturing method of parts by melting or sintering powder particles, using a powder suitable for the target method / material combination together with a high-energy beam
JP2016532773A